Process release film, its uses, and method for manufacturing resin-encapsulated semiconductors using the same
A laminated film with specific thermal dimensional control and water contact angle properties addresses the issue of wrinkles in mold release films, ensuring high releasability and mold followability for defect-free semiconductor encapsulation.
Patent Information
- Application Number
- JP2023076115
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-05-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2035-12-03
AI Technical Summary
Conventional mold release films for semiconductor encapsulation processes suffer from wrinkles and poor mold followability, leading to defects in the molded products due to thermal dimensional mismatch between the film and the mold.
A laminated film comprising a release layer with a water contact angle of 90° to 130° and a heat-resistant resin layer with a thermal dimensional change rate of 3% or less in the transverse direction from 23°C to 120°C or 170°C, ensuring minimal thermal expansion and contraction, thereby suppressing wrinkles.
The film achieves high mold releasability, effective wrinkle suppression, and excellent mold followability, allowing for defect-free resin-sealed semiconductor products with improved productivity.
Smart Images

Figure 0007569882000003 
Figure 0007569882000004 
Figure 0007569882000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a process release film, preferably a process release film for semiconductor encapsulation, and in particular to a process release film that is placed between a semiconductor chip or the like and the inner surface of a mold when a semiconductor chip or the like is placed in the mold and resin is injected for molding, and a method for manufacturing a resin-encapsulated semiconductor using the same. [Background technology]
[0002] In recent years, along with the trend toward smaller and lighter semiconductor packages, etc., it has been considered to reduce the amount of encapsulating resin used. In order to ensure strong adhesion at the interface between the semiconductor chip, etc. and the resin even when the amount of encapsulating resin used is reduced, it is desirable to reduce the amount of release agent contained in the encapsulating resin. For this reason, a method of arranging a release film between the inner surface of the mold and the semiconductor chip, etc., has been adopted as a method for obtaining releasability between the encapsulating resin and the mold after curing and molding.
[0003] As such a release film, fluororesin films (e.g., Patent Documents 1-2), poly4-methyl-1-pentene resin films (e.g., Patent Document 3), etc., which have excellent releasability and heat resistance, have been proposed. However, these release films have the problem that they are prone to wrinkles when attached to the inner surface of a mold, and these wrinkles are transferred to the surface of the molded product, causing poor appearance.
[0004] In response to this, a laminated release film having a release layer and a heat-resistant layer has been proposed. These release films aim to obtain releasability through the release layer and suppress wrinkles through the heat-resistant layer. Representative of these proposals is one that focuses on the relationship between the storage modulus of the release layer and the heat-resistant layer (see, for example, Patent Documents 4 and 5). For example, Patent Document 4 describes a laminated release film having a configuration in which the storage modulus of the release layer is relatively low and the storage modulus of the heat-resistant layer is relatively high, more specifically, a release film for semiconductor encapsulation process in which the storage modulus E' of the release layer at 175°C is 45 MPa or more and 105 MPa or less, and the storage modulus E' of the heat-resistant layer at 175°C is 100 MPa or more and 250 MPa or less. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-310336 A [Patent Document 2] JP 2002-110722 A [Patent Document 3] JP 2002-361643 A [Patent Document 4] JP 2010-208104 A [Patent Document 5] International Publication No. 2015 / 133631 A1 Brochure Summary of the Invention [Problem to be solved by the invention]
[0006] However, with the development of this technical field, the requirements for process release films such as release films for semiconductor encapsulation processes are increasing year by year, and there is a demand for process release films that suppress the occurrence of wrinkles even under more severe process conditions. In particular, there is a strong demand for process release films that have a higher level of balance between releasability, wrinkle suppression, and mold followability.
[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a process release film that allows a molded article after resin encapsulation to be easily released from the mold regardless of the mold structure or amount of release agent, and that allows a molded article to be obtained that is free of appearance defects such as wrinkles or chips. [Means for solving the problem]
[0008] As a result of extensive research into solving the above problems, the inventors have discovered that appropriately controlling the thermal dimensional change rate of a process release film at a specific temperature, in particular the thermal dimensional change rate in the TD direction (a direction within the plane of the film that is perpendicular to the longitudinal direction during the production of the film; hereinafter also referred to as the "transverse direction") of the laminated film that constitutes the process release film, is important in preventing wrinkles when the film is attached to the inner surface of a mold, and have thus completed the present invention. That is, the present invention and each aspect thereof are as described below in [1] to
[19] .
[0009] [1] A process release film which is a laminated film including a release layer A and a heat-resistant resin layer B, The contact angle of the release layer A with respect to water (hereinafter, the "contact angle with respect to water" may be referred to as the "water contact angle") is from 90° to 130°, The release film for process use, wherein the heat-resistant resin layer B has a thermal dimensional change rate in the transverse (TD) direction from 23° C. to 120° C. of 3% or less. [2] The process release film according to [1], wherein the sum of the thermal dimensional change rate in the transverse (TD) direction of the laminate film from 23°C to 120°C and the thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 120°C is 6% or less. [3] A process release film which is a laminated film including a release layer A and a heat-resistant resin layer B, The contact angle of the release layer A with respect to water is 90° to 130°, The release film for process use, wherein the heat-resistant resin layer B has a thermal dimensional change rate in the transverse (TD) direction from 23° C. to 170° C. of 4% or less. [4] The process release film according to [3], wherein the sum of the thermal dimensional change rate in the transverse (TD) direction of the laminate film from 23°C to 170°C and the thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 170°C is 7% or less. [5] The release film for process use according to any one of [1] to [4], wherein the heat-resistant resin layer B has a thermal dimensional change rate in a transverse (TD) direction from 23° C. to 120° C. of 3% or less. [6] The release film for process according to [5], wherein the sum of the thermal dimensional change rate of the heat-resistant resin layer B in the transverse (TD) direction from 23°C to 120°C and the thermal dimensional change rate of the heat-resistant resin layer B in the longitudinal (MD) direction from 23°C to 120°C is 6% or less. [7] The release film for process use according to any one of [1] to [4], wherein the heat-resistant resin layer B has a thermal dimensional change rate in a transverse (TD) direction from 23° C. to 170° C. of 3% or less. [8] The heat-resistant resin layer B has a sum of a thermal dimensional change rate in the transverse (TD) direction from 23°C to 170°C and a thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 120°C of 4% or less. [9] The release film for process use according to any one of [1] to [8], wherein the release layer A contains a resin selected from the group consisting of a fluororesin, a 4-methyl-1-pentene (co)polymer, and a polystyrene-based resin.
[10] The release film for process use according to any one of [1] to [9], wherein the heat-resistant resin layer B comprises a stretched film.
[11] The release film for process use according to
[10] , wherein the stretched film is selected from the group consisting of a stretched polyester film, a stretched polyamide film, and a stretched polypropylene film.
[12] The release film for process use according to any one of [1] to
[11] , wherein the heat of crystalline fusion of the heat-resistant resin layer B in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JIS K7221 is 15 J / g or more and 60 J / g or less.
[13] The laminated film further has a release layer A', and contains the release layer A, the heat-resistant resin layer B, and the release layer A' in this order, The release film for process use according to any one of [1] to
[12] , wherein the contact angle of the release layer A' with water is from 90° to 130°.
[14] At least one of the release layer A and the release layer A' contains a resin selected from the group consisting of a fluororesin, a 4-methyl-1-pentene (co)polymer, and a polystyrene-based resin.
[15] The release film for process according to any one of [1] to
[14] , which is used in a sealing process using a thermosetting resin.
[16] The release film for process according to any one of [1] to
[15] , which is used in a semiconductor encapsulation process.
[17] The release film for process according to any one of [1] to
[15] , which is used in a fiber-reinforced plastic molding process or a plastic lens molding process.
