Solid Electrolytic Capacitor
Incorporating depolarizers into the solid electrolyte of capacitors stabilizes conductive polymers, addressing high leakage current issues and ensuring stable performance under high voltage and humidity conditions.
Patent Information
- Application Number
- JP2021568523
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-17
- Filing Date
- 2020-05-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-05-15
AI Technical Summary
Conventional solid electrolytic capacitors using in-situ polymerized polymers suffer from high leakage currents and failure at high voltages due to issues with conductive polymers, such as poly(3,4-ethylenedioxythiophene) and poly(styrene sulfonic acid) complexes, which are prone to degradation by hydrogen radicals formed during high voltage operations.
Incorporation of a depolarizer, such as aromatic quinones or nitroaromatic compounds, into the solid electrolyte to react with hydrogen radicals and stabilize the conductive polymer, thereby enhancing the capacitor's electrical properties.
The capacitors exhibit stable electrical characteristics with low equivalent series resistance (ESR), leakage current, and capacitance retention under high voltage, temperature, and humidity conditions, maintaining performance over extended periods.
Smart Images

Figure 0007571057000010 
Figure 0007571057000001 
Figure 0007571057000002
Abstract
Description
[Technical field]
[0001] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 849,395, having a filing date of May 17, 2019, which is incorporated by reference in its entirety. [Background technology]
[0002] Solid electrolytic capacitors (e.g., tantalum capacitors) are typically fabricated by pressing metal powder (e.g., tantalum) around metal leads, sintering the pressed part, anodizing the sintered anode, and then applying a solid electrolyte. Intrinsically conductive polymers are often used as the solid electrolyte due to their advantageous low equivalent series resistance (ESR) and "non-burn / non-ignition" failure mode. For example, such electrolytes can be formed by in-situ chemical polymerization of 3,4-dioxythiophene monomer (EDOT) in the presence of a catalyst and a dopant. However, conventional capacitors using in-situ polymerized polymers have relatively high leakage currents (DCL) and tend to fail at high voltages such as those experienced during fast switching or operating current spikes. In an attempt to overcome these problems, dispersions formed from a composite of poly(3,4-ethylenedioxythiophene) and poly(styrenesulfonic acid) (PEDOT:PSS) have also been used. Although some benefits are achieved with these capacitors, problems remain. Therefore, a need exists for improved solid electrolytic capacitors that can exhibit stable electrical properties. Summary of the Invention
[0003] According to one embodiment of the present invention, a solid electrolytic capacitor is disclosed that includes a capacitor element comprising a sintered porous anode body, a dielectric disposed on the anode body, and a solid electrolyte disposed on the dielectric, the solid electrolyte comprising a conductive polymer and a depolarizer.
[0004] Other features and aspects of the invention are set forth in more detail below.
[0005] A full and enabling disclosure of the present invention, including the best mode thereof, directed to one of ordinary skill in the art, is set forth more particularly in the remainder of the specification, which makes reference to the appended drawings, in which: [Brief description of the drawings]
[0006] [Figure 1] FIG. 1 is a perspective view of one embodiment of a capacitor of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Repeat use of reference characters in the present specification and drawings is intended to represent same or analogous features or components of the invention.
[0008] It will be appreciated by those skilled in the art that this discussion is a description of exemplary embodiments only and is not intended to limit the broader aspects of the invention, which may be embodied in the exemplary configurations.
[0009] Generally speaking, the present invention relates to a solid electrolytic capacitor comprising a capacitor element comprising a sintered porous anode body, a dielectric disposed on the anode body, and a solid electrolyte disposed on the dielectric, the solid electrolyte comprising a conductive polymer. While not intending to be limited by theory, it is believed that certain conditions (e.g., high relative humidity and temperature) can result in condensation of water on the capacitor, thereby forming a dissolved salt that results in ionic conduction between the anode and the cathode. This ionic conduction can involve current flow and electrolysis, which can generate hydrogen radicals that decompose the conductive polymer. However, the inventors have found that by incorporating a depolarizer into the solid electrolyte, it is possible to produce ions (e.g., metal ions) that can react with the hydrogen radicals and thus protect the polymer, which can be more easily reduced. In this regard, it is generally desirable to use a depolarizer that has a standard reduction potential (E0) greater than 0, in some embodiments greater than about 0.1 volts, in some embodiments greater than 0.2 volts, and in some embodiments greater than about 0.4 volts (e.g., from about 0.5 to about 1 volt), measured against a standard hydrogen electrode at 25° C. and 1 mole / liter (for liquid).Some examples of such depolarizers include aromatic quinones such as 1,4-benzoquinone, 2-phenyl-1,4-benzoquinone, 2-methyl-1,4-benzoquinone, 2-tert-butyl-1,4-benzoquinone, 2-methoxy-1,4-benzoquinone, 2,6-dimethyl-1,4-benzoquinone, 2,3-dimethyl-1,4-benzoquinone, trimethyl-1,4-benzoquinone, 2,6-dimethoxy-1,4-benzoquinone, 2,5-dimethoxy-1,4-benzoquinone, tetramethyl-1,4-benzoquinone, tetrafluoro-1,4-benzoquinone, 2,5-dichloro-1,4-benzoquinone, tetrachloro-1,4-benzoquinone, 2-chloro-1,4-benzoquinone, etc.; 2-nitrophenol, 3-nitrophenol, 4-nitrophenol, 2-nitrobenzoic acid, 3-nitrobenzoic acid, etc. Nitroaromatic compounds such as benzoic acid, 4-nitrobenzoic acid, 2-nitroacetophenone, 3-nitroacetophenone, 4-nitroacetophenone, 2-nitroanisole, 3-nitroanisole, 4-nitroanisole, 2-nitrobenzaldehyde, 3-nitrobenzaldehyde, 4-nitrobenzaldehyde, 2-nitrobenzyl alcohol, 3-nitrobenzyl alcohol, 4-nitrobenzyl alcohol, 2-nitrophthalic acid, 3-nitrophthalic acid, 4-nitrophthalic acid, 2-methyl-3-nitrobenzoic acid, 2-methyl-6-nitrobenzoic acid, 3-methyl-2-nitrobenzoic acid, 3-methyl-4-nitrobenzoic acid, 3-methyl-6-nitrobenzoic acid, 4-methyl-3-nitrobenzoic acid; and the like, as well as derivatives, salts, anhydrides, and mixtures of any of the above. Typically, the depolarizer comprises from about 1 to about 500 ppm, in some embodiments from about 10 to about 200 ppm, and in some embodiments, from about 20 to about 150 ppm of the solid electrolyte.
[0010] As a result of the unique properties of the solid electrolyte, the resulting capacitor may exhibit excellent electrical properties. For example, the capacitor may exhibit a relatively low equivalent series resistance (ESR), such as about 200 milliohms, in some embodiments less than about 200 milliohms, in some embodiments less than about 150 milliohms, in some embodiments from about 0.01 to about 125 milliohms, and in some embodiments from about 0.1 to about 100 milliohms, measured at an operating frequency of 100 kHz and a temperature of about 23° C. The capacitor may also exhibit a relatively low equivalent series resistance (ESR), such as about 30 nanofarads per square centimeter (nF / cm), measured at a frequency of 120 Hz and a temperature of about 23° C. 2 ) or more, and in some embodiments, about 100 nF / cm 2 In some embodiments, the range is about 200 to about 3,000 nF / cm 2 In some embodiments, the range is from about 400 to about 2,000 nF / cm 2After being subjected to an applied voltage (e.g., 120 volts) for a period of time from about 30 minutes to about 20 hours, in some embodiments from about 1 hour to about 18 hours, and in some embodiments from about 4 hours to about 16 hours, the capacitor may also exhibit a leakage current (DCL) of about 100 microamps (μA) or less, in some embodiments from about 70 μA or less, and in some embodiments, from about 1 to about 50 μA. Notably, such electrical properties (e.g., ESR, DCL, and / or capacitance) may remain stable even at elevated temperatures. For example, the capacitor may exhibit ESR, DCL, and / or capacitance values within the above ranges even after exposure to temperatures of about 80° C. or higher, in some embodiments, from about 100° C. to about 180° C., and in some embodiments, from about 105° C. to about 150° C. (e.g., about 105° C., 125° C., or 150° C.), for a substantial period of time, such as about 100 hours or more, in some embodiments, from about 150 hours to about 3,000 hours, and in some embodiments, from about 200 hours to about 2,500 hours (e.g., 250, 500, 750, or 1,000 hours). For example, in one embodiment, the ratio of the ESR, DCL, and / or capacitance value of a capacitor after 1,000 hours of exposure to an elevated temperature (e.g., about 125° C.) to the initial ESR, DCL, and / or capacitance value of the capacitor (e.g., about 23° C.) is about 3.0 or less, in some embodiments about 2.0 or less, in some embodiments about 1.8 or less, in some embodiments about 1.6 or less, and in some embodiments, from about 0.9 to about 1.3.
[0011] The capacitors may also exhibit ESR, DCL, and / or capacitance values within the ranges described above after exposure to high relative humidity levels, either at room temperature or at elevated temperatures (e.g., about 85° C.). Such high relative humidity levels may be, for example, about 40% or more, in some embodiments about 45% or more, in some embodiments about 50% or more, and in some embodiments about 70% or more (e.g., about 85%-100%) for a significant period of time as described above. Relative humidity may be determined, for example, according to ASTM-E337-02, Method A (2007). For example, in one embodiment, the ratio of the ESR, DCL, and / or capacitance value of a capacitor after exposure to a high humidity level (e.g., about 85%) and high temperature (e.g., about 85° C.) for 1,000 hours to the initial ESR, DCL, and / or capacitance value (e.g., about 23° C.) is about 2.0 or less, in some embodiments about 1.8 or less, in some embodiments about 1.6 or less, and in some embodiments, from about 0.9 to about 1.3.
