Rinse composition for silicon wafers

The use of alkyl polyglucosides with a specific degree of condensation in a rinsing agent composition addresses the issue of LPD and silica adhesion on silicon wafers, improving the quality of semiconductor substrates by reducing light point defects.

JP7569677B2Active Publication Date: 2024-10-18KAO CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020209559
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-17
Publication Date
2024-10-18
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing polishing liquid compositions for silicon wafers fail to sufficiently reduce light point defects (LPD) due to silica adhesion and decreased wettability caused by amphiphilic polymers and alkyl polyglucosides with inadequate degrees of condensation, which are used in semiconductor manufacturing.

Method used

A rinsing agent composition containing alkyl polyglucosides with an average degree of condensation of 1.9 or more, combined with water, is used to rinse polished silicon wafers, improving wettability and reducing LPD.

Benefits of technology

The composition effectively reduces LPD on silicon wafer surfaces by minimizing silica adhesion and enhancing wettability, facilitating the production of high-quality semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569677000001
    Figure 0007569677000001
Patent Text Reader

Abstract

To provide a rinsing agent composition capable of reducing LPD on a polished silicon wafer surface.SOLUTION: A rinsing agent composition is used for rinsing the surface of a polished silicon wafer containing component A and component B: the component A being alkyl polyglucoside with an average degree of condensation of 1.9 or higher; and the component B being water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a rinse agent composition used for rinsing the surface of a polished silicon wafer, as well as a rinsing method and a method for manufacturing a semiconductor substrate using the same. [Background technology]

[0002] In recent years, the design rules for semiconductor devices have become finer due to the increasing demand for higher storage capacity of semiconductor memories. As a result, the depth of focus in photolithography used in the manufacturing process of semiconductor devices has become shallower, and the demand for reducing surface defects (LPD: Light point defects) and surface roughness (Haze) of silicon wafers (bare wafers) has become increasingly strict.

[0003] The polishing process for polishing silicon wafers to improve their quality includes the lapping (rough polishing) process, which flattens the silicon wafers obtained by slicing silicon single crystal ingots into thin disks, and the finish polishing process, which mirror-finishes the surface of the lapped silicon wafer after etching it.The finish polishing process, which is carried out in the final stage of polishing, is particularly aimed at suppressing haze and reducing LPD such as particles, scratches, and pits by improving the wettability (hydrophilicity) of the polished silicon wafer surface.

[0004] For example, Patent Documents 1 and 2 propose polishing liquid compositions containing an amphiphilic polymer such as hydroxyethyl cellulose (HEC) or cationized polyvinyl alcohol (PVA) and an alkyl polyglucoside (AG) for the purpose of reducing surface roughness and LPD. Furthermore, Patent Document 3 proposes an immersion cleaner for silicon wafers for solar cells that uses alkyl polyglucoside (AG) for the purpose of reducing residues on the substrate surface. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-105954 A [Patent Document 2] JP 2017-155198 A [Patent Document 3] JP 2012-248738 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the polishing liquid compositions proposed in Patent Documents 1 and 2, the amphiphilic polymer causes a large amount of silica to adhere to the silicon wafer surface, and thus LPD is not sufficiently reduced. Furthermore, when an alkyl polyglucoside (AG) with an average condensation degree of 1.3-1.7 used in the examples of Patent Document 1 is used in the rinsing process of semiconductor silicon wafers, the wettability of the silicon wafer surface decreases, and LPD is not sufficiently reduced. Patent Document 3 does not disclose the use of alkyl polyglucosides (AG) in the rinsing process of semiconductor silicon wafers. In addition, when alkyl polyglucosides (AG) with average condensation degrees of 1.2 and 1.8 used in the examples of the document are used in the rinsing process of semiconductor silicon wafers, the reduction in LPD is not sufficient.

[0007] Therefore, the present disclosure provides a rinse agent composition capable of reducing LPD on a polished silicon wafer surface, as well as a rinsing method and a method for manufacturing a semiconductor substrate using the rinse agent composition. [Means for solving the problem]

[0008] In one aspect, the present disclosure relates to a rinse agent composition used for rinsing a polished surface of a silicon wafer, comprising the following component A and the following component B: Component A: Alkyl polyglucoside with an average condensation degree of 1.9 or more Component B: Water

[0009] In one aspect, the present disclosure relates to a method for rinsing a polished silicon wafer, comprising the step of rinsing a polished silicon wafer with a rinse agent composition of the present disclosure.

