Resin composition and film for covering material
A resin composition with ethylene-vinyl acetate copolymer, tackifier, and antifogging agent addresses weak adhesion and fogging issues in conventional lids, offering superior adhesion, antifogging, and slip properties for PET, PLA, and polypropylene containers.
Patent Information
- Application Number
- JP2020164053
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Conventional resin compositions for container lids face challenges with weak adhesive strength, leading to lid opening during transportation or storage, poor moldability, and inadequate antifogging and slip properties, especially for polyethylene terephthalate (PET) containers, and fail to meet the needs of biodegradable plastics like polylactic acid (PLA).
A resin composition comprising ethylene-vinyl acetate copolymer with specific vinyl acetate content and molecular weight ratio, combined with a tackifier and antifogging agent, provides excellent adhesion, antifogging properties, and slip properties for various plastic containers, including PET, PLA, and polypropylene.
The composition ensures high adhesive strength, effective antifogging performance, and appropriate slip properties, enhancing the moldability and sealing integrity of container lids, particularly for PET, PLA, and polypropylene containers.
Smart Images

Figure 0007571439000001 
Figure 0007571439000002 
Figure 0007571439000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition used for a lid material for a container, and more specifically, to an adhesive resin composition which has excellent moldability, high adhesion to a container, anti-fogging properties, and moderate slip properties, and which can be suitably used as a sealant for a lid material, and a film for a lid material which has this as a sealant layer. [Background technology]
[0002] 2. Description of the Related Art Conventionally, plastic containers such as polyethylene, polypropylene, and polystyrene, and paper containers mainly made of paper have been used for packaging food and beverages, pharmaceuticals, industrial parts, etc., and the lids of these containers are made of easily peelable films that have stable adhesive properties to protect the contents and have appropriate peelability so that they can be opened when peeled off.
[0003] So far, many materials for easily peelable films have been known for containers such as polypropylene and polystyrene, but no practically excellent easily peelable films have been found for containers made of amorphous polyethylene terephthalate (hereinafter referred to as "A-PET"), which has been increasingly used in recent years due to its low cost, transparency, and cold resistance. When conventional easily peelable films are used as lids for A-PET containers, there are problems such as the lid opening due to vibration or dropping during transportation or storage due to weak adhesive strength, and the container deforming and losing its sealing ability as a result of setting a high heat seal temperature in an attempt to obtain high adhesive strength. In addition, there is a drawback that the sealing strength decreases when stored in a low-temperature environment after adhesion, making it difficult to use in practice. In addition, conventional easily peelable films have problems such as the lid becoming cloudy due to the cold air outside and the humidity and air inside the container, making it difficult to see the food inside, reducing the product value, and moisture adhering to the inside of the lid adversely affecting the food inside. Furthermore, conventional resin compositions have problems in that they adhere to the cooling roll during extrusion lamination or cast molding, making the film impossible to mold or leaving peeling marks on the film, reducing its commercial value. In addition, when a slip agent is added to improve adhesion to the cooling roll, there is a problem that the adhesive strength with the container is reduced.
[0004] Generally, mixtures of polyethylene, ethylene-vinyl acetate copolymer, ethylene-α-olefin copolymer, etc. and tackifiers are known as adhesives for lid material sealants. However, such materials may not be able to provide sufficient adhesive strength for containers made of a wide range of materials, from polyolefin to A-PET. Due to the weak adhesive strength, there are problems such as the lid opening due to vibration or dropping during transportation or storage, and the container deforming and the sealing ability being reduced as a result of setting a high heat sealing temperature in an attempt to obtain high adhesive strength. Further, there have been used resin compositions comprising an ethylene-α-olefin copolymer, an olefin-based elastomer and / or a styrene-based elastomer, and a tackifier (see, for example, Patent Document 1); sealing materials comprising an ethylene-α-olefin copolymer, an ethylene-polar monomer copolymer, an ABA block copolymer, and a tackifier (see, for example, Patent Document 2); compositions containing an anti-fogging agent such as a polyhydric alcohol fatty acid ester (see, for example, Patent Document 3); and a method of applying a minimum amount of a surfactant required to exhibit an anti-fogging effect to the surface (see, for example, Patent Document 4). However, none of these methods were able to satisfy all of the requirements for moldability, adhesive strength, anti-fogging property, and appropriate slip property.
[0005] In recent years, the demand for biodegradable plastics has been increasing due to growing awareness of environmental conservation. In the field of food packaging materials, the amount of biodegradable plastics such as polylactic acid (PLA) used as container materials is increasing, but the conventional adhesive resins for sealants used in the lids of these containers do not have sufficient adhesiveness to PLA, etc., and an adhesive resin that can be used suitably for these applications has been desired. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 1999-269319 A [Patent Document 2] Patent No. 4438108 [Patent Document 3] Japanese Unexamined Patent Publication No. 58-79044 [Patent Document 4] Japanese Patent Application Publication No. 4-103639 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a resin composition and a film for a lid material that have excellent moldability, excellent adhesion, anti-fogging properties, and slip properties to plastic containers, particularly containers made of polyethylene terephthalate, polylactic acid, polystyrene, and polypropylene, and that can be suitably used as a sealant layer for a lid material for the container. [Means for solving the problem]
[0008] Means for Solving the Problems The inventors of the present invention conducted intensive research into the above-mentioned problems and discovered that a resin composition containing an ethylene-vinyl acetate copolymer having specific properties, a tackifier, and an anti-fogging agent has excellent moldability, and excellent adhesion, anti-fogging properties, and slip properties to various plastic containers including A-PET and polylactic acid, thereby completing the present invention.
[0009] That is, the present invention relates to a resin composition comprising 58 to 94.9 parts by weight of an ethylene-vinyl acetate copolymer (A) having a vinyl acetate content (VA) of 3 to 13% by weight and a ratio Qw of weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.5 to 4.5, 5 to 40 parts by weight of a tackifier resin (B), and 0.1 to 2% by weight of an anti-fogging agent (C) (wherein the total of (A), (B), and (C) is 100 parts by weight). Effect of the Invention
[0010] According to the present invention, it is possible to provide a resin composition which has excellent moldability, excellent adhesion, anti-fogging properties, and slip properties to various types of plastic containers, particularly containers made of polyethylene terephthalate, polylactic acid, polystyrene, and polypropylene, and which is useful for producing an adhesive layer for a sealant of a container lid material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The resin composition according to one embodiment of the present invention will be described in detail below.
