Fixing belt and method for manufacturing the same
The fixing belt with a sliding layer containing anisotropic fillers and controlled Benard cells addresses abrasion resistance and surface roughness issues, enhancing durability and performance in electrophotographic devices.
Patent Information
- Application Number
- JP2020147983
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-09-03
AI Technical Summary
Existing fixing belts in electrophotographic image forming devices face issues with reduced abrasion resistance in the belt rotation direction due to filler orientation, difficulty in achieving desired surface roughness, and potential impairment of lubricant retention, leading to problems like stick-slip and torque increase.
The fixing belt features a sliding layer with fillers having shape anisotropy, where the orientation ratio of fillers is varied across different positions, and includes Benard cells with specific size and roughness ranges, along with controlled drying and coating processes to enhance wear resistance and lubricant retention.
The solution improves abrasion resistance, reduces torque increase, and minimizes stick-slip phenomena throughout the durability life of the fixing belt, maintaining effective sliding properties and fixing performance.
Smart Images

Figure 0007570852000006 
Figure 0007570852000007 
Figure 0007570852000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a fixing belt that is applied to an image forming apparatus of an electrophotographic system, an electrostatic recording system, or the like, and a manufacturing method thereof. [Background technology]
[0002] Conventionally, in the fixing device used in electrophotographic image forming apparatuses such as copying machines and laser printers, a belt heating type fixing device is widely used, which heats toner on a recording material with heat from a heater through a fixing belt having a small heat capacity. In such a fixing device, a fixing nip is formed between the fixing belt and the rotating body by being sandwiched between a roller-shaped rotating body provided on the outside and a backup member provided on the inside. In such a fixing device, friction and wear may occur between the inner peripheral surface of the fixing belt and the backup member, and as the durability progresses, problems such as self-excited vibration called stick-slip and torque increase may occur.
[0003] To solve this problem, a fixing belt has been developed in which fillers having specific shapes, such as needle-like, whisker-like, or fibrous shapes, are blended into the sliding layer on the inner periphery of the fixing belt, and the orientation rate of the fillers in the rotation axis direction of the fixing belt is increased (see Patent Document 1). With this fixing belt, the fillers oriented in the rotation axis direction improve the sliding properties, wear resistance, and lubricant retention, and the life span can be extended. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-228729 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the fixing device described in the above-mentioned Patent Document 1, since the filler is oriented in the direction of the rotation axis of the fixing belt, it is difficult to obtain abrasion resistance in the belt rotation direction, which is the sliding direction between the fixing belt and the backup member. In addition, it is desired that the fixing belt has a surface roughness that reduces the actual contact area with the backup member and retains the lubricant interposed between the belt and the backup member. In contrast, with the above-mentioned filler orientation, it is difficult to effectively obtain such a desired surface roughness with a small filler content. In addition, if the filler content is increased to obtain the desired surface roughness, there is a risk that the abrasion resistance of the sliding layer will be impaired.
[0006] An object of the present invention is to provide a fixing belt capable of improving abrasion resistance and a method for manufacturing the fixing belt. [Means for solving the problem]
[0007] The fixing belt of the present invention is a rotatable endless fixing belt that heats an unfixed toner image carried on a recording material and fixes it to the recording material, and is sandwiched between a rotating body provided on the outside of the fixing belt and a backup member provided on the inside of the fixing belt, thereby forming a nip portion between the rotating body and the fixing belt, where the toner image is fixed to the recording material, the fixing belt comprising a substrate and a sliding layer formed on the inner peripheral side of the substrate and sliding in contact with the backup member, the sliding layer containing a filler having shape anisotropy, and characterized in that, when a direction along the inner peripheral surface of the substrate is taken as a reference direction, an orientation rate of the filler in the reference direction at a first position in the thickness direction of the sliding layer is a first value, and an orientation rate of the filler in the reference direction at a second position located on the inner peripheral surface side of the sliding layer than the first position is a second value smaller than the first value.
[0008] The fixing belt of the present invention is a rotatable endless fixing belt which heats an unfixed toner image carried on a recording material and fixes it to the recording material, and is sandwiched between a rotating body provided on the outside of the fixing belt and a backup member provided on the inside of the fixing belt, thereby forming a nip portion between the rotating body and the fixing belt, where the toner image is fixed to the recording material, the fixing belt comprising: a substrate; and a sliding layer formed on the inner peripheral side of the substrate and in contact with and sliding against the backup member, the sliding layer containing a filler having shape anisotropy, the sliding layer having a plurality of Benard cells on its inner peripheral surface, the plurality of cells having an average diameter of 50 μm or more and less than 200 μm, and the arithmetic mean roughness of the inner peripheral surface being 0.20 μm or more and 0.50 μm or less.
[0009] The present invention also provides a method for producing a fixing belt, comprising: a rotatable endless fixing belt for heating an unfixed toner image carried on a recording material and fixing the toner image to the recording material, the fixing belt being sandwiched between a rotating body provided on the outside of the fixing belt and a backup member provided on the inside of the fixing belt to form a nip portion between the rotating body and the fixing belt, where the toner image is fixed to the recording material, the fixing belt comprising a substrate and a sliding layer formed on an inner peripheral side of the substrate and in contact with and slid against the backup member, the fixing belt comprising a precursor of the sliding layer and The aspect ratio is between 5 and 200. The method includes a coating step of coating a solution in which a filler is dispersed in a solvent, and a drying step of drying the solvent from the solution coated on the inner peripheral surface of the substrate, and is characterized in that in the drying step, when the temperature of the outer peripheral surface of the substrate is set to a first temperature and the temperature of the atmosphere on the inner peripheral side of the sliding layer is set to a second temperature lower than the first temperature, the solvent is dried such that the difference between the first temperature and the second temperature is 10°C or more and 30°C or less. Effect of the Invention
[0010] According to the present invention, the abrasion resistance can be improved. [Brief description of the drawings]
[0011] [Figure 1] 1 is a cross-sectional view showing a schematic configuration of an image forming apparatus according to a first embodiment. [Diagram 2] 1 is a cross-sectional view showing a schematic configuration of a fixing device according to a first embodiment. [Diagram 3] 1 is a cross-sectional view showing a schematic configuration of a fixing belt according to a first embodiment. [Figure 4] 5 is a flowchart showing a procedure for forming a sliding layer of the fixing belt according to the first embodiment. [Diagram 5] FIG. 2 is a schematic diagram showing a coating device for forming a sliding layer of the fixing belt according to the first embodiment. [Figure 6] FIG. 2 is a schematic diagram showing a heating and drying furnace for forming a sliding layer of the fixing belt according to the first embodiment. [Figure 7] 3 is a schematic diagram of an SEM image of a cross section of the fixing belt according to the first embodiment. FIG. [Figure 8] FIG. 11 is a schematic diagram showing a Benard cell in a cross section of a fixing belt according to a second embodiment. [Figure 9] 10A and 10B are longitudinal sectional views of a fixing belt according to a fourth embodiment, in which (a) shows the state after a coating step and before a drying step, and (b) shows the state after baking. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <First embodiment> The first embodiment will be described with reference to Figures 1 to 7. First, the schematic configuration of an image forming apparatus according to the present embodiment will be described with reference to Figure 1.
[0013] [Image forming equipment] The image forming apparatus 100 has a photosensitive drum (photoconductor) 101 as an image carrier, and the photosensitive drum 101 is rotated at a predetermined process speed (circumferential speed) in the direction of the arrow. The surface of the photosensitive drum 101 is charged to a predetermined polarity by a charging roller 102 as a charging device during the rotation process. Next, the charged surface is exposed to a laser beam 103 output from an exposure device 110 constituted by a laser optical system based on input image information. The exposure device 110 outputs the laser beam 103 modulated (on / off) in response to pixel signals corresponding to each color of image information from an external terminal such as an image reading device (not shown) or a personal computer. Then, the surface of the photosensitive drum 101 is scanned and exposed. As a result, an electrostatic latent image corresponding to the image information is formed on the surface of the photosensitive drum 101 by this scanning exposure. The laser beam 103 output from the exposure device 110 is deflected by a deflection mirror 109 to an exposure position of the photosensitive drum 101.
[0014] The electrostatic latent image formed on the photosensitive drum 101 is visualized as a yellow toner image by the developing device 104Y using yellow toner. This yellow toner image is transferred onto the surface of the intermediate transfer drum 105 at a primary transfer portion T1, which is a contact portion between the photosensitive drum 101 and the intermediate transfer drum 105. Any toner remaining on the surface of the photosensitive drum 101 is cleaned by a cleaner 107.
[0015] The above-mentioned process cycle of charging, exposing, developing, primary transfer, and cleaning is repeated in the same manner when forming a magenta toner image, a cyan toner image, and a black toner image. That is, when forming a magenta toner image, the electrostatic latent image formed on the photosensitive drum 101 corresponding to magenta is visualized as a magenta toner image by the developing device 104M using magenta toner. Similarly, the cyan toner image is visualized by the developing device 104C, and the black toner image is visualized by the developing device 104K.