[0010] In one aspect, the present disclosure relates to a method for producing a semiconductor substrate, the method including the following steps (1), (2), and (3): (1) A step of polishing a silicon wafer to be polished with a polishing composition containing abrasive grains. (2) A step of rinsing the silicon wafer polished in step (1) with the rinse agent composition of the present disclosure. (3) A step of cleaning the silicon wafer rinsed in step (2). Effect of the Invention

[0011] According to the present disclosure, it is possible to provide a rinse agent composition capable of reducing LPD on the surface of a polished silicon wafer, as well as a rinsing method and a method for manufacturing a semiconductor substrate that use the rinse agent composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present disclosure is based on the discovery that by rinsing the surface of a polished silicon wafer with an alkyl polyglucoside having a specific condensation degree, the wettability of the wafer surface can be improved and LPD can be reduced.

[0013] That is, in one aspect, the present disclosure relates to a rinse agent composition (hereinafter also referred to as the "rinse agent composition of the present disclosure") used for rinsing a surface of a polished silicon wafer, the rinse agent composition containing the following component A and the following component B: Component A: Alkyl polyglucoside with an average condensation degree of 1.9 or more Component B: Water

[0014] According to one or more embodiments of the present disclosure, LPD on a polished surface of a silicon wafer can be reduced.

[0015] Although the details of the mechanism by which the effects of the present disclosure are manifested are not clear, it is presumed as follows. It is known that cleaning with a surfactant that has both hydrophobic and hydrophilic groups is effective in removing organic matter and abrasive particles such as silica particles that are adsorbed on the hydrophobic surface of silicon wafers. However, if the hydrophilic group of the surfactant is short, the wettability of the wafer surface after rinsing is poor, and if the surface becomes hydrophobic, silica particles tend to adhere to the silicon wafer surface, which is thought to cause recontamination at the silicon wafer interface. In contrast, in the rinsing step using the rinse agent composition of the present disclosure, it is presumed that the number of silica particles remaining on the wafer surface is reduced by modifying the silicon wafer surface to a sufficiently hydrophilic surface using an alkyl polyglucoside (component A) having a specific condensation degree. Therefore, it is presumed that the amount of residual silica particles on the polished silicon wafers subjected to the cleaning step can be significantly reduced, and the reduction in LPD of the silicon wafers is realized. However, the present disclosure need not be construed as being limited to these mechanisms.

[0016] [Alkyl polyglucoside (ingredient A)] The alkyl polyglucoside (hereinafter also referred to as "Component A") contained in the rinse agent composition of the present disclosure is an alkyl polyglucoside having an average condensation degree of 1.9 or more. Component A may be one type or a combination of two or more types. In one or more embodiments, Component A is preferably a compound represented by the following general formula (I). R-Gy (I) In the formula (I), R represents an alkyl group having 8 to 18 carbon atoms, G represents a residue derived from a sugar, and y represents the average degree of condensation of the sugar and is a number between 1.9 and 5.

[0017] In the above formula (I), R is an alkyl group having 8 to 18 carbon atoms from the viewpoint of reducing LPD. From the viewpoint of reducing LPD, the number of carbon atoms in the alkyl group is preferably 8 or more, more preferably 10 or more, and from the viewpoint of storage stability, it is preferably 18 or less, more preferably 16 or less, even more preferably 14 or less, even more preferably 12 or less, and even more preferably 10 or less. Therefore, from the viewpoint of reducing LPD and improving wettability, the number of carbon atoms in the alkyl group is preferably 8 to 16, more preferably 8 to 14, and even more preferably 10 to 12. R may be a straight chain or a branched chain.

[0018] In the above formula (I), G is a residue derived from a sugar from the viewpoint of reducing LPD, for example, a residue derived from glucose. From the viewpoint of reducing LPD, the average condensation degree y is 1.9 or more, preferably 2 or more, more preferably 2.1 or more, even more preferably 2.2 or more, even more preferably 2.3 or more, even more preferably 2.4 or more, even more preferably 2.5 or more, even more preferably 2.6 or more, even more preferably 2.7 or more, and 5 or less, preferably 4 or less, more preferably 3.5 or less, even more preferably 3.4 or less, even more preferably 3.3 or less, even more preferably 3.2 or less, even more preferably 3.1 or less, and even more preferably 3.0 or less. The average condensation degree is the average value of the residue derived from a sugar, and can be measured by nuclear magnetic resonance spectroscopy (NMR). Specifically, it can be measured by the method described in the Examples.

[0019] Component A can be produced, for example, by reacting a sugar with an excess of alcohol in the presence of an acid catalyst, and then distilling off the unreacted alcohol from the reaction solution after the reaction. For example, it can be produced by a method in which a sugar is reacted with an excess of alcohol in the presence of an acid catalyst, an inorganic acid salt is added to the reaction solution containing an alkyl polyglycoside and the unreacted alcohol, and then the unreacted alcohol is distilled off.