[0012] The ethylene-vinyl acetate copolymer (A) constituting the present invention has a vinyl acetate content of 3% by weight or more and 15% by weight or less, preferably 3% by weight or more and 13% by weight or less, and more preferably 5% by weight or more and 10% by weight or less. If the vinyl acetate content is less than 3% by weight, the resulting composition is undesirably inferior in low-temperature heat sealability. On the other hand, if the vinyl acetate content exceeds 15% by weight, the resulting composition is undesirably inferior in moldability and adhesive strength.
[0013] Here, the vinyl acetate content in the ethylene-vinyl acetate copolymer can be measured by a method in accordance with JIS K 6924-1.
[0014] The ethylene-vinyl acetate copolymer (A) constituting the present invention has a ratio Mw / Mn (hereinafter referred to as "Qw") of its weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.5 to 4.5, preferably 2.0 to 4.5, more preferably 2.5 to 4.2. If Qw is less than 1.5, the extrusion load during molding increases, which is undesirable because it increases energy consumption. Also, if Qw exceeds 4.5, the adhesive strength and sealing strength of the composition of the present invention are undesirable.
[0015] Here, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the ethylene-vinyl acetate copolymer (A) can be calculated as the molecular weight of linear polyethylene by measuring a universal calibration curve, for example, using gel permeation chromatography.
[0016] Furthermore, the ethylene-vinyl acetate copolymer (A) constituting the present invention is preferably such that the vinyl acetate content VA (unit: weight %) and Qw satisfy the following relational formula (1), since this increases the adhesive strength and sealing strength of the composition of the present invention. Qw<-1.9×lnVA+9.0 (1) Here, lnVA indicates the natural logarithm of the vinyl acetate content VA (% by weight).
[0017] The ethylene-vinyl acetate copolymer (A) constituting the present invention can be obtained by a known production method, and there is no particular restriction on the production method. However, a method of radical polymerization under high pressure using a tubular reactor is preferred because it can easily produce an ethylene-vinyl acetate copolymer having a vinyl acetate content and Qw that satisfy the requirements of the present application.
[0018] The ethylene-vinyl acetate copolymer (A) in the present invention may be either a single component or a composition containing two or more types of copolymers. When the copolymer (A) is a composition, the vinyl acetate content of the composition means a value measured on the composition using the method of JIS K 6924-1 described above. Similarly, the Qw of the composition means a value measured on the composition using the method of gel permeation chromatography described above. It is sufficient that the vinyl acetate content and the ratio Qw of the weight average molecular weight to the number average molecular weight obtained for these compositions satisfy the requirements of the ethylene-vinyl acetate copolymer (A).
[0019] The blending ratio of the ethylene-vinyl acetate copolymer (A) constituting the present invention is 58 parts by weight or more and 94.9 parts by weight or less, preferably 70 parts by weight or more and 90 parts by weight or less, more preferably 75 parts by weight or more and 90 parts by weight or less. If the blending ratio of (A) is less than 58 parts by weight, the molding process stability of the resulting resin composition is inferior, which is not preferred. On the other hand, if it exceeds 94.9 parts by weight, the adhesiveness of the resulting resin composition is insufficient, which is not preferred. The blending ratio of (A) is preferably 81 parts by weight or more and 90 parts by weight or less. This allows the resin composition of the present application to maintain sufficient adhesive strength even if the blending amount of the tackifier (B) is reduced.
[0020] The tackifier resin (B) constituting the present invention can be any resin that falls within the category of tackifier resins. Examples of the tackifier resin (B) include synthetic petroleum resin-based tackifiers such as petroleum resin-based, coumarone resin-based, and styrene-based tackifiers, and natural resin-based tackifiers such as rosin-based, methyl ester-based, glycerin ester-based, pentaerythritol ester-based, terpene-based, and modified products thereof. Among these tackifier resins, synthetic petroleum resin-based tackifiers include aliphatic petroleum resins, aliphatic hydrogenated petroleum resins, aromatic petroleum resins, aromatic hydrogenated petroleum resins, alicyclic petroleum resins, alicyclic hydrogenated petroleum resins, and copolymerized hydrogenated petroleum resins. Of these, it is preferable to use either aromatic hydrogenated petroleum resins or alicyclic hydrogenated petroleum resins. In particular, tackifier resins consisting of at least one type selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, alicyclic hydrogenated petroleum resins, and copolymerized petroleum resins are preferred because of their excellent adhesiveness. These tackifiers can be used alone or in combination of two or more kinds.
[0021] The tackifier resin (B) constituting the present invention preferably has a softening point measured by the ring and ball method in the range of 90° C. to 140° C., more preferably 100° C. to 135° C., and even more preferably 105° C. to 130° C. When the softening point is in the above range, blocking of the film after molding is small, and adhesive strength retention in a low-temperature environment is favorable.
[0022] The tackifier resin (B) constituting the present invention may be a commercially available product. Specifically, examples of petroleum resins include (trade names) Alcon P100, Alcon P125, Alcon P140, Alcon M90, Alcon M115, and Alcon M135 (all manufactured by Arakawa Chemical Industries Co., Ltd.), Imave S110, Imave P125 (all manufactured by Idemitsu Kosan Co., Ltd.), T-REZ RC115, and T-REZ HA125 (all manufactured by JXTG Energy Corporation). Examples of rosin resins include Pine Crystal KE-311 (manufactured by Arakawa Chemical Industries Co., Ltd.). Examples of terpene resins include YS Resin PX1150 and YS Resin PX1150N (all manufactured by Yasuhara Chemical Co., Ltd.).
[0023] The blending ratio of the tackifier resin (B) constituting the present invention is 5 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, more preferably 10 parts by weight or more and 25 parts by weight or less. If the blending ratio of (B) is less than 5 parts by weight, the adhesiveness of the resulting resin composition is insufficient, which is not preferable. On the other hand, if it exceeds 40 parts by weight, blocking between the films when molded into a film may become strong, which may adversely affect secondary processing, which is not preferable. The blending ratio of (B) is preferably 10 parts by weight or more and 19 parts by weight or less. This allows the resin composition of the present application to maintain sufficient adhesive strength even if the blending amount of the tackifier (B) is reduced.
