All-solid secondary battery
By introducing an intermediate layer of specific oxides at the electrode interface in all-solid-state secondary batteries, the discharge capacity is improved, addressing the issue of electrolyte deterioration and enhancing battery performance.
Patent Information
- Application Number
- JP2021554925
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-06
- Filing Date
- 2020-10-30
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-10-30
AI Technical Summary
All-solid-state secondary batteries using low melting point solid electrolytes, such as 3LiOH·Li2SO4, exhibit lower discharge capacity than expected due to deterioration of the solid electrolyte at the electrode interface, likely caused by reactions with active materials.
Incorporating an intermediate layer made of oxides such as Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, or Mn, or their lithium composite oxides at the interface between the electrode active materials and the solid electrolyte, specifically LiOH·Li2SO4, to enhance interfacial contact and stability.
The intermediate layer improves discharge capacity and suppresses the deterioration of the solid electrolyte, leading to enhanced battery performance and capacity.
Smart Images

Figure 0007569328000006 
Figure 0007569328000007 
Figure 0007569328000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-solid-state secondary battery, and in particular to an all-solid-state lithium secondary battery. [Background technology]
[0002] In recent years, with the development of portable devices such as personal computers and mobile phones, the demand for batteries as their power sources has increased significantly. In batteries used for such purposes, a liquid electrolyte (electrolytic solution) using a flammable organic solvent as a diluting solvent has been used as a medium for moving ions. In batteries using such electrolyte solutions, problems such as electrolyte leakage, fire, explosion, etc. may occur. In order to solve such problems, and to ensure essential safety, development of all-solid-state batteries is being promoted in which a solid electrolyte is used instead of a liquid electrolyte and all other elements are composed of solids. Since such all-solid-state batteries use a solid electrolyte, there is no risk of fire, they do not leak, and they are less likely to cause problems such as deterioration of battery performance due to corrosion.
[0003] Various all-solid-state batteries have been proposed. For example, Patent Document 1 (JP Patent Publication No. 2009-193940) discloses that in a pressed powder all-solid-state battery of a sulfide-based solid electrolyte and lithium cobalt oxide, the surface of the lithium cobalt oxide is coated with lithium niobate to reduce the interface resistance. Reducing the interface resistance leads to improved charge / discharge characteristics. The battery disclosed in Patent Document 1 is an all-solid-state battery using a pressed powder, and the energy density of the electrode decreases if pores remain between the particles or if a conductive additive that ensures electronic conduction between active materials is added.
[0004] In response to this, all-solid-state batteries using sintered electrodes instead of compact electrodes have also been proposed. Such batteries have the advantage of having high energy density because the sintered electrodes do not contain conductive additives. For example, Patent Document 2 (WO2019 / 093222A1) describes an oriented positive electrode plate that is a lithium composite oxide sintered plate with a porosity of 10 to 50%, and a lithium composite oxide sintered plate that contains Ti and has a voltage of 0.4 V (vs. Li / Li +) or higher, and a solid electrolyte having a melting point lower than the melting point or decomposition temperature of the oriented positive or negative electrode plate. This document discloses various materials such as Li3OCl, xLiOH·yLi2SO4 (wherein x+y=1, 0.6≦x≦0.95) (e.g., 3LiOH·Li2SO4) as solid electrolytes having such low melting points. Such solid electrolytes can be infiltrated into the gaps of the electrode plates as a molten liquid, and strong interface contact can be achieved. As a result, it is said that a remarkable improvement in battery resistance and rate performance during charging and discharging, as well as a significant improvement in battery manufacturing yield can be achieved. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-193940 A [Patent Document 2] WO2019 / 093222A1 Summary of the Invention
[0006] The present inventors have found that, among the above-mentioned low melting point solid electrolytes, LiOH·Li2SO4-based solid electrolytes such as 3LiOH·Li2SO4 exhibit high lithium ion conductivity. However, when a cell was constructed using a LiOH·Li2SO4-based solid electrolyte such as 3LiOH·Li2SO4 in a sintered electrode as disclosed in Cited Document 2 and operated as a battery, it was found that the discharge amount was lower than the theoretical capacity expected from the amount of active material.
[0007] The present inventors have now discovered that in an all-solid-state secondary battery that employs a LiOH·Li2SO4-based solid electrolyte, the discharge capacity can be improved by providing an intermediate layer of a specific composition at the interface between an electrode active material and a LiOH·Li2SO4-based solid electrolyte.
[0008] Therefore, an object of the present invention is to improve the discharge capacity of an all-solid-state secondary battery that employs a LiOH·Li2SO4-based solid electrolyte.
[0009] According to one aspect of the present invention, a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; a LiOH·Li2SO4-based solid electrolyte interposed between the positive electrode and the negative electrode and also penetrating into voids in at least one of the positive electrode and the negative electrode; Including, In at least one of the positive electrode and the negative electrode into which the solid electrolyte has been permeated, an intermediate layer is further provided at an interface between the solid electrolyte and at least one of the positive electrode active material and the negative electrode active material, the intermediate layer being composed of at least one oxide selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn, and / or a lithium composite oxide containing Li and at least one selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn. [Brief description of the drawings]
[0010] [Figure 1] 1 is a SEM image of the positive electrode plate / solid electrolyte interface produced in Example 6. [Diagram 2] 13 is a TEM image of the positive electrode plate / solid electrolyte interface produced in Example 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] All-solid-state secondary battery The all-solid-state secondary battery of the present invention includes a positive electrode, a negative electrode, and a LiOH·Li2SO4-based solid electrolyte. The positive electrode includes a positive electrode active material. The negative electrode includes a negative electrode active material. The LiOH·Li2SO4-based solid electrolyte is interposed between the positive electrode and the negative electrode, and also enters the voids of at least one of the positive electrode and the negative electrode. This all-solid-state secondary battery further includes an intermediate layer at the interface between at least one of the positive electrode active material and the negative electrode active material and the solid electrolyte in at least one of the positive electrode and the negative electrode into which the solid electrolyte has entered. This intermediate layer is composed of at least one oxide selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn, and / or a lithium composite oxide containing at least one oxide selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn and Li. In this way, in all-solid-state secondary batteries that use a LiOH·Li2SO4-based solid electrolyte, the discharge capacity can be improved by having an intermediate layer of a specific composition at the interface between the electrode active material and the LiOH·Li2SO4-based solid electrolyte.
[0012] As described above, all-solid-state lithium batteries employing low-melting-point solid electrolytes such as LiOH·Li2SO4-based solid electrolytes are known (see, for example, Patent Document 2), and interface contact can be realized by allowing the solid electrolyte to penetrate into the voids of the electrode plate as a melt. As a result, it is possible to improve the battery resistance and the rate performance during charge and discharge, and also to improve the yield of battery manufacturing. In particular, LiOH·Li2SO4-based solid electrolytes such as 3LiOH·Li2SO4 exhibit high lithium ion conductivity. However, when a cell was constructed using a LiOH·Li2SO4-based solid electrolyte for the sintered electrode and the battery was operated, it was found that the discharge amount was lower than the theoretical capacity assumed from the amount of the active material. Although the details of the cause are unknown, it is presumed to be due to the deterioration of the solid electrolyte caused by the reaction between the solid electrolyte and the active material. That is, when the solid electrolyte is melted and penetrated into the voids of the electrode plate, the LiOH·Li2SO4-based solid electrolyte, which is a strong alkali material, becomes in a molten state at high temperature, so that the components of the electrode plate dissolve into the solid electrolyte, and the surface of the electrode plate deteriorates and the activity decreases. In this regard, according to the present invention, by providing the intermediate layer at the interface between the electrode active material / solid electrolyte, the above problem can be solved and the discharge capacity can be improved (compared with those without the intermediate layer).
