Plastic injection molding
A resin composition of biomass-derived polyethylene and fossil fuel-derived polypropylene addresses the challenge of uneven density and low fluidity in injection molding, enabling transparent, carbon-neutral products with uniform density and ease of manufacturing.
Patent Information
- Application Number
- JP2020113883
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-01
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Existing injection molding processes face challenges in producing transparent plastic products with uniform density using resin compositions containing biomass-derived polyethylene, often resulting in low fluidity and uneven density, which complicates the molding of thin-walled items.
A resin composition comprising biomass-derived polyethylene and fossil fuel-derived polypropylene is formulated, with specific density and melt flow rate ranges to ensure high transparency and uniform density, allowing for easy manufacturing of thin-walled products.
The composition enables the production of carbon-neutral, transparent plastic injection molded products with uniform density, reducing environmental impact and facilitating the manufacturing of thin-walled items like cups.
Smart Images

Figure 0007571400000003 
Figure 0007571400000001 
Figure 0007571400000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a plastic injection-molded article, for example, to a plastic injection-molded article made of a resin composition containing biomass-derived polyethylene. [Background technology]
[0002] In recent years, with the growing demand for the creation of a recycling-oriented society, there is a desire to move away from fossil fuels in the materials field, just as there is in energy, and the use of biomass has been attracting attention. Biomass is an organic compound that is photosynthesized from carbon dioxide and water, and since it becomes carbon dioxide and water again when used, biomass energy can be said to be a carbon-neutral renewable energy. Recently, the practical application of biomass plastics made from biomass has progressed rapidly, and attempts are being made to manufacture various resins from biomass raw materials.
[0003] Polylactic acid (PLA), which is produced via lactic acid fermentation, is known as a biomass-derived resin, and commercial production has already begun. However, since its performance as a plastic differs significantly from current general-purpose plastics, including its biodegradability, there are limitations to its product applications and manufacturing methods, and it has not yet become widely used. In addition, a life cycle assessment (LCA) is being conducted on PLA, and discussions are being held on the energy consumption during PLA production and its equivalence when replacing general-purpose plastics.
[0004] Various types of general-purpose plastics are known, including polyethylene, polyvinyl chloride, polystyrene, and ABS resin. In particular, polyethylene is molded into films, sheets, bottles, cups, and the like, and is used in a variety of applications, such as packaging materials, and is used in large quantities around the world. Therefore, since the use of conventional fossil fuel-derived polyethylene places a large burden on the environment, it is desirable to use biomass-derived raw materials in the production of polyethylene to reduce the amount of fossil fuel used. From this perspective, a technology for producing ethylene, a raw material for polyolefin resins, from renewable natural raw materials has been proposed in Patent Document 1 and elsewhere. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2011-506628 Summary of the Invention [Problem to be solved by the invention]
[0006] Injection molding is used in many plastic molding processes. However, when injection molding is performed using a resin composition containing biomass-derived polyethylene, it is not easy to produce an injection-molded product with high transparency and no uneven shading. For example, the low fluidity of the resin composition makes it difficult to mold thin parts, or uneven shading occurs, reducing transparency.
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a plastic injection-molded product which has high transparency without unevenness in shading, is easy to manufacture, and has a small environmental impact. [Means for solving the problem]
[0008] In order to achieve the above object, a plastic injection-molded article of a first invention is a plastic injection-molded article made of a resin composition containing biomass-derived polyethylene obtained by polymerizing a monomer containing ethylene derived from biomass, and fossil fuel-derived polypropylene obtained by polymerizing fossil fuel-derived propylene and ethylene monomers, The biomass-derived polyethylene has a density of 0.91 to 0.96 g / cm 3 and a melt flow rate of 15 g / 10 min or more; The fossil fuel-derived polypropylene has a viscosity of 0.89 to 0.93 g / cm 3 and a melt flow rate of 30 g / 10 min or more; The resin composition is characterized in that it contains the biomass-derived polyethylene in an amount of 5% by mass or more based on the entire resin composition.
[0009] The plastic injection-molded article of a second invention is the above-mentioned first invention, characterized in that the resin composition contains the biomass-derived polyethylene in an amount of 5 to 30% by mass based on the total mass of the resin composition.
[0010] The third invention is a plastic injection-molded product according to the first invention, which is a plastic injection-molded product having a side wall thickness of 0.5 to 0.9 mm and a haze value of less than 30% on the side wall, The fossil fuel-derived polypropylene is a transparent block-type polypropylene resin, The resin composition is characterized in that the biomass-derived polyethylene is contained in an amount of 5 to 15% by mass based on the entire resin composition.
