Packaging paper
A polyvinylidene chloride polymer-based heat-resistant layer in packaging paper addresses the challenge of plastic waste by providing microwave-safe, easily recyclable packaging with reduced plastic content.
Patent Information
- Application Number
- JP2021149461
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-09-14
AI Technical Summary
Existing packaging papers, especially those used for microwave ovens, still contain significant amounts of plastic laminates like polypropylene, which are difficult to decompose and contribute to plastic waste, and there is a need for a solution that reduces plastic use while maintaining heat resistance and ease of collection as waste paper.
A packaging paper with a heat-resistant layer made of polyvinylidene chloride polymer, applied in multiple layers to achieve a density of 1.6 to 2.0 g/cm³, which provides heat resistance equivalent to conventional polypropylene films and allows easy disintegration for waste collection, using a water-based emulsion to minimize environmental impact.
The packaging paper achieves heat resistance suitable for microwave use and can be easily recycled, reducing plastic waste by minimizing polypropylene use and ensuring effective disintegration for waste recovery.
Smart Images

Figure 0007569295000001
Abstract
Description
[Technical field]
[0001] The present invention relates to wrapping paper, and in particular to wrapping paper for microwave ovens. [Background technology]
[0002] In recent years, the problem of plastic waste has become more serious. It is said that the world's plastic production exceeds 400 million tons per year, and a large amount of plastic is produced in the packaging container sector, which is one of the major causes of plastic waste. Plastic does not decompose for a long time, and the waste turns into microplastics in the natural environment, causing serious adverse effects on the ecosystem. The most commonly used plastics for packaging containers are polyethylene terephthalate (PET), which is used for beverage bottles, and polyethylene (PE) and polypropylene (PP), which are used for plastic bags and container lamination. In particular, marine pollution by plastic waste is severe, and it is said that the plastic waste cannot be recovered. In the future, it will be necessary for the global environment to reduce the use of plastic.
[0003] On the other hand, the use of biodegradable plastics that can be completely decomposed by microorganisms has been proposed around the world as a measure against plastic waste. Biodegradable plastics decompose in nature within a certain period of time, but until they decompose they are still waste, and unless their usage and disposal amounts are reduced, this cannot be said to be an immediate solution (see Patent Documents 1 and 2).
[0004] As an immediate solution, it has been proposed to replace plastic with paper. However, when processing paper into bags or containers, a large amount of plastic such as polyethylene or polypropylene is laminated as a barrier layer. The amount of plastic laminate varies depending on the product concept, but is generally 20 to 50 g / m 2 and 300 g / m 2Therefore, even in packaging containers where plastic has been replaced with paper, the amount of plastic used remains a problem, and there is an urgent need for a means to directly reduce the use of plastic.
[0005] Furthermore, heat-resistant packaging paper, particularly recent packaging paper for microwave ovens, is laminated with a large amount of polypropylene (PP) film to impart heat resistance, and is likely to become plastic waste when released into the environment by littering, etc. In addition, since it is practically impossible to separate the plastic from the paper, it cannot be recovered as waste paper, and is therefore likely to be littered. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-148444 A [Patent Document 2] JP 2013-141763 A Summary of the Invention [Problem to be solved by the invention]
[0007] In view of the above-mentioned current state of the prior art, an object of the present invention is to provide a wrapping paper that can reduce plastic waste, in particular a wrapping paper that is heat resistant, can be suitably used in a microwave oven, and can be easily collected as waste paper. [Means for solving the problem]
[0008] In the present invention, a polyvinylidene chloride polymer is used in order to reduce the amount of polypropylene laminate used in conventional heat-resistant plastic laminated paper (hereinafter sometimes abbreviated as heat-resistant polylaminated paper). That is, the packaging paper according to the present invention is a packaging paper having at least one heat-resistant layer on at least one side of a paper base material, the heat-resistant layer being made only of a polyvinylidene chloride polymer (sometimes abbreviated as PVDC), and the density of the heat-resistant layer is 1.6 to 2.0 g / cm. 3 The wrapping paper of the present invention having such a structure has heat resistance almost equivalent to that of the heat-resistant layer of conventional heat-resistant polylaminated paper, and is particularly suitable for use as wrapping paper for microwave ovens. Furthermore, the wrapping paper of the present invention is easy to disintegrate the plastic and paper, so it is easy to collect as waste paper.