[18] A method for manufacturing a resin-encapsulated semiconductor device, comprising the steps of: A step of placing a semiconductor device to be resin-encapsulated at a predetermined position in a molding die; A step of disposing the release film for semiconductor encapsulation process according to any one of [1] to
[14] on an inner surface of the molding die such that the release layer A faces the semiconductor device; After clamping the molding die, a step of injecting an encapsulation resin between the semiconductor device and the release film for semiconductor encapsulation process; The method for producing the resin-encapsulated semiconductor device according to claim 1,
[19] A method for manufacturing a resin-encapsulated semiconductor device, comprising the steps of: A step of placing a semiconductor device to be resin-encapsulated at a predetermined position in a molding die; A step of disposing the release film for semiconductor encapsulation process according to
[13] or
[14] on an inner surface of the molding die such that the release layer A' faces the semiconductor device; After clamping the molding die, a step of injecting an encapsulation resin between the semiconductor device and the release film for semiconductor encapsulation process; The method for producing the resin-encapsulated semiconductor device according to claim 1, Effect of the Invention
[0010] The process release film of the present invention has a high level of releasability, wrinkle suppression, and mold followability that could not be achieved by conventional techniques. Therefore, by using this film, molded products obtained by resin encapsulation of semiconductor chips or the like can be easily released from the mold, and molded products without appearance defects such as wrinkles or chips can be produced with high productivity. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a release film for process use according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing another example of the release film for process of the present invention. [Diagram 3] 1 is a schematic diagram showing an example of a method for producing a resin-encapsulated semiconductor using a process release film of the present invention. FIG. [Figure 4A] 1 is a schematic diagram showing an example of a method for producing a resin-encapsulated semiconductor using a process release film of the present invention. FIG. [Figure 4B] 1 is a schematic diagram showing an example of a method for producing a resin-encapsulated semiconductor using a process release film of the present invention. FIG. [Diagram 5] 4C is a schematic diagram showing an example of a resin-sealed semiconductor obtained by the method for producing a resin-sealed semiconductor shown in FIG. 4A and FIG. 4B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Process release film The release film for process of the present invention includes the following four aspects. (First aspect) A process release film which is a laminated film including a release layer A and a heat-resistant resin layer B, The contact angle of the release layer A with respect to water is 90° to 130°, The release film for process use, wherein the thermal dimensional change rate of the laminated film in the transverse (TD) direction from 23°C to 120°C is 3% or less. (Second aspect) A process release film which is a laminated film including a release layer A and a heat-resistant resin layer B, The contact angle of the release layer A with respect to water is 90° to 130°, The release film for process use, wherein the thermal dimensional change rate of the laminated film in the transverse (TD) direction from 23°C to 170°C is 4% or less. (Third aspect) A process release film which is a laminated film including a release layer A, a heat-resistant resin layer B, and a release layer A' in this order, The contact angle of the release layer A and the release layer A' with respect to water is 90° to 130°, The release film for process use, wherein the thermal dimensional change rate of the laminated film in the transverse (TD) direction from 23°C to 120°C is 3% or less. (Fourth aspect) A process release film which is a laminated film including a release layer A, a heat-resistant resin layer B, and a release layer A' in this order, The contact angle of the release layer A and the release layer A' with respect to water is 90° to 130°, The release film for process use, wherein the thermal dimensional change rate of the laminated film in the transverse (TD) direction from 23°C to 170°C is 4% or less.
[0013] As is clear from the above aspects, the process release film of the present invention (hereinafter also simply referred to as "release film") is a laminated film comprising a release layer A having releasability against molded articles and molds, and optionally a release layer A', and a heat-resistant resin layer B supporting the release layer.
[0014] The process release film of the present invention is disposed on the inner surface of a molding die when a semiconductor element or the like is resin-sealed inside the molding die. At this time, it is preferable to dispose the release layer A of the release film (or the release layer A' if a release layer A' exists) on the side of the semiconductor element or the like (molded product) to be resin-sealed. By disposing the release film of the present invention, the resin-sealed semiconductor element or the like can be easily released from the die. The contact angle of the release layer A with water is 90° to 130°. Due to having such a contact angle, the release layer A has low wettability and does not adhere to the hardened sealing resin or the mold surface, allowing the molded product to be easily released from the mold. The contact angle of the release layer A to water is preferably from 95° to 120°, more preferably from 98° to 115°, and even more preferably from 100° to 110°.
[0015] As described above, since the release layer A (or the release layer A' in some cases) is disposed on the molded product side, it is preferable to suppress the occurrence of wrinkles in the release layer A (or the release layer A' in some cases) during the resin sealing step. This is because there is a high possibility that the wrinkles that occur will be transferred to the molded product, causing defects in the appearance of the molded product.
[0016] In the present invention, in order to achieve the above-mentioned object, a laminate film constituting a process release film is used which includes a release layer A (and optionally a release layer A') and a heat-resistant resin layer B supporting the release layer, and whose thermal dimensional change rate in the transverse (TD) direction shows a specific value. That is, a laminate film including release layer A (and release layer A' if desired) and heat-resistant resin layer B supporting the release layer has a thermal dimensional change rate of 3% or less in the TD direction (horizontal direction) from 23°C to 120°C, or a thermal dimensional change rate of 4% or less in the TD direction (horizontal direction) from 23°C to 170°C. Furthermore, it is more preferable that the laminate film has a thermal dimensional change rate of 3% or less in the TD direction (horizontal direction) from 23°C to 120°C and a thermal dimensional change rate of 4% or less in the TD direction (horizontal direction) from 23°C to 170°C. When the thermal dimensional change rate of the laminated film in the TD direction (horizontal direction) from 23° C. to 120° C. is 3% or less, or when the thermal dimensional change rate of the laminated film in the TD direction (horizontal direction) from 23° C. to 170° C. is 4% or less, the occurrence of wrinkles in the release layer in a resin sealing process, etc. The mechanism by which the occurrence of wrinkles in the release layer is suppressed by using a laminated film that shows the above-mentioned specific value of thermal dimensional change rate in the lateral (TD) direction as a component of the process release film is not necessarily clear, but it is presumed to be related to the fact that the use of a laminated film with relatively small thermal expansion / contraction suppresses the thermal expansion / contraction of the release layer A (or release layer A') due to heating / cooling during processing.
[0017] The laminated film constituting the process release film of the present invention preferably has a thermal dimensional change rate in its TD direction (transverse direction) of 2.5% or less from 23° C. to 120° C., more preferably 2.0% or less, and even more preferably 1.5% or less. On the other hand, the laminated film preferably has a thermal dimensional change rate in its TD direction (transverse direction) of -5.0% or more from 23° C. to 120° C. The laminated film constituting the process release film of the present invention preferably has a thermal dimensional change rate in its TD direction (transverse direction) of 3.5% or less from 23° C. to 170° C., more preferably 3.0% or less, and even more preferably 2.0% or less. On the other hand, the laminated film preferably has a thermal dimensional change rate in its TD direction (transverse direction) of -5.0% or more from 23° C. to 170° C.
[0018] The mechanism by which the use of a resin layer whose thermal dimensional change rate in the transverse (TD) direction exhibits the above-mentioned specific value as heat-resistant resin layer B more effectively suppresses the occurrence of wrinkles in the release layer is not entirely clear; however, it is presumed to be related to the fact that the use of a heat-resistant resin layer B with relatively small thermal expansion / contraction suppresses the thermal expansion / contraction of release layer A (or release layer A') due to heating / cooling during processing.
[0019] The process release film of the present invention, which is a laminated film containing a release layer A (and optionally a release layer A'), and a heat-resistant resin layer B supporting the release layer, preferably has a sum of the thermal dimensional change rate in the TD direction (horizontal direction) and the thermal dimensional change rate in the MD direction (the longitudinal direction during the production of the film; hereinafter also referred to as the "longitudinal direction") of a specific value or less. In other words, it is preferable that the sum of the thermal dimensional change rate of the above-mentioned laminated film in the transverse direction (TD) from 23°C to 120°C and the thermal dimensional change rate of the laminated film in the longitudinal direction (MD) from 23°C to 120°C is 6% or less, while it is preferable that the sum of the thermal dimensional change rate of the laminated film in the TD direction (transverse direction) from 23°C to 120°C and the thermal dimensional change rate of the laminated film in the longitudinal direction (MD) from 23°C to 120°C is -5.0% or more. By having the sum of the thermal dimensional change rate in the transverse (TD) direction from 23°C to 120°C and the thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 120°C of the laminated film including release layer A (and release layer A' if desired), and heat-resistant resin layer B, be 6% or less, the occurrence of wrinkles when attached to the inner surface of a mold can be more effectively suppressed.
[0020] In addition, it is preferable that the sum of the thermal dimensional change rate in the transverse direction (TD) from 23°C to 170°C and the thermal dimensional change rate in the longitudinal direction (MD) from 23°C to 170°C of the laminated film including the release layer A (and release layer A' if desired), and the heat-resistant resin layer B is 7% or less, while it is preferable that the sum of the thermal dimensional change rate in the TD direction (transverse direction) from 23°C to 170°C and the thermal dimensional change rate in the longitudinal direction (MD) from 23°C to 170°C of the laminated film is -5.0% or more. By having the sum of the thermal dimensional change rate in the transverse (TD) direction from 23°C to 170°C of the above-mentioned laminated film and the thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 170°C be 7% or less, the occurrence of wrinkles when attached to the inner surface of a mold can be more effectively suppressed.