[0012] The capacitors may also exhibit a high percentage of their wet capacitance, which allows the capacitor to have only a small capacitance loss and / or variation in the presence of atmospheric moisture. This performance characteristic is determined by the formula: Wet to dry capacitance = (dry capacitance / wet capacitance) x 100 The wet-to-dry capacitance is quantified by the "wet-to-dry capacitance percentage" as determined by:
[0013] The present capacitors may exhibit a wet to dry capacitance percent of about 50% or greater, in some embodiments about 60% or greater, in some embodiments about 70% or greater, and in some embodiments, about 80%-100%.
[0014] It is also believed that the dissipation factor of the capacitor can be maintained at a relatively low level. Dissipation factor generally refers to the losses that occur in a capacitor and is usually expressed as a percentage of ideal capacitor performance. For example, the dissipation factor of the capacitor is typically about 250% or less, in some embodiments about 200% or less, and in some embodiments about 1% to about 180% at a frequency of 120 Hz. The capacitor can also be used in high voltage applications, such as rated voltages of about 35 volts or more, in some embodiments about 50 volts or more, and in some embodiments about 60 volts to about 200 volts. The capacitor can exhibit a relatively high "breakdown voltage" (the voltage at which the capacitor breaks down), such as, for example, about 60 volts or more, in some embodiments about 70 volts or more, in some embodiments about 80 volts or more, and in some embodiments about 100 volts to about 300 volts. In addition, the capacitor can also withstand relatively high surge currents that are also common in high voltage applications. The peak surge current may be, for example, greater than or equal to about 100 amps, in some embodiments greater than or equal to about 200 amps, and in some embodiments, between about 300 amps and about 800 amps.
[0015] Various embodiments of the capacitor will now be described in detail.
[0016] I. Capacitor element A. Anode body The capacitor element includes an anode including a dielectric formed on a sintered porous body. The porous anode body can be formed from a powder including a valve metal (i.e., a metal that can be oxidized) or a valve metal-based compound, such as tantalum, niobium, aluminum, hafnium, titanium, alloys thereof, oxides thereof, nitrides thereof, and the like. The powder is typically formed from a reduction process in which a tantalum salt (e.g., potassium fluotantalate (K2TaF7), sodium fluotantalate (Na2TaF7), tantalum pentachloride (TaCl5), and the like) is reacted with a reducing agent. The reducing agent can be provided in the form of a liquid, gas (e.g., hydrogen), or solid, such as a metal (e.g., sodium), a metal alloy, or a metal salt. For example, in one embodiment, a tantalum salt (e.g., TaCl5) can be heated at a temperature of about 900°C to about 2,000°C, in some embodiments about 1,000°C to about 1,800°C, and in some embodiments about 1,100°C to about 1,600°C to form a vapor, which can be reduced in the presence of a gaseous reducing agent (e.g., hydrogen). Further details of such reduction reactions are described in WO-2014 / 199480 by Maeshima et al. After reduction, the product can be cooled, crushed, and washed to form a powder.
[0017] The specific charge of the powder typically varies from about 2,000 to about 800,000 microfarads·volts per gram (μF·V / g) depending on the desired application. As is known in the art, the specific charge can be determined by multiplying the capacitance by the anodization voltage used and then dividing this product by the weight of the anodized electrode body. For example, low charge powders can be used having a specific charge of about 2,000 to about 70,000 μF·V / g, in some embodiments about 5,000 to about 60,000 μF·V / g, and in some embodiments about 10,000 to about 50,000 μF·V / g. Of course, highly charged powders can also be used, such as those having a specific charge of about 70,000 to about 800,000 μF·V / g, and in some embodiments, about 80,000 to about 700,000 μF·V / g, and in some embodiments, about 100,000 to about 600,000 μF·V / g.
[0018] The powder may be a free-flowing fine powder comprising primary particles. The primary particles of the powder generally have a median diameter (D50) of about 5 to about 500 nanometers, in some embodiments about 10 to about 400 nanometers, and in some embodiments about 20 to about 250 nanometers, as determined, for example, using a laser particle size distribution analyzer (e.g., LS-230) from BECKMAN COULTER Corporation, optionally after subjecting the particles to ultrasonic vibration for 70 seconds. Primary particles typically have a three-dimensional particle shape (e.g., spherical or angular). Such particles typically have a relatively low "aspect ratio," i.e., the average diameter or width of the particle divided by the average thickness (D / T). For example, the aspect ratio of the particles may be about 4 or less, in some embodiments about 3 or less, and in some embodiments about 1 to about 2. In addition to primary particles, the powder may include other types of particles, such as secondary particles formed by aggregation (or agglomeration) of the primary particles. Such secondary particles may have a median diameter (D50) of from about 1 to about 500 micrometers, and in some embodiments, from about 10 to about 250 micrometers.
[0019] The particles can be aggregated by heating the particles and / or by using a binder, for example, at a temperature of from about 0° C. to about 40° C., in some embodiments from about 5° C. to about 35° C., and in some embodiments from about 15° C. to about 30° C. Also suitable binders may include, for example, poly(vinyl butyral); poly(vinyl acetate); poly(vinyl alcohol); poly(vinylpyrrolidone); cellulose polymers such as carboxymethyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, and methylhydroxyethyl cellulose; atactic polypropylene, polyethylene; polyethylene glycols (e.g., Carbowax from Dow Chemical Co.); polystyrene, poly(butadiene / styrene); polyamides, polyimides, and polyacrylamides, high molecular weight polyethers; copolymers of ethylene oxide and propylene oxide; fluoropolymers such as polytetrafluoroethylene, polyvinylidene fluoride, and fluoroolefin copolymers; acrylic polymers such as sodium polyacrylate, poly(lower alkyl acrylates), poly(lower alkyl methacrylates), and copolymers of lower alkyl acrylates and methacrylates; and fatty acids and waxes such as stearic acid and other soap fatty acids, vegetable waxes, microcrystalline waxes (refined paraffins), and the like.
[0020] The resulting powder can be compressed to form pellets using any conventional powder pressing equipment. For example, a press can be used that is a single station compression press that includes a die and one or more punches. Alternatively, an anvil type compression press can be used that uses only a die and a single lower punch. Single station compression presses are available in several basic types such as cam presses, toggle / knuckle presses, and eccentric / crank presses with various capabilities such as single action, double action, floating die, moving platen, opposed ram, screw, impact, hot pressing, coining, or sizing. The powder can be compressed around the anode lead, which can be in the form of a wire, sheet, or the like. The lead can extend longitudinally from the anode body and can be formed from any conductive material such as tantalum, niobium, aluminum, hafnium, titanium, and the like, as well as conductive oxides and / or nitrides thereof. Connection of the lead to the anode body can also be accomplished using other known techniques, such as by welding the lead to the anode body or embedding it within the anode body during formation (e.g., prior to pressing and / or sintering).
[0021] After compression, the resulting anode body can be cut into any desired shape, such as square, rectangular, circular, oval, triangular, hexagonal, octagonal, heptagonal, pentagonal, etc. The anode body can then be subjected to a heating step that removes most, if not all, of the binder / lubricant. For example, the binder can be removed by heating the pellets under vacuum at a certain temperature (e.g., about 150°C to about 500°C) for several minutes. Alternatively, the binder can be removed by contacting the pellets with an aqueous solution, such as described in U.S. Patent No. 6,197,252 to Bishop et al. The pellets are then sintered to form a porous, integral member. The pellets are typically sintered at a temperature of about 700°C to about 1600°C, in some embodiments about 800°C to about 1500°C, in some embodiments about 900°C to about 1200°C, for about 5 minutes to about 100 minutes, in some embodiments about 8 minutes to about 15 minutes. This can be done in one or more steps. If desired, sintering can be carried out in an atmosphere that limits the migration of oxygen atoms to the anode. For example, sintering can be carried out in a reducing atmosphere, such as in a vacuum, in an inert gas, or in hydrogen. The reducing atmosphere can be at a pressure of about 10 Torr to about 2000 Torr, in some embodiments about 100 Torr to about 1000 Torr, and in some embodiments about 100 Torr to about 930 Torr. Mixtures of hydrogen and other gases, such as argon or nitrogen, can also be used.
[0022] B. Dielectric The anode is coated with a dielectric. The dielectric can be formed by anodizing a sintered anode body such that a dielectric layer is formed on and / or within the anode. For example, a tantalum (Ta) anode can be anodized to tantalum pentoxide (Ta2O5). Typically, anodization is performed by first applying a solution to the anode, such as by immersing the anode in the electrolyte. A solvent such as water (e.g., deionized water) is typically used. To increase ionic conductivity, compounds that can dissociate in the solvent to form ions can be used. Examples of such compounds include acids, such as those described below with respect to the electrolyte. For example, an acid (e.g., phosphoric acid) can comprise about 0.01% to about 5% by weight, in some embodiments about 0.05% to about 0.8% by weight, and in some embodiments about 0.1% to about 0.5% by weight of the anodization solution. Blends of acids can also be used if desired.
[0023] A current is passed through the anodizing solution to form the dielectric layer. The thickness of the dielectric layer is controlled by the value of the anodizing voltage. For example, the power supply can first be set in constant current mode until the required voltage is reached. The power supply can then be switched to potentiostatic mode to ensure that the desired dielectric thickness is formed over the entire surface of the anode. Of course, other known methods such as pulse or step potentiostatic methods can also be used. The voltage at which the anodizing is performed is typically in the range of about 4 to about 250 V, in some embodiments about 9 to about 200 V, and in some embodiments about 20 to about 150 V. During oxidation, the anodizing solution can be maintained at an elevated temperature, for example, at about 30° C. or higher, in some embodiments about 40° C. to about 200° C., and in some embodiments about 50° C. to about 100° C. Anodizing can also be performed at or below ambient temperature. The resulting dielectric layer can be formed on the surface of the anode and within its pores.