[0013] (1) Positive electrode The positive electrode (typically a positive electrode plate) contains a positive electrode active material. As the positive electrode active material, a positive electrode active material generally used in a lithium secondary battery can be used, but preferably contains a lithium composite oxide. The lithium composite oxide is an oxide represented by Li x MO2 (where 0.05 < x < 1.10, M is at least one kind of transition metal, and M typically contains one or more of Co, Ni, Mn, and Al). The lithium composite oxide preferably has a layered rock salt structure or a spinel-type structure. A more preferable positive electrode active material is a lithium composite oxide having a layered rock salt structure. Examples of the lithium composite oxide having a layered rock salt structure include Li x CoO2 (lithium cobaltate), Li x NiO2 (lithium nickelate), Li x MnO2 (lithium manganate), Li xNiMnO2 (Lithium Nickel Manganese Oxide), Li x NiCoO2 (Lithium Nickel Cobalt Oxide), Li x CoNiMnO2 (Lithium Cobalt Nickel Manganese Oxide), Li x Examples include CoMnO2 (lithium cobalt manganese oxide), Li2MnO3, and solid solutions of the above compounds. Particularly preferred are Li x CoNiMnO2 (cobalt nickel manganese oxide), and Li x CoO2 (lithium cobalt oxide, typically LiCoO2). A particularly preferred lithium composite oxide having a layered rock salt structure is lithium cobalt nickel manganese oxide (e.g., Li(Ni 0.5 Co 0.2 Mn 0.3 )O2) or lithium cobalt oxide (typically LiCoO2). On the other hand, examples of lithium composite oxides with spinel structure include LiMn2O4-based materials, LiNi 0.5 Mn 1.5 O4-based materials, etc.
[0014] The lithium composite oxide may contain one or more elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Ag, Sn, Sb, Te, Ba, Bi, and W. In addition, LiMPO4 (wherein M is at least one selected from Fe, Co, Mn, and Ni) having an olivine structure can also be suitably used.
[0015] The positive electrode may be in the form of a molded mixture of a positive electrode active material, an electronic conductive assistant, a lithium ion conductive material, a binder, etc., generally called a composite electrode, but is preferably in the form of a sintered plate obtained by sintering a positive electrode raw material powder. That is, the positive electrode or the positive electrode active material is preferably in the form of a sintered plate. Since the sintered plate does not need to contain an electronic conductive assistant or a binder, the energy density of the positive electrode can be increased. The sintered plate may be a dense body or a porous body, and the pores of the porous body may contain a solid electrolyte.
[0016] The positive electrode active material or its sintered plate preferably has a density of 50 to 80 volume %, more preferably 55 to 80 volume %, further preferably 60 to 80 volume %, and particularly preferably 65 to 75 volume %. With a density within such a range, the voids in the positive electrode active material can be sufficiently filled with the solid electrolyte via the intermediate layer, and the proportion of the positive electrode active material in the positive electrode increases, so that a high energy density as a battery can be realized.
[0017] From the viewpoint of improving the energy density of the battery, the thickness of the positive electrode active material or the sintered plate thereof is preferably 50 to 350 μm, more preferably 75 to 350 μm, even more preferably 75 to 325 μm, even more preferably 100 to 325 μm, particularly preferably 100 to 300 μm, especially more preferably 125 to 300 μm, especially even more preferably 150 to 275 μm, and most preferably 100 to 275 μm.
[0018] (2) Negative electrode The negative electrode (typically a negative plate) contains a negative electrode active material. As the negative electrode active material, a negative electrode active material generally used in lithium secondary batteries can be used. Examples of such general negative electrode active materials include carbon-based materials, metals or semimetals such as Li, In, Al, Sn, Sb, Bi, and Si, or alloys containing any of these. In addition, oxide-based negative electrode active materials may be used.
[0019] Particularly preferred negative electrode active materials are those with a voltage of 0.4V (vs. Li / Li + ) or more and capable of inserting and extracting lithium ions, and preferably contains Ti. A negative electrode active material that satisfies such conditions is preferably an oxide that contains at least Ti. A preferred example of such a negative electrode active material is lithium titanate Li4Ti5O 12 Examples of the lithium-ion battery include Li4Ti5O (hereinafter referred to as LTO), niobium titanium composite oxide Nb2TiO7, and titanium oxide TiO2. More preferred are LTO and Nb2TiO7, and even more preferred is LTO. Although LTO is known to have a typical spinel structure, it can also adopt other structures during charging and discharging. For example, LTO is Li4Ti5O12 (spinel structure) and Li7Ti5O 12 The reaction proceeds in the coexistence of two phases, i.e., spinel and tetrahydrofuran (rock salt structure). Therefore, LTO is not limited to a spinel structure.
[0020] The negative electrode may be in the form of a molded mixture of a negative electrode active material, an electronic conductive assistant, a lithium ion conductive material, a binder, etc., generally called a composite electrode, but is preferably in the form of a sintered plate obtained by sintering a negative electrode raw material powder. That is, the negative electrode or the negative electrode active material is preferably in the form of a sintered plate. Since the sintered plate does not need to contain an electronic conductive assistant or a binder, the energy density of the negative electrode can be increased. The sintered plate may be a dense body or a porous body, and the pores of the porous body may contain a solid electrolyte.
[0021] The negative electrode active material or its sintered plate preferably has a density of 55 to 80% by volume, more preferably 60 to 80%, and further preferably 65 to 75%. With a density within such a range, the voids in the negative electrode active material can be sufficiently filled with the solid electrolyte via the intermediate layer, and the proportion of the negative electrode active material in the negative electrode increases, thereby realizing a high energy density as a battery.
[0022] From the viewpoint of improving the energy density of the battery, the thickness of the negative electrode active material or its sintered plate is preferably 75 to 350 μm, more preferably 100 to 325 μm, further preferably 125 to 300 μm, and particularly preferably 150 to 275 μm.
[0023] (3) Solid electrolyte The solid electrolyte is a LiOH·Li2SO4-based solid electrolyte. The LiOH·Li2SO4-based solid electrolyte is a composite compound of LiOH and Li2SO4, and has a typical composition represented by the general formula: xLiOH·yLi2SO4 (wherein x+y=1, 0.6≦x≦0.95). A representative example is 3LiOH·Li2SO4 (wherein x=0.75, y=0.25 in the above general formula). Preferably, the LiOH·Li2SO4-based solid electrolyte includes a solid electrolyte identified as 3LiOH·Li2SO4 by X-ray diffraction. This preferred solid electrolyte contains 3LiOH·Li2SO4 as the main phase. Whether or not the solid electrolyte contains 3LiOH·Li2SO4 can be confirmed by identifying it using 032-0598 of the ICDD database in the X-ray diffraction pattern. Here, "3LiOH·Li2SO4" refers to a material whose crystal structure can be regarded as the same as that of 3LiOH·Li2SO4, and the crystal composition does not necessarily have to be the same as that of 3LiOH·Li2SO4. In other words, as long as it has the same crystal structure as that of 3LiOH·Li2SO4, the solid electrolyte of the present invention also includes those whose composition is outside of LiOH:Li2SO4=3:1. Therefore, even if the solid electrolyte contains a dopant such as boron (for example, 3LiOH·Li2SO4 in which boron is dissolved and the X-ray diffraction peak is shifted to the high angle side), it will be referred to as 3LiOH·Li2SO4 in this specification as long as the crystal structure can be regarded as the same as that of 3LiOH·Li2SO4. Similarly, the solid electrolyte used in the present invention is also allowed to contain inevitable impurities.