[0016] The toner images of each color formed in this way on the intermediate transfer drum 105 in sequence are transferred collectively onto the recording material S (paper, sheet material such as an OHP sheet, etc.) at the secondary transfer portion T2, which is a contact portion with the transfer roller 106. The toner remaining on the intermediate transfer drum 105 is cleaned by the toner cleaner 108. The toner cleaner 108 is capable of moving in and out of contact with the intermediate transfer drum 105, and is configured to be in contact with the intermediate transfer drum 105 only when cleaning the intermediate transfer drum 105. The transfer roller 106 is also capable of moving in and out of contact with the intermediate transfer drum 105, and is configured to be in contact with the intermediate transfer drum 105 only during secondary transfer. The recording material S that has passed through the secondary transfer portion T2 is introduced into the fixing device 200, which serves as a heating device, and is subjected to a fixing process (image heating process) of the unfixed toner image carried thereon. The recording material S that has been subjected to the fixing process is then discharged outside the machine, and a series of image forming operations is completed.
[0017] [Fixing device] Next, a schematic configuration of the fixing device 200 will be described with reference to FIG. 2. The fixing device 200 has a fixing belt 201 as a heating member, a pressure roller 206 as a rotating body, and the like. Then, between the fixing belt 201 and the pressure roller 206, a fixing nip portion N that is a nip portion that sandwiches and conveys the recording material S introduced into the fixing device 200 as described above is formed. As will be described in detail later, the fixing belt 201 is an endless belt provided with a silicone rubber elastic layer or the like, and is a rotating member that rotates with the recording material in contact with its surface (outer surface). Also, the fixing belt 201 is a fixing rotating body for fixing a toner image formed on the recording material S.
[0018] A fixing heater 202, a heater holder 204, a fixing belt stay 205, etc. are arranged inside the fixing belt 201. The fixing heater 202 is a heat source that presses the fixing belt 201 against the pressure roller 206 and heats the fixing belt 201, and is composed of, for example, a ceramic heater. For example, the fixing heater 202 has an alumina substrate and a resistance heating element formed by applying a conductive paste containing a silver-palladium alloy on the substrate in a uniform film shape of about 10 μm thickness by screen printing. A glass coating of pressure-resistant glass is further applied on the substrate to form a ceramic heater. The fixing heater 202 generates heat when electricity is applied.
[0019] The fixing heater 202 is disposed along the longitudinal direction of the fixing belt 201 (the direction along the surface of the fixing belt 201 and perpendicular to the direction of rotation) so that the inner surface of the fixing belt 201 and its heating surface can slide on each other. A semi-solid lubricant, which will be described later, is applied to the inner surface of the fixing belt 201 to ensure sliding properties between the fixing heater 202 and the heater holder 204.
[0020] The heater holder 204 is made of a material having high heat resistance, such as a liquid crystal polymer resin, and is formed long in the longitudinal direction of the fixing belt 201. It holds the fixing heater 202 and also serves to give the fixing belt 201 a shape for separating it from the recording material S. That is, the fixing heater 202 is fixed to the surface of the heater holder 204 on the pressure roller 206 side. In addition, cylindrical support parts are integrally provided at both ends of the heater holder 204 in the longitudinal direction, and both ends of the fixing belt 201 in the longitudinal direction are fitted onto the support parts with some degree of freedom. This supports the fixing belt 201 so that it can rotate freely, and makes the fixing belt 201 approximately cylindrical, making it easier to separate the recording material S due to its curvature.
[0021] The fixing belt stay 205 is disposed along the longitudinal direction of the fixing belt 201 on the opposite side of the heater holder 204 to the fixing heater 202, and both ends of the fixing belt stay 205 are urged toward the pressure roller 206 by a pressure mechanism (not shown). For example, one end of the fixing belt stay 205 is urged toward the pressure roller 206 with a force of 156.8 N (16 kgf), total pressure of 313.6 N (32 kgf). The heating surface of the fixing heater 202 is pressed against the pressure roller 206 (described below) via the heater holder 204 and the fixing belt 201 with a predetermined pressing force. This causes the pressure roller 206 to elastically deform, and a fixing nip N of a predetermined width required for fixing is formed between the fixing belt 201 and the pressure roller 206.
[0022] The pressure roller 206 is an elastic roller with a multi-layer structure in which, for example, a silicone rubber elastic layer with a thickness of about 3 mm and further, for example, a PFA resin tube with a thickness of about 40 μm are laminated on a metal core. PFA is a tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer. The pressure roller 206 is arranged so that its rotation axis direction (longitudinal direction) is approximately parallel to the longitudinal direction of the fixing belt 201, and both longitudinal ends of the core are rotatably supported by bearings between the rear and front side plates (not shown) of the frame 213 of the fixing device 200. The pressure roller 206 is rotated at a predetermined peripheral speed in the direction of the arrow by a motor, which is a driving source (not shown). The fixing belt 201, which is in a pressure-contact relationship with the pressure roller 206, rotates at a predetermined speed driven by the pressure roller 206. At this time, the fixing belt 201 is guided by the heater holder 204 while its inner surface is in close contact with and sliding against the heating surface of the fixing heater 202, and is rotated in the direction of the arrow.
[0023] A thermistor 203 is provided on the back surface (the surface opposite to the heating surface) of the fixing heater 202 to detect the temperature of the fixing heater 202. Thermistor 203 is disposed so as to be in contact with the back surface of the fixing heater 202, and is connected via an A / D converter 209 to a control circuit section (CPU) 210 serving as a control means.
[0024] This control circuit section 210 samples the output from the thermistor 203 at a predetermined cycle, and reflects the temperature information thus obtained in the temperature control of the fixing heater 202. In other words, the control circuit section 210 determines the temperature control content of the fixing heater 202 based on the output of the thermistor 203. Then, a heater drive circuit section 211 controls the supply of electricity to the fixing heater 202 so that the temperature of the fixing heater 202 becomes a target temperature (set temperature). The control circuit section 210 is also connected to a motor that drives the pressure roller 206 via an A / D converter 209, and controls the drive of the pressure roller 206.
[0025] The fixing device 200 thus configured forms a fixing nip portion N between the fixing belt 201 and the pressure roller 206 as described above. As shown in Fig. 2, when the recording material S carrying the toner image t is transported in the direction of the arrow, the recording material S is guided to the fixing nip portion N by a transport guide 207. Then, when the recording material S is nipped and transported in the fixing nip portion N, the surface of the recording material S carrying the toner image t comes into contact with the fixing belt 201 and is heated and pressurized, so that the toner image t is fixed to the recording material S. Thereafter, the recording material S is transported out of the fixing device 200 by a discharge roller 208.
[0026] [Fuser belt configuration] Next, the configuration of the fixing belt 201 will be described in detail with reference to Fig. 3. The fixing belt 201 is a rotatable endless belt that heats an unfixed toner image carried on the recording material S and fixes the toner image to the recording material S. The fixing belt 201 is sandwiched between a pressure roller 206 provided on the outside of the fixing belt 201 and a fixing heater 202 provided on the inside of the fixing belt 201 as a backup member, and forms a fixing nip portion N between the pressure roller 206 and the fixing belt 201.
[0027] As shown in FIG. 3, the fixing belt 201 includes a substrate 1 formed in an endless shape, a sliding layer 2, an elastic layer 3, and a release layer 4. The sliding layer 2 is formed on the inner peripheral surface of the substrate 1. The sliding layer 2 is provided to improve the sliding property with the fixing heater 202, and is brought into contact with and slid on the fixing heater 202, and contains a filler 2a having shape anisotropy. The elastic layer 3 is an elastic layer made of silicone rubber that covers the outer peripheral surface of the substrate 1 via a primer layer (not shown). The release layer 4 is a release layer (fluororesin layer) made of resin (fluororesin), and is provided on the outer peripheral surface of the elastic layer 3 via an adhesive layer (not shown).
[0028] Next, the substrate 1, the sliding layer 2, the elastic layer 3, and the release layer 4 of the fixing belt 201 described above will be described in more detail.
[0029] [Base] Considering the need for heat resistance and bending resistance, metals such as stainless steel (SUS), nickel, and nickel alloys are preferably used for the base 1. Since the base 1 needs to have a small heat capacity while having high mechanical strength, it is desirable for the thickness to be 20 to 50 μm, preferably 25 to 45 μm. In this embodiment, SUS with an inner diameter of 24 mm and a thickness of 30 μm is used as the base material.