[0024] The antifogging agent (C) constituting the present invention can be any agent that falls within the category of antifogging agents. Examples of the antifogging agent (C) include ethylene oxide adducts such as glycerin fatty acid esters, diglycerin fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, polyethylene glycol fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene sorbitan fatty acid esters, and polyoxyethylene fatty acid esters, amine compounds such as alkylamines and alkyldiethanolamines, dialkyl sulfosuccinates, linear alkylbenzene sulfonates, and organic sulfonates such as alkyl sulfonates. The antifogging agent (C) is preferably at least one of the group consisting of ethylene oxide adducts, amine compounds, and organic sulfonates. Among these, it is preferable to use any of glycerin fatty acid esters, diglycerin fatty acid esters, and amine compounds. These antifogging agents can be used alone or in combination of two or more.
[0025] Glycerol fatty acid esters are compounds obtained by esterification reaction of fatty acid and glycerol. The fatty acid is generally a linear or branched alkyl or alkenyl group, and preferably has 8 to 22 carbon atoms, since sufficient anti-fogging performance can be obtained. Examples of such compounds include lauric acid monoglyceride, palmitic acid monoglyceride, stearic acid monoglyceride, oleic acid monoglyceride, linoleic acid monoglyceride, and diglycerol stearate, with stearic acid monoglyceride and diglycerol stearate being preferred. These compounds can be used alone or in mixtures.
[0026] Specific examples of commercially available glycerol fatty acid esters include Rikemal P-100, Rikemal S-100, Rikemal S-71D, Rikemal O-71D, Rikemal L-71D, Poem M-200, Poem M-300 (manufactured by Riken Vitamin), Leodol MS-50 (manufactured by Kao), and Monogly D, M, and I (manufactured by Nippon Oil & Fats).
[0027] Sorbitan fatty acid ester is a compound obtained by esterification reaction of sorbitan and fatty acid. Examples of sorbitan fatty acid ester include sorbitan sesquioleate, sorbitan monooleate, sorbitan monostearate, sorbitan monolaurate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, etc., and sorbitan monooleate, sorbitan monostearate, and sorbitan monolaurate are preferred. These sorbitan fatty acid esters may be used alone or in combination of two or more.
[0028] Specific examples of commercially available sorbitan fatty acid esters include Rikemal L-250A, Rikemal P-300, and Rikemal S-300W (manufactured by Riken Vitamin).
[0029] Ethylene oxide adducts are compounds in which ethylene oxide is added to alcohols, fatty acids, their esters, fats and oils, etc., and are generally known as nonionic surfactants. The chain length of the polymerized portion of ethylene oxide is adjusted to a desired HLB. Specific examples of ethylene oxide adducts include polyoxyethylene alkyl ethers, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene fatty acid esters, etc. Specific examples of fatty acids constituting polyoxyethylene sorbitan fatty acid esters and polyoxyethylene fatty acid esters are the same as those listed as examples of fatty acids constituting the monoglycerin fatty acid esters, and among them, saturated or unsaturated fatty acids having 12 to 20 carbon atoms are preferably used. These fatty acids may be used alone or in combination of two or more.
[0030] Specific examples of commercially available ethylene oxide adducts include Rikemal O-852 (polyoxyethylene sorbitan trioleate) and Rikemal B-205 (polyoxyethylene alkyl ether) manufactured by Riken Vitamin Co., Ltd., and the Rheodor TW series (polyoxyethylene sorbitan fatty acid esters) and Emanone series (polyoxyethylene fatty acid esters) manufactured by Kao Corporation.
[0031] The amine compound may be an aliphatic amine, an aliphatic amine derivative, or an amine salt of sulfonic acid, and the like. Since they have excellent anti-fogging properties, the aliphatic amine or an aliphatic amine derivative is preferred. The aliphatic amine includes saturated aliphatic amines and unsaturated aliphatic amines having 6 to 30 carbon atoms, and is preferably a primary aliphatic amine or a secondary aliphatic amine. For example, primary aliphatic amines such as hexylamine, octylamine, isooctylamine, caprylamine, caproleylamine, laurylamine, myristylamine, myristoleylamine, heptadecylamine, palmitylamine, isopalmitylamine, palmitoleylamine, stearylamine, isostearylamine, arachylamine, ricinoleylamine, linoleylamine, behenylamine, oleylamine, and lignoceylamine; and secondary aliphatic amines such as N,N-dicaprylamine, N,N-dioctylamine, N,N-dicaprylamine, N,N-dicaproleylamine, N,N-dilaurylamine, and N,N-dimyristylamine can be mentioned. Examples of the aliphatic amine derivatives include polyoxyethylene alkylamines, decylethanolamine, dodecyldiethanolamine, tetradecyldiethanolamine, hexadecyldiethanolamine, octadecyldiethanolamine, eicosyldiethanolamine, etc., with polyoxyethylene alkylamines, polyoxyethylene stearylamine, dodecyldiethanolamine, tetradecyldiethanolamine, hexadecyldiethanolamine, and octadecyldiethanolamine being preferred, and polyoxyethylene alkylamines being particularly preferred. These compounds may be used alone or in mixture.
[0032] A specific example of a commercially available amine compound is Armostat 310 (manufactured by Lion Corporation).