[0024] Therefore, the LiOH·Li2SO4-based solid electrolyte may contain a heterogeneous phase in addition to the main phase 3LiOH·Li2SO4. The heterogeneous phase may contain a plurality of elements selected from Li, O, H, S, and B, or may be composed of only a plurality of elements selected from Li, O, H, S, and B. Examples of the heterogeneous phase include LiOH, Li2SO4, and / or Li3BO3 derived from the raw materials. These heterogeneous phases are considered to be unreacted raw materials remaining when 3LiOH·Li2SO4 is formed, but since they do not contribute to lithium ion conduction, it is desirable that the amount of the heterogeneous phases other than Li3BO3 is small. For example, the LiOH·Li2SO4-based solid electrolyte may contain LiOH and / or Li2SO4 as a heterogeneous phase such that the molar ratio of LiOH / Li2SO4 in the entire composition including 3LiOH·Li2SO4 is typically within the range of 1.8 to 3.0, more typically 2.0 to 2.6. However, a heterogeneous phase containing boron such as Li3BO3 may be contained in a desired amount since it can contribute to improving the retention of lithium ion conductivity after long-term storage at high temperatures. However, the solid electrolyte may be composed of a single phase of 3LiOH·Li2SO4 with boron dissolved therein.
[0025] It is preferable that the LiOH·Li2SO4-based solid electrolyte (particularly 3LiOH·Li2SO4) further contains boron. By further containing boron in the solid electrolyte identified as 3LiOH·Li2SO4, it is possible to significantly suppress the decrease in lithium ion conductivity even after long-term storage at high temperatures. It is presumed that boron is incorporated into one of the sites of the crystal structure of 3LiOH·Li2SO4, improving the stability of the crystal structure against temperature. The molar ratio (B / S) of boron B to sulfur S contained in the solid electrolyte is preferably more than 0.002 and less than 1.0, more preferably 0.003 to 0.9, and even more preferably 0.005 to 0.8. If the B / S is within the above range, it is possible to improve the retention rate of lithium ion conductivity. In addition, if the B / S is within the above range, the content of unreacted heterogeneous phases containing boron is low, and therefore the absolute value of lithium ion conductivity can be increased.
[0026] The LiOH·Li2SO4-based solid electrolyte may be a compact of a powder obtained by pulverizing a molten solid, but a molten solid (i.e., solidified after being heated and melted) is preferable.
[0027] The LiOH·Li2SO4-based solid electrolyte fills the gaps in the positive electrode (positive electrode active material) and / or negative electrode (negative electrode active material) when melted, and the remaining part is preferably interposed between the positive electrode and the negative electrode as a solid electrolyte layer. From the viewpoints of charge / discharge rate characteristics and insulating properties of the solid electrolyte, the thickness of the solid electrolyte layer (excluding the part that has filled the gaps in the positive electrode and negative electrode) is preferably 1 to 500 μm, more preferably 3 to 50 μm, and even more preferably 5 to 40 μm.
[0028] (4) Middle class The intermediate layer is provided at the interface between at least one of the positive electrode active material and the negative electrode active material and the solid electrolyte. The intermediate layer is preferably present at the interface between the positive electrode active material and the solid electrolyte, but may be present at the interface between the negative electrode active material and the solid electrolyte. The intermediate layer may be present at both the interface between the positive electrode active material and the solid electrolyte and the interface between the negative electrode active material and the solid electrolyte. The thickness of the intermediate layer is not particularly limited as long as the desired effect of improving the discharge capacity is obtained, but is preferably 0.001 to 1 μm, more preferably 0.005 to 0.2 μm, and even more preferably 0.01 to 0.1 μm.
[0029] The intermediate layer is composed of at least one oxide selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn, and / or a lithium composite oxide containing at least one selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn and Li. Preferred examples of such oxides and / or lithium composite oxides include Y oxide (typically Y2O3), oxides of Li and Nb (typically LiNbO3 or LiNb3O8), oxides of Li and Ta (typically LiTaO3), oxides of Li and Al (typically LiAlO2), and oxides of Li and Y (typically LiYO2), oxides of Li and Ti (typically Li2TiO3), oxides of Li, La, and Zr or Li, La, Zr, and Al (typically Li 7-3x Al x La3Zr2O 12 (0 ≦ x < 0.4, more typically 0.02 < x < 0.4), oxides of Li, La, and Ti (typically Li 0.33 La 0.55 TiO3), oxides of Li and W (typically Li2WO4), oxides of Li and Sn (typically LiSnO3), oxides of Li and Ce (typically Li8CeO6), oxides of Li, La, and Nb (typically Li5La3Nb2O 12 ), as well as oxides of Li and Mn (typically LiMnO2), and any combination thereof, more preferably oxides of Li and Nb (typically LiNbO3), oxides of Li and Al (typically LiAlO2), and oxides of Li and Y (typically LiYO2), oxides of Li and Ti (typically Li2TiO3), oxides of Li, La, Zr, and Al (typically Li 6.7 Al 0.1 La3Zr2O 12 ), oxides of Li, La, and Ti (typically Li 0.33 La 0.55 TiO3) are mentioned.
[0030] The intermediate layer can be formed by mixing metal salts such as metal alkoxides and nitrates of one or more metal elements constituting the intermediate layer with alcohol such as ethanol or water in a predetermined molar ratio to prepare a solution, immersing an electrode active material (preferably a sintered plate) in the solution and allowing it to penetrate into the inside under reduced pressure, then removing it, wiping it off, and leaving it to stand in the air to hydrolyze the alkoxide or dry the solvent. It is preferable to repeat the above-mentioned process from immersion to leaving it to stand in the air multiple times (for example, 1 to 20 times). It is preferable to heat treat the electrode active material (preferably a sintered plate) on which the intermediate layer has been formed in this way at 400 to 700 ° C for 5 to 60 minutes. In addition, when a metal alkoxide is used, the process from preparing the solution to wiping off the solution is preferably performed in a glove box in an Ar atmosphere with a dew point of -50 ° C or less so that the solution does not deteriorate due to hydrolysis or the like.
[0031] (5) Manufacturing of all-solid-state secondary batteries The all-solid-state secondary battery can be manufactured, for example, by i) preparing a positive electrode (with an intermediate layer or a current collector formed as necessary) and a negative electrode (with an intermediate layer or a current collector formed as necessary), and ii) sandwiching a solid electrolyte between the positive electrode and the negative electrode and applying pressure, heat, or the like to integrate the positive electrode, the solid electrolyte, and the negative electrode. The positive electrode, the solid electrolyte, and the negative electrode may be bonded by other methods. In this case, examples of the method for forming the solid electrolyte between the positive electrode and the negative electrode include a method of placing a molded body or powder of the solid electrolyte on one electrode, a method of applying a paste of the solid electrolyte powder on the electrode by screen printing, a method of impacting and solidifying the powder of the solid electrolyte by an aerosol deposition method or the like using the electrode as a substrate, and a method of depositing the solid electrolyte powder on the electrode by electrophoresis to form a film. EXAMPLES
[0032] The present invention will be described in more detail with reference to the following examples. 0.5 Co 0.2 Mn 0.3 )O2 is abbreviated as "NCM" and Li4Ti5O 12 is abbreviated as "LTO" and LiCoO2 is abbreviated as "LCO".
