Brazing material, brazing member and heat exchanger
A brazing material with fluoride flux, solidifying agent, and coating film homogenization aid addresses the challenge of uniform application in solid fluxes, achieving superior coating uniformity and efficiency in brazing aluminum or aluminum alloys.
Patent Information
- Application Number
- JP2021540754
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-20
- Filing Date
- 2020-08-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-08-13
AI Technical Summary
Conventional brazing compositions using solid fluxes face challenges in uniformly applying the composition to metal surfaces due to their solid state, leading to complications in production lines and potential scattering issues.
A brazing material containing fluoride flux, a solidifying agent, and a coating film homogenization aid, which remains solid at room temperature, ensuring excellent coating uniformity by reducing interaction between solidifying agents and improving shape retention.
The brazing material achieves uniform coating films on aluminum or aluminum alloys, enhancing production efficiency and reducing scattering issues, resulting in improved brazing quality and uniformity.
Smart Images

Figure 0007571030000003 
Figure 0007571030000001 
Figure 0007571030000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a brazing material, a brazing member, and a heat exchanger, and more particularly to a brazing material for brazing aluminum or an aluminum alloy, a brazing member provided with a coating film formed by applying the brazing material, and a heat exchanger provided with the brazing member. [Background technology]
[0002] Conventionally, when welding metal members, a flux is used to remove oxides from the metal members to be welded.
[0003] Usually, flux is liquid, so when it is applied to a welded part, the flux may flow. In addition, when the flux is liquid, a solvent drying facility is required to solidify the coating, which may cause the manufacturing line to become complicated, and further, the workability may be poor due to the scattering of the liquid flux.
[0004] Therefore, in order to simplify the production line and improve workability, the use of solid flux has been considered, and for example, a brazing composition has been proposed that is a uniform blend of brazing material powder, fluoride-based flux powder, and wax that is solid at room temperature (see, for example, Patent Document 1 below). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-314380 Summary of the Invention [Problem to be solved by the invention]
[0006] On the other hand, when the brazing composition is applied to an object to be coated by contacting the brazing composition in a solid state with the object to be coated and rubbing the composition as necessary, it is difficult to apply the brazing composition uniformly.
[0007] The present invention relates to a brazing material having excellent coating uniformity, a brazing member provided with a coating formed by applying the brazing material, and a heat exchanger provided with the brazing member. [Means for solving the problem]
[0008] The present invention [1] relates to a brazing material for brazing aluminum or an aluminum alloy, the brazing material including a fluoride-based flux, a solidifying agent, and a coating homogenizing aid, and being solid at 25°C.
[0009] The present invention [2] includes the brazing material according to the above [1], wherein the coating homogenizing auxiliary has a half-width of the largest peak in a diffraction angle (2θ) range of 19±2° in an X-ray diffraction pattern obtained under conditions of 10°C of 1° or more, and is at least one compound selected from the group consisting of esters of carboxylic acids having 10 or more carbon atoms and alcohols having less than 8 carbon atoms, esters of carboxylic acids having less than 10 carbon atoms and alcohols having 8 or more carbon atoms, and acetals having 10 or more carbon atoms.
[0010] The present invention [3] includes the brazing material according to the above [1] or [2], in which the coating homogeneity aid has a molecular weight of 1,000 or less.
[0011] The present invention [4] comprises the brazing material according to any one of the above [1] to [3], wherein the coating homogeneity aid has a half-width of 1° or more and 10° or less.
[0012] The present invention [5] further comprises the brazing material according to any one of the above [1] to [4], which further comprises a brazing material powder, the brazing material powder being made of a metal capable of forming a eutectic alloy with aluminum and / or an alloy of the metal and aluminum.
[0013] The present invention [6] includes a brazed member comprising aluminum or an aluminum alloy and a coating formed by applying the brazing material described in any one of the above [1] to [5] to the aluminum or the aluminum alloy.
[0014] The present invention [7] includes a heat exchanger comprising the brazed member described in [6] above. Effect of the Invention
[0015] The brazing material of the present invention contains a fluoride-based flux, a solidifying agent, and a coating uniformity aid, and is solid at 25° C., so that it has excellent coating uniformity.
[0016] The brazed member of the present invention has a coating film formed by applying the brazing material of the present invention, and therefore has excellent coating uniformity.
[0017] The heat exchanger of the present invention is obtained by using the brazing member of the present invention, and therefore has excellent coating uniformity. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is an X-ray diffraction pattern at 10° C. of stearylaldehyde methyl ethyl diethyl ether acrylate acetal obtained in Synthesis Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The brazing material of the present invention is a brazing material for brazing aluminum or an aluminum alloy, and contains a fluoride-based flux, a solidifying agent, and a coating homogeneity aid.
[0020] Examples of fluoride-based fluxes include Cs-Al-F based fluxes, K-Al-F based fluxes, and K-Zn-F based fluxes.
[0021] The Cs-Al-F flux is a fluoride flux containing cesium (Cs), aluminum (Al) and fluorine (F), such as cesium fluoroaluminate (non-reactive cesium flux).Specific examples include CsAlF4, Cs2AlF5, and Cs3AlF6.
[0022] The K-Al-F flux is a fluoride flux containing potassium (K), aluminum (Al) and fluorine (F), and examples thereof include potassium fluoroaluminate, etc. Specific examples include KAlF4, K2AlF5, and K3AlF6.
[0023] The K-Zn-F flux is a fluoride flux containing potassium (K), zinc (Zn) and fluorine (F), and examples thereof include potassium zinc fluoride. Specifically, examples thereof include KZnF3.
[0024] As the fluoride-based flux, preferably, a K-Al-F-based flux is used.