[0021] Release layer A The release layer A constituting the process release film of the present invention has a contact angle with water of 90° to 130°, preferably 95° to 120°, more preferably 98° to 115°, and even more preferably 100° to 110°. In view of excellent releasability of molded articles and ease of availability, it preferably contains a resin selected from the group consisting of fluororesins, 4-methyl-1-pentene (co)polymers, and polystyrene-based resins.
[0022] The fluororesin that can be used in the release layer A may be a resin containing a structural unit derived from tetrafluoroethylene. It may be a homopolymer of tetrafluoroethylene, but may also be a copolymer with other olefins. Examples of other olefins include ethylene. A preferred example is a copolymer containing tetrafluoroethylene and ethylene as monomer structural units, and in such a copolymer, the proportion of structural units derived from tetrafluoroethylene is preferably 55 to 100% by mass, and the proportion of structural units derived from ethylene is preferably 0 to 45% by mass.
[0023] The 4-methyl-1-pentene (co)polymer that can be used in the release layer A may be a homopolymer of 4-methyl-1-pentene, or a copolymer of 4-methyl-1-pentene with another olefin having 2 to 20 carbon atoms (hereinafter referred to as "olefin having 2 to 20 carbon atoms").
[0024] In the case of a copolymer of 4-methyl-1-pentene and an olefin having 2 to 20 carbon atoms, the olefin having 2 to 20 carbon atoms copolymerized with 4-methyl-1-pentene is 4-methyl-1-pentene. It is possible to impart flexibility to the ethylene-1-pentene. Examples of olefins having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-eicosene, etc. These olefins may be used alone or in combination of two or more.
[0025] In the case of a copolymer of 4-methyl-1-pentene and an olefin having 2 to 20 carbon atoms, it is preferable that the ratio of the structural units derived from 4-methyl-1-pentene is 96 to 99% by mass, and the ratio of the other structural units derived from an olefin having 2 to 20 carbon atoms is 1 to 4% by mass. By reducing the content of the structural units derived from an olefin having 2 to 20 carbon atoms, the copolymer can be made hard, that is, the storage modulus E' can be increased, which is advantageous for suppressing the occurrence of wrinkles in a sealing process, etc. On the other hand, by increasing the content of the structural units derived from an olefin having 2 to 20 carbon atoms, the copolymer can be made soft, that is, the storage modulus E' can be decreased, which is advantageous for improving mold conformability.
[0026] The 4-methyl-1-pentene (co)polymer can be produced by a method known to those skilled in the art. For example, it can be produced by a method using a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst. The 4-methyl-1-pentene (co)polymer is preferably a (co)polymer having high crystallinity. The crystalline copolymer may be either a copolymer having an isotactic structure or a copolymer having a syndiotactic structure, but a copolymer having an isotactic structure is particularly preferable in terms of physical properties and is also easy to obtain. Furthermore, the 4-methyl-1-pentene (co)polymer can be molded into a film and has strength to withstand the temperature, pressure, etc. during molding in a mold, so long as it has no particular restriction on stereoregularity or molecular weight. The 4-methyl-1-pentene copolymer may be a commercially available copolymer, such as TPX (registered trademark) manufactured by Mitsui Chemicals, Inc.
[0027] Polystyrene-based resins that can be used for the release layer A include styrene homopolymers and copolymers, and the styrene-derived structural units contained in the polymer preferably account for at least 60% by weight, more preferably 80% by weight or more. The polystyrene resin may be isotactic polystyrene or syndiotactic polystyrene, but isotactic polystyrene is preferred from the viewpoints of transparency, availability, etc., and syndiotactic polystyrene is preferred from the viewpoints of releasability, heat resistance, etc. One type of polystyrene may be used alone, or two or more types may be used in combination.
[0028] It is preferable that the release layer A has heat resistance capable of withstanding the temperature of the mold during molding (typically 120 to 180° C.) From this viewpoint, it is preferable that the release layer A contains a crystalline resin having a crystalline component, and the melting point of the crystalline resin is preferably 190° C. or higher, and more preferably 200° C. or higher and 300° C. or lower. In order to impart crystallinity to the release layer A, for example, a fluororesin preferably contains at least a structural unit derived from tetrafluoroethylene, a 4-methyl-1-pentene (co)polymer preferably contains at least a structural unit derived from 4-methyl-1-pentene, and a polystyrene resin preferably contains at least syndiotactic polystyrene. By containing a crystalline component in the resin constituting the release layer A, wrinkles are less likely to occur during the resin sealing process, etc., and this is suitable for suppressing the wrinkles from being transferred to the molded product and causing poor appearance.
[0029] The resin containing the crystalline component constituting the release layer A preferably has a crystalline fusion heat of 15 J / g or more and 60 J / g or less, more preferably 20 J / g or more and 50 J / g or less, in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JISK7221. If it is 15 J / g or more, it is possible to more effectively exhibit heat resistance and releasability that can withstand hot press molding in the resin sealing step, etc., and the dimensional change rate can also be suppressed, so that the occurrence of wrinkles can be prevented. On the other hand, if the crystalline fusion heat is 60 J / g or less, the release layer A has an appropriate hardness, so that the film can have sufficient followability to the mold in the resin sealing step, etc., and there is no risk of damage to the film.
[0030] The release layer A may further contain other resins in addition to the fluororesin, 4-methyl-1-pentene copolymer, and / or polystyrene resin. In this case, it is preferable that the other resins have a relatively high hardness. Examples of the other resins include polyamide-6, polyamide-66, polybutylene terephthalate, and polyethylene terephthalate. In this way, even if the release layer A contains a large amount of soft resin (for example, a large amount of olefin having 2 to 20 carbon atoms in 4-methyl-1-pentene copolymer), the release layer A can be hardened by further containing a resin having a relatively high hardness, which is advantageous in suppressing the occurrence of wrinkles in the sealing process, etc.
[0031] The content of these other resins is preferably, for example, 3 to 30% by mass with respect to the resin components constituting the release layer A. By making the content of the other resins 3% by mass or more, the effect of adding them can be substantial, and by making it 30% by mass or less, the releasability from a mold or a molded product can be maintained.
[0032] Furthermore, in addition to the fluororesin, 4-methyl-1-pentene (co)polymer, and / or polystyrene-based resin, the release layer A may contain known additives that are generally blended into resins for films, such as a heat stabilizer, a weather stabilizer, an anti-rust agent, a copper-damage stabilizer, an antistatic agent, etc., within a range that does not impair the object of the present invention. The content of these additives can be, for example, 0.0001 to 10 parts by weight per 100 parts by weight of the fluororesin, 4-methyl-1-pentene copolymer, and / or polystyrene-based resin.
[0033] The thickness of the release layer A is not particularly limited as long as it provides sufficient releasability for the molded article, but it is usually 1 to 50 μm, and preferably 5 to 30 μm.
[0034] The surface of the release layer A may have an uneven shape as required, thereby improving the release property. The method for imparting the unevenness to the surface of the release layer A is not particularly limited, but may be Common methods such as embossing can be used.
[0035] Release layer A' The release film for process use of the present invention may further have a release layer A' in addition to the release layer A and the heat-resistant resin layer B. That is, the release film for process use of the present invention may be a laminated film including the release layer A, the heat-resistant resin layer B, and the release layer A' in this order. The contact angle of the release layer A', which may constitute the process release film of the present invention, to water is 90° to 130°, preferably 95° to 120°, more preferably 98° to 115°, and even more preferably 100° to 110°. The preferred materials, configuration, physical properties, etc. of the release layer A' are the same as those explained for the release layer A above.
[0036] When the process release film is a laminated film containing a release layer A, a heat-resistant resin layer B, and a release layer A' in that order, the release layer A and the release layer A' may be layers of the same composition or layers of different compositions. From the standpoint of preventing warping and ease of handling due to the fact that both sides have similar release properties, it is preferable that release layer A and release layer A' have the same or approximately the same configuration. However, from the standpoint of optimally designing release layer A and release layer A' in relation to the process in which they are used, for example, by making release layer A have excellent releasability from a mold and release layer A' have excellent peelability from a molded product, it is preferable that release layer A and release layer A' have different configurations. When the release layer A and the release layer A' have different configurations, the release layer A and the release layer A' may be made of the same material but have different configurations such as thickness, or the material and other configurations may be different.