[0020] The proportion of the alkyl glycoside with a degree of condensation of 1 contained in Component A is preferably 10% or more, more preferably 20% or more, still more preferably 30% or more, still more preferably 40% or more, and preferably 70% or less, more preferably 60% or less, still more preferably 50% or less, from the viewpoints of reducing LPD and wettability. The measurement method of the alkyl glycoside with a degree of condensation of 1 can be measured by NMR, similar to the above-mentioned average degree of condensation.

[0021] The content of Component A in the rinse composition of the present disclosure is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, still more preferably 0.05% by mass or more, and, from the same viewpoints, preferably 1% by mass or less, more preferably 0.5% by mass or less, still more preferably 0.1% by mass or less, from the viewpoints of improving wettability and reducing LPD. When Component A is a combination of two or more kinds, the content of Component A means their total content. In the present disclosure, 1% by mass is 10,000 ppm by mass.

[0022] [Water (Component B)] The rinse composition of the present disclosure contains water (hereinafter also referred to as "Component B") as a medium. Examples of Component B include distilled water, ion-exchanged water, pure water, ultrapure water, and the like. The content of Component B in the rinse composition of the present disclosure can be the remainder excluding Component A and optional components described later.

[0023] [Optional Component (Auxiliary Agent)] The rinse composition of the present disclosure can further contain at least one optional component selected from a pH adjuster, a preservative, alcohols, a chelating agent, an anionic surfactant, a nonionic surfactant, and an oxidizing agent, as long as the effects of the present disclosure are not impaired.

[0024] [pH Adjuster]< Examples of the pH adjuster include basic compounds, acidic compounds, and their salts. The salt of the acidic compound is preferably at least one selected from alkali metal salts, ammonium salts, and amine salts, and more preferably ammonium salts. When the basic compound is in the form of a salt, the counter ion is preferably at least one selected from hydroxide ions, chloride ions, and iodide ions, and more preferably at least one selected from hydroxide ions and chloride ions.

[0025] (Basic compounds) Examples of basic compounds include sodium hydroxide, potassium hydroxide, ammonia, ammonium hydroxide, ammonium carbonate, ammonium hydrogen carbonate, methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-methyl-N,N-diethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-dibutylethanolamine, N-(β-aminoethyl)ethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, ethylenediamine, hexamethylenediamine, piperazine hexahydrate, anhydrous piperazine, 1-(2-aminoethyl)piperazine, N-methylpiperazine, diethylenetriamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and tetrabutylammonium hydroxide. Two or more of these basic compounds may be used. As the basic compound, ammonia is more preferable from the viewpoint of achieving both reduction in haze and LPD of the silicon wafer and improvement in the storage stability of the rinse agent composition.

[0026] (acidic compound) Examples of the acidic compound include inorganic acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, and organic acids such as acetic acid, oxalic acid, succinic acid, glycolic acid, malic acid, citric acid, and benzoic acid.

[0027] <Preservatives> Examples of preservatives include benzalkonium chloride, benzethonium chloride, 1,2-benzisothiazolin-3-one, (5-chloro-)2-methyl-4-isothiazolin-3-one, hydrogen peroxide, and hypochlorite.

[0028] <Alcoholic drinks> Examples of the alcohols include methanol, ethanol, propanol, butanol, isopropyl alcohol, 2-methyl-2-propanool, ethylene glycol, propylene glycol, polyethylene glycol, glycerin, etc. The content of the alcohols in the rinse agent composition of the present invention is preferably 0.01% by mass to 10% by mass.

[0029] <Chelating agent> Examples of the chelating agent include ethylenediaminetetraacetic acid, sodium ethylenediaminetetraacetate, nitrilotriacetic acid, sodium nitrilotriacetate, ammonium nitrilotriacetate, hydroxyethylethylenediaminetriacetic acid, sodium hydroxyethylethylenediaminetriacetate, triethylenetetraminehexaacetic acid, sodium triethylenetetraminehexaacetate, etc. The content of the chelating agent in the rinse composition of the present invention is preferably 0.01 to 1% by weight.

[0030] <Anionic surfactants> Examples of the anionic surfactant include fatty acid soaps, carboxylates such as alkyl ether carboxylates, sulfonates such as alkylbenzenesulfonates and alkylnaphthalenesulfonates, sulfates such as higher alcohol sulfates, and phosphates such as alkyl phosphates.

[0031] <Nonionic surfactant> Examples of nonionic surfactants include polyethylene glycol-type surfactants such as polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbit fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, and polyoxyalkylene (hydrogenated) castor oil; polyhydric alcohol-type surfactants such as sucrose fatty acid esters; and fatty acid alkanolamides.

[0032] <Oxidizing agent> The oxidizing agent includes peroxides such as permanganic acid and peroxoacid, chromic acid, nitric acid, and salts thereof.