[0025] These fluoride-based fluxes can be used alone or in combination of two or more kinds.
[0026] The blending ratio of the fluoride-based flux, based on the total amount of the fluoride-based flux, solidifier, and coating homogeneity aid (hereinafter, the fluoride-based flux, solidifier, and coating homogeneity aid are collectively referred to as "brazing components"), from the viewpoint of brazing property (brazing break), is, for example, 1 mass% or more, preferably 10 mass% or more, more preferably 20 mass% or more, and even more preferably 30 mass% or more, and from the viewpoint of coating uniformity, is, for example, 80 mass% or less, preferably 60 mass% or less.
[0027] The content of the brazing components is, relative to the total amount of the brazing material, for example, 50 mass% or more, preferably 70 mass% or more, and for example, 100 mass% or less. For example, when the brazing material contains a brazing material described later, it is preferably 90 mass% or less, more preferably 80 mass% or less.
[0028] The solidifier is a component (excluding gelling agents) that adjusts the melting temperature and improves the shape retention so that the brazing material is solid at 25°C. In the present invention, 25°C is room temperature. Also, being in a solid state at 25°C may be referred to as "room temperature solid."
[0029] In the present invention, the solidifying agent is defined as at least one compound selected from the group consisting of hydrocarbons that are solid at room temperature, alkyl alcohols that are solid at room temperature, ether alcohols that are solid at room temperature, and high-carbon carboxylic acid-high-carbon alcohol esters.
[0030] Examples of the hydrocarbons that are solid at room temperature include waxes that are solid at room temperature, such as natural waxes and synthetic waxes.
[0031] Examples of natural waxes include petroleum waxes such as paraffin wax and microcrystalline wax.
[0032] Examples of synthetic waxes include polyethylene wax and Fischer-Tropsch wax.
[0033] These room temperature solid hydrocarbons can be used alone or in combination of two or more kinds.
[0034] As the hydrocarbon that is solid at room temperature, preferably, natural wax is used, and more preferably, paraffin wax is used.
[0035] The mixing ratio of the room temperature solid hydrocarbon, relative to the total amount of the brazing components, from the viewpoint of shape retention and coating uniformity, is, for example, 1 mass% or more, preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, and for example, 99 mass% or less, more preferably 98 mass% or less, even more preferably 95 mass% or less.
[0036] The mixing ratio of the room temperature solid hydrocarbon relative to 100 parts by mass of the fluoride-based flux is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 100 parts by mass or more, even more preferably 150 parts by mass or more, and for example, 2000 parts by mass or less, preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 300 parts by mass or less.
[0037] Examples of alkyl alcohols that are solid at room temperature include normal alcohols (straight-chain alkyl alcohols) having 14 to 30 carbon atoms, such as tetradecanol, hexadecanol, octadecanol (stearyl alcohol), and eicosanol; normal dialcohols having 6 to 30 carbon atoms, such as 1,6-hexanediol; and polyhydric alcohols having 5 to 30 carbon atoms, such as trimethylolpropane and pentaerythritol.
[0038] These alkyl alcohols which are solid at room temperature can be used alone or in combination of two or more kinds.
[0039] From the viewpoint of shape retention and coating uniformity, the blending ratio of the room-temperature solid alkyl alcohol, relative to the total amount of the brazing components, is, for example, 1 mass% or more, preferably 5 mass% or more, more preferably 12 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, and for example, 99 mass% or less, more preferably 98 mass% or less, even more preferably 95 mass% or less.
[0040] The mixing ratio of the room temperature solid alkyl alcohol relative to 100 parts by mass of the fluoride-based flux is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 100 parts by mass or more, and for example, 2000 parts by mass or less, preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, and even more preferably 300 parts by mass or less.
[0041] Examples of ether alcohols that are solid at room temperature include polyether glycols such as polyoxyethylene glycol, polyoxypropylene glycol, and polyoxybutylene glycol; and polyether alcohols such as polyether monools such as polyethylene glycol monomethyl ether and polyethylene glycol monoethyl ether.
[0042] The molecular weight of these polyether alcohols is adjusted so that they are in a solid state at 25° C. For example, in ether alcohols that are solid at room temperature, the weight average molecular weight of polyoxyethylene glycol is 1,000 or more.
[0043] These ether alcohols which are solid at room temperature can be used alone or in combination of two or more kinds.
[0044] From the viewpoint of shape retention and coating uniformity, the blending ratio of the room-temperature solid ether alcohol relative to the total amount of the brazing components is, for example, 1 mass% or more, preferably 5 mass% or more, more preferably 12 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, and for example, 99 mass% or less, more preferably 98 mass% or less, even more preferably 95 mass% or less.
[0045] The mixing ratio of the room temperature solid ether alcohol relative to 100 parts by mass of the fluoride-based flux is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 100 parts by mass or more, and for example, 2000 parts by mass or less, preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, and even more preferably 300 parts by mass or less.
[0046] High carbon carboxylic acid-high carbon alcohol esters are esters that are the reaction products of carboxylic acids having 10 or more carbon atoms (described below) and alcohols having 8 or more carbon atoms (described below).
[0047] More specifically, the high-carbon carboxylic acid-high-carbon alcohol ester is an ester that is solid at 25° C. (solid at room temperature) and has relatively high crystallinity at 10° C., and more specifically, is an ester in which the half-width of the peak with the largest peak area width in the diffraction angle (2θ) range of 19±2° is less than 1° in an X-ray diffraction pattern obtained at 10° C. as described below. Such a high-carbon carboxylic acid-high-carbon alcohol ester improves the shape retention of the brazing material.
