Polymer Electrolytes

A polymer electrolyte with optimized polyarylene sulfide copolymer and alkali metal salt structure addresses low conductivity and hygroscopicity issues, offering high ionic conductivity, wide potential window, and improved productivity for high-voltage batteries.

JP7571547B2Active Publication Date: 2024-10-23TORAY INDUSTRIES INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021001900
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-05
Filing Date
2021-01-08
Publication Date
2024-10-23
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Conventional polymer-based solid electrolytes face issues with low ionic conductivity at room temperature, high hygroscopicity, poor mechanical properties, and environmental unsuitability due to high-temperature processing, which affects productivity and safety, especially in high-voltage battery applications.

Method used

A polymer electrolyte comprising an alkali metal salt, an ionization aid, and a polyarylene sulfide copolymer with specific structural units, optimized for low crystallinity and low processing temperatures, enhances ionic conductivity and reduces hygroscopicity, while using environmentally friendly ionization aids.

Benefits of technology

The polymer electrolyte achieves good ionic conductivity at room temperature, wide potential window, low moisture absorption, and improved productivity, making it suitable for high-voltage battery applications with enhanced safety and environmental compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571547000001
    Figure 0007571547000001
  • Figure 0007571547000002
    Figure 0007571547000002
  • Figure 0007571547000003
    Figure 0007571547000003
Patent Text Reader

Abstract

To provide a polymer electrolyte that exhibits good ion conductivity even in a room temperature environment and has excellent productivity.SOLUTION: The polymer electrolyte includes: an alkali metal salt; a dissociation auxiliary agent; and polyarylene sulfide, where the polyarylene sulfide is a polyarylene sulfide copolymer composed of a constitutional unit represented by the formula: -(Ar-S)-, where Ar has a constitutional unit represented by a predetermined chemical formula, and at least one constitutional unit selected from the group consisting of other predetermined chemical formulae. The predetermined chemical formula has two substituent groups selected from an alkyl group, an alkoxy group, an amino group, and a hydroxyl group, and the other predetermined chemical formulae have two or more substitutional groups selected from hydrogen, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer electrolyte. [Background technology]

[0002] In recent years, alkaline secondary batteries, including lithium secondary batteries, have been used for a variety of purposes, such as portable devices such as smartphones and mobile phones, hybrid vehicles, electric vehicles, and home electricity storage devices, and research and development into these batteries is being actively conducted.

[0003] There is a strong demand for improved safety in lithium secondary batteries, especially for use in electric vehicles. Conventional electrolyte batteries use flammable electrolytes, which can lead to battery combustion or explosion. For this reason, research into solid electrolytes that can contribute to improved safety has become active.

[0004] Solid electrolytes are solids that easily conduct ions, and are generally divided into oxide-based, sulfide-based, and polymer-based solid electrolytes. Polymer-based solid electrolytes have been attracting attention due to their advantages such as productivity and flexibility, but they have low ionic conductivity at room temperature, and a solution to this problem is required.

[0005] In recent years, among polymer-based solid electrolytes, polyarylene sulfide (hereinafter abbreviated as PAS)-based electrolytes, represented by polyphenylene sulfide (hereinafter abbreviated as PPS), have been attracting attention for their flame retardancy and mechanical properties. As in Patent Document 1, it is known that PPS is a conjugated polymer and can be made electronically conductive by adding an electron-accepting dopant, and in recent years, Patent Documents 2 to 4 disclose solid electrolytes in which a mixture of PPS and an alkali metal salt is doped with an electron acceptor. Furthermore, in Patent Documents 2 to 4, the PPS solid electrolyte is produced by a method in which raw materials such as PPS, an alkali metal salt, and an electron-accepting dopant are mixed at high temperature and then molded.