[0033] In one or more embodiments, the rinse agent composition of the present disclosure preferably contains substantially no abrasive grains from the viewpoint of reducing LPD. For example, the content of abrasive grains in the rinse agent composition of the present disclosure is preferably 0.1 mass % or less, more preferably 0.01 mass % or less, and even more preferably substantially 0 mass %.

[0034] [pH of rinse agent composition] The pH of the rinse agent composition of the present disclosure at 25°C is preferably 2 or more, more preferably 2.5 or more, even more preferably 3 or more, even more preferably 3.5 or more, even more preferably 4 or more, and from the same viewpoints, is preferably 12 or less, more preferably 10 or less, even more preferably 9 or less, even more preferably 8 or less, even more preferably 7 or less, and even more preferably 6.5 or less. The pH can be adjusted by appropriately adding a pH adjuster as necessary. Here, the pH at 25°C can be measured using a pH meter, specifically, by the method described in the Examples.

[0035] [Method of producing rinse agent composition] The rinse agent composition of the present disclosure can be produced, for example, by a production method including a step of blending component A, component B, and optional components as required by a known method. In the present disclosure, "blending" includes mixing component A, component B, and optional components as required simultaneously or in any order. The blending can be performed using a mixer such as a homomixer, a homogenizer, an ultrasonic disperser, or a wet ball mill. The preferred blending amount of each component in the production method of the rinse agent composition of the present disclosure can be the same as the preferred content of each component in the rinse agent composition of the present disclosure described above.

[0036] In the present disclosure, "the content of each component in the rinse agent composition" refers to the content of each component at the time of use of the rinse agent composition, i.e., at the time when the rinse agent composition is used for rinsing treatment.

[0037] [Concentrated rinse agent composition] The rinse agent composition of the present disclosure may be stored and supplied in a concentrated state to the extent that its storage stability is not impaired. In this case, it is preferable in that the manufacturing and transportation costs can be further reduced. The concentrated solution of the rinse agent composition of the present disclosure may be used by diluting it with water as appropriate so that the content of each component is the above-mentioned content of each component when used. The concentration ratio is not particularly limited as long as the concentration during polishing after dilution can be secured, but is preferably 2 times or more, more preferably 10 times or more, and even more preferably 20 times or more from the viewpoint of further reducing the manufacturing and transportation costs.

[0038] When the rinse agent composition of the present disclosure is in the form of a concentrate, the content of component A in the concentrate of the rinse agent composition of the present disclosure is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, from the viewpoint of reducing production and transportation costs, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of improving storage stability.

[0039] When the rinse agent composition of the present disclosure is in the form of a concentrate, the pH of the concentrate of the rinse agent composition of the present disclosure at 25° C. is preferably 1.5 or more, more preferably 1.7 or more, even more preferably 2 or more, and is preferably 12 or less, more preferably 11 or less, even more preferably 10 or less.

[0040] [Method of manufacturing semiconductor substrate] In one or a plurality of embodiments, the rinse agent composition of the present disclosure is used for removing residues remaining on the surface of a silicon wafer after polishing with a polishing liquid composition containing abrasive grains. In one or a plurality of embodiments, the rinse agent composition of the present disclosure is used in a rinsing step after a polishing step of a silicon wafer in the manufacturing process of a semiconductor substrate. That is, in one aspect, the present disclosure relates to a method for producing a semiconductor substrate (hereinafter also referred to as the "semiconductor substrate producing method of the present disclosure"), which includes the following steps (1), (2), and (3): (1) A step of polishing a silicon wafer to be polished using a polishing composition containing abrasive grains (hereinafter also referred to as a "polishing step"). (2) A step of rinsing the silicon wafer polished in step (1) (hereinafter also referred to as the "polished silicon wafer") with the rinse agent composition of the present disclosure (hereinafter also referred to as the "rinsing step"). (3) A step of cleaning the silicon wafer rinsed in the step (2) (hereinafter also referred to as a "rinsed silicon wafer") (hereinafter also referred to as a "cleaning step").

[0041] <Silicon wafer to be polished> Examples of the silicon wafer to be polished include single crystal 100-face silicon wafers, 111-face silicon wafers, 110-face silicon wafers, etc. From the viewpoint of reducing residues on the wafer surface, the resistivity of the silicon wafer is preferably 0.0001 Ω·cm or more, more preferably 0.001 Ω·cm or more, even more preferably 0.01 Ω·cm or more, even more preferably 0.1 Ω·cm or more, and is preferably 100 Ω·cm or less, more preferably 50 Ω·cm or less, even more preferably 20 Ω·cm or less. From a similar viewpoint, the resistivity of the silicon wafer is preferably 0.0001 Ω·cm or more and 100 Ω·cm or less, more preferably 0.001 Ω·cm or more and 100 Ω·cm or less, even more preferably 0.01 Ω·cm or more and 100 Ω·cm or less, even more preferably 0.1 Ω·cm or more and 100 Ω·cm or less, even more preferably 0.1 Ω·cm or more and 50 Ω·cm or less, and even more preferably 0.1 Ω·cm or more and 20 Ω·cm or less.

