Manufacturing method for mold for diffraction grating light guide plate and manufacturing method for diffraction grating light guide plate
The use of a Faraday cage and controlled mask films with specific adhesive properties addresses the challenges of mask etching in diffraction grating light guide plate manufacturing, enabling precise and efficient pattern formation on the mold base material.
Patent Information
- Application Number
- JP2023068780
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-06-20
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2039-06-18
AI Technical Summary
Existing methods for manufacturing diffraction grating light guide plates face challenges such as the need for frequent mask film replacement and thermal deformation or adhesion issues during mask etching, leading to potential damage to the mold base material.
A method involving the use of a Faraday cage with a mesh portion and specific mask films with controlled adhesive properties and glass transition temperatures, combined with plasma etching, to form pattern parts of various shapes efficiently on the mold base material.
This approach allows for precise and efficient formation of pattern parts on the mold, reducing thermal deformation, adhesive residue, and maintaining etching accuracy, thereby improving the manufacturing process.
Smart Images

Figure 0007570756000001 
Figure 0007570756000002 
Figure 0007570756000003
Abstract
Description
[Technical field]
[0001] This specification claims the benefit of the filing date of Korean Patent Application No. 10-2018-0070583, filed with the Korean Intellectual Property Office on June 20, 2018, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a method for efficiently manufacturing a mold for a diffraction grating light guide plate and a method for manufacturing a diffraction grating light guide plate. [Background technology]
[0003] Recently, as interest in display units that realize Augmented Reality (AR), Mixed Reality (MR), or Virtual Reality (VR) has increased, research on display units that realize such display units has been actively conducted. A display unit that realizes Augmented Reality, Mixed Reality, or Virtual Reality includes a diffraction grating light guide plate that utilizes a diffraction phenomenon based on the wave properties of light. The diffraction grating light guide plate includes a diffraction grating pattern that can internally reflect or totally internally reflect incident light and guide the light that has entered the diffraction grating light guide plate to one point.
[0004] Such a diffraction grating light guide plate includes a first region where light enters the diffraction grating light guide plate and a second region where the light entering the diffraction grating light guide plate is extracted, and each of the first and second regions is provided with a diffraction grating pattern. Further, a diffraction grating light guide plate has been developed that includes a third region that guides light from the first region to the second region, and a fourth region that can effectively guide light from the third region to the second region. In this case, each of the third and fourth regions is provided with a diffraction grating pattern.
[0005] Various methods are used to manufacture such a diffraction grating light guide plate, and generally, the diffraction grating light guide plate is manufactured by an imprinting method using a mold. A mask etching process can be used to manufacture a mold for the diffraction grating light guide plate. At this time, a mold base material used to manufacture a diffraction grating light guide plate having a desired diffraction grating pattern is provided with diffraction grating patterns of different shapes. However, mask etching conditions for forming the diffraction grating patterns of different shapes are different, and there is a problem that the mask film must be replaced every time each diffraction grating pattern is formed.
[0006] In addition, during the mask etching process, if the mask film provided on the mold substrate is thermally deformed or the adhesive strength between the mask film and the mold substrate is not appropriate, the mold substrate may be damaged.
[0007] Therefore, there is a current need for a technique that can effectively form a diffraction grating pattern on a mold substrate. Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention provides a method for efficiently manufacturing a mold for a diffraction grating light guide plate and a method for manufacturing a diffraction grating light guide plate.
[0009] However, the problems to be solved by the present invention are not limited to the problems described above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0010] One embodiment of the present invention provides a method for manufacturing a mold for a diffraction grating light guide plate, the method comprising the steps of: preparing a first mask film including a first opening and a second opening formed in separate regions; attaching the first mask film to one side of a mold substrate, opening only the first opening, and then positioning the mold substrate with the first mask film attached in a Faraday cage having a mesh portion on its upper surface, and forming a first pattern portion by plasma etching in a first region of the one side of the mold substrate exposed by the first opening; and opening only the second opening, forming a second pattern portion by plasma etching in a second region of the one side of the mold substrate exposed by the second opening, the first mask film including a first substrate and a first adhesive layer provided on one side of the first substrate, the first substrate having a glass transition temperature of 70° C. or more and 100° C. or less, and the first adhesive layer having an adhesive strength of 30 gf / in or more and 50 gf / in or less.
[0011] In addition, another embodiment of the present invention provides a method for manufacturing a diffraction grating light guide plate, comprising the steps of: preparing a mold for a diffraction grating light guide plate manufactured by the method for manufacturing a mold for a diffraction grating light guide plate; applying a resin composition onto one surface of the mold for the diffraction grating light guide plate on which a pattern portion is formed; and curing the resin composition. Effect of the Invention
[0012] According to an embodiment of the present invention, a method for manufacturing a mold for a diffraction grating light guide plate can efficiently manufacture a mold for a diffraction grating light guide plate having pattern portions of various shapes on one surface.
[0013] The effects of the present invention are not limited to those described above, and effects not mentioned will be clearly understood by those skilled in the art from the present specification and the accompanying drawings. [Brief description of the drawings]
[0014] [Figure 1A]1 shows a first mask film having a first opening and a second opening according to one embodiment of the present invention. [Figure 1B] 4 shows a second mask film provided with a third opening. [Figure 1C] 1 shows a first mask film having a first opening, a second opening and a fourth opening. [Figure 2A] 1 shows a step of forming a first pattern portion according to one embodiment of the present invention. [Figure 2B] 4 shows a step of forming a second pattern portion. [Figure 2C] 13 shows a step of forming a third pattern portion. [Figure 2D] 11 shows a step of forming a fourth pattern portion. [Diagram 3] 1 is a photograph of a Faraday cage according to one embodiment of the present invention. [Figure 4] 1 shows one surface of a mold for a diffraction grating light guide plate manufactured by a method for manufacturing a mold for a diffraction grating light guide plate according to one embodiment of the present invention. [Diagram 5] 1 is a photograph of the mask film manufactured in Example 1 of the present invention after plasma etching treatment. [Figure 6] 1 is a photograph of the mask film produced in Comparative Example 3 after plasma etching treatment. [Figure 7] 1 is a photograph of the mask film produced in Comparative Example 5 after plasma etching treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Throughout this specification, when a part is described as "comprising" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0016] Throughout this specification, when an element is said to be "on" another element, this includes not only when the element is in contact with the other element, but also when there is another element between the two elements.
[0017] As used throughout this specification, the terms "step of" or "step of" do not mean "a step for."