[0009] In the present invention, the heat-resistant layer may be formed in two or more layers on at least one surface of the paper. By adopting such a configuration, the coating layer density is increased, and a wrapping paper having excellent heat resistance can be obtained.
[0010] The method for producing packaging paper in the present invention preferably includes a step of preparing a coating liquid for a heat-resistant layer containing a polyvinylidene chloride-based polymer emulsion, and a step of applying two or more layers of the coating liquid for a heat-resistant layer to at least one surface of a paper substrate. In particular, by using an aqueous polyvinylidene chloride-based polymer emulsion as the polyvinylidene chloride-based polymer emulsion, it is possible to control the coating amount to a relatively low level, and since there is no VOC (volatile organic compound) emission, packaging paper with a low environmental impact can be obtained. Effect of the Invention
[0011] According to the present invention, it is possible to produce heat-resistant packaging paper that can reduce plastic waste, particularly packaging paper for use in microwave ovens. Container products using the packaging paper of the present invention can be easily disintegrated and thus can be recycled as waste paper, helping to solve the plastic waste problem. The packaging paper of the present invention can be processed into general packaging containers, such as bags, cartons, cups, trays, boxes, cases, and vessels, in which food can be placed (or placed) and heated in a microwave oven. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, the present invention will be described in detail with reference to the embodiments, but the present invention is not limited to these descriptions. Various modifications of the embodiments may be made as long as the effects of the present invention are achieved.
[0013] The present invention relates to a packaging paper having at least one heat-resistant layer on at least one side of a paper substrate, the heat-resistant layer being made of only a polyvinylidene chloride polymer. In this embodiment, the polyvinylidene chloride polymer is a copolymer polymer mainly composed of vinylidene chloride monomer and one or more of various vinyl compounds (acrylonitrile, vinyl chloride, vinyl acetate, acrylic acid ester, allyl ester, styrene, etc.). In the present invention, only an emulsion of the polyvinylidene chloride polymer is coated on the paper to form a heat-resistant layer. If other resins are present in the heat-resistant layer, resins other than the polyvinylidene chloride polymer will melt, and further crystallization of the polyvinylidene chloride polymer will be inhibited, resulting in poor microwave resistance. Furthermore, if a pigment (e.g., light calcium carbonate, heavy calcium carbonate, talc, clay, kaolin clay, calcined clay, titanium dioxide, aluminum hydroxide) is added to the heat-resistant layer, crystallization of the polyvinylidene chloride polymer will be inhibited, and the density of the heat-resistant layer coating will decrease. In order to reduce the burden on the natural environment, the emulsion is preferably an aqueous emulsion. The packaging paper having the heat-resistant layer of the present invention can obtain heat resistance equivalent to that of a conventional heat-resistant layer mainly made of polypropylene film, and can be used practically without melting when heated in a microwave oven.
[0014] In this embodiment, a heat-resistant layer can be provided by applying a coating liquid for a heat-resistant layer containing a polyvinylidene chloride-based polymer emulsion to at least one surface of a paper substrate and drying the coating liquid. By using a polyvinylidene chloride-based polymer emulsion, it becomes possible to control the coating weight to a relatively low level. Furthermore, by using a water-based polyvinylidene chloride-based polymer emulsion, VOC emissions are eliminated, and the burden on the natural environment can be reduced. The coating weight of the heat-resistant layer is 3 to 30 g / m2 in terms of solid content per one surface of the paper substrate. 2 and preferably 4 to 25 g / m 2 3g / m 2 If it is less than 30 g / m, the polyvinylidene chloride emulsion is absorbed into the paper layer, reducing the density of the coating layer and making it difficult to obtain sufficient heat resistance. 2 If it exceeds this value, the quality is excessive in terms of heat resistance, the effect of reducing plastics is poor, and disintegration of paper and plastics becomes difficult. In addition, when the polyvinylidene chloride emulsion is water-based, diluting it with water to reduce the concentration too much also causes a decrease in the density of the coating layer. The solid content concentration of the water-based polyvinylidene chloride polymer emulsion is preferably 15 to 50%. Furthermore, foaming of the heat-resistant layer coating liquid causes a decrease in the density of the coating layer, so it is preferable to take measures such as using a defoamer, setting the degree of stirring appropriately, installing a strainer at the outlet of the coating liquid piping, and lining the coating liquid along the tank wall when pouring it.