[0048] The high-carbon carboxylic acid-high-carbon alcohol ester can be obtained by subjecting one or more molecules of a carboxylic acid having 10 or more carbon atoms (described below) to an esterification reaction with one or more molecules of an alcohol having 8 or more carbon atoms (described below) by a known method.
[0049] More specific examples of the high carbon carboxylic acid-high carbon alcohol ester include carnauba wax, candelilla wax, and triacontanyl palmitic acid.
[0050] The high carbon carboxylic acid-high carbon alcohol esters can be used alone or in combination of two or more kinds.
[0051] From the viewpoint of shape retention and coating uniformity, the blending ratio of the high-carbon carboxylic acid-high-carbon alcohol ester relative to the total amount of the brazing components is, for example, 1 mass% or more, preferably 5 mass% or more, more preferably 12 mass% or more, even more preferably 20 mass% or more, even more preferably 30 mass% or more, and for example, 99 mass% or less, more preferably 98 mass% or less, even more preferably 95 mass% or less.
[0052] The mixing ratio of the high carbon carboxylic acid-high carbon alcohol ester relative to 100 parts by mass of the fluoride-based flux is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 100 parts by mass or more, and for example, 2000 parts by mass or less, preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, and even more preferably 300 parts by mass or less.
[0053] These solidifying agents can be used alone or in combination of two or more kinds.
[0054] As the solidifying agent, preferably, a room temperature solid hydrocarbon is used alone, or a room temperature solid alkyl alcohol is used alone. In addition, a room temperature solid hydrocarbon and a room temperature solid alkyl alcohol can be used in combination as the solidifying agent. When a room temperature solid hydrocarbon and a room temperature solid alkyl alcohol are used in combination, the mixing ratio of the room temperature solid hydrocarbon and the mixing ratio of the room temperature solid alkyl alcohol are appropriately adjusted within the above range.
[0055] The mixing ratio (total amount) of the solidifying agent relative to 100 parts by mass of the fluoride-based flux is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 100 parts by mass or more, and for example, 2000 parts by mass or less, preferably 1000 parts by mass or less, more preferably 500 parts by mass or less, and even more preferably 300 parts by mass or less.
[0056] The coating homogenizing aid is a component that reduces the interaction between the solidifiers in the brazing components and makes the brazing material easier to crumble, thereby improving the uniformity (homogenity) of the coating. The state of the coating homogenizing aid at room temperature (25°C) is not particularly limited, and it may be a solid or a liquid.
[0057] Such coating uniformity aids are solid at 10° C. and have relatively low crystallinity.
[0058] More specifically, a crystalline organic compound refers to an organic compound having a degree of crystallinity of 0 or more, which is defined as the peak area due to crystallinity at a diffraction angle (2θ) of 5° to 85° / (peak area due to crystallinity+peak area due to non-crystallinity) in an X-ray diffraction pattern obtained at 10°C.
[0059] Furthermore, among such organic compounds having crystallinity, a coating homogeneity aid (an organic compound having relatively low crystallinity) is defined as an organic compound in which, in an X-ray diffraction pattern obtained at 10°C, the half-value width of the peak having the largest peak area width within a diffraction angle (2θ) range of 19±2° is 1° or more.
[0060] The half width of the coating film uniformity aid is specifically, for example, 1° or more, preferably 1.5° or more, more preferably 2.0° or more, and even more preferably 3.5° or more, and while there is no particular upper limit, it is, for example, 10° or less, preferably 9.0° or less, more preferably 8.0° or less, even more preferably 6.0° or less, and particularly preferably 5.0° or less.
[0061] In the present invention, the coating homogeneity aid is at least one compound selected from the group consisting of high carbon carboxylic acid-low carbon alcohol esters, low carbon carboxylic acid-high carbon alcohol esters, and high carbon acetals.
[0062] In other words, in the present invention, the coating homogenizing aid is defined as at least one compound having the half-width of 1° or more and selected from the group consisting of high-carbon carboxylic acid-low-carbon alcohol ester, low-carbon carboxylic acid-high-carbon alcohol ester, and high-carbon acetal. The coating homogenizing aid is distinguished from the solidifying agent by its chemical structure. That is, the coating homogenizing aid does not include the solidifying agent. The coating homogenizing aid is also distinguished from a surfactant by its chemical structure. That is, the coating homogenizing aid does not include a surfactant.
[0063] High carbon carboxylic acid-low carbon alcohol esters are esters that are the reaction products of carboxylic acids containing 10 or more carbon atoms with alcohols containing less than 8 carbon atoms.
[0064] In the high carbon carboxylic acid-low carbon alcohol ester, examples of the carboxylic acid having 10 or more carbon atoms include monocarboxylic acids having 10 or more carbon atoms such as capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, lignoceric acid, etc., dicarboxylic acids having 10 or more carbon atoms such as decanedioic acid, dodecanedioic acid, etc., and anhydrides thereof. These can be used alone or in combination of two or more kinds.
[0065] Specifically, the carboxylic acid has 10 or more carbon atoms, preferably 14 or more, more preferably 16 or more, and further preferably 18 or more carbon atoms.
[0066] In the high carbon carboxylic acid-low carbon alcohol ester, examples of the alcohol having less than 8 carbon atoms include monohydric alcohols having less than 8 carbon atoms, such as methyl alcohol, ethyl alcohol, propyl alcohol, butyl alcohol, pentyl alcohol, hexyl alcohol, heptyl alcohol, and 3-methoxy-3-methyl-1-butyl alcohol, and polyhydric alcohols having less than 8 carbon atoms, such as methanediol, ethanediol, propanediol, butanediol, pentanediol, neopentyl glycol, hexanediol, and heptanediol. These may be used alone or in combination of two or more types.