[0024] Although not required, in some embodiments, the dielectric layer can have a differentiated thickness throughout the anode in that it has a first portion disposed on the outer surface of the anode and a second portion disposed on the inner surface of the anode. In such embodiments, the first portion is selectively formed such that its thickness is greater than the thickness of the second portion. However, it should be understood that the thickness of the dielectric layer need not be uniform within a particular region. Some portions of the dielectric layer adjacent to the outer surface, for example, may actually be thinner than some portions of the layer at the inner surface, and vice versa. Nevertheless, the dielectric layer can be formed such that at least a portion of the layer at the outer surface has a greater thickness than at least a portion at the inner surface. While the actual difference in these thicknesses can vary depending on the particular application, the ratio of the thickness of the first portion to the thickness of the second portion is typically about 1.2 to about 40, in some embodiments about 1.5 to about 25, and in some embodiments about 2 to about 20.
[0025] To form dielectric layers having differentiated thicknesses, a multi-step process is typically used. In each step of the process, a sintered anode is anodized to form a dielectric layer (e.g., tantalum pentoxide). During the first step of anodization, a relatively small formation voltage is typically used to ensure that the desired dielectric thickness is achieved for the interior region, for example, a formation voltage in the range of about 1 to about 90 volts, in some embodiments about 2 to about 50 volts, and in some embodiments about 5 to about 20 volts. The sintered body can then be anodized in a second step of the process to increase the dielectric thickness to the desired level. This is typically accomplished by anodizing in an electrolyte at a formation voltage higher than that used during the first step, for example, a formation voltage in the range of about 50 to about 350 volts, in some embodiments about 60 to about 300 volts, and in some embodiments about 70 to about 200 volts. During the first and / or second stages, the electrolyte may be maintained at a temperature within the range of from about 15°C to about 95°C, in some embodiments from about 20°C to about 90°C, and in some embodiments, from about 25°C to about 85°C.
[0026] The electrolyte used during the first and second stages of the anodization process may be the same or different. However, it is usually desirable to use different solutions to help better facilitate achieving a greater thickness at the outer portion of the dielectric layer. For example, it may be desirable for the electrolyte used in the second stage to have a lower ionic conductivity than the electrolyte used in the first stage to prevent a significant amount of oxide film from forming on the inner surface of the anode. In this regard, the electrolyte used during the first stage may include an acidic compound such as hydrochloric acid, nitric acid, sulfuric acid, phosphoric acid, polyphosphoric acid, boric acid, boronic acid, and the like. Such electrolytes may have a conductivity of about 0.1 to about 100 mS / cm, in some embodiments about 0.2 to about 20 mS / cm, and in some embodiments about 1 to about 10 mS / cm, measured at a temperature of 25° C. The electrolyte used during the second stage may typically include a salt of a weak acid such that the hydronium ion concentration increases in the pores as a result of charge passage therethrough. Ion transport or diffusion occurs such that anions of the weak acid migrate into the pores as needed to balance the charge. As a result, the concentration of the main conductive species (hydronium ions) decreases as an equilibrium is formed between hydronium ions, acid anions, and undissociated acid, forming poorly conductive species. The decrease in the concentration of the conductive species results in a relatively high voltage drop in the electrolyte, which prevents further anodization in the interior, while a thicker oxide layer builds up on the exterior for high formation voltages in the successive high conductivity regions. Suitable weak acid salts include, for example, ammonium or alkali metal salts (e.g., sodium, potassium, etc.) of boric acid, boronic acid, acetic acid, oxalic acid, lactic acid, adipic acid, and the like. Particularly suitable salts include sodium tetraborate and ammonium pentaborate. Such electrolytes typically have a conductivity of about 0.1 to about 20 mS / cm, in some embodiments about 0.5 to about 10 mS / cm, and in some embodiments about 1 to about 5 mS / cm, measured at a temperature of 25°C.
[0027] If desired, each step of anodization can be repeated for one or more cycles to achieve the desired dielectric thickness. Additionally, the anode can be rinsed or washed with other solvents (e.g., water) after the first and / or second steps to remove the electrolyte.
[0028] C. Precoat layer: Optionally, but by no means required, a precoat layer containing an organometallic compound can be disposed over the dielectric film. The organometallic compound has the general formula:
[0029] [ka] (In the formula, M is an organometallic atom such as silicon, titanium, etc.; R1, R2, and R3 are independently alkyl (e.g., methyl, ethyl, propyl, etc.), or hydroxyalkyl (e.g., hydroxymethyl, hydroxyethyl, hydroxypropyl, etc.), and at least one of R1, R2, and R3 is hydroxyalkyl; n is an integer from 0 to 8, in some embodiments from 1 to 6, and in some embodiments from 2 to 4 (e.g., 3); and X is an organic or inorganic functional group such as glycidyl, glycidyloxy, mercapto, amino, vinyl, etc. may have:
[0030] In some embodiments, R1, R2, and R3 may be hydroxyalkyl (e.g., OCH3), however, in other embodiments, R1 may be alkyl (e.g., CH3) and R2 and R3 may be hydroxyalkyl (e.g., OCH3).
[0031] Additionally, in some embodiments, M may be silicon and the organometallic compound is an organosilane compound such as an alkoxysilane. Suitable alkoxysilanes include, for example, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, glycidoxymethyltrimethy ... oxysilane, glycidoxymethyltriethoxysilane, glycidoxymethyltripropoxysilane, glycidoxymethyltributoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, β-glycidoxyethyltripropoxysilane, β-glycidoxyethyltributoxysilane, β-glycidoxyethyltrimethoxysilane, α-glycidoxyethyltriethoxysilane, α-glycidoxyethyltripropoxysilane, α-glycidoxyethyltributoxy Silane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyltripropoxysilane, γ-glycidoxypropyltributoxysilane, β-glycidoxypropyltrimethoxysilane, β-glycidoxypropyltriethoxysilane, β-glycidoxypropyltripropoxysilane, α-glycidoxypropyltributoxysilane, α-glycidoxypropyltrimethoxysilane, α-glycidoxypropyltriethoxysilane, α-glycidoxypropyltriethoxysilane glycidoxypropyl tripropoxysilane, α-glycidoxypropyl tributoxysilane, γ-glycidoxybutyl trimethoxysilane, δ-glycidoxybutyl triethoxysilane, δ-glycidoxybutyl tripropoxysilane, δ-glycidoxybutyl tributoxysilane, δ-glycidoxybutyl trimethoxysilane, γ-glycidoxybutyl triethoxysilane, γ-glycidoxybutyl tripropoxysilane, γ-propoxybutyl tributoxysilane, δ-glycidoxybutyl trimethoxysilane,δ-glycidoxybutyltriethoxysilane, δ-glycidoxybutyltripropoxysilane, α-glycidoxybutyltrimethoxysilane, α-glycidoxybutyltriethoxysilane, α-glycidoxybutyltripropoxysilane, α-glycidoxybutyltributoxysilane, (3,4-epoxycyclohexyl)-methyltrimethoxysilane, (3,4-epoxycyclohexyl)methyltriethoxysilane, (3,4-epoxycyclohexyl)methyltripropoxysilane, (3,4-epoxycyclohexyl)methyltributoxysilane, (3,4-epoxycyclohexyl)ethyltrimethoxysilane, (3,4-epoxycyclohexyl)ethyltriethoxysilane, (3,4 -epoxycyclohexyl)ethyl tripropoxysilane, (3,4-epoxycyclohexyl)ethyl tributoxysilane, (3,4-epoxycyclohexyl)propyl trimethoxysilane, (3,4-epoxycyclohexyl)propyl triethoxysilane, (3,4-epoxycyclohexyl)propyl tripropoxysilane, (3,4-epoxycyclohexyl)propyl tributoxysilane, (3,4-epoxycyclohexyl)butyl trimethoxysilane, (3,4-epoxycyclohexyl)butyl triethoxysilane, (3,4-epoxycyclohexyl)butyl tripropoxysilane, (3,4-epoxycyclohexyl)butyl tributoxysilane, and the like can be mentioned.
[0032] The particular method of applying the precoat layer to the capacitor body can vary as desired. In one particular embodiment, the compound is dissolved in an organic solvent and applied to the component as a solution by screen printing, dipping, electrophoretic coating, spraying, or the like. The organic solvent can vary, but is typically an alcohol, such as methanol, ethanol, and the like. The organometallic compound can comprise from about 0.1% to about 10% by weight of the solution, in some embodiments from about 0.2% to about 8% by weight, and in some embodiments from about 0.5% to about 5% by weight. Additionally, the solvent can comprise from about 90% to about 99.9% by weight, in some embodiments from about 92% to about 99.8% by weight, and in some embodiments from about 95% to about 99.5% by weight of the solution. Once applied, the component can then be dried to remove the solvent therefrom to form a precoat layer including the organometallic compound.
