Aqueous polyorganosiloxane hybrid dispersion

Aqueous polyorganosiloxane hybrid resin dispersions with controlled solids and residual solvent content address solvent-related health and safety issues, ensuring stable and safe coating applications.

JP7569623B2Active Publication Date: 2024-10-18EVONIK OPERATIONS GMBH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020047527
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-01
Filing Date
2020-03-18
Publication Date
2024-10-18
Estimated Expiration
2040-03-18

AI Technical Summary

Technical Problem

Existing polyorganosiloxane hybrid resin dispersions have high residual solvent content, which poses health and safety risks and environmental concerns, and existing methods to reduce solvent content compromise coating properties and stability.

Method used

Aqueous polyorganosiloxane hybrid resin dispersions with a solids content of 30.0% to 70.0%, preferably 45.0% to 55.0%, and a residual solvent content of <6.0%, preferably <2.5%, achieved through a process involving emulsification with partially hydrolyzed polyvinyl acetate and solvent removal, ensuring high flash points and stability.

Benefits of technology

The process achieves low residual solvent content without compromising coating properties, enhancing occupational safety and environmental sustainability while maintaining storage stability and formulation flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569623000001
    Figure 0007569623000001
  • Figure 0007569623000002
    Figure 0007569623000002
  • Figure 0007569623000003
    Figure 0007569623000003
Patent Text Reader

Abstract

To provide an aqueous polyorganosiloxane hybrid resin dispersion liquid which is usable in various coating for a residual solvent content related to a lower solid content than a conventional solid content without impairing characteristics, and a method for producing the same.SOLUTION: A polyorganosiloxane hybrid resin dispersion liquid contains at least one polyorganosiloxane hybrid resin, and at least one emulsifier containing partially hydrolyzed polyvinyl acetate as a base, in which the dispersion liquid has 30.0 wt.% to 70.0 wt.% of a solid content, preferably, 45.0 wt.% to 55.0 wt.% thereof with respect to the polyorganosiloxane hybrid resin dispersion liquid, and a residual solvent content is less than 6.0 wt.%, preferably less than 2.5 wt.%, and more preferably less than 1.0 wt.% with respect to the polyorganosiloxane hybrid resin dispersion liquid.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous polyorganosiloxane hybrid resin dispersion, its preparation process, and its use. [Background technology]

[0002] Pure silicone resins, called polyorganosiloxanes, are known for their thermal and weathering stability. They are used for impregnation on concrete, in high thermal stability coatings, or in weathering exterior coatings. To increase the stability of polyorganosiloxanes, they are modified with other polymers. The mutual chemical bonding of the silicone resins with these polymers occurs early in the preparation process.

[0003] Known organically modified polyorganosiloxane resins, hereinafter referred to as polyorganosiloxane hybrid resins, are silicone-alkyd resins, silicone-polyester resins, silicone-epoxide hybrid resins, silicone-polyurethane resins and silicone-polyacrylate resins.

[0004] It is therefore possible to combine the desirable properties of pure silicone resins, such as thermal stability, weather stability, and low surface tension, with the desirable properties of polyesters, such as low thermoplasticity, high elasticity, and good pigment wetting.

[0005] The properties of silicone-polyester resins have been found to be particularly advantageous in decorative coatings for thermally durable household appliances, such as toasters, sunlamp housings, fan heaters, and stoves, as well as in the outer coatings of deep-frying pans and pots. Furthermore, household appliance coatings must be detergent-resistant. This means that they must withstand washing in a dishwasher in the presence of highly alkaline detergent compositions containing surfactants without permanent damage, as is now a specification. The detergent resistance of the coating is generally determined by the lacquer formulation, but in particular by the resin used.

[0006] The properties of epoxy resins can also be combined with those of silicone resins.These silicone-epoxy hybrid resins are notable for better metal adhesion and corrosion protection, as well as better stability against chemicals, compared to pure silicone resins.Typical applications are the coating of exhaust pipes, but also coating systems for ceramic substrates, such as all kinds of stoneware, or concrete.This type of coating system is also used in the shipping industry, for example, for coating ship hulls, underwater and abovewater marine equipment, and port facilities.

[0007] Typically, polyorganosiloxane hybrid resins are provided in organic solvents, such as aromatic hydrocarbons, esters, ethers, or ketones, such as xylene, toluene, sorbeso, and methoxypropyl acetate, ethyl acetate, and butyl acetate. The advantages of solvent-based formulations are the ease of application, good leveling, and initial film formation on the substrate. The polyorganosiloxane hybrid resin film can be physically dried, cured by reaction as a two-component system, or baked. Systems that cure at room temperature are also known.

[0008] However, solvent systems have toxicological and ecological drawbacks. The high content of flammable solvents, some of which are harmful to health, is increasingly being viewed critically for health and safety reasons and environmental protection. Furthermore, the use of solvents is increasingly subject to legal restrictions worldwide. Moreover, in many cases, environmental labels (Blue Angel, Nordic Swan, etc.) or industrial standards along the value creation chain (RAL, IKEA, etc.) require the complete elimination or significant reduction of solvents.

[0009] Thus, the search continues for low-solvent or completely solvent-free systems. The prior art describes a number of proposed solutions to pure silicone resins, called polyorganosiloxanes.

[0010] EP 098940 describes a process in which liquid oligomeric siloxanes are emulsified with polyvinyl alcohol or cellulose ethers, and the condensation of the liquid oligomeric siloxanes in this emulsion gives highly viscous or solid polyorganosiloxanes.The disadvantage of this process lies in the additional technical complexity, since the synthesis of the liquid oligomeric siloxanes requires a different methodology than the synthesis of polymeric organosiloxanes, and the condensation in emulsion can only be controlled with difficulty.

[0011] German Patent No. 2158348 describes a process for preparing high-viscosity siloxane-based emulsions crosslinkable with rubber, in which a highly diluted pre-emulsion based on siloxane is prepared containing at least 150% water and at least 80% emulsifier, and the emulsion is concentrated by distilling off the solvent / water mixture. This process requires a relatively large amount of emulsifier, which is undesirable in many applications due to a significant change in the performance profile and also increases the cost. The maximum siloxane content is 45%, with 5% to 7% remaining in the emulsion.