[0033] Example 1 (1) Preparation of the positive electrode plate (1a) Preparation of NCM green sheet Commercially available (Ni 0.5 Co 0.2 Mn 0.3 )(OH)2 powder (average particle size 9 μm) and Li2CO3 powder (average particle size 3 μm) were mixed and held at 750°C for 15 hours to obtain a powder consisting of NCM particles. This powder was pulverized to adjust the average particle size to about 5 μm, and then mixed with a solvent for tape casting, a binder, a plasticizer, and a dispersant. The viscosity of the resulting paste was adjusted, and the paste was tape-cast onto a film to produce an NCM green sheet. The thickness of the NCM green sheet was adjusted so that the thickness after firing would be 100 μm.
[0034] (1b) Preparation of NCM sintered plate The NCM green sheet was degreased by holding it at 450°C for 6 hours, and then heated to 870°C at a heating rate of 200°C / h and held at that temperature for 10 hours to sinter it. In this way, an NCM sintered plate was obtained as a positive electrode plate. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of the obtained NCM sintered plate by sputtering.
[0035] (1c) Deposition of the intermediate layer Niobium ethoxide: lithium ethoxide: ethanol were mixed in a molar ratio of 0.03:0.03:1 to prepare a solution for forming an intermediate layer. The NCM sintered plate prepared in (1b) above was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. The above-mentioned operation was carried out in a glove box in an Ar atmosphere with a dew point of -50°C or less. The NCM sintered plate was then taken out of the glove box and left to stand in the air for 10 minutes to form an intermediate layer. The above series of operations was then repeated once more (i.e., a total of two film formations were performed). Finally, the NCM sintered plate was heat-treated at 400°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0036] (2) Preparation of negative electrode plate (2a) Preparation of LTO green sheet Commercially available TiO2 powder (average particle size 1μm or less) and Li2CO3 powder (average particle size 3μm) were mixed so that the molar ratio of Li / Ti was 0.84, and then held at 1000℃ for 2 hours to obtain a powder consisting of LTO particles. This powder was pulverized to adjust the average particle size to about 2μm, and then mixed with a solvent, binder, plasticizer, and dispersant for tape casting. After adjusting the viscosity of the obtained paste, this paste was tape-cast onto a film to produce an LTO green sheet. The thickness of the LTO green sheet was adjusted so that the thickness after firing would be 100μm.
[0037] (2b) Preparation of LTO sintered plate The LTO green sheet was degreased by holding it at 450°C for 6 hours, and then heated to 1000°C at a heating rate of 200°C / h and held there for 2 hours to sinter it. In this way, an LTO sintered plate was obtained as a negative electrode plate. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of the obtained LTO sintered plate by sputtering.
[0038] (3) Preparation of solid electrolyte (3a) Preparation of raw powder A raw material mixed powder was obtained by mixing Li2SO4 powder (commercial product, purity 99% or more), LiOH powder (commercial product, purity 98% or more), and Li3BO3 (commercial product, purity 99% or more) in a molar ratio of Li2SO4:LiOH:Li3BO3 = 1:3:0.05. These powders were handled in a glove box in an Ar atmosphere with a dew point of -50°C or less, and care was taken to prevent deterioration such as moisture absorption.
[0039] (3b) Melt synthesis The raw material powder mixture was placed in a crucible in an Ar atmosphere. The crucible was then placed in an electric furnace and heat-treated at 430°C for 2 hours to produce a melt. The melt was then cooled in the electric furnace at 100°C / h to form a solidified product.
[0040] (3c) Mortar grinding The obtained solidified product was pulverized in a mortar in an Ar atmosphere to obtain a solid electrolyte powder having an average particle size D50 of 5 to 50 μm.
[0041] (4) Fabrication of all-solid-state batteries A solid electrolyte powder containing 5% by weight of 30 μm diameter ZrO2 beads was placed on the positive plate, and then the negative plate was placed on top of that. A weight was placed on the negative plate, and the plate was heated at 400°C in an electric furnace for 45 minutes. At this time, the solid electrolyte powder melted, and after subsequent solidification, a solid electrolyte layer was formed between the electrode plates. A battery was fabricated using the resulting cell consisting of a positive plate / solid electrolyte / negative plate.
[0042] (5) Evaluation (5a) Analysis of the electrode plate / solid electrolyte interface The battery fabricated in (4) above was disassembled in a glove box, and EDX analysis was performed by SEM and TEM on the interface between the electrode plate on which the intermediate layer was formed and the solid electrolyte.
[0043] (5b) Measurement of compactness The density (volume %) of each of the positive electrode plate (NCM sintered plate not including an intermediate layer or solid electrolyte) prepared in (1b) above and the negative electrode plate (LTO sintered plate not including an intermediate layer or solid electrolyte) prepared in (2b) above was measured as follows. First, the positive electrode plate (or negative electrode plate) was filled with resin, and then the cross section was polished by ion milling, and the polished cross section was observed with an SEM to obtain a cross-sectional SEM image. The SEM image was an image with a magnification of 1000 times. The obtained image was first subjected to a 100% blurring process with a 2D filter using image analysis software (Image-Pro Premier manufactured by Media Cybernetics, Inc.), and then subjected to binarization processing. The ratio (%) of the area of the positive electrode active material portion (or negative electrode active material) to the total area of the positive electrode active material portion (or negative electrode active material) and the resin-filled portion (originally a void portion) in the positive electrode plate (or negative electrode plate) was calculated to obtain the density of the positive electrode active material (or negative electrode active material). The threshold value for binarization was set using Otsu's binarization as a discriminant analysis method.
[0044] (5c) Charge / discharge evaluation The discharge capacity of the battery prepared in (4) above at an operating temperature of 150° C. was measured in the voltage range of 2.7 V to 1.5 V by the following procedure. The battery was charged at a constant current until the battery voltage reached the upper limit of the voltage range, and then charged at a constant voltage until the current value reached a 0.01 C rate, and then discharged to the lower limit of the voltage range. The discharge capacity was calculated as a relative value when the discharge capacity of a battery (comparative example) having the same configuration except that no intermediate layer was formed was taken as 100.
[0045] Example 2 A battery was produced and evaluated in the same manner as in Example 1, except that the intermediate layer was formed five times in total in the above (1c).
[0046] Example 3 A battery was produced and evaluated in the same manner as in Example 1, except that the intermediate layer in the above (1c) was formed as follows.
[0047] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium nitrate, yttrium nitrate, and water (solvent) in a molar ratio of 0.015:0.015:1. The NCM sintered plate was immersed in this solution, and after decompression, the NCM sintered plate was removed from the solution. Then, the plate was heat-treated at 400°C for 30 minutes to form the intermediate layer. The above process was then repeated four more times (i.e., a total of five film formations). Finally, the NCM sintered plate was heat-treated at 700°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0048] Example 4 A battery was produced and evaluated in the same manner as in Example 1, except that the intermediate layer in the above (1c) was formed as follows.