[0030] [Sliding layer] For the sliding layer 2, a resin having high durability and high heat resistance, such as polyimide resin, polyamideimide resin, or polyetheretherketone resin, is suitable. In particular, polyimide resin is preferable in terms of ease of production, heat resistance, elastic modulus, strength, etc. When the sliding layer 2 is formed from a polyimide resin, for example, the following is performed. A polyimide precursor solution obtained by reacting an aromatic tetracarboxylic dianhydride or its derivative with an aromatic diamine in an organic polar solvent is applied to the inner surface of the above-mentioned base 1, dried, heated, and dehydrated and cyclized (see FIG. ). This allows the sliding layer 2 made of polyimide resin to be formed on the inner surface of the base 1. The thickness of the sliding layer 2 is preferably about 5 to 25 μm. In particular, if it is about 7 to 20 μm, it is easy to achieve both wear resistance at the fixing nip portion N and heat transferability for transmitting heat from the heater to the base 1.
[0031] [Polyimide precursor solution] Representative examples of aromatic tetracarboxylic dianhydrides include the following, and these aromatic tetracarboxylic dianhydrides can be used alone or in combination of two or more kinds. (1) Pyromellitic dianhydride (2) 3,3',4,4'-biphenyltetracarboxylic dianhydride (3) 3,3',4,4'-Benzophenonetetracarboxylic dianhydride (4) 2,3,6,7-Naphthalenetetracarboxylic dianhydride
[0032] Representative examples of aromatic diamines include the following, and these aromatic diamines can be used alone or in combination of two or more. (1) 4,4'-oxydianiline (4,4'-ODA) (2) Paraphenylenediamine (PPDA) (3) Metaphenylenediamine (MPDA)
[0033] Examples of organic polar solvents include the following: (1) N,N-Dimethylacetamide (DMAc) (2) Dimethylformamide (DMF) (3) N-methyl-2-pyrrolidone (NMP)
[0034] [Filler] The filler 2a is blended to impart surface roughness and abrasion resistance to the sliding layer 2, and therefore preferably has shape anisotropy, and is particularly preferably a scaly filler. Examples of the material of the filler 2a include the following. (1) Fluorphlogopite (KMg3(AlSi3)O 10 F2) and potassium tetrasilicic mica (KMg 2.5 SiO 10 F2) (2) Sodium tetrasilicic mica (NaMg2.5 SiO 10 F2) and sodium hectorite (Na 0.33 Mg 2.67 Li 0.33 SiO 10 F2) (3) Silica (SiO2) Hexagonal Boron Nitride (BN) (4) Graphite (5) Graphene
[0035] As a method for dispersing the filler 2a in the polyimide precursor solution, the following method may be mentioned as an example. (1) A method in which the filler 2a is directly added to the polyimide precursor solution, premixed with a mixer or other mixing device, and then dispersed with a three-roll mill or the like. (2) A method in which filler 2a is added to a polar solvent (such as NMP) similar to the polyimide precursor solution in advance, a filler dispersion solvent is prepared using a sand mill or a bead mill, and then the filler is mixed with a separately obtained polyimide precursor solution using a mixer or other mixer.
[0036] The aspect ratio of the filler 2a (ratio of long side to short side) is preferably 5 or more and about 200 or less. In particular, if it is 30 or more and about 100 or less, the orientation rate of the filler 2a in the surface direction in the sliding layer 2 obtained in the process of coating and drying a polyimide precursor solution described later tends to be inner circumferential surface side (surface side) < substrate side. This makes it easier to obtain the effect of improving the sliding properties and lubricant retention on the inner circumferential surface side.
[0037] The optimum amount of the filler 2a varies depending on the type of polyimide precursor solution and filler 2a. For example, in order to adjust the surface roughness of the sliding layer 2 to an appropriate range and to keep the wear resistance of the sliding layer 2 within a range that does not impair the wear resistance, the filler 2a is preferably 7% by volume or more and 15% by volume or less with respect to the volume of the sliding layer 2. If the volume of the filler 2a is less than 7% by volume, it is difficult to obtain the surface roughness required to reduce the real contact area with the sliding counter material and to obtain the retention of the intervening lubricant. Also, if the volume of the filler 2a is more than 15% by volume, the polyimide becomes hard and brittle due to the filler 2a, impairing the wear resistance, and it becomes difficult to maintain the appropriate surface roughness, i.e., the sliding property and the lubricant retention, throughout the durability.
[0038] [Method of forming the sliding layer] Next, the procedure for forming the sliding layer will be described with reference to Figures 4 to 6. In order to make the thickness of the sliding layer 2 about 12 µm, the polyimide precursor solution 5 containing the filler 2a is applied to the inner surface of the substrate 1 by a ring coating method or the like so as to have a thickness of about 70 to 80 µm.
[0039] As shown in Fig. 4, first, the substrate 1 is placed in a coating device 20 (step S1), and the inner surface of the substrate 1 is coated with a polyimide precursor solution 5 (step S2, coating step). This coating step will be specifically described with reference to Fig. 5. In Fig. 5, U indicates the upward direction, and L indicates the downward direction.
[0040] 5 is a schematic diagram of a coating device 20 for the ring coating method. Supports 22 and 23 are formed on a base 21. A coating head 24 is fixed on the support 22 and connected to a coating liquid supply device (not shown). A work moving device 25 is provided on the support 23 so as to be capable of ascending and descending, and a work hand 26 that holds the base body 1 is provided on the work moving device 25. The work moving device 25 can be moved up and down by a motor 27 provided on the support 23, and the work hand 26 that holds the base body 1 can also be moved up and down by the movement of the work moving device 25.
[0041] A slit (not shown) perpendicular to the axis of the cylinder is formed on the outer periphery of the coating head 24. A polyimide precursor solution 5 containing a filler 2a mixed therein to be uniform is supplied to the outside through the slit, and the inner periphery of the substrate 1 is coated by moving the substrate 1 in the vertical direction along the outer periphery of the coating head 24. In this coating device 20, the thickness of the sliding layer 2 is determined by the coating amount, and any coating amount can be obtained by changing the clearance, the supply speed of the polyimide precursor solution 5, and the movement speed of the workpiece moving device 25.
[0042] Next, as shown in Fig. 4, the substrate 1 coated with the polyimide precursor solution 5 is placed in a heating and drying furnace 30 (step S3), and the polyimide precursor solution 5 is dried (step S4, drying step). In this way, after the polyimide precursor solution 5 containing the filler 2a is coated on the inner surface of the substrate 1, the substrate is heated to evaporate the organic polar solvent contained in the polyimide precursor solution 5, thereby increasing the viscosity of the polyimide precursor solution 5 and maintaining its shape. This drying step will be specifically described with reference to Fig. 6. In Fig. 6, U indicates the upward direction, and L indicates the downward direction.
[0043] 6 is a schematic diagram of a heating and drying furnace 30. The heating and drying furnace 30 has a heating cylinder 31 that accommodates the substrate 1, an inlet 32 that is provided at the bottom of the heating cylinder 31 and allows high-temperature oil to flow into the heating cylinder 31, and an outlet 33 that is provided at the top of the heating cylinder 31 and allows high-temperature oil inside the heating cylinder 31 to flow out. The heating and drying furnace 30 also has an air intake 34 that is provided at the top of the heating cylinder 31 and allows air to flow into the heating cylinder 31, and an exhaust port 35 that is provided at the bottom of the heating cylinder 31 and allows air to be exhausted from inside the heating cylinder 31. The high-temperature oil that flows in from the inlet 32 flows outside the substrate 1 as shown by the solid arrow, heating the substrate 1 from the outside at that time, and flows out from the outlet 33. In addition, the air sucked in from the air intake port 34 flows inside the base 1 as indicated by the dashed arrows, and is exhausted from the exhaust port 35 together with the solvent evaporated from the polyimide precursor solution 5 applied to the inner surface of the base 1.
[0044] Using a heating and drying furnace 30, the polyimide precursor solution 5 applied to the inner surface of the substrate 1 is heated for about 300 seconds by, for example, passing high-temperature oil at 160°C from an inlet 32 through a heating cylinder 31 and discharging it from an outlet 33. This reduces the organic polar solvent contained in the polyimide precursor solution 5 from about 90% by volume to less than about 30% by volume, thereby increasing the viscosity of the polyimide precursor solution 5 and preventing it from flowing out from the inner surface of the substrate 1. When evaporating the organic polar solvent, air is sucked in from an intake port 34, circulated around the inner periphery of the substrate 1, and discharged from an exhaust port 35, thereby maintaining the organic polar solvent below the lower explosion limit.
[0045] That is, in the drying process, high-temperature oil as a first fluid is circulated from the inlet 32 side, which is one end side (lower side) in the rotation axis direction of the base 1, to the outlet 33 side, which is the other end side (upper side), outside the base 1. Also, in the drying process, air, which is a second fluid having a lower temperature than the high-temperature oil, is circulated from the intake port 34 side, which is the other end side (upper side), to the exhaust port 35 side, which is one end side (lower side), inside the base 1.