[0012] German Patent Application Publication No. 4415322 (A1) describes a process for preparing aqueous siloxane resin emulsions using polymeric organosilicon compounds dissolved in organic solvents, such as toluene, in which an emulsifier mixture consisting of ethoxylated triglycerides and ethoxylated tridecyl alcohols and water is added to the polymeric organosilicon compounds, and after achieving a homogeneous mixture that is no longer free-flowing, the organic solvent is removed as a solvent / water mixture, and then the amount of water required to achieve the desired final concentration and optionally known additives are homogeneously incorporated.There is no mention in this document that this process is suitable for other resins than the described polyorganosiloxanes, such as polyorganosiloxane hybrid resins.

[0013] Furthermore, WO 2015 / 091901 is also known from the prior art, which describes an aqueous dispersion of silicone modified polyester resin, in which the residual solvent content of the aqueous dispersion in relation to the solid content of the silicone modified polyester resin in the dispersion cannot reach less than 6% by weight due to the process described in the document.This drawback is demonstrated in the comparative example. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] European Patent No. 098940 [Patent Document 2] German patent no. 2158348 [Patent Document 3] DE 4415322(A1) [Patent Document 4] International Publication No. 2015 / 091901 Summary of the Invention [Problem to be solved by the invention]

[0015] Therefore, the object of the present invention is to provide an aqueous polyorganosiloxane hybrid resin dispersion that can be used in various coatings due to its lower residual solvent content associated with the solids content than known in the prior art, without significant loss of other coating properties and utility for the respective applications. [Means for solving the problem]

[0016] This object has surprisingly been achieved by an aqueous polyorganosiloxane hybrid resin dispersion according to claim 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Surprisingly, it has been found that the dispersions according to the invention have a residual solvent content of <6.0% by weight, preferably <2.5% by weight, more preferably <1.0% by weight, based on the polyorganosiloxane hybrid resin dispersion, at a solids content of 30.0% to 70.0% by weight, preferably 45.0% to 55.0% by weight, based on the polyorganosiloxane hybrid resin dispersion.

[0018] The solids content selected according to the invention is particularly advantageous since it reflects the user's requirements with regard to storage stability, dosage, freedom in formulation and use.

[0019] It has been shown in comparative examples that the dispersions produced by the process according to WO 2015 / 091901 reach a residual solvent content of at most 6% by weight at a solids content of 30.0% by weight relative to the polyorganosiloxane hybrid resin dispersion. If the solids content increases, the residual solvent content in the dispersion also increases.

[0020] In the context of the present invention, the solids consist of polyorganosiloxane hybrid resin and emulsifier.

[0021] A further advantage of the present invention is the occupational safety aspect. Even when products containing small amounts of flammable solvents are used, some basic occupational protection measures are necessary. For example, flash point is an important value for occupational safety precautions. To avoid fire and explosion hazards, solvent-based products with high flash points are preferred over those with low flash points.

[0022] Surprisingly, it has been found that the dispersions according to the invention contribute to occupational safety, since the flash point increases with decreasing residual solvent content in the dispersion.

[0023] Preferably, the polyorganosiloxane hybrid resin dispersion according to the present invention has a flash point according to the methods described in this application of >30.0°C, preferably >60.0°C, more preferably >90.0°C.

[0024] In principle, those skilled in the art classify aqueous polymer dispersions as secondary and primary dispersions. Secondary dispersions are formed from conventionally prepared polymers, which are then converted in a subsequent step from solution or melt into aqueous dispersions. In contrast, primary dispersions are those in which the polymer itself is directly obtained in a dispersed distribution in an aqueous dispersion medium in the presence of an emulsifier. What is common to all preparation processes is that essentially monomers are used in part to build the polymer, or this building is achieved exclusively from such monomers.

[0025] EP 0008090 A1 describes a process for preparing water-miscible silicone-polyester resins, where stable dispersions are based on the use of "acidified" polyesters in the preparation of the silicone-polyester resins. In addition to the very complex process, there is an additional risk of redissociation of the polyester (acid ester hydrolysis) as a result of the acid numbers of 25 to 110 required in this process.

[0026] The requirement for reduced solvent emissions can be taken into account by the aqueous polyorganosiloxane hybrid resin dispersion according to the invention.

[0027] Preferably, the polyorganosiloxane hybrid resin is an organic polymer modified polyorganosiloxane.

[0028] More preferably, the polyorganosiloxane hybrid resin is Component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight, of one or more polyorganosiloxanes of the general formula R a Si(OR') b O (4-a-b / 2) Formula (I) In this case, 0 <a<2、0<b<2、およびa+b<4である、 Optionally, component B) 0 to 20 parts by weight, preferably 1 to 10 parts by weight, of one or more linear and / or branched polyorganosiloxanes of the following formulae: R”O-[R'”2Si-O] n - Formula (II) component C) from 5 to 95 parts by weight, preferably from 30 to 90 parts by weight, of an organic polymer, and a reaction product of a composition comprising: In these formulas: R a , R', R'', and R''' are each independently an alkyl group having 1 to 8 carbon atoms or an aromatic group having 6 to 20 carbon atoms, and n is a number ranging from 4 to 250.

[0029] The polyorganosiloxane hybrid resins can be prepared in known manner. Standard methods can be found in DE 102013218976 (A1), DE 102013218981 (A1), US Pat. No. 3,154,597, or US Pat. No. 3,170,962. The skilled person is aware of further literature, for example "Silicone resins and their combination" by Wernfried Heilen, chapter 2.2 Silicone combination resins / silicone resin hybrids, 2015, or "High Silicones and Silicone-Modified Materials strength Silicone-Urethane Copolymers: Synthesis and Properties", Chapter 26, pp 395-407.

[0030] In this case, for example, a polyorganosiloxane is reacted with an organic polymer having hydroxyl groups or the organic polymer is prepared in the presence of the polyorganosiloxane by a suitable monomer or an organic polymer having alkoxysilane functionality by hydrolysis / condensation or equilibration with an alkoxysilane monomer or siloxane oligomer.

[0031] Preferably, the polyorganosiloxane is a linear or singly or multiply branched Si—OH— or SiOR 3 -functional polyorganosiloxanes.

[0032] Polyorganosiloxanes are also referred to in the literature as siloxane oligomers, alkoxy-functional methyl-, phenyl-, and methyl / phenyl siloxanes, hydroxy-functional methyl-, phenyl-, and methyl / phenyl silicone resins, or silanols.

[0033] Alkoxy-functional methyl-, phenyl-, or methyl / phenyl siloxane oligomers can be obtained from ShinEtsu under trademarks such as KC-89S, KR-500, X40-9225, X40-9246, X40-9250, KR-401N, X-40-9227, KR-510, KR-9218, KR-213, and the like.