[0011] The fourth invention is a plastic injection-molded product according to the first invention, which is a plastic injection-molded product having a side wall thickness of 0.5 to 0.9 mm and a haze value of less than 30% on the side wall, The fossil fuel-derived polypropylene is a transparent random type polypropylene resin, The resin composition is characterized in that the biomass-derived polyethylene is contained in an amount of 5 to 10% by mass based on the entire resin composition.
[0012] The plastic injection-molded product of the fifth invention is any one of the above first to fourth inventions, characterized in that a label is integrated by in-mold label molding.
[0013] The plastic injection-molded article of a sixth invention is characterized in that, in any one of the above first to fifth inventions, it has a cup shape. Effect of the Invention
[0014] According to the present invention, since the resin composition constituting the plastic injection molded product contains 5% by mass or more of biomass-derived polyethylene relative to the entire resin composition, a carbon-neutral plastic injection molded product can be realized. In other words, the amount of fossil fuel used can be significantly reduced compared to the conventional method, and the environmental load can be reduced. Furthermore, since the biomass-derived polyethylene and the fossil fuel-derived polypropylene each have an appropriate density and melt flow rate, the injection molded product can be easily manufactured while having high transparency without uneven shading. For example, even a cup with a thin wall thickness can be easily manufactured due to the high fluidity of the resin composition. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram showing an embodiment of a plastic injection molded product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a plastic injection-molded product according to an embodiment of the present invention will be described with reference to the drawings. Fig. 1 shows a schematic structure of a plastic injection-molded product 10 according to one embodiment. In Fig. 1, (A) is a plan view showing the plastic injection-molded product 10, and (B) is a front view showing the plastic injection-molded product 10 in partial cross section.
[0017] The plastic injection molded product 10 has a cup shape as shown in Fig. 1, with a preferred side wall thickness d of 0.5 to 0.9 mm and a preferred haze value of less than 30%. Here, it is assumed that the side wall thickness is d = 0.7 mm, the cup height is h = 100 mm, and the label is integrated by in-mold label molding, but the molded product size, injection molding method, etc. are not limited to these.
[0018] In-mold label molding is a technology in which a label is inserted into the mold during injection molding, and labeling is performed at the same time as molding. Labels can be beautifully printed using gravure printing or laminated with a film that has barrier properties. This labeling gives the injection-molded container a design and function (barrier properties). In contrast, painting on general injection-molded products requires secondary processing such as direct printing (dry offset printing) and shrink processing after injection molding.
[0019] The plastic injection molded product 10 is made of a resin composition containing biomass-derived polyethylene (PE) obtained by polymerizing a monomer containing ethylene derived from biomass, and fossil fuel-derived polypropylene (PP) obtained by polymerizing fossil fuel-derived propylene and ethylene monomers, and the resin composition contains 5% by mass or more of biomass-derived polyethylene relative to the entire resin composition. By containing 5% by mass or more of biomass-derived polyethylene in this way, a carbon-neutral plastic injection molded product can be realized. In other words, the amount of fossil fuel used can be significantly reduced compared to the past, and the environmental load can be reduced.
[0020] In order to perform injection molding, it is necessary to set the density and melt flow rate (MFR) of the resin appropriately. In other words, when performing injection molding, biomass-derived polyethylene has a density of 0.91 to 0.96 g / cm 3 and a melt flow rate of 15 g / 10 min or more, and the fossil fuel-derived polypropylene preferably has a density of 0.89 to 0.93 g / cm 3 and a melt flow rate of 30 g / 10 min or more. These density ranges provide suitable molded body strength and transparency and cover readily available biomass-derived polyethylene and fossil fuel-derived polypropylene, and these MFR ranges indicate the range of fluidity suitable for injection molding.
[0021] If the melt flow rate of the biomass-derived polyethylene is less than 15 g / 10 min, the fluidity of the resin composition is poor, making it difficult to mold thin-walled containers (cups, etc.). The same is true when the melt flow rate of the main material, fossil fuel-derived polypropylene, is less than 30 g / 10 min, making it difficult to mold thin-walled containers (cups, etc.). In this way, by configuring the biomass-derived polyethylene and the fossil fuel-derived polypropylene to have appropriate densities and melt flow rates, respectively, it becomes possible to easily manufacture injection-molded products while having high transparency without uneven shading. For example, even a cup with a thin wall thickness can be easily manufactured due to the high fluidity of the resin composition.
[0022] Biomass-derived polyethylene has poor resin fluidity compared to fossil fuel-derived polypropylene. For example, when the size of the plastic injection molded product 10 is a side wall thickness d=0.5 mm and a cup height h=100 mm, if the biomass-derived polyethylene is added in an amount exceeding 30% by mass relative to the entire resin composition, the resin may not flow to the flange of the cup, resulting in molding defects. Moreover, if the haze value on the side is 30% or more, it becomes difficult to use the molded product in applications where the contents of the molded product should be visible. Therefore, it is preferable that the amount of biomass-derived polyethylene added relative to the entire resin composition is 30% by mass or less. In other words, it is preferable that the resin composition contains 5 to 30% by mass of biomass-derived polyethylene relative to the entire resin composition.