[0033] The organic sulfonate is composed of an organic sulfonic acid and a base. The organic sulfonic acids constituting the organic sulfonate include: 1) alkylsulfonic acids having an alkyl group with 8 to 24 carbon atoms, such as octyl sulfonic acid, dodecyl sulfonic acid, tetradecyl sulfonic acid, stearyl sulfonic acid, tetracosyl sulfonic acid, and 2-ethylhexyl sulfonic acid; 2) aromatic sulfonic acids, such as benzenesulfonic acid and naphthalenesulfonic acid; 3) alkylbenzenesulfonic acids having an alkyl group with 6 to 18 carbon atoms, such as hexylbenzenesulfonic acid, octylbenzenesulfonic acid, nonylbenzenesulfonic acid, dodecylbenzenesulfonic acid, and octadecylbenzenesulfonic acid; 4) dibutylbenzenesulfonic acid, dioctylbenzenesulfonic acid, didodecylbenzenesulfonic acid, and tetradecylbenzenesulfonic acid; 5) alkyl naphthalene sulfonic acids having an alkyl group of 1 to 18 carbon atoms, such as methyl naphthalene sulfonic acid, isopropyl naphthalene sulfonic acid, butyl naphthalene sulfonic acid, etc.; 6) dialkyl naphthalene sulfonic acids having an alkyl group of 1 to 18 carbon atoms, such as dimethyl naphthalene sulfonic acid, diisopropyl naphthalene sulfonic acid, dibutyl naphthalene sulfonic acid, dioctadecyl naphthalene sulfonic acid, etc., alkyl chain alkanesulfonic acids and hydroxyalkanesulfonic acids having an alkyl group of 10 to 18 carbon atoms. Examples of the base that constitutes the organic sulfonate include 1) alkali metals such as sodium, potassium, and lithium; 2) phosphoniums such as tetrabutylphosphonium, tributylbenzylphosphonium, triethylhexadecylphosphonium, and tetraphenylphosphonium; and 3) ammoniums such as tetrabutylammonium, tributylbenzylammonium, and triphenylbenzylammonium.As the organic sulfonate, an appropriate combination of the sulfonic acid and base described above can be used, but among them, as the organic sulfonate, alkylsulfonates in which the alkyl group has 8 to 24 carbon atoms, alkylbenzenesulfonates in which the alkyl group has 6 to 18 carbon atoms, alkylnaphthalenesulfonates in which the alkyl group has 1 to 18 carbon atoms, alkyl chain alkanesulfonates in which the alkyl group has 10 to 18 carbon atoms, and hydroxyalkanesulfonates are preferred, and salts such as sodium, potassium, and ammonium salts of alkylsulfonic acids having 8 to 20 carbon atoms, and sodium, potassium, and ammonium salts of alkanesulfonates having 10 to 18 carbon atoms are more preferred.
[0034] A specific example of a commercially available organic sulfonate is Dasper 802D (manufactured by Miyoshi Oil Co., Ltd.).
[0035] The blending ratio of the anti-fog agent (C) constituting the present invention is 0.1 parts by weight or more and 2 parts by weight or less, preferably 0.2 parts by weight or more and 1 part by weight or less, more preferably 0.2 parts by weight or more and 0.8 parts by weight or less. If the blending ratio of (C) is less than 0.1 parts by weight, the moldability, anti-fog property, and slip property of the obtained resin composition are insufficient, which is not preferable. On the other hand, if it exceeds 2 parts by weight, the adhesive strength is insufficient, which is not preferable.
[0036] The antifogging agent (C) can be used in combination of two or more kinds. In this case, it is preferable to use a glycerin fatty acid ester and an amine compound in combination. When a glycerin fatty acid ester and an amine compound are used in combination, the mixing ratio by weight is preferably 1 / 3 to 3 / 1.
[0037] The resin composition of the present invention may contain a thermoplastic block copolymer (D) containing at least one of an olefin and a diolefin as a structural unit and a vinyl aromatic hydrocarbon as a structural unit. The thermoplastic block copolymer (D) is represented by the following formula: (AB)n (AB)nA´ or (AB)mX (wherein A and A' each independently represent a vinyl aromatic hydrocarbon polymer block; B represents a polymer block of either an olefin or a diolefin; n represents an integer of 1 to 5; m represents an integer of 2 to 7; and X represents an m-valent polyfunctional compound.)
[0038] The thermoplastic block copolymer (D) is at least one of a linear structure, a radial structure, and a branched structure, and is a polymer having a block structure in which at least one end is a vinyl aromatic hydrocarbon polymer block. The thermoplastic block copolymer (D) may be a hydrogenated product thereof.
[0039] Examples of the vinyl aromatic hydrocarbons used herein include styrene, α-methylstyrene, vinyltoluene, p-tert-butylstyrene, vinylxylene, ethylvinylxylene, vinylnaphthalene, and mixtures thereof, etc. Of these, styrene is particularly preferred.
[0040] Examples of the olefins that can be used include α-olefins such as ethylene, propylene, and 1-butene, and examples of the diolefins that can be used include conjugated diolefins such as butadiene and isoprene.
[0041] As the thermoplastic block copolymer (D), as long as the block B is predominantly an olefin unit, it is preferable to use a copolymer of either an olefin or a conjugated diolefin with a vinyl aromatic hydrocarbon, and it is more preferable to use a polymer block obtained by polymerizing a conjugated diolefin and hydrogenating it. In the present invention, a thermoplastic block copolymer of a vinyl aromatic hydrocarbon having vinyl aromatic hydrocarbon polymer blocks at both ends and an olefin or a diolefin is preferable, and in particular, a hydrogenated product of a polystyrene-polybutadiene-polystyrene block copolymer (styrene-ethylene / butylene-styrene triblock copolymer, hereinafter referred to as "hydrogenated SEBS") can be particularly preferably used from the viewpoint of improving thermal stability.
[0042] The thermoplastic block copolymer (D) constituting the resin composition of the present invention may be a copolymer consisting of a single component, or a composition containing at least two or more types of copolymers. In particular, since it is a sealant adhesive excellent in moldability and adhesive strength, it is preferably a composition mixture of a hydrogenated styrene-butadiene-diblock copolymer and a hydrogenated styrene-butadiene-styrene-triblock copolymer, and the mixing ratio thereof is preferably 5 / 5 to 9 / 1 calculated as diblock copolymer / triblock copolymer. In addition, the styrene content in the mixture is preferably 10% by weight or more and 50% by weight or less based on the total amount of the thermoplastic block copolymer (D).
[0043] An example of a method for measuring the styrene content is to measure the infrared absorption spectrum of a standard sample with a known styrene content, create a calibration curve using the absorption intensity due to the benzene ring at about 700 cm-1, and then determine the styrene content of a sample with an unknown styrene content from the absorption intensity due to the benzene ring.
[0044] The blending ratio of the thermoplastic block copolymer (D) of vinyl aromatic hydrocarbon and olefin or diolefin constituting the present invention is preferably from 0.5 to 5 parts by weight, more preferably from 1 to 5 parts by weight, and even more preferably from 2 to 4 parts by weight, per 100 parts by weight of the total mixture of the ethylene-vinyl acetate copolymer (A), the tackifier resin (B), and the anti-fogging agent (C).