[0018] The Faraday cage in the present invention means a sealed space made of a conductor, and when the Faraday cage is placed in plasma, a sheath is formed on the outer surface of the cage, and the electric field inside is maintained at a constant state. At this time, when the upper surface of the Faraday cage is formed of a mesh part, the sheath is formed along the surface of the mesh part. Therefore, when performing plasma etching using the Faraday cage, ions accelerated in a direction perpendicular to the sheath formed horizontally on the surface of the mesh part enter the inside of the Faraday cage, and then reach the substrate while maintaining the directionality at the time of entry, and etch the substrate. Furthermore, the surface of the mold substrate inside the Faraday cage in the present invention is fixed horizontally or inclined with respect to the mesh surface, and ions enter in a direction perpendicular to the mesh surface, so that etching in a direction perpendicular or inclined with respect to the surface of the mold substrate is possible. The Faraday cage may also be a conductive cage whose upper surface is made of a mesh part having electrical conductivity.
[0019] In the case of plasma etching using a Faraday cage, ions that have passed through the mesh section lose kinetic energy while moving toward the substrate by colliding with neutral particles present inside the Faraday cage, and as a result, the density of ions tends to be inversely proportional to the distance between the mesh sections. That is, the closer to the mesh section where the ions are incident, the higher the etching rate, and the farther from the mesh section, the lower the etching rate.
[0020] The present inventors have studied a method for manufacturing a mold for a diffraction grating light guide plate using a Faraday cage having the above-mentioned characteristics, and have specifically studied a method for effectively manufacturing a mold for a diffraction grating light guide plate having pattern parts on four independent regions, leading to the development of the following invention.
[0021] The present specification will be explained in further detail below.
[0022] One embodiment of the present invention provides a method for manufacturing a mold for a diffraction grating light guide plate, the method comprising the steps of: preparing a first mask film including a first opening and a second opening formed in separate regions; attaching the first mask film to one side of a mold substrate, opening only the first opening, and then positioning the mold substrate with the first mask film attached in a Faraday cage having a mesh portion on its upper surface, and forming a first pattern portion by plasma etching in a first region of the one side of the mold substrate exposed by the first opening; and opening only the second opening, forming a second pattern portion by plasma etching in a second region of the one side of the mold substrate exposed by the second opening, the first mask film including a first substrate and a first adhesive layer provided on one side of the first substrate, the first substrate having a glass transition temperature of 70° C. or more and 100° C. or less, and the first adhesive layer having an adhesive strength of 30 gf / in or more and 50 gf / in or less.
[0023] According to an embodiment of the present invention, a method for manufacturing a mold for a diffraction grating light guide plate can efficiently manufacture a mold for a diffraction grating light guide plate having pattern portions of various shapes on one surface.
[0024] Fig. 1A shows a first mask film having a first opening and a second opening according to an embodiment of the present invention, Fig. 1B shows a second mask film having a third opening, and Fig. 1C shows a first mask film having a first opening, a second opening, and an additional fourth opening. Specifically, Fig. 1A shows a first mask film 200 having a first opening H1 and a second opening H2 formed on an independent region, and Fig. 1C shows a first mask film 200' having a first opening H1, a second opening H2, and a fourth opening H4 formed on an independent region. Fig. 1B shows a second mask film 300 having a third opening H3 formed on one region.
[0025] According to one embodiment of the present invention, the method of forming the first and second openings on the region of the first mask film can use any cutting method for members used in the industry without limitation. For example, the first mask film can be cut with a knife or cut using a laser along the shape of the desired first and second openings. Specifically, in order to improve the cutting efficiency and cutting accuracy, the present invention can use laser cutting to form the first and second openings on the first mask film. In addition, a third opening can be formed in the second mask film by the same method as described above, and a fourth opening can be additionally formed in the first mask film.
[0026] According to one embodiment of the present invention, the mold substrate may be a quartz substrate or a silicon wafer. During plasma etching, specifically, during an etching process using an inductively coupled plasma reactive ion etching (ICP-RIE), a problem may occur in which needle-like structures having low reflectivity are formed in the etching region due to a self-masking mechanism. However, according to one embodiment of the present invention, by using a quartz substrate or a silicon wafer as the mold substrate, it is possible to effectively prevent needle-like structures from being formed during a process of etching the first to fourth pattern portions on one side of the mold substrate.
[0027] According to one embodiment of the present invention, a first pattern portion and a second pattern portion can be formed on the mold substrate by plasma etching one surface of the mold substrate using a Faraday cage having a mesh portion on its upper surface, and a third pattern portion and a fourth pattern portion can be additionally formed on the mold substrate. The mesh portion can attract free electrons at a surface in contact with the plasma during plasma etching to form a sheath. The mesh portion can also be conductive, thereby attracting and accelerating positively charged ions. Furthermore, the mesh portion is provided flat on one surface of the Faraday cage, and if there is a bent portion, the etching speed at the bent portion can be locally different.
[0028] According to an embodiment of the present invention, the mesh part may have a sheet resistance of 0.5Ω / □ or more. Specifically, the sheet resistance of the mesh part may be 0.5Ω / □ or more and 100Ω / □ or less. When the mold substrate is plasma etched using a conventional Faraday cage, there is a problem that high etching regions and low etching regions are irregularly mixed at each position of the Faraday cage, thereby reducing the accuracy of the plasma etching. In contrast, according to an embodiment of the present invention, by adjusting the sheet resistance of the mesh part within the above-mentioned range, high etching regions and low etching regions can be uniformly formed within the Faraday cage during plasma etching. That is, the first pattern part to the fourth pattern part can be precisely etched on the mold substrate. In addition, when the sheet resistance of the mesh part is within the above-mentioned range, the etching efficiency can be improved while reducing the manufacturing cost of the Faraday cage.
[0029] According to one embodiment of the present invention, the mesh portion may be a metal mesh having a fluorocarbon radical adsorbed thereon. Specifically, the fluorocarbon radical may be -CF, -CF2, -CF3, or -C2F x(x is an integer of 1 to 5). More specifically, the mesh portion of the Faraday cage is etched by F radicals and surface polymerized during plasma etching, so that fluorocarbon radicals are adsorbed to the mesh portion. In addition, the mesh portion can have a sheet resistance in the above-mentioned range by adsorbing the fluorocarbon radicals onto a conductive material such as a metal.
[0030] According to one embodiment of the present invention, the mesh part can be made of stainless steel. Specifically, a commercial mesh made of SUS304 material #200 (pitch 125 μm, wire diameter 50 μm, aperture ratio 36%) can be used. However, the material of the mesh part is not limited, and the mesh part may be made of Al, Cu, W, Ni, Fe, or an alloy containing at least two of these. Furthermore, the porosity and lattice size of the mesh can be freely adjusted depending on the application of etching.
[0031] FIG. 2A shows a step of forming a first pattern portion according to one embodiment of the present invention, FIG. 2B shows a step of forming a second pattern portion, FIG. 2C shows a step of forming a third pattern portion, and FIG. 2D shows a step of forming a fourth pattern portion.