[0034] Methoxy-functional methyl-, phenyl-, and methyl / phenyl siloxanes are available from Dow Corning under the trademarks Dow Corning® US-CF 2403 Resins, US-CF 2405 Resins, 3037 Intermediate, 3074 Intermediate, RSN-5314 Intermediate. Silanol-functional methyl / phenyl resins are sold under the trademarks RSN-0409HS Resins, RSN-0431HS Resins, RSN-0804 Resins, RSN-0805 Resins, RSN-0806 Resins, RSN-0808 Resins, RSN-0840 Resins.

[0035] Alkoxy-functional methyl / phenyl-, phenyl- and methyl silicone resins are also supplied in hydrolyzed form relative to the corresponding silanols and are commercially available, for example, from Wacker Chemie under the trademark SILRES® with the additional designations REN50, REN60, REN80, KX, HK46, MSE100 or SY300, IC836, REN168, SY409, IC232, SY231, IC368, IC678.

[0036] The preparation of silicone resins of this type has long been known in the literature (see, in this regard, W. Noll - Chemie und Technologie der Silicone [Chemistry and Technology of the Silicones], Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, 1960) and is also described in DE 3412648.

[0037] The organic polymers in question preferably comprise polyepoxides, polyesters, polyacrylates and / or methacrylates and their copolymers, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamideimides, polyimides, polyethers, aromatic and aliphatic glycidyl-functional polymers, oligomers, phenoxy resins, polycarbonates, ketone-formaldehyde resins, as well as polyvinyl resins selected from polyvinyl alcohols, polyglycerols, polyvinyl acetates, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins, and mixtures thereof.

[0038] Preference is given to using polyesters selected from reaction products of aromatic and / or aliphatic and / or cycloaliphatic mono- and / or di- and / or polycarboxylic acids, and their anhydrides and / or esters, with linear and / or branched aliphatic and / or cycloaliphatic and / or aromatic diols and / or polyols. Examples of customary carboxylic acids are phthalic acid, phthalic anhydride, dimethyl terephthalate, isophthalic acid, terephthalic acid, cyclohexane-1,4-dicarboxylic acid, succinic acid, succinic anhydride, sebacic acid, maleic acid, maleic anhydride, fumaric acid, methyltetrahydrophthalic acid, methyltetrahydrophthalic anhydride, methylhexahydrophthalic acid, methylhexahydrophthalic anhydride, hexahydrophthalic acid, tetrahydrophthalic acid, dodecanedioic acid, adipic acid, azelaic acid, isononanoic acid, 2-ethylhexanoic acid, pyromellitic acid, pyromellitic dianhydride, trimellitic acid and / or trimellitic anhydride. Examples of customary diols and / or polyols are ethylene glycol, propane-1,2- and / or -1,3-diol, diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, butane-1,2- and / or -1,4-diol, butylethylpropane-1,3-diol, methylpropane-1,3-diol, pentane-1,5-diol, cyclohexanedimethanol, glycerol, hexanediol, neopentyl glycol, trimethylolethane, trimethylolpropane and / or pentaerythritol, as well as bisphenols A, B, C, F, norbornyl ene glycol, 1,4-benzyldimethanol and -ethanol, 2,4-dimethyl-2-ethylhexane-1,3-diol.

[0039] Preference is given to using epoxy resins with at least two 1,2-epoxy groups per molecule.Examples of suitable epoxy resins are aliphatic or aromatic epoxides: Eponex® and EPON® resins from Hexion, Epalloy® resins from Emerald Performance Materials Company, Epotec® resins from Aditya Birla Chemicals, Denacol® resins from Nagase ChemteX, Araldite® resins from Huntsman, Beckopox® from Allnex, VORAFORCE® resins from Dow Chemical Company.

[0040] The various fragments of the siloxane chain shown in formula (I) or formula (II) can be statistically distributed, the statistical distribution can have a block-like structure with any number of blocks and any sequence, or can be in a randomized distribution, they can also have an alternating structure or form a gradient along the chain, and in particular they can also form any hybrid.

[0041] The indices listed herein and the ranges of values ​​for the indicated indices can be understood as meaning average values ​​for the possible statistical distributions in the actually existing structures and mixtures thereof. This also applies to structural formulae reproduced as such, for example, formula (I).

[0042] The word fragment "poly" in the context of the present invention encompasses not only compounds having at least three repeat units of one or more monomers in the molecule, but also in particular compositions of compounds having a molecular weight distribution and an average molecular weight of at least 200 g / mol. This definition takes into account the fact that it is customary in the industrial sector of interest to refer to compounds as polymers, even if they do not appear to correspond to the definition of a polymer according to the OECD or REACH guidelines.

[0043] Unless otherwise stated, percentages are by weight.

[0044] Where measurements are reported below, these measurements were carried out under standard conditions (25° C. and 1013 mbar) unless otherwise stated.

[0045] Where average values ​​are reported below, the values ​​of interest are weighted averages unless otherwise stated.

[0046] More preferably, the organic polymer contains hydroxyl groups and / or acidic hydrogens.

[0047] Preferably, the emulsifier is a partially hydrolyzed polyvinyl acetate having an alcoholysis level between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), more preferably between 70% and 90% (mol / mol).

[0048] Preferably, the partially hydrolyzed polyvinyl acetate has a viscosity of 1 to 50 mPa·s, preferably 1 to 40 mPa·s, more preferably 1 to 30 mPa·s, measured in a 4% polyvinyl acetate solution in water at 20° C. according to DIN 53015.

[0049] Preferably, the emulsifier does not contain any bound silanes.

[0050] It is also conceivable to use the emulsifiers according to the invention together with other emulsifiers, for example anionic, cationic or non-ionic emulsifiers. If several emulsifiers are used, these should be considered as an emulsifier system according to the invention.

[0051] The weight ratio of polyorganosiloxane hybrid resin to emulsifier or emulsifier system is preferably between 5-50, preferably between 7-40, more preferably between 10-30.

[0052] If desired, the polyorganosiloxane hybrid resin dispersion preferably contains an antifoaming agent, a degassing agent, a rheology additive, Preservatives , and further additives selected from substrate wetting agents, crosslinking agents, drying aids, catalysts, antioxidants, antiskinning agents, antisettling agents, thickeners, coalescing agents, coalescing aids, fillers, pigments, and / or dispersants.