[0045] The thermoplastic block copolymer (D) of vinyl aromatic hydrocarbon and olefin or diolefin constituting the present invention may be a commercially available product, specifically, for example, Kraton G1726VS, Kraton G1657VS, Kraton G1730VS (all manufactured by Kraton Polymer Co., Ltd.), etc.
[0046] The resin composition of the present invention may contain an ethylene-α-olefin copolymer (E). As the ethylene-α-olefin copolymer (E), any copolymer that is generally within the category of ethylene-α-olefin copolymers may be used. The α-olefin is not particularly limited, but examples thereof include propene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, and 1-dodecane, each of which has 3 to 12 carbon atoms. These ethylene-α-olefin copolymers (E) can be suitably produced by copolymerizing ethylene and an α-olefin using a Ziegler catalyst, a chromium catalyst, or a metallocene catalyst. Examples of the polymerization method include a solution polymerization method, a high-pressure polymerization method, and a gas phase polymerization method.
[0047] The ethylene-α-olefin copolymer (E) constituting the present invention has excellent low-temperature sealing property and sealing strength, and therefore has a density of 860 kg / m as measured according to JIS K6922-1 (1998). 3 More than 910kg / m 3 The following ranges are preferred:
[0048] The blending ratio of the ethylene-α-olefin copolymer (E) constituting the present invention is preferably 5 parts by weight or more and 100 parts by weight or less, more preferably 10 parts by weight or more and 50 parts by weight or less, and even more preferably 18 parts by weight or more and 40 parts by weight or less, based on 100 parts by weight of the total of the mixture of the ethylene-vinyl acetate copolymer (A), the tackifier resin (B) and the anti-fogging agent (C).
[0049] The resin composition of the present invention comprises an ethylene-vinyl acetate copolymer (A), a tackifier resin (B), and an antifogging agent (C), and further comprises 0.5 to 5 parts by weight of a thermoplastic block copolymer (D) containing at least either an olefin or a diolefin as a constituent unit and containing a vinyl aromatic hydrocarbon as a constituent unit, per 100 parts by weight of the total of (A), (B), and the antifogging agent (C), and further comprises a density of 860 kg / m as measured according to JIS K6922-1 (1998). 3 More than 910kg / m3 The composition may contain 5 parts by weight or more and 100 parts by weight or less of an ethylene-α-olefin copolymer (E) in the following range.
[0050] The resin composition of the present invention may be blended with other thermoplastic resins or rubbers, as well as light stabilizers, ultraviolet absorbers, nucleating agents, lubricants, antioxidants, antiblocking agents, flow improvers, release agents, flame retardants, colorants, inorganic neutralizing agents, hydrochloric acid absorbers, fillers, conductive agents, and the like, within the scope of not impairing the effects of the present invention.
[0051] There is no particular restriction on the method for preparing the resin composition of the present invention. For example, the ethylene-vinyl acetate copolymer (A), the tackifier resin (B), the antifogging agent (C) and materials to be added thereto are pre-blended simultaneously in a mixer such as a Henschel mixer or a tumbler, and then melt-kneaded in a single-screw or twin-screw extruder.
[0052] The sealant adhesive according to one embodiment of the present invention will be described in detail below.
[0053] The resin composition of the present invention can be used as an adhesive. In particular, the resin composition can be suitably used as a sealant adhesive for plastic containers mainly composed of resins such as polyethylene terephthalate, polystyrene, polypropylene, polylactic acid, etc., and other various resins, particularly as a lid sealant adhesive. Here, the term "sealant" refers to use for sealing a container. By using the lid sealant adhesive of the present invention, the lid and the container can be sealed.
[0054] Specific examples of materials for the plastic container include polyolefin resins, acrylic resins, polyamide resins, polyester resins, polycarbonate resins, polystyrene resins, styrene-acrylonitrile copolymers, and polyvinyl chloride resins.
[0055] Examples of polyolefin resins include low-density polyethylene, high-density polyethylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, and polypropylene.
[0056] Examples of the acrylic acid resin include polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polybutyl acrylate, polyoctyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, and polyoctyl methacrylate.
[0057] Examples of polyamide resins include nylon 6, nylon 6,6, nylon 11, and nylon 12.
[0058] Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly 3-hydroxybutyrate, and polycaprolactone.
[0059] When the resin composition of the present invention is used as an adhesive for adhering a plastic container containing these materials, the main component of the plastic container may be a single component or a composition of multiple resins. The container may also be a multi-layered laminate in which multiple materials are laminated.
[0060] The resin composition of the present invention can be suitably used for containers made of, inter alia, polyethylene terephthalate, polylactic acid, polystyrene, or polypropylene.
[0061] The covering film, which is one embodiment of the present invention, will be described in detail below.
[0062] When the resin composition of the present invention is used as an adhesive, it is preferably used as an adhesive layer containing the composition (hereinafter referred to as a "sealant adhesive layer"). Furthermore, it can be suitably used as a film for a covering material having a configuration including at least two layers, a supporting substrate layer and a sealant adhesive layer, with the sealant adhesive layer being the outermost layer.
[0063] The supporting substrate constituting the supporting substrate layer is not particularly limited as long as it has self-supporting properties, and examples thereof include olefin-based resins such as polyethylene, polypropylene, ethylene-α-olefin copolymer, ethylene-vinyl acetate copolymer, and saponified ethylene-vinyl acetate copolymer, polyethylene terephthalate, polybutylene terephthalate, polylactic acid (including poly-L-lactic acid, poly-D-lactic acid, copolymers of L-lactic acid and D-lactic acid, and stereocomplexes of poly-L-lactic acid and poly-D-lactic acid), polybutylene succinate, poly(butylene succinate / adipate), polyethylene succinate, poly(butylene Examples of the material include plastic films made of thermoplastic resins such as polyester resins such as poly(3-hydroxybutyrate / hydroxyhexanoate), poly(succinate / terephthalate), poly(butylene adipate / terephthalate), poly(hydroxybutyrate / hydroxyhexanoate), polyglycolic acid, poly(3-hydroxybutyrate), and polycaprolactone; polyamide resins such as nylon 6, nylon 6,6, nylon 11, and nylon 12; paper such as Japanese paper and composite paper; metal foils made of metals such as aluminum; vapor-deposited films in which aluminum or silica is vapor-deposited on the surface of polyester resin films; and films made of these alone or laminates. The thickness of the support substrate layer can be selected according to the application as long as the mechanical strength, workability, and the like are not impaired, but is generally about 5 to 100 μm, and preferably 10 to 50 μm.