[0037] Heat-resistant resin layer B The heat-resistant resin layer B constituting the process release film of the present invention has the function of supporting the release layer A (and optionally the release layer A') and suppressing the occurrence of wrinkles due to the mold temperature or the like. In the process release film of the present invention, it is preferable that the heat-resistant resin layer B has a thermal dimensional change rate of 3% or less in the transverse (TD) direction from 23° C. to 120° C., or the heat-resistant resin layer B has a thermal dimensional change rate of 3% or less in the transverse (TD) direction from 23° C. to 170° C. Furthermore, it is more preferable that the heat-resistant resin layer B has a thermal dimensional change rate of 3% or less in the transverse (TD) direction from 23° C. to 120° C. and a thermal dimensional change rate of 3% or less in the transverse (TD) direction from 23° C. to 170° C. The heat-resistant resin layer B may be any resin layer including a non-stretched film, but it is particularly preferable that the heat-resistant resin layer B comprises a stretched film. Stretched films tend to have a low or negative coefficient of thermal expansion due to the effect of stretching in the manufacturing process, and it is relatively easy to achieve the property that the thermal dimensional change rate in the transverse (TD) direction from 23°C to 120°C is 3% or less, or the thermal dimensional change rate in the transverse (TD) direction of the heat-resistant resin layer B is 3% or less from 23°C to 170°C, and therefore can be suitably used as the heat-resistant resin layer B. The thermal dimensional change rate of the heat-resistant resin layer B in the transverse (TD) direction from 23°C to 120°C is preferably 2% or less, more preferably 1.5% or less, and even more preferably 1% or less, while it is preferably -10% or more. The thermal dimensional change rate of the heat-resistant resin layer B in the transverse (TD) direction from 23°C to 170°C is preferably 2% or less, more preferably 1.5% or less, and even more preferably 1% or less, while it is preferably -10% or more.
[0038] The stretched film may be a uniaxially stretched film or a biaxially stretched film. In the case of a uniaxially stretched film, it may be stretched either longitudinally or transversely, but it is preferable that the film is stretched at least in the transverse (TD) direction. There are no particular limitations on the method and apparatus for obtaining the stretched film, and the film may be stretched by a method known in the art, for example, by using a heated roll or a tenter type stretching machine.
[0039] The stretched film is preferably a stretched film selected from the group consisting of a stretched polyester film, a stretched polyamide film, and a stretched polypropylene film. These stretched films are particularly suitable as the stretched film in the heat-resistant resin layer B because the coefficient of thermal expansion in the transverse (TD) direction can be relatively easily reduced or made negative by stretching, the mechanical properties are suitable for the application of the present invention, and they are relatively easy to obtain at low cost.
[0040] As the stretched polyester film, a stretched polyethylene terephthalate (PET) film or a stretched polybutylene terephthalate (PBT) film is preferred, and a biaxially stretched polyethylene terephthalate (PET) film is particularly preferred. The polyamide constituting the stretched polyamide film is not particularly limited, but polyamide-6, polyamide-66, etc. can be preferably used. As the stretched polypropylene film, a uniaxially stretched polypropylene film, a biaxially stretched polypropylene film, etc. can be preferably used. There is no particular limitation on the stretching ratio, and it is sufficient to appropriately set an appropriate value so as to appropriately control the thermal dimensional change rate and realize favorable mechanical properties. For example, in the case of a stretched polyester film, it is preferable that the stretching ratio is in the range of 2.7 to 8.0 times in both the longitudinal and transverse directions, and in the case of a stretched polyamide film, it is preferable that the stretching ratio is in the range of 2.7 to 5.0 times in both the longitudinal and transverse directions. In the case of a stretched polypropylene film, it is preferable that the stretching ratio is in the range of 5.0 to 10.0 times in both the longitudinal and transverse directions for a biaxially stretched polypropylene film, and it is preferable that the stretching ratio is in the range of 1.5 to 10.0 times in the longitudinal direction for a uniaxially stretched polypropylene film.
[0041] From the viewpoint of controlling the strength of the film and its thermal dimensional change rate within an appropriate range, the heat-resistant resin layer B preferably has heat resistance capable of withstanding the temperature of the mold during molding (typically 120 to 180°C). From this viewpoint, the heat-resistant resin layer B preferably contains a crystalline resin having a crystalline component, and the melting point of the crystalline resin is preferably 125°C or higher, more preferably 155°C or higher and 300°C or lower, further preferably 185°C or higher and 210°C or lower, and particularly preferably 185°C or higher and 205°C or lower.
[0042] As described above, it is preferable that the heat-resistant resin layer B contains a crystalline resin having a crystalline component. As the crystalline resin contained in the heat-resistant resin layer B, for example, a crystalline resin such as a polyester resin, a polyamide resin, or a polypropylene resin can be used in part or in whole. Specifically, it is preferable to use polyethylene terephthalate or polybutylene terephthalate as the polyester resin, polyamide 6 or polyamide 66 as the polyamide resin, and isotactic polypropylene as the polypropylene resin.
[0043] By including the crystalline component of the crystalline resin in the heat-resistant resin layer B, wrinkles are less likely to occur during the resin sealing process and the like, which is advantageous in preventing wrinkles from being transferred to the molded product and causing poor appearance. The resin constituting the heat-resistant resin layer B has a crystal fusion heat of 20 J / g or more and 100 J / g or less in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JISK7221, more preferably 25 J / g or more and 65 J / g or less, more preferably 25 J / g or more and 55 J / g or less, more preferably 28 J / g or more and 50 J / g or less, more preferably 28 J / g or more and 40 J / g or less, and even more preferably 28 J / g or more and 35 J / g or less. If it is 20 J / g or more, it is possible to effectively express heat resistance and releasability that can withstand hot press molding in the resin sealing step, etc., and the dimensional change rate can be suppressed to a small extent, so that the occurrence of wrinkles can be prevented. On the other hand, when the heat of crystalline fusion is 100 J / g or less, an appropriate hardness can be imparted to the heat-resistant resin layer B, so that sufficient conformability of the film to the mold can be ensured in the resin sealing process, etc., and the film is not likely to be easily damaged. In this embodiment, the heat of crystalline fusion refers to a value calculated by summing up the areas of peaks having peaks at 120°C or higher in a chart showing the relationship between the heat quantity (J / g) on the vertical axis and the temperature (°C) on the horizontal axis obtained in the first heating step in measurement by differential scanning calorimetry (DSC) in accordance with JIS K7221. The heat of crystal fusion of the heat-resistant resin layer B can be adjusted by appropriately setting the heating and cooling conditions and the stretching conditions during the production of the film.
[0044] The thickness of the heat-resistant resin layer B is not particularly limited as long as the film strength can be ensured. 00 μm, preferably 5 to 50 μm.
[0045] Other layers The process release film of the present invention may have layers other than the release layer A, the heat-resistant resin layer B, and the release layer A', so long as they do not deviate from the object of the present invention. For example, an adhesive layer may be provided between the release layer A (or the release layer A') and the heat-resistant resin layer B, as necessary. The material used for the adhesive layer is not particularly limited as long as it can firmly bond the release layer A and the heat-resistant resin layer B and does not peel off during the resin sealing step or the release step.
[0046] For example, when the release layer A (or the release layer A') contains a 4-methyl-1-pentene copolymer, the adhesive layer is preferably a modified 4-methyl-1-pentene copolymer resin graft-modified with an unsaturated carboxylic acid or the like, an olefin adhesive resin consisting of a 4-methyl-1-pentene copolymer and an α-olefin copolymer, or the like. When the release layer A (or the release layer A') contains a fluororesin, the adhesive layer is preferably a polyester-based, acrylic-based, fluororubber-based, or other adhesive. The thickness of the adhesive layer is not particularly limited as long as it can improve the adhesion between the release layer A (or the release layer A') and the heat-resistant resin layer B, but is, for example, 0.5 to 10 μm.
[0047] The total thickness of the process release film of the present invention is not particularly limited, but is preferably, for example, 10 to 300 μm, and more preferably 30 to 150 μm. If the total thickness of the release film is within the above range, the handling property when used as a roll is good, and the amount of the film to be discarded is small, which is preferable.
[0048] A preferred embodiment of the process release film of the present invention will be described in more detail below. Fig. 1 is a schematic diagram showing an example of a process release film having a three-layer structure. As shown in Fig. 1, the release film 10 has a heat-resistant resin layer 12 and a release layer 16 formed on one side thereof with an adhesive layer 14 interposed therebetween.