[0006] In addition, a method is known in which an electrolyte solution is added to a solid electrolyte polymer to improve ionic conductivity (Patent Documents 5 to 6). The electrolyte produced by this method is called Polymer Matrix Ectrolyte (PME). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Publication No. 59-157151 [Patent Document 2] US Patent Application Publication No. 2018 / 006308 [Patent Document 3] China Patent Application Publication No. 106450424 [Patent Document 4] US Patent Application Publication No. 2017 / 0005356 [Patent Document 5] Taiwan Patent Application Publication No. 202015279 [Patent Document 6] US Patent Application Publication No. 2006 / 0177740 Summary of the Invention [Problem to be solved by the invention]

[0008] In Patent Documents 2 to 4, it has been shown that a high degree of crystallinity of a solid electrolyte containing PPS is important for ionic conductivity, and a solid electrolyte using PPS with a high degree of crystallinity has been disclosed. However, when using PPS with a high degree of crystallinity, it must be processed at a high temperature of around 300°C, which causes deterioration of the components contained therein, such as lithium salts and dopants, and may cause a decrease in ionic conductivity at room temperature and instability of quality. In addition, the inclusion of an electron-accepting dopant may cause a decrease in mechanical properties such as oxidative deterioration and embrittlement of the polymer matrix. Furthermore, when producing the solid electrolyte, if a decrease in mechanical properties occurs due to high-temperature processing, the film may crack or collapse during film formation, which is a problem in productivity. In Patent Documents 5 to 6, since the solvent casting method is used to prepare PME, a process of evaporating the solvent is required in the manufacturing process of PME, which is a problem in productivity. In addition, while the solvent for dissolving the polymer does not contribute to improving the conductivity of the polymer electrolyte, there is a problem that the raw material cost increases and productivity decreases. In addition, the evaporated solvent may dissipate into the environment, which is also a problem in environmental suitability. From this perspective, conventional PME electrolytes have problems in terms of productivity and environmental compatibility.

[0009] In addition, the polyimide (PI) described in Patent Document 6 has a problem that it is easily hygroscopic as a base material for a polymer electrolyte. When the polymer electrolyte contains water as an ionization assistant, the ratio of the components of the polymer electrolyte may change due to moisture absorption, which may decrease the potential window of the polymer electrolyte and make water more susceptible to electrolysis. On the other hand, when the polymer electrolyte contains an organic solvent as an ionization assistant, deterioration such as electrolysis of the ionization assistant due to moisture absorption occurs. From the above viewpoint, there are problems with storage and preservation. In addition, a general PI base material has a problem that the potential window of electrolysis is less than 2V, making it difficult to apply to high-voltage battery applications. [Means for solving the problem]

[0010] As a result of intensive research aimed at solving the above problems, the inventors have found a polymer electrolyte that exhibits good ionic conductivity at room temperature, has low hygroscopicity, and is excellent in terms of productivity, environmental suitability, wide potential window, etc., and have completed the present invention.

[0011] That is, in order to solve the above problems, the present invention comprises the following configuration.

[0012] (1) A polymer electrolyte containing an alkali metal salt, an ionization assistant, and a polyarylene sulfide, wherein the polyarylene sulfide is a polyarylene sulfide copolymer having a structural unit of the formula -(Ar-S)-, and Ar has a structural unit represented by (A) in chemical formula (1) and at least one structural unit selected from the group consisting of (B) to (G) in chemical formula (1).

[0013] [ka]

[0014] (R1 and R2 are substituents selected from an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R1 and R2 may be the same or different. R3 and R4 are substituents selected from a hydrogen atom, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R3 and R4 may be the same or different. Y is selected from an alkylene group, O, CO, SO, and SO2.) (2) The polymer electrolyte according to (1), wherein the ionization assistant contains one or more solvents having a degree of ionic dissociation (1-ξ) at 25°C of 0.1 or more, as calculated by the formula (1), and a solvent diffusion coefficient at 25°C of 15 or less, as calculated by the formula (2).

[0015]

number

[0016]

number

[0017] (3) The polymer electrolyte according to (1) or (2), wherein the ionization assistant comprises at least one selected from the group consisting of water, gamma-butyrolactone, N-methylpyrrolidone (NMP), butylene carbonate (BC), ethylene carbonate (EC), propylene carbonate (PC), methyl-gamma-butyrolactone (GVL), triglyme (TG), diglyme (DG), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).

[0018] (4) The polymer electrolyte according to any one of (1) to (3), wherein the alkali metal salt comprises one or more of LIFSI and LITFSI.