[0032] According to one embodiment of the present invention, the step of forming the first pattern portion can open only the first opening of the first mask film and form the first pattern portion on the surface of the mold base material exposed by the first opening. In the first mask film in which the first opening and the second opening are formed, the second opening can be blocked in order to open only the first opening. Specifically, an overlay film can be attached on the second opening to block the second opening. The overlay film can be the same as the first mask film or the second mask film, cut to an appropriate size and used.
[0033] According to one embodiment of the present invention, the step of forming the first pattern portion may include positioning one surface of the mold substrate at an incline to the bottom surface of the Faraday cage and performing plasma etching to form an inclined pattern portion. Referring to FIG. 2A, the step of forming the first pattern portion may include positioning the mold substrate 100 on a support stage 430 having an inclined surface and performing plasma inclined etching on a first region of the mold substrate 100. As a result, a first pattern portion having an incline may be formed on the first region of the mold substrate.
[0034] According to an embodiment of the present invention, an inclination angle of the support stand with respect to a bottom surface of the Faraday cage may be from 0° to 60°, or from 35° to 45°. The inclination angle of the support stand can be adjusted to adjust the inclination angle of the first pattern portion.
[0035] By adjusting the inclination angle of the support stand within the above-mentioned range, the average inclination angle of the first pattern part can be adjusted to 0° to 55° or 30° to 40°. For example, when the inclination angle of the support stand is adjusted to 35°, the minimum inclination angle of the first pattern part is adjusted to 27°, the maximum inclination angle is adjusted to 36°, and the average inclination angle is adjusted to 33°. Also, when the inclination angle of the support stand is adjusted to 40°, the minimum inclination angle of the first pattern part is adjusted to 32°, the maximum inclination angle is adjusted to 40°, and the average inclination angle is adjusted to 36°.
[0036] According to one embodiment of the present invention, the step of forming the second pattern portion may include positioning one side of the mold substrate at an incline toward the bottom surface of the Faraday cage, shielding at least a portion of the mesh portion using a shutter, and then performing plasma etching to form an inclined pattern portion having a depth gradient.
[0037] When plasma etching is performed using a conventional Faraday cage without a shutter, the etching rate is determined according to the distance from the mesh part of the Faraday cage to the mold substrate, and the change in the etching rate cannot be adjusted to a desired level. In contrast, according to one embodiment of the present invention, by shielding a part of the mesh part of the Faraday cage with a shutter, the change in the etching rate according to the increase in the distance from the mesh part to the mold substrate can be greatly adjusted in the etching region adjacent to the region shielded by the shutter. That is, by shielding a part of the mesh part with a shutter to greatly adjust the change in the etching rate, a second pattern part having a depth gradient can be easily formed on the second region of the mold substrate.
[0038] Specifically, the step of forming the second pattern portion may include forming a pattern over the entire second region by performing plasma etching without a shutter, and then shielding a portion of the mesh portion with a shutter and performing plasma etching, thereby forming a second pattern portion having a desired depth gradient. Referring to Fig. 2B, the step of forming the second pattern portion may include a process of positioning the mold substrate 100 on a support 430 having an inclined surface, shielding a portion of the mesh portion 410 with a shutter 420, and then performing plasma gradient etching. As a result, a second pattern portion having an inclined pattern shape with a depth gradient may be formed on the second region of the mold substrate.
[0039] According to one embodiment of the present invention, the method for manufacturing a mold for a diffraction grating light guide plate may further include the steps of preparing a second mask film having a third opening formed in one region and removing the first mask film from one side of the mold base, and attaching the second mask film to one side of the mold base and forming a third pattern portion in a third region of the one side of the mold base exposed by the third opening using plasma etching.
[0040] That is, the first mask film having the first opening and the second opening is used to form the first pattern portion and the second pattern portion on one side of the mold substrate, and the first mask film can be removed from the one side of the mold substrate. Thereafter, the second mask film can be attached to the one side of the mold substrate having the first pattern portion and the second pattern portion, and plasma etching can be performed to form the third pattern portion on the one side of the mold substrate. In addition, the first mask film having the first opening, the second opening, and the fourth opening is used to form the first pattern portion, the second pattern portion, and the fourth pattern portion on the one side of the mold substrate, and the third pattern portion can be formed on the one side of the mold substrate using the second mask film.
[0041] According to an embodiment of the present invention, the step of forming the third pattern portion may include: positioning one surface of the mold substrate parallel to a bottom surface of the Faraday cage, shielding at least a portion of the mesh portion with a shutter, and performing plasma etching to form a pattern portion having a depth gradient. Specifically, the step of forming the third pattern portion may form a third pattern portion having a desired depth gradient by performing plasma etching without a shutter to form a pattern in the entire third region, and then shielding a portion of the mesh portion with a shutter and performing plasma etching. Referring to FIG. 2C, the step of forming the third pattern portion may include a process of positioning the mold substrate 100 parallel to a bottom surface of the Faraday cage 400, shielding a portion of the mesh portion 410 with a shutter 420, and performing plasma gradient etching. As a result, a third pattern portion having a gradient pattern shape having a depth gradient may be formed on the third region of the mold substrate.
[0042] According to one embodiment of the present invention, the shutter may cover 20% to 80% of the mesh portion. Specifically, the shutter may cover 30% to 60% of the mesh portion, or 40% to 60% of the mesh portion. More specifically, the shutter may cover 50% of the mesh portion. The shutter may also cover a fixed area of the mesh portion continuously.
[0043] Fig. 3 is a photograph of a Faraday cage according to one embodiment of the present invention. Specifically, Fig. 3(a) is an image of the surface of the mesh part of a Faraday cage not provided with a shutter, and Fig. 3(b) is an image of the surface of the mesh part of a Faraday cage provided with a shutter.
[0044] According to one embodiment of the present invention, the shutter may be made of an aluminum oxide material, but the material of the shutter is not limited, and various materials that are not etched by the plasma can be used.
[0045] According to one embodiment of the present invention, the first mask film additionally includes a fourth opening, and the method for manufacturing the mold for the diffraction grating light guide plate may further include a step of forming a fourth pattern portion on a fourth region of one surface of the mold substrate exposed by the fourth opening using plasma etching after opening only the fourth opening.
[0046] According to an embodiment of the present invention, the step of forming the fourth pattern portion may include positioning one surface of the mold substrate parallel to the bottom surface of the Faraday cage and performing plasma etching. Referring to FIG. 2D, the step of forming the fourth pattern portion may include a process of positioning the mold substrate 100 on the bottom surface of the Faraday cage 400 and performing plasma etching to form a fourth pattern portion having substantially no depth gradient. In the present invention, substantially no depth gradient may mean that the depth (height) of the pattern portion is completely uniform, or the pattern portion has a depth gradient of 20 nm or less per 5 mm length, and the optical properties are substantially uniform throughout the pattern portion.
