Photoelectric conversion element and method for producing the same

A graded structure in the photoelectric conversion layer with controlled Ag distribution addresses lattice mismatch and recombination issues, enhancing efficiency by maintaining band gap and adhesion.

JP7569218B2Active Publication Date: 2024-10-17IDEMITSU KOSAN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020561354
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-19
Filing Date
2019-12-12
Publication Date
2024-10-17
Estimated Expiration
2039-12-12

AI Technical Summary

Technical Problem

Lattice mismatch and increased carrier recombination occur when high concentrations of Ag are added to the photoelectric conversion layer, leading to reduced efficiency in CIS-based photoelectric conversion elements.

Method used

A photoelectric conversion element with a graded structure where the region exhibiting the minimum band gap and maximum Ag concentration are located in the intermediate region, with controlled Ag concentrations in the front and back regions to minimize lattice mismatch and recombination.

Benefits of technology

This configuration suppresses carrier recombination and improves photoelectric conversion efficiency by maintaining the desired band gap and adhesion, reducing series resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569218000005
    Figure 0007569218000005
  • Figure 0007569218000006
    Figure 0007569218000006
  • Figure 0007569218000007
    Figure 0007569218000007
Patent Text Reader

Abstract

A photoelectric conversion element (10) includes a photoelectric conversion layer (13) formed between a first electrode layer (12) and a second electrode layer (15). The photoelectric conversion layer includes group I elements Cu and Ag, group III elements In and Ga, and group VI elements Se and S. The photoelectric conversion layer has a front-side region (13A) located on the light-receiving surface side, a back-side region (13C) located on the back side of the light-receiving surface, and an intermediate region (13B) located between the front-side region and the back-side region. The intermediate region (13B) includes a portion exhibiting a minimum band gap in the thickness direction of the photoelectric conversion layer. When the Ag concentration is defined as the ratio of the molar amount of Ag to the sum of the molar amounts of group I elements, group III elements, and group VI elements other than Ag, the intermediate region (13B) includes a portion exhibiting a maximum Ag concentration in the thickness direction of the photoelectric conversion layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photoelectric conversion element and a method for manufacturing the photoelectric conversion element. [Background technology]

[0002] Conventionally, CIS-based photoelectric conversion elements have been proposed that use, as a photoelectric conversion layer, a I-III-VI2 group compound semiconductor with a chalcopyrite structure that contains Cu, In, Ga, Se, and S. This type of photoelectric conversion element is relatively inexpensive to manufacture, and is expected to have high photoelectric conversion efficiency because it has a large absorption coefficient in the visible to near-infrared wavelength range.

[0003] A CIS-based photoelectric conversion element is constructed, for example, by forming a metal back electrode layer on a substrate, forming a photoelectric conversion layer made of a Group I-III-VI2 compound on top of that, and then forming a buffer layer and a window layer made of a transparent conductive film in that order. In addition, in CIS photoelectric conversion elements, it is important to shift the minimum value of the band gap of the photoelectric conversion layer to the inside in the thickness direction of the photoelectric conversion layer (double graded structure) in order to avoid interface recombination. A known method for achieving a double graded structure is to control the concentration of S / VI or Ga / III in the depth direction of the photoelectric conversion layer.

[0004] Furthermore, as a technique for increasing the efficiency of CIS-based photoelectric conversion elements, it is known to substitute a portion of Cu, which is a Group I element, in the CIS-based photoelectric conversion layer with Ag. For example, US Patent No. 5,999,633 discloses an optoelectronic device in which (Ag,Cu)(In,Ga)(Se,S)2 is applied to an absorber layer to substantially change the band gap of the absorber with Ag. US Patent No. 5,999,633 also discloses that the absorber layer has a transition region disposed between a surface region and a bulk region, and that the transition region Ag / (Ag+Cu) molar ratio in the transition region is higher than the surface region Ag / (Ag+Cu) ratio in the surface region. Furthermore, Patent Document 2 discloses that an ACIGS thin film that can be used as a light absorbing layer in a solar cell is formed by partially substituting Ag for Cu in CIGS. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2014-524145 [Patent Document 2] JP 2017-128792 A Summary of the Invention [Problem to be solved by the invention]

[0006] Adding a high concentration of Ag to the surface side of the photoelectric conversion layer, which is the light receiving surface of the photoelectric conversion element, increases the lattice mismatch at the interface between the photoelectric conversion layer and the buffer layer (or the second electrode layer if there is no buffer layer). It is desirable to avoid such an increase in lattice mismatch, as it increases carrier recombination and reduces the efficiency of photoelectric conversion. On the other hand, adding a high concentration of Ag to the back side of the photoelectric conversion layer facing the substrate leads to an increase in S in the photoelectric conversion layer on the back side and an increase in voids in the photoelectric conversion layer on the back side. As a result, there is concern about a decrease in adhesion between the photoelectric conversion layer and the back electrode and an increase in the series resistance Rs of the photoelectric conversion element to which this photoelectric conversion layer is applied.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and provides a means for effectively suppressing carrier recombination in a photoelectric conversion layer doped with Ag and improving the photoelectric conversion efficiency of a photoelectric conversion element. [Means for solving the problem]

[0008] A photoelectric conversion element according to an embodiment of the present invention has a photoelectric conversion layer formed between a first electrode layer and a second electrode layer, the photoelectric conversion layer including group I elements Cu and Ag, group III elements In and Ga, and group VI elements Se and S. The photoelectric conversion layer has a front side region located on the light receiving surface side, a back side region located on the back side of the light receiving surface, and an intermediate region located between the front side region and the back side region. The light receiving surface side of the intermediate region faces the front side region, and the back side of the intermediate region faces the back side region. The intermediate region is located in a range of 0.1 to 0.7 in the thickness direction of the photoelectric conversion layer from the light-receiving surface of the photoelectric conversion layer when the thickness of the photoelectric conversion layer is normalized to 1, and the front side region, the intermediate region, and the back side region each contain Ag. The intermediate region includes a portion showing the minimum band gap in the thickness direction of the photoelectric conversion layer. When the Ag concentration is defined as the ratio of the molar amount of Ag to the sum of the molar amounts of group I elements, group III elements, and group VI elements other than Ag, the intermediate region includes a portion showing the maximum Ag concentration in the thickness direction of the photoelectric conversion layer. The molar amount of Ag included in the back side region is 0.19 or less of the molar amount of Ag included in the entire photoelectric conversion layer. Effect of the Invention