[0046] Next, as shown in Fig. 4, the base 1 on which the polyimide precursor solution 5 has been dried is placed in a hot air circulating oven (step S5), and the polyimide precursor solution 5 is baked (step S6). Specifically, after the organic polar solvent is reduced to less than about 30% by volume, the base 1 is left for 30 minutes in a hot air circulating oven at 200°C, for example, to dry, and then left for 20 to 120 minutes in a hot air circulating oven at 300°C to 400°C, which is a temperature range that does not reduce the fatigue strength of the base 1, to bake. This allows the sliding layer 2 of polyimide resin in which the filler 2a is dispersed to be formed by a dehydration ring-closing reaction.
[0047] [Elastic layer] The elastic layer 3 functions as an elastic layer supported by the fixing member in order to apply uniform pressure to the unevenness of the toner image and the recording material S during fixing. That is, the elastic layer 3 functions as a layer that imparts to the fixing belt 201 elasticity having flexibility to follow the unevenness of the paper fibers when the recording material is paper, without crushing the toner more than necessary, when the toner image is fixed to the recording material at the fixing nip N. In order to realize such a function, it is preferable to use an addition reaction crosslinking type liquid silicone rubber as the material of the elastic layer 3, because it is easy to process, can be processed with high dimensional accuracy, and does not generate reaction by-products during heat curing. In addition, the elasticity can be adjusted by adjusting the degree of crosslinking according to the type and amount of filler to be described later.
[0048] In general, addition reaction crosslinking type liquid silicone rubber contains an organopolysiloxane having an unsaturated aliphatic group, an organopolysiloxane having active hydrogen bonded to silicon, and a platinum compound as a crosslinking catalyst. The organopolysiloxane having active hydrogen bonded to silicon reacts with the alkenyl group of the organopolysiloxane component having an unsaturated aliphatic group under the catalytic action of the platinum compound to form a crosslinked structure.
[0049] The elastic layer 3 may contain a filler for improving the thermal conductivity, reinforcement, and heat resistance of the fixing belt 201. In particular, for the purpose of improving the thermal conductivity, it is preferable that the filler has high thermal conductivity. Specific examples of the filler include inorganic materials, particularly metals and metal compounds. Specific examples of the highly thermally conductive filler include silicon carbide (SiC), silicon nitride (Si3N4), boron nitride (BN), aluminum nitride (AlN), alumina (Al2O3), zinc oxide (ZnO), and magnesium oxide (MgO). Specific examples of the highly thermally conductive filler include silica (SiO2), copper (Cu), aluminum (Al), silver (Ag), iron (Fe), and nickel (Ni).
[0050] These fillers can be used alone or in combination of two or more. The average particle size of the highly thermally conductive filler is preferably 1 μm or more and 50 μm or less from the viewpoints of handling and dispersibility. The shape may be spherical, pulverized, plate-like, whisker-like, etc., but spherical is preferred from the viewpoint of dispersibility. From the viewpoints of contribution to the surface hardness of the fixing belt 201 and efficiency of heat conduction to unfixed toner during fixing, the preferred range of the thickness of the elastic layer 3 is 100 μm or more and 500 μm or less, more preferably 200 μm or more and 400 μm or less. In this embodiment, alumina is used as the highly thermally conductive filler, and the thermal conductivity of the elastic layer 3 is 1.0 W / mK and the thickness is 300 μm.
[0051] [Release layer] For example, a resin such as PFA, PTFE, or FEP molded into a tube shape is used as the release layer 4. PFA is a tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer, PTFE is polytetrafluoroethylene, and FEP is a tetrafluoroethylene-hexafluoropropylene copolymer. Among the materials listed above, PFA is preferable as the release layer 4 from the viewpoint of moldability and toner releasability.
[0052] The thickness of the release layer 4 is preferably 50 μm or less. This is because the elasticity of the lower elastic layer 3 can be maintained when laminated, and the surface hardness as a fixing member can be prevented from becoming too high. The adhesiveness of the inner surface of the fluororesin tube can be improved by previously treating it with sodium, excimer laser, ammonia, or the like. In this embodiment, a PFA tube with a thickness of 20 μm obtained by extrusion molding is used. The inner surface of the tube is treated with ammonia to improve wettability with the adhesive described below.
[0053] The silicone rubber adhesive layer that fixes the PFA tube 1e as the release layer 4 to the elastic layer 3 is made of a cured product of an addition-curing silicone rubber adhesive applied to the surface of the elastic layer 3. The addition-curing silicone rubber adhesive contains an addition-curing silicone rubber that is blended with a self-adhesive component represented by a silane having a functional group such as an acryloxy group, a hydrosilyl group (SiH group), an epoxy group, or an alkoxysilyl group. The addition-curing silicone rubber adhesive is cured and bonded by heating for a predetermined time with a heating means such as an electric furnace, and both ends are cut to the desired length to obtain a fixing belt 201 as the fixing member of this embodiment.
[0054] [Examples and Comparative Examples] Hereinafter, there will be described examples and comparative examples in which the drying temperature and the blending ratio of the filler 2a were changed when forming the sliding layer 2. Here, the drying temperature and the blending ratio of the filler 2a were changed to form the sliding layer 2, and the orientation rate Ro and surface roughness (arithmetic mean roughness) Ra of the filler 2a of the obtained sliding layer 2 were calculated, and the durability was evaluated and the results were compared.
[0055] Example 1 The materials used to form the sliding layer 2 were as follows. As the polyimide precursor solution 5, a polyimide precursor solution "U-Varnish S; manufactured by Ube Industries, Ltd." was used, which used 3,3',4,4'-biphenyltetracarboxylic dianhydride as the aromatic tetracarboxylic dianhydride and paraphenylenediamine as the aromatic diamine. As the filler 2a, fluorine phlogopite with an aspect ratio of 80 (average particle diameter 8 μm, particle thickness 100 nm) was mixed so as to be 7 volume % with respect to the total volume of the solid content formed as the sliding layer 2. The filler dispersion solution was prepared by directly adding the filler 2a (fluorine phlogopite) to the polyimide precursor solution (U-Varnish S), pre-stirring with a mixer, and then dispersing with a three-roll mill.
[0056] The polyimide precursor solution 5 in which the filler 2a was dispersed was applied to the inner surface of the substrate 1 by a ring coating method using a coating device 20 so that the coating thickness was 77 μm. After application, the coating film was heated and dried for 300 seconds in a heating and drying oven 30 in which the temperature of high-temperature oil was set to 160° C. Thereafter, the substrate 1 was left to dry in a hot air circulation oven at 200° C. for 30 minutes, and then left to bake in another hot air circulation oven at 400° C. for 30 minutes to form a sliding layer 2. The thickness of the sliding layer 2 formed on the inner surface of the substrate 1 was 12 μm.
[0057] A hydrosilyl silicone primer "DY39-051 A / B; manufactured by Dow Corning Toray Co., Ltd." was applied to the surface of the substrate 1 and cured by heating at 200°C for 5 minutes. An addition reaction crosslinking liquid silicone rubber was applied to the outer peripheral surface of the substrate 1 to a thickness of 300 μm and cured by heating at 200°C for 30 minutes to form an elastic layer 3. The outer peripheral surface of the substrate 1 was further covered with a 20 μm thick PFA tube as a release layer 4 via a silicone adhesive "SE1819 CV A / B; manufactured by Dow Corning Toray Co., Ltd." and cured by heating at 200°C for 2 minutes to produce a fixing belt 201.
[0058] Example 2 Compared to Example 1, the filler 2a, fluorine-containing mica, was changed to be 15 volume % relative to the total volume of the solid content formed as the sliding layer 2, but otherwise the fixing belt 201 was produced in the same manner as Example 1.
[0059] Example 3 Compared to Example 1, the temperature of the high-temperature oil in the heating and drying furnace 30 was changed to 190° C. and the drying process was performed, but in other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0060] Comparative Example 1 Compared to Example 1, the amount of fluorine mica as the filler 2a was changed to 17 volume % relative to the total volume of the solid content formed as the sliding layer 2, and the temperature of the high-temperature oil in the heating and drying furnace 30 was changed to 100° C. to carry out the drying process. In other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0061] Comparative Example 2 Compared to Example 1, the temperature of the high-temperature oil in the heating and drying furnace 30 was changed to 100° C. and the drying process was performed, but in other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0062] [Filler orientation rate] Here, the orientation ratio Ro of the filler 2a in the sliding layer 2 will be described. Here, as shown in FIG. 7, the orientation ratio Ro of the filler 2a blended in the sliding layer 2 was calculated for each region by dividing the sliding layer 2 into an inner peripheral side (surface side) region 2b and a substrate side region 2c in the thickness direction Dt. The orientation ratio Ro is defined as the ratio of the number N1 of fillers inclined (oriented) within a predetermined angle range along the surface direction to the number N0 of fillers contained in the two regions 2b and 2c. Here, the fixing belt 201 was cut in the rotation direction (circumferential direction), and the sliding layer 2 of the cut surface was cross-sectionally milled using an ion milling device (IM4000PLUS; manufactured by Hitachi High-Technologies Corporation). Thereafter, the cross section was observed with a scanning electron microscope (SEM) and quantified by image processing.