[0023] When obtaining a transparent plastic injection-molded product, a random-type polypropylene resin is generally used, but when biomass-derived polyethylene is added to a random-type polypropylene resin, the random bonds are inhibited and the transparency is significantly reduced. In contrast, with a transparent block-type polypropylene, the polyethylene penetrates into the block bonds to suppress the loss of transparency, so a plastic injection-molded product that is more transparent than a random-type polypropylene resin is obtained. Therefore, in applications where the contents of the molded product need to be visible, a blend with a transparent block-type polypropylene resin is desirable.
[0024] As described above, the transparency (haze value) differs depending on the type of fossil fuel-derived polypropylene used (block type, random type), so it is preferable from the viewpoint of transparency to set the content of biomass-derived polyethylene according to the type of fossil fuel-derived polypropylene. In addition, in general injection molded products (cup-shaped containers, etc.), the side wall thickness d is preferably 0.5 to 0.9 mm in terms of the balance between strength and moldability, and in the case of injection molded products such as refrigerated beverage cups and dessert cups, the haze value on the side is preferably less than 30% so that the contents can be seen (ensuring visibility of the contents).
[0025] Therefore, in a plastic injection-molded product having a side thickness d of 0.5 to 0.9 mm and a haze value at the side of less than 30%, when the fossil fuel-derived polypropylene is a transparent block-type polypropylene resin, it is preferable that the resin composition contains 5 to 15 mass% of biomass-derived polyethylene based on the entire resin composition, and when the fossil fuel-derived polypropylene is a transparent random-type polypropylene resin, it is preferable that the resin composition contains 5 to 10 mass% of biomass-derived polyethylene based on the entire resin composition.
[0026] Biomass-derived ethylene, which is the raw material for biomass-derived polyethylene, can be produced using biomass-derived ethanol as the raw material. Examples of biomass-derived ethanol include biomass-derived fermented ethanol obtained from plant raw materials, and examples of plant raw materials include corn, sugarcane, beet, and manioc. Biomass-derived fermented ethanol is ethanol produced by contacting a culture solution containing a carbon source obtained from a plant raw material with a microorganism that produces ethanol or a product derived from its crushed material, and then purifying the ethanol. Conventionally known methods such as distillation, membrane separation, and extraction can be used to purify ethanol from the culture solution. Then, when a dehydration reaction of ethanol is performed by a conventionally known method using a catalyst, a mixture of ethylene, water, and a small amount of unreacted ethanol is obtained, and when the water and ethanol are removed from the mixture by gas-liquid separation, biomass-derived ethylene is obtained. The polymerization method of a monomer containing biomass-derived ethylene can also be performed by a conventionally known method.
[0027] Biomass-derived polyethylene is obtained by polymerizing a monomer containing biomass-derived ethylene. Therefore, the raw material monomer does not have to contain 100% by mass of biomass-derived ethylene. For example, it may further contain ethylene or α-olefin derived from fossil fuel, or may further contain α-olefin derived from biomass. As the α-olefin, for example, one having 3 to 20 carbon atoms can be used, and preferred ones from the viewpoint of production, etc. include butylene, hexene, and octene.
[0028] The biomass-derived ethylene concentration (hereinafter also referred to as "biomass degree") in biomass-derived polyethylene can be measured as the content of biomass-derived carbon by radiocarbon (C14) measurement. Carbon dioxide in the atmosphere contains a certain percentage (105.5 pMC) of C14, and it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain almost no C14. Therefore, the percentage of biomass-derived carbon can be calculated by measuring the percentage of C14 contained in the total carbon atoms in the polyethylene. For example, when the content of C14 in biomass-derived polyethylene is PC14, the biomass degree of biomass-derived polyethylene can be calculated by the formula: Pbio (%) = PC14 / 105.5 x 100, where Pbio is the content of biomass-derived carbon.