[0049] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing yttrium nitrate and water (solvent) at a molar ratio of 0.015:1. The NCM sintered plate was immersed in this solution, and after reducing the pressure, the NCM sintered plate was removed from the solution. The plate was then heat-treated at 400°C for 30 minutes to form the intermediate layer. The above process was then repeated four more times (i.e., a total of five film formations). Finally, the NCM sintered plate was heat-treated at 700°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0050] Example 5 A battery was produced and evaluated in the same manner as in Example 1, except that the intermediate layer in the above (1c) was formed as follows.
[0051] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium ethoxide, aluminum butoxide, and ethanol (solvent) in a molar ratio of 0.015:0.015:1. The NCM sintered plate was immersed in this solution, and after depressurization, the NCM sintered plate was removed from the solution. The above-mentioned operation was carried out in a glove box in an Ar atmosphere with a dew point of -50°C or less. The NCM sintered plate was then removed from the glove box and left to stand in the air for 10 minutes to form the intermediate layer. The above series of operations was then repeated another nine times (i.e., a total of 10 film formations). Finally, the NCM sintered plate was heat-treated at 700°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0052] Example 6 A battery was produced and evaluated in the same manner as in Example 1, except that the intermediate layer in the above (1c) was formed as follows.
[0053] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium ethoxide, tantalum ethoxide, and ethanol (solvent) in a molar ratio of 0.03:0.03:1. The NCM sintered plate was immersed in this solution, and after depressurization, the NCM sintered plate was removed from the solution. The above-mentioned operation was carried out in a glove box in an Ar atmosphere with a dew point of -50°C or less. The NCM sintered plate was then removed from the glove box and left to stand in the air for 10 minutes to form the intermediate layer. The above series of operations was then repeated four more times (i.e., a total of five film formations). Finally, the NCM sintered plate was heat-treated at 500°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0054] Example 7 (comparison) Except for not forming the intermediate layer in the above (1c), a battery was produced and evaluated in the same manner as in Example 1. The discharge capacity measured in this example was set as the reference value 100 for calculating the relative values of the discharge capacities in Examples 1 to 6.
[0055] Example 8 A battery was produced and evaluated in the same manner as in Example 1, except that the preparation of the NCM green sheet in (1a) above and the preparation of the NCM sintered plate in (1b) above were carried out as follows.
[0056] (Preparation of NCM green sheets) Commercially available (Ni 0.5 Co 0.2 Mn 0.3 )(OH)2 powder (average particle size 9 μm) and Li2CO3 powder (average particle size 3 μm) were mixed and held at 750°C for 10 hours to obtain a powder consisting of NCM particles. This powder was pulverized to adjust the average particle size to about 5 μm, and then mixed with a solvent, binder, plasticizer, and dispersant for tape casting. The viscosity of the resulting paste was adjusted, and the paste was tape cast onto a film to produce an NCM green sheet. The thickness of the NCM green sheet was adjusted so that the thickness after firing would be 100 μm.
[0057] (Production of NCM sintered plates) The NCM green sheet was degreased by holding it at 450°C for 6 hours, and then heated to 920°C at a heating rate of 200°C / h and held at that temperature for 10 hours to sinter it. In this way, an NCM sintered plate was obtained as a positive electrode plate. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of the obtained NCM sintered plate by sputtering.
[0058] Example 9 (comparison) Except for not forming the intermediate layer in the above (1c), a battery was produced and evaluated in the same manner as in Example 8. The discharge capacity measured in this example was set as the reference value 100 for calculating the relative values of the discharge capacities in Examples 8 and 10.
[0059] Example 10 (comparison) A battery was produced and evaluated in the same manner as in Example 8, except that the intermediate layer in the above (1c) was formed as follows.
[0060] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium ethoxide, tetraethoxysilane, and ethanol (solvent) in a molar ratio of 0.030:0.015:1. The NCM sintered plate was immersed in this solution, and after decompression, the NCM sintered plate was removed from the solution. The work from preparation of the solution to wiping off the solution was carried out in a glove box in an Ar atmosphere with a dew point of -50°C or less. The NCM sintered plate was then removed from the glove box and left to stand in the air for 10 minutes to form the intermediate layer. The above series of work was then repeated three more times (i.e., a total of four film formations). Finally, the NCM sintered plate was heat-treated at 400°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0061] Example 11 A battery was produced and evaluated in the same manner as in Example 8, except that the raw material powder in (3a) above was prepared as follows.
[0062] (Preparation of raw powder) A raw material mixed powder was obtained by mixing Li2SO4 powder (commercial product, purity 99% or more), LiOH powder (commercial product, purity 98% or more), and Li3BO3 (commercial product, purity 99% or more) in a molar ratio of Li2SO4:LiOH:Li3BO3 = 1:1.8:0.05. These powders were handled in a glove box in an Ar atmosphere with a dew point of -50°C or less, and care was taken to prevent deterioration such as moisture absorption.
[0063] Example 12 (comparison) Except for not forming the intermediate layer in the above (1c), a battery was produced and evaluated in the same manner as in Example 11. The discharge capacity measured in this example was set as the reference value 100 for calculating the relative value of the discharge capacity in Example 11.
[0064] Example 13 (1) Preparation of the positive electrode plate (1a) Preparation of LCO green sheet Commercially available Co3O4 powder (average particle size 0.9 μm) and commercially available Li2CO3 powder (average particle size 3 μm) were mixed so that the molar ratio of Li / Co was 1.02, and then the mixture was kept at 750°C for 5 hours. The obtained powder was pulverized in a pot mill so that the average particle size was 0.4 μm to obtain LCO powder. The obtained LCO powder was mixed with a dispersion medium, a binder, a plasticizer, and a dispersant. The viscosity of the obtained mixture was adjusted to prepare an LCO slurry. The slurry thus prepared was tape-cast onto a film to form an LCO green sheet. The thickness of the LCO green sheet was set to a value such that the thickness after firing was 60 μm.
[0065] (1b) Preparation of Li2CO3 green sheet A commercially available Li2CO3 raw powder (average particle size 3 μm) was mixed with a dispersion medium, a binder, a plasticizer, and a dispersant. The resulting mixture was adjusted in viscosity to prepare a Li2CO3 slurry. The Li2CO3 slurry thus prepared was tape-cast onto a film to form a Li2CO3 green sheet. The thickness of the dried Li2CO3 green sheet was set so that the Li / Co ratio, which is the molar ratio of the Li content in the Li2CO3 green sheet to the Co content in the LCO green sheet, could be 0.2.
[0066] (1c) Preparation of sintered LCO plate The LCO green sheet peeled off from the PET film was heated to 600°C at a heating rate of 200°C / h, degreased for 3 hours, and then calcined at 900°C for 3 hours. The dried Li2CO3 green sheet was cut out to a size such that the Li / Co ratio, which is the molar ratio of the Li content in the Li2CO3 green sheet to the Co content in the obtained calcined LCO plate, was 0.1. The cut out Li2CO3 green sheet piece was placed on the calcined LCO plate. The sintered plate and the green sheet piece were stacked, and the stack was heated to 600°C at a heating rate of 200°C / h, degreased for 3 hours, then heated to 800°C at 200°C / h, held for 5 hours, and then heated to 850°C at 200°C / h, held for 24 hours, and sintered. In this way, the LCO sintered plate was obtained as a positive electrode plate. An Au film (thickness 100 nm) was formed as a current collecting layer on the obtained LCO sintered body plate by sputtering.