[0063] FIG. 7 is a schematic diagram of an image of the sliding layer 2 after cross-section milling observed with an SEM. The image thus observed with an SEM was binarized, and N fillers 2a were observed using an optical microscope. At this time, the number of fillers 2a whose inclination θ with respect to the reference direction D0, which is the direction (surface direction) along the inner circumferential surface 1a of the substrate 1 of the fixing belt 201, is 0≦θ≦10° or 170°≦θ≦180°, was defined as N1. The orientation rate Ro was calculated by defining Ro=(N1 / N0)×100(%). It should be noted that the number N0 of fillers 2a observed using an optical microscope is sufficient if it is about 50 pieces.
[0064] The calculation results of the orientation rate Ro in each Example and Comparative Example are shown in Table 1. As shown in Table 1, in Examples 1 to 3, the orientation rate Ro in the inner peripheral region 2b was smaller than the orientation rate Ro in the base side region 2c. For example, in Example 1, when the direction along the inner peripheral surface 1a of the base 1 is set as the reference direction D0, the first position in the thickness direction Dt of the slide layer 2 is set as the base side region 2c, and the second position located on the inner peripheral surface 2d side of the slide layer 2 from the first position is set as the inner peripheral region 2b. In this case, the orientation rate Ro of the filler 2a in the base side region 2c in the reference direction D0 is 91% (first value), and the orientation rate Ro of the filler 2a in the inner peripheral region 2b in the reference direction D0 is 75% (second value) which is smaller than 91%. On the other hand, in Comparative Examples 1 to 2, the orientation rate Ro in the inner peripheral region 2b was almost equal to the orientation rate Ro in the base side region 2c.
[0065] [Surface roughness of sliding layer] The surface roughness Ra of the inner peripheral surface of the sliding layer 2 was measured as the arithmetic mean roughness Ra (μm, JIS B0601) using a surface roughness measuring device (Surfcorder, manufactured by Kosaka Laboratory Co., Ltd.). The measurement conditions were an evaluation length of 4 mm, a cutoff value of 0.8 mm, and a feed rate of 0.1 mm / s. The calculation results of the surface roughness Ra in each of the examples and comparative examples are shown in Table 1.
[0066] In addition, in Examples 1 to 3, the sliding layer 2 has a plurality of Benard cells on the inner surface 2d, the cells having an average diameter of 50 μm or more and less than 200 μm, and the arithmetic mean roughness of the inner surface 2d is 0.20 μm or more and 0.50 μm or less.
[0067] [Durability evaluation] The durability of the fixing belt 201 was evaluated by mounting the fixing belt 201 of each of the examples and comparative examples in a belt heating type fixing device 200 shown in Fig. 2. Here, the pressure roller 206 was rotated so that the surface movement speed (circumferential speed) of the pressure roller 206 was 246 mm / sec with a pressure of about 156.8 N at one end and a total pressure of about 313.6 N (32 kgf). Paper of the same size (A4 landscape) was continuously passed through the fixing belt 201 with the surface temperature of the paper passing portion of the fixing belt 201 adjusted to 170°C. Note that 1.2 g of grease (Molycoat HP-300, manufactured by Dow Corning Toray Co., Ltd.) was applied to the inner surface of the fixing belt 201 as a lubricant.
[0068] Next, the evaluation method will be described. Regarding the evaluation of the sliding property, if the fixing belt 201 does not make any abnormal noise due to the self-excited vibration caused by the occurrence of stick-slip at the minimum speed of 120 mm / s of the device and the load torque is 800 mN·m or less, it is evaluated as ◯, and if not, it is evaluated as ×. This sliding property is evaluated by comparing the initial state before the durability test and the state of the fixing belt 201 with the load torque of GF-C081 (manufactured by Nippon Paper Industries Co., Ltd., 80 g / m 2 The condition of the paper after 500,000 sheets of paper were passed through the printer was evaluated. The results are shown in Table 1. [Table 1]
[0069] As shown in Table 1, by making the orientation rate Ro of the filler 2a of the slide layer 2 smaller in the inner peripheral region 2b than in the base-side region 2c in the thickness direction Dt of the slide layer 2, good results were obtained in terms of the occurrence of abnormal noise due to stick-slip and torque stability through durability. This is believed to be due to the following reasons.
[0070] By setting a higher temperature for drying (evaporating the solvent) the coating film of the polyimide precursor solution 5 applied to the inner surface of the substrate 1, the orientation ratio Ro of the filler 2a in the inner circumferential region 2b can be made smaller than that in the substrate region 2c. This is because the temperature gradient in the thickness direction Dt generated in the coating film becomes large, causing Benard convection in the solvent, and the filler 2a oriented in the reference direction (plane direction) D0 is rolled up along this Benard convection. Due to this phenomenon, in Examples 1 to 3, the orientation ratio Ro of the inner circumferential region 2b of the sliding layer 2 becomes small, and a desired surface roughness Ra can be obtained with an appropriate amount of filler 2a. This makes it possible to suppress the generation of abnormal noise and torque increase during durability due to a decrease in wear strength.
[0071] On the other hand, in Comparative Example 1, the surface roughness Ra is adjusted by increasing the amount of filler 2a in a state where the orientation rate Ro of the inner peripheral region 2b of the sliding layer 2 is as large as that of the substrate side region 2c. However, the wear strength is reduced by increasing the amount of filler 2a, and the torque is increased due to excessive wear of the sliding layer 2 during durability testing. In Comparative Example 2, although the amount of filler 2a is the same as that of Example 1, the orientation rate Ro of the inner peripheral region 2b is as large as that of the substrate side region 2c, so that a surface roughness Ra sufficient for suppressing abnormal noise cannot be imparted.
[0072] From the above, by optimally arranging the filler 2a in the sliding layer 2 so that (orientation rate Ro of the filler 2a in the inner peripheral region 2b)<(orientation rate Ro of the filler 2a in the base side region 2c), the surface roughness Ra of the inner peripheral surface 2d of the sliding layer 2 is effectively imparted. At the same time, the wear resistance of the fixing belt 201 in the rotational direction is improved, so that the fixing belt 201 having the sliding layer 2 capable of reducing torque increase and stick-slip throughout its durable life can be obtained.
[0073] As described above, in the fixing belt 201 of this embodiment, the orientation rate Ro of the filler 2a in the inner peripheral region 2b is set to be smaller than the orientation rate Ro of the filler 2a in the substrate side region 2c. This effectively imparts the surface roughness Ra to the inner peripheral surface 2d of the sliding layer 2, and improves the wear resistance in the rotational direction of the fixing belt 201. This makes it possible to reduce torque increase and stick-slip throughout the durability life, and improve the wear resistance strength.
[0074] <Second embodiment> Next, a second embodiment of the present invention will be described in detail with reference to Fig. 8. In this embodiment, the size of the Benard cells in the sliding layer 2 is set within an appropriate range, thereby improving the wear resistance. However, other configurations are the same as those in the first embodiment, so the same reference numerals are used and detailed description is omitted.
[0075] First, the Benard cell 6 will be described. As shown in FIG. 8, in the sliding layer 2, Benard convection (indicated by arrows in the figure) occurs in the drying process, and the Benard cell 6 remains in the sliding layer 2 after formation. The diameter of the Benard cell 6 when viewed from the inner peripheral surface 2d of the sliding layer 2 is defined as the Benard cell diameter d1. In this embodiment, in the drying process when forming the sliding layer 2, a temperature difference is created in the thickness direction of the polyimide precursor solution 5 to form the Benard cell 6. Specifically, air is sent inside the substrate 1, and the temperature of the polyimide precursor solution 5 on the substrate side is set to be high, and the atmospheric temperature on the inner surface side is set to be low.
[0076] [Examples and Comparative Examples] Hereinafter, there will be described examples and comparative examples in which the Benard cell diameter d1 was changed when forming the slide layer 2. Here, the surface roughness Ra of the obtained slide layer 2 was calculated, and the durability was evaluated and the results were compared.
[0077] Example 4 A fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 11% by volume and the Benard cell diameter d1 was set to 50 μm.
[0078] Example 5 A fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 11% by volume and the Benard cell diameter d1 was set to 100 μm.
[0079] Example 6 A fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 11% by volume and the Benard cell diameter d1 was set to 150 μm.
[0080] Example 7 A fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 11% by volume and the Benard cell diameter d1 was set to 200 μm.
[0081] Example 8 A fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 11% by volume and the Benard cell diameter d1 was set to 250 μm.
[0082] Comparative Example 3 A fixing belt 201 was produced in the same manner as in Example 1, except that the filler 2a was not mixed.
[0083] Comparative Example 4 The fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 5.0 wt % and the Benard cell diameter d1 was set to 25 μm.
[0084] Comparative Example 5 The fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 20.0 wt % and the Benard cell diameter d1 was set to 25 μm.