[0049] The release layer 16 is the aforementioned release layer A, the heat-resistant resin layer 12 is the aforementioned heat-resistant resin layer B, and the adhesive layer 14 is the aforementioned adhesive layer. The release layer 16 is preferably disposed on the side that comes into contact with the encapsulating resin in the encapsulating process; the heat-resistant resin layer 12 is preferably disposed on the side that comes into contact with the inner surface of the mold in the encapsulating process.
[0050] Fig. 2 is a schematic diagram showing an example of a process release film having a five-layer structure. The same reference numerals are used for components having the same functions as those in Fig. 1. As shown in Fig. 2, the release film 20 has a heat-resistant resin layer 12 and release layers 16A and 16B formed on both sides of the heat-resistant resin layer 12 with an adhesive layer 14 interposed therebetween. The release layer 16A is the aforementioned release layer A, the heat-resistant resin layer 12 is the aforementioned heat-resistant resin layer B, the release layer 16B is the aforementioned release layer A', and the adhesive layer 14 is each of the aforementioned adhesive layers.
[0051] The compositions of the release layers 16A and 16B may be the same or different. The thicknesses of the release layers 16A and 16B may also be the same or different. However, if the release layers 16A and 16B have the same composition and thickness, they will have a symmetrical structure, which is preferable because the release film itself is less likely to warp. In particular, since the release film of the present invention may be subjected to stress due to heating in the sealing process, it is preferable to suppress warping. In this way, if the release layers 16A and 16B are formed on both sides of the heat-resistant resin layer 12, good releasability can be obtained both in the molded product and on the inner surface of the mold, which is preferable.
[0052] Method for manufacturing process release film The process release film of the present invention can be produced by any method. For example, there are 1) a method of producing a process release film by laminating the release layer A and the heat-resistant resin layer B by co-extrusion molding (co-extrusion method), 2) a method of producing a process release film by applying and drying a molten resin of the resin to be the release layer A or the adhesive layer on a film to be the heat-resistant resin layer B, or applying and drying a resin solution in which the resin to be the release layer A or the adhesive layer is dissolved in a solvent, (coating method), and 3) a method of producing a process release film by previously producing a film to be the release layer A and a film to be the heat-resistant resin layer B, and laminating (laminating) these films (lamination method).
[0053] In the method 3), the resin films can be laminated by any of various known lamination methods, such as extrusion lamination, dry lamination, and thermal lamination. In the dry lamination method, each resin film is laminated using an adhesive. As the adhesive, any adhesive known for dry lamination can be used. For example, polyvinyl acetate adhesives; polyacrylic ester adhesives made of homopolymers or copolymers of acrylic esters (ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, etc.), or copolymers of acrylic esters and other monomers (methyl methacrylate, acrylonitrile, styrene, etc.); cyanoacrylate adhesives; ethylene copolymer adhesives made of copolymers of ethylene and other monomers (vinyl acetate, ethyl acrylate, acrylic acid, methacrylic acid, etc.); cellulose adhesives; polyester adhesives; polyvinyl acetate adhesives; Adhesives that can be used include: amide adhesives; polyimide adhesives; amino resin adhesives made of urea resin or melamine resin; phenol resin adhesives; epoxy adhesives; polyurethane adhesives in which polyol (polyether polyol, polyester polyol, etc.) is crosslinked with isocyanate and / or isocyanurate; reactive (meth)acrylic adhesives; rubber adhesives made of chloroprene rubber, nitrile rubber, styrene-butadiene rubber, etc.; silicone adhesives; inorganic adhesives made of alkali metal silicate, low melting point glass, etc.; and others. The resin film to be laminated in method 3) may be a commercially available product, and may be any of a variety of adhesives that are available from a publicly-available company. The resin film may be manufactured by a known manufacturing method. The resin film may be subjected to a surface treatment such as a corona treatment, an atmospheric pressure plasma treatment, a vacuum plasma treatment, a primer coating treatment, etc. The manufacturing method of the resin film is not particularly limited, and a known manufacturing method can be used.
[0054] 1) The co-extrusion molding method is preferable in that defects caused by foreign matter being caught between the resin layer to be the release layer A and the resin layer to be the heat-resistant resin layer B, and warping of the release film are unlikely to occur. 3) The lamination method is a manufacturing method suitable for using a stretched film for the heat-resistant resin layer B. In this case, it is preferable to form an appropriate adhesive layer at the interface between the films as necessary. In order to increase the adhesion between the films, the interface between the films may be subjected to a surface treatment such as a corona discharge treatment as necessary.
[0055] The process release film may be uniaxially or biaxially stretched as necessary, which can increase the film strength.
[0056] The coating means in the above-mentioned 2) coating method is not particularly limited, but for example, various coaters such as a roll coater, a die coater, a spray coater, etc. The melt extrusion means is not particularly limited, but for example, an extruder having a T-type die or an inflation type die, etc., is used.
[0057] Manufacturing Process The process release film of the present invention can be used by being placed between a semiconductor chip or the like and the inner surface of a mold when a resin is injected into the mold after placing the semiconductor chip or the like in the mold. By using the process release film of the present invention, it is possible to effectively prevent problems such as poor release from the mold and the generation of burrs. The resin used in the above manufacturing process may be either a thermoplastic resin or a thermosetting resin, but in this technical field, thermosetting resins are widely used, and in particular, it is preferable to use an epoxy-based thermosetting resin. The most typical example of the above manufacturing process is the encapsulation of semiconductor chips, but the present invention is not limited to this, and can also be applied to fiber-reinforced plastic molding processes, plastic lens molding processes, and the like.
[0058] 3, 4A, and 4B are schematic diagrams showing an example of a method for producing a resin-encapsulated semiconductor using the release film of the present invention. As shown in FIG. 3a, the release film 1 of the present invention is supplied from a roll-shaped wound by rolls 1-2 and 1-3 into the molding die 2. Next, the release film 1 is placed on the inner surface of the upper die 2. If necessary, the inner surface of the upper die 2 may be evacuated to make the release film 1 adhere to the inner surface of the upper die 2. A semiconductor chip 6 arranged on a substrate is placed on the lower die 5 of the molding device, and a sealing resin is placed on the semiconductor chip 6 or a liquid sealing resin is injected to cover the semiconductor chip 6, so that the sealing resin 4 is accommodated between the upper die 2 and the lower die 5 on which the release film 1 is placed and adhered by exhaust and suction. Next, as shown in FIG. 3b, the upper die 2 and the lower die 5 are closed via the release film 1 of the present invention, and the sealing resin 4 is cured.
[0059] 3c, the sealing resin 4 flows into the mold and flows into the space, surrounding the sides of the semiconductor chip 6, and the encapsulated semiconductor chip 6 is removed by opening the upper mold 2 and the lower mold 5. After opening the mold and removing the molded product, the release film 1 can be reused multiple times or a new release film can be supplied, and the product is subjected to the next resin molding process.
[0060] The release film of the present invention is adhered to the upper mold and interposed between the mold and the sealing resin, and a resin mold is formed. By doing so, it is possible to prevent the resin from adhering to the mold, to keep the resin molding surface of the mold clean, and The molded product can be easily released from the mold. In addition, a new release film is supplied for each resin molding operation. Or you can supply a new one for each resin molding operation. can.
[0061] The sealing resin may be a liquid resin or a resin that is solid at room temperature, but a sealing material that becomes liquid during resin sealing can be appropriately used. Specifically, epoxy resins (biphenyl type epoxy resin, bisphenol epoxy resin, o-cresol novolac type epoxy resin, etc.) are mainly used as sealing resin materials, and polyimide resins (bismaleimide type), silicone resins (thermosetting addition type), and other commonly used sealing resins can be used as sealing resins other than epoxy resins. In addition, the resin sealing conditions vary depending on the sealing resin used, but for example, a curing temperature of 120°C to 180°C and a molding pressure of 10 to 50 kg / cm are used. 2 The curing time can be appropriately set within the range of 1 to 60 minutes.
[0062] The order of the process of placing the release film 1 on the inner surface of the molding die 8 and the process of placing the semiconductor chip 6 inside the molding die 8 is not particularly limited, and they may be performed simultaneously, or the release film 1 may be placed after the semiconductor chip 6 is placed, or the release film 1 may be placed after the semiconductor chip 6 is placed.