[0067] (1d) Deposition of the intermediate layer Niobium ethoxide: lithium ethoxide: ethanol were mixed in a molar ratio of 0.015:0.015:1 to prepare a solution for forming an intermediate layer. The LCO sintered plate prepared in (1b) above was immersed in this solution, and after depressurization, the LCO sintered plate was removed from the solution. The above-mentioned operation was carried out in a glove box in an Ar atmosphere with a dew point of -50°C or less. The LCO sintered plate was then removed from the glove box and left to stand in the air for 10 minutes to form an intermediate layer. The above series of operations was then repeated two more times (i.e., a total of three film formations). Finally, the LCO sintered plate was heat-treated at 400°C for 30 minutes to obtain a positive electrode plate on which an intermediate layer was formed.
[0068] (2) Preparation of negative electrode plate (2a) Preparation of LTO green sheet A commercially available LTO powder (average particle size 0.7 μm) was mixed with a dispersion medium, a binder, a plasticizer, and a dispersant. The viscosity of the resulting negative electrode raw material mixture was adjusted to prepare an LTO slurry. The slurry thus prepared was tape-cast onto a film to form an LTO green sheet. The thickness of the LTO green sheet after drying was set to a value such that the thickness after firing would be 60 μm.
[0069] (2b) Preparation of LTO sintered plate The obtained green sheet was held at 500° C. for 5 hours, then heated at a rate of 200° C. / h, and sintered at 800° C. for 5 hours. A Au film (thickness 100 nm) was formed as a current collecting layer on the obtained LTO sintered body by sputtering.
[0070] (3) Preparation of solid electrolyte (3a) Preparation of raw powder A raw material mixed powder was obtained by mixing Li2SO4 powder (commercial product, purity 99% or more) and LiOH powder (commercial product, purity 98% or more) in a molar ratio of Li2SO4:LiOH = 1:3. These powders were handled in a glove box in an Ar atmosphere with a dew point of -50°C or less, and care was taken to prevent deterioration such as moisture absorption.
[0071] (3b) Melt synthesis The raw material powder mixture was placed in a crucible in an Ar atmosphere, and the crucible was placed in an electric furnace and heat-treated at 430°C for 2 hours to produce a melt. The melt was then cooled in the electric furnace at 100°C / h to form a solid.
[0072] (3c) Mortar grinding The obtained solidified product was pulverized in a mortar in an Ar atmosphere to obtain a solid electrolyte powder having an average particle size D50 of 5 to 50 μm.
[0073] (4) Fabrication of all-solid-state batteries A battery was fabricated in the same manner as in Example 1(4).
[0074] (5) Evaluation In the same manner as in Example 1(5), the electrode plate / solid electrolyte interface was analyzed and the charge / discharge characteristics were evaluated.
[0075] Example 14 A battery was produced and evaluated in the same manner as in Example 13, except that after the production of the LTO sintered plate in the above (2b), an intermediate layer was formed on the LTO sintered plate in the following manner.
[0076] (Deposition of intermediate layer) Niobium ethoxide: lithium ethoxide: ethanol were mixed in a molar ratio of 0.015:0.015:1 to prepare a solution for forming an intermediate layer. The LTO sintered plate prepared in (2b) of Example 13 was immersed in this solution, and after depressurization, the LTO sintered plate was taken out of the solution. The above-mentioned operation was carried out in a glove box in an Ar atmosphere with a dew point of -50°C or less. The LTO sintered plate was then taken out of the glove box and left to stand in the air for 10 minutes to form an intermediate layer. The above series of operations was then repeated two more times (i.e., a total of three film formations). Finally, the LTO sintered plate was heat-treated at 400°C for 30 minutes to obtain a negative electrode plate on which an intermediate layer was formed.
[0077] Example 15 (comparison) Except for not forming the intermediate layer in the above (1c), a battery was produced and evaluated in the same manner as in Example 13. The discharge capacity measured in this example was set as the reference value 100 for calculating the relative values of the discharge capacities in Examples 13 and 14.
[0078] Example 16 (1) Preparation of the positive electrode plate (1a) Preparation of NCM green sheet Commercially available (Ni 0.5 Co 0.2 Mn 0.3 )(OH)2 powder (average particle size 9 μm) and Li2CO3 powder (average particle size 3 μm) were mixed and held at 750°C for 10 hours to obtain a powder consisting of NCM particles. This powder was pulverized to adjust the average particle size to about 5 μm, and then mixed with a solvent for tape casting, a binder, a plasticizer, and a dispersant. The viscosity of the resulting paste was adjusted, and the paste was tape-cast onto a film to produce an NCM green sheet. The thickness of the NCM green sheet was adjusted so that the thickness after firing would be 100 μm.
[0079] (1b) Preparation of NCM sintered plate The NCM green sheet was degreased by holding it at 450°C for 6 hours, and then heated to 920°C at a heating rate of 200°C / h and held at that temperature for 10 hours to sinter it. In this way, an NCM sintered plate was obtained as a positive electrode plate. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of the obtained NCM sintered plate by sputtering.
[0080] (1c) Deposition of the intermediate layer Titanium tetraisopropoxide: lithium ethoxide: ethanol were mixed in a molar ratio of 0.0225:0.05:1 to prepare a solution for forming an intermediate layer. The NCM sintered plate prepared in (1b) above was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. The above-mentioned operation was performed in an atmosphere with a dew point of -30°C or less. The NCM sintered plate was then left to stand in the air for 5 minutes to form an intermediate layer. The above series of operations was then repeated another 7 times (i.e., a total of 8 times for film formation). Finally, the NCM sintered plate was heat-treated at 400°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0081] (2) Preparation of negative electrode plate (2a) Preparation of LTO green sheet Commercially available TiO2 powder (average particle size 1μm or less) and Li2CO3 powder (average particle size 3μm) were mixed so that the molar ratio of Li / Ti was 0.84, and then held at 1000℃ for 2 hours to obtain a powder consisting of LTO particles. This powder was pulverized to adjust the average particle size to about 2μm, and then mixed with a solvent, binder, plasticizer, and dispersant for tape casting. After adjusting the viscosity of the obtained paste, this paste was tape-cast onto a film to produce an LTO green sheet. The thickness of the LTO green sheet was adjusted so that the thickness after firing would be 200μm.
[0082] (2b) Preparation of LTO sintered plate The LTO green sheet was degreased by holding it at 450°C for 6 hours, and then heated to 850°C at a heating rate of 200°C / h and held there for 2 hours for sintering. In this way, an LTO sintered plate was obtained as a negative electrode plate. A Au film (thickness 100 nm) was formed as a current collecting layer on one side of the obtained LTO sintered plate by sputtering.
[0083] (3) Preparation of solid electrolyte (3a) Preparation of raw powder A raw material mixed powder was obtained by mixing Li2SO4 powder (commercial product, purity 99% or more), LiOH powder (commercial product, purity 98% or more), and Li3BO3 (commercial product, purity 99% or more) in a molar ratio of Li2SO4:LiOH:Li3BO3 = 1:2.6:0.05. These powders were handled in a glove box in an Ar atmosphere with a dew point of -50°C or less, and care was taken to prevent deterioration such as moisture absorption.
[0084] (3b) Melt synthesis The raw material powder mixture was placed in a crucible in an Ar atmosphere. The crucible was then placed in an electric furnace and heat-treated at 430°C for 2 hours to produce a melt. The melt was then cooled in the electric furnace at 100°C / h to form a solidified product.