[0067] Specifically, the number of carbon atoms of the alcohol is less than 8, preferably 7 or less, more preferably 6 or less, and further preferably 4 or less.
[0068] The high-carbon carboxylic acid-low-carbon alcohol ester can be obtained by esterification of one or more molecules of a carboxylic acid having 10 or more carbon atoms with one or more molecules of an alcohol having less than 8 carbon atoms in the presence of a known ester catalyst under appropriate conditions.
[0069] More specifically, examples of high carbon carboxylic acid-low carbon alcohol esters include myristic acid esters such as methyl myristate (half width 3.4°) and methoxymethylbutane myristate (half width 1.1°), palmitic acid esters such as methyl palmitate (half width 3.4°), stearic acid esters such as methyl stearate (half width 3.3°), butyl stearate (half width 3.8°), and methoxymethylbutane stearate (half width 1.1°), dicapric acid esters such as butyl dicaprate (half width 2.0°) and hexyl dicaprate (half width 1.5°), and lignoceric acid esters such as methyl lignocerate (half width 3.0°). These can be used alone or in combination of two or more types.
[0070] Low carbon carboxylic acid-high carbon alcohol esters are esters that are the reaction products of carboxylic acids containing less than 10 carbon atoms with alcohols containing 8 or more carbon atoms.
[0071] In the low carbon carboxylic acid-high carbon alcohol ester, examples of the carboxylic acid having less than 10 carbon atoms include monocarboxylic acids having less than 10 carbon atoms, such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, acrylic acid, and methacrylic acid, and dicarboxylic acids having less than 10 carbon atoms, such as phthalic acid, isophthalic acid, terephthalic acid, hydrogenated phthalic acid, hydrogenated isophthalic acid, and hydrogenated terephthalic acid, as well as anhydrides thereof. These may be used alone or in combination of two or more kinds.
[0072] Specifically, the carboxylic acid has less than 10 carbon atoms, preferably 9 or less, and more preferably 5 or less.
[0073] In the low carbon carboxylic acid-high carbon alcohol ester, examples of the alcohol having 8 or more carbon atoms include monohydric alcohols having 8 or more carbon atoms, such as octyl alcohol, lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, oleyl alcohol, and linolyl alcohol, and polyhydric alcohols having 8 or more carbon atoms, such as octanediol, nonanediol, decanediol, and dodecanediol. These may be used alone or in combination of two or more kinds.
[0074] Specifically, the alcohol has 8 or more carbon atoms, preferably 14 or more carbon atoms, and more preferably 18 or more carbon atoms.
[0075] The low-carbon carboxylic acid-high-carbon alcohol ester can be obtained by esterifying one or more molecules of a carboxylic acid having less than 10 carbon atoms with one or more molecules of an alcohol having 8 or more carbon atoms in the presence of a known ester catalyst under appropriate conditions.
[0076] More specifically, examples of low carbon carboxylic acid-high carbon alcohol esters include hydrogenated stearyl phthalate (half width 3.5°), hydrogenated lauryl phthalate (half width 3.0°), stearyl methacrylate (stearyl methacrylate (half width 1.0°)), etc. These can be used alone or in combination of two or more kinds.
[0077] High carbon acetals are acetals with 10 or more carbon atoms.
[0078] Specifically, the carbon number of the aldehyde or ketone of the high-carbon acetal is 10 or more, preferably 14 or more, and more preferably 18 or more.
[0079] More specifically, examples of high carbon acetals include acetals having 10 to 30 carbon atoms, such as stearylaldehyde methyl ethyl diethyl ether acrylate acetal (SteAc-VEEA, half-width 4.5°) and stearylaldehyde methyl ethyl diethyl ether methacrylate acetal (SteAc-VEEM, half-width 4.5°). These can be used alone or in combination of two or more kinds.
[0080] High-carbon acetals can be obtained, for example, by subjecting one or more molecules of a carboxylic acid having 10 or more carbon atoms to an acetalization reaction with a (meth)acrylate (e.g., vinyl ether ethoxy (meth)acrylate) under appropriate conditions, optionally in the presence of a catalyst.
[0081] These coating homogeneity aids can be used alone or in combination of two or more kinds.
[0082] The coating uniformity aid preferably includes a high carbon carboxylic acid-low carbon alcohol ester, more preferably a stearic acid ester.
[0083] The molecular weight of the coating homogeneity aid is, for example, 20 or more, preferably 50 or more, and for example, 1,000 or less, preferably 500 or less, from the viewpoint of coating uniformity.
[0084] When the coating homogenizing agent is a monomer, its molecular weight can be calculated from the molecular skeleton and the number of atoms. When the coating homogenizing agent is a polymer, its molecular weight is determined as a weight average molecular weight in terms of standard polystyrene by gel permeation chromatography. The molecular weight of the coating homogenizing agent is calculated as the average molecular weight of each component.
[0085] The content of the coating homogeneity aid relative to the total amount of the brazing components is, for example, 60 mass% or less, preferably 55 mass% or less, more preferably 50 mass% or less, even more preferably 40 mass% or less, and particularly preferably 25 mass% or less, and for example, 1 mass% or more, preferably, 5 mass% or more, more preferably, 10 mass% or more, and even more preferably, 15 mass% or more.
[0086] In addition, from the viewpoint of coating uniformity, the content of the coating film homogeneity auxiliary is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and more preferably 8 parts by mass or more, relative to 100 parts by mass of the total amount of the solidifier, and for example, 100 parts by mass or less, preferably 80 parts by mass or less, and more preferably 50 parts by mass or less.
[0087] The mixing ratio of the coating homogeneity auxiliary relative to 100 parts by mass of the fluoride-based flux is, for example, 1 part by mass or more, preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and for example, 100 parts by mass or less, preferably 80 parts by mass or less, more preferably 50 parts by mass or less.