[0053] Preferably, the pigment is an organic or inorganic pigment or a carbon black pigment. Examples of inorganic pigments include iron oxide, chromium oxide, or titanium oxide. Suitable organic pigments are, for example, azo pigments, metal complex pigments, anthraquinoid pigments, phthalocyanine pigments, and polycyclic pigments, in particular the series of thioindigo, quinacridone, dioxazine, pyrrolopyrrole, naphthalenetetracarboxylic acid, perylene, isoamidoline (isoamidrinone), flavanthrone, pyranthrone, or isoviolanthrone. The carbon black used can be gas black, lamp black, or furnace black. These carbon blacks can additionally be post-oxidized and / or converted into beads.

[0054] Optionally, further additives can be added. An additive in this context is any component that has a desired effect on the properties of the dispersion according to the invention. It is possible to add one or more additives independently of each other. Listed below in this specification are some additives that can be used for the dispersion according to the invention. The list is non-exhaustive. Additives that can be advantageously used are, inter alia, wetting and dispersing additives. A large number of wetting and dispersing additives that can be used for the dispersion according to the invention are commercially available. These dispersing additives are, for example, from polymer classes that are well known in the prior art, such as styrene-maleic anhydride copolymers, acrylates, polyethers, such as styrene oxide polyethers, polyesters, amino polyesters, polyurethanes, and amino polyethers. The additives can have different topologies, such as linear, branched, comb-shaped, or star-shaped. Typically, wetting and dispersing additives have a heterogeneous structure that is divided into a linking group and a stabilizing side chain.

[0055] As well as pigments, it is also possible to use fillers in the dispersions according to the invention. Suitable fillers are, for example, those based on kaolin, talc, mica, other silicates, quartz, cristobalite, wollastonite, perlite, diatomaceous earth, fibrous fillers, aluminium hydroxide, barium sulphate, glass or calcium carbonate.

[0056] The use of defoamers or deaerators can be advantageous to actively reduce the amount of air introduced in processing or manufacturing operations, examples of which include those based on mineral or vegetable oils, or polyether siloxanes, optionally filled with particulate components such as silica.

[0057] Examples of further additives may include binders, dyes, surface additives, compatibilizers, wetting and spreading agents, crosslinking agents, rheology additives, thickeners, UV stabilizers, and preservatives.

[0058] Preferably, the preservatives used are fungicides, bactericides, insecticides, algaecides and / or herbicides.

[0059] Preferably, the polyorganosiloxane hybrid resin particles have an average volume-weighted diameter between 0.1 and 10.0 μm, preferably between 0.1 and 2.0 μm, more preferably between 0.2 and 1.0 μm, and most preferably between 0.2 and 0.7 μm, as measured according to ISO 13320: 2009. In the present invention, the average volume-weighted diameter of the particles can be determined using a Coulter LS 13320 instrument manufactured by Beckman Coulter.

[0060] Preferably, the polyorganosiloxane hybrid resin dispersion has a solid content of 30.0% to 70.0% by weight, preferably 45.0% to 55.0% by weight, based on the dispersion. The present invention further comprises: a. emulsifying a polyorganosiloxane hybrid resin solution containing an organic solvent with an emulsifier solution containing at least one emulsifier based on partially hydrolyzed polyvinyl acetate; b. removing the solvent; The present invention provides a process for producing an aqueous polyorganosiloxane hybrid resin dispersion, comprising:

[0061] It is preferred to add more water in step a) so that, for example, the solids content in this step can be fixed or at least contained within a desired solids content range.

[0062] Preferably, after step b), it is possible to adjust the solids content of the aqueous polyorganosiloxane hybrid resin dispersion.

[0063] More preferably, it is possible to both include a desired solids range in step a) and set said solids content of the aqueous polyorganosiloxane hybrid resin dispersion of the present invention after step b).

[0064] The method of the present invention therefore allows for an elegant manufacturing process in which the solids content can be predetermined at the start, and fine adjustments can be included downstream if required.

[0065] Preference is given to using partially hydrolyzed polyvinyl acetates having an alcoholysis level between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), more preferably between 70% and 90% (mol / mol).

[0066] Preferably, the emulsifier does not contain any bound silanes.

[0067] Preferably, the partially hydrolyzed polyvinyl acetate has a viscosity, measured in a 4% polyvinyl acetate solution in water according to DIN 53015 at 20° C., of 1 to 50 mPa·s, preferably 1 to 40 mPa·s, more preferably 1 to 30 mPa·s.

[0068] Such emulsifiers are available, for example, under the brand names Mowiol, Elvanol, or Poval (Kuraray), Gohsenol (Nippon Gohsei), Selvol (Sekisui), Polyviol (Wacker).

[0069] It is also possible to use further emulsifiers, preferably selected from the group of the anionic, cationic, zwitterionic or nonionic emulsifiers.

[0070] Preferably, the polyorganosiloxane hybrid resin used is Component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight, of one or more polyorganosiloxanes of the general formula R a Si(OR') b O (4-a-b / 2) Formula (I) In this case, 0 <a<2、0<b<2、およびa+b<4である、 Optionally, component B) 0 to 20 parts by weight, preferably 1 to 10 parts by weight, of one or more linear and / or branched polyorganosiloxanes of the following formulae: R”O-[R'”2Si-O] n - Formula (II) Component C) 5 to 95 parts by weight, preferably 30 to 90 parts by weight, of an organic polymer and a reaction product of a composition comprising: In these formulas: R a , R', R'', and R''' are each independently an alkyl group having 1 to 8 carbon atoms or an aromatic group having 6 to 20 carbon atoms, and n is a number ranging from 4 to 250.

[0071] Preferably, the polyorganosiloxane is a linear or singly or multiply branched Si—OH— or SiOR 3 -functional polyorganosiloxanes. Commercially available polyorganosiloxanes are described above.

[0072] The organic polymers in question preferably comprise polyepoxides, polyesters, polyacrylates and / or methacrylates and their copolymers, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamideimides, polyimides, polyethers, aromatic and aliphatic glycidyl-functional polymers, oligomers, phenoxy resins, polycarbonates, ketone-formaldehyde resins, as well as polyvinyl resins selected from polyvinyl alcohols, polyglycerols, polyvinyl acetates, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins, and mixtures thereof.

[0073] More preferably, the organic polymer comprises an organic polymer having hydroxyl groups, preferably selected from the group of polyepoxides, polyesters, polyacrylates, polymethacrylates, polyurethanes, and cellulose derivatives.