[0085] (3c) Mortar grinding The obtained solidified product was pulverized in a mortar in an Ar atmosphere to obtain a solid electrolyte powder having an average particle size D50 of 5 to 50 μm.
[0086] (4) Fabrication of all-solid-state batteries A battery was fabricated in the same manner as in Example 1(4).
[0087] (5) Evaluation In the same manner as in Example 1(5), the electrode plate / solid electrolyte interface was analyzed and the charge / discharge characteristics were evaluated.
[0088] Example 17 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0089] (Deposition of intermediate layer) A solution for forming an intermediate layer was prepared by mixing lithium ethoxide, aluminum butoxide, lanthanum nitrate (anhydrous), zirconium tetra-n-butoxide, and 2-ethoxyethanol in a molar ratio of 0.000335:0.000005:0.00015:0.0001:1. An NCM sintered plate was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. The above-mentioned operation was performed in an atmosphere with a dew point of -30°C or less. Then, the plate was heat-treated at 700°C for 30 minutes to form an intermediate layer. The above operation was then repeated once more (i.e., a total of two film formations were performed). A positive electrode plate with an intermediate layer formed thereon was obtained.
[0090] Example 18 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0091] (Deposition of intermediate layer) A solution for forming an intermediate layer was prepared by mixing lithium ethoxide, lanthanum nitrate (anhydrous), titanium tetraisopropoxide, and ethanol in a molar ratio of 0.00099:0.00165:0.003:1. An NCM sintered plate was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. The above-mentioned operation was performed in an atmosphere with a dew point of -30°C or less. Then, the plate was heat-treated at 700°C for 30 minutes to form an intermediate layer. The above operation was then repeated once more (i.e., a total of two film formations) to obtain a positive electrode plate with an intermediate layer formed thereon.
[0092] Example 19 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0093] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium hydroxide, tungsten (IV) oxide, and water in a molar ratio of 0.048:0.024:1. The NCM sintered plate was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. Then, the plate was heat-treated at 800°C for 30 minutes to form the intermediate layer. The above process was then repeated once more (i.e., a total of two film formations) to obtain a positive electrode plate with an intermediate layer formed thereon.
[0094] Example 20 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0095] (Deposition of intermediate layer) Niobium ethoxide: lithium ethoxide: ethanol were mixed in a molar ratio of 0.0225:0.0225:1 to prepare a solution for forming an intermediate layer. An NCM sintered plate was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. The above-mentioned operation was performed in an atmosphere with a dew point of -30°C or less. The NCM sintered plate was then left to stand in the air for 5 minutes to form an intermediate layer. The above series of operations was then repeated another 7 times (i.e., a total of 8 times for film formation). Finally, the NCM sintered plate was heat-treated at 400°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0096] Example 21 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0097] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium ethoxide, aluminum butoxide, and ethanol (solvent) in a molar ratio of 0.0225:0.0225:1. The NCM sintered plate was immersed in this solution, and the pressure was reduced to impregnate the pores of the positive electrode plate with the solution. The above-mentioned operation was carried out in an atmosphere with a dew point of -30°C or less. The NCM sintered plate was then left to stand in the air for 5 minutes to form the intermediate layer. The above series of operations was then repeated another 7 times (i.e., the film was formed a total of 8 times). Finally, the NCM sintered plate was heat-treated at 400°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0098] Example 22 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0099] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium ethoxide, tin isopropoxide, and ethanol (solvent) in a molar ratio of 0.015:0.015:1. The NCM sintered plate was immersed in this solution, and the pressure was reduced to impregnate the pores of the positive electrode plate with the solution. The above-mentioned operation was carried out in an atmosphere with a dew point of -30°C or less. The NCM sintered plate was then left to stand in the air for 5 minutes to form the intermediate layer. The above series of operations was then repeated 7 more times (i.e., the film was formed a total of 8 times). Finally, the NCM sintered plate was heat-treated at 600°C for 30 minutes to obtain a positive electrode plate with an intermediate layer formed thereon.
[0100] Example 23 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0101] (Deposition of intermediate layer) A solution for forming the intermediate layer was prepared by mixing lithium nitrate, cerium nitrate, and water in a molar ratio of 0.008:0.001:1. The NCM sintered plate was immersed in this solution and the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. Then, the plate was heat-treated at 800°C for 30 minutes to form the intermediate layer. The above process was then repeated once more (i.e., the film was formed twice in total) to obtain a positive electrode plate with an intermediate layer formed thereon.
[0102] Example 24 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0103] (Deposition of intermediate layer) A solution for forming an intermediate layer was prepared by mixing lithium ethoxide, lanthanum nitrate (anhydrous), niobium ethoxide, and ethanol in a molar ratio of 0.00025:0.00015:0.0001:1. An NCM sintered plate was immersed in this solution, the pressure was reduced, and the solution was impregnated into the pores of the positive electrode plate. The above-mentioned operation was performed in an atmosphere with a dew point of -30°C or less. Then, the plate was heat-treated at 800°C for 30 minutes to form an intermediate layer. The above operation was then repeated once more (i.e., a total of two film formations) to obtain a positive electrode plate with an intermediate layer formed thereon.
[0104] Example 25 A battery was produced and evaluated in the same manner as in Example 16, except that the intermediate layer in the above (1c) was formed as follows.
[0105] (Deposition of intermediate layer) A solution for forming an intermediate layer was prepared by mixing lithium nitrate, manganese nitrate, and water in a molar ratio of 0.006:0.006:1. An NCM sintered plate was immersed in this solution, and the pressure was reduced to allow the solution to penetrate into the pores of the positive electrode plate. The plate was then heat-treated at 400°C for 30 minutes to form an intermediate layer. The above process was then repeated once more (i.e., a total of two film formations) to obtain a positive electrode plate with an intermediate layer formed thereon.
[0106] Example 26(comparison) Except for not forming the intermediate layer in the above (1c), a battery was produced and evaluated in the same manner as in Example 16. The discharge capacity measured in this example was set as the reference value 100 for calculating the relative values of the discharge capacities in Examples 16 to 25.
[0107] result The evaluation results of Examples 1 to 26 are explained below with reference to Tables 1 to 5 and FIGS.
[0108] (Analysis of the electrode plate / solid electrolyte interface) In the interface between the electrode plate on which the intermediate layer was formed and the solid electrolyte in each of the cells in Examples 1 to 26, metals other than Li used as the intermediate layer and oxygen were detected by EDX analysis. Although Li cannot be detected by EDX, when the solution of the intermediate layer is evaporated to dryness and heat-treated at the same temperature as that for forming the intermediate layer, it can be confirmed by XRD evaluation that an oxide of each metal element (Example 4) or a lithium composite oxide (other than Example 4) is formed. From this, it is presumed that an intermediate layer consisting of an oxide of the element used in the intermediate layer (Example 4) or its lithium composite oxide (other than Example 4) is formed at the interface between the electrode plate and the solid electrolyte in each of Examples 1 to 15. SEM images of the positive electrode plate / solid electrolyte interface actually produced in Examples 6 and 13 are shown in Figures 1 and 2, respectively. In Figure 1 (Example 6), there is a bright area at the interface between the NCM particles and the solid electrolyte, and Ta is detected from this area, and it was found that an intermediate layer of oxides consisting of Li and Ta with a thickness of 0.1 to 1 μm was formed. In addition, in Figure 2 (Example 13), a layer (between the arrows) exists at the interface between the LCO particle and the solid electrolyte (in the figure, 3LHS stands for 3LiOH Li2SO4), and Nb was detected in this part, indicating that an intermediate layer of an oxide consisting of Li and Nb with a thickness of 20 to 30 nm had been formed.