[0064] When used as a film for a covering material, the thickness of the sealant adhesive layer can be selected according to the application as long as the adhesiveness, workability, etc. are not impaired, but is generally about 5 to 50 μm, preferably 10 μm to 40 μm, and more preferably 15 to 30 μm.
[0065] In the present invention, an intermediate layer may be provided between the support substrate layer and the sealant adhesive layer to enhance the adhesion between the two layers. The intermediate layer may be composed of components such as thermoplastic resins, such as polyolefins, and thermoplastic elastomers, and these components may be used alone or in combination of two or more. For example, polyolefins include polyethylene and ethylene copolymers (ethylene-α-olefin copolymers, propylene-ethylene copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-methyl acrylate copolymers, etc.) and modified products thereof. The intermediate layer may contain various additives, such as antioxidants, lubricants, antistatic agents, conductive agents, antiblocking agents, and tackifiers, within the scope of the present invention.
[0066] The thickness of the intermediate layer can be selected depending on the application as long as workability is not impaired, but is generally about 5 to 30 μm.
[0067] In the present invention, an anchor coat layer of polyurethane or the like can be provided between the supporting substrate layer and the sealant adhesive layer, or between the supporting substrate layer and the intermediate layer, in order to improve adhesion between the two layers.
[0068] The lid material film having the sealant adhesive layer of the present invention as the outermost layer is suitable as a lid material for various types of plastic containers, including A-PET (amorphous polyethylene terephthalate), polystyrene, polypropylene, polylactic acid, and others, and has high sealing strength and easy peelability.
[0069] There are no particular limitations on the method for producing the covering film, but examples include a method in which the sealant adhesive and the supporting substrate layer are laminated together, and a method in which the sealant adhesive and the supporting substrate layer are co-extruded together.
[0070] Examples of lamination methods include: (1) an extrusion lamination method in which an anchor coating agent is applied to a supporting substrate layer, and an adhesive layer is melt-extruded; (2) an extrusion lamination method in which an anchor coating agent is applied to a supporting substrate layer, and an intermediate layer is melt-extruded, and then an adhesive layer for a sealant is melt-extruded thereon; (3) an extrusion lamination method in which an intermediate layer made of an ethylene-methacrylic acid copolymer, an ethylene-methyl methacrylate copolymer, or the like, which has excellent adhesion to the supporting substrate, is melt-extruded onto the supporting substrate layer, and then an adhesive layer for a sealant is melt-extruded thereon; (4) a co-extrusion lamination method in which an anchor coating agent is applied to a supporting substrate layer, and then the intermediate layer and the adhesive layer are melt-extruded simultaneously; and (5) Examples of the method include a coextrusion lamination method in which an intermediate layer made of an ethylene-methacrylic acid copolymer or an ethylene-methyl methacrylate copolymer, which has excellent adhesion to the support substrate, and a sealant adhesive layer are simultaneously melt-extruded onto the support substrate layer, (6) a dry lamination method in which a film containing at least one layer of sealant adhesive is formed in advance by an inflation molding method or a cast molding method, and then laminated to a support substrate layer coated with an anchor coating agent, and (7) a sandwich extrusion lamination method in which an intermediate layer is melt-extruded using an extrusion lamination to laminate between a support substrate layer coated with an anchor coating agent and a film containing at least one layer of sealant adhesive. On the other hand, examples of the method of coextrusion of a sealant adhesive and a support substrate layer include a coextrusion inflation method and a coextrusion T-die method. EXAMPLES
[0071] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0072] (Measurement of molecular weight of ethylene-vinyl acetate copolymer (A)) The weight average molecular weight (Mw) and number average molecular weight (Mn) of the ethylene-vinyl acetate copolymer (A) were determined by gel permeation chromatography under the conditions shown below, using a universal calibration curve measured with monodisperse polystyrene, and calculated as the molecular weight of linear polyethylene. Model: Waters 150C ALC / GPC Solvent: 1,2,4-trichlorobenzene Flow rate: 1ml / min Temperature: 140℃ Measured concentration: 30mg / 30ml Injection volume: 100μl Column: 3 TSKgel GMH HR-H columns manufactured by Tosoh Corporation Qw was calculated from the obtained weight average molecular weight (Mw) and number average molecular weight (Mn).
[0073] The moldability of the resin compositions and the films for covering materials obtained in the examples were measured for adhesive strength, anti-fogging properties, and slip properties by the methods described below.
[0074] (Evaluation of moldability) The resin composition pellets were extrusion laminated at a processing temperature of 250°C using an extrusion laminator (manufactured by Placo Corporation, screw diameter 25 mmφ) and the releasability from the lamination roll (peelability from the roll, presence or absence of peeling marks on the film) was evaluated. The test was judged based on the following criteria: ◯: good releasability, ×: difficult to peel, or peeling marks were observed on the film.
[0075] (Adhesive strength measurement) The adhesive surface of the covering film was placed on a 0.35 mm thick A-PET sheet (Minelon Chemical Industry Co., Ltd.) and pressure-heated and bonded using a heat seal tester (Tester Sangyo Co., Ltd., TP-701 model) at 170°C, 0.2 MPa, and 1 second. After cooling, the seal strength was measured at a peel angle of 180° and a peel speed of 300 mm / min. The PS, PP, and polylactic acid (PLA) sheets with the thicknesses described below were also measured under the same conditions.
[0076] (Measurement of anti-fogging properties) 20 ml of hot water at 80° C. was poured into a 200 ml polypropylene container, the opening of the container was covered with a lid film, and the degree of cloudiness and the state of water droplets on the surface of the lid were observed. The test was judged as follows: ◯ (no water droplets, transparent), △ (some water droplets, but almost transparent), × (completely cloudy or opaque with water droplets).
[0077] (Measurement of slipperiness) The biaxially oriented polyester film surface and the adhesive layer surface of the covering film were overlapped and rubbed together by hand to evaluate slip properties. The test was judged based on the following criteria: ◯ - slips without resistance, △ - there is some resistance but it slips, and × - it does not slip at all.