[0019] (5) A battery comprising the polymer electrolyte according to any one of (1) to (4). Effect of the Invention

[0020] According to the present invention, it is possible to provide a polymer electrolyte which exhibits good ionic conductivity even at room temperature, has low hygroscopicity, is excellent in productivity and environmental suitability, and has a wide potential window. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] (Definition of Polymer Electrolyte) The polymer electrolyte of the present invention refers to a substance that has a polymer matrix and easily migrates ions when an electric field is applied from the outside. The polymer electrolyte contains an ionization assistant described below. The ease of migration of alkali metal ions in the polymer electrolyte of the present invention can be judged by the ion diffusion coefficient at 25°C. The ion diffusion coefficient (m 2 / s) may be measured by nuclear magnetic resonance spectroscopy (NMR) of the ion.

[0022] In addition, since the ion diffusion coefficient measured by NMR may take multiple values ​​even under the same temperature conditions, the ion diffusion coefficient in the present invention refers to the maximum ion diffusion coefficient of the ion at 25° C. From the viewpoint of ion conductivity, the ion diffusion coefficient of the polymer electrolyte of the present invention at 25° C. is 10 -13 m 2 / s or more is preferable, and 10 -12 m 2 / s or more is more preferable, and 10 -11 m 2 / s or more is more preferable. The polymer electrolyte of the present invention contains an alkali metal salt, an ionization assistant, and polyarylene sulfide (hereinafter, sometimes referred to as PAS). The alkali metal salt, the ionization assistant, and the PAS will be described below.

[0023] (alkali metal salts) It is important that the polymer electrolyte of the present invention contains an alkali metal salt from the viewpoint of ion conductivity. The alkali metal salt in the present invention refers to a salt containing an alkali metal ion as a constituent ion. For example, metal salts containing lithium metal ions, sodium metal ions, potassium metal ions, etc. are included. From the viewpoint of ion diffusibility, metal ions with small ion diameters are preferred.

[0024] The anion is preferably a soft base based on the HSAB rule because of its high dissociation property into ions, and is preferably a bis(trifluoromethanesulfonyl)imide anion or a bis(fluorosulfonyl)imide anion. That is, the alkali metal salt preferably contains at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethane)sulfonimide.

[0025] The HSAB rule (Principle of Hard and Soft Acids and Bases) is a classification of acids and bases proposed by R.G. Pearson in terms of their strength. Hard acids have a high affinity for hard bases, and soft acids have a high affinity for soft bases. A hard acid is an acid whose electron acceptor atom is small, has no valence electrons in an orbit that can be easily deformed, and has a large positive charge. A soft acid is an acid whose electron acceptor atom is large, has valence electrons in an orbit that can be easily deformed, and has no or only a small charge. A hard base is a base whose valence electrons are strongly bonded to the atom, and a soft base is a base whose valence electrons are easily polarized. The HSAB rule and the classification of acids and bases according to the HSAB rule are described in Chapter 9, Section 15 on Acids and Bases in "Inorganic Chemistry - A Guide to Advanced Study" by R.B. Heslop and K. Jones.

[0026] Specifically, the alkali metal salt preferably contains lithium salts and sodium salts, and more preferably contains one or more selected from lithium hydroxide (LiOH), lithium carbonate (LiCO3), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalate)borate (LiBOB), sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium bis(fluorosulfonyl)imide (NaFSI), and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI). From the viewpoint of high ion dissociability, it is even more preferable to contain LiTFSI and one or more obtained from LiFSI.

[0027] Moreover, a plurality of types of alkali metal salts may be mixed in an appropriate ratio for use.

[0028] From the viewpoint of the degree of ion dissociation and ion conductivity, the molar ratio of all constitutional units to the alkali metal salt in the polymer is preferably 100:2 to 100:400, more preferably 100:2 to 100:100, and even more preferably 100:2 to 100:50.