[0085] Comparative Example 6 A fixing belt 201 was produced in the same manner as in Example 1, except that the blending amount of the filler 2a was set to 20.0 wt % and the Benard cell diameter d1 was set to 250 μm.
[0086] Next, the surface roughness Ra will be described. The surface roughness Ra is determined by the size of the Benard cell 6 and the amount of filler 2a added, and when the amount of filler is large, the diameter of the Benard cell 6 is small, that is, when the frequency is high, the surface roughness Ra becomes large.
[0087] FIG. 8 is a schematic diagram showing the state of filler 2a in sliding layer 2 containing Benard cell 6. When Benard cell 6 is generated during imidization of polyimide precursor solution 5 of sliding layer 2, liquid circulation occurs within the layer as shown by the arrows. As a result, (1) filler 2a floats up to the surface side and is fixed on the surface, and (2) at the same time, the sliding layer 2 itself rises at the end of Benard cell 6, which increases the surface roughness Ra. Therefore, when the amount of filler is large, there is a tendency that the surface roughness Ra increases because the amount of filler that floats up increases (1), and there is a tendency that the surface roughness Ra increases because the frequency of the end rises increases when Benard cell 6 becomes smaller. As a result, the surface roughness Ra shown in Table 2 was obtained from the relationship between the shape of Benard cell 6 and the amount of filler blended.
[0088] [Durability evaluation] The durability evaluation of the fixing belt 201 was performed by mounting the fixing belt 201 of each of the examples and comparative examples in a belt heating type fixing device 200 shown in Fig. 2. Here, the fixing device 200 was incorporated in a Canon full-color copier "iR ADVANCE C5051", and the pressure was set to 320 N, the fixing temperature to 170°C (fixing belt surface temperature), and the process speed to 320 mm / sec. Note that 1.2 g of grease (HP300 manufactured by Dow Corning Asia) was applied to the inner surface of the fixing belt 201 as a lubricant.
[0089] Next, the evaluation method will be described. The evaluation of the sliding property was performed in the same manner as in the first embodiment. The fixability was evaluated using GFC-081 (manufactured by Nippon Paper Industries Co., Ltd., 80 g / m 2 Paper) with a toner load of 0.9 mg / cm 2 The image printed with the above method was folded, and evaluation was performed by assigning a rating of ◯ to a case where the toner peeled off width when folded was less than 1 mm, and an X to a case where the toner peeled off width was 1 mm or more. The results are shown in Table 2. [Table 2]
[0090] In Examples 4 to 8, the sliding layer 2 has a plurality of Benard cells 6 with an average diameter of 50 μm or more and less than 200 μm on the inner peripheral surface 2d, and the surface roughness Ra, which is the arithmetic mean roughness of the inner peripheral surface 2d, is 0.20 μm or more and 0.50 μm or less. In Examples 4 to 8, good results were obtained in both the sliding property evaluation and the fixing property evaluation. First, with regard to the sliding property, the initial roughness was sufficiently high, so that the initial stage was good, and since the amount of the filler 2a was small, the scraping after the durability test was reduced, so that the sliding property after the durability test was also good. In this way, by defining the shape of the Benard cells 6, it was possible to efficiently obtain the surface roughness Ra with a small amount of the filler 2a, and it was possible to achieve a good state of sliding property from the initial stage to the endurance test. In addition, with regard to the fixing property, it was confirmed that the fixing property was not impaired because the surface roughness Ra was less than a predetermined value.
[0091] In contrast, in Comparative Example 3, since the filler 2a was not included, the surface roughness Ra was small and the fixing property was good, but the surface roughness Ra was insufficient, so the sliding property was poor from the beginning to the endurance. In Comparative Example 4, although the filler 2a was present and the diameter of the Benard cell 6 was small, the surface roughness Ra was insufficient like in Comparative Example 3, so the sliding property was poor from the beginning to the endurance.
[0092] In Comparative Example 5, the surface roughness Ra was large because of the high amount of filler, and the initial sliding properties were good, but the inner wear after the endurance test during paper passing was large, and the sliding properties after the endurance test were poor. In addition, the initial surface roughness Ra was too high, and the fixing properties were also poor. In Comparative Example 6, the diameter of the Benard cell 6 was large, and the surface roughness Ra was reduced, and the fixing properties were good, but the amount of filler added was large, and the inner wear was large, and the sliding properties after the endurance test were poor. In this way, by setting the diameter and surface roughness Ra of the Benard cell 6 as shown in Examples 4 to 8, a fixing belt 201 with good sliding properties and fixing properties from the initial stage to the endurance test could be obtained.
[0093] As described above, in the fixing belt 201 of this embodiment, the average diameter of the Benard cell 6 on the inner circumferential surface 2d of the sliding layer 2 is 50 μm or more and less than 200 μm, and the surface roughness Ra of the inner circumferential surface 2d is set to 0.20 μm≦Ra≦0.50 μm. This effectively imparts the surface roughness Ra to the inner circumferential surface 2d of the sliding layer 2, and improves the wear resistance in the rotational direction of the fixing belt 201. This makes it possible to reduce torque increase and stick-slip throughout the durability life, and improve the wear resistance strength.
[0094] The fixing belt 201 of this embodiment may have the same configuration as the fixing belt 201 of the first embodiment, i.e., the orientation rate Ro of the filler 2a in the inner peripheral region 2b is smaller than the orientation rate Ro of the filler 2a in the base side region 2c.
[0095] <Third embodiment> Next, a third embodiment of the present invention will be described in detail. In this embodiment, the temperature difference between the inside and outside of the substrate 1 is set within an appropriate range in the drying process, thereby improving the abrasion resistance. However, other configurations are the same as those in the first embodiment, so the same reference numerals are used and detailed description is omitted.
[0096] In this embodiment, the method for manufacturing the fixing belt 201 includes at least a coating step (see step S2 in FIG. 4) and a drying step (see step S4 in FIG. 2) when forming the sliding layer 2. The coating step is a step of coating the inner circumferential surface 1a of the base 1 with a polyimide precursor solution 5 in which a precursor of the sliding layer 2 and a filler 2a are dispersed in a solvent. The drying step is a step of drying the solvent from the polyimide precursor solution 5 coated on the inner circumferential surface 1a of the base 1.
[0097] In this embodiment, in the drying step for forming the sliding layer 2, a temperature difference is created in the thickness direction Dt of the polyimide precursor solution 5 to form the Benard cell 6. Specifically, air is sent inside the substrate 1 so that the temperature of the polyimide precursor solution 5 on the substrate side is high and the atmospheric temperature on the inner surface side is low.
[0098] Here, when the temperature of the substrate side of the polyimide precursor solution 5 is X and the atmospheric temperature of the inner side is Y, it is important to make 10°C≦XY≦30°C. When XY≧10°C, Benard cell 6 is generated when the polyimide precursor solution 5 dries, and liquid circulation occurs within the layer as shown by the arrows in FIG. 8. As a result, (1) the filler 2a is blown up to the surface side and fixed on the surface, and (2) at the same time, the sliding layer 2 itself is raised at the end of the Benard cell 6, which increases the surface roughness Ra. When XY<10°C, the Benard cell 6 cannot be formed well, and the surface roughness Ra may not be a desired value. Also, when XY>30°C, the Benard cell 6 causes the sliding layer 2 to be raised significantly, and the surface roughness Ra may become too large. As a result, the contact thermal resistance with the fixing heater 202 arranged on the inner surface of the fixing belt 201 increases, and the heat transfer may become insufficient.
[0099] [Examples and Comparative Examples] Hereinafter, examples and comparative examples will be described in which the substrate side temperature X and the inner circumference side temperature Y were changed in the drying process when forming the sliding layer 2. Here, the surface roughness Ra of the obtained sliding layer 2 was calculated, and the durability was evaluated and the results were compared.
[0100] Example 9 The fixing belt 201 was produced in the same manner as in Example 1, except that the substrate side temperature X was set to 160° C. and the inner circumference side temperature Y was set to 140° C.
[0101] Example 10 The fixing belt 201 was produced in the same manner as in Example 1, except that the substrate side temperature X was set to 160° C. and the inner circumference side temperature Y was set to 150° C.
[0102] Example 11 The fixing belt 201 was produced in the same manner as in Example 1, except that the substrate side temperature X was set to 190° C. and the inner circumference side temperature Y was set to 160° C.
[0103] Comparative Example 7 The fixing belt 201 was produced in the same manner as in Example 1, except that the substrate side temperature X was set to 100° C. and the inner circumference side temperature Y was set to 95° C.
[0104] Comparative Example 8 The fixing belt 201 was produced in the same manner as in Example 1, except that the substrate side temperature X was set to 190° C. and the inner circumference side temperature Y was set to 150° C.