[0042] <Process (1): Polishing process> The polishing step includes a lapping (rough polishing) step of planarizing a silicon wafer obtained by slicing a silicon single crystal ingot into a thin disk shape, and a finish polishing step of etching the lapped silicon wafer and then mirror-finishing the silicon wafer surface. The rinse composition of the present disclosure is more preferably used after the finish polishing step.

[0043] In the polishing step, for example, the silicon substrate to be polished can be pressed against a platen to which a polishing pad is attached, and the silicon substrate to be polished can be polished at a polishing pressure of 3 to 20 kPa. The polishing pressure refers to the pressure of the platen applied to the surface of the silicon substrate to be polished during polishing. In the polishing step, for example, the silicon substrate to be polished can be pressed against a platen to which a polishing pad is attached, and the silicon substrate to be polished can be polished at a temperature of the polishing liquid composition and the surface temperature of the polishing pad of preferably 15°C or higher, more preferably 20°C or higher, and preferably 40°C or lower, more preferably 30°C or lower.

[0044] The polishing agent composition used in the polishing step contains silica particles, although it is not particularly limited. Examples of silica particles include colloidal silica, fumed silica, pulverized silica, and silica obtained by surface modification of these. From the viewpoints of improving the polishing rate, reducing surface roughness (haze), and reducing surface defects (LPD) on the wafer surface, colloidal silica is preferred. The silica particles may be one type or a combination of two or more types. The content of the silica particles in the polishing agent composition may be, for example, 0.05% by mass or more and 10% by mass or less. The polishing agent composition preferably contains a nonionic water-soluble polymer, more preferably a nonionic water-soluble polymer having an alkylene oxide group or a hydroxyl group in the molecule and a weight average molecular weight of 1,000 or more and less than 500,000, from the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD). In the present disclosure, "water-soluble" means having a solubility of 0.5 g / 100 mL or more in water (20°C), preferably a solubility of 2 g / 100 mL or more. When the nonionic polymer has an alkylene oxide group in the molecule, examples of the alkylene oxide group include an ethylene oxide group and a propylene oxide group. From the viewpoint of achieving an improvement in the polishing rate, a reduction in surface roughness (haze), and a reduction in surface defects (LPD), the nonionic polymer may be at least one selected from polyglycerin, hydroxyalkyl cellulose, polyvinyl alcohol, and polyhydroxyethyl acrylamide. From the viewpoint of achieving both improved removal rate and storage stability, the pH of the polishing composition is preferably greater than 8.5, more preferably 9 or more, even more preferably 9.5 or more, and even more preferably 10 or more, and from the viewpoint of improving surface quality, the pH is preferably 14 or less, more preferably 13 or less, even more preferably 12.5 or less, even more preferably 12 or less, even more preferably 11.5 or less, and even more preferably 11 or less. The polishing composition contains water as a medium, and the content of water in the polishing composition can be the balance of the abrasive grains, the nonionic polymer, and optional components described below. In one or more embodiments, the polishing composition may contain optional components such as a water-soluble polymer, a basic compound, a pH adjuster, a preservative, an alcohol, and a chelating agent.

[0045] <Step (2): Rinse step> In the rinsing step, for example, the rinse agent composition of the present disclosure is supplied between the silicon wafer polished in step (1) (hereinafter also referred to as "polished silicon wafer") and a pad, and the pad is moved relative to the polished silicon wafer while the polished silicon wafer and the pad are in contact with each other. The rinsing process in the rinsing step can be performed using a polishing device used in the polishing step. The rotation speed of the pad, the rotation speed of the polished silicon wafer, the load set on the polishing device equipped with the pad, the supply speed of the rinse agent composition of the present disclosure, and the like may be the same as or different from the corresponding conditions in the polishing step. The rinsing time is preferably 1 second or more, more preferably 3 seconds or more, from the viewpoint of suppressing adhesion of abrasive grains, and is preferably 60 seconds or less, more preferably 30 seconds or less, from the viewpoint of improving productivity. Here, the rinsing time means the time during which the rinse agent composition is supplied.

[0046] The rinsing step may include a water rinse treatment using water as a rinse liquid prior to the rinsing treatment using the rinse agent composition of the present disclosure. The water rinse treatment time is preferably 2 seconds or more and 30 seconds or less.