[0029] (Ionization agent) The ionization assistant contained in the polymer electrolyte of the present invention includes a solvent. From the viewpoint of dissociation of the alkali metal salt and ionic conductivity, it is important that this solvent is as follows: That is, this solvent has a degree of ionic dissociation (1-ξ) at 25°C obtained by formula (1) of 0.1 or more, and a solvent diffusion coefficient (Dsolvent) obtained by formula (2) of 15 or less.

[0030]

number

[0031]

number

[0032] The degree of ionic dissociation (1-ξ) obtained by formula (1) may vary depending on the ionization assistant, temperature, ion concentration, and ion type. Here, the degree of ionic dissociation is calculated for a temperature of 25°C, an ion concentration of 0.2 mol / L, a cation of lithium ion, and an anion of N(SO2CF3)2 - This refers to the degree of ionic dissociation when

[0033] The notations in formula (1) and formula (2) represent the following values. σ imp : ionic conductivity, e0: electron charge, N: Avogadro constant, k: Boltzmann constant, T: temperature, D Lithium : Diffusion coefficient of lithium ions, D Anion :N(SO2CF3)2 - Diffusion coefficient of , (1-ξ): degree of ion dissociation, D solvent : Solvent diffusion coefficient, c: Boundary condition constant, η: Viscosity, r a : Spread radius.

[0034] The ionization assistant can combine with lithium ions at the interface or amorphous portion of the polymer electrolyte to form a third phase having better ionic conductivity than the polymer matrix, forming a conductive path and improving the ionic conductivity of the polymer electrolyte.

[0035] The degree of ionic dissociation (1-ξ) obtained by formula (1) indicates the rate of ionic dissociation. From the viewpoint of promoting dissociation of the alkali metal salt, the degree of ionic dissociation (1-ξ) of the solvent obtained by formula (1) is preferably 0.1 or more.

[0036] In addition, the solvent diffusion coefficient (Dsolvent) obtained by formula (2) indicates the viscosity of the solvent, and the lower this value, the higher the ion conductivity of the alkali metal ion tends to be. From the above viewpoint, the solvent diffusion coefficient (Dsolvent) obtained by formula (2) of the solvent is preferably 15 or less.

[0037] From the above viewpoint, it is preferable that the ionization assistant contains one or more solvents having a degree of ion dissociation (1-ξ) obtained by the above formula (1) of 0.1 or more and a solvent diffusion coefficient (Dsolvent) obtained by the above formula (2) of 15 or less.

[0038] From the same viewpoint, the ionization assistant preferably contains one or more selected from the group consisting of water, gamma-butyrolactone (GBL), n-methylpyrrolidone (NMP), butylene carbonate (BC), ethylene carbonate (EC), propylene carbonate (PC), methyl-gamma-butyrolactone (GVL), triglyme (TG), diglyme (DG), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Among them, from the viewpoint of the potential window of the electrolyte, the ionization assistant more preferably contains at least one of gamma-butyrolactone (GBL) and n-methylpyrrolidone (NMP), and from the viewpoint of the affinity with the above-mentioned polymer, the ionization assistant most preferably contains gamma-butyrolactone (GBL).

[0039] (Polyarylene sulfide) The PAS (arylene group is abbreviated as "Ar") in the present invention is a polymer having a structural unit of the formula -(Ar-S)-. Furthermore, Ar in the structural unit -(Ar-S)- has a structural unit (A) in chemical formula (1) and at least one structural unit selected from the group consisting of (B) to (G) in chemical formula (1). From the viewpoint of controlling the melting point and molecular weight, it is particularly preferable that Ar has a structural unit (B) in chemical formula (1) or a structural unit (C) in chemical formula (1).