[0105] The durability of fixing belt 201 was evaluated by the same evaluation method as in the first and second embodiments. Table 3 shows the durability evaluation results of Examples 9 to 11 and Comparative Examples 7 and 8. [Table 3]
[0106] For example, in Examples 9 to 11, the base-side temperature X and the inner periphery-side temperature Y satisfy the relationship 10° C.≦XY≦30° C. For example, in Example 9, when the temperature of the outer periphery surface of the base 1 is set to a first temperature (160° C.) and the temperature of the atmosphere on the inner periphery side of the sliding layer 2 is set to a second temperature (150° C.) lower than the first temperature, the difference between the first temperature and the second temperature is set to be 10° C. or more and 30° C. or less.
[0107] As a result, in Examples 9 to 11, both the sliding property evaluation and the fixing property evaluation were good. With regard to the sliding property, the initial surface roughness Ra was sufficiently high, so the initial state was good, and since the amount of filler was small, the scraping after the endurance test was reduced, so the sliding property after the endurance test was also good. In this way, by specifying the temperature conditions when evaporating the organic polar solvent after applying the polyimide precursor solution 5 to the substrate 1, the Benard cell 6 was well formed, and the surface roughness Ra could be efficiently obtained with a small amount of filler 2a. Therefore, a good sliding property was achieved from the initial state to the endurance test. In addition, with regard to the fixing property, it was confirmed that the fixing property was not impaired because the surface roughness Ra was less than a predetermined value.
[0108] In contrast, in Comparative Example 7, the Benard cell 6 was small and the fixation was good, but the surface roughness Ra was insufficient, so the sliding properties were low and the sliding properties were poor from the beginning to the endurance. Also, in Comparative Example 8, the Benard cell 6 was large, so the surface roughness Ra was large, and the initial sliding properties and the sliding properties after the endurance test during paper passing were good, but the fixation was poor because the initial surface roughness Ra was too high.
[0109] Therefore, the temperature conditions for evaporating the organic polar solvent after coating the substrate 1 with the polyimide precursor solution 5 as shown in Examples 9 to 11 are specified. This allows the Benard cell 6 to be formed and the desired surface roughness Ra to be achieved, thereby making it possible to obtain a fixing belt 201 with good sliding properties and fixing properties from the initial stage to after endurance testing.
[0110] As described above, in the fixing belt 201 of this embodiment, the base side temperature X and the inner periphery side temperature Y satisfy the relationship of 10° C.≦XY≦30° C. This effectively imparts the surface roughness Ra to the inner periphery surface 2d of the sliding layer 2, and improves the wear resistance in the rotational direction of the fixing belt 201. This makes it possible to reduce torque increase and stick-slip throughout the durability life, and improve the wear resistance.
[0111] The fixing belt 201 manufactured by the manufacturing method of this embodiment may have the configuration of the fixing belt 201 of the first embodiment, that is, the configuration in which the orientation rate Ro of the filler 2a in the inner peripheral side region 2b is smaller than the orientation rate Ro of the filler 2a in the base side region 2c. Alternatively, the fixing belt 201 manufactured by the manufacturing method of this embodiment may have the configuration of the fixing belt 201 of the second embodiment, that is, the configuration in which the average diameter of the Benard cell 6 is 50 μm or more and less than 200 μm.
[0112] <Fourth embodiment> Next, a third embodiment of the present invention will be described in detail with reference to Fig. 9. In this embodiment, the thickness of the polyimide precursor solution 5 applied in the application step is set to an appropriate range depending on the location, thereby improving the abrasion resistance. However, other configurations are the same as those in the first embodiment, so the same reference numerals are used and detailed description is omitted.
[0113] In the drying process for forming the sliding layer 2, air is circulated on the inner periphery side of the substrate 1. Here, by ventilating air at room temperature, the temperature of the intake side portion 1U of the substrate 1 becomes lower than the temperature of the exhaust side portion 1L, as shown in FIG. 9(a), and a temperature difference occurs in the longitudinal direction (up and down direction) of the substrate 1. In the drying process, the temperature when the organic polar solvent is reduced from about 85% by volume to less than about 30% by volume and the thickness of each portion of the polyimide precursor solution 5 shown in FIG. 9(a) affect the surface roughness Ra of each portion of the sliding layer 2 shown in FIG. 9(b).
[0114] In this embodiment, in the coating step, the thickness of the polyimide precursor solution 5 at a third position in the vertical direction of the base 1 is set to a third value. In addition, the thickness of the polyimide precursor solution 5 at a fourth position located above the third position is set to a fourth value that is thicker than the third value. That is, the polyimide precursor solution 5 is coated so that the thickness gradually decreases from the upper side to the lower side in the air flow direction. Furthermore, in the drying step, the temperature of the outer peripheral surface of the base 1 at the lower third position is set to a third temperature, and the temperature of the outer peripheral surface of the base 1 at the upper fourth position is set to a fourth temperature that is lower than the third temperature, to dry the solvent.
[0115] This makes it possible to reduce the difference in surface roughness Ra between the third position and the fourth position, and to uniformize the surface roughness Ra over the entire area of the base 1. In this embodiment, similarly to the third embodiment, the base side temperature X and the inner periphery side temperature Y are set to satisfy the relationship 10° C.≦XY≦30° C. This makes it possible to uniformize the surface roughness Ra within an appropriate range.
[0116] [Examples and Comparative Examples] Hereinafter, examples and comparative examples will be described in which the thickness of the polyimide precursor solution 5 was changed between the intake side portion 1U, the middle portion 1M, and the exhaust side portion 1L of the substrate 1 in the coating process when forming the sliding layer 2. Here, the surface roughness Ra of the obtained sliding layer 2 was calculated, and the durability was evaluated and the results were compared. In the following examples and comparative examples, the substrate side temperature X and the inner periphery side temperature Y were set to satisfy the relationship 10°C≦XY≦30°C.
[0117] Example 12 In the coating process, the coating thickness of the polyimide precursor solution 5 was made thicker on the intake side of the ventilation of the heating and drying furnace 30 and thinner on the exhaust side. Here, the thickness was 90 μm at the intake side portion 1U of the base 1, 77 μm at the middle portion 1M, and 64 μm at the exhaust side portion 1L. In other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0118] Example 13 The thickness was 90 μm at the intake side portion 1U of the substrate 1, 77 μm at the intermediate portion 1M, and 58 μm at the exhaust side portion 1L. In other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0119] Example 14 The thickness was 83 μm at the intake side portion 1U of the substrate 1, 77 μm at the intermediate portion 1M, and 58 μm at the exhaust side portion 1L. In other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0120] Comparative Example 9 The thickness was 77 μm at the intake side portion 1U of the substrate 1, 77 μm at the intermediate portion 1M, and 77 μm at the exhaust side portion 1L. A fixing belt 201 was produced in the same manner as in Example 1 except for the above.
[0121] Comparative Example 10 The thickness was 64 μm at the intake side portion 1U of the substrate 1, 77 μm at the intermediate portion 1M, and 90 μm at the exhaust side portion 1L. In other respects, the fixing belt 201 was produced in the same manner as in Example 1.
[0122] In Examples 12 to 14 and Comparative Examples 9 and 10, the surface temperatures and surface roughness Ra of the intake side portion 1U, the middle portion 1M, and the exhaust side portion 1L of the substrate 1 were measured 60 seconds after the substrate 1 was placed in the heating and drying furnace 30. The results are shown in Table 4. [Table 4]
[0123] [Surface roughness] As shown in Table 4, there is no significant difference in the surface roughness Ra in the longitudinal direction among Examples 12 to 14. In contrast, there is a difference in the surface roughness Ra in the longitudinal direction among Comparative Examples 9 and 10.
[0124] In Examples 12 to 14 and Comparative Examples 9 and 10, the surface temperature of the substrate 1 was (Temperature of intake side part 1U) < (Temperature of middle part 1M) < (Temperature of exhaust side part 1L) This is because room temperature air enters from the intake side portion 1U, warms up as it passes through the heating and drying furnace 30, and leaves from the exhaust side portion 1L, so the surface temperature of the base 1 is lower on the intake side portion 1U and higher on the exhaust side portion 1L. Accordingly, it is thought that the temperature of the polyimide precursor solution 5 applied to the inner surface of the base 1 is also lower on the intake side portion 1U and higher on the exhaust side portion 1L.
[0125] From the results of Comparative Example 9, when the thickness of the polyimide precursor solution 5 is constant, the lower the temperature, the smaller the surface roughness Ra of the inner circumferential surface side of the sliding layer 2 after baking, and the higher the temperature, the larger the surface roughness Ra. From the results of Comparative Examples 9 and 10, there is a relationship between the thickness of the polyimide precursor solution 5 and the surface roughness Ra of the inner circumferential surface side of the sliding layer 2 after baking, and the thinner the thickness of the polyimide precursor solution 5, the smaller the surface roughness Ra, and the thicker the thickness, the larger the surface roughness Ra.