[0009] According to the photoelectric conversion element of the present invention, the portion showing the minimum band gap and the portion showing the maximum Ag concentration in the thickness direction of the photoelectric conversion layer are both included in the intermediate region, and carrier recombination is suppressed in the portion showing the minimum band gap, thereby improving the photoelectric conversion efficiency of the photoelectric conversion element. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a cross-sectional view illustrating an example of a photoelectric conversion element according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a photoelectric conversion layer. [Diagram 3] 3 is a cross-sectional view showing one step of a method for manufacturing a photoelectric conversion element. FIG. [Figure 4] 3 is a cross-sectional view showing one step of a method for manufacturing a photoelectric conversion element. FIG. [Diagram 5] 3 is a cross-sectional view showing one step of a method for manufacturing a photoelectric conversion element. FIG. [Figure 6]3 is a cross-sectional view showing one step of a method for manufacturing a photoelectric conversion element. FIG. [Figure 7] Graph (A) is a graph showing a profile of the band gap (Eg) of the photoelectric conversion layer of the example, and graphs (B) and (C) are graphs showing profiles of the element concentration composition ratio of the photoelectric conversion layer of the example. [Figure 8] 1 is a graph showing the quantum efficiency of a photoelectric conversion element having Ag added to the photoelectric conversion layer, and the wavelength dependency of the change in quantum efficiency. [Figure 9] 1 is a graph showing the change in correlation between the band gap and the open circuit voltage loss depending on whether or not Ag is added. [Figure 10] FIG. 1 is a diagram showing an example of a solar cell submodule to which a photoelectric conversion element is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment will be described with reference to the drawings. In the embodiments, in order to make the description easier to understand, structures or elements other than the main parts of the present invention will be described in a simplified or omitted manner. Also, in the drawings, the same elements are given the same reference numerals. Note that in the drawings, the thickness, shape, etc. of each layer are shown only diagrammatically and do not represent the actual thickness, shape, etc.

[0012] <Structure of photoelectric conversion element 10> FIG. 1 is a cross-sectional view in the thickness direction showing an example of a photoelectric conversion element 10 according to an embodiment. The photoelectric conversion element 10 has a substrate structure in which, for example, a first electrode layer 12, a photoelectric conversion layer 13, a buffer layer 14, and a second electrode layer 15 are laminated on a substrate 11. Light 20, such as sunlight, is incident on the photoelectric conversion element 10 from the side opposite to the substrate 11 side.

[0013] (Substrate 11) The substrate 11 can be selected from a glass substrate, a resin substrate, a metal substrate, and the like. The substrate 11 may contain an alkali metal such as sodium or potassium. The shape of the substrate 11 is, for example, a rectangle, but is not limited to this. In addition, the substrate 11 is assumed to be a hard substrate, but instead, a flexible substrate having flexibility may be used. The flexible substrate includes, for example, a stainless steel foil, a titanium foil, a molybdenum foil, a ceramic sheet, or a resin sheet.

[0014] (First electrode layer 12) The first electrode layer 12 is disposed on the substrate 11. The first electrode layer 12 is, for example, a metal electrode layer. The first electrode layer 12 preferably comprises a material that is unlikely to react with the photoelectric conversion layer 13 in the manufacturing method described below. The first electrode layer 12 can be selected from molybdenum (Mo), titanium (Ti), chromium (Cr), and the like. The first electrode layer 12 may contain the same material as that contained in the second electrode layer 15 described below. For example, the thickness of the first electrode layer 12 is set to 200 nm to 500 nm.

[0015] (Photoelectric conversion layer 13) The photoelectric conversion layer 13 is disposed on the first electrode layer 12. The photoelectric conversion layer 13 functions as a polycrystalline or microcrystalline p-type compound semiconductor layer. The photoelectric conversion layer 13 includes a mixed crystal compound (I-III-(Se,S)2) having a chalcopyrite structure, which includes a group I element, a group III element, and a group VI element (chalcogen element) including selenium (Se) and sulfur (S). The group I element can be selected from copper (Cu), silver (Ag), gold (Au), and the like. The group III element can be selected from indium (In), gallium (Ga), aluminum (Al), and the like. The photoelectric conversion layer 13 may also include tellurium (Te) and the like as a group VI element, in addition to selenium and sulfur. The photoelectric conversion layer 13 may also include an alkali metal such as Li, Na, K, Rb, or Cs. For example, the thickness of the photoelectric conversion layer 13 is set to 1.0 μm to 3.0 μm.

[0016] Photoelectric conversion layer 13 of this embodiment contains at least indium and gallium as group III elements, and at least sulfur as group VI element. Photoelectric conversion layer 13 has a double graded structure due to gallium and sulfur, in which the band gap is large on the light receiving surface side (upper side in the figure) and the substrate 11 side (lower side in the figure), and is small in the interior (middle).

[0017] The photoelectric conversion layer 13 of this embodiment has three regions, a front side region 13A, an intermediate region 13B, and a back side region 13C, along the thickness direction of the photoelectric conversion layer 13 (the vertical direction in the figure). The front side region 13A is located on the light receiving surface side of the photoelectric conversion layer 13, and the back side region 13C is located on the substrate 11 side of the photoelectric conversion layer 13, which is the back side with respect to the light receiving surface. The intermediate region 13B is located between the front side region 13A and the back side region 13C in the photoelectric conversion layer 13. The portion showing the minimum value of the band gap in the thickness direction of the photoelectric conversion layer 13 is present in the intermediate region 13B.

[0018] When the film thickness of the photoelectric conversion layer 13 is normalized to 1, the intermediate region 13B of the photoelectric conversion layer 13 is preferably in the range of 0.1 to 0.7 of the film thickness of the photoelectric conversion layer 13 based on the surface on the light-receiving surface side of the photoelectric conversion layer 13. In the above case, the front side region 13A is formed in a range of film thickness from the surface on the light-receiving surface side of the photoelectric conversion layer 13 to less than 0.1. Similarly, the back side region 13C is formed in a range of film thickness from more than 0.7 to 1.0 from the surface on the light-receiving surface side of the photoelectric conversion layer 13.

[0019] As described above, by setting the film thickness of the surface side region 13A, it is possible to suppress the expansion of the lattice mismatch at the interface between the photoelectric conversion layer 13 and the buffer layer 14 (or the second electrode layer 15 if the buffer layer 14 is not present), and it is possible to suppress the increase in carrier recombination. Moreover, by setting the film thickness of the back surface side region 13C as described above, it is possible to suppress an increase in S and an increase in voids in the photoelectric conversion layer 13 on the first electrode layer 12 side (back surface electrode side). As a result, it is possible to suppress a decrease in adhesion between the photoelectric conversion layer 13 and the first electrode layer 12. It is also possible to suppress an increase in the series resistance Rs of the photoelectric conversion element 10 to which this photoelectric conversion layer 13 is applied.

[0020] The photoelectric conversion layer 13 of this embodiment contains at least Ag as a group I element. The Ag added to the photoelectric conversion layer 13 reduces the antisite defect In Cu As a result, the carrier density in the photoelectric conversion layer 13 can be increased, and the recombination of carriers generated in the photoelectric conversion layer 13 can be reduced.

[0021] The portion showing the maximum value of the Ag concentration in the thickness direction of the photoelectric conversion layer 13 is present in the intermediate region 13B. Here, the Ag concentration is defined as the ratio of the molar amount of Ag to the sum of the molar amounts of group I elements, group III elements, and group VI elements other than Ag in the photoelectric conversion layer 13 (Ag / I+III+other than Ag) VI ) is shown. In this embodiment, the portion showing the minimum band gap of the photoelectric conversion layer 13 is present in the intermediate region 13B, and therefore the portion showing the minimum band gap and the portion showing the maximum Ag concentration are close to each other in the thickness direction of the photoelectric conversion layer 13. Therefore, in this embodiment, carrier recombination is suppressed in the portion showing the minimum band gap, which leads to improvements in the open circuit voltage and short circuit photocurrent of the photoelectric conversion element 10, and the photoelectric conversion efficiency of the photoelectric conversion layer 13 is improved.