[0040] [ka]

[0041] (R1 and R2 are substituents selected from an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R1 and R2 may be the same or different. R3 and R4 are substituents selected from a hydrogen atom, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R3 and R4 may be the same or different. Y is selected from an alkylene group, O, CO, SO, and SO2.) Furthermore, the proportion of copolymer units (-(Ar-S)- in which Ar has at least one structural unit selected from the group consisting of (B) to (G) of chemical formula (1) per mole of structural units represented by -(Ar-S)- is preferably 1 mol % or more and 50 mol % or less, more preferably 3 mol % or more and 30 mol % or less, and even more preferably 5 mol % or more and 25 mol % or less. When the copolymerization unit is 1 mol % or more, the melting point of the PAS is significantly lowered, and the processing temperature when producing a solid electrolyte can be lowered, leading to improved ionic conductivity and quality stability of the polymer electrolyte. On the other hand, when the proportion is 50 mol % or less, recovery of the PAS copolymer from the reaction solution after completion of the polymerization reaction of the PAS copolymer tends to be more efficient. The content ratio of copolymerization units in the PAS copolymer is the same as the ratio of the amount of the compounds (B') to (G') added as copolymerization components to the total amount of the dihalogenated aromatic compounds represented by (A') to (G') of chemical formula (2) added during polymerization.

[0042] [ka]

[0043] As long as the unit represented by -(Ar-S)- is the main structural unit, it may contain branch units or crosslinking units represented by (H) to (J) in the following chemical formula (3). The copolymerization amount of these branch units or crosslinking units is preferably in the range of 0 to 1 mol % per 1 mol of the structural unit represented by -(Ar-S)-.

[0044] [ka]

[0045] The PAS copolymer in the present invention may be any one of a random copolymer, a block copolymer, and a mixture thereof.

[0046] The method for synthesizing the PAS copolymer for solid electrolytes of the present invention is not particularly limited, and examples thereof include a method in which a sulfidizing agent is reacted with a dihalogenated aromatic compound in an organic polar solvent, and a method in which a diiodo aromatic compound is melt-reacted with sulfur in the absence of a solvent. From the viewpoint of versatility, however, it is preferable to adopt the former polymerization method, which is industrially produced.

[0047] (Crystallization degree) Here, the crystallinity of the polymer electrolyte refers to the crystallinity in a state in which the polymer electrolyte does not contain an ionization assistant. From the viewpoints of melting point, processability, and impregnation of the ionization assistant, the polymer contained in the polymer electrolyte of the present invention preferably has a crystallinity of 20% or less.

[0048] The degree of crystallinity generally refers to the proportion of crystalline regions in the entire polymer, but here, the value obtained by dividing the heat of crystalline fusion of the polymer electrolyte before impregnation with the ionization assistant by the heat of fusion of perfectly crystalline paraphenylene sulfide (146.2 J / g) is regarded as the degree of crystallinity of the polymer.

[0049] It is known from Patent Document 1 and the like that a high degree of crystallinity of a polymer electrolyte is important for ionic conductivity. By lowering the degree of crystallinity, the melting point of the polymer tends to be lower, making it possible to process it at a low temperature, suppressing the decomposition of lithium salts, oxidation and crosslinking of the polymer, etc., increasing the affinity with the ionization assistant, and facilitating the formation of conductive paths, so that high ionic conductivity can be achieved even with a low degree of crystallinity.

[0050] In addition, when the crystallinity is low, the temperature required to mold the polymer electrolyte is lower. In particular, when a component such as an alkali metal salt is contained, the process of mixing the components and molding can be carried out successively or simultaneously.

[0051] From the above viewpoints, the crystallinity of the polymer electrolyte in the present invention is preferably 20% or less, more preferably 15% or less. The crystallinity of the polymer electrolyte in the present invention can be measured by a differential scanning calorimeter (DSC). Specifically, the polymer electrolyte is heated from 25°C to 120°C at a rate of 10°C / min under a nitrogen atmosphere and kept at 120°C for 2 hours. Then, the temperature is raised to 400°C at a rate of 10°C / min, and the peak with the widest area among the obtained endothermic peaks is regarded as the melting peak, and the heat of fusion (J / g) calculated from the melting peak area is divided by 146.2 (J / g) to obtain the crystallinity (%).