[0015] It is preferable to coat the coating liquid for the heat-resistant layer in two or more layers on at least one surface. This makes it possible to further increase the density of the heat-resistant layer, and the heat-resistant layer has excellent microwave resistance. In the present invention, the density of the heat-resistant layer is 1.6 to 2.0 g / cm 3 It is necessary that the density is 1.6g / cm 3 If it is less than 2.0g / cm, the microwave resistance is poor. 3 If it exceeds this value, the heat-resistant layer becomes easily cracked during processing.
[0016] The method of applying the coating liquid for the heat-resistant layer is not particularly limited, and any commonly used coating device can be used. For example, various known coating devices such as an air knife coater, blade coater, gravure coater, rod blade coater, roll coater, reverse roll coater, bar coater, curtain coater, die slot coater, champlex coater, metering blade type size press coater, short dwell coater, spray coater, gate roll coater, and lip coater can be used. Furthermore, the coating liquid for the heat-resistant layer is generally dried after application. This allows the density of the heat-resistant layer to be in an appropriate range. When the density of the heat-resistant layer is 1.6 to 2.0 g / cm 3 If so, the drying temperature and drying time are not particularly specified, but depend on the coating weight of the heat-resistant layer. As described above, if the coating weight of the heat-resistant layer is 3 to 30 g / m2 in terms of solid content per side of the paper base material, 2 In this case, the drying temperature after coating of the heat-resistant layer coating liquid is preferably 105 to 200° C. The drying time is preferably 2 to 60 seconds. If the drying temperature is less than 105° C., the density of the heat-resistant layer decreases, and if the drying temperature exceeds 200° C., the moisture content of the paper decreases, making the heat-resistant layer more likely to crack.
[0017] The paper base material used in this embodiment is not particularly limited, and a known paper base material containing pulp as a main component can be used. As the pulp that is the main component of the paper base material, chemical pulp such as LBKP (hardwood bleached kraft pulp) and NBKP (softwood bleached kraft pulp), mechanical pulp such as GP (groundwood pulp), PGW (pressurized groundwood pulp), RMP (refiner mechanical pulp), TMP (thermo-mechanical pulp), CTMP (chemi-thermo-mechanical pulp), CMP (chemi-mechanical pulp), and CGP (chemi-ground pulp), wood pulp such as DIP (deinked pulp), and non-wood pulp such as kenaf, bagasse, bamboo, and cotton can be used. These can be used alone or mixed in any ratio. For example, 90 to 100 parts by mass of LBKP (hardwood bleached kraft pulp) can be used as the pulp. In addition, synthetic fibers can be further blended within a range that does not impair the intended effect of the present invention. From the viewpoint of environmental conservation, ECF (Elemental Chlorine Free) pulp, TCF (Total Chlorine Free) pulp, waste paper pulp, and pulp obtained from planted trees are preferred. In addition, for example, the appropriate beating degree of pulp is 200 to 700 ml CSF, for example, 450 to 620 ml CSF in Canadian Standard Freeness (JIS P 8121:1995 "Testing Method for Pulp Freeness").
[0018] The paper base material may contain a filler. Examples of the filler include light calcium carbonate, heavy calcium carbonate, talc, clay, kaolin, calcined clay, titanium dioxide, and aluminum hydroxide. The filler content in the paper base material is, for example, 1 to 30 parts by mass per 100 parts by mass of the dry mass of the pulp. For example, light calcium carbonate may be contained in an amount of 1 to 10 parts by mass per 100 parts by mass of the dry mass of the pulp.