[0022] Moreover, the Ag concentration in the photoelectric conversion layer 13 is preferably set to a concentration that does not substantially change the band gap of the photoelectric conversion layer 13 . In the photoelectric conversion layer 13, the band gap is substantially enlarged in the portion where a large amount of Ag is added. In other words, when the Ag concentration is increased, the band gap of the region including the portion showing the minimum value of the band gap of the double graded structure tends to be enlarged. In addition, depending on the Ag concentration profile, the photoelectric conversion layer 13 may not have a desired band profile. For the above reasons, it is preferable that the Ag concentration of the photoelectric conversion layer 13 in this embodiment is set to a level that does not substantially change the band gap of the photoelectric conversion layer 13. As a result, in this embodiment, the band gap of the photoelectric conversion layer 13 does not need to be substantially enlarged compared to when Ag is not added, and a desired band profile similar to that when Ag is not added can be obtained for the photoelectric conversion layer 13. Therefore, the efficiency of photoelectric conversion can be improved.

[0023] As an example, the maximum value of the Ag concentration in the photoelectric conversion layer 13 is preferably 0.00519 to 0.0140. When the maximum value of the Ag concentration exceeds 0.0140, the band gap of the photoelectric conversion layer 13 is substantially enlarged compared to the case where Ag is not added. On the other hand, when the maximum value of the Ag concentration is smaller than 0.00519, the band gap is not substantially enlarged. However, in this case, it is difficult to sufficiently obtain the effect of increasing the carrier density of the photoelectric conversion layer 13 and the effect of reducing the recombination of carriers generated in the photoelectric conversion layer 13.

[0024] In addition, the portion showing the maximum value of Ag concentration is preferably disposed closer to the light receiving surface of the photoelectric conversion layer 13 than to the back surface of the photoelectric conversion layer 13 in the thickness direction of the photoelectric conversion layer 13. In other words, when the entire photoelectric conversion layer 13 is divided into two regions, a light receiving surface side region and a back surface side region, the portion showing the maximum value of Ag concentration is included in the light receiving surface side region of the two equally divided photoelectric conversion layer 13. More carriers are generated in the light receiving surface side region of the photoelectric conversion layer 13. Therefore, according to the above configuration, the contribution to suppressing carrier recombination is greater than when the portion showing the maximum value of Ag concentration is included in the back surface side region of the photoelectric conversion layer 13.

[0025] Similarly, the portion showing the maximum value of Ag concentration is preferably disposed closer to the boundary of the intermediate region 13B on the light receiving surface side than to the boundary of the intermediate region 13B on the back surface side in the thickness direction of the photoelectric conversion layer 13. In other words, when only the intermediate region 13B is divided into two equal parts, a region on the light receiving surface side and a region on the back surface side, the portion showing the maximum value of Ag concentration is included in the above-mentioned region on the light receiving surface side in the intermediate region 13B divided into two equal parts. In the intermediate region 13B as well, more carriers are generated in the region on the light receiving surface side. Therefore, according to the above configuration, the contribution to suppressing carrier recombination is greater than when the portion showing the maximum value of Ag concentration is included in the region on the back surface side of the intermediate region 13B.

[0026] In addition, in the thickness direction of the photoelectric conversion layer 13, the portion of the photoelectric conversion layer 13 showing the maximum Ag concentration is preferably located on the side opposite to the light receiving surface, relative to the portion of the photoelectric conversion layer 13 showing the minimum band gap. This allows the portion of the photoelectric conversion layer 13 showing the maximum Ag concentration to be located at a position with a high Ga concentration. As a result, the antisite Ga due to the addition of Ag is increased in the portion of the photoelectric conversion layer 13 where the Ga amount is relatively large. Cu The effect of suppressing the increase in

[0027] On the other hand, the molar amount of Ag contained in the surface side region 13A is preferably 0.06 or less relative to the molar amount of Ag contained in the entire photoelectric conversion layer 13. As described above, by setting the molar amount of Ag in the surface side region 13A to 0.06 or less of the entire molar amount of Ag, it is possible to further suppress the expansion of the lattice mismatch at the interface between the photoelectric conversion layer 13 and the buffer layer 14 (or the second electrode layer 15), and to suppress the increase in carrier recombination.

[0028] In addition, the molar amount of Ag contained in the back surface side region 13C is preferably 0.19 or less relative to the molar amount of Ag contained in the entire photoelectric conversion layer 13. As described above, by setting the molar amount of Ag in the back surface side region 13C to 0.19 or less of the total molar amount of Ag, it is possible to further suppress an increase in S and an increase in voids in the photoelectric conversion layer 13 on the first electrode layer 12 side (back electrode side). As a result, it is possible to suppress a decrease in adhesion between the photoelectric conversion layer 13 and the first electrode layer 12. In addition, it is possible to suppress an increase in the series resistance Rs of the photoelectric conversion element 10 to which this photoelectric conversion layer 13 is applied.

[0029] Furthermore, by lowering the molar amount of Ag in regions other than the intermediate region 13B where Ag is effectively utilized (the front side region 13A and the back side region 13C), the utilization efficiency of Ag in the photoelectric conversion layer 13 is increased and the amount of Ag used can be reduced.

[0030] In addition, in the entire photoelectric conversion layer 13, Cu / III (I / III other than Ag) is smaller than 1. In addition, Cu / III in the front side region 13A, which is the region on the light-receiving surface side of the photoelectric conversion layer 13, may exceed 1. Furthermore, the concentration profile of Cu / III in the photoelectric conversion layer 13 may increase from the back side (substrate 11 side) toward the front side (light-receiving surface side) in the thickness direction. Here, Cu / III indicates the ratio of the molar amount of Cu to the sum of the molar amounts of group III elements in the photoelectric conversion layer 13. The above Cu / III may be interpreted as the ratio of the sum of the molar amounts of group I elements other than Ag to the sum of the molar amounts of group III elements (I / III other than Ag).

[0031] The band gap of the photoelectric conversion layer determined from the quantum efficiency of the photoelectric conversion element is preferably 1.04 eV to 1.20 eV.

[0032] The methods for measuring various parameters related to the photoelectric conversion layer 13 will be described below. In the above, the concentration profile of the elements in the photoelectric conversion layer 13 can be measured by glow discharge optical emission spectrometry while scraping the surface of the sample by sputtering. The band gap profile of the photoelectric conversion layer 13 can be calculated from the concentration profile of the elements obtained above. The band gap of the photoelectric conversion layer 13 is calculated from the absorption edge on the long wavelength side of the quantum efficiency of the photoelectric conversion element 10. Specifically, the rate of change of the quantum efficiency on the long wavelength side with respect to the wavelength is calculated, and the energy of the wavelength at which the rate of change is the maximum value is taken as the band gap. Note that the band gap does not substantially change means that the band gap calculated from the quantum efficiency of the photoelectric conversion element changes by 1.5% or less.