[0052] (Melting Point) The melting point of the polymer electrolyte here refers to the melting point in a state in which the ionization assistant is not contained. The melting point of the polymer electrolyte is preferably 200°C or more and 320°C or less from the viewpoints of moldability, productivity, and quality stability. The low melting point of the polymer electrolyte allows mixing at a lower temperature, and sublimation and deterioration of the raw materials can be prevented. In addition, when there are raw materials that are prone to sublimation in a molten state, it is necessary to mix each raw material with the polymer separately to prevent sublimation, but the low melting point of the polymer electrolyte allows melt mixing in one go. This simplifies the process. From the above viewpoints, the melting point of the polymer electrolyte in the present invention is preferably 200°C or more and 320°C or less, more preferably 200°C or more and 280°C or less, and even more preferably 200°C or more and 250°C or less. The melting point of the polymer electrolyte in the present invention is measured as follows. The polymer electrolyte is heated from 25°C to 120°C at a rate of 10°C / min in a nitrogen atmosphere and held at 120°C for 2 hours. The temperature is then increased to 400° C. at a rate of 10° C. / min., and the endothermic peak having the widest area is regarded as the melting peak, and the peak temperature of the melting peak is regarded as the melting point.

[0053] (Ionic Conductivity) From the viewpoint of the ionic conductivity as an electrolyte for battery applications and the charge / discharge performance of the battery, the ionic conductivity of the polymer electrolyte of the present invention is 10 -6 From the same viewpoint, it is preferable that the viscosity is 10 -5 More preferably, it is 10 S / cm or more. -4 It is more preferable that the ionic conductivity of the polymer electrolyte is 25° C. or more.

[0054] The ionic conductivity can be measured by the following method. The polymer electrolyte is sampled in a circle with a diameter of 10 mm to be used as a measurement sample. The thickness of this sample is measured with a micrometer, and then the sample is placed on a sample holder. Using a high-frequency impedance measurement system (4990EDMS-120K manufactured by Toyo Corporation), an AC voltage of 100 Hz to 100 MHz is applied to measure the ionic conductivity by the complex impedance method. The lithium ion conductivity in the present invention is determined to be 100% or less from the viewpoint of the internal resistance and rate characteristics of the solid-state battery. -6 S / cm or more is preferable, and 10 -5 More preferably, 10 S / cm or more. -4 S / cm or more is most preferable.

[0055] (Atomization of raw materials) The method of atomizing the raw material in the present invention is not limited as long as it does not impair the effects of the present invention, and examples thereof include methods such as ball milling, jet milling, and cryomilling. The raw material may be atomized before mixing, or may be mixed and then atomized. From the viewpoint of uniformity of mixing, the average particle size of the atomized material is preferably 20 micrometers or less, and more preferably 10 micrometers or less.

[0056] (Polymer electrolyte thickness) The thickness of the polymer electrolyte in the present invention is preferably 200 micrometers or less, more preferably 100 micrometers or less, and even more preferably 30 micrometers or less, from the viewpoint of electrical resistance. The thickness of the polymer electrolyte in the present invention is measured with a constant pressure thickness gauge in accordance with JIS K6250 (2019).

[0057] (Moisture absorption) The moisture absorption in the present invention refers to the moisture absorption capacity of the polymer electrolyte. Specifically, the polymer electrolyte is taken out of a drying chamber with a dew point of -40°C or less, and treated at 25°C and a relative humidity of 80% for 1 hour. The moisture absorption is calculated by dividing the weight increase before and after the treatment by the weight of the polymer electrolyte before the treatment. From the viewpoint of storage of the polymer electrolyte, moisture absorption of the electrolyte may lead to a change in the component ratio and deterioration of the electrolyte. From this viewpoint, the moisture absorption of the polymer electrolyte in the present invention is preferably 0% or more and 20% or less, more preferably 0% or more and 10% or less.

[0058] (battery) The battery of the present invention preferably contains the polymer electrolyte of the present invention. It can be manufactured by a known method, which is not limited as long as it does not impair the effects of the present invention. For example, first, a polymer electrolyte film, a positive electrode material, and a negative electrode material are wound by a winding machine to obtain a wound body. The wound body is then sealed with an exterior material to obtain a battery having a polymer electrolyte. EXAMPLES

[0059] The present invention will be described below with reference to examples, but the present invention is not necessarily limited to these.