[0033] D. Solid electrolyte As indicated above, the solid electrolyte is disposed over the dielectric and the optional precoat layer and generally functions as the cathode for the capacitor. The solid electrolyte includes at least one layer including a conductive polymer and is disposed over the dielectric and the optional precoat layer. The conductive polymer is typically π-conjugated and has a conductivity, such as a conductivity of at least about 1 μS / cm after oxidation or reduction. Examples of such π-conjugated conductive polymers include, for example, polyheterocycles (e.g., polypyrroles, polythiophenes, polyanilines, etc.), polyacetylenes, poly-p-phenylenes, polyphenolates, etc. For example, in one embodiment, the polymer has the following general formula (I):
[0034] [ka] (In the formula, T is O or S; D is an optionally substituted C1-C5 alkylene group (e.g., methylene, ethylene, n-propylene, n-butylene, n-pentylene, etc.); R7 is a linear or branched C1-C 18Alkyl groups (e.g., methyl, ethyl, n- or isopropyl, n-, iso-, sec-, or tert-butyl, n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1-ethylpropyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 2,2-dimethylpropyl, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, etc.); C5 to C 12 Cycloalkyl groups (e.g., cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, etc.); C6-C 14 Aryl groups (e.g., phenyl, naphthyl, etc.); C7-C 18 aralkyl groups (e.g., benzyl, o-, m-, p-tolyl, 2,3-, 2,4-, 2,5-, 2,6-, 3,4-, 3,5-xylyl, mesityl, etc.); q is an integer of 0 to 8, in some embodiments 0 to 2, and in one embodiment 0. It is a substituted polythiophene having a repeat unit of:
[0035] Examples of substituents for the group "D" or "R7" include, for example, alkyl, cycloalkyl, aryl, aralkyl, alkoxy, halogen, ether, thioether, disulfide, sulfoxide, sulfone, sulfonate, amino, aldehyde, keto, carboxylic acid ester, carboxylic acid, carbonate, carboxylate, cyano, alkylsilane and alkoxysilane groups, carboxylamide groups, and the like.
[0036] Particularly suitable thiophene polymers are those in which "D" is an optionally substituted C2-C3 alkylene group. For example, the polymer may have the following general formula (II):
[0037] [ka] The compound may be an optionally substituted poly(3,4-ethylenedioxythiophene) having the repeat unit:
[0038] In one particular embodiment, "q" is 0. One commercially suitable example of 3,4-ethylenedioxythiophene is available from Heraeus under the name Clevios® M. Other suitable monomers are also described in U.S. Patents 5,111,327 to Blohm et al. and 6,635,729 to Groenendaal et al. Derivatives of these monomers can also be used, for example dimers or trimers of the above monomers. Higher molecular weight derivatives of the monomers, i.e. tetramers, pentamers, etc., are suitable for use in the present invention. The derivatives can be composed of the same or different monomer units and can be used in pure form as well as in mixtures with each other and / or with the monomers. Oxidized or reduced forms of these precursors can also be used.
[0039] A variety of techniques can be used to introduce conductive polymers into the solid electrolyte. For example, in one embodiment, the polymer can be formed in situ on the dielectric. In such an embodiment, a precursor monomer, such as those referenced above, is polymerized (e.g., chemically polymerized) in the presence of an oxidation catalyst. The oxidation catalyst typically includes a transition metal cation, such as iron (III), copper (II), chromium (VI), cerium (IV), manganese (IV), manganese (VII), or ruthenium (III) cation. Dopants can also be used to provide an excess of charge to the conductive polymer and stabilize the conductivity of the polymer. Dopants typically include inorganic or organic anions, such as ions of sulfonic acid (e.g., p-toluenesulfonate). In some embodiments, the oxidation catalyst has both catalytic and doping functionality in that it includes a cation (e.g., a transition metal) and an anion (e.g., a sulfonic acid). For example, the oxidation catalyst may be a transition metal salt containing an iron(III) cation, such as an iron(III) halide (e.g., FeCl3), or other iron(III) salts of inorganic acids, such as Fe(ClO4)3 or Fe2(SO4)3, as well as organic acids and iron(III) salts of inorganic acids containing organic groups. Examples of iron(III) salts of inorganic acids with organic groups include, for example, C1-C 20 Examples of iron(III) salts of sulfate monoesters of alkanols (e.g., iron(III) salt of lauryl sulfate) are also included. Examples of iron(III) salts of organic acids include, for example, C1-C 20 Iron(III) salts of alkanesulfonic acids (e.g., methane, ethane, propane, butane, or dodecanesulfonic acid); Iron(III) salts of aliphatic perfluorosulfonic acids (e.g., trifluoromethanesulfonic acid, perfluorobutanesulfonic acid, or perfluorooctanesulfonic acid); Aliphatic C1-C 20 Iron(III) salts of carboxylic acids (e.g. 2-ethylhexyl carboxylic acid); Iron(III) salts of aliphatic perfluorocarboxylic acids (e.g. trifluoroacetic acid or perfluorooctanoic acid); optionally C1-C 20Iron(III) salts of aromatic sulfonic acids substituted with alkyl groups (e.g., benzenesulfonic acid, o-toluenesulfonic acid, p-toluenesulfonic acid, or dodecylbenzenesulfonic acid); iron(III) salts of cycloalkanesulfonic acids (e.g., camphorsulfonic acid); and the like. Mixtures of these aforementioned iron(III) salts can also be used. Iron(III)-p-toluenesulfonate, iron(III)-o-toluenesulfonate, and mixtures thereof are particularly suitable for use in the present invention. One commercially suitable example of iron(III)-p-toluenesulfonate is available under the name Clevios® C from Heraeus.
[0040] The oxidation catalyst and precursor monomer can be applied either sequentially or together to initiate the polymerization reaction. As an example, the monomer can first be mixed with the oxidation catalyst to form a precursor solution. In some embodiments, less than the stoichiometric amount of oxidation catalyst normally required can be used to help retard the polymerization of the monomer, producing shorter oligomers than would be produced if the polymer were fully polymerized, allowing for better penetration into the high specific charge powder. For example, when the monomer comprises a thiophene monomer (e.g., 3,4-ethylenedioxythiophene), the normally required molar ratio used to polymerize the monomer is about 1 mole of monomer to 18 moles of oxidation catalyst. However, less than 18 moles, e.g., less than 15 moles, in some embodiments about 4 to about 12 moles, in some embodiments about 5 to about 10 moles of oxidation polymerization catalyst per mole of monomer (e.g., 3,4-ethylenedioxythiophene) can be present in the polymerization solution.
[0041] In addition to monomers, oxidation catalyst, and optional dopants, the polymerization solution may also contain other components, such as one or more solvents. Particularly suitable solvents include, for example, water, alcohols (e.g., methanol, ethanol, n-propanol, isopropanol, and butanol); glycols (e.g., propylene glycol, butylene glycol, triethylene glycol, hexylene glycol, polyethylene glycol, ethoxydiglycol, and dipropylene glycol); glycol ethers (e.g., methyl glycol ether, ethyl glycol ether, and isopropyl glycol ether); ethers (e.g., diethyl ether and tetrahydrofuran); triglycerides; ketones; esters (e.g., ethyl acetate, butyl acetate, diethylene glycol ether acetate, and methoxypropyl acetate); amides (e.g., dimethylformamide, dimethylacetamide, dimethylcapryl / capric fatty acid amide, and N-alkylpyrrolidone); nitriles (e.g., acetonitrile, propionitrile, butyronitrile, and benzonitrile), sulfoxides or sulfones (e.g., dimethylsulfoxide (DMSO) and sulfolane), and the like, as well as mixtures of any of the above (e.g., water and alcohols).
[0042] The polymerization solution is typically maintained at a relatively low temperature during the reaction, such as from about -20°C to about 50°C, in some embodiments from about -15°C to about 30°C, and in some embodiments from about -10°C to about 10°C. The solution can be applied to the anode body using any suitable application technique known in the art, such as screen printing, dipping, electrophoretic coating, and spraying. Regardless of the application technique used, the monomers generally begin to react to form a polymer layer when present on the anode body. The time for which the monomers are allowed to react on the anode body is typically long enough to allow good impregnation of the polymer into the small pores of the high specific charge powder. For example, in most embodiments, this time (impregnation time) is about 1 minute or more, in some embodiments about 1.5 minutes or more, and in some embodiments about 2 to about 5 minutes. After the reaction, the resulting conductive polymer layer or layers can be contacted with a washing solution to remove various by-products, excess catalyst, and the like. The time that the cleaning solution is placed in contact with the conductive polymer layer or layers (cleaning time) is typically long enough to ensure that by-products, excess catalyst, etc. can be adequately removed from the small pores of the high specific charge powder. The cleaning time may be, for example, about 25 minutes or more, in some embodiments about 30 minutes or more, and in some embodiments about 45 minutes to about 90 minutes. During this time, cleaning can be performed in a single step or in multiple steps, with the total time of each step being within the above ranges. The cleaning solution can vary as desired, but typically is one or more solvents (e.g., water, alcohol, etc.) and, optionally, a dopant, as described above.
[0043] Once washed, the conductive polymer layer(s) can be dried, typically at a temperature of about 15° C. or higher, in some embodiments about 20° C. or higher, and in some embodiments from about 20° C. to about 80° C. The polymer layer(s) can also be healed after formation. Healing can be performed after each application of a conductive polymer layer, or after application of the entire conductive polymer coating. In some embodiments, the anode body can be healed by immersing it in an electrolyte solution and then applying a constant voltage to the solution until the current drops to a preselected level. If desired, such healing can be accomplished in multiple steps. For example, the electrolyte solution can be a dilute solution of monomer, catalyst, and dopant in an alcoholic solvent (e.g., ethanol).
[0044] In addition to in situ polymerization, the conductive polymers can also be applied in the form of pre-polymerized intrinsically and / or extrinsically conductive polymer particles. One advantage of using such particles is that they prevent the formation of ionic species (e.g., Fe) that can cause dielectric breakdown under high electric fields due to ionic migration, which are generated during conventional in situ polymerization processes. 2+ or Fe 3+ ) can be minimized. Thus, by applying the conductive polymer as prepolymerized particles rather than by in-situ polymerization, the resulting capacitor can exhibit a relatively high "breakdown voltage."