[0088] These coating homogeneity aids can be used alone or in combination of two or more kinds.
[0089] Furthermore, the brazing material may optionally contain a brazing filler metal.
[0090] Examples of the brazing material include brazing materials made of metals capable of forming a eutectic alloy with aluminum, and brazing materials made of alloys of such metals with aluminum.
[0091] More specifically, the brazing material may be, for example, metal silicon, silicon-aluminum alloy, or alloys thereof containing small amounts of magnesium, copper, germanium, or the like.
[0092] The brazing material is preferably prepared in a powder form. That is, the brazing material is preferably a brazing material powder. The average particle size of the brazing material powder is not particularly limited and may be appropriately set depending on the purpose and application.
[0093] If the brazing material contains a brazing material, the working efficiency is excellent in brazing aluminum or an aluminum alloy.
[0094] The mixing ratio of the brazing material is, for example, 3 parts by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and for example, 300 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 45 parts by mass or less, relative to 100 parts by mass of the brazing components.
[0095] The mixing ratio of the brazing material is, relative to the total amount of the brazing material, for example, 1 mass% or more, preferably 10 mass% or more, more preferably 20 mass% or more, and for example, 60 mass% or less, preferably 40 mass% or less, more preferably 30 mass% or less.
[0096] In addition, the brazing material may contain various additives, such as antioxidants (e.g., dibutylhydroxytoluene, etc.), corrosion inhibitors (e.g., benzotriazole, etc.), defoamers (e.g., silicone oil, etc.), thickeners (e.g., fatty acid amides, polyamides, etc.), colorants, etc., in a proportion of 5 mass % or less based on the total amount of the brazing material, as necessary.
[0097] The brazing material can be obtained by mixing and stirring the above-mentioned components in the above-mentioned mixing ratio by a known method. At this time, the fluoride-based flux, the solidifying agent, and the coating homogenizing assistant are uniformly mixed, and then the brazing material is solidified by the solidifying agent. That is, the brazing material is solid, specifically, it is solid at 25°C.
[0098] Furthermore, in the brazing material, the coating homogenizing aid reduces the interaction between the solidifying agents, so the brazing material is prone to crumbling.
[0099] "Solid" at 25°C is defined as a substance that is determined to be "not liquid" when tested at 25°C in accordance with the method described in "Method of Confirming Liquidity" in "Fire Safety Hazard No. 11: Promulgation of the Cabinet Order Partially Amending the Cabinet Order Concerning the Control of Hazardous Materials (Part Relating to the Testing and Properties of Hazardous Materials) and the Ministerial Ordinance Concerning the Testing and Properties of Hazardous Materials (Notice)."
[0100] Furthermore, the brazing material is softened by heating.
[0101] More specifically, for example, when the above brazing material is applied to aluminum or an aluminum alloy, as described in detail below, it may be used in a solid state, but the brazing material may also be melted by heating and used.
[0102] The heating temperature is, for example, 40°C or more, preferably 60°C or more, more preferably 70°C or more, even more preferably 80°C or more, and particularly preferably 90°C or more, and for example, 400°C or less, preferably 300°C or less, more preferably 200°C or less, even more preferably 180°C or less, and particularly preferably 150°C or less.
[0103] That is, the brazing material particularly preferably melts at or below 150° C. In other words, the brazing material is preferably in a molten state at least at 150° C.
[0104] In such a case, the viscosity of the brazing material at 150°C (molten state) is, for example, 0.001 Pa·s or more, preferably 0.003 Pa·s or more, more preferably 0.006 Pa·s or more, even more preferably 0.02 Pa·s or more, and particularly preferably 0.05 Pa·s or more, and is, for example, 300 Pa·s or less, preferably 100 Pa·s or less.
[0105] If the viscosity at 150° C. is within the above range, particularly excellent coating uniformity can be obtained.
[0106] The viscosity at 150° C. is measured by a rheometer.
[0107] The brazing material contains a fluoride-based flux, a solidifying agent, and a coating homogeneity aid, and is solid at 25° C., so that it has excellent coating uniformity.
[0108] Therefore, the brazing material is used for brazing members made of aluminum or an aluminum alloy (Al members).
[0109] More specifically, the brazing material is, for example, melted by heating and applied to the substrate using a jet dispenser or the like, or is pressed in a solid state and applied to the substrate without melting.
[0110] Preferably, the brazing material is pressed in a solid state and applied to the workpiece without melting. In this case, for example, as described in International Publication WO2018 / 235906, a method of contacting a member (Al member) made of aluminum or an aluminum alloy with a solid brazing material, winding the Al member with a roll-type conveyor or the like, and moving the Al member relative to the brazing material, can be mentioned. By such a method, the solid brazing material is scraped off, and the scraped brazing material adheres (is applied) to the Al member.
[0111] Furthermore, when the above brazing material is used, excellent coating uniformity is achieved even when the material is applied in a solid state by contacting it with the workpiece.
[0112] Therefore, the brazing material is suitable for use in aluminum or aluminum alloy products. Specifically, the brazing material is suitable for use in the manufacture of brazing members including aluminum or aluminum alloys, and in the manufacture of heat exchangers using the brazing members.
[0113] The brazed member thus obtained has a coating film formed by applying the brazing material, and therefore has excellent coating uniformity. In addition, the heat exchanger obtained by using the brazed member thus obtained has excellent coating uniformity. EXAMPLES
[0114] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0115] 1.Measurement method (1) Half-width The coating homogeneity aid was subjected to X-ray analysis under the following conditions.