[0047] 4 shows one surface of a mold for a diffraction grating light guide plate manufactured by a manufacturing method for a mold for a diffraction grating light guide plate according to an embodiment of the present invention. Referring to FIG. 4, a first pattern portion P1 having no depth gradient but having an inclined shape is provided on a first region of one surface of the mold for a diffraction grating light guide plate 1000, and a second pattern portion P2 having a depth gradient and having an inclined shape is provided on a second region. In addition, a third pattern portion P3 having a depth gradient but not inclined is provided on a third region, and a fourth pattern portion P4 having no depth gradient and not inclined is provided on a fourth region.
[0048] According to an embodiment of the present invention, the first pattern portion and the second pattern portion may have an inclination direction opposite to each other. In the process of forming the first pattern portion and the second pattern portion, the inclination direction of the pattern portion may be changed by adjusting the direction in which one side and the other side of the mold substrate are located. Also, in the process of forming the first pattern portion and the second pattern portion, the inclination direction of the pattern portion may be changed by adjusting the inclination direction of the mold substrate and the bottom surface of the Faraday cage. Referring to FIG. 2A and FIG. 2B, the inclination directions of the inclined patterns of the first pattern portion and the second pattern portion may be opposite to each other by differently positioning one side and the other side of the mold substrate 100 at positions adjacent to the mesh portion of the Faraday cage.
[0049] According to one embodiment of the present invention, the depth gradient of the third pattern portion may be more than 20 nm and not more than 40 nm per 5 mm of the length of the pattern portion. However, the depth gradient of the third pattern portion is not limited to the above range, and the depth gradient can be changed depending on the design items of the mold for the diffraction grating light guide plate.
[0050] According to one embodiment of the present invention, the second pattern portion may have a depth gradient in which the pattern depth at one side where the pattern starts is about 40 nm and the pattern depth at the other side where the pattern ends is about 350 nm. However, the depth gradient of the second pattern portion is not limited to the above range, and the depth gradient may be changed according to design items of the mold for the diffraction grating light guide plate.
[0051] According to one embodiment of the present invention, the plasma etching can be performed using an inductively coupled plasma reactive ion etching apparatus (ICP-RIE). Specifically, the plasma etching process can be performed by providing the Faraday cage inside an inductively coupled plasma reactive ion etching apparatus. In addition, the plasma etching can be performed using a helicon plasma method, a helical resonant plasma method, or an electron resonant plasma method.
[0052] According to one embodiment of the present invention, the plasma etching may include adjusting the output of a plasma etching apparatus to 0.75 kW or more and 4 kW or less. Specifically, the output of the plasma etching apparatus is adjusted to 0.75 kW or more and 3 kW or less, 0.75 kW or more and 1.5 kW or less, or 0.75 kW or more and 1 kW or less. By adjusting the output of the plasma etching apparatus within the above-mentioned range, the first pattern portion to the fourth pattern portion can be more precisely formed on the mold substrate. In addition, when the output of the plasma etching apparatus is within the above-mentioned range, the formation of needle-like structures generated during etching of the mold substrate can be more suppressed, and the size of the needle-like structures generated can be significantly reduced.
[0053] According to an embodiment of the present invention, the plasma etching may include supplying a mixed gas containing a reactive gas and an oxygen gas to a plasma etching apparatus at 10 sccm to 75 sccm. Specifically, the mixed gas may be supplied to the plasma etching apparatus at 15 sccm to 75 sccm, 25 sccm to 70 sccm, 30 sccm to 70 sccm, 40 sccm to 60 sccm, or 45 sccm to 55 sccm. When the supply flow rate of the mixed gas is adjusted to the above range, the first pattern portion to the fourth pattern portion can be stably formed on the mold base material. In addition, by adjusting the supply flow rate of the mixed gas to the above range, the formation of needle-like structures generated during etching of the mold base material can be further suppressed, and the size of the needle-like structures generated can be significantly reduced.
[0054] According to one embodiment of the present invention, the reactive gas may be a typical reactive gas used in plasma etching, such as SF6, CHF3, C4F8, CF4, and Cl2.
[0055] According to one embodiment of the present invention, the content of oxygen gas in the total flow rate of the mixed gas may be 1% or more and 20% or less. Specifically, the content of oxygen gas in the total flow rate of the mixed gas may be 1% or more and 15% or less, 1% or more and 10% or less, or 1% or more and 5% or less. When the content of oxygen in the mixed gas flow rate is within the above range, the formation of needle-like structures generated during etching of the mold substrate can be further suppressed, and the size of the generated needle-like structures can be significantly reduced.
[0056] According to one embodiment of the present invention, a first pattern portion can be formed on the mold substrate and then a fourth pattern portion can be formed from a second pattern portion, or a fourth pattern portion can be formed on the mold substrate and then a first pattern portion can be formed.
[0057] Hereinafter, the first mask film having the first opening, the second opening and the fourth opening will be mainly described.
[0058] According to one embodiment of the present invention, the first mask film includes a first substrate and a first adhesive layer provided on one surface of the first substrate, and the glass transition temperature of the first substrate may be 70°C or more and 100°C or less, and the adhesive strength of the first adhesive layer may be 30gf / in or more and 50gf / in or less. Specifically, the glass transition temperature of the first substrate may be 80°C or more and 90°C or less, or 85°C or more and 90°C or less. The melting point of the first substrate may be 250°C or more and 300°C or less, or 265°C or more and 290°C or less. Furthermore, the adhesive strength of the first adhesive layer may be 30gf / in or more and 50gf / in or less, 35gf / in or more and 40gf / in or less, 30gf / in or more and 37gf / in or less, or 38gf / in or more and 45gf / in or less, against a stainless steel 304 substrate at 25°C.
[0059] According to one embodiment of the present invention, the first substrate can be a polyethylene terephthalate substrate having the above-mentioned glass transition temperature and / or melting point, and the first adhesive layer can be a silicone adhesive layer having the above-mentioned adhesive strength.
[0060] According to one embodiment of the present invention, in the step of forming the first pattern portion, the surface temperature of the mold substrate may be 155° C. or more and 165° C. or less. Also, in the step of forming the fourth pattern portion, the surface temperature of the mold substrate may be 150° C. or more and 160° C. or less.
[0061] In addition, in the step of forming the second pattern portion, the surface temperature of the mold substrate may be 100°C or more and 150°C or less. The step of forming the second pattern portion is performed by performing plasma etching twice. A pattern portion may be formed in the entire second region without a shutter, and the surface temperature of the mold substrate at this time may be 100°C or more and 115°C or less. After forming a pattern in the entire second region, plasma etching may be performed by shielding a part of the mesh portion with a shutter, and the surface temperature of the mold substrate not shielded by the shutter may be 130°C or more and 150°C or less.