[0045] For example, in some embodiments, an "extrinsic" conductive polymer having repeat units of formula (I) or (II) above can be used in the solid electrolyte. Such polymers are generally considered to be "extrinsic" conductive in that they typically require the presence of another counterion that is not covalently bonded to the polymer. The counterion can be a monomeric or polymeric anion that neutralizes the charge of the conductive polymer. The polymeric anion can be, for example, a polymeric carboxylic acid (e.g., polyacrylic acid, polymethacrylic acid, polymaleic acid, etc.); a polymeric sulfonic acid (e.g., polystyrene sulfonic acid (PSS), polyvinyl sulfonic acid, etc.); and the like. The acid can also be a copolymer, such as a copolymer of vinyl carboxylic acid and vinyl sulfonic acid with other polymerizable monomers, such as acrylic acid esters and styrene. Additionally, suitable monomeric anions include, for example, C1-C 20 Alkanesulfonic acids (e.g., dodecanesulfonic acid); aliphatic perfluorosulfonic acids (e.g., trifluoromethanesulfonic acid, perfluorobutanesulfonic acid, or perfluorooctanesulfonic acid); aliphatic C1-C 20 Carboxylic acids (e.g. 2-ethylhexyl carboxylic acid); aliphatic perfluorocarboxylic acids (e.g. trifluoroacetic acid or perfluorooctanoic acid); optionally C1-C 20 Examples of the counter anion include an aromatic sulfonic acid substituted with an alkyl group (e.g., benzenesulfonic acid, o-toluenesulfonic acid, p-toluenesulfonic acid, or dodecylbenzenesulfonic acid); a cycloalkanesulfonic acid (e.g., camphorsulfonic acid, or tetrafluoroborate, hexafluorophosphate, perchlorate, hexafluoroantimonate, hexafluoroarsenate, or hexachloroantimonate); and the like. Particularly suitable counter anions are polymeric anions such as polymeric carboxylic or sulfonic acids (e.g., polystyrene sulfonic acid (PSS)). The molecular weight of such polymeric anions is usually in the range of about 1,000 to about 2,000,000, and in some embodiments, about 2,000 to about 500,000.
[0046] Also, inherently conductive polymers can be used that have positive charges disposed on the backbone that are at least partially compensated by anions covalently attached to the polymer. For example, one example of a suitable inherently conductive polymer has the following formula (III):
[0047] [ka] (In the formula, R is (CH2) a -O-(CH2) b and; a is 0 to 10, in some embodiments 0 to 6, and in some embodiments 1 to 4 (e.g., 1); b is 1 to 18, in some embodiments 1 to 10, and in some embodiments 2 to 6 (e.g., 2, 3, 4, or 5); Z is SO3 - , C(O)O - , BF4 - , CF3SO3 - , SbF6 - , N(SO2CF3)2 - , C4H3O4 - , ClO4 - etc., anions such as; X is a cation such as hydrogen, an alkali metal (e.g., lithium, sodium, rubidium, cesium, or potassium), ammonium, etc. It may have the repeat unit:
[0048] In one particular embodiment, Z in formula (I) is a sulfonate ion and the intrinsically conductive polymer has the following formula (IV):
[0049] [ka] (wherein R and X are as defined above). In formula (III) or (IV), a is preferably 1, and b is preferably 3 or 4. Furthermore, X is preferably sodium or potassium.
[0050] If desired, the polymer may be a copolymer containing other types of repeat units. In such embodiments, the repeat units of formula (III) typically constitute at least about 50 mol %, in some embodiments from about 75 mol % to about 99 mol %, and in some embodiments from about 85 mol % to about 95 mol % of the total amount of repeat units in the copolymer. Of course, the polymer may be a homopolymer in that it contains 100 mol % of the repeat units of formula (III). Specific examples of such homopolymers include poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-ylmethoxy)-1-butanesulfonic acid, salt) and poly(4-(2,3-dihydrothieno-[3,4-b][1,4]dioxin-2-ylmethoxy)-1-propanesulfonic acid, salt).
[0051] Regardless of the particular nature of the polymer, the conductive polymer particles typically have an average size (e.g., diameter) of about 1 to about 80 nanometers, in some embodiments about 2 to about 70 nanometers, and in some embodiments about 3 to about 60 nanometers. The diameter of the particles can be determined using known techniques such as ultracentrifugation, laser diffraction, and the like. Additionally, the shape of the particles can vary. For example, in one particular embodiment, the particles are spherical in shape. However, it should be understood that other shapes, such as plates, rods, disks, bars, tubes, irregular shapes, and the like, are also contemplated by the present invention.
[0052] Although not required, the conductive polymer particles can be applied in the form of a dispersion. The concentration of the conductive polymer in the dispersion can vary depending on the desired viscosity of the dispersion and the particular method of applying the dispersion to the capacitor element. Typically, however, the polymer comprises from about 0.1 to about 10 weight percent of the dispersion, in some embodiments from about 0.4 to about 5 weight percent, and in some embodiments, from about 0.5 to about 4 weight percent. The dispersion can also include one or more components to improve the overall properties of the resulting solid electrolyte. For example, the dispersion can include a binder to further enhance the adhesion of the polymer layer and also to increase the stability of the particles in the dispersion. The binder may be of organic nature, such as polyvinyl alcohol, polyvinylpyrrolidone, polyvinyl chloride, polyvinyl acetate, polyvinyl butyrate, polyacrylic esters, polyacrylic amides, polymethacrylic esters, polymethacrylic amides, polyacrylonitrile, styrene / acrylic esters, vinyl acetate / acrylic esters and ethylene / vinyl acetate copolymers, polybutadiene, polyisoprene, polystyrene, polyethers, polyesters, polycarbonates, polyurethanes, polyamides, polyimides, polysulfones, melamine formaldehyde resins, epoxide resins, silicone resins or cellulose. Crosslinking agents may also be used to increase the adhesive capacity of the binder. Such crosslinking agents may include, for example, melamine compounds, masked isocyanates or crosslinkable polymers such as polyurethanes, polyacrylates or polyolefins, which may include subsequent crosslinking. Dispersing agents may also be used to facilitate the ability to apply the layer to the anode.Suitable dispersants include solvents such as aliphatic alcohols (e.g., methanol, ethanol, i-propanol, and butanol), aliphatic ketones (e.g., acetone and methyl ethyl ketone), aliphatic carboxylic acid esters (e.g., ethyl acetate and butyl acetate), aromatic hydrocarbons (e.g., toluene and xylene), aliphatic hydrocarbons (e.g., hexane, heptane, and cyclohexane), chlorinated hydrocarbons (e.g., dichloromethane and dichloroethane), aliphatic nitriles (e.g., acetonitrile), aliphatic sulfoxides and sulfones (e.g., dimethyl sulfoxide and sulfolane), aliphatic carboxylic acid amides (e.g., methylacetamide, dimethylacetamide, and dimethylformamide), aliphatic and aromatic aliphatic ethers (e.g., diethyl ether and anisole), water, and any mixture of the above solvents.A particularly suitable dispersant is water.
[0053] In addition to those mentioned above, further components can be used in the dispersion. For example, conventional fillers having dimensions of about 10 nanometers to about 100 micrometers, in some embodiments about 50 nanometers to about 50 micrometers, in some embodiments about 100 nanometers to about 30 micrometers can be used. Examples of such fillers include calcium carbonate, silicates, silica, calcium or barium sulfate, aluminum hydroxide, glass fibers or glass spheres, wood flour, cellulose powder, carbon black, conductive polymers, and the like. The fillers can be introduced into the dispersion in powder form, but can also be present in other forms, such as fibers.
[0054] Surface active substances such as ionic or non-ionic surfactants can also be used in the dispersion. In addition, adhesives such as organofunctional silanes or their hydrolysates, for example, 3-glycidoxypropyltrialkoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane or octyltriethoxysilane can be used. The dispersion can also contain ether group-containing compounds (e.g., tetrahydrofuran), lactone group-containing compounds (e.g., γ-butyrolactone or γ-valerolactone), amide or lactam group-containing compounds (e.g., caprolactam, N-methylcaprolactam, N,N-dimethylacetamide, N-methylacetamide, N,N-dimethylformamide (DMF), N-methylformamide, N-methylformanilide, N-methylpyrrolidone (NMP), N-octylpyrrolidone, or pyrrolidone), sulfones and Additives that increase conductivity may also be included, such as sulfoxides (e.g., sulfolane (tetramethylene sulfone) or dimethyl sulfoxide (DMSO)), sugars or sugar derivatives (e.g., saccharose, glucose, fructose, or lactose), sugar alcohols (e.g., sorbitol or mannitol), furan derivatives (e.g., 2-furan carboxylic acid or 3-furan carboxylic acid), alcohols (e.g., ethylene glycol, glycerol, di- or triethylene glycol).
[0055] The dispersion can be applied using a variety of known techniques, such as by spin coating, impregnation, pouring, drop application, injection, spraying, doctor blade application, brush application, printing (e.g., inkjet, screen, or pad printing), or immersion. The viscosity of the dispersion is typically from about 0.1 to about 100,000 mPa·s (100 s -1 (measured at a shear rate of about 10,000 mPa·sec in some embodiments, about 10 to about 1,500 mPa·sec in some embodiments, and about 100 to about 1000 mPa·sec in some embodiments.