[0060] (Measurement of crystallinity) The crystallinity of the polymer electrolyte referred to here refers to the crystallinity of a film that does not contain an ionization assistant. The crystallinity of the polymer electrolyte in the present invention was measured by a differential scanning calorimeter (DSC). First, the polymer electrolyte was pulverized to an average particle size of 0.5 mm or less using a cryomill. 2.5 mg of the polymer electrolyte was filled into an aluminum sample holder and placed on the sample stage. The polymer electrolyte was heated from 25°C to 120°C at a rate of 10°C / min in a nitrogen atmosphere and held at 120°C for 2 hours. Thereafter, the temperature was raised to 400°C at a rate of 10°C / min, and the peak with the widest area among the obtained endothermic peaks was regarded as the melting peak, and the heat of fusion (J / g) calculated from the melting peak area was divided by 146.2 (J / g) to obtain the crystallinity (%).

[0061] (Melt point measurement) The melting point of the polymer electrolyte was measured by a differential scanning calorimeter (DSC). 2.5 mg of the polymer electrolyte, which had been pulverized to an average particle size of about 0.5 mm or less using a cryomill, was filled into an aluminum sample holder and placed on the sample stage. The polymer electrolyte was heated from 25°C to 120°C at a rate of 10°C / min in a nitrogen atmosphere and held at 120°C for 2 hours. It was then heated to 400°C at a rate of 10°C / min, and the peak with the widest area among the obtained endothermic peaks was regarded as the melting peak, and the peak temperature of the melting peak was taken as the melting point.

[0062] (Measurement of ionic conductivity) The ionic conductivity in the present invention was measured by the following method. After measuring the thickness of the polymer electrolyte film, a sample was taken to have a diameter of 10 mm and an area (S) of 78.5 mm2. 2 The polymer electrolyte film was placed in a sample holder with a diameter of 10 mm (KP-SolidCell manufactured by Hohsen). Then, an AC voltage of 100 Hz to 100 MHz was applied using a high-frequency impedance measurement system (4990EDMS-120K manufactured by Toyo Corporation) to measure the impedance by the complex impedance method. The resistance value (R) was calculated from the obtained impedance, and the ionic conductivity (σ) was calculated using the following formula (3) together with the measured thickness (D) and area (S).

[0063]

number

[0064] (Measurement of ion diffusion coefficient) The ion diffusion coefficient of the polymer electrolyte referred to here means the ion diffusion coefficient of a film containing an ionization assistant, a polymer, and an alkali metal salt. The ion diffusion coefficient in the present invention was measured by PFG-NMR (Pulsed Field Gradient Nuclear Magnetic Resonance Spectroscopy). It was measured at 25°C under a dry nitrogen atmosphere using AVANCE III HD400 manufactured by Bruker Biospin. The observation was performed. 7The measurements were performed at 155.6 MHz using Li. The diffusion plot was fitted with two components using the least squares method. The maximum value obtained was taken as the ion diffusion coefficient.

[0065] (Film thickness measurement) The thickness of the polymer electrolyte film in the present invention was measured using a constant pressure thickness gauge in accordance with JIS K6250 (2019).

[0066] (Film containing alkali metal salt) The film containing the alkali metal salt in the present invention is prepared by melt-kneading the alkali metal salt and the polymer, and then forming the film in a film-forming process. The film-forming method in the present invention may be a known method. The film-forming method in the present invention may include a stretching process, but the PAS may crystallize due to the stretching of the film, which may make it difficult to incorporate the ionization assistant described below. From the above viewpoint, it is preferable that the film-forming method in the present invention does not include a stretching process.

[0067] (Impregnation of ionization agent) In the present invention, the impregnation of the ionization assistant was performed by impregnating the film containing the alkali metal salt and the ionization assistant under certain conditions in a sealed container. The impregnation conditions included conditions such as temperature and pressure during impregnation, and were appropriately selected depending on the types of PAS, alkali metal salt, and ionization assistant. For example, when impregnating a PPS film containing a lithium salt with GBL, the film and GBL were placed in a sealed container and heated in an oven at normal pressure at 120°C for 1 hour. When reducing the pressure, the PPS film containing the lithium salt and GBL were placed in an open container and heated in a vacuum oven at 120°C for 1 hour while evacuating.