[0078] Example 1 The ethylene-vinyl acetate copolymer (A) was 84.9 parts by weight of a resin (A-1) having a vinyl acetate content of 5.0%, a melt mass flow rate of 1.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 3.8. The tackifier resin (B) was 15 parts by weight of a fully hydrogenated petroleum resin (B-1) (manufactured by Arakawa Chemical Industries, Ltd., product name Alcon P125; softening temperature 125°C). The anti-fogging agent (C) was a diglycerol fatty acid ester (C-1) (manufactured by Riken Vitamin Co., Ltd., product name Alcon P125; softening temperature 125°C) obtained by esterification of polyglycerin obtained by polymerizing glycerin with stearic acid, whose fatty acid residue is a saturated fatty acid and has 18 carbon atoms. After pre-blending 0.1 parts by weight of Rikemal S-71D in a tumbler mixer, the mixture was melt-kneaded at 180°C in a twin-screw extruder to obtain pellets of the resin composition. In addition, in consideration of thermal stability, 0.05 parts by weight of a phenolic antioxidant (manufactured by BASF Ltd., product name Irganox 1010) was added to the resin composition per 100 parts by weight of the sealant adhesive. Thereafter, the resin composition pellets were extrusion laminated at a processing temperature of 250°C using an extrusion laminator (manufactured by Placo Corporation, screw diameter 25 mmφ) onto the low-density polyethylene surface of the two-layer film, which had previously been extrusion laminated with a biaxially oriented polyester film (thickness 12 μm) serving as a supporting substrate layer and a low-density polyethylene intermediate layer (thickness 25 μm, product name Petrothene 203, manufactured by Tosoh Corporation), to obtain a lid material film with a resin composition layer thickness of 25 μm. The evaluation results of the obtained resin composition and the covering film are shown in Table 1.
[0079] Example 2 A resin composition and a film for a covering material were obtained in the same manner as in Example 1, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.9 parts by weight to 84.7 parts by weight, and the blending ratio of the anti-fogging agent (C-1) was changed from 0.1 parts by weight to 0.3 parts by weight. The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0080] Example 3 A resin composition and a film for a lid material were obtained in the same manner as in Example 2, except that the resin composition of the ethylene-vinyl acetate copolymer (A-1), tackifier resin (B-1), and anti-fogging agent (C-1) of Example 2 was further blended with 3 parts by weight of a thermoplastic block copolymer (D-1) (Kraton G1726VS) of vinyl aromatic hydrocarbon and diolefin, in which the mixing ratio of hydrogenated styrene-butadiene-diblock copolymer and hydrogenated styrene-butadiene-styrene-triblock copolymer is 7 / 3 and the styrene content is 30% by weight. The evaluation results of the obtained resin composition and the covering film are shown in Table 1.
[0081] Example 4 A resin composition and a film for a covering material were obtained in the same manner as in Example 3, except that 0.3 parts by weight of a glycerin fatty acid ester (C-2) (manufactured by Riken Vitamin Co., Ltd., product name Rikemal S-100) obtained by esterification reaction of stearic acid, whose fatty acid residue is a saturated fatty acid and has 18 carbon atoms, with monoglycerin, was added instead of 0.3 parts by weight of the anti-fogging agent (C-1). The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0082] Example 5 A resin composition and a film for a covering material were obtained in the same manner as in Example 3, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.7 parts by weight to 84.5 parts by weight, and 0.3 parts by weight of the anti-fogging agent (C-1) was changed to 0.5 parts by weight of an amine compound (C-3) (manufactured by Lion Corporation, trade name Armostat 310). The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0083] Example 6 A resin composition and a film for a covering material were obtained in the same manner as in Example 3, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.7 parts by weight to 84.5 parts by weight, and 0.3 parts by weight of the anti-fogging agent (C-1) was replaced with 0.5 parts by weight of a sorbitan fatty acid ester (C-4) (manufactured by Riken Vitamin Co., Ltd., product name Rikemal S-300) obtained by esterification reaction of stearic acid, a saturated fatty acid having a carbon number of 18, and sorbitan.
[0084] Example 7 A resin composition and a film for a lid material were obtained in the same manner as in Example 3, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.7 parts by weight to 84.5 parts by weight, and 0.3 parts by weight of the anti-fogging agent (C-1) was replaced with 0.5 parts by weight of an organic sulfonate salt (C-5) (manufactured by Miyoshi Oil Co., Ltd., product name: Dasper 802D). The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0085] Example 8 A resin composition and a film for a covering material were obtained in the same manner as in Example 3, except that the blending ratio of the anti-fog agent (C-1) was changed from 0.1 parts by weight to 0.15 parts by weight as the anti-fog agent (C), and 0.15 parts by weight of an amine compound (C-3) was further blended. The evaluation results of the obtained resin composition and covering film are shown in Table 1.
[0086] Example 9 A resin composition and a film for a covering material were obtained in the same manner as in Example 3, except that 84.7 parts by weight of a resin (A-2) having a vinyl acetate content of 7.5%, a melt mass flow rate of 2.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 4.2 was blended in place of 84.7 parts by weight of the ethylene-vinyl acetate copolymer (A-1). The evaluation results of the obtained resin composition and covering film are shown in Table 2.
[0087] Example 10 The resin composition of Example 2 was mixed with 3 parts by weight of a thermoplastic block copolymer (D-1), and an ethylene-α-olefin copolymer (E) was a random copolymer of ethylene and propylene having a density of 860 kg / m 3 A resin composition and a film for covering material were obtained in the same manner as in Example 2, except that 20 parts by weight of an ethylene-α-olefin copolymer (E-1) (manufactured by Mitsui Chemicals, Inc., trade name Tafmer P-0375) was added. The evaluation results of the obtained resin composition and covering film are shown in Table 2.
[0088] Example 11 Using the resin composition and the film for covering material obtained by the method of Example 2, the adhesive strength was measured in the same manner as described in (Measurement of adhesive strength) except that a PS sheet having a thickness of 0.4 mm was used instead of the A-PET sheet. The evaluation results of the obtained resin composition and covering film are shown in Table 2.
[0089] Example 12 The adhesive strength of the covering film obtained in the method of Example 3 was measured in the same manner as in Example 11. The evaluation results of the obtained resin composition and covering film are shown in Table 2.