[0019] The paper base material may contain various known papermaking additives in addition to the pulp and filler. Examples of papermaking additives include sizing agents, internal paper strength enhancers such as wet paper strength enhancers, bulk enhancers, retention improvers, drainage improvers, coloring dyes, coloring pigments, fluorescent brighteners, fluorescent decolorizers, and pitch control agents. In the present invention, for example, 0.1 to 0.5 parts of cationic starch and 0.1 to 0.5 parts of neutral rosin size may be added per 100 parts by mass of dry pulp. In addition, water-soluble polymers such as starch, polyvinyl alcohol, and polyacrylamide may be applied. For example, oxidized starch may be applied in a dry coating amount of 1 to 5 g / m2 on both sides. 2 The coating may be applied so as to achieve the above result.
[0020] The method for making the paper base material is not particularly limited, and the paper base material can be produced by various paper machines such as a Fourdrinier paper machine, a multi-layer Fourdrinier paper machine, a cylinder paper machine, a multi-layer cylinder paper machine, a multi-layer Fourdrinier cylinder combination paper machine, a twin-wire paper machine, etc. In the present invention, the paper base material may be a single layer or multi-layer paper machine, or a laminate of multiple layers.
[0021] The paper base material may have one or more pigment coating layers other than the heat-resistant layer, for example, a pigment coating layer containing a pigment and an adhesive. The pigment in the pigment coating layer may be a known pigment used in the coating layer of a general printing coated paper, for example, calcium carbonate (heavy calcium carbonate, light calcium carbonate, etc.), kaolin (including clay), calcined clay, talc, magnesium carbonate, barium sulfate, calcium sulfate, titanium dioxide, zinc oxide, zinc sulfate, zinc carbonate, calcium silicate, aluminum silicate, magnesium silicate, diatomaceous earth, aluminum hydroxide, magnesium hydroxide, and other inorganic pigments, or acrylic, styrene, vinyl chloride, nylon itself, or organic pigments obtained by copolymerizing these (so-called plastic pigments). For example, a combination of 20 to 40 parts by mass of kaolin and 60 to 80 parts by mass of heavy calcium carbonate can be used as the pigment. The adhesive may be a known adhesive used in the coating layer of a general printing coated paper, for example, starches such as butadiene-based copolymer latex, crosslinking agent modified starch, oxidized starch, enzyme modified starch, esterified starch, etherified starch, cationic starch, amphoteric starch, gelatin, casein, soy protein, water-soluble polymers such as polyvinyl alcohol, vinyl acetate, ethylene vinyl acetate, polyurethane resin, acrylic resin, polyester resin, polyamide resin, and other synthetic resins. The blending ratio of the pigment and adhesive in the pigment coating layer is not particularly limited, but it is preferable to use 5 to 50 parts by weight of adhesive per 100 parts by weight of pigment. For example, the adhesive may be a combination of 1 to 5 parts by weight of phosphate esterified starch and 5 to 15 parts by weight of styrene butadiene latex per 100 parts by weight of pigment. The pigment coating layer may contain various auxiliaries within the range that does not impair the intended effect of the present invention, such as colorants, viscosity regulators, softeners, gloss-imparting agents, water-resistant agents, dispersants, flow modifiers, UV absorbers, stabilizers, antistatic agents, crosslinking agents, sizing agents, pH regulators, defoamers, plasticizers, and preservatives. The coating amount of such a pigment coating layer is, for example, 2 to 40 g / m2 in terms of solid content per one side of the paper base material. 2In one embodiment of the packaging paper of the present invention, a heat-resistant layer may be provided on such a pigment coating layer, and in another embodiment, a heat-resistant layer may be provided on the side of a paper base having a pigment coating layer on only one side thereof, the side not having a pigment coating layer.
[0022] In this embodiment, the basis weight of the packaging paper is not particularly limited, but is, for example, 10 to 500 g / m 2 Considering the coating and processing suitability of the heat-resistant layer, the preferred range is 20 to 400 g / m 2 is preferred. EXAMPLES
[0023] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" refer to "parts by mass" and "% by mass", respectively, unless otherwise specified. The number of parts added is a value calculated as a solid content.