[0056] As mentioned above, depolarizers are also used in solid electrolytes in combination with conductive polymers. The depolarizers can be introduced into the solid electrolyte in a variety of different ways. For example, in some embodiments, the depolarizer can simply be applied in combination with the conductive polymer, such as in a solution containing the precursor monomer, the oxidation catalyst, or a mixture thereof, or in a dispersion containing conductive polymer particles. However, in other embodiments, the depolarizer can be applied after one or more layers of conductive polymer have been formed. In such embodiments, the technique used to apply the depolarizer can vary. For example, the depolarizer can be applied in the form of a liquid solution using various methods such as immersion, dipping, pouring, dripping, injecting, spraying, spreading, painting, or printing, such as inkjet or screen printing. Solvents known to those skilled in the art, such as water, alcohols (e.g., methanol, ethanol, n-propanol, iso-propanol, and butanol); glycols (e.g., propylene glycol, butylene glycol, triethylene glycol, hexylene glycol, polyethylene glycol, ethoxydiglycol, and dipropylene glycol); glycol ethers (e.g., methyl glycol ether, ethyl glycol ether, and isopropyl glycol ether); ethers (e.g., diethyl ether and tetrahydrofuran); triglycerides; ketones; esters (e.g., ethyl acetate, butyl acetate, diethylene glycol ether acetate, and methoxypropyl acetate); amides (e.g., dimethylformamide, dimethylacetamide, dimethylcapryl / capric fatty acid amide, and N-alkylpyrrolidone); nitriles (e.g., acetonitrile, propionitrile, butyronitrile, and benzonitrile); sulfoxides or sulfones (e.g., dimethylsulfoxide (DMSO) and sulfolane), and the like, as well as mixtures of these (e.g., water and alcohols) can be used in the solution. The concentration of the depolarizer in such solutions typically ranges from about 0.1% to about 50% by weight of the solution, in some embodiments from about 0.5% to about 30% by weight, and in some embodiments, from about 1% to about 20% by weight. If desired, such solutions may be generally free of conductive polymers.For example, the conductive polymer may comprise about 2% by weight or less of the solution, in some embodiments, about 1% by weight or less, and in some embodiments, about 0.5% by weight or less.
[0057] E. Cathode Coating: If desired, a cathode coating may also be used that is disposed over the solid electrolyte and other optional layers. The cathode coating may include a metal particle layer that includes a multiplicity of conductive metal particles dispersed within a polymer matrix. The particles typically comprise from about 50% to about 99% by weight of the layer, in some embodiments from about 60% to about 98% by weight, and in some embodiments from about 70% to about 95% by weight, while the polymer matrix typically comprises from about 1% to about 50% by weight, in some embodiments from about 2% to about 40% by weight, and in some embodiments from about 5% to about 30% by weight of the layer.
[0058] The conductive metal particles can be formed from a variety of different metals, such as copper, nickel, silver, nickel, zinc, tin, lead, copper, aluminum, molybdenum, titanium, iron, zirconium, magnesium, and the like, as well as alloys thereof. Silver is a particularly suitable conductive metal for use in such layers. The metal particles often have relatively small dimensions, such as an average diameter of about 0.01 to about 50 micrometers, in some embodiments about 0.1 to about 40 micrometers, and in some embodiments about 1 to about 30 micrometers. It should be understood that, although typically only one layer of metal particles is used, multiple layers can be used if desired. The total thickness of such one or more layers is in the range of about 1 μm to about 500 μm, in some embodiments about 5 μm to about 200 μm, and in some embodiments about 10 μm to about 100 μm.
[0059] The polymer matrix typically comprises a polymer which may be thermoplastic or thermosetting in nature. However, the polymer is typically selected to contain a relatively small amount of polar groups which can act as a barrier to electromigration of silver ions and also minimize the degree of water adsorption in the cathode coating. In this regard, vinyl acetal polymers such as polyvinyl butyral, polyvinyl formal, and the like, may be particularly suitable for this purpose. For example, polyvinyl butyral may be formed by reacting polyvinyl alcohol with an aldehyde (e.g., butyraldehyde). Because this reaction is usually not complete, polyvinyl butyral will generally have a residual hydroxyl content. However, by minimizing this content, the polymer may have a lower degree of strongly polar groups which would otherwise cause a high degree of moisture adsorption and migration of silver ions. For example, the residual hydroxyl content in polyvinyl acetal may be about 35 mol % or less, in some embodiments about 30 mol % or less, and in some embodiments, about 10 mol % to about 25 mol %. One commercially available example of such a polymer is available from Sekisui Chemical Co., Ltd. under the designation "BH-S" (polyvinyl butyral).
[0060] To form the cathode coating, a conductive paste is typically applied to the capacitor over the solid electrolyte. One or more organic solvents are typically used in the paste. In general, a variety of different organic solvents can be used, such as glycols (e.g., propylene glycol, butylene glycol, triethylene glycol, hexylene glycol, polyethylene glycol, ethoxydiglycol, and dipropylene glycol); glycol ethers (e.g., methyl glycol ether, ethyl glycol ether, and isopropyl glycol ether); ethers (e.g., diethyl ether and tetrahydrofuran); alcohols (e.g., benzyl alcohol, methanol, ethanol, n-propanol, iso-propanol, and butanol); triglycerides; ketones (e.g., acetone, methyl ethyl ketone, and methyl isobutyl ketone); esters (e.g., ethyl acetate, butyl acetate, diethylene glycol ether acetate, and methoxypropyl acetate); amides (e.g., dimethylformamide, dimethylacetamide, dimethylcapryl / capric fatty acid amide, and N-alkylpyrrolidones); nitriles (e.g., acetonitrile, propiononitrile, butyronitrile, and benzonitrile); sulfoxides or sulfones (e.g., dimethylsulfoxide (DMSO) and sulfolane); and the like, as well as mixtures thereof. The organic solvent or solvents typically comprise about 10% to about 70% by weight of the paste, in some embodiments about 20% to about 65% by weight, and in some embodiments about 30% to about 60% by weight. The metal particles typically comprise about 10% to about 60% by weight of the paste, in some embodiments about 20% to about 45% by weight, and in some embodiments about 25% to about 40% by weight, and the resinous matrix typically comprises about 0.1% to about 20% by weight of the paste, in some embodiments about 0.2% to about 10% by weight, and in some embodiments about 0.5% to about 8% by weight.
[0061] The paste may have a relatively low viscosity, which allows it to be easily handled and applied to the capacitor element. The viscosity may range from about 50 to about 3,000 centipoise, in some embodiments from 100 to about 2,000 centipoise, and in some embodiments from about 200 to about 1,000 centipoise, as measured, for example, using a Brookfield DV-1 viscometer (cone plate) or the like, operating at a speed of 10 rpm and a temperature of 25° C. If desired, thickeners or other viscosity modifiers can be used in the paste to increase or decrease the viscosity. Additionally, the paste may be applied at a relatively thin thickness and still achieve the desired properties. For example, the paste may have a thickness of about 0.01 to about 50 micrometers, in some embodiments from about 0.5 to about 30 micrometers, and in some embodiments from about 1 to about 25 micrometers. Once applied, the metal paste may be optionally dried to remove some components, such as the organic solvent. For example, drying can be carried out at a temperature of about 20°C to about 150°C, in some embodiments, about 50°C to about 140°C, and in some embodiments, about 80°C to about 130°C.
[0062] F. Other Components: If desired, other layers known in the art may also be included in the capacitor. For example, in some embodiments, a carbon layer (e.g., graphite) may be disposed between the solid electrolyte and the silver layer to help further limit contact between the silver layer and the solid electrolyte. Additionally, a precoat layer disposed over the dielectric and including an organometallic compound, as described in more detail below, may also be used.
[0063] II. Termination: Once the layers of the capacitor element are formed, the resulting capacitor can be provided with terminations. For example, the capacitor can include an anode termination to which the anode lead of the capacitor element is electrically connected, and a cathode termination to which the cathode of the capacitor is electrically connected. Any conductive material can be used to form the terminations, such as conductive metals (e.g., copper, nickel, silver, nickel, zinc, tin, palladium, lead, copper, aluminum, molybdenum, titanium, iron, zirconium, magnesium, and alloys thereof). Particularly suitable conductive metals include, for example, copper, copper alloys (e.g., copper-zirconium, copper-magnesium, copper-zinc, or copper-iron), nickel, and nickel alloys (e.g., nickel-iron). The thickness of the terminations is generally selected to minimize the thickness of the capacitor. For example, the thickness of the terminations can range from about 0.05 to about 1 millimeter, in some embodiments, from about 0.05 to about 0.5 millimeters, and from about 0.07 to about 0.2 millimeters. One exemplary conductive material is a metal plate of copper-iron alloy available from Wieland (Germany). If desired, the surfaces of the terminations can be electroplated with nickel, silver, gold, tin, etc., as known in the art, to ensure that the final component can be mounted to a circuit board. In one particular embodiment, both surfaces of the terminations are plated with nickel and silver flash, respectively, while the mounting surface is also plated with a tin solder layer.
[0064] The terminations may be connected to the capacitor elements using any technique known in the art. For example, in one embodiment, a lead frame may be provided that defines a cathode termination and an anode termination. To attach the electrolytic capacitor elements to the lead frame, a conductive adhesive may first be applied to the surface of the cathode termination. The conductive adhesive may include, for example, conductive metal particles contained in a resin composition. The metal particles may be silver, copper, gold, platinum, nickel, zinc, bismuth, etc. The resin composition may include a thermosetting resin (e.g., an epoxy resin), a hardener (e.g., an acid anhydride), and a compound (e.g., a silane compound). Suitable conductive adhesives are described in U.S. Patent Application Publication No. 2006 / 0038304 to Osako et al. The conductive adhesive may be applied to the cathode termination using any of a variety of techniques. For example, printing techniques may be used for their practical and cost-saving benefits. The anode lead may also be electrically connected to the anode termination using any technique known in the art, such as mechanical welding, laser welding, conductive adhesives, etc. Once the anode lead has been electrically connected to the anode termination, the conductive adhesive may then be cured to ensure proper adhesion of the electrolytic capacitor element to the cathode termination.
[0065] For example, referring to Figure 1, an electrolytic capacitor 30 is shown as including an anode termination 62 and a cathode termination 72 electrically connected to a capacitor element 33 having a top surface 37, a bottom surface 39, a back surface 38, and a front surface 36. Although not explicitly shown in Figure 1, it should be understood that the configuration of the capacitor may correspond to the configuration of the anode body discussed above. That is, the capacitor element may also include channels in one or more of its exterior surfaces (e.g., top surface 37 and / or bottom surface 39).