[0116] More specifically, the coating homogeneity aid was melted, poured into a 3 cm square mold, and allowed to crystallize at 10° C. for one day.
[0117] The sample thus obtained was subjected to XRD (X-Ray Diffraction) analysis at 10°C to measure the diffraction peaks. Based on this, the peaks were separated at a separation width (2θ) of 0.5° and fitting was performed to determine the peak assignments and half-widths of the coating homogeneity aids.
[0118] This allowed us to determine the "half-width of the peak with the largest peak width within the diffraction angle (2θ) range of 19±2° in the X-ray diffraction pattern obtained under conditions of 10°C."
[0119] The measurement conditions are as follows. Light source: Empyrean X-ray tube, Energy used: 40 kV·15 mA, X-ray exposure time: 260 seconds, Detector: Medipix3 PIXcel detector, Measurement range: 5°~85°, Step size: 0.0027166°2θ, Goniometer radius: 145 mm FIG. 1 shows the X-ray diffraction pattern at 10° C. of stearylaldehyde methyl ethyl diethyl ether acrylate acetal obtained in Synthesis Example 1 described later.
[0120] 2. Synthesis of coating homogeneity aid Synthesis Example 1 60 parts of stearic acid (product name: STEARIC ACID 98%, manufactured by Miyoshi Oil Co., Ltd.) and 40 parts of vinyl ether ethoxy acrylate (product name: VEEA, manufactured by NOF Corporation) were mixed, then heated to 100°C and reacted for 5 hours to obtain stearylaldehyde methyl ethyl diethyl ether acrylate acetal (hereinafter referred to as SteAC-VEEA; half-width 4.5°, molecular weight 470).
[0121] Synthesis Example 2 60 parts of stearic acid (product name: STEARIC ACID 98%, manufactured by Miyoshi Oil Co., Ltd.) and 40 parts of vinyl ether ethoxy methacrylate (product name: VEEM, manufactured by NOF Corporation) were mixed and reacted in the same manner as in Synthesis Example 1 to obtain stearylaldehyde methyl ethyl diethyl ether methacrylate acetal (hereinafter referred to as SteAC-VEEM, half-width 4.5°, molecular weight 484).
[0122] Synthesis Example 3 70.6 parts of stearic acid (trade name: STEARIC ACID 98%, manufactured by Miyoshi Oil Co., Ltd.) and 29.4 parts of 3-methoxy-3-methyl-1-butyl alcohol (trade name: Solfit, manufactured by Kuraray Co., Ltd.) were mixed, 0.05 parts of an ester catalyst (trade name: IRGANOX1425, manufactured by BASF) was added, and the mixture was heated to 160°C and stirred for 12 hours to obtain methoxymethylbutane stearate (half width: 1.1°, molecular weight: 384).
[0123] Synthesis Example 4 79.3 parts of capric acid (product name: Capric Acid 98, manufactured by Miyoshi Oil Co., Ltd.) and 20.7 parts of butanediol (product name: Primary 1,4-butanediol, manufactured by Kishida Chemical Co., Ltd.) were mixed and reacted in the same manner as in Synthesis Example 3 to obtain butyl dicaprate (half width 2.0°, molecular weight 398).
[0124] Synthesis Example 5 74.5 parts of capric acid (trade name: Capric Acid 98, manufactured by Miyoshi Oil Co., Ltd.) and 25.5 parts of hexanediol (trade name: 1,6-hexanediol, manufactured by Ube Industries, Ltd.) were mixed and reacted in the same manner as in Synthesis Example 3 to obtain hexyl dicaprate (half width: 1.5°, molecular weight: 426).
[0125] Synthesis Example 6 63.7 parts of stearyl alcohol (product name: Kalcol 8098, manufactured by Kao Corporation) and 36.3 parts of hydrogenated phthalic anhydride (product name: Rikacid HH, manufactured by New Japan Chemical Co., Ltd.) were mixed, 0.05 parts of triphenylphosphine (product name: PP-360, manufactured by K.I. Chemical Co., Ltd.) was added as a catalyst, and the mixture was reacted at 120°C for 8 hours to obtain stearyl phthalic anhydride (half width: 3.5°, molecular weight: 438).
[0126] 3. Manufacturing of brazing materials Example 1 According to the formulation shown in Table 1, a brazing material was obtained.
[0127] Specifically, 50.0 parts of potassium fluoroaluminate flux, 45.0 parts of paraffin wax, and 5.0 parts of SteAC-VEEA of Synthesis Example 1 above as a coating homogeneity aid were heated and mixed, poured into a specified mold, and cooled and molded to obtain a brazing material.
[0128] The braze material was solid at 25°C.
[0129] Examples 2 to 19, and Comparative Examples 1 and 2 A brazing material was obtained in the same manner as in Example 1, except that the compounding recipe was changed to that shown in Tables 1 and 2.
[0130] Regarding the brazing filler metal, Al-12%Si is an Al brazing filler metal containing 12% Si (product name: ECKA Aluminium-Silicon 12AN <0.025mm, manufactured by ECKA Granules Germany GmbH).
[0131] 4. Evaluation (1) Coating film uniformity The brazing material of each Example and Comparative Example was melted at 100°C, poured into a cylindrical mold (aluminum chiffon cake mold 10 cm) with a diameter of 10 cm (inner diameter 9 cm), and left at room temperature for 1 hour to solidify. A rotating shaft was inserted into the inner space of the obtained cylindrical sample, and the sample was cut so that the width of the curved surface was 5 cm and the curved surface was parallel to the rotating shaft, to prepare a sample for coating.