[0033] (Buffer layer 14) The buffer layer 14 is disposed on the photoelectric conversion layer 13. The buffer layer 14 is, for example, an n-type or i (intrinsic)-type high-resistance conductive layer. Here, "high resistance" means having a resistance value higher than the resistance value of the second electrode layer 15 described later.

[0034] The buffer layer 14 can be selected from compounds containing zinc (Zn), cadmium (Cd), and indium (In). Examples of compounds containing zinc include ZnO, ZnS, Zn(OH)2, or mixed crystals thereof such as Zn(O,S) and Zn(O,S,OH), as well as ZnMgO and ZnSnO. Examples of compounds containing cadmium include CdS, CdO, or mixed crystals thereof such as Cd(O,S) and Cd(O,S,OH). Examples of compounds containing indium include InS, InO, or mixed crystals thereof such as In(O,S) and In(O,S,OH), as well as In2O3, In2S3, and In(OH). x etc. can be used. The buffer layer 14 may have a laminated structure of these compounds. The thickness of the buffer layer 14 is set to 10 nm to 100 nm.

[0035] Here, Zn(O,S) xThe lattice constant of ZnO ranges from 4.28 Å (ZnO) to 5.41 Å (ZnS), depending on the ratio of O and S. The lattice constant of CdS is 5.82 Å. On the other hand, the lattice constants of the photoelectric conversion layer 13 are as follows. For Cu(Ga,In)(Se,S)2, it is 5.36 Å (CuGaS2) to 5.78 Å (CuInSe2) depending on the ratio of Ga, In, Se, and S. For Ag(Ga,In)(Se,S)2, it is 5.74 Å (AgGaS2) to 6.09 Å (AgInSe2) depending on the ratio of Ga, In, Se, and S. When Ag is added to Cu(Ga,In)(Se,S)2 as in this embodiment, the lattice constant increases.

[0036] Therefore, in particular, the buffer layer 14 is preferably made of Zn(O,S). x In this case, the greater the amount of Ag, the greater the difference (lattice mismatch) in the lattice constants between the photoelectric conversion layer 13 and the buffer layer 14. Therefore, the smaller the molar amount of Ag contained in the region of the photoelectric conversion layer 13 on the buffer layer 14 side (i.e., the surface side region 13A of the photoelectric conversion layer 13) and the smaller the Ag concentration at the outermost surface of the photoelectric conversion layer 13 on the buffer layer 14 side (the outermost surface of the surface side region 13A), the better. On the other hand, when the buffer layer 14 is made of CdS, the lattice constant of Cu(Ga,In)(Se,S) 2 containing Ag approaches the lattice constant of the buffer layer 14 by the addition of Ag.

[0037] The buffer layer 14 has the effect of improving characteristics such as photoelectric conversion efficiency, but it can be omitted. When the buffer layer 14 is omitted, the second electrode layer 15 described later is disposed on the photoelectric conversion layer 13.

[0038] (Second electrode layer 15) The second electrode layer 15 is disposed on the buffer layer 14. The second electrode layer 15 is, for example, an n-type conductive layer. The second electrode layer 15 preferably comprises, for example, a material with a wide band gap and a sufficiently low resistance value. In addition, since the second electrode layer 15 serves as a passageway for light such as sunlight, it is preferable that the second electrode layer 15 has a property of transmitting light of a wavelength that can be absorbed by the photoelectric conversion layer 13. In this sense, the second electrode layer 15 is called a transparent electrode layer or a window layer.

[0039] The second electrode layer 15 includes, for example, a metal oxide to which a group III element (B, Al, Ga, or In) is added as a dopant. Examples of the metal oxide include ZnO and SnO2. The second electrode layer 15 can be selected from, for example, ITO (indium tin oxide), ITiO (indium titanium oxide), IZO (indium zinc oxide), ZTO (zinc tin oxide), FTO (fluorine doped tin oxide), GZO (gallium doped zinc oxide), etc. The thickness of the second electrode layer 15 is set to 0.5 μm to 2.5 μm.

[0040] <Method of manufacturing photoelectric conversion element> Next, an example of a method for manufacturing the photoelectric conversion element 10 shown in FIG. 1 will be described.

[0041] (Formation of the First Electrode Layer 12) 3, a first electrode layer 12 is formed on a substrate 11 by, for example, a sputtering method. The sputtering method may be a direct current (DC) sputtering method or a radio frequency (RF) sputtering method. Alternatively, the first electrode layer 12 may be formed by using a chemical vapor deposition (CVD) method, an atomic layer deposition (ALD) method, or the like instead of the sputtering method.

[0042] (Formation of precursor layer 13p) Next, a precursor layer 13p containing a group I element and a group III element is formed on the first electrode layer 12 (see FIG. 3). The precursor layer 13p can be formed, for example, by the sputtering method, the vapor deposition method, or the ink coating method. The vapor deposition method is a method of forming a film using atoms or the like that are vaporized by heating a vapor deposition source. The ink coating method is a method of dispersing a powder of the precursor film material in a solvent such as an organic solvent and coating the powder on the first electrode layer 12, and then evaporating the solvent to form the precursor layer 13p.

[0043] In this embodiment, the precursor layer 13p contains Ag. The group I elements other than Ag contained in the precursor layer 13p can be selected from copper, gold, etc., and the group III elements contained in the precursor layer 13p can be selected from indium, gallium, aluminum, etc. The precursor layer 13p may also contain an alkali metal such as Li, Na, K, Rb, or Cs. The precursor layer 13p may also contain tellurium (Te) as a group VI element in addition to selenium and sulfur.

[0044] The precursor layer 13p has three regions in the thickness direction (the vertical direction in the drawing): a front side region 13pA, an intermediate region 13pB, and a rear side region 13pC. The front side region 13pA, the intermediate region 13pB, and the rear side region 13pC in the precursor layer 13p can be obtained by stacking films formed by the above-mentioned sputtering method or deposition method. Among the three regions of the precursor layer 13p, the layer containing the largest amount of Ag exists in the intermediate region 13pB.

[0045] A method for forming a layer containing Ag in the precursor layer 13p includes, for example, using a sputtering source or a deposition source containing Ag (an Ag target or an Ag deposition source) to form a thin film (layer) by a sputtering method or a deposition method.

[0046] When the precursor layer 13p is formed by a sputtering method using multiple sputtering sources, a sputtering source containing Ag (such as an Ag target) and a sputtering source not containing Ag can be combined to form a region containing Ag at a desired position in the precursor layer 13p. Similarly, when the precursor layer 13p is formed by a deposition method using multiple deposition sources, a deposition source containing Ag (such as an Ag deposition source) and a deposition source not containing Ag can be combined to form a region containing Ag at a desired position in the precursor layer 13p. When the precursor layer 13p is formed using multiple sputtering sources or multiple deposition sources, the molar amount of Ag in the precursor layer 13p can be adjusted by the film amount (molar amount) ratio of the layer containing Ag to the layer not containing Ag and / or the amount of Ag added to the sputtering source or deposition source containing Ag.