[0024] Example 1 (Preparation of paper substrate) A paper stock was prepared by adding 100 parts of hardwood bleached kraft pulp with a Canadian Standard Freeness of 550 mlcsf, 5 parts of light calcium carbonate (product name: TP-121, manufactured by Okutama Kogyo Co., Ltd.), 0.3 parts of cationic starch (product name: Neotack 30T, manufactured by Nippon Shokuhin Kako Co., Ltd.), and 0.4 parts of neutral rosin size (product name: CC167, manufactured by Seiko PMC Co., Ltd.) with water, and the paper stock was made into a paper with a basis weight of 248 g / m using a fourdrinier multi-cylinder papermaking machine. 2 A base paper of 2 g / m2 was prepared. Oxidized starch (product name: MS3800, manufactured by Nippon Shokuhin Kako Co., Ltd.) was applied to this base paper by a gate roll coater in a dry coating amount of 2 g / m2 on both sides. 2 Apply so that the thickness becomes 250 g / m2 and dry. 2 Thus, a paper substrate of 100 g was obtained.
[0025] (Preparation of coating liquid for pigment coating layer) 20 parts of kaolin (trade name: Contour 1500, manufactured by Imerys) and 80 parts of heavy calcium carbonate (trade name: Carbilux, manufactured by Imerys) were mixed with 0.1 parts of a dispersant (trade name: Aron T-50, manufactured by Toa Gosei Co., Ltd.), and water was added and dispersed in water using a Coles disperser to prepare a pigment slurry. 2 parts of phosphated starch (trade name: MS4600, manufactured by Nihon Shokuhin Kako Co., Ltd.) and 8 parts of styrene butadiene latex (trade name: PA0372, Nippon A&L Co., Ltd.) were added as binders to this pigment slurry, and further water was added and dispersed to prepare a coating liquid for a pigment coating layer with a solids concentration of 50%.
[0026] (Preparation of coated paper) The coating solution for the pigment coating layer was applied to both sides of the base paper obtained above, with a dry coating amount of 10 g / m per side. 2 The coated film was then dried using a blade coater so that the basis weight was 270 g / m. 2 Coated paper was prepared.
[0027] (Making wrapping paper) A water-based polyvinylidene chloride polymer emulsion (product name: L536B, manufactured by Asahi Kasei Corporation) was applied to one side of the coated paper obtained above, diluted with water to a solids concentration of 45%, and the total dry coating amount was 10 g / m 2 The mixture was coated twice using an air knife coater so that the total coating amount was 10 g / m 2 ) and dried at 130°C for 15 seconds to provide a heat-resistant layer, thereby producing packaging paper.
[0028] Example 2 In Example 1, the coating weight of the heat-resistant layer was 20 g / m 2 A wrapping paper was prepared in the same manner as in Example 1, except that the above-mentioned was used.
[0029] Example 3 In Example 1, the coating weight of the heat-resistant layer was 3 g / m 2 A wrapping paper was produced in the same manner as in Example 1, except that the above-mentioned change was made.
[0030] Example 4 In Example 1, the coating weight of the heat-resistant layer was 25 g / m 2 A wrapping paper was produced in the same manner as in Example 1, except that the above-mentioned change was made.
[0031] Example 5 (Preparation of paper substrate) A paper stock was prepared by adding 100 parts of hardwood bleached kraft pulp with a Canadian standard freeness of 580 mlcsf, 5 parts of light calcium carbonate (product name: TP-121, manufactured by Okutama Kogyo Co., Ltd.), 0.2 parts of cationic starch (product name: Neotack 30T, manufactured by Nippon Shokuhin Kako Co., Ltd.), and 0.2 parts of neutral rosin size (Size Pine NT-78: manufactured by Arakawa Chemical Industries Co., Ltd.) and water, and the paper stock was made into a paper with a basis weight of 38 g / m using a fourdrinier multi-cylinder papermaking machine. 2 A base paper of 2 g / m2 was prepared. Oxidized starch (product name: MS3800, manufactured by Nippon Shokuhin Kako Co., Ltd.) was applied to this base paper by a gate roll coater in a dry coating amount of 2 g / m2 on both sides. 2 Apply so that the thickness becomes 40 g / m2 and dry. 2 Thus, a paper substrate of 100 g was obtained.