[0062] Therefore, the first mask film including the first substrate having the above-mentioned glass transition temperature and / or melting point can effectively withstand thermal shock during the plasma etching process for forming the first pattern portion, the second pattern portion, and the fourth pattern portion. In addition, by adjusting the adhesive strength of the first adhesive layer within the above-mentioned range, the first mask film can be prevented from peeling off from one side of the mold substrate during the plasma etching process for forming the first pattern portion, the second pattern portion, and the fourth pattern portion. Furthermore, when the adhesive strength of the first adhesive layer is within the above-mentioned range, the penetration of reactive gas between the first adhesive layer and the mold substrate during the process for forming the first pattern portion, the second pattern portion, and the fourth pattern portion can be effectively suppressed, and the generation of bubbles between the first adhesive layer and the mold substrate can be suppressed. This can effectively prevent damage from occurring on one side of the mold substrate. In addition, when the adhesive strength of the first adhesive layer is within the above-mentioned range, it is easy to peel off the first mask film after the process of forming the first pattern portion, the second pattern portion, and the fourth pattern portion is completed, and it is possible to effectively prevent residue of the adhesive layer from remaining on one side of the mold substrate even after peeling off the first mask film that has been subjected to thermal shock.
[0063] According to one embodiment of the present invention, the thickness of the first substrate may be 30 μm or more and 50 μm or less, and the thickness of the first adhesive layer may be 5 μm or more and 20 μm or less. Specifically, the thickness of the first substrate may be 35 μm or more and 40 μm or less, and the thickness of the first adhesive layer may be 10 μm or more and 15 μm or less. By adjusting the thickness of the first substrate within the above-mentioned range, the first mask film can be easily handled. Furthermore, when the thickness of the first substrate is within the above-mentioned range, the first mask film can maintain excellent thermal shock resistance during the process of forming the first pattern portion, the second pattern portion, and the fourth pattern portion.
[0064] In addition, by adjusting the thickness of the first adhesive layer within the above-mentioned range, it is possible to effectively prevent the adhesive layer from remaining on one side of the mold substrate even after the first mask film is peeled off. Furthermore, by adjusting the thicknesses of the first substrate and the first adhesive layer within the above-mentioned range, it is possible to improve the durability of the first mask film and effectively prevent the occurrence of the shadowing phenomenon due to the thickness of the first mask film.
[0065] According to one embodiment of the present invention, the second mask film includes a second substrate and a second adhesive layer provided on one surface of the second substrate, and the glass transition temperature of the second substrate may be 230°C or more and 350°C or less, and the adhesive strength of the second adhesive layer may be 30gf / in or more and 80gf / in or less. Specifically, the glass transition temperature of the second substrate may be 250°C or more and 320°C or less, 280°C or more and 310°C or less, or 285°C or more and 300°C or less. The melting point of the second substrate may be 350°C or more and 450°C or less, and specifically, the melting point of the second substrate may be 370°C or more and 430°C or less, or 390°C or more and 410°C or less. Furthermore, the adhesive strength of the second adhesive layer may be 30 gf / in to 80 gf / in, 55 gf / in to 65 gf / in, 50 gf / in to 60 gf / in, or 65 gf / in to 70 gf / in at 25° C. against a stainless steel 304 substrate.
[0066] According to one embodiment of the present invention, the second substrate may be a polyimide substrate having the above-mentioned glass transition temperature, and the second adhesive layer may be a silicone-based adhesive layer having the above-mentioned adhesive strength.
[0067] According to one embodiment of the present invention, the glass transition temperatures of the first and second substrates can be measured using methods and equipment commonly used in the industry.
[0068] According to one embodiment of the present invention, in the step of forming the third pattern portion, the surface temperature of the mold substrate may be 110°C or more and 200°C or less. The step of forming the third pattern portion is performed by two plasma etchings. A pattern portion may be formed in the entire third region without a shutter, and the surface temperature of the mold substrate at this time may be 110°C or more and 130°C or less. After forming a pattern in the entire third region, a part of the mesh portion may be shielded with a shutter to perform plasma etching, and the surface temperature of the mold substrate not shielded by the shutter may be 180°C or more and 190°C or less.
[0069] Therefore, the second mask film including the second substrate having the above-mentioned glass transition temperature and / or melting point can withstand thermal shock during the plasma etching process for forming the third pattern portion. Specifically, when the glass transition temperature and / or melting point of the second substrate is within the above-mentioned range, damage to the mold substrate caused by plasma etching can be effectively suppressed in the region protected by the second mask film, i.e., the region other than the third region.
[0070] In addition, by adjusting the adhesive strength of the second adhesive layer within the above-mentioned range, the second mask film can be prevented from peeling off from one side of the mold substrate during the plasma etching process for forming the third pattern portion. Furthermore, when the adhesive strength of the second adhesive layer is within the above-mentioned range, the penetration of reactive gas between the second adhesive layer and the mold substrate during the process for forming the third pattern portion can be effectively suppressed, and the generation of air bubbles between the second adhesive layer and the mold substrate can be suppressed. This can effectively prevent damage from occurring on one side of the mold substrate. In addition, when the adhesive strength of the second adhesive layer is within the above-mentioned range, the second mask film can be easily peeled off after the process for forming the third pattern portion is completed, and even after the peeling of the second mask film that has been subjected to thermal shock, the residue of the adhesive layer can be effectively suppressed from remaining on one side of the mold substrate.
[0071] According to one embodiment of the present invention, the thickness of the second substrate may be 30 μm or more and 70 μm or less, and the thickness of the second adhesive layer may be 5 μm or more and 20 μm or less. Specifically, the thickness of the second substrate may be 45 μm or more and 55 μm or less, and the thickness of the second adhesive layer may be 5 μm or more and 8 μm or less. By adjusting the thickness of the second substrate within the above-mentioned range, the second mask film can be easily handled. Furthermore, when the thickness of the second substrate is within the above-mentioned range, the second mask film can maintain excellent thermal shock resistance during the formation of the third pattern portion.
[0072] In addition, by adjusting the thickness of the second adhesive layer within the above-mentioned range, it is possible to effectively prevent the adhesive layer from remaining on one side of the mold substrate even after the second mask film is peeled off. Furthermore, by adjusting the thicknesses of the second substrate and the second adhesive layer within the above-mentioned range, it is possible to improve the durability of the second mask film and effectively prevent the occurrence of the shadowing phenomenon due to the thickness of the second mask film.
[0073] In the present invention, the surface temperature of the mold substrate in the plasma etching process can be measured using a temperature detection tape. For example, after attaching the temperature detection tape to the surface of the mold substrate, the surface temperature of the mold substrate can be measured under the plasma etching process conditions for forming the first to fourth pattern portions.