[0047] The pad used in the rinsing step may be the same as the pad used in the polishing step, and may be any type such as a nonwoven type or a suede type. The pad used in the polishing step may be used in the rinsing step as it is without being replaced, and in this case, the pad may contain a small amount of abrasive grains of the polishing composition. The rinsing step may also be performed on the silicon wafer while it is still attached to the polishing device immediately after the polishing step.

[0048] The temperature of the rinse agent composition used in the rinsing step may be, for example, 5 to 60°C.

[0049] The rinsing step is preferably carried out at least after the finish polishing step, but may be carried out after each of the rough polishing step and the finish polishing step.

[0050] <Step (3): Cleaning step> In the cleaning step, for example, the silicon wafer rinsed in step (2) (hereinafter also referred to as "rinsed silicon wafer") is immersed in a cleaning agent, or the cleaning agent is sprayed onto the surface of the rinsed silicon wafer to be cleaned. Any conventionally known cleaning agent may be used as the cleaning agent, and examples of such cleaning agents include inorganic cleaning agents containing at least one selected from ozone, hydrogen peroxide, ammonia, hydrochloric acid, sulfuric acid, hydrofluoric acid, and ozone water. The cleaning time may be set depending on the cleaning method.

[0051] The semiconductor substrate manufacturing method of the present disclosure may further include a step of forming an element isolation film, a step of planarizing an interlayer insulating film, a step of forming metal wiring, and the like.

[0052] [Silicon wafer rinsing method] In one aspect, the present disclosure relates to a method for rinsing a silicon wafer (hereinafter also referred to as the "rinsing method of the present disclosure") including a step (rinsing step) of rinsing a polished silicon wafer with the rinse agent composition of the present disclosure. The rinse step in the rinsing method of the present disclosure can be performed in the same manner as the rinse step (2) in the semiconductor substrate manufacturing method of the present disclosure described above. According to the rinsing method of the present disclosure, since the rinse agent composition of the present disclosure is used, the amount of abrasive grains remaining on the silicon wafer after polishing can be significantly reduced, and in addition, the aggregation of the abrasive grains can be suppressed, so that the time for cleaning the silicon wafer performed after the rinsing process can be shortened and LPD can be reduced. EXAMPLES

[0053] The present disclosure will be described in more detail below with reference to examples, but these are merely illustrative and the present disclosure is not limited to these examples.

[0054] 1.Measuring methods for various parameters [Average condensation degree of alkyl polyglucoside] The average degree of condensation of alkyl polyglucosides (AG) was calculated by the method described below after removing polysaccharides by solid phase extraction under the conditions described below. (solid phase extraction) After conditioning with methanol and ion-exchanged water, the sample (2 mL) was charged, and the sugar components were eluted with an aqueous acetonitrile solution (5 wt %: 10 mL), and then the AG components were eluted with methanol (10 mL). Column: InertSep C18 2000mg (GL Science) Sample: 2wt% (dissolved in 5wt% acetonitrile aqueous solution)

[0055] (Method for calculating average degree of condensation) The average degree of condensation of the alkyl polyglucoside used in the preparation of the rinse composition was measured by nuclear magnetic resonance spectroscopy (NMR) under the following conditions after solid phase extraction, and calculated based on the peaks in the obtained chart. Equipment: Mercury400BB (400 MHz, Varian) Observation width: 6410.3Hz Data points: 64K Pulse width: 45 μS Pulse delay time: 10 seconds Number of times accumulated: 64 Measurement temperature: room temperature Spin: x16 Solvent: pyridine-d5 (a few drops of D2O) Condensation degree calculation method: Degree of condensation = {[(number of protons adjacent to oxygen atoms appearing between 3.5 and 5.3 ppm) / (number of protons in alkyl moieties appearing between 0 and 2.0 ppm)]-2} / 7

[0056] [pH of rinse agent composition] The pH values ​​of the rinse agent composition and its concentrate at 25°C were measured using a pH meter ("HM-30G" manufactured by DKK-TOA Corporation) and were measured one minute after the electrode of the pH meter was immersed in the rinse agent composition or its concentrate.

[0057] 2. Preparation of Rinse Agent Compositions (Examples 1 to 6 and Comparative Examples 1 to 3) The alkyl polyglucoside (component A or non-component A) shown in Table 1 and ion-exchanged water were mixed with stirring, and the pH at 25°C was adjusted to 4 using an aqueous hydrochloric acid solution or 28% by mass ammonia water (special grade reagent, Kishida Chemical Co., Ltd.) as necessary, to obtain concentrated solutions (concentration ratio: 20 times) of the rinse agent compositions of Examples 1 to 6 and Comparative Examples 1 to 3. The content of component A or non-component A shown in Table 1 is the value for the rinse agent composition obtained by diluting the concentrated solution by 20 times. The content of ion-exchanged water is the remainder excluding alkyl polyglucoside (component A or non-component A), hydrochloric acid, or ammonia.