[0132] The obtained cylindrical sample was then set in a solid material pressing applicator (manufactured by Daiseki) and pressed against an aluminum substrate (length: 250 m, width: 5 cm, thickness: 100 μm) conveyed at 150 m / min. At this time, the rotating shaft of the sample was rotated at 2000 rpm by a drill (manufactured by Makita, DF-458D) with a set load of 10 kg.
[0133] This resulted in an aluminum substrate having the brazing material applied thereto in a solid state.
[0134] Thereafter, the coating uniformity was evaluated according to the following criteria, and the results are shown in Tables 1 and 2.
[0135] That is, the aluminum substrate of the prepared test piece was observed under the specified conditions (magnification: 20x, illumination: ring illumination, illumination intensity: 50%, reflected light removed) using an optical microscope (digital microscope VHX-1000, manufactured by Keyence).
[0136] The upper and lower limits of brightness in the obtained observation image were set to 255 and 0, respectively, and binarization was performed with 140 as the boundary.
[0137] Thereafter, the area with high brightness (brightness) in the obtained observation image was regarded as the area where the coating film was formed, and the ratio of the area where the coating film was formed (coating film area) to the whole was calculated and evaluated according to the following criteria. Note that a larger coating film area was regarded as more excellent in uniformity.
[0138] S: Coating area is less than 100% and more than 92%.
[0139] A: The coating area is less than 91% and more than 84%.
[0140] B: Coating area is less than 83% and more than 76%.
[0141] C: Coating area is less than 75% and more than 66%.
[0142] ×: Coating area is 66% or less.
[0143] *: Because it is difficult to form a coating, the coating area was corrected as follows for evaluation.
[0144] That is, when the brazing material was melted at 100°C to prepare a sample for coating, the brazing material did not become a homogeneous liquid. In addition, even when the molten brazing material was poured into a cylindrical mold and the solidified brazing material was scraped, it could not be formed into the desired cylindrical shape, and the curved surface was irregular. Then, when the obtained sample was applied to an aluminum substrate, the obtained coating film had areas where the sample was not applied (holes in the film). Therefore, the "tentative coating film area" of the obtained coating film was corrected as follows and evaluated as the "coating film area".
[0145] More specifically, first, before applying the sample, a solution containing a dye was applied to the curved surface of the sample. Then, the surface shape was transferred to paper and captured as an image by a scanner. Next, the transferred image was binarized using image analysis software ImageJ (Wayne Rasband, version 1.52a). In the binarization process, the border was set to a count number of 95% or less of the peak of the transferred image. After that, the ratio of the actual contact area between the actual sample and the paper to the desired transfer shape (the contact area between the sample of the desired shape and the paper) was measured and used as a correction parameter. Then, the coating area was corrected according to the following formula.
[0146] Corrected coating area = Pre-corrected coating area / Correction parameters (2) Brazeability (2-1) Appearance The brazing material of each Example and Comparative Example was heated to 90°C to melt, and then applied with 10 g / m2 of fluoride-based flux to an aluminum member (150 mm x 70 mm x 0.8 mm). 2 The coating was applied in a circle with a diameter of 10 mm so as to prepare a test specimen.
[0147] Thereafter, the test pieces were brazed by heating at 600° C. in a nitrogen gas atmosphere (oxygen concentration 100 ppm or less) using a brazing furnace (box-shaped electric furnace, manufactured by Noritake TGF, A(V)-DC-M).
[0148] The performance was evaluated in the following tests, and the results are shown in Tables 1 and 2.
[0149] The appearance after the brazing test was visually evaluated according to the following criteria. A: There was almost no black color. B: Black color was observed in part of the applied area.
[0150] (2-2) Braze cut The brazing material of each Example and Comparative Example was heated to 90°C to melt, and then applied with 10 g / m of fluoride-based flux to an aluminum member (JIS-BAS121P (cladding rate 10%), 60 mm x 25 mm x 1.0 mm) made of a brazing sheet in which an aluminum alloy was clad with a silicon-aluminum alloy (brazing material). 2 Next, an aluminum alloy (JIS-A3003, 55mm x 25mm x 1.0mm) was used as a vertical member, which was attached to the horizontal member in an inverted T-shape and fixed with stainless steel wire to prepare a test piece for brazing evaluation.
[0151] Thereafter, the test pieces were brazed by heating at 600° C. in a nitrogen gas atmosphere (oxygen concentration 100 ppm or less) using a brazing furnace (box-shaped electric furnace, manufactured by Noritake TGF, A(V)-DC-M).
[0152] The performance was evaluated in the following tests, and the results are shown in Tables 1 and 2.
[0153] After the brazing test, the fillets were visually evaluated according to the following criteria. ○: A continuous fillet was formed over the entire area where the horizontal and vertical members met. ×: A fillet was formed in part of the area where the horizontal and vertical materials came into contact, but the fluoride-based flux had poor dispersibility and was not evenly applied, so the fillet was found to be discontinuous.
[0154] (3) Coating adhesion The brazing material of each Example and Comparative Example was melted at 100°C, poured into a cylindrical mold (aluminum chiffon cake mold 10 cm) with a diameter of 10 cm (inner diameter 9 cm), and left at room temperature for 1 hour to solidify. A rotating shaft was inserted into the inner space of the obtained cylindrical sample, and the sample was cut so that the width of the curved surface was 5 cm and the curved surface was parallel to the rotating shaft, to prepare a sample for coating.
[0155] The obtained cylindrical sample was then set in a solid material pressing applicator (manufactured by Daiseki) and pressed against an aluminum substrate (length: 250 m, width: 5 cm, thickness: 100 μm) conveyed at 150 m / min. At this time, the rotating shaft of the sample was rotated at 2000 rpm by a drill (manufactured by Makita, DF-458D) with a set load of 10 kg.