[0047] As a specific method for disposing the layer containing the most Ag in the intermediate region 13pB of the precursor layer 13p, the following method may be mentioned. For example, when the precursor layer 13p is configured as a laminated film of Cu, Ga, and In in that order from the substrate 11 side, a layer containing the most Ag may be disposed between Cu and Ga or between Ga and In. When the precursor layer 13p is configured as a laminated film of Cu-Ga and In in that order from the substrate 11 side, a layer containing the most Ag may be disposed between Cu-Ga and In. Note that a Cu-Ga layer not containing Ag may be further included between the Cu-Ga layer containing Ag and the In layer.

[0048] Furthermore, the layer containing the most Ag in precursor layer 13p is not disposed on the outer surface of precursor layer 13p located at the top in FIG. 3, nor is it disposed at the boundary surface between first electrode layer 12 and precursor layer 13p. As a result, when the precursor layer 13p is chalcogenized to form the photoelectric conversion layer 13, the intermediate region 13B of the photoelectric conversion layer 13 includes a portion exhibiting a maximum value of Ag concentration. Therefore, in the photoelectric conversion layer 13 after chalcogenization, the Ag concentration in the intermediate region 13B can be made higher than that in the front side region 13A and the back side region 13C. In other words, in the photoelectric conversion layer 13 after chalcogenization, the Ag concentration in both the front side region 13A and the back side region 13C is lower than that in the intermediate region 13B.

[0049] Moreover, when the film amount (molar amount) of precursor layer 13p is divided into two regions, a light-receiving surface region and a back surface region, it is preferable that the molar amount of Ag contained in the light-receiving surface region is greater. As a result, when photoelectric conversion layer 13 after chalcogenization is divided into two regions, a light-receiving surface region and a back surface region, a portion of photoelectric conversion layer 13 showing a maximum value of Ag concentration is contained in the light-receiving surface region. Similarly, when the film amount of the intermediate region 13pB of the precursor layer 13p is divided into two regions on the light-receiving surface side and the back surface side, it is preferable that the molar amount of Ag contained in the region on the light-receiving surface side is larger. As a result, when the intermediate region 13B of the photoelectric conversion layer 13 after chalcogenization is divided into two regions on the light-receiving surface side and the back surface side, the part showing the maximum value of the Ag concentration in the intermediate region 13B is contained in the region on the light-receiving surface side.

[0050] In the entire precursor layer 13p, the molar ratio of Cu to group III elements (Cu / III) is lower than 1.0. From the viewpoint of further increasing the efficiency of photoelectric conversion, the above Cu / III is preferably in the range of 0.86 to 0.98, and more preferably in the range of 0.91 to 0.96.

[0051] (Chalcogenization treatment of precursor layer 13p) Next, the precursor layer 13p is heat-treated in an atmosphere containing a Group VI element to convert it into chalcogen, thereby forming the photoelectric conversion layer 13. First, as shown in Fig. 4, selenization is performed by, for example, a gas phase selenization method. Selenization is performed by heating the precursor layer 13p in an atmosphere of a selenium source gas (for example, hydrogen selenide or selenium vapor) 16 containing selenium as a group VI element source. Although not particularly limited, selenization is preferably performed at a temperature in the range of 300°C to 600°C in a heating furnace.

[0052] As a result, the precursor layer 13p is converted into a compound (photoelectric conversion layer 13) containing a Group I element, a Group III element, and selenium. The compound containing a group I element, a group III element, and selenium (photoelectric conversion layer 13) may be formed by a method other than the gas-phase selenization method. For example, such a compound can be formed by a solid-phase selenization method, a vapor deposition method, an ink application method, an electrodeposition method, or the like.

[0053] Next, as shown in Fig. 5, the photoelectric conversion layer 13 containing a group I element, a group III element, and selenium is sulfurized. The sulfurization is performed by heating the photoelectric conversion layer 13 in an atmosphere of a sulfur-containing sulfur source gas (e.g., hydrogen sulfide or sulfur vapor) 17. As a result, the photoelectric conversion layer 13 is converted into a compound containing a group I element, a group III element, and selenium and sulfur as group VI elements. The sulfur source gas 17 serves to replace selenium with sulfur in crystals, such as chalcopyrite crystals, made of a group I element, a group III element, and selenium on the surface of the photoelectric conversion layer 13. Although there is no particular limitation, the sulfurization is preferably carried out at a temperature within the range of 450° C. to 650° C. in a heating furnace, for example.

[0054] In this way, by selenizing and sulfurizing the precursor layer 13p, the concentration profile of Ga and S in the formed photoelectric conversion layer 13 results in a double-graded structure in which the minimum value of the band gap is shifted toward the inside in the thickness direction of the photoelectric conversion layer. The photoelectric conversion layer 13 has, in order from the light receiving surface side, a front side region 13A, an intermediate region 13B, and a back side region 13C. The portion of the photoelectric conversion layer 13 showing the minimum value of the band gap and the portion of the photoelectric conversion layer 13 showing the maximum value of the Ag concentration are both included in the intermediate region 13B.

[0055] (Formation of Buffer Layer 14 and Second Electrode Layer 15) As shown in Fig. 6, a buffer layer 14 is formed on a photoelectric conversion layer 13 by a method such as a CBD (chemical bath deposition) method or a sputtering method. Then, a second electrode layer 15, indicated by a dashed line in Fig. 6, is formed on the buffer layer 14 by a method such as a sputtering method, a CVD method or an ALD method. Note that the buffer layer 14 may be omitted and the second electrode layer 15 may be formed directly on the photoelectric conversion layer 13. Through the above steps, the photoelectric conversion element 10 shown in FIG. 1 is completed.

[0056] <Example> Examples of the photoelectric conversion element of the present invention will now be described.

[0057] (Elemental concentration composition and band gap of the photoelectric conversion layer) Fig. 7(A) shows the profile of the band gap (Eg) of the photoelectric conversion layer in the photoelectric conversion element of the embodiment. Fig. 7(B) and Fig. 7(C) show the profile of the element concentration composition ratio of the photoelectric conversion layer in the photoelectric conversion element of the embodiment. The band gap in Fig. 7(A) is calculated from the element concentration composition of the photoelectric conversion layer.

[0058] In each graph in Fig. 7, the horizontal axis indicates the normalized film thickness of the photoelectric conversion layer, with 0 corresponding to the interface on the light receiving surface side (the surface of the photoelectric conversion layer) and 1.0 corresponding to the interface on the substrate side (the back surface of the photoelectric conversion layer). The vertical axis in Fig. 7(A) indicates the band gap (Eg). The vertical axis of FIG. 7(B) indicates the molar ratio of Ga to group III elements (Ga / III) for the dashed line profile, and the vertical axis of FIG. 7(B) indicates the molar ratio of Ga to group III elements (Ga / III) for the solid line profile. VI The molar ratio of group elements (S / VI) is shown. The vertical axis of FIG. 7(C) indicates the molar ratio of group I elements other than Ag to group III elements (I other than Ag / III, for example, Cu / III) for the dashed profile (see the vertical axis on the right side of FIG. 7(C)). Also, the vertical axis of FIG. 7(C) indicates the Ag concentration (Ag / I+III+other than Ag) for the solid profile. VI ) (see the vertical axis on the left side of Figure 7(C)).