[0029] If all biomass-derived ethylene is used as the raw material for polyethylene, the concentration of biomass-derived ethylene will be 100%, and therefore the biomass degree of the biomass-derived polyethylene will be 100%. If biomass-derived polyethylene is used even as a part of the resin composition, the amount of fossil fuel used will be reduced, so the biomass degree of the biomass-derived polyethylene does not need to be 100%. However, in the case of ordinary biomass-derived polyethylene, the effect of reducing the amount of fossil fuel used will be significant if the content of the polyethylene is 5% by mass or more relative to the entire resin composition, so the biomass degree of the biomass-derived polyethylene is preferably 80% or more, and more preferably 90% or more. EXAMPLES
[0030] The plastic injection molded products embodying the present invention will be described in more detail below with reference to examples and comparative examples. Table 1 shows the specific name of the fossil fuel-derived polypropylene (PP), the specific name of the biomass-derived polyethylene (PE), the blend ratio of each resin (PP / PE), the haze value (%) on the side, and the appearance for Comparative Examples 1 and 2 and Examples 1 to 10 (side thickness d=0.7 mm, cup height h=100 mm). Table 2 also shows the molding conditions, moldability, and condition changes for Comparative Examples 1 and 2 and Examples 1 to 10. Note that Comparative Examples 1 and 2 are examples with a large environmental load because no biomass-derived polyethylene was added (PP / PE=100 / 0).
[0031] As a fossil fuel-derived polypropylene, Sanallomer Co., Ltd., product name: CMA70V (transparent block PP, density: 0.90 g / cm 3 , MFR: 50g / 10min (JIS standard 6921-2)) and Japan Polypropylene Corporation, product name: MG05ES (random PP, density: 0.90g / cm 3 , MFR: 45g / 10min (JIS standard 6921-2) was used.
[0032] As a biomass-derived polyethylene, Braskem's product name: SHA7260 (density: 0.955 g / cm 3The following conditions were used: MFR 20g / 10min (190℃, extrusion with 2.16kg), biomass ratio 94%). Note that the biomass ratio is the amount of carbon derived from biomass measured by radiocarbon (C14) as mentioned above.
[0033] In Table 1, the "appearance" was evaluated as follows: ○: transparent with no unevenness in shading, △: unevenness in some areas, ×: transparent / opaque unevenness in shading seen throughout. In Table 2, "moldability" shows only those that could not be molded, and "condition changes" show the holding pressure etc. of Comparative Examples 1 and 2 as the standard. In order to improve the fluidity of a resin, it is common to increase the resin temperature, but when polyethylene is added, if the resin temperature is raised to 210°C or higher, the polyethylene burns and carbonized foreign matter is generated, so the holding pressure and holding pressure switching position were changed and the resin was forced into the mold. The adoption of in-mold label molding does not affect the evaluation results.
[0034] [Table 1]
[0035] [Table 2] [Explanation of symbols]
[0036] 10 Plastic injection moldings
Claims
1. A plastic injection-molded product made of a resin composition containing a biomass-derived polyethylene obtained by polymerizing a monomer containing ethylene derived from a biomass, and a fossil fuel-derived polypropylene obtained by polymerizing a monomer of propylene and ethylene derived from a fossil fuel, the product having a side wall thickness of 0.5 to 0.9 mm and a haze value of less than 30% on the side wall, The biomass-derived polyethylene has a density of 0.91 to 0.96 g / cm 3 and a melt flow rate (extrusion at 190° C. and 2.16 kg) of 15 g / 10 min or more; The fossil fuel-derived polypropylene is a block type polypropylene resin having a viscosity of 0.89 to 0.93 g / cm 3 and a melt flow rate (JIS standard 6921-2) of 30 g / 10 min or more, The plastic injection-molded product, characterized in that the resin composition contains 5% by mass to 15% by mass of the biomass-derived polyethylene based on the entire resin composition.
2. A plastic injection-molded product made of a resin composition containing a biomass-derived polyethylene obtained by polymerizing a monomer containing ethylene derived from a biomass, and a fossil fuel-derived polypropylene obtained by polymerizing a monomer of propylene and ethylene derived from a fossil fuel, the product having a side wall thickness of 0.5 to 0.9 mm and a haze value of less than 30% on the side wall, The biomass-derived polyethylene has a density of 0.91 to 0.96 g / cm 3 and a melt flow rate (extrusion at 190° C. and 2.16 kg) of 15 g / 10 min or more; The fossil fuel-derived polypropylene is a random type polypropylene resin having a viscosity of 0.89 to 0.93 g / cm 3 and a melt flow rate (JIS standard 6921-2) of 30 g / 10 min or more, The resin composition contains 5% by mass to 10% by mass of the biomass-derived polyethylene based on the entire resin composition.
3. 3. The plastic injection molded product according to claim 1, wherein a label is integrated with the product by in-mold label molding.
4. The plastic injection molded article according to any one of claims 1 to 3, characterized in that it has a cup shape.
Citation Information
Patent Citations
Polypropylene resin composition
JP2001026686A
Plastic container with in-mold label
JP2009227316A
Integrated method for the production of ethylene-butylene copolymer, ethylene-butylene copolymer and use of ethylene and 1-butylene as comonomers supplied from renewable natural raw materials.
JP2011506628A
Resin molded article
JP2013227462A
Injection molding using polypropylene resin composition
JP2017193066A