[0074] Preference is given to using polyesters selected from reaction products of aromatic and / or aliphatic and / or cycloaliphatic mono- and / or di- and / or polycarboxylic acids, and their anhydrides and / or esters, with linear and / or branched aliphatic and / or cycloaliphatic and / or aromatic diols and / or polyols. Examples of customary carboxylic acids are phthalic acid, phthalic anhydride, dimethyl terephthalate, isophthalic acid, terephthalic acid, cyclohexane-1,4-dicarboxylic acid, succinic acid, succinic anhydride, sebacic acid, maleic acid, maleic anhydride, fumaric acid, methyltetrahydrophthalic acid, methyltetrahydrophthalic anhydride, methylhexahydrophthalic acid, methylhexahydrophthalic anhydride, hexahydrophthalic acid, tetrahydrophthalic acid, dodecanedioic acid, adipic acid, azelaic acid, isononanoic acid, 2-ethylhexanoic acid, pyromellitic acid, pyromellitic dianhydride, trimellitic acid and / or trimellitic anhydride. Examples of customary diols and / or polyols are ethylene glycol, propane-1,2- and / or -1,3-diol, diethylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, butane-1,2- and / or -1,4-diol, butylethylpropane-1,3-diol, methylpropane-1,3-diol, pentane-1,5-diol, cyclohexanedimethanol, glycerol, hexanediol, neopentyl glycol, trimethylolethane, trimethylolpropane and / or pentaerythritol, as well as bisphenols A, B, C, F, norbornyl ene glycol, 1,4-benzyldimethanol and -ethanol, 2,4-dimethyl-2-ethylhexane-1,3-diol.

[0075] Preferred are epoxy resins with at least two 1,2-epoxy groups per molecule. Examples of suitable epoxy resins are aliphatic or aromatic epoxides: Eponex® and EPON® resins from Hexion, Epalloy® resins from Emerald Performance Materials Company, Epotec® resins from Aditya Birla Chemicals, Denacol® resins from Nagase ChemteX, Araldite® resins from Huntsman, Beckopox® from Allnex, VORAFORCE® resins from Dow Chemical Company.

[0076] Preferably, the solvent is the organic solvent or mixture of organic solvents used in the preparation of the polyorganosiloxane hybrid resin.

[0077] The solvent may preferably be a semi-organic solvent.

[0078] Preference is given to using solvents selected from the group of ketones selected from methyl ethyl ketone, acetone, methyl isobutyl ketone, diethyl ketone, methyl propyl ketone, cyclohexanone or methylcyclohexanone, esters selected from ethyl acetate, butyl acetate, ethyl propionate, isobutyl acetate or tert-butyl acetate, carbonates such as dialkyl carbonates or cyclic carbonates such as ethylene carbonate, propylene carbonate or glycerol carbonate, aromatic hydrocarbons such as xylene, cyclic hydrocarbons such as cyclohexane, crown ethers or ethers such as dibutyl ether, ester ethers such as methoxypropyl acetate, siloxanes such as hexamethyldisiloxane, octamethylcyclotetrasiloxane or decamethylcyclopentasiloxane, organometallic germanium compounds such as tetramethylgermanium, etc. It is also conceivable to use other solvents or mixtures of different solvents known to those skilled in the art.

[0079] More preferably, the organic solvent or mixture thereof at standard pressure or 1013 mbar has a boiling range of 50°C to 150°C, preferably 90°C to 120°C.

[0080] Preferably, the solvent is removed by vacuum distillation in the presence or absence of a stripping gas, by steam distillation or by a (diffusion) membrane process or thin film evaporator.

[0081] Preferably, the polyorganosiloxane hybrid resin solution has a polyorganosiloxane hybrid resin concentration of 40.0% by weight to 95.0% by weight, preferably 60.0% by weight to 70.0% by weight, based on the polyorganosiloxane hybrid resin solution.

[0082] Preferably, an aqueous emulsifier or emulsifier-based solution is used whose concentration is between 5 and 40% by weight, preferably between 10 and 30% by weight, more preferably between 15 and 25% by weight, based on the emulsifier solution.

[0083] The process according to the present invention differs from WO 2015 / 091901 in that the removal of the solvent is carried out in the presence of an emulsifier solution.It was surprising that the solvent can be removed to a large extent from the polyorganosiloxane hybrid resin.Irrespective of the starting solvent concentration of the polyorganosiloxane hybrid resin, it is possible to produce a low residual solvent content without impairing the stability and therefore the processability of the polyorganosiloxane hybrid resin dispersion.

[0084] The process according to WO2015 / 091901 describes the first step of removing the solvent of silicone polyester hybrid resin, the second step of homogenizing the still processable resin with concentrated emulsifier solution, and the third step of dispersing by adding water to produce the dispersion.Nothing is written in the document about the temperature and time required in the first step.Therefore, the advantage of the process according to the present invention also lies in the reduction of the production steps, which leads to time saving.

[0085] Thus, the present invention also provides an inventive aqueous polyorganosiloxane hybrid resin dispersion produced by the process according to the present invention.

[0086] A further advantage of the process according to the invention is the increased flash point of the aqueous polyorganosiloxane hybrid resin dispersions produced by the process according to the invention.

[0087] The present invention also provides the use of the polyorganosiloxane hybrid resin dispersion of the present invention in coating materials, as well as coatings and paints, substrate coatings, adhesives, structural adhesives, compounding matrices and sizing agents.A further field of use is in the manufacture of printing inks or 3D printing materials.

[0088] Also included are substrates according to the invention, especially baking trays, baking tins, pans, metal pots, etc., coated with a composition comprising a polyorganosiloxane hybrid resin dispersion according to the invention. The substrate is preferably a ceramic substrate, a polymer substrate, or a metal substrate.

[0089] The subject matter of the present invention is illustrated by the following examples, without, however, intending to limit the invention to these illustrative embodiments.

[0090] method: Particle size measurement The particle size of the dispersion is determined according to ISO 13320:2009. A Beckman-Coulter LS13320 instrument was used. The particle size is determined by the refractive index n d = 1.51. The calculated mean particle diameter is volume weighted.

[0091] Identification of solids The content of non-volatile constituents is determined according to DIN EN ISO 3251:2008, and in the context of the present invention, for the determination of the solids content, the polyorganosiloxanes and the polyorganosiloxane hybrid resin solutions are tested at 180° C. for 60 minutes and the dispersions at 105° C. for 60 minutes.