[0059] As shown by the solid line in Fig. 7(B), the S / VI profile of the photoelectric conversion layer in the thickness direction shows a high value on the front side. Similarly, as shown by the dashed line in Fig. 7(B), the Ga / III profile of the photoelectric conversion layer in the thickness direction shows a shape in which the value increases from the front side to the back side. Due to the increase in S / VI on the front side of the photoelectric conversion layer and the increase in Ga / III on the back side, the band gap profile of the photoelectric conversion layer shown in Fig. 7(A) has a downwardly convex shape. In other words, the above band gap profile shows a double-graded structure in which the values ​​are large on the front side and back side and small between them, and as shown in Fig. 7(A), the band gap has a minimum value at a position near the film thickness of 0.2 from the front side.

[0060] As shown by the dashed line in Fig. 7(C), the Cu / III (I / III other than Ag) profile of the photoelectric conversion layer in the thickness direction has a shape in which the value increases from the back side to the front side. The Cu / III value shown by the dashed line in Fig. 7(C) exceeds 1 in the region from the front side to a film thickness of 0.18 or less. The average Ag concentration (Ag / (I+III+VI other than Ag)) in the photoelectric conversion layer is 0.0062. This average Ag concentration is the average value obtained by integrating the Ag concentration in the thickness direction of the photoelectric conversion layer. As shown by the solid line in FIG. 7(C), the maximum value of the Ag concentration is 0.0091, which is within the film thickness range of 0.3 to 0.4.

[0061] (Ag content in each region of the photoelectric conversion layer) Next, with reference to Table 1, the molar amount of Ag (Ag amount) in each region in the photoelectric conversion layer of the example will be described. Table 1 shows the ratio of the amount of Ag contained in each region to the total amount when the film thickness range of the intermediate region is changed, when the photoelectric conversion layer of the photoelectric conversion element is divided into a front side region, an intermediate region, and a rear side region in that order from the light receiving surface side. Note that the film thickness range in Table 1 is shown as a normalized film thickness, with 0 corresponding to the interface on the light receiving surface side (the front side of the photoelectric conversion layer) and 1.0 corresponding to the interface on the substrate side (the rear side of the photoelectric conversion layer).

[0062] [Table 1]

[0063] For example, when the intermediate region of the photoelectric conversion layer is the region of 0.1 to 0.7 thickness from the surface side of the photoelectric conversion layer, the amount of Ag contained in the intermediate region is 75%, the amount of Ag contained in the surface side region is 6%, and the amount of Ag contained in the back side region is 19% (see Table 1(c)). Note that the portion showing the minimum value of the band gap of the photoelectric conversion layer and the portion showing the maximum value of the Ag concentration are both present in the intermediate region.

[0064] Table 1(f) shows that the thickness of the front side region where the Ag content is 15% or less is in the range of 0.18 or less from the front side, and Tables 1(d) and 1(e) show that the thickness of the back side region where the Ag content is 30% or less is in the range of 0.6 or more from the front side. In addition, in any of the intermediate region settings shown in Tables 1(a) to (g), the position in the film thickness direction of the portion showing the maximum value of the Ag concentration is located on the back side of the position in the film thickness direction of the portion showing the minimum value of the band gap of the photoelectric conversion layer.

[0065] (Photoelectric conversion element characteristics with and without Ag addition) Next, referring to Table 2, the difference in the characteristics of the photoelectric conversion element depending on whether Ag is added to the photoelectric conversion layer will be described. The examples correspond to the photoelectric conversion element with Ag added, and the comparative examples correspond to the photoelectric conversion element without Ag added. The characteristic values ​​of the examples in Table 2 are shown normalized based on the characteristic values ​​of the comparative examples. Here, Eff is the photoelectric conversion efficiency, Voc is the open circuit voltage, Isc is the short circuit current, and FF is the fill factor.

[0066] [Table 2]

[0067] The average Ag concentration of the photoelectric conversion layer in the examples is 0.00655. In the examples, the addition of Ag reduces V oc Improved (V ocIn the embodiment, the recombination of carriers generated in the surface region and the intermediate region of the photoelectric conversion layer was suppressed, and the V oc This is believed to have led to improvements in performance and FF.

[0068] Next, with reference to Table 3, the change in photoelectric conversion efficiency depending on the amount of Ag added to the photoelectric conversion layer will be described. Table 3 compares the average and maximum values ​​of Ag concentration (Ag / (I+III+VI other than Ag)) and Eff values ​​for a comparative example corresponding to a photoelectric conversion element without added Ag and a photoelectric conversion element with added Ag. In Table 3, the values ​​for the comparative examples are shown in the leftmost column of the table. The Eff values ​​are normalized with respect to the comparative example with no added Ag. In addition, the average and maximum values ​​of the Ag concentration are both zero in the comparative examples because no Ag is added.

[0069] [Table 3]

[0070] As shown in Table 3, the average Ag concentration was 0.00355 ~ 0.00961 and when the maximum value of the Ag concentration was in the range of 0.00519 to 0.00140, an improvement in the conversion efficiency of the photoelectric conversion element was observed.

[0071] (Quantum efficiency of photoelectric conversion layer and wavelength dependence of change in quantum efficiency) Fig. 8 is a graph showing the quantum efficiency of a photoelectric conversion element with Ag added to the photoelectric conversion layer, and the wavelength dependency of the change in quantum efficiency. The solid line in the figure shows the quantum efficiency (EQE) curve, and the dashed line in the figure shows the quantum efficiency derivative (d(EQE) / dλ) curve with respect to the wavelength derivative, showing the wavelength dependency of the change in quantum efficiency.

[0072] In the long wavelength region of quantum efficiency, the energy of the wavelength at which the rate of change of quantum efficiency with respect to wavelength is the maximum was defined as the band gap (Eg) of the photoelectric conversion layer. The Eg of the photoelectric conversion layer with Ag added was not substantially different from the Eg of the photoelectric conversion layer without Ag added.

[0073] (Eg and V with and without Ag addition) oc Changes in correlation of losses FIG. 9 is a graph showing the change in correlation between the band gap and the open circuit voltage loss depending on whether or not Ag is added. The horizontal axis of FIG. 9 indicates the band gap (Eg) of the photoelectric conversion layer of the photoelectric conversion element. The vertical axis of FIG. 9 indicates the relationship between Eg and the V oc V is calculated from the difference oc 9, the output result based on the photoelectric conversion layer of the comparative example to which Ag is not added is indicated by "Ref. (●)", and the output result based on the photoelectric conversion layer of the embodiment to which Ag is added is indicated by "Ag-incorporated (◇)".