[0126] In Examples 12 to 14, the thickness of the polyimide precursor solution 5 has a relationship of (1U>1M>1L) so that the difference in surface temperature (1U<1M<1L) of the base 1 is covered by the thickness of the polyimide precursor solution 5. The thickness of the polyimide precursor solution 5 is made thicker on the side of the base 1 where the surface temperature is low, and made thinner on the side where the temperature is high, thereby preventing a large difference in the surface roughness Ra of the inner peripheral surface of the sliding layer 2 after firing in the longitudinal direction.
[0127] For example, in Example 12, in the coating step, the thickness of the polyimide precursor solution 5 at a third position (1L) in the vertical direction of the substrate 1 is set to a third value (64 μm). Also, the thickness of the polyimide precursor solution 5 at a fourth position (1U) located above the third position is set to a fourth value (90 μm) thicker than the third value. That is, the polyimide precursor solution 5 is coated so that the thickness gradually decreases from the upper side to the lower side in the air flow direction. Furthermore, in the drying step, the temperature of the outer peripheral surface of the substrate 1 at the lower third position is set to a third temperature (153° C.), and the temperature of the outer peripheral surface of the substrate 1 at the upper fourth position is set to a fourth temperature (115° C.) lower than the third temperature, to dry the solvent.
[0128] [Durability evaluation] Here, the length Lb of the fixing belt 201 in the initial state before the durability test was measured. 2 The length La of the fixing belt 201 after the endurance test of passing 500,000 sheets of paper was measured. The lengths Lb and La of the fixing belt 201 are shown in Table 5. [Table 5]
[0129] As shown in Table 2, the fixing belts 201 of Examples 12 to 14 were about 0.2 to 0.3 mm shorter after the endurance test than before the endurance test, but there was nothing noticeable at the end of the fixing belt 201. On the other hand, the fixing belt 201 of Comparative Example 9 was 1.1 mm shorter after the endurance test. In addition, wear powder was attached to the end of the intake side portion 1U. In Comparative Example 2, damage was confirmed at the end of the intake side portion 1U of the fixing belt 201 when 460,000 sheets were passed through.
[0130] From the results of Comparative Examples 9 and 10, it is considered that since there is a difference in the surface roughness Ra of the inner peripheral side of the sliding layer 2 in the longitudinal direction, a difference in the frictional force with the sliding counterpart material in the fixing nip portion N occurs, and the fixing belt 201 is always subjected to a force in one direction. It is considered that this makes the end portion susceptible to wear. In contrast, since there is almost no difference in the surface roughness Ra of the inner peripheral side of the sliding layer 2 in Examples 12 to 14 in the longitudinal direction, there is no difference in the frictional force with the sliding counterpart material in the fixing nip portion N. Therefore, since the force with which the fixing belt 201 hits the member that regulates the fixing belt 201 is small, the end portion wears little, resulting in a fixing belt 201 with good durability.
[0131] As described above, in the fixing belt 201 of this embodiment, the thickness of the polyimide precursor solution 5 applied is set to an appropriate range depending on the location. This effectively imparts the surface roughness Ra to the inner circumferential surface 2d of the sliding layer 2, and improves the wear resistance in the rotational direction of the fixing belt 201. This makes it possible to reduce torque increase and stick-slip throughout the durability life, and improve the wear resistance.
[0132] The fixing belt 201 manufactured by the manufacturing method of this embodiment may have the configuration of the fixing belt 201 of the first embodiment, that is, the configuration in which the orientation rate Ro of the filler 2a in the inner peripheral side region 2b is smaller than the orientation rate Ro of the filler 2a in the base side region 2c. Alternatively, the fixing belt 201 manufactured by the manufacturing method of this embodiment may have the configuration of the fixing belt 201 of the second embodiment, that is, the configuration in which the average diameter of the Benard cell 6 is 50 μm or more and less than 200 μm.
[0133] In addition, in this embodiment, the case where the base-side temperature X and the inner periphery-side temperature Y satisfy the relationship of 10° C.≦XY≦30° C. has been described, but the present invention is not limited to this. Even if the relationship of 10° C.≦XY≦30° C. is not satisfied, it is sufficient that the surface roughness Ra is uniform within an appropriate range. [Explanation of symbols]
[0134] 1...substrate, 1a...inner circumferential surface, 1L...exhaust side portion (third position), 1U...suction side portion (fourth position), 2...sliding layer, 2a...filler, 2b...inner circumferential region (second position), 2c...substrate side region (first position), 2d...inner circumferential surface, 5...polyimide precursor solution (solution), 6...Benard cell, 201...fixing belt, 202...fixing heater (backup member), 206...pressure roller (rotating body), D0...reference direction, Dt...thickness direction, N...fixing nip portion (nip portion), S...recording material, t...toner image
Claims
1. A rotatable endless fixing belt that heats an unfixed toner image carried on a recording material and fixes the toner image on the recording material, the fixing belt being sandwiched between a rotating body provided on the outside of the fixing belt and a backup member provided on the inside of the fixing belt to form a nip portion between the rotating body and the fixing belt, where the toner image is fixed to the recording material, A substrate; a sliding layer formed on the inner circumferential side of the base body and in sliding contact with the backup member, The sliding layer contains a filler having shape anisotropy, when a direction along an inner circumferential surface of the base is taken as a reference direction, an orientation rate of the filler in the reference direction at a first position in a thickness direction of the sliding layer is a first value, and an orientation rate of the filler in the reference direction at a second position located closer to the inner circumferential surface of the sliding layer than the first position is a second value smaller than the first value. The fixing belt is characterized by the above-mentioned.
2. The sliding layer has a plurality of Benard cells having an average diameter of 50 μm or more and less than 200 μm on an inner circumferential surface of the sliding layer, and the arithmetic mean roughness of the inner circumferential surface of the sliding layer is 0.20 μm or more and 0.50 μm or less.
2. The fixing belt according to claim 1,
3. A rotatable endless fixing belt that heats an unfixed toner image carried on a recording material and fixes the toner image on the recording material, the fixing belt being sandwiched between a rotating body provided on the outside of the fixing belt and a backup member provided on the inside of the fixing belt to form a nip portion between the rotating body and the fixing belt, where the toner image is fixed to the recording material, A substrate; a sliding layer formed on the inner circumferential side of the base body and in sliding contact with the backup member, The sliding layer contains a filler having shape anisotropy, The sliding layer has a plurality of Benard cells having an average diameter of 50 μm or more and less than 200 μm on an inner circumferential surface, and the arithmetic mean roughness of the inner circumferential surface is 0.20 μm or more and 0.50 μm or less. The fixing belt is characterized by the above-mentioned.
4. The filler has an aspect ratio of 5 or more and 200 or less.
4. The fixing belt according to claim 1, wherein the fixing belt is a fixing belt having a thickness of 100 nm or less.
5. A method for manufacturing a fixing belt comprising: a rotatable endless fixing belt for heating an unfixed toner image carried on a recording material and fixing the toner image to the recording material, the fixing belt being sandwiched between a rotating body provided on the outside of the fixing belt and a backup member provided on the inside of the fixing belt to form a nip portion between the rotating body and the fixing belt, where the toner image is fixed to the recording material; a base body; and a sliding layer formed on an inner peripheral side of the base body and in contact with and slidable against the backup member, a coating step of coating an inner circumferential surface of the substrate with a solution in which a precursor of the sliding layer and a filler having an aspect ratio of 5 or more and 200 or less are dispersed in a solvent; a drying step of drying the solvent from the solution applied to the inner circumferential surface of the substrate, In the drying step, when the temperature of the outer peripheral surface of the base is set to a first temperature and the temperature of the atmosphere on the inner peripheral side of the sliding layer is set to a second temperature lower than the first temperature, the solvent is dried in such a manner that the difference between the first temperature and the second temperature is 10° C. or more and 30° C. or less. A method for manufacturing a fixing belt comprising the steps of:
6. In the drying step, a first fluid is caused to flow from one end side to the other end side in the rotation axis direction of the substrate outside the substrate, and a second fluid having a lower temperature than the first fluid is caused to flow from the other end side to the one end side inside the substrate, thereby drying the solvent. The method for manufacturing a fixing belt according to claim 5 .
7. In the coating step, a thickness of the solution at a third position in the direction of the rotation axis is set to a third value, and a thickness of the solution at a fourth position located on the other end side of the third position is set to a fourth value that is thicker than the third value; In the drying step, the temperature of the outer peripheral surface of the substrate at the third position is set to a third temperature, and the temperature of the outer peripheral surface of the substrate at the fourth position is set to a fourth temperature lower than the third temperature, thereby drying the solvent. The method for manufacturing a fixing belt according to claim 6 .
Citation Information
Patent Citations
Fixing belt
JP2007240845A
Image heating film, and image heating apparatus using the same
JP2008139777A
Method of measuring thickness-directional electric resistance distribution of conductive polymer sheet, intermediate transfer medium comprising conductive polymer sheet, and image forming device with intermediate transfer medium
JP2009075534A
Tubular body and method for manufacturing the same
JP2011209578A
Fixing member and fixing device including the same
JP2014077990A