[0074] The method for manufacturing a mold for a diffraction grating light guide plate according to an embodiment of the present invention can effectively reduce the time and cost required to manufacture the mold for a diffraction grating light guide plate by using optimal first and second mask films that can improve the efficiency of forming a pattern part. In addition, the method for manufacturing a mold for a diffraction grating light guide plate has a process advantage in that the mold for a diffraction grating light guide plate can be manufactured by only one replacement process using two mask films, the first and second mask films.
[0075] Furthermore, according to one embodiment of the present invention, the mold for the diffraction grating light guide plate can also be manufactured using a third mask film in which the second opening and the third opening are formed in separate areas, and a fourth mask film in which the first opening and the fourth opening are formed in separate areas.
[0076] In this case, the second and third openings of the third mask film and the first and fourth openings of the fourth mask film may be formed at positions corresponding to the positions where the first to fourth openings of the first and second mask films are formed. Also, the third mask film may be of the same type as the first mask film, and the fourth mask film may be of the same type as the second mask film.
[0077] Another embodiment of the present invention provides a method for manufacturing a diffraction grating light guide plate, comprising the steps of: preparing a mold for a diffraction grating light guide plate manufactured by the method for manufacturing a mold for a diffraction grating light guide plate; applying a resin composition onto one surface of the mold for the diffraction grating light guide plate on which a pattern portion is formed; and curing the resin composition.
[0078] According to one embodiment of the present invention, the resin composition may be any resin composition commonly used in the art. The step of applying the resin composition may be performed using a coating method commonly used in the art, such as spin coating, dip coating, or drop casting. The method of curing the resin composition may be any curing method commonly used in the art, without limitation. For example, when a photocurable resin composition is used, a photocuring method may be used, and when a thermosetting resin composition is used, a thermocuring method may be used.
[0079] According to an embodiment of the present invention, the manufactured diffraction grating light guide plate may include a pattern portion provided on a first region DOE1 where light is incident, a pattern portion provided on a second region DOE2 where the incident light moves while being diffused, a pattern portion provided on a third region DOE3 where the moved light is extracted, and a pattern portion provided on a fourth region DOE2-2 for guiding the light moving from the second region to the third region. Referring to FIG. 4, the pattern portion provided on the DOE1 of the manufactured diffraction grating light guide plate may correspond to the first pattern portion P1 of the mold 1000 for the diffraction grating light guide plate. Also, the pattern portion provided on the DOE2 of the diffraction grating light guide plate may correspond to the third pattern portion P3 of the mold 1000 for the diffraction grating light guide plate, and the pattern portion provided on the DOE2-2 of the diffraction grating light guide plate may correspond to the fourth pattern portion P4 of the mold 1000 for the diffraction grating light guide plate. Furthermore, a pattern portion provided on the DOE 3 of the diffraction grating light guide plate may correspond to the second pattern portion P2 of the mold 1000 for the diffraction grating light guide plate.
[0080] According to one embodiment of the present invention, the diffraction grating light guide plate can be directly used as a diffraction grating light guide plate. The diffraction grating light guide plate can also be used as an intermediate mold to manufacture a final product by duplicating the intermediate mold. Specifically, when the manufactured diffraction grating light guide plate is used as an intermediate mold to manufacture a diffraction grating light guide plate, the inclination of the grating pattern of the diffraction grating light guide plate used as the intermediate mold can be reversed. Furthermore, when a diffraction grating light guide plate is manufactured after a mold for a diffraction grating light guide plate is manufactured using a diffraction grating light guide plate with a reversed inclination of the grating pattern as an intermediate mold, a grating pattern in the same direction as that of the initial diffraction grating light guide plate can be realized.
[0081] [Example] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention can be modified into various different forms, and the scope of the present invention is not to be construed as being limited to the examples described below. The examples in the present specification are provided to more completely explain the present invention to those having average knowledge in the art.
[0082] Preparation of mask film Example 1 - Second mask film A polyimide (PI) film with a glass transition temperature of about 280°C, a melting point of about 390°C, and a thickness of about 50 μm was prepared as the substrate. A silicone-based adhesive film with a thickness of about 6 μm was also prepared as the adhesive layer. Then, the adhesive film was attached to one side of the PI film to produce a masking film. The produced masking film was cut to a size of 2.54 cm wide and 30 cm long to produce a sample, which was then attached to one side of stainless steel 304. Then, the force required to peel the sample from the stainless steel 304 was measured based on the evaluation method of ASTM D3330, and was found to be about 60 gf / in.
[0083] Example 2 - First mask film As the substrate, a polyethylene terephthalate (PET) film with a glass transition temperature of about 85°C, a melting point of about 280°C, and a thickness of about 38 μm was prepared. In addition, as the adhesive layer, a silicone-based adhesive film with a thickness of about 10 μm was prepared. Then, the adhesive film was attached to one side of the PET film to manufacture a mask film. Then, the adhesive strength of the adhesive layer was measured in the same manner as in Example 1, and the adhesive strength of the adhesive layer was about 40 gf / in.
[0084] Comparative Example 1 As the substrate, the PET film of Example 2 having a thickness of about 25 μm was prepared, and as the adhesive layer, a silicone-based adhesive film having a thickness of about 8 μm was prepared. After that, the adhesive film was attached to one side of the PET film to manufacture a mask film. After that, the adhesive strength of the adhesive layer was measured in the same manner as in Example 1, and the adhesive strength of the adhesive layer was about 25 gf / in.
[0085] Comparative Example 2 The PI film of Example 1 having a thickness of about 25 μm was prepared as the substrate, and an acrylate-based adhesive film having a thickness of about 25 μm was prepared as the adhesive layer. Then, the adhesive film was attached to one side of the PI film to produce a mask film. Then, the adhesive strength of the adhesive layer was measured in the same manner as in Example 1, and the adhesive strength of the adhesive layer was about 70 gf / in.
[0086] Comparative Example 3 The PI film of Example 1 having a thickness of about 25 μm was prepared as the substrate, and the silicone-based adhesive film having a thickness of about 10 μm was prepared as the adhesive layer. Then, the adhesive film was attached to one side of the PI film to produce a mask film. Then, the adhesive strength of the adhesive layer was measured in the same manner as in Example 1, and the adhesive strength of the adhesive layer was about 10 gf / in.
[0087] Comparative Example 4 The PI film of Example 1 having a thickness of about 25 μm was prepared as the substrate, and the silicone-based adhesive film having a thickness of about 10 μm was prepared as the adhesive layer. Then, the adhesive film was attached to one side of the PI film to produce a mask film. Then, the adhesive strength of the adhesive layer was measured in the same manner as in Example 1, and the adhesive strength of the adhesive layer was about 80 gf / in.
[0088] Comparative Example 5 The PI film of Example 1 having a thickness of about 50 μm was prepared as the substrate, and the silicone-based adhesive film having a thickness of about 10 μm was prepared as the adhesive layer. After that, the adhesive film was attached to one side of the PI film to produce a mask film. After that, the adhesive strength of the adhesive layer was measured in the same manner as in Example 1, and the adhesive strength of the adhesive layer was about 10 gf / in.