[0066] The cathode termination 72 in the illustrated embodiment is in electrical contact with the bottom surface 39 via a conductive adhesive. More specifically, the cathode termination 72 includes a first part 73 in electrical contact with and generally parallel to the bottom surface 39 of the capacitor element 33. The cathode termination 72 may also include a second part 74 that is substantially perpendicular to the first part 73 and in electrical contact with the back surface 38 of the capacitor element 33. The anode termination 62 also includes a first part 63 that is disposed substantially perpendicular to a second part 64. The first part 63 is in electrical contact with and generally parallel to the bottom surface 39 of the capacitor element 33. The second part 64 includes a region 51 that supports the anode lead 16. Although not shown in FIG. 1, the region 51 may have a "U-shape" to further increase the surface contact and mechanical stability of the lead 16.
[0067] The terminations may be connected to the capacitor elements using any technique known in the art. For example, in one embodiment, a lead frame may be provided that defines the cathode termination 72 and the anode termination 62. To attach the electrolytic capacitor element 33 to the lead frame, a conductive adhesive may first be applied to the surface of the cathode termination 72. The conductive adhesive may include, for example, conductive metal particles included with a resin composition. The metal particles may be silver, copper, gold, platinum, nickel, zinc, bismuth, etc. The resin composition may include a thermosetting resin (e.g., an epoxy resin), a hardener (e.g., an acid anhydride), and a coupling agent (e.g., a silane coupling agent). Suitable conductive adhesives are described in U.S. Patent Publication No. 2006 / 0038304 to Osako et al. The conductive adhesive may be applied to the cathode termination 72 using any of a variety of techniques. For example, printing techniques may be used for their implementation and cost-saving benefits.
[0068] In general, the terminations can be attached to the capacitor using a variety of methods. For example, in one embodiment, the second part 64 of the anode termination 62 is first bent upward to the position shown in FIG. 1. The capacitor element 33 is then placed over the cathode termination 72 such that the lower surface 39 of the capacitor element 33 contacts the adhesive and the anode lead 16 is received by the region 51. If desired, an insulating material (not shown), such as a plastic pad or tape, can be placed between the lower surface 39 of the capacitor element 33 and the first part 63 of the anode termination 62 to electrically insulate the anode and cathode terminations. The anode lead 16 is then electrically connected to the region 51 using any technique known in the art, such as mechanical welding, laser welding, conductive adhesives, and the like. For example, the anode lead 16 can be welded to the anode termination 62 using a laser. A laser generally includes a resonator that includes a laser medium capable of emitting photons by stimulated emission, and an energy source that excites the elements of the laser medium. One type of suitable laser is one in which the laser medium consists of aluminum yttrium garnet (YAG) doped with neodymium (Nd). The excited particles are neodymium ions: Nd 3+ The laser medium may be continuously energized by an energy source to emit a continuous laser beam or may be radiated with energy to emit a pulsed laser beam. Once the anode lead 16 is electrically connected to the anode termination 62, the conductive adhesive may then be cured. For example, a heat press may be used to apply heat and pressure to ensure that the adhesive properly bonds the electrolytic capacitor element 33 to the cathode termination 72.
[0069] III. Housing: Due to the ability of the capacitor to exhibit good electrical performance in various environments, it is not necessary for the capacitor element to be hermetically sealed in the housing. Nevertheless, in some embodiments, it may be desirable to hermetically seal the capacitor element in the housing. The capacitor element can be sealed in the housing in a variety of ways. For example, in some embodiments, the capacitor element can be housed in a case, which can then be filled with a resin material, such as a thermosetting resin (e.g., epoxy resin), which can be cured to form a hardened housing. Examples of such resins include, for example, epoxy resins, polyimide resins, melamine resins, urea-formaldehyde resins, polyurethane resins, phenolic resins, polyester resins, and the like. Epoxy resins are also particularly suitable. Still other additives can be used, such as photoinitiators, viscosity modifiers, suspending aids, pigments, stress reducers, non-conductive fillers, stabilizers, and the like. For example, non-conductive fillers can include inorganic oxide particles, such as silica, alumina, zirconia, magnesium oxide, iron oxide, copper oxide, zeolites, silicates, clays (e.g., smectite clays), and the like, and composites (e.g., alumina-coated silica particles), and mixtures thereof. Regardless, the capacitor element can be surrounded and encapsulated with a resin material such that at least a portion of the anode and cathode terminations are exposed for mounting on a circuit board. When encapsulated in this manner, the capacitor element and resin material form an integral capacitor assembly. For example, as shown in FIG. 1, capacitor element 33 is encapsulated within housing 28 such that a portion of anode termination 62 and a portion of cathode termination 72 are exposed.
[0070] Of course, in other embodiments, it may be desirable to house the capacitor elements separately in a housing. In this way, the atmosphere of the housing can be gaseous and include at least one inert gas, such as nitrogen, helium, argon, xenon, neon, krypton, radon, and the like, as well as mixtures thereof. Typically, the inert gas constitutes a majority of the atmosphere within the housing, for example, about 50% to 100% by weight, in some embodiments about 75% to 100% by weight, and in some embodiments about 90% to about 99% by weight of the atmosphere. If desired, relatively small amounts of non-inert gases, such as carbon dioxide, oxygen, water vapor, and the like, can also be used. However, in such cases, the non-inert gas typically constitutes no more than 15% by weight, in some embodiments no more than 10% by weight, in some embodiments no more than about 5% by weight, in some embodiments no more than about 1% by weight, and in some embodiments about 0.01% to about 1% by weight of the atmosphere within the housing. Any of a variety of different materials, such as metals, plastics, ceramics, and the like, can be used to form the separate housing. For example, in one embodiment, the housing includes one or more layers of a metal, such as tantalum, niobium, aluminum, nickel, hafnium, titanium, copper, silver, steel (e.g., stainless steel), alloys thereof (e.g., conductive oxides), composites thereof (e.g., metals coated with conductive oxides), etc. In other embodiments, the housing can include one or more layers of a ceramic material, such as aluminum nitride, aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, glass, etc., as well as combinations thereof. The housing can have any desired shape, such as cylindrical, D-shaped, rectangular, triangular, prismatic, etc. EXAMPLES
[0071] The invention may be better understood with reference to the following examples.
[0072] Test procedure: Equivalent Series Resistance (ESR) The equivalent series resistance can be measured using an HP4284A LCR meter with Kelvin leads, with a DC bias of 0 volts and a signal of 10 mVAC. The operating frequency was 100 kHz and the temperature was 23°C ± 2°C.
[0073] Loss factor The dissipation factor can be measured using an LCZHP4284A LCR meter with Kelvin leads, with 0 volts DC bias and a 10 mVAC signal. The operating frequency can be 120 Hz and the temperature can be 23°C ± 2°C. capacitance Capacitance can be measured using a Keithley 3300 precision LCZ meter with Kelvin leads, using a DC bias of 2.2 volts and a sine wave signal of 0.5 volts peak-to-peak. The operating frequency can be 120 Hz and the temperature can be 23°C ± 2°C.
[0074] Leakage Current The leakage current can be measured using a leakage test meter (YHP4140B) at a temperature of 23°C ± 2°C, using a 1 kilohm resistor to limit the charging current, at the rated voltage after a minimum of 60 seconds.
[0075] Humidity Load Test The humidity test is based on the standard IEC68-2-67:1995 (85°C / relative humidity 85%). 25 test parts (mounted on a printed circuit board) can be subjected to the rated voltage under the humidity test conditions mentioned above. After 2 to 24 hours from the recovery of the humidity test conditions, the capacitance and ESR can be measured at temperatures of 23°C ± 2°C at 0, 500, and 1000 hours.
[0076] High temperature storage test The high temperature storage test is based on IEC 60068-2-2:2007 (condition Bb, temperature 150°C). 25 test components (mounted on a printed circuit board) can be tested at the above temperature conditions. All measurements of capacitance and ESR can be performed at a temperature of 23°C ± 2°C, 1 to 2 hours after recovery of the temperature test conditions.
[0077] Example 1 Anode samples were prepared using 50,000 μFV / g tantalum powder. Each anode sample was embedded with a tantalum wire, sintered at 1350 °C, and pressed to a mass of 5.8 g / cm. 3The resulting pellet had dimensions of 1.7×2.4×1.0 mm. The pellet was anodized to 23.5 volts in a water / phosphoric acid electrolyte with a conductivity of 8.6 mS at a temperature of 85° C. to form a dielectric layer. The pellet was anodized again to 80 volts in a water / boric acid / disodium tetraborate electrolyte with a conductivity of 2.0 mS at a temperature of 30° C. for 25 seconds to form a thicker oxide layer deposited on the outside. The anode was then immersed in a butanol solution of iron(III) toluenesulfonate (Clevios® C, Heraeus) and then in 3,4-ethylenedioxythiophene (Clevios® M, Heraeus) and polymerized to form a conductive polymer coating. After 45 minutes of polymerization, a thin layer of poly(3,4-ethylenedioxythiophene) was formed on the surface of the dielectric. The anode was washed in methanol to remove reaction by-products, anodized in liquid electrolyte, and washed again in methanol. This process was repeated six times. The parts were then immersed in a dispersed poly(3,4-ethylenedioxythiophene) (Clevios® K, Heraeus) with 2.0% solids and a viscosity of 20 mPa·s. Once coated, the parts were dried at 125°C for 20 minutes. This process was repeated three times. The parts were then immersed in a dispersed poly(3,4-ethylenedioxythiophene) (Clevios® K, Heraeus) with 2% solids and a viscosity of 160 mPa·s. Once coated, the parts were dried at 125°C for 20 minutes. This process was repeated twelve times. The parts were then immersed in a graphite dispersion and allowed to dry. The parts were immersed in a silver dispersion and allowed to dry. Finally, the parts were mounted to metal terminations formed from a copper substrate. A large number of components (2,000) of 47 μF / 10 V capacitors were made in this manner and encapsulated in standard silica resin.