[0063] Thus, since the release film 1 has the release layer A (and release layer A', if desired) with high releasability, the semiconductor package 4-2 can be easily released from the mold. In addition, since the release film 1 has appropriate flexibility, it has excellent conformability to the mold shape and is not easily wrinkled by the heat of the molding die 8. Therefore, wrinkles are not transferred to the resin sealing surface of the sealed semiconductor package 4-2, and no portions are filled with resin (resin chipping) occur, and a sealed semiconductor package 4-2 with a good appearance can be obtained.
[0064] Further, the method is not limited to the compression molding method in which the solid sealing resin material 4 is pressurized and heated as shown in FIG. 3, but a transfer molding method in which a fluid sealing resin material is injected as described later may be adopted.
[0065] 4A and 4B are schematic diagrams showing a transfer molding method, which is one example of a method for producing a resin-encapsulated semiconductor using the release film of the present invention.
[0066] 4A, the release film 22 of the present invention is supplied from a roll-shaped wound material by rolls 24 and 26 into a molding die 28 (step a). Next, the release film 22 is placed on the inner surface 30A of the upper die 30 (step b). If necessary, the upper die inner surface 30A may be evacuated to make the release film 22 adhere to the upper die inner surface 30A. Next, a semiconductor chip 34 to be resin-encapsulated (semiconductor chip 34 fixed to substrate 34A) is placed in the molding die 28, and an encapsulation resin material 36 is set (step c), and the die is clamped (step d).
[0067] 4B, under predetermined heating and pressure conditions, the encapsulating resin material 36 is injected into the molding die 28 (step e). The temperature (molding temperature) of the molding die 28 at this time is, for example, 165 to 185°C, the molding pressure is, for example, 7 to 12 MPa, and the molding time is, for example, about 90 seconds. After maintaining the temperature for a certain period of time, the upper die 30 and the lower die 32 are opened, and the resin-encapsulated semiconductor package 40 and the release film 22 are simultaneously or sequentially released (step f).
[0068] 5, by removing excess resin portion 42 from the obtained semiconductor package 40, a desired semiconductor package 44 can be obtained. Although the release film 22 may be used as is for resin sealing of other semiconductor chips, it is preferable to operate the roll to advance the film and supply new release film 22 to the molding die 28 each time a molding cycle is completed.
[0069] The order of the process of placing the release film 22 on the inner surface of the molding die 28 and the process of placing the semiconductor chip 34 inside the molding die 28 is not particularly limited, and they may be performed simultaneously, or the release film 22 may be placed after the semiconductor chip 34 is placed, or the semiconductor chip 34 may be placed after the release film 22 is placed.
[0070] Thus, since the release film 22 has the release layer A (and release layer A', if desired) with high releasability, the semiconductor package 40 can be easily released from the mold. In addition, since the release film 22 has appropriate flexibility, it has excellent conformability to the shape of the mold, while being less likely to wrinkle due to the heat of the molding mold 28. Therefore, wrinkles are not transferred to the resin sealing surface of the semiconductor package 40, and no portions are left unfilled with resin (resin chipping), and a semiconductor package 40 with a good appearance can be obtained.
[0071] The release film of the present invention is not limited to the process of resin encapsulation of semiconductor elements, but can also be used in a molding process using a molding die. The composition can also be preferably used in processes for molding and releasing various molded products, such as fiber-reinforced plastic molding and releasing processes, and plastic lens molding and releasing processes. EXAMPLES
[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. It is not something that is done.
[0073] In the following Examples and Comparative Examples, the physical properties and characteristics were evaluated by the following methods. (Thermal dimensional change rate) The film sample was cut into a length of 20 mm and a width of 4 mm in the longitudinal and transverse directions of the film, and measured using a TA Instruments TMA (thermomechanical analyzer, product name: Q400) with a chuck distance of 8 mm and a load of 0.005 N applied, held at 23°C for 5 minutes, and then heated from 23°C to 120°C at a heating rate of 10°C / min. The dimensional changes in each direction were measured, and the dimensional change rate was calculated using the following formula (1). Thermal dimensional change rate (%) (23 → 120℃) = {[(L2-L1) / L1]×100} (1) L1: Sample length at 23℃ (mm) L2: Sample length at 120℃ (mm) Similarly, the temperature was increased from 23° C. to 170° C. at a rate of 10° C. / min, and the dimensional change in each direction was measured, and the dimensional change rate was calculated according to the following formula (2). Thermal dimensional change rate (%) (23 → 170℃) = {[(L3-L1) / L1]×100} (2) L1: Sample length at 23℃ (mm) L3: Sample length at 170℃ (mm)
[0074] Contact angle with water (water contact angle) The water contact angle of the surface of release layer A was measured using a contact angle measuring instrument (manufactured by Kyowa Interface Science, Inc., FACECA-W) in accordance with JIS R 3257.
[0075] (Melting point (Tm), heat of crystal fusion) A differential scanning calorimeter (DSC) Q100 manufactured by TA Instruments was used. Approximately 5 mg of the polymer sample was precisely weighed out, and the thermal melting curve was measured in accordance with JIS K7121 under the conditions of nitrogen gas inflow: 50 ml / min, heating rate: 10°C / min from 25°C to 280°C. The melting point (Tm) and heat of crystal fusion of the sample were calculated from the obtained thermal melting curve.
[0076] (Mold releasability) The process release film prepared in each Example / Comparative Example was placed between the upper and lower dies with a tension of 10 N applied, as shown in FIG. 3, and then vacuum-adsorbed onto the parting surface of the upper die. Next, the substrate was filled with sealing resin so as to cover the semiconductor chip, and the semiconductor chip fixed to the substrate was placed on the lower die and clamped. At this time, the temperature of the molding die (molding temperature) was 120° C., the molding pressure was 10 MPa, and the molding time was 400 seconds. Then, as shown in FIG. 3c, the semiconductor chip was sealed with sealing resin, and the resin-sealed semiconductor chip (semiconductor package) was released from the release film. The releasability of the release film was evaluated according to the following criteria. ◯: The release film peels off naturally as soon as the mold is opened. △: The release film does not peel off naturally, but it peels off easily when pulled by hand (when tension is applied). ×: The release film is in close contact with the resin sealing surface of the semiconductor package and cannot be peeled off by hand.
[0077] (wrinkle) After the mold release was performed in the above process, the state of wrinkles on the release film and the resin sealing surface of the semiconductor package was evaluated according to the following criteria. ◯: There are absolutely no wrinkles on either the release film or the semiconductor package. △: The release film is slightly wrinkled, but the wrinkles are not transferred to the semiconductor package. ×: There are many wrinkles not only on the release film but also on the semiconductor package.
[0078] (Mold followability) The mold followability of the release film when the mold was released in the above process was evaluated according to the following criteria. ◯: There is absolutely no resin chipping (area not filled with resin) in the semiconductor package. △: There are a few chips in the resin on the edge of the semiconductor package (but chips due to wrinkles are not included) ×: There are many chips in the resin on the edge of the semiconductor package (but chips due to wrinkles are not included)
[0079] [Example 1] A biaxially stretched PET (polyethylene terephthalate) film (manufactured by Toray Industries, Inc., product name: Lumirror F865) having a thickness of 16 μm was used as the heat-resistant resin layer B. The thermal dimensional change rate of the biaxially stretched PET film from 23°C to 120°C was -1.6% in the machine direction (MD) and -1.2% in the transverse direction (TD). The melting point of the biaxially stretched PET film was 187°C, and the heat of crystal fusion was 30.6 J / g.
[0080] As the release layers A and A', a non-stretched 4-methyl-1-pentene copolymer resin film was used. Specifically, 4-methyl-1-pentene copolymer resin (product name: TPX, brand name: MX022) manufactured by Mitsui Chemicals Inc. was melt-extruded at 270°C, and a non-stretched film having a thickness of 15 μm was formed by adjusting the slit width of a T-shaped die. One of the film surfaces of the unstretched 4-methyl-1-pentene copolymer resin film was subjected to a corona treatment from the viewpoint of improving the adhesiveness of the adhesive so that the water contact angle based on JIS R3257 would be 30° or less if it was 30° or more. The thermal dimensional change rate of the 4-methyl-1-pentene copolymer resin film from 23° C. to 120° C. was 6.5% in the machine direction (MD) and 3.1% in the transverse direction (TD).
[0081] (glue) The adhesive used in the dry lamination process for bonding the films was the following urethane adhesive A. [Urethane adhesive A] Base agent: Takelac A-616 (manufactured by Mitsui Chemicals, Inc.). Hardener: Takenate A-65 (manufactured by Mitsui Chemicals, Inc.). The base agent and hardener were mixed in a mass ratio (base agent:hardener) of 16:1, and ethyl acetate was used as a diluent.