[0089] Measurement of the surface temperature of substrate molds during plasma etching process A Faraday cage was prepared with a mesh surface resistance of 0.5605 Ω / □ and a stainless steel (SUS304) plate at the bottom. The Faraday cage was placed in an inductively coupled plasma reactive ion etching device (ICP-RIE) (Oxford's plasmaLab system 100).
[0090] A quartz substrate was prepared as a mold base material, and a temperature detection tape was attached to one surface of the quartz substrate.
[0091] First pattern portion forming step A support made of aluminum with a 40° inclination was installed inside the Faraday cage, and the quartz substrate with the temperature detection tape was placed on the support without blocking the mesh part with a separate shutter.
[0092] After this, plasma etching was performed using ICP-RIE (Oxford's plasmaLab system100), and the reactive gas was a mixture of O2 and C4F8 in a ratio of 5:45, which was supplied at a flow rate of 50sccm. The etching conditions were ICP power 2kW, RF power 150W, and operating pressure 7-10mTorr, and the etching was performed for 4 minutes. At this time, the maximum surface temperature of the quartz substrate measured with a temperature detection tape was about 160°C.
[0093] Second pattern portion forming step A support made of aluminum with a 40° inclination was installed inside the Faraday cage, and the quartz substrate with the temperature detection tape was placed on the support without blocking the mesh part with a separate shutter.
[0094] After that, the reactive gas was supplied under the same conditions as the first pattern forming step, and etching was performed for 4 minutes with an ICP power of 2 kW, an RF power of 150 W, and an operating pressure of 7 to 10 mTorr. At this time, the maximum surface temperature of the quartz substrate measured with a temperature detection tape was about 110°C.
[0095] Then, the shutter was placed on the mesh section so that half of the quartz substrate was covered by the shutter. Reactive gas was supplied under the same conditions as in the first pattern section formation step, and etching was performed for 5 minutes at ICP power 2kW, RF power 150W, and operating pressure of 7-10mTorr. At this time, the maximum surface temperature of the quartz substrate area not covered by the shutter was about 140°C.
[0096] Third pattern portion forming step The quartz substrate with the temperature detection tape was placed on the bottom of the Faraday cage, and the mesh portion was not blocked by a separate shutter.
[0097] After that, the reactive gas was supplied under the same conditions as the first pattern forming step, and etching was performed for 3 minutes with an ICP power of 2 kW, an RF power of 150 W, and an operating pressure of 7 to 10 mTorr. At this time, the maximum surface temperature of the quartz substrate measured with a temperature detection tape was about 125°C.
[0098] Then, the shutter was placed on the mesh so that half of the quartz substrate was covered by the shutter. Reactive gas was supplied under the same conditions as above, and etching was performed for 7 minutes with ICP power of 2 kW, RF power of 150 W, and operating pressure of 7 to 10 mTorr. At this time, the maximum surface temperature of the quartz substrate area not covered by the shutter was about 190°C.
[0099] Fourth pattern portion forming step The quartz substrate with the temperature detection tape was placed on the bottom of the Faraday cage, and the mesh portion was not blocked by a separate shutter.
[0100] After that, the reactive gas was supplied under the same conditions as the first pattern forming step, and etching was performed for 4 minutes with an ICP power of 2 kW, an RF power of 150 W, and an operating pressure of 7 to 10 mTorr. At this time, the maximum surface temperature of the quartz substrate measured with a temperature detection tape was about 155°C.
[0101] Mask film test (general ICP-RIE) The quartz substrate with the temperature detection tape was placed in an inductively coupled plasma reactive ion etching device (ICP-RIE) (Oxford's plasmaLab system 100). After this, O2 and C4F8 were mixed in a ratio of 5:45 as reactive gas and supplied at a flow rate of 50sccm. The etching conditions were ICP power 2kW, RF power 150W, and operating pressure 7-10mTorr, and etching was performed for 4 minutes. At this time, it was confirmed that the average surface temperature of the quartz substrate measured with the temperature detection tape was about 235°C.
[0102] Mask films of Examples 1 and 2 and Comparative Examples 1 to 5 were prepared, and openings were formed in predetermined areas of the mask films. Thereafter, the quartz substrate samples to which the mask films of Examples 1 and 2 and Comparative Examples 1 to 5 were attached were placed in an inductively coupled plasma reactive ion etching apparatus, and plasma etching was performed under the same conditions as described above.
[0103] FIG. 5 is a photograph of the mask film manufactured in Example 1 of the present invention after plasma etching. Specifically, FIG. 5(a) is a photograph of the mask film manufactured in Example 1 after plasma etching, and FIG. 5(b) is a photograph of the quartz substrate after the mask film is peeled off. Referring to FIG. 5(a), it was confirmed that in the case of the mask film manufactured in Example 1, there is no thermal deformation of the substrate due to plasma etching, and no adhesive residue occurs near the quartz substrate exposed by the opening. Also, referring to FIG. 5(b), it was confirmed that no adhesive layer residue remains on the surface of the quartz substrate from which the mask film of Example 1 is peeled off after plasma etching.
[0104] Figure 6 is a photograph taken after plasma etching of the mask film manufactured in Comparative Example 3. Referring to Figure 6, in the case of the mask film manufactured in Comparative Example 3 in which the thickness of the PI substrate is about 25 μm and the adhesive strength of the adhesive layer is about 10 gf / in, it was confirmed that the substrate was thermally deformed, causing wrinkles and air bubbles, and that glue residue occurred on the surface of the quartz substrate exposed by the opening.
[0105] Fig. 7 is a photograph of the mask film manufactured in Comparative Example 5 after plasma etching. Specifically, Fig. 7(a) is a photograph of the mask film manufactured in Comparative Example 5 after plasma etching, and Fig. 7(b) is a photograph of the quartz substrate after the mask film is peeled off. Referring to Fig. 7, in the case of the mask film manufactured in Comparative Example 5, in which the adhesive strength of the adhesive layer is about 10 gf / in, it was confirmed that the adhesive strength of the adhesive layer was poor, and gas penetrated between the adhesive layer and the quartz substrate, causing damage to the quartz substrate, and that a glue residue phenomenon occurred at the corners of the mask film.
[0106] In addition, it was confirmed that thermal deformation occurred in the masking films manufactured in Example 2, Comparative Example 1, Comparative Example 3, and Comparative Example 4 of the present invention. In particular, in the case of Comparative Example 2, which used an acrylate-based adhesive film, it was confirmed that the adhesive layer was denatured, resulting in a large amount of adhesive residue.
[0107] Mask Film Test (ICP-RIE with Faraday Cage) A Faraday cage was prepared with a mesh surface resistance of 0.5605 Ω / □ and a stainless steel (SUS304) plate at the bottom. The Faraday cage was placed in an inductively coupled plasma reactive ion etching device (ICP-RIE) (Oxford's plasmaLab system 100).