[0109] (Charge / discharge evaluation) Table 1 shows the cell configurations and discharge capacities of Examples 1 to 7. From the results shown in Table 1, it was found that Examples 1 to 6 in which an intermediate layer was formed on the positive electrode plate had improved discharge capacity compared to Example 7 (Comparative Example) in which no intermediate layer was formed. The mechanism by which the intermediate layer improves the discharge capacity is unclear, but it is thought that it may be due to the suppression of degradation of the solid electrolyte (reduction in conductivity) due to the reaction between the NCM and the solid electrolyte, and the suppression of the formation of a high resistance layer at the interface. The above-mentioned phenomenon depends on the type of solid electrolyte and the type of electrode active material, and it was found that oxides of Li and Nb, oxides of Li and Y, oxides of Y, oxides of Li and Al, and oxides of Li and Ta are effective in combinations of LiOH·Li2SO4-based electrolytes and positive electrode active materials.
[0110] Table 2 shows the cell configurations and discharge capacities of Examples 8 to 10. In Examples 8 to 10, the density (volume %) of the active material was changed by changing the method of making the positive electrode plate. Table 2 also shows that Example 8, in which an oxide of Li and Nb was formed as the intermediate layer, had an improved discharge capacity compared to Example 9 (Comparative Example), in which no intermediate layer was formed. That is, it was found that the intermediate layer has an effect even if the microstructure of the positive electrode plate changes. Moreover, Example 10 (Comparative Example), in which an oxide of Li and Si was formed as the intermediate layer, had a lower discharge capacity compared to Example 8, and it was found that the above-mentioned suitable material was present as the intermediate layer.
[0111] Table 3 shows the cell configurations and discharge capacities of Examples 11 and 12. The molar ratio of LiOH:Li2SO4 in the LiOH·Li2SO4-based solid electrolyte was changed in Examples 11 and 12. Table 3 also shows that Example 11, in which an oxide made of Li and Nb was formed as an intermediate layer, had an improved discharge capacity compared to Example 12 (Comparative Example), in which no intermediate layer was formed, demonstrating that the intermediate layer is effective even when the composition of the LiOH·Li2SO4-based solid electrolyte is changed.
[0112] Table 4 shows the cell configurations and discharge capacities of Examples 13 to 15. In Examples 13 to 15, an LCO sintered plate was used as the positive electrode, and the LiOH·Li2SO4-based solid electrolyte was changed. Table 4 also shows that Example 13, in which an oxide of Li and Nb was formed as an intermediate layer, had an improved discharge capacity compared to Example 15 (Comparative Example), in which no intermediate layer was formed, and that the intermediate layer was effective even when LCO, which has a layered rock salt structure different from NCM, was used as the positive electrode plate. Example 14, in which an oxide of Li and Nb was formed as an intermediate layer on the negative electrode plate, also had an increased discharge capacity compared to Example 15 (Comparative Example), and that the intermediate layer was effective. From the above, it was found that forming an oxide of Li and Nb, an oxide of Li and Y, an oxide of Y, an oxide of Li and Al, or an oxide of Li and Ta as an intermediate layer at the interface between various electrode active materials and a LiOH·Li2SO4-based solid electrolyte improves discharge characteristics, and that the effect is particularly remarkable at the interface between the positive electrode plate and a LiOH·Li2SO4-based solid electrolyte.
[0113] Table 5 shows the cell configurations and discharge capacities of Examples 16 to 26. In Examples 16 to 26, an NCM sintered plate was used as the positive electrode, and the molar ratio of LiOH:Li2SO4 in the LiOH·Li2SO4 solid electrolyte was changed. In Table 5, it was found that Examples 16 to 25, in which various lithium composite oxides were formed as intermediate layers, had improved discharge capacities compared to Example 26 (Comparative Example), in which no intermediate layer was formed. From the above, it was found that discharge characteristics were improved by forming an intermediate layer of an oxide of Li and Ti, an oxide of Li, La and Zr or an oxide of Li, La, Zr and Al, an oxide of Li, La and Ti, an oxide of Li and W, an oxide of Li and Al, an oxide of Li and Nb, an oxide of Li and Sn, an oxide of Li and Ce, an oxide of Li, La and Nb, or an oxide of Li and Mn at the interface between the positive electrode active material and the LiOH·Li2SO4 solid electrolyte.
[0114] [Table 1]
[0115] [Table 2]
[0116]
Table 3
[0117]
Table 4
[0118]
Table 5
Claims
1. a positive electrode including a positive electrode active material; a negative electrode including a negative electrode active material; LiOH.Li is interposed between the positive electrode and the negative electrode and also enters the gaps of at least one of the positive electrode and the negative electrode. 2 SO 4 a solid electrolyte based on ZnO; The LiOH.Li 2 SO 4 based solid electrolyte further contains boron; an all-solid-state secondary battery, wherein at least one of the positive electrode and the negative electrode into which the solid electrolyte has been permeated further comprises an intermediate layer composed of an oxide of Y and / or a lithium composite oxide containing Li and at least one selected from the group consisting of Y, Nb, Ta, Al, Ti, La, Zr, W, Sn, Ce, and Mn, at an interface between the solid electrolyte and at least one of the positive electrode active material and the negative electrode active material, and the intermediate layer is present at the interface between the positive electrode active material and the solid electrolyte.
2. 2. The all-solid-state secondary battery according to claim 1, wherein the oxide and / or lithium composite oxide is at least one selected from the group consisting of Y oxide, Li and Nb oxide, Li and Ta oxide, Li and Al oxide, Li and Y oxide, Li and Ti oxide, Li, La and Zr or Li, La, Zr and Al oxide, Li, La and Ti oxide, Li and W oxide, Li and Nb oxide, Li and Sn oxide, Li and Ce oxide, Li, La and Nb oxide, and Li and Mn oxide.
3. The LiOH.Li 2 SO 4 The solid electrolyte was found to be 3LiOH.Li by X-ray diffraction. 2 SO 4 The all-solid-state secondary battery according to claim 1 or 2, comprising a solid electrolyte identified as:
4. The all-solid-state secondary battery according to any one of claims 1 to 3, wherein the positive electrode active material is a lithium composite oxide having a layered rock salt structure.
5. 5. The all-solid-state secondary battery according to claim 4, wherein the lithium composite oxide having a layered rock salt structure is lithium cobalt nickel manganese oxide or lithium cobalt oxide.
6. The all-solid-state secondary battery according to any one of claims 1 to 5, wherein the positive electrode active material is in the form of a sintered plate.
7. The all-solid-state secondary battery according to any one of claims 1 to 6, wherein the positive electrode active material has a density of 50 to 80 volume %.
Citation Information
Patent Citations
JP1974081898A
Electrode and method of manufacturing the same, and lithium ion secondary battery
JP2009193940A
Nonaqueous electrolyte battery
JP2011044368A
All-solid-state battery
JP2013062133A
Solid electrolyte, composite electrolyte, and lithium ion secondary battery having the same
JP2014067574A
Cited By
All-solid-state secondary battery
JPWO2022091983A1