[0074] As for the Ref. in Figure 9, as Eg of the photoelectric conversion layer increases, V oc The loss is also large. The V of Ref. oc The distribution of losses is V oc = 650mV line. In other words, even if Eg of the photoelectric conversion layer increases, V oc It can be seen that there is no significant improvement in On the other hand, in the photoelectric conversion layer of the embodiment in which Ag was added, as Eg of the photoelectric conversion layer increases, V oc The loss will also be large, but V oc The increase in loss tends to be generally smaller than the increase in Eg of the photoelectric conversion layer. In other words, in the photoelectric conversion layer of the embodiment in which Ag was added, the larger the Eg of the photoelectric conversion layer, the smaller the V oc It is seen that the improvement

[0075] For a specific Eg of the photoelectric conversion layer, V oc Low loss (V ocSpecifically, the larger the Ag added to the photoelectric conversion layer, the better the characteristics of the photoelectric conversion element. Cu It is believed that this can suppress the increase in carrier density in the photoelectric conversion layer and the recombination of carriers generated in the photoelectric conversion element, thereby reducing the increase in carrier density in the photoelectric conversion layer and the recombination of carriers generated in the photoelectric conversion element. In particular, it is believed that suppressing the recombination of carriers in the vicinity of the portion showing the minimum value of the band gap of the photoelectric conversion layer leads to an improvement in the open circuit voltage and short circuit photocurrent of the photoelectric conversion element. In addition, since the amount of Ag added to the surface side region of the photoelectric conversion layer is small, it is believed that the expansion of the lattice mismatch at the interface between the photoelectric conversion layer and the buffer layer due to the addition of Ag can be suppressed, and the increase in carrier recombination can be suppressed.

[0076] The above effects were obtained by adding Ag to the photoelectric conversion layer of the photoelectric conversion element when the Eg of the photoelectric conversion layer was in the range of 1.04 eV to 1.15 eV. Effects thought to be the above effects were also obtained when the Eg of the photoelectric conversion layer was in the range of more than 1.15 eV to 1.20 eV (no Reference data). In the experiment of Figure 9, the Eg of the photoelectric conversion layer was adjusted by the formation conditions of the photoelectric conversion layer (temperature, gas concentration, etc.). The change in Eg of the photoelectric conversion layer is due to the change in the amount of Ga in the intermediate region. In cases where the Eg of the photoelectric conversion layer was large, the amount of Ga in the intermediate region increased.

[0077] In addition, the larger the Eg of the photoelectric conversion layer, the greater the V oc Loss Reduction (V oc This is because the Ga content in the photoelectric conversion layer is high, and the antisite defect Ga Cu As a result, in the photovoltaic layer with a relatively large amount of Ga, the antisite defect Ga Cu It is believed that this has had a significant effect in suppressing the increase in

[0078] (Example of photoelectric conversion layer manufacturing) Next, an example of manufacturing the photoelectric conversion layer will be described. In the manufacturing example, a first electrode layer containing molybdenum was formed on a substrate, which was a glass plate, by sputtering. Next, a sputtering target of Cu-Ga, In was sputtered to form a precursor on the first electrode layer.

[0079] In the manufacturing example, Cu-Ga targets that did not contain Ag and those that contained Ag were prepared, and these were combined to form a Cu-Ga layer that did not contain Ag and a Cu-Ga layer that contained Ag. A Cu-Ga target that did not contain Ag was used for the first layer of the precursor (the layer that included the first surface on the first electrode layer side). A Cu-Ga target that contained Ag was used for the subsequent Cu-Ga layers. An In layer was formed on the multiple Cu-Ga layers.

[0080] In the manufacturing example of this embodiment, a Cu-Ga layer containing Ag is a precursor sandwiched between a Cu-Ga layer not containing Ag and an In layer. That is, the precursor includes a layer containing at least Cu, a layer containing at least one of In and Ga, and a layer containing Ag. The precursor also has a first surface on the first electrode layer side and a second surface on the second electrode layer side, and the layer containing Ag is between the layer including the first surface and the layer including the second surface of the precursor.

[0081] In the manufacturing example, the precursor has a Cu / (In+Ga) ratio of 0.94. The ratio of the number of atoms of Cu to the number of atoms of group III elements (Cu / III) in the entire precursor is lower than 1.0. The precursor was then chalcogenized to form a photoelectric conversion layer, followed by forming a buffer layer and a second electrode layer.

[0082] Table 4 shows the characteristics of the photoelectric conversion element depending on the difference in the stacking structure of the precursor of the photoelectric conversion element. The precursor structure in the manufacturing example is as follows. Example 1: Cu-Ga / Cu-Ga (Ag added) / In from the first electrode layer side Example 2: Cu-Ga / Cu-Ga (Ag added) / Cu-Ga / In from the first electrode layer side Comparative Example: Cu-Ga / In from the first electrode layer side

[0083] [Table 4]

[0084] In Table 4, the characteristic values ​​of Examples 1 and 2 are normalized based on the characteristic values ​​of the Comparative Example in which Ag was not added. The average Ag concentration in Examples 1 and 2 is 0.00655. Note that Eff, Voc, Isc, and FF in Table 4 are the same as those in Table 2, Rs is the series resistance, and Rsh is the parallel resistance.

[0085] When the molar amount (number of atoms) of the precursor element is divided into two equal parts in the film thickness direction, the region on the first electrode layer side is defined as the first region, and the region on the second electrode layer side (light receiving surface side) is defined as the second region, the amount of Ag in the second region was greater than the amount of Ag in the first region in Example 1. In Example 2, the amount of Ag in the second region was less than the amount of Ag in the first region.

[0086] In Example 1 shown in Table 4, V oc Improved (V oc In particular, the recombination of carriers generated in the surface and intermediate regions of the photoelectric conversion layer was suppressed, and V oc This is believed to have led to improvements in performance and FF.

[0087] <Applications of photoelectric conversion elements> FIG. 10 shows an example of a solar cell submodule as an application example of the photoelectric conversion element of the present invention. 10 has a so-called integrated structure. That is, the solar cell submodule 100 includes a plurality of photoelectric conversion elements 10-1, 10-2, ... 10-k connected in series, where k is a natural number of 2 or more.

[0088] The substrate 11 is common to the multiple photoelectric conversion elements 10-1, 10-2, ... 10-k. The substrate 11 is, for example, a flexible substrate having a laminated structure of stainless steel (SUS), aluminum, and aluminum oxide. An insulating layer 21 is formed on the substrate 11. The insulating layer 21 is, for example, a coating of aluminum oxide, glass frit, or the like.

[0089] A plurality of first electrode layers 12-1, 12-2, . . . 12-k, 12-(k+1) are arranged side by side on the insulating layer 21 of the substrate 11. Each of the photoelectric conversion elements 10-1, 10-2, ..., 10-k has a photoelectric conversion layer 13 and a buffer layer 14. The photoelectric conversion layer 13 and the buffer layer 14 correspond to the photoelectric conversion layer 13 and the buffer layer 14 of the photoelectric conversion element 10 shown in FIG.