[0058] Details of the alkyl polyglucosides (Component A or non-Component A) used in preparing each rinse agent composition are shown in Table 1 and below. (Component A) A1: Alkyl polyglucoside [straight-chain alkyl group with 10 carbon atoms, average sugar condensation degree 2.1] A2: Alkyl polyglucoside [straight-chain alkyl group with 10 carbon atoms, average sugar condensation degree 2.7] A3: Alkyl polyglucoside [straight-chain alkyl group with 12 carbon atoms, average sugar condensation degree 2.1] A4: Alkyl polyglucoside [straight-chain alkyl group with 12 carbon atoms, average sugar condensation degree 2.3] A5: Alkyl polyglucoside [straight-chain alkyl group with 10 carbon atoms, average sugar condensation degree 3.4] A6: Alkyl polyglucoside [straight-chain alkyl group with 12 carbon atoms, average sugar condensation degree 2.9] (Non-ingredient A) A7: Alkyl polyglucoside [branched alkyl group with 10 carbon atoms, average sugar condensation degree 1.3] A8: Alkyl polyglucoside [straight-chain alkyl group with 9 carbon atoms, average sugar condensation degree 1.5] A9: Alkyl polyglucoside [straight-chain alkyl group with 9 carbon atoms, average sugar condensation degree 1.6]

[0059] (Method of synthesizing alkyl glycosides) The alkyl polyglycoside was produced by reacting a sugar with an excess of alcohol in the presence of an acid catalyst, adding an inorganic acid salt to the reaction solution containing the alkyl polyglycoside and unreacted alcohol, and then distilling off the unreacted alcohol.

[0060] 3. Rinse method The rinse composition (concentrate) was diluted 20 times with ion-exchanged water to obtain a rinse composition (pH 5). The rinse composition was filtered with a filter (Advantec Co., Ltd. compact cartridge filter "MCP-LX-C10S") just before the start of the rinse process, and rinsed on the following silicon wafers (single-sided mirror-finished silicon wafers with a diameter of 200 mm (conductivity type: P, crystal orientation: 100, resistivity 0.1 Ω·cm or more and less than 100 Ω·cm) under the following rinse conditions. Prior to the rinse process, the silicon wafers were preliminarily coarsely polished using a commercially available polishing composition. Then, finish polishing was performed under the following conditions, and immediately thereafter, rinse treatment was performed using each rinse composition under the following conditions. The haze of the silicon wafers subjected to finish polishing after the completion of the coarse polishing was 2.680 (ppm). The haze was measured using a KLA Tencor "Surfscan SP1-DLS" in a dark-field wide grazing incidence channel (DWO).

[0061] [Polishing composition used in finish polishing] The polishing liquid composition used for the final polishing was prepared by stirring and mixing silica particles ("PL-3" manufactured by Fuso Chemical Co., Ltd.), HEC (hydroxyethyl cellulose, "SE-400" manufactured by Daicel Corporation, weight average molecular weight 250,000), PEG (polyethylene glycol, "PEG6000" manufactured by Wako Pure Chemical Industries, Ltd., Wako Grade 1, weight average molecular weight 6,000), ammonia water (manufactured by Kishida Chemical Co., Ltd., special grade reagent), and ion-exchanged water to prepare a concentrated liquid. The concentrated liquid was then diluted 40 times with ion-exchanged water immediately before use to obtain a polishing liquid composition for final polishing. The content of each component in the polishing liquid composition for final polishing was 0.17% by mass for silica particles, 0.01% by mass for HEC, 0.01% by mass for ammonia, and 0.0008% by mass for PEG. The pH of the polishing liquid composition for final polishing was 10.

[0062] [Finishing polishing conditions] Grinding machine: Okamoto Kogyo's single-sided 8-inch grinding machine "GRIND-X SPP600s" Polishing pad: Suede pad manufactured by Toray Coatex (Asker hardness: 64, thickness: 1.37 mm, nap length: 450 μm, opening diameter: 60 μm) Silicon wafer polishing pressure: 100g / cm 2 Plate rotation speed: 60 rpm Polishing time: 5 minutes Supply rate of polishing composition: 150 g / min Temperature of the polishing composition: 23°C Carrier rotation speed: 60 rpm

[0063] [Rinse conditions] Grinding machine: Okamoto Kogyo's single-sided 8-inch grinding machine "GRIND-X SPP600s" Polishing pad: Suede pad manufactured by Toray Coatex (Asker hardness: 64, thickness: 1.37 mm, nap length: 450 μm, opening diameter: 60 μm) Silicon wafer resiliency pressure: 60g / cm 2 Plate rotation speed: 30 rpm Rinse time: 20 seconds Rinse composition feed rate: 1000 mL / min Rinse composition temperature: 23°C Carrier rotation speed: 30 rpm