[0092] Viscosity determination Unless stated otherwise, the viscosity was determined using a Brookfield LV-DV-I+ spindle viscometer. The Brookfield viscometer is a rotational viscometer with a defined spindle set as the rotor. The rotor used was from the LV spindle set. Due to the temperature dependence of the viscosity, the temperature of the viscometer and the measured liquid was kept constant during the measurements with an accuracy of ±-0.5°C. In addition to the LV spindle set, further materials used were a thermostatable water bath, a 0-100°C thermometer (with a scale of 1°C or less) and a timer (scale value of 0.1 seconds or less). For the measurements, 100 ml of the sample was placed in a wide-mouth flask and, after prior calibration, the measurements were carried out under temperature-controlled conditions and in the absence of air bubbles. To determine the viscosity, the viscometer was positioned relative to the sample so that the spindle was immersed in the product up to the mark. The measurement was started by activating the start button and care was taken to ensure that the measurement was performed in the most favorable measurement region, which is 50% (±20%) of the maximum measurable torque. The measurement results are given in mPa·s on the viscometer and can be expressed in mm by dividing by the density (g / ml). 2 Viscosity was given in s / sec.

[0093] Residual solvent content Determination of residual solvent content was performed according to the European Pharmacopoeia 5.4 Residual solvents.

[0094] Konig pendulum hardness For the Konig measurement of pendulum hardness (DIN 53157 or EN ISO 1522), the measure used is the damping of an oscillating pendulum. A pendulum with two stainless steel balls is positioned on the coating film. There is a physical relationship between the duration, amplitude and geometric dimensions of the pendulum. The viscoelastic behavior of the coating is the determining factor for the hardness. When the pendulum is set in an oscillating motion, the balls roll on the surface and thus exert pressure on it. A greater or lesser recovery depends on the elasticity. The absence of elastic forces results in significant damping in the pendulum motion. In contrast, high elastic forces result in only slight damping. "Konig" pendulum hardness: Number of oscillations in vibration 1 cycle = 1.4 seconds

[0095] Further conditions When percentage figures are given in the context of the present invention, the figures of interest are weight percent unless otherwise specified. In the case of compositions, the percentage figures are relative to the total composition unless otherwise specified. When averages are reported in the following embodiments, they are number averages unless otherwise specified. When measurements are reported hereinafter, these measurements are specified at a pressure of 101,325 Pa, a temperature of 23° C., and an ambient relative atmospheric humidity of about 40%, unless otherwise specified.

[0096] Identifying the flash point The flash points were determined in accordance with DIN EN ISO 2719 by the Pensky-Martens method in a closed crucible using a flash point tester.

[0097] The Pensky-Martens flash point tester with closed crucible measures the flash point, which is the lowest temperature reading at which an ignition source can ignite the vapor phase of a sample.

[0098] 70 ml of each dispersion according to the invention of Table 5 were used. Prior to the measurement, the samples were pretreated as follows: those dispersions with a residual solvent content >2.0% by weight were cooled to 10° C. and analyzed immediately. Dispersions with a residual solvent content ≦2.0% were cooled to 15° C.

[0099] All dispersions were adjusted to 50% solids by weight.

[0100] A heating rate of 1.5° C. / min and a stirring rate of 120 rpm were selected. The air pressure was 994 mbar. No conversion was performed since the correction was smaller than the maximum error of the measurement. Materials and Equipment Glass plate, Glaserei Glanzer: 90 x 150 x 5 mm ·PVC sheet, manufactured by KVG Kunststoff Betriebs GmbH, Mat No: 4364002858 300μm bar applicator, manufactured by Simex 300μm cube applicator, manufactured by TQC GmbH Dispermat with Teflon disc, manufactured by VMA Getzmann Wide-mouth glass bottle Flash point tester with closed crucible - PMA4 (semi-automatic), manufactured by Petrotest Silikopon® EW, manufactured by Evonik Industries Poval® 04-88, manufactured by Kuraray Poval® 03-80, manufactured by Kuraray Poval® 18-88, manufactured by Kuraray Gohsenol (registered trademark) KL-03, manufactured by Nippon Gohsei Gohsenol (registered trademark) KL-05, manufactured by Nippon Gohsei Tergitol® 15-S-5, manufactured by DOW Chemical EXAMPLES

[0101] Preparation of the aqueous polyorganosiloxane hybrid dispersion according to the present invention To prepare the aqueous polyorganosiloxane hybrid dispersion according to the present invention, a solvent-based polyorganosiloxane hybrid solution is first prepared, and then the solvent is removed by the method according to the present invention.

[0102] 1. Preparation of a solvent-based polyorganosiloxane hybrid solution with polyester (which for simplicity is referred to hereinafter as silicone-polyester hybrid solution) 1.1 Preparation of polyorganosiloxane as component A Solvents used: methyl isobutyl ketone (MIBK), diethyl carbonate (DEC), methyl propyl ketone (MPK), ethyl acetate (EtAc), isobutyl acetate (iBuAc), ethyl isobutyrate (EtiBu).

[0103] First, three polyorganosiloxanes POS 1, POS 2 and POS 3 were prepared according to EP 0157318 according to the parameters in Table 1 below.

[0104] POS 4 is a polyorganosiloxane commercially available from Dow Corning.

[0105] [Table 1]

[0106] 1.2 Preparation of hydroxy-functional polyester as component C The hydroxy-functional polyesters PES 1 to PES 5 were prepared by esterification of trimethylolpropane, isophthalic acid and ethylene glycol according to the process described in German Patent No. 3728414 (C1). The solids content and viscosity were adjusted by solvents according to Table 2.

[0107] [Table 2]

[0108] 1.3 Preparation of solvent-based silicone-polyester hybrid solutions (variant 1) The silicone-polyester hybrid solutions SiPES 6 to SiPES 11 were prepared by the process according to EP 0092701.

[0109] The silicone-polyester hybrid solution SiPES 12 was prepared by the process according to EP1072660.

[0110] In this case, components A and C from Tables 1 and 2 were used. Table 3 shows further relevant data.

[0111] [Table 3]

[0112] 1.4 Preparation of solvent-based silicone-polyester hybrid solutions (variant 2) The silicone-polyester hybrid solutions SiPES 1 to SiPES 5 were prepared by the process according to example 1 of DE 102013218981 A1.

[0113] In this case, the organic polymer was used as a monomer. Table 4 shows the relevant data of the silicone-polyester hybrid solutions SiPES 1 to SiPES 5.