[0090] In each of the photoelectric conversion elements 10-1, 10-2, ..., 10-k, the second electrode layer 15 is connected to one of the multiple first electrode layers 12-1, 12-2, ..., 12-k. For example, the second electrode layer 15 of the photoelectric conversion element 10-1 is connected to the first electrode layer 12-2 of the photoelectric conversion element 10-2 located adjacent thereto. The same is true for the remaining photoelectric conversion elements 10-2, ..., 10-k. As a result, the multiple photoelectric conversion elements 10-1, 10-2, ..., 10-k are connected in series with each other.

[0091] The first electrode layer 12-1 is connected to, for example, a positive electrode 18, and the first electrode layer 12-(k+1) is connected to, for example, a negative electrode 19.

[0092] Here, in the solar cell submodule 100, in order to eliminate initial insulation defects in the insulating layer 21, a test is performed in the manufacturing process after the formation of the photoelectric conversion element 10 in which a voltage is applied between the conductive substrate 11 and the first electrode layer 12. The voltage is applied by increasing it from 0 V, and the upper limit voltage is, for example, several hundred V. The upper limit voltage is appropriately adjusted depending on the film thickness of the insulating layer 21 and the number of photoelectric conversion elements connected in series.

[0093] If there is an initial insulation defect, applying a voltage between the substrate 11 and the first electrode layer 12 will cause electricity to flow. In the above test of the solar cell submodule 100, the voltage is increased from 0 V until an open state is reached. Once the open state is reached, the resistance between the substrate 11 and the first electrode layer is measured. If the measured resistance is equal to or greater than a specified value (for example, equal to or greater than 1 MΩ), the solar cell submodule 100 is treated as having passed the test.

[0094] According to the solar cell submodule 100 described above, when a plurality of photoelectric conversion elements 10-1, 10-2, ... 10-k are made into one unit, the plurality of units can be connected in parallel between the positive electrode 18 and the negative electrode 19. Moreover, these plurality of units can be formed on one substrate 11. For example, a solar cell panel using such a solar cell submodule 100 only experiences a limited decrease in the amount of power generated even when it is partially shaded. Therefore, a solar cell panel that generates power stably can be realized.

[0095] <Conclusion> Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the present invention. These embodiments can be implemented in various forms other than those described above, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the present invention. These embodiments and their modifications are included in the scope and spirit of the present invention, and the inventions described in the claims and their equivalents are also included in the scope and spirit of the present invention.

[0096] This application also claims priority based on Japanese Patent Application No. 2018-237248, filed on December 19, 2018, the entire contents of which are incorporated herein by reference. [Explanation of symbols]

[0097] 10 Photoelectric conversion element 11 Substrate 12 First electrode layer 13 Photoelectric conversion layer 13A Surface side area 13B Intermediate area 13C Back area 13p precursor layer 14 Buffer layer 15 Second electrode layer 16 Selenium Source Gas 17 Sulfur source gas 18 positive electrode 19 Negative electrode 21 Insulating layer 100 Solar cell submodules

Claims

1. A photoelectric conversion element having a photoelectric conversion layer formed between a first electrode layer and a second electrode layer, The photoelectric conversion layer contains group I elements Cu and Ag, group III elements In and Ga, and group VI elements Se and S, the photoelectric conversion layer has a front side region located on the light receiving surface side, a back side region located on the back side of the light receiving surface, and an intermediate region located between the front side region and the back side region, a light receiving surface side of the intermediate region faces the front side region, and a back side of the intermediate region faces the back side region; the intermediate region is located in a range of 0.1 to 0.7 in a thickness direction of the photoelectric conversion layer with respect to a light receiving surface of the photoelectric conversion layer when the thickness of the photoelectric conversion layer is normalized to 1, the front surface side region, the intermediate region, and the back surface side region each contain Ag, a portion exhibiting a minimum band gap in a thickness direction of the photoelectric conversion layer is included in the intermediate region, When the ratio of the molar amount of Ag to the sum of the molar amounts of group I elements, group III elements, and group VI elements other than Ag (Ag / (I other than Ag+III+VI)) is defined as the Ag concentration, a portion showing a maximum value of the Ag concentration in the thickness direction of the photoelectric conversion layer is included in the intermediate region, The molar amount of Ag contained in the back surface side region is 0.19 or less of the molar amount of Ag contained in the entire photoelectric conversion layer. Photoelectric conversion element.

2. The maximum value of the Ag concentration is 0.00519 to 0.0140. The photoelectric conversion element according to claim 1 .

3. the portion exhibiting the maximum value of the Ag concentration is located closer to the light receiving surface of the photoelectric conversion layer than to the back surface of the photoelectric conversion layer in a thickness direction of the photoelectric conversion layer; The photoelectric conversion element according to claim 1 or 2.

4. the portion exhibiting the maximum value of the Ag concentration is located, in a thickness direction of the photoelectric conversion layer, closer to a boundary of the intermediate region on a light receiving surface side than to a boundary of the intermediate region on a back surface side; The photoelectric conversion element according to claim 1 .

5. the portion showing the maximum value of the Ag concentration is located on the back surface side of the photoelectric conversion layer relative to the portion showing the minimum value of the band gap in the thickness direction of the photoelectric conversion layer; The photoelectric conversion element according to claim 1 .

6. the molar amount of Ag contained in the surface-side region is 0.06 or less of the molar amount of Ag contained in the entire photoelectric conversion layer; The photoelectric conversion element according to claim 1 .

7. The band gap of the photoelectric conversion layer is 1.04 eV to 1.20 eV. The photoelectric conversion element according to claim 1 .

8. A method for producing the photoelectric conversion element according to any one of claims 1 to 7, comprising the steps of: forming the first electrode layer; forming a precursor layer containing group I elements Cu and Ag and group III elements In and Ga on the first electrode layer; chalcogenizing the precursor layer to form the photoelectric conversion layer; forming the second electrode layer on the photoelectric conversion layer; In the step of forming the precursor layer, a layer containing at least Cu, a layer containing at least one of In and Ga, and a layer containing Ag are formed, the layer including Ag in the precursor layer is formed between a layer including a first surface on the first electrode layer side and a layer including a second surface on the second electrode layer side, The layer containing Ag contains more Ag than the layer containing at least Cu and the layer containing at least one of In and Ga. A method for manufacturing a photoelectric conversion element.

9. a first region is a region on the first electrode side and a second region is a region on the light receiving surface side of the precursor layer, the second region being a region obtained by dividing the molar amount of an element of the precursor layer into two equal regions in a thickness direction, the second region having a larger molar amount of Ag than the first region; The method for producing the photoelectric conversion element according to claim 8 .

Citation Information

Patent Citations

  • Solar cell

    JP2014232764A

  • Multi-order IB and VIA family semiconductors

    JP2014524145A

  • Method for forming acigs thin film at low-temperature and method for manufacturing solar cell using the same

    JP2017128792A

  • Method for manufacturing a compound film

    US20100247745A1

  • Multi-nary group IB and via based semiconductor

    US20120168910A1