[0082] (Production of release films) One side of a biaxially oriented PET (polyethylene terephthalate) film is gravure coated with urethane adhesive A at 1.5 g / m. 2 The corona-treated surface of a non-oriented 4-methyl-1-pentene copolymer resin film was then dry-laminated to bond the film to the biaxially oriented PET (polyethylene terephthalate) film side of the laminate film. Then, 1.5 g / m of urethane adhesive A was applied to the biaxially oriented PET (polyethylene terephthalate) film side of the laminate film. 2 The corona-treated surface of a non-stretched 4-methyl-1-pentene copolymer resin film was then dry laminated to obtain a process release film with a five-layer structure (release layer A / adhesive layer / heat-resistant resin layer B / adhesive layer / release layer A'). The dry lamination conditions were as follows: substrate width 900 mm, conveying speed 30 m / min, drying temperature 50 to 60° C., laminating roll temperature 50° C., and roll pressure 3.0 MPa.
[0083] The thermal dimensional change rate of this process release film from 23°C to 120°C was 2.1% in the machine direction (MD) and 1.5% in the transverse direction (TD). The evaluation results of releasability, wrinkles, and mold followability are shown in Table 1. The release film exhibited good releasability, being naturally peeled off at the same time as the mold was opened, and there were no wrinkles on either the release film or the semiconductor package, i.e., wrinkles were sufficiently suppressed, and the semiconductor package showed good mold followability with no resin chipping. That is, the process release film of Example 1 was a process release film with good releasability, wrinkle suppression, and mold followability.
[0084] [Examples 2 to 12] Except for using the films shown in Table 1 in the combinations shown in Table 1 as the release layers A and A' and the heat-resistant resin layer B, the process release films were prepared in the same manner as in Example 1, and sealing and release were performed, and the properties were evaluated. The results are shown in Table 1. Although some of the films did not achieve the same wrinkle prevention or mold conformity as Example 1, all of the films were excellent process release films with a high level of balance between releasability, wrinkle prevention, and mold conformity.
[0085] Details of each film listed in the table are as follows. (A1) Unstretched 4MP-1 (TPX) film A 15μm-thick unstretched film was formed using 4-methyl-1-pentene copolymer resin (product name: TPX, brand name: MX022) manufactured by Mitsui Chemicals, Inc. (melting point: 229℃, heat of crystal fusion: 21.7J / g) (A2) Unstretched 4MP-1 (TPX) film A 15μm-thick unstretched film was formed using 4-methyl-1-pentene copolymer resin (product name: TPX, brand name: DX818) manufactured by Mitsui Chemicals, Inc. (melting point: 235℃, heat of crystal fusion: 28.1J / g) (A3) Unstretched 4MP-1 (TPX) film A 50μm-thick unstretched film was formed using 4-methyl-1-pentene copolymer resin (product name: TPX, brand name: MX022) manufactured by Mitsui Chemicals, Inc. (melting point: 229℃, heat of crystal fusion: 21.7J / g) (A4) Unstretched 4MP-1 (TPX) film A 50μm-thick unstretched film was formed using 4-methyl-1-pentene copolymer resin (product name: TPX, brand name: DX818) manufactured by Mitsui Chemicals, Inc. (melting point: 235℃, heat of crystal fusion: 28.1J / g) (A5) Fluorine resin film ETFE (ethylene-tetrafluoroethylene) film with a thickness of 25 μm (manufactured by Asahi Glass Co., Ltd., product name: Aflex 25N) (melting point: 256°C, heat of crystal fusion: 33.7 J / g) (A6) Polystyrene resin film Polystyrene film with a thickness of 50 μm (manufactured by Kurabo Industries, Ltd., product name: Eudis CA-F) (melting point: 253°C, heat of crystal fusion: 19.2 J / g) (B1) Biaxially stretched PET film Biaxially oriented PET (polyethylene terephthalate) film with a thickness of 16 μm (manufactured by Toray Industries, Inc., product name: Lumirror F865) (melting point: 187°C, heat of crystalline fusion: 30.6 J / g) (B2) Biaxially stretched PET film Biaxially oriented PET (polyethylene terephthalate) film with a thickness of 12 μm (manufactured by Toray Industries, Inc., product name: Lumirror S10) (melting point: 258°C, heat of crystalline fusion: 39.4 J / g) (B3) Biaxially oriented nylon film Biaxially oriented nylon film with a thickness of 15 μm (manufactured by Kohjin Film & Chemicals Co., Ltd., product name: Bonyl RX) (melting point: 212°C, heat of crystalline fusion: 53.1 J / g) (B4) Biaxially oriented nylon film Biaxially oriented nylon film with a thickness of 15 μm (manufactured by Idemitsu Unitech Co., Ltd., product name: Unilon S330) (melting point: 221°C, heat of crystalline fusion: 60.3 J / g) (B5) Biaxially oriented polypropylene film Biaxially oriented polypropylene film with a thickness of 20 μm (manufactured by Mitsui Chemicals Tocello, Inc., product name: U-2) (melting point: 160°C, heat of crystalline fusion: 93.3 J / g) (B6) Non-oriented nylon film 20μm thick non-oriented nylon film (Mitsubishi Plastics, Inc., product name: Dynamiron C) (melting point: 220℃, heat of crystalline fusion: 39.4J / g) (B7) Biaxially oriented PET film Biaxially stretched PET film with a thickness of 25 μm (Teijin DuPont Films, product name: FT3PE) (melting point: 214°C, heat of crystalline fusion: 40.3 J / g) (B8) Unstretched polybutylene terephthalate film A 20μm-thick unstretched film was formed using polybutylene terephthalate resin (brand name: 5020) manufactured by Mitsubishi Engineering Plastics Corporation. (Melting point: 223℃, heat of crystal fusion: 49.8J / g) (B9) Unstretched polybutylene terephthalate film A 20μm-thick unstretched film was formed using polybutylene terephthalate resin (brand name: 5505S) manufactured by Mitsubishi Engineering Plastics Corporation. (Melting point: 219℃, heat of crystal fusion: 48.3J / g) (B10) Unstretched polybutylene terephthalate film A 50μm-thick unstretched film was formed using polybutylene terephthalate resin (brand name: 5020) manufactured by Mitsubishi Engineering Plastics Corporation. (Melting point: 223℃, heat of crystal fusion: 49.8J / g) (B11) Unstretched polybutylene terephthalate film A 50μm-thick unstretched film was formed using polybutylene terephthalate resin (brand name: 5505S) manufactured by Mitsubishi Engineering Plastics Corporation. (Melting point: 219℃, heat of crystal fusion: 48.3J / g)
[0086] [Comparative Examples 1 to 4] Films A3, A4, B10, and B11 shown in Table 1 were each used alone as a process release film, and sealing and release were carried out in the same manner as in Example 1, to evaluate the properties of the process release film. All of the Comparative Examples had performances inferior to those of the Examples overall, and in particular were unable to suppress the occurrence of wrinkles.
[0087] [Table 1]
[0088] [Examples 13 to 20] Using the release films shown in Table 2 in the combinations shown in Table 2, in which each film described in Table 2 was used as release layers A and A' and heat-resistant resin layer B, process release films were prepared in the same manner as in Example 1, and sealing and release were performed, and the properties were evaluated. As shown in FIG. 4, the release film was placed between the upper and lower dies with a tension of 20 N applied, and then vacuum-adsorbed onto the parting surface of the upper die. Next, the substrate was filled with sealing resin so as to cover the semiconductor chip, and the semiconductor chip fixed to the substrate was placed in the lower die and clamped. At this time, the temperature of the molding die (molding temperature) was 170°C, the molding pressure was 10 MPa, and the molding time was 100 seconds. Then, as shown in FIG. 3c, the semiconductor chip was sealed with sealing resin, and the resin-sealed semiconductor chip (semiconductor package) was released from the release film. The results are shown in Table 2. Although some of the films had lower mold tracking properties than Example 1, all of the Examples were good process release films with a high level of balance between releasability, wrinkle prevention, and mold tracking properties. In particular, Example 11 and Examples 13 to 15 were process release films with good releasability, wrinkle prevention, and mold tracking properties.
[0089] [Comparative Examples 5 to 7] Except for using the films shown in Table 2 in the combinations shown in Table 2 as the release layers A and A' and the heat-resistant resin layer B, the process release films were prepared in the same manner as in Examples 11 to 16, and sealing and release were performed, and the properties were evaluated. The results are shown in Table 2. The mold releasability and mold followability were as good as in the Examples, but the occurrence of wrinkles could not be suppressed.