[0114] [Table 4]

[0115] 1.5 Solvent-based epoxy-polyorganosiloxane hybrid solutions (for simplicity, hereafter referred to as silicone-polyepoxide hybrid solutions) Silikopon® EW, available from Evonik Industries, was used.

[0116] 2. Preparation of polyorganosiloxane hybrid dispersion The solvent-based silicone-polyester hybrid solutions described above (variations 1 and 2) and the solvent-based silicone-polyepoxide hybrid solutions described above, referred to as polyorganosiloxane hybrid resins in the method descriptions below, were used.

[0117] 2.1 Method 1, working example: First, 100.0 grams of a 20% solution of Poval® 4-88 in deionized water are placed in a container at room temperature. Then, 360.0 grams of polyorganosiloxane hybrid resin dissolved in an appropriate amount of solvent are added. In this case, the speed of the stirrer system is 1000 rpm. The result is a very viscous paste, which is stirred at 1000 rpm for another 60 minutes after the addition of the resin is finished. Then, 140.0 grams of demineralized water are added. In the next step, the solvent is removed by distillation. For this, the temperature is increased to 50° C. and the pressure is reduced to 40 mbar. Then, the solids content of the dispersion is determined. Then, the dispersion is adjusted to a solids content of 50.0% by adding demineralized water while stirring.

[0118] 2.2 Method 2, Example: Similar to method 1, except the emulsifier solution was a 20% solution of Poval® 3-80 in deionized water.

[0119] 2.3 Method 3, Example: Similar to method 1, except the emulsifier solution was a 12.5% ​​solution of Poval® 18-88 in deionized water.

[0120] 2.4 Method 4, Example: Similar to method 1, except the emulsifier solution was a 20% solution of Gohsenol® KL-03 in deionized water.

[0121] 2.5 Method 5, Example: Similar to method 1, except the emulsifier solution was a 20% solution of Gohsenol® KL-05 in deionized water.

[0122] 2.6 Method 6, Example: Similar to method 1, except 70.0 grams of a 20% solution of Poval® 4-88 in deionized water and 30.0 grams of a 50% solution of Tergitol® 15-S-5 in deionized water are first placed in a container at room temperature.

[0123] The particle size, flash point, and residual solvent content were determined for each of the prepared dispersions E1-E30 and the values ​​can be found in Table 5.

[0124] All dispersions were adjusted to 50% solids by weight.

[0125] [Table 5]

[0126] The residual solvent content of the dispersions according to the invention was less than 6% by weight. The flash points of the dispersions according to the invention were in all cases higher than that of the comparative example (VE24). In particular, for the dispersions according to the invention with a residual solvent content of <1% by weight, the dispersions boiled due to the water content, so a flash point of >100° C. was reported, whereas it was not possible to determine the flash point.

[0127] Comparative Example VE24 was a dispersion with a residual solvent content of 6.1 wt.% and a solids content of 50 wt.%. To produce VE24 with this residual solvent content, the process according to the invention was conveniently terminated early. The flash point was correspondingly low.

[0128] It was therefore possible to find that the process according to the invention makes it possible to increase the flash point of an aqueous polyorganosiloxane hybrid resin dispersion.

[0129] 3. Limitations of WO 2015 / 091901, hereinafter referred to as "Wacker" Silicone modified polyester resins having 40 wt. % solvent content according to Wacker examples 5, 6, 7, 10, 11, and 12 were used to make the dispersions by the "Wacker" process.

[0130] For this purpose, the silicone polyester resin was vacuum distilled at up to 90°C until the resin mass reached a certain viscosity such that the resin was still processable. Processability is necessary to allow emulsification in the next step. Since WO2015 / 091901 does not disclose any details about temperature and duration, a temperature below the boiling point of water was used. Then, the solid content was determined.

[0131] At solids contents above 85% by weight, it was found that the resin mass was no longer processable: it was no longer emulsifiable.

[0132] At a maximum solid content of 80% by weight, the resin mass still has adequate processability and is used to produce a dispersion with a solid content of 30% by weight for the polyorganosiloxane hybrid resin dispersion.In theory, this dispersion results in a residual solvent content of 6% by weight.It is conceivable to reduce the residual solvent content of this dispersion by diluting with additional water, which will correspondingly reduce the solid content of the dispersion.

[0133] Therefore, the process according to WO 2015 / 091901 cannot be used to achieve the dispersion according to the invention.

[0134] Performance Testing 1. Coating and curing methods 1.1 Method 1: Two-component isocyanate crosslinking Example dispersions E1-E15 were mixed with Bayhydur® 3100 in a 3:1 ratio and coated by a spiral coating bar onto Q-Panel® aluminum color test panels from Q-Lab (Alloy 3003H14; 0.025 inch thick (0.6 mm); bare mill finish). The wet film thickness is 100 μm. After drying for 24 hours at room temperature, the outcome is a clear, defect-free film with a dry film thickness of 50 μm. The test panels were aged for 10 days at 23° C. and 65% relative humidity.

[0135] 1.2 Method 2: Thermal crosslinking Example dispersions E16-E23 and E25-E30 were coated by a spiral coating bar onto Q-Panel® aluminum color test panels (Alloy 3003H14; 0.025 inch thick (0.6 mm); bare mill finish) from Q-Lab. The wet film thickness is 100 μm. After drying at room temperature for 0.5 hours, the outcome is a clear, defect-free film with a dry film thickness of 50 μm. After this flash-off time at room temperature, the air-dried test panels were baked at 250° C. for 15 minutes in an air-circulating oven.

[0136] Similarly, solvent-based SiPES 1, SiPES 2, SiPES 8, SiPES 9, and SiPES 12 were applied and cured.

[0137] 4. Measurement of pendulum hardness The films were characterized by the Konig pendulum hardness (DIN 53 157).

[0138] This value can be found in Table 6.

[0139] [Table 6]

[0140] It was found that the aqueous dispersions of the present invention have pendulum hardness values ​​that are just as good as solvent-based polyorganosiloxane hybrid resins. Pendulum hardness is important because it gives direct conclusions regarding the durability of the polyorganosiloxane hybrid resin dispersions according to the present invention in the final coating application.