[0032] (Making wrapping paper) A water-based polyvinylidene chloride polymer emulsion (product name: L411A, manufactured by Asahi Kasei Corporation) was diluted with water to a solids concentration of 30% on one side of the paper substrate obtained above, and the total dry coating amount was 10 g / m 2 The mixture was coated twice using an air knife coater so that the total coating amount was 10 g / m 2 ) and dried at 115°C for 25 seconds to provide a heat-resistant layer, thereby producing packaging paper.
[0033] Example 6 In Example 5, the coating weight of the heat-resistant layer was 20 g / m 2 A wrapping paper was prepared in the same manner as in Example 5, except that the above-mentioned was used.
[0034] Example 7 In Example 5, the coating weight of the heat-resistant layer was 3 g / m 2 A wrapping paper was produced in the same manner as in Example 5, except that the above-mentioned change was made.
[0035] Example 8 In Example 5, the coating weight of the heat-resistant layer was 25 g / m 2 A wrapping paper was produced in the same manner as in Example 5, except that the above-mentioned change was made.
[0036] Comparative Example 1 On one side of the paper substrate prepared in Example 5, low-density polyethylene (Tosoh Corporation, Petrothene DLZ19A) was coated at a coating amount of 30 g / m using an extrusion coater (melt extruder). 2 The laminate was then laminated to form a heat-resistant layer to prepare a wrapping paper.
[0037] Comparative Example 2 Polypropylene (Novatec FL03H, manufactured by Japan Polypropylene Corporation) was applied to one side of the paper substrate prepared in Example 5 in an amount of 30 g / m using an extrusion coater (melt extruder). 2 The laminate was then laminated to form a heat-resistant layer to prepare a wrapping paper.
[0038] Comparative Example 3 A wrapping paper was prepared in the same manner as in Example 7, except that the aqueous polyvinylidene chloride polymer emulsion was changed to an aqueous acrylic emulsion (Viniblan 2685, manufactured by Nisshin Chemical Industry Co., Ltd.).
[0039] Comparative Example 4 A packaging paper was prepared in the same manner as in Example 7, except that the heat-resistant layer coating liquid was prepared by diluting 80 parts by mass of an aqueous polyvinylidene chloride polymer emulsion (product name: L411A, manufactured by Asahi Kasei Corporation) and 20 parts of kaolin (product name: Contour 1500, manufactured by Imerys) with water to change the solids concentration to 28%.
[0040] Comparative Example 5 A wrapping paper was prepared in the same manner as in Example 7, except that the aqueous polyvinylidene chloride polymer emulsion was applied once.
[0041] Comparative Example 6 A wrapping paper was prepared in the same manner as in Example 7, except that the drying temperature when forming the heat-resistant layer was 103°C.
[0042] The wrapping papers obtained in each of the Examples and Comparative Examples were evaluated by the methods described below. The results are shown in Table 1.
[0043] (1) Microwave resistance The wrapping paper was cut into 15cm squares, a drop of commercially available salad oil was placed on the heat-resistant layer, and the paper was heated in a commercially available microwave oven at 500W for 3 minutes. After heating, the sample was removed and visually evaluated as follows. If the heat-resistant layer melts and the oil penetrates when heated in the microwave oven, the microwave resistance is poor. ◎: No salad oil has soaked in and it is usable. ○: A small amount of salad oil has soaked in, but it is still usable. △: Soaked in salad oil and not usable. ×: The salad oil has completely soaked in and penetrated to the back side, making it unusable.
[0044] (2) Coating layer density The heat-resistant layer density was determined as follows. Density (g / cm 3 ) = Coating amount (g / m 2 ) / Heat-resistant layer thickness (μm) The thickness of the heat-resistant layer was determined by averaging the cross-sectional thickness measured at 20 points using an electron microscope.