[0078] Example 2 The resulting parts were mounted with metal terminations formed from a stainless steel base material, and capacitors were formed as described in Example 1. A large number of parts (1,000) of 47 μF / 10 V capacitors were thus made and encapsulated in standard silica resin.
[0079] Example 3 Once polymerized in situ, the capacitors were formed as described in Example 1, except that the parts were immersed in a 0.3% solution of 2,5-dimethoxybenzoquinone in dimethylsulfoxide. Once coated, the parts were dried at 125° C. for 30 minutes. This process was repeated 10 times. Prior to immersion in the graphite dispersion, the parts were immersed in a 0.3% solution of 2,5-dimethoxybenzoquinone in dimethylsulfoxide. Once coated, the parts were dried at 125° C. for 30 minutes. This process was repeated 5 times. A large number of parts (1,000) of 47 μF / 10 V capacitors were thus made and encapsulated in standard silica resin.
[0080] Example 4 Once polymer coated, capacitors were formed as described in Example 2, except that the parts were immersed in a 0.3% solution of 2,5-dimethoxybenzoquinone in dimethylsulfoxide. Once coated, the parts were dried at 125° C. for 30 minutes. This process was repeated 10 times. A large number of parts (1,000) of 47 μF / 10 V capacitors were thus made and encapsulated in standard silica resin.
[0081] The capacitance and ESR results in the stress humidity test and high temperature storage test are shown in Tables 1 and 2 below.
[0082] [Table 1]
[0083] [Table 2] These and other modifications and variations of the present invention may be implemented by those skilled in the art without departing from the spirit and scope of the present invention. Moreover, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Moreover, those skilled in the art will recognize that the above description is by way of example only and is not intended to limit the invention as further described in the appended claims. The present invention includes the following embodiments. [1] Sintered porous anode body; a dielectric disposed over the anode body; and a solid electrolyte disposed over the dielectric, the solid electrolyte comprising a conductive polymer and a depolarizer; A solid electrolytic capacitor comprising a capacitor element comprising: [2] The solid electrolytic capacitor according to [1], wherein the depolarizer has a standard reduction potential greater than 0. [3] The solid electrolytic capacitor according to [1], wherein the depolarizer is an aromatic quinone, a nitroaromatic compound, or a combination thereof. [4] The solid electrolytic capacitor according to [3], wherein the depolarizer is 1,4-benzoquinone, 2-phenyl-1,4-benzoquinone, 2-methyl-1,4-benzoquinone, 2-tert-butyl-1,4-benzoquinone, 2-methoxy-1,4-benzoquinone, 2,6-dimethyl-1,4-benzoquinone, 2,3-dimethyl-1,4-benzoquinone, trimethyl-1,4-benzoquinone, 2,6-dimethoxy-1,4-benzoquinone, 2,5-methoxy-1,4-benzoquinone, tetramethyl-1,4-benzoquinone, tetrafluoro-1,4-benzoquinone, 2,5-dichloro-1,4-benzoquinone, tetrachloro-1,4-benzoquinone, 2-chloro-1,4-benzoquinone, or a combination thereof. [5] The solid electrolytic capacitor of [1], further comprising an anode termination in electrical contact with the anode body, and a cathode termination in electrical contact with the solid electrolyte. [6] The solid electrolytic capacitor according to [1], further comprising a housing in which the capacitor element is housed. [7] The solid electrolytic capacitor according to [6], wherein the housing is formed from a resin material that encapsulates the capacitor element. [8] The solid electrolytic capacitor according to [1], wherein the anode body contains tantalum. [9] The conductive polymer has the following formula: [ka] (In the formula, R 7 is linear or branched C 1 ~C 18 Alkyl group, C 5 ~C 12 Cycloalkyl groups, C 6 ~C 14 Aryl group, C 7 ~C 18 aralkyl groups, or combinations thereof; q is an integer from 0 to 8. The solid electrolytic capacitor according to [1], having a repeating unit represented by the formula:
[10] The solid electrolytic capacitor according to [9], wherein the conductive polymer is poly(3,4-ethylenedioxythiophene).
[11] The solid electrolytic capacitor according to [1], wherein the conductive polymer is formed by in situ polymerization.
[12] The solid electrolytic capacitor according to [1], wherein the conductive polymer is in the form of particles.
[13] The solid electrolytic capacitor of
[12] , wherein the solid electrolyte also contains a polymeric counterion.
[14] The solid electrolytic capacitor of [1], wherein the capacitor element further comprises a cathode coating including a metal particle layer disposed on the solid electrolyte, the metal particle layer comprising a plurality of conductive metal particles.
[15] The solid electrolytic capacitor of [1], wherein the capacitor exhibits an initial ESR at a temperature of about 23°C and a high-temperature ESR after exposure to a temperature of about 125°C for 1,000 hours, and the ratio of the high-temperature ESR to the initial ESR is less than or equal to about 3.0.
[16] The solid electrolytic capacitor of [1], wherein the capacitor exhibits an initial capacitance at a temperature of about 23° C. and a high temperature capacitance after exposure to a temperature of about 125° C. for 1,000 hours, and the ratio of the high temperature capacitance to the initial capacitance is less than or equal to about 3.0.
[17] The solid electrolytic capacitor of [1], wherein the capacitor exhibits an initial ESR at a temperature of about 23° C. and a high-humidity ESR after exposure to a relative humidity of about 85% and a temperature of about 85° C. for 1,000 hours, and the ratio of the high-humidity ESR to the initial ESR is less than or equal to about 2.0.
[18] The solid electrolytic capacitor of [1], wherein the capacitor exhibits an initial capacitance at a temperature of about 23° C. and a high humidity capacitance after exposure to a relative humidity of about 85% and a temperature of about 85° C. for 1,000 hours, wherein the ratio of the high humidity capacitance to the initial capacitance is less than or equal to about 2.0.
Claims
1. sintered porous anode body; a dielectric disposed over the anode body; and a layer of a solid electrolyte disposed over the dielectric, the solid electrolyte comprising a conductive polymer and a depolarizer; A solid electrolytic capacitor comprising a capacitor element comprising: the depolarizer is an aromatic quinone and has a standard reduction potential greater than 0; The conductive polymer has the following formula: 【Chemistry 1】 (In the formula, R 7 is a linear or branched C 1 -C 18 alkyl group, a C 5 -C 12 cycloalkyl group, a C 6 -C 14 aryl group, a C 7 -C 18 aralkyl group, or a combination thereof; q is an integer from 0 to 8. The repeat unit has the formula: The solid electrolytic capacitor, wherein the anode body comprises tantalum.
2. The depolarizer is 1,4-benzoquinone, 2-phenyl-1,4-benzoquinone, 2-methyl-1,4-benzoquinone, 2-tert-butyl-1,4-benzoquinone, 2-methoxy-1,4-benzoquinone, 2,6-dimethyl-1,4-benzoquinone, 2,3-dimethyl-1,4-benzoquinone, trimethyl-1,4-benzoquinone, 2,6-dimethoxy-1,4-benzoquinone, 2,5-methoxy-1,4-benzoquinone, tetramethyl-1,4-benzoquinone, tetrafluoro-1,4-benzoquinone, 2,5-dichloro-1,4-benzoquinone, tetrachloro-1,4-benzoquinone, 2-chloro-1,4-benzoquinone, or a combination thereof. The solid electrolytic capacitor of claim 1.
3. 10. The solid electrolytic capacitor of claim 1, further comprising an anode termination in electrical contact with the anode body, and a cathode termination in electrical communication with the solid electrolyte.
4. 10. The solid electrolytic capacitor of claim 1 further comprising a housing within which the capacitor element is contained.
5. The solid electrolytic capacitor of claim 4 , wherein the housing is formed from a resin material that encapsulates the capacitor element.
6. 2. The solid electrolytic capacitor of claim 1, wherein the conductive polymer is poly(3,4-ethylenedioxythiophene).
7. The solid electrolytic capacitor of claim 1 , wherein the conductive polymer is formed by in situ polymerization.
8. The solid electrolytic capacitor of claim 1 , wherein the conductive polymer is in the form of particles.
9. 9. The solid electrolytic capacitor of claim 8, wherein the solid electrolyte also includes a polymeric counterion.
10. 10. The solid electrolytic capacitor of claim 1, wherein the capacitor element further comprises a cathode coating comprising a metal particle layer disposed on the solid electrolyte, the metal particle layer comprising a plurality of conductive metal particles.
11. 2. The solid electrolytic capacitor of claim 1, wherein the capacitor exhibits an initial ESR at a temperature of 23° C. and a high temperature ESR after exposure to a temperature of 125° C. for 1,000 hours, the ratio of the high temperature ESR to the initial ESR being 3.0 or less.
12. 10. The solid electrolytic capacitor of claim 1, wherein the capacitor exhibits an initial capacitance at a temperature of 23° C. and a high temperature capacitance after exposure to a temperature of 125° C. for 1,000 hours, the ratio of the high temperature capacitance to the initial capacitance being 3.0 or less.
13. 2. The solid electrolytic capacitor of claim 1, wherein the capacitor exhibits an initial ESR at a temperature of 23° C. and a high humidity ESR after exposure to a relative humidity of 85% and a temperature of 85° C. for 1,000 hours, wherein the ratio of the high humidity ESR to the initial ESR is less than or equal to 2.
0.
14. 2. The solid electrolytic capacitor of claim 1, wherein the capacitor exhibits an initial capacitance at a temperature of 23° C. and a high humidity capacitance after exposure to 85% relative humidity and a temperature of 85° C. for 1,000 hours, wherein the ratio of the high humidity capacitance to the initial capacitance is less than or equal to 2.0.
Citation Information
Patent Citations
Method for producing conductive organic polymer
JP1993247204A
Method for manufacturing solid electrolytic capacitor
JP2008047654A
Solid electrolytic capacitor
WO2014091744A1