[0156] This resulted in an aluminum substrate having the brazing material applied thereto in a solid state.
[0157] Thereafter, the coating adhesion was evaluated according to the following criteria, and the results are shown in Tables 1 and 2.
[0158] That is, the prepared test pieces were subjected to an abrasion test under specified conditions (speed: 60 mm / min, scale: 7 mm, count: single, traction force: 20 N, steel wool: Bonstar #0000) using Tribogear (manufactured by Shinto Chemical Industry Co., Ltd.) to evaluate the adhesion of the coating film to the aluminum substrate.
[0159] S: When a load of 50 g was applied, the coating did not fall off and the substrate was not exposed.
[0160] A: When a load of 40 g was applied, the coating did not fall off to expose the substrate.
[0161] B: When a load of 30 g was applied, the coating film did not fall off to expose the substrate.
[0162] C: When a load of 10 g was applied, the coating film did not fall off and the substrate was not exposed.
[0163] D: When a load of 5 g was applied, the coating film did not fall off and the substrate was not exposed.
[0164] [Table 1]
[0165] [Table 2]
[0166] The details of each component in the table are as follows: Brazing material Al-12%Si: Al brazing material containing 12% Si, product name ECKA Aluminium-Silicon 12AN <0.025mm, manufactured by ECKA Granules Germany GmbH ·Fluoride-based flux K-Al-F flux: Product name: Nocolok flux, manufactured by SOLVAY Solidification agent Paraffin wax: Product name: Paraffin Wax-135, manufactured by Nippon Seiro Co., Ltd. Stearyl alcohol: Product name: Kalcol 8098, Kao (melting point: 59°C) ·Coating homogeneity aid SteAc-VEEA: Stearyl aldehyde methyl ethyl diethyl ether acrylate = acetal, half width 4.5°, synthesis example 1 SteAc-VEEM: Stearyl aldehyde methyl ethyl diethyl ether methacrylate = acetal, half width 4.5°, synthesis example 2 Stearyl methacrylate: Product name SMA, manufactured by Mitsubishi Gas Chemical Company, half-width 1.0, molecular weight 339 Methoxymethylbutane stearate: Half width 1.1°, molecular weight 384, synthesis example 3 Methyl stearate: Product name: Methyl stearate 95, NOF Corporation, half-width 3.3°, molecular weight 298 Butyl stearate: Product name: Butyl stearate, NOF Corporation, half-width 3.8°, molecular weight 340 Butyl dicaprate: half width 2.0°, molecular weight 398, synthesis example 4 Hexyl dicaprate: Half width 1.5°, molecular weight 426, synthesis example 5 Stearyl phthalate anhydride: Half-width 3.5°, molecular weight 438, synthesis example 6 Methyl Lignocerate: Product name: Methyl Lignocerate, manufactured by Tokyo Chemical Industry Co., Ltd., half-width 3.0°, molecular weight 382 Methyl palmitate: Product name: Methyl Palmitate, manufactured by Tokyo Chemical Industry Co., Ltd., half-width 3.4°, molecular weight 270 Methyl myristate: Product name: Methyl Myristate, manufactured by Tokyo Chemical Industry Co., Ltd., half-width 3.4°, molecular weight 242 Polyethylene: Product name Nipolon Hard 7300A, Tosoh Corporation, half-width 4.5°, molecular weight 20,000 The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as being limited. Modifications of the present invention that are obvious to those skilled in the art are included in the scope of the following claims. [Industrial Applicability]
[0167] The brazing material and brazing member of the present invention are suitably used in the manufacture of heat exchangers comprising aluminum or an aluminum alloy.
Claims
1. A brazing material for brazing aluminum or an aluminum alloy, Fluoride-based flux, A solidifying agent; Coating homogeneity aid and Including, It is a solid at 25°C; The coating homogeneity aid is In an X-ray diffraction pattern obtained under conditions of 10° C., the half-width of the peak having the largest peak width within a diffraction angle (2θ) range of 19±2° is 1° or more; at least one compound selected from the group consisting of esters of carboxylic acids having 10 or more carbon atoms and alcohols having less than 8 carbon atoms, esters of carboxylic acids having less than 10 carbon atoms and alcohols having 8 or more carbon atoms, and acetals having 10 or more carbon atoms, The solidifying agent is at least one compound selected from the group consisting of a room-temperature solid hydrocarbon, a room-temperature solid alkyl alcohol, a room-temperature solid ether alcohol, and a high-carbon carboxylic acid-high-carbon alcohol ester, which are in a solid state at 25°C; The high carbon carboxylic acid-high carbon alcohol ester is an ester of a carboxylic acid having 10 or more carbon atoms and an alcohol having 8 or more carbon atoms, and the half width is less than 1°.
2. The coating homogeneity aid has a molecular weight of 1000 or less. The brazing material according to claim 1 , characterized in that
3. The coating homogeneity aid has a half-width of 1° or more and 10° or less. The brazing material according to claim 1 , characterized in that
4. Further, the brazing material powder is included, The brazing material powder is made of a metal capable of forming a eutectic alloy with aluminum and / or an alloy of the metal and aluminum. The brazing material according to claim 1 , characterized in that
5. Aluminum or an aluminum alloy; A coating film formed by applying the brazing material according to claim 1 to the aluminum or the aluminum alloy. A brazed member comprising:
6. A heat exchanger comprising the brazed member according to claim 5.
Citation Information
Patent Citations
Brazing material
JP1978033952A
Composition for brazing aluminum material, brazing aluminum material, and brazing method for aluminum material
JP1997314380A
Paste composition for aluminum brazing
JP2009166122A
Brazing paste
JP2014237145A
Brazing FLUX composition comprising a lubricant
WO2007080160A1