[0064] 4. Cleaning method After the rinsing process, the silicon wafer was subjected to ozone cleaning and dilute hydrofluoric acid cleaning as follows. In the ozone cleaning, an aqueous solution containing 20 ppm ozone was sprayed from a nozzle toward the center of the silicon wafer rotating at 600 rpm at a flow rate of 1 L / min for 3 minutes. The temperature of the ozone water was kept at room temperature. Next, dilute hydrofluoric acid cleaning was performed. In the dilute hydrofluoric acid cleaning, an aqueous solution containing 0.5 mass% ammonium hydrogen fluoride (special grade: Nacalai Tesque, Inc.) was sprayed from a nozzle toward the center of the silicon wafer rotating at 600 rpm at a flow rate of 1 L / min for 5 seconds. The above ozone cleaning and dilute hydrofluoric acid cleaning were performed as one set, for a total of two sets, and finally spin drying was performed. In the spin drying, the silicon wafer was rotated at 1500 rpm.

[0065] 5. Evaluation [Evaluation of LPD on silicon wafers] The LPD of the silicon wafer surfaces after cleaning was evaluated by measuring the number of particles with a particle size of 45 nm or more on the silicon wafer surface using a surface roughness measuring device "Surfscan SP1-DLS" (KLA Tencor). The smaller the LPD evaluation result, the fewer the surface defects. LPD measurements were performed on four silicon wafers each, and the average values ​​for each are shown in the table below. In addition, in Comparative Examples 1 to 3, the number of particles was so large that it was impossible to measure.

[0066] [Evaluation of wettability of silicon wafer surface (wet area of ​​silicon wafer)] As a pretreatment, a silicon wafer cut into a 40×40 mm square was immersed in a 1% dilute hydrofluoric acid solution for 3 minutes to remove the oxide film, then washed with ultrapure water for 10 seconds and dried by air blowing. After that, the wafer was polished for 5 minutes using the same polishing composition as that used in the above-mentioned finish polishing, rinsed with ultrapure water for 10 seconds, and then rinsed for 20 seconds using each of the rinse agent compositions described above. After that, the silicon wafer was immersed in a tub filled with ultrapure water, and after 10 seconds of pulling it out, the area of ​​the hydrophilized part when the silicon wafer was fixed horizontally was calculated by image analysis. The area of ​​the hydrophilized part was calculated by image analysis when the entire surface of the silicon wafer was wetted. <Evaluation criteria> A: 100% B: More than 80% but less than 100% C: 80% or less

[0067] [Table 1]

[0068] As shown in Table 1 above, it was found that the rinse compositions of Examples 1 to 6 were able to reduce LPD on the polished silicon wafer surface, compared to the rinse compositions of Comparative Examples 1 to 3. [Industrial Applicability]

[0069] The rinse agent composition of the present disclosure can reduce LPD on the polished silicon wafer surface, and therefore can produce silicon wafers with reduced surface defects, making it useful in mass production of semiconductor substrates.

Claims

1. A rinse agent composition used for rinsing a polished surface of a silicon wafer, comprising the following component A and component B: Component A: an alkyl polyglucoside having an average condensation degree of 1.9 or more, represented by the following general formula (I): Component B: Water R-Gy (I) In the formula (I), R represents an alkyl group having 8 to 18 carbon atoms, G represents a residue derived from a sugar, and y represents the average degree of condensation of the sugar and is a number ranging from 1.9 to 5.

2. 2. The rinse agent composition according to claim 1, wherein the proportion of alkyl glycosides having a condensation degree of 1 contained in component A is 20% or more.

3. 3. The rinse agent composition according to claim 1, which is substantially free of abrasive grains.

4. A method for rinsing a polished silicon wafer, comprising a step of rinsing a polished silicon wafer with the rinse agent composition according to any one of claims 1 to 3.

5. A method for manufacturing a semiconductor substrate, comprising the following steps (1), (2), and (3): (1) A step of polishing a silicon wafer to be polished using a polishing composition containing abrasive grains. (2) A step of rinsing the silicon wafer polished in the step (1) with the rinse agent composition according to any one of claims 1 to 3. (3) A step of cleaning the silicon wafer rinsed in the step (2).

Citation Information

Patent Citations

  • Production of Alkyl Polyglycosides

    JP1995500322A

  • Cleansing agent composition

    JP1996060182A

  • Detergent composition for wafer or plate-like material

    JP2009040828A

  • Method of cleaning semiconductor wafers

    JP2010226089A

  • Method of manufacturing semiconductor device, polishing method, and apparatus for manufacturing semiconductor

    JP2011071285A