[0108] Mask film test of Example 1 The mask film of Example 1 was prepared, and an opening was formed in a predetermined area of the mask film. After that, the mask film of Example 1 was attached to a quartz substrate and placed in a Faraday cage as shown in FIG. 2A.
[0109] After this, the shutter was placed on the mesh so that half of the quartz substrate was covered by the shutter. Reactive gases, O2 and C4F8, were mixed in a ratio of 5:45 and supplied at a flow rate of 50sccm. Etching was performed for 7 minutes with an ICP power of 2kW, an RF power of 150W, and an operating pressure of 7-10mTorr.
[0110] It was confirmed that the mask film manufactured in Example 1 did not undergo thermal deformation of the substrate due to plasma etching, and no adhesive residue occurred near the quartz substrate exposed by the opening. It was also confirmed that no adhesive layer residue remained on the surface of the quartz substrate from which the mask film of Example 1 was peeled off after plasma etching.
[0111] Mask film test of Example 2 The mask film of Example 2 was prepared, and an opening was formed in a predetermined area of the mask film. After that, the mask film of Example 2 was attached to a quartz substrate and placed in a Faraday cage as shown in FIG. 2D.
[0112] After this, the shutter was placed on the mesh so that half of the quartz substrate was covered by the shutter. Reactive gases, O2 and C4F8, were mixed in a ratio of 5:45 and supplied at a flow rate of 50sccm. Etching was performed for 5 minutes with an ICP power of 2kW, an RF power of 150W, and an operating pressure of 7-10mTorr.
[0113] It was confirmed that the mask film manufactured in Example 2 hardly had any thermal deformation of the substrate due to plasma etching, and no adhesive residue occurred near the quartz substrate exposed by the opening. In addition, it was confirmed that no adhesive layer residue remained on the surface of the quartz substrate from which the mask film of Example 2 was peeled off after the plasma etching process.
[0114] Therefore, it can be seen that by using the mask film of Example 1 as a second mask film according to one embodiment of the present invention and the mask film of Example 2 as a first mask film according to one embodiment of the present invention, the first pattern portion to the fourth pattern portion can be easily formed on the mold substrate. [Explanation of symbols]
[0115] 100:Mold base material 200, 200': 1st mask film 300: 2nd mask film H1: 1st opening H2: 2nd opening H3: 3rd opening H4: 4th opening 400: Faraday cage 410: Mesh section 420: Shutter 430: Support stand P1: First pattern part P2: Second pattern part P3: Third pattern section P4: 4th pattern part 1000: Mold for diffraction grating light guide plate
Claims
1. providing a first mask film including a first opening and a second opening formed in separate regions; a step of attaching the first mask film onto one surface of a mold base material, opening only the first opening, placing the mold base material with the first mask film attached within a Faraday cage having a mesh portion on an upper surface thereof, and forming a first pattern portion on a first region of the one surface of the mold base material exposed by the first opening using plasma etching; forming a second pattern portion on a second region of the one surface of the mold base material exposed by the second opening using plasma etching after opening only the second opening; preparing a second mask film having a third opening formed in one region, and removing the first mask film from one surface of the mold base material; attaching the second mask film onto one surface of the mold base, and forming a third pattern portion on a third region of the one surface of the mold base exposed by the third opening using plasma etching; The first mask film includes a first substrate and a first adhesive layer provided on one surface of the first substrate, the glass transition temperature of the first substrate being 70° C. or more and 100° C. or less, and the adhesive strength of the first adhesive layer being 30 gf / in. or more and 50 gf / in. or less, the second mask film includes a second substrate and a second adhesive layer provided on one surface of the second substrate, the second substrate having a glass transition temperature of 230° C. or higher and 350° C. or lower, and the second adhesive layer having an adhesive strength of 30 gf / in or higher and 80 gf / in or lower.
2. the first mask film additionally includes a fourth opening; 2. The method for manufacturing a mold for a diffraction grating light guide plate according to claim 1, further comprising the step of forming a fourth pattern portion on a fourth region of one surface of the mold base material exposed by the fourth opening by using plasma etching after opening only the fourth opening.
3. The step of forming the first pattern portion includes:
3. The method for manufacturing a mold for a diffraction grating light guide plate according to claim 1, further comprising: positioning one surface of the mold base material at an incline against a bottom surface of the Faraday cage, and performing plasma etching to form an inclined pattern portion.
4. The step of forming the second pattern portion includes:
4. A method for manufacturing a mold for a diffraction grating light guide plate according to claim 1, comprising: positioning one surface of the mold base material at an incline toward a bottom surface of the Faraday cage; shielding at least a portion of the mesh portion with a shutter; and performing plasma etching to form an inclined pattern portion having a depth gradient.
5. The step of forming the third pattern portion includes:
5. A method for manufacturing a mold for a diffraction grating light guide plate according to claim 1, comprising: positioning one surface of the mold substrate parallel to a bottom surface of the Faraday cage, shielding at least a portion of the mesh portion with a shutter, and then performing plasma etching to form a pattern portion having a depth gradient.
6. The step of forming the fourth pattern portion includes: The method for manufacturing a mold for a diffraction grating light guide plate according to claim 2 , further comprising: positioning one surface of the mold base material parallel to a bottom surface of the Faraday cage and performing plasma etching.
7. The method for producing a mold for a diffraction grating light guide plate according to claim 4 , wherein the shutter blocks 20% to 80% of the area of the mesh portion.
8. The thickness of the first base material is 30 μm or more and 50 μm or less, The method for producing a mold for a diffraction grating light guide plate according to claim 1 , wherein the first adhesive layer has a thickness of 5 μm or more and 20 μm or less.
9. The thickness of the second base material is 30 μm or more and 70 μm or less, The method for producing a mold for a diffraction grating light guide plate according to claim 1 , wherein the second adhesive layer has a thickness of 5 μm or more and 20 μm or less.
10. The method for producing a mold for a diffraction grating light guide plate according to claim 1 , wherein the mesh portion has a surface resistance of 0.5 Ω / □ or more.
11. A method for manufacturing a mold for a diffraction grating light guide plate according to any one of claims 1 to 10, applying a resin composition onto one surface of the mold for the diffraction grating light guide plate on which a pattern portion is formed; and curing the resin composition.
Citation Information
Patent Citations
Adhesive sheet and circuit board using the same and method for manufacturing the same
JP2001352171A
Transfer die, diffraction grating and optical device using transfer die, projection / depression formation method using transfer die and method for manufacturing diffraction grating using projection / depression formation method
JP2015093399A
Device chip manufacturing method
JP2017162999A
Reactive sputter etching apparatus
US4309267A
Self-limiting isotropic wet etching process
US6379573B1