[0090] [Comparative Examples 8 to 11] Films A1, A2, B10, and B11 shown in Table 2 were each used alone as a process release film, and sealing and release were carried out in the same manner as in Examples 11 to 16, and the properties of the process release film were evaluated. All of the Comparative Examples had performances that were generally inferior to those of the Examples, and in particular were unable to suppress the occurrence of wrinkles.
[0091] [Table 2] [Industrial Applicability]
[0092] The process release film of the present invention combines high levels of releasability, wrinkle suppression, and mold followability that could not be achieved with conventional technologies. Therefore, by using this film, molded products obtained by resin encapsulation of semiconductor chips or the like can be easily released from the mold, and molded products free of appearance defects such as wrinkles and chips can be produced with high productivity. This technical effect has great practical value, and the film has high applicability in various industrial fields including the semiconductor process industry. In addition, the process release film of the present invention can be used not only for semiconductor packages but also for various mold molding in fiber reinforced plastic molding processes, plastic lens molding processes, etc., and therefore has high applicability in various fields of industries performing mold molding other than the semiconductor industry. [Explanation of symbols]
[0093] 1, 1-2, 1-3: Release film 2: Upper mold 3: Suction port 4: Sealing resin 4-2: Semiconductor packages 5: Lower mold 6. Semiconductor chips 7: Substrate 8: Mould 10, 20, 22: Release film 12: Heat-resistant resin layer B 14: Adhesive layer 16, 16A: Release layer A 16B: Release layer A´ 24, 26: Roll 28: Mould 30: Upper mold 32: Lower mold 34: Semiconductor chips 34A: Circuit board 36: Sealing resin 40, 44: Semiconductor packages
Claims
1. A process release film which is a laminated film including a release layer A and a heat-resistant resin layer B, The contact angle of the release layer A with respect to water is 90° to 130°, the thermal dimensional change rate of the laminated film in the transverse (TD) direction from 23° C. to 120° C. is 3% or less, the thermal dimensional change rate being calculated from the sample length at 23° C. and the sample length at 120° C., which are measured by holding the sample at 23° C. for 5 minutes under a load of 0.005 N and then raising the temperature from 23° C. to 120° C. at a heating rate of 10° C. / min; The above-mentioned process release film, in which the heat of crystalline fusion of the heat-resistant resin layer B in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JIS K7221 is 20 J / g or more and 100 J / g or less (excluding the case where the heat of crystalline fusion of the heat-resistant resin layer B in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JIS K7221 is 20 J / g or more and 55 J / g or less).
2. 2. The process release film according to claim 1, wherein the sum of the thermal dimensional change rate in the transverse (TD) direction from 23°C to 120°C and the thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 120°C is 6% or less, the sample length at 23°C and the sample length at 120°C are measured by holding the sample at 23°C for 5 minutes under a load of 0.005 N and then increasing the temperature from 23°C to 120°C at a heating rate of 10°C / min.
3. A process release film which is a laminated film including a release layer A and a heat-resistant resin layer B, The contact angle of the release layer A with respect to water is 90° to 130°, the thermal dimensional change rate of the laminated film in the transverse (TD) direction from 23° C. to 170° C. is 4% or less, the thermal dimensional change rate being calculated from the sample length at 23° C. and the sample length at 170° C., which are measured by holding the sample at 23° C. for 5 minutes under a load of 0.005 N and then raising the temperature from 23° C. to 170° C. at a heating rate of 10° C. / min; and The above-mentioned process release film, in which the heat of crystalline fusion of the heat-resistant resin layer B in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JIS K7221 is 20 J / g or more and 100 J / g or less (excluding the case where the heat of crystalline fusion of the heat-resistant resin layer B in the first heating step measured by differential scanning calorimetry (DSC) in accordance with JIS K7221 is 20 J / g or more and 55 J / g or less).
4. 4. The process release film according to claim 3, wherein the sum of the thermal dimensional change rate in the transverse (TD) direction from 23°C to 170°C and the thermal dimensional change rate in the longitudinal (MD) direction from 23°C to 170°C is 7% or less, the sample length at 23°C and the sample length at 170°C are measured by holding the sample at 23°C for 5 minutes under a load of 0.005 N and then increasing the temperature from 23°C to 170°C at a heating rate of 10°C / min.
5. 5. The process release film according to claim 1, wherein the thermal dimensional change rate of the heat-resistant resin layer B in the transverse (TD) direction from 23° C. to 120° C. is 3% or less, as calculated from the sample length at 23° C. and the sample length at 120° C., which are measured by holding the sample at 23° C. for 5 minutes under a load of 0.005 N and then raising the temperature from 23° C. to 120° C. at a heating rate of 10° C. / min.
6. 6. The process release film according to claim 5, wherein the sum of the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 120°C in the transverse (TD) direction and the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 120°C in the longitudinal (MD) direction is 6% or less, the sum of the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 120°C in the transverse (TD) direction and the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 120°C in the longitudinal (MD) direction being measured by holding the sample at 23°C for 5 minutes under a load of 0.005 N and then raising the temperature from 23°C to 120°C at a heating rate of 10°C / min is calculated from the sample length at 23°C and the sample length at 120°C.
7. 5. The process release film according to claim 1, wherein the thermal dimensional change rate of the heat-resistant resin layer B in the transverse (TD) direction from 23° C. to 170° C. is 3% or less, as calculated from the sample length at 23° C. and the sample length at 170° C., which are measured by holding the sample at 23° C. for 5 minutes under a load of 0.005 N and then raising the temperature from 23° C. to 170° C. at a heating rate of 10° C. / min.
8. 8. The process release film according to claim 7, wherein the sum of the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 170°C in the transverse (TD) direction and the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 170°C in the longitudinal (MD) direction is 4% or less, the sum of the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 170°C in the transverse (TD) direction and the thermal dimensional change rate of the heat-resistant resin layer B from 23°C to 170°C in the longitudinal (MD) direction being measured by holding the sample at 23°C for 5 minutes under a load of 0.005 N and then raising the temperature from 23°C to 170°C at a heating rate of 10°C / min is calculated from the sample length at 23°C and the sample length at 170°C.
9. The process release film according to any one of claims 1 to 8, wherein the release layer A comprises a resin selected from the group consisting of fluororesins, 4-methyl-1-pentene (co)polymers, and polystyrene-based resins.
10. The release film for process use according to claim 1 , wherein the heat-resistant resin layer B comprises a stretched film.
11. 11. The process release film of claim 10, wherein the oriented film is selected from the group consisting of oriented polyester films, oriented polyamide films, and oriented polypropylene films.
12. The laminated film further has a release layer A', and includes the release layer A, the heat-resistant resin layer B, and the release layer A' in this order, The release film for process use according to claim 1 , wherein the contact angle of the release layer A′ with water is from 90° to 130°.
13. At least one of the release layer A and the release layer A' contains a resin selected from the group consisting of fluororesin, 4-methyl-1-pentene (co)polymer, and polystyrene-based resin.
14. The release film for process according to any one of claims 1 to 13, which is used in a sealing process using a thermosetting resin.
15. A method for manufacturing a resin-encapsulated semiconductor device, comprising the steps of: A step of placing a semiconductor device to be resin-encapsulated at a predetermined position in a molding die; A step of disposing the release film for semiconductor encapsulation process according to any one of claims 1 to 13 on an inner surface of the molding die such that the release layer A faces the semiconductor device; After clamping the molding die, a step of injecting an encapsulation resin between the semiconductor device and the release film for semiconductor encapsulation process; The method for producing the resin-encapsulated semiconductor device according to claim 1,
16. A method for manufacturing a resin-encapsulated semiconductor device, comprising the steps of: A step of placing a semiconductor device to be resin-encapsulated at a predetermined position in a molding die; A step of disposing the release film for semiconductor encapsulation process according to claim 12 or 13 on an inner surface of the molding die such that the release layer A' faces the semiconductor device; After clamping the molding die, a step of injecting an encapsulation resin between the semiconductor device and the release film for semiconductor encapsulation process; The method for producing the resin-encapsulated semiconductor device according to claim 1,
Citation Information
Patent Citations
Releasing film for molding resin mold
JP2001310336A
Method for encapsulating semiconductor chip with resin, and mold release film for encapsulating semiconductor chip with resin
JP2002110722A
Release sheet for semiconductor mold
JP2002361643A
Mold release film for manufacturing printed board
JP2006175672A
Mold-releasing film
JP2009034947A