[0090] Example 13 Using the resin composition and the film for covering material obtained by the method of Example 2, the adhesive strength was measured in the same manner as described in (Measurement of adhesive strength) except that a 0.3 mm PP sheet was used instead of the A-PET sheet. The evaluation results of the covering film are shown in Table 2.
[0091] Example 14 Using the covering film obtained by the method of Example 3, the adhesive strength was measured in the same manner as in Example 13. The evaluation results of the covering film are shown in Table 2.
[0092] Example 15 Using the resin composition and the covering film obtained by the method of Example 2, the adhesive strength was measured in the same manner as described in (Measurement of adhesive strength) except that a 0.3 mm PLA sheet was used instead of the A-PET sheet. The evaluation results of the covering film are shown in Table 2.
[0093] Example 16 The adhesive strength of the covering film obtained in the method of Example 3 was measured in the same manner as in Example 15. The evaluation results of the covering film are shown in Table 2.
[0094] Comparative Example 1 A sealant adhesive and a covering film were obtained in the same manner as in Example 1, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.9 parts by weight to 85 parts by weight, and the blending ratio of the anti-fogging agent (C-1) was changed from 0.1 parts by weight to 0 parts by weight. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained resin composition and the film for a covering material were poor in moldability, anti-fogging property and slip property.
[0095] Comparative Example 2 A sealant adhesive and a covering film were obtained in the same manner as in Example 1, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.9 parts by weight to 84.95 parts by weight, and the blending ratio of the anti-fogging agent (C-1) was changed from 0.1 parts by weight to 0.05 parts by weight. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained resin composition and the film for a covering material were poor in moldability, anti-fogging property and slip property.
[0096] Comparative Example 3 A sealant adhesive and a covering film were obtained in the same manner as in Example 1, except that the blending ratio of the ethylene-vinyl acetate copolymer (A-1) was changed from 84.9 parts by weight to 82 parts by weight, and the blending ratio of the anti-fogging agent (C-1) was changed from 0.1 parts by weight to 3 parts by weight. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained resin composition and the film for a covering material were poor in adhesive strength.
[0097] Comparative Example 4 A sealant adhesive and a covering film were obtained in the same manner as in Example 2, except that 84.7 parts by weight of the ethylene-vinyl acetate copolymer (A-1) was replaced with 84.7 parts by weight of a resin (A-3) having a vinyl acetate content of 7.5%, a melt mass flow rate of 2.0 g / 10 min, and a ratio Qw of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of 6.4. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained resin composition and the film for a covering material were poor in adhesive strength.
[0098] Comparative Example 5 A sealant adhesive and a covering film were obtained in the same manner as in Example 2, except that 84.7 parts by weight of ethylene-vinyl acetate copolymer (A-1) was replaced with 84.7 parts by weight of ethylene-vinyl acetate copolymer (A-4) (manufactured by Tosoh Corporation, product name Ultrathene 537) having a vinyl acetate content of 5.5%, a melt mass flow rate of 8.5 g / 10 min, and a ratio Qw of weight average molecular weight (Mw) to number average molecular weight (Mn) of 5.8. The evaluation results of the obtained resin composition and the film for a covering material are shown in Table 3. The obtained resin composition and the film for a covering material were poor in adhesive strength.
[0099] By comparing the examples of the present invention with the comparative examples, it is clear that a resin composition containing an ethylene-vinyl acetate copolymer having both VA and Qw of the present invention has higher adhesive strength and superior anti-fogging properties than a composition containing the same amount of a composition containing a single component or multiple components of an ethylene-vinyl acetate copolymer not having both VA and Qw.
[0100] [Table 1]
[0101] [Table 2]
[0102] [Table 3]
Claims
1. An adhesive for sealants comprising a resin composition comprising 58 to 94.9 parts by weight of ethylene-vinyl acetate copolymer (A) having a vinyl acetate content (VA) of 3 to 13% by weight and a ratio Qw of weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.5 to 4.5, 5 to 40 parts by weight of a tackifier resin (B), and 0.1 to 2% by weight of an anti-fogging agent (C) (wherein the total of (A), (B), and (C) is 100 parts by weight).
2. The sealant adhesive described in claim 1, further comprising, per 100 parts by weight of the resin composition, 0.5 parts by weight or more and 5 parts by weight or less of a thermoplastic block copolymer (D) which further contains at least one of an olefin or a diolefin as a constituent unit and contains a vinyl aromatic hydrocarbon as a constituent unit.
3. The sealant adhesive according to claim 1, comprising 5 parts by weight or more and 100 parts by weight or less of an ethylene-α-olefin copolymer (E) having a density in the range of 860 kg / m 3 or more and 910 kg / m 3 or less, measured in accordance with JIS K6922-1 (1998), relative to 100 parts by weight of the resin composition.
4. The sealant adhesive according to claim 1, comprising, per 100 parts by weight of the resin composition, 0.5 to 5 parts by weight of a thermoplastic block copolymer (D) which contains at least either an olefin or a diolefin as a constituent unit and which contains a vinyl aromatic hydrocarbon as a constituent unit, and further comprising 5 to 100 parts by weight of an ethylene-α-olefin copolymer (E) having a density in the range of 860 to 910 kg / m3 as measured in accordance with JIS K6922-1 (1998).
5. A sealant adhesive described in any one of claims 1 to 4, wherein the tackifier resin (B) is at least one type selected from the group consisting of aliphatic petroleum resins, aromatic petroleum resins, alicyclic hydrogenated petroleum resins, and copolymer petroleum resins.
6. A sealant adhesive described in any one of claims 1 to 5, wherein the anti-fogging agent (C) is at least one member selected from the group consisting of ethylene oxide adducts, amine compounds and organic sulfonates.
7. A sealant adhesive described in any one of claims 1 to 6, which is used for at least one type of container selected from the group consisting of polyethylene terephthalate, polystyrene, polypropylene, and polylactic acid.
8. A film for use as a covering material for containers, which is composed of at least two layers, the film comprising a layer containing the sealant adhesive according to any one of claims 1 to 6 and a supporting substrate layer.
Citation Information
Patent Citations
Polyolefin film for stretch wrapping
JP1977107043A
Resin composition for polypropylene film having improved fog resistance
JP1983079044A
Production of readily openable sealed film having Anti-fogging property imparted thereto
JP1992103639A
Co-extruded adhesive film
JP1994328632A
Thermoplastic resin composition
JP1999269319A