[0045] [Table 1]
[0046] As is clear from Table 1, the packaging papers of Examples 1 to 8 (coated with aqueous polyvinylidene chloride emulsion) have superior heat resistance and are suitable for use in microwave ovens compared to Comparative Examples 1, 3, 4, 5, and 6. In addition, they have the same level of heat resistance as the conventional polypropylene laminate product of Comparative Example 2. As described above, it has been made clear that the packaging paper of the present invention having a heat-resistant layer made of polyvinylidene chloride having a specific density exhibits excellent heat resistance and is suitable for use in microwave ovens.
Claims
1. A microwave oven packaging paper having two or more heat-resistant layers on at least one side of a paper base, the heat-resistant layers being made of only polyvinylidene chloride polymers, the coating amount of the heat-resistant layers being 3 to 30 g / m 2 in terms of solid content per side of the paper base, and the density of the heat-resistant layers being 1.6 to 2.0 g / cm 3 The packaging paper for microwave ovens is characterized in that
2. A packaging paper for microwave ovens as described in claim 1, characterized in that the paper base material contains a filler, and the filler content in the paper base material is 1 to 30 parts by mass per 100 parts by mass of the dry mass of the pulp.
3. A microwave packaging paper as described in claim 1 or 2, further having a pigment coating layer containing a pigment and an adhesive, characterized in that the pigment used is a combination of 20 to 40 parts by mass of kaolin and 60 to 80 parts by mass of heavy calcium carbonate.
4. A packaging paper for use in a microwave oven as described in any one of claims 1 to 3, further having a pigment coating layer containing a pigment and an adhesive, wherein the adhesive used is a combination of 1 to 5 parts by mass of phosphated starch and 5 to 15 parts by mass of styrene butadiene latex per 100 parts by mass of the pigment.
5. The packaging paper for microwave ovens according to claim 1, wherein the coating amount of the heat-resistant layer is more than 10 g / m 2 and up to 30 g / m 2 in terms of solid content per side of the paper substrate.
6. The packaging paper for microwave ovens according to claim 1, wherein the coating amount of the heat-resistant layer is 20 g / m 2 to 30 g / m 2 calculated as solid content per side of the paper substrate.
7. The method for producing a packaging paper for microwave ovens includes the steps of: preparing a coating liquid for a heat-resistant layer that contains only an emulsion of a polyvinylidene chloride polymer; and applying two or more layers of the coating liquid for a heat-resistant layer to at least one surface of a paper substrate in an amount of 3 to 30 g / m2 in terms of solid content per surface of the paper substrate, the density of the heat-resistant layer being 1.6 to 2.0 g / cm3.
8. A method for producing microwave packaging paper as described in claim 7, characterized in that the paper base material contains a filler, and the filler content in the paper base material is 1 to 30 parts by mass per 100 parts by mass of the dry mass of the pulp.
9. A method for producing packaging paper for microwave ovens as described in claim 7 or 8, comprising the steps of applying and drying a coating liquid for a pigment coating layer which contains 20 to 40 parts by mass of kaolin and 60 to 80 parts by mass of heavy calcium carbonate as pigments and which contains 1 to 5 parts by mass of phosphated starch and 5 to 15 parts by mass of styrene butadiene latex as adhesives per 100 parts by mass of pigment, and then applying two or more layers of the coating liquid for a heat-resistant layer on top of the pigment coating layer or on a surface on which the pigment coating layer is not provided.
10. A method for manufacturing microwave packaging paper as described in any one of claims 7 to 9, comprising a drying process for a drying time of 2 to 60 seconds and a drying temperature of 105 to 200°C after the process of applying two or more layers of the heat-resistant layer coating liquid.
Citation Information
Patent Citations
Packaging material
JP1995137206A
Gas barrier packaging material
JP1995285191A
Moisture-proof paper and its production
JP1999012982A
Method for treating baked cake or the like
JP2000157151A
Biodegradable laminated paper