Claims

1. An organic solvent, Component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight, of one or more polyorganosiloxanes of the general formula: R a Si(OR') b O (4-a-b/2) Formula (I) In this case, 0<a<2, 0<b<2, and a+b<4. Optionally, component B) 0 to 20 parts by weight, preferably 1 to 10 parts by weight, of one or more linear and / or branched polyorganosiloxanes of the formula R”O−[R’” 2 Si−O] n − Formula (II) Component C) 5 to 95 parts by weight, preferably 30 to 90 parts by weight, of an organic polymer; In these formulas, R a R', R", and R'" are each independently an alkyl group having 1 to 8 carbon atoms or an aromatic group having 6 to 20 carbon atoms, and n is a number ranging from 4 to 250; At least one polyorganosiloxane hybrid resin produced by the reaction of a composition comprising: and emulsifying a polyorganosiloxane hybrid resin solution comprising the above-mentioned with an emulsifier solution comprising at least one emulsifier based on partially hydrolyzed polyvinyl acetate, and removing the organic solvent. The dispersion has a solids content of 30.0% to 70.0% by weight, preferably 45.0% to 55.0% by weight, based on the polyorganosiloxane hybrid resin dispersion, and the residual solvent content of the organic solvent is <6.0% by weight, preferably <2.5% by weight, more preferably <1.0% by weight, based on the polyorganosiloxane hybrid resin dispersion; A method for producing an aqueous polyorganosiloxane hybrid resin dispersion.

2. The method for producing a polyorganosiloxane hybrid resin dispersion according to claim 1, characterized in that the organic polymer is selected from the group consisting of polyepoxides, polyesters, polyacrylates and / or methacrylates and copolymers thereof, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamideimides, polyimides, polyethers, aromatic and aliphatic glycidyl functional polymers, oligomers, phenoxy resins, polycarbonates, ketone-formaldehyde resins, and polyvinyl resins selected from polyvinyl alcohols, polyglycerols, polyvinyl acetates, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins, and mixtures thereof.

3. The method for producing a polyorganosiloxane hybrid resin dispersion according to claim 1 or 2, characterized in that the organic polymer contains a hydroxyl group and / or an acidic hydrogen.

4. The method for producing a polyorganosiloxane hybrid resin dispersion according to any one of claims 1 to 3, characterized in that the emulsifier is a partially hydrolyzed polyvinyl acetate having an alcoholysis level between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), more preferably between 70% and 90% (mol / mol).

5. The partially hydrolyzed polyvinyl acetate has a viscosity of 1 to 50 mPa s, preferably 1 to 40 mPa s, more preferably 1 to 30 mPa s, as measured at 20 ° C. according to DIN 53015 in a 4% aqueous polyvinyl acetate solution. The method for producing a polyorganosiloxane hybrid resin dispersion according to any one of claims 1 to 4.

6. The method for producing the polyorganosiloxane hybrid resin dispersion according to any one of claims 1 to 5, characterized in that it comprises a further emulsifier selected from the group of anionic, cationic, zwitterionic, or nonionic emulsifiers.

7. A method for producing a polyorganosiloxane hybrid resin dispersion described in any one of claims 1 to 6, characterized in that the flash point of the dispersion is >30.0°C, preferably >60.0°C, and more preferably >90.0°C.

8. A method for producing a polyorganosiloxane hybrid resin dispersion described in any one of claims 1 to 7, characterized in that the weight ratio of the polyorganosiloxane hybrid resin to the at least one emulsifier is between 5 and 50, preferably between 7 and 40, and more preferably between 10 and 30.

9. The method for producing a polyorganosiloxane hybrid resin dispersion according to any one of claims 1 to 8, further comprising an additive selected from antifoaming agents, degassing agents, rheology additives, preservatives, substrate wetting agents, crosslinking agents, drying aids, catalysts, antioxidants, antiskinning agents, antisettling agents, thickeners, coalescing agents, film-forming agents, fillers, pigments, and / or dispersants.

10. 10. The method for producing a polyorganosiloxane hybrid resin dispersion according to claim 9, characterized in that the preservative used is a fungicide, bactericide, insecticide, algaecide, and / or herbicide.

11. The average volume-weighted diameter of the particles of the polyorganosiloxane hybrid resin, as measured according to ISO 13320:2009, is between 0.1 and 10.0 μm, preferably between 0.1 and 2.0 μm, more preferably between 0.2 and 1.0 μm, and most preferably between 0.2 and 0.7 μm. The method for producing a polyorganosiloxane hybrid resin dispersion according to any one of claims 1 to 10, characterized in that the average volume-weighted diameter of the particles of the polyorganosiloxane hybrid resin, as measured according to ISO 13320:2009, is between 0.1 and 2.0 μm, more preferably between 0.2 and 1.0 μm, and most preferably between 0.2 and 0.7 μm.

12. The method for producing a polyorganosiloxane hybrid resin dispersion liquid according to any one of claims 1 to 11, characterized in that the organic solvent is a solvent selected from the group consisting of a ketone selected from methyl ethyl ketone, acetone, methyl isobutyl ketone, diethyl ketone, methyl propyl ketone, cyclohexanone, or methylcyclohexanone, an ester selected from ethyl acetate, butyl acetate, ethyl propionate, isobutyl acetate, tert-butyl acetate, or ethyl isobutyrate, a carbonate, a cyclic carbonate, an aromatic hydrocarbon, a cyclic hydrocarbon, a crown ether or ether, an ester ether, a siloxane, and an organometallic germanium compound, or a mixture of one or more of these solvents.

13. A method for producing a polyorganosiloxane hybrid resin dispersion described in any one of claims 1 to 12, characterized in that the organic solvent has a boiling point range of 50 to 150°C, preferably 90°C to 120°C.

14. The method for producing a polyorganosiloxane hybrid resin dispersion according to any one of claims 1 to 13, characterized in that the organic solvent is removed by vacuum distillation with or without a stripping gas, by steam distillation, or by a membrane process, a thin film evaporator, or a countercurrent process.

15. The method for producing a polyorganosiloxane hybrid resin dispersion described in any one of claims 1 to 14, characterized in that the polyorganosiloxane hybrid resin solution has a polyorganosiloxane hybrid resin concentration of 40.0 to 95.0 weight %, preferably 60.0 to 70.0 weight %, relative to the polyorganosiloxane hybrid resin solution.

Citation Information

Patent Citations

  • process for the production of stable emulsions of crosslinkable, high-viscosity organopolysiloxanes

    DE2158348A1

  • Process for preparing aqueous silicone emulsions

    DE4415322A1

  • Process for manufacturing aqueous compositions containing an organosilicon compound

    EP0098940A2

  • JP1973064138A

  • Preparattion of polyester-modified silicone resin

    JP1995053723A