[0068] (Measurement of moisture absorption) In the present invention, the moisture absorption refers to the moisture absorption ability of the polymer electrolyte. Specifically, the polymer electrolyte was taken out of a drying chamber with a dew point of -40°C or less, and was treated at 25°C and a relative humidity of 80% for 1 hour. The moisture absorption was calculated by dividing the weight increase before and after the treatment by the weight of the polymer electrolyte before the treatment.

[0069] (Polymer 1) A copolymer consisting of 85 mol % of paraphenylene sulfide structural units in which Ar is represented by (A) and 15 mol % of metaphenylene sulfide structural units in which Ar is represented by (C) and R1 and R2 are both hydrogen, relative to 100 mol % of all -(Ar-S)- repeating units.

[0070] (Polymer 2) A copolymer consisting of 90 mol % of paraphenylene sulfide structural units in which Ar is represented by (A) and 10 mol % of metaphenylene sulfide structural units in which Ar is represented by (C) and R1 and R2 are both hydrogen, relative to 100 mol % of all -(Ar-S)- repeating units.

[0071] (Polymer 3) A polymer consisting only of paraphenylene sulfide structural units in which Ar is represented by (A) relative to 100 mol % of -(Ar-S)- repeating units (polyphenylene sulfide "TORELINA" (registered trademark) E2080 manufactured by Toray Industries, Inc.).

[0072] (Polymer 4) A copolymer consisting of 100 mol% of -(Ar-S)- repeating units, 84 mol% of paraphenylene sulfide structural units where Ar is represented by (A), 15 mol% of metaphenylene sulfide structural units where Ar is represented by (C) and R1 and R2 are both hydrogen, and 1 mol% of a branching unit represented by (H).

[0073] (Polymer 5) Polymer 1 and polymer 3 are mixed in a molar ratio of 1:1.

[0074] (Polymer 6) Polyethylene (PE).

[0075] (Polymer 7) Polyethylene terephthalate (PET).

[0076] (Polymer 8) Polystyrene (PS).

[0077] (Polymer 9) Polypyromellitimide (PI) ("Kapton" (registered trademark) manufactured by DuPont Co., Ltd.).

[0078] (Alkali metal salt 1) Lithium bis(trifluoromethanesulfonyl)imide (Tokyo Chemical Industry Co., Ltd.).

[0079] (Alkali metal salt 2) Lithium bis(fluorosulfonyl)imide (Tokyo Chemical Industry Co., Ltd.).

[0080] (Alkali metal salt 3) Lithium hydroxide (Alfa Aesar).

[0081] Example 1 Polymer 1 was pulverized to an average particle size of 20 micrometers or less. The pulverized powder was then mixed with alkali metal salt 1. At this time, the mixture was prepared so that the molar ratio of the number of structural units contained in polymer 1 to alkali metal salt 1 was 100:45.4. Specifically, 121 g of alkali metal salt 1 was mixed with 100 g of polymer 1 powder.

[0082] The mixture powder was put into a melt kneader under dry room conditions with a dew point of -40°C and kneaded at 260°C. It was then cooled to 25°C by air cooling. The obtained sample was again pulverized so that the average particle size was 20 micrometers or less. The obtained powder was formed into a film by a known method and was not stretched. A film of 30 micrometers was obtained by the above method. A small amount of the obtained film was sampled and the polymer electrolyte was pulverized in a cryomill until the diameter was 0.5 mm or less, and the crystallinity and melting point were measured.

[0083] The obtained film and gamma-butyrolactone (GBL) were placed in a container and immersed in a vacuum oven at 120°C for 1 hour to adjust the pressure to 0.5 atm. After cooling, the conductive assistant remaining on the surface was wiped off. The ionic conductivity and moisture absorption of the obtained polymer electrolyte film were measured at 25°C. The measurement results are shown in Table 2. In Example 1, since the melting point of the polymer was low, kneading was possible at a relatively low temperature of 260°C, decomposition or deterioration of the raw materials did not occur, and productivity was excellent. In other words, the polymer electrolyte of Example 1 had good ionic conductivity at room temperature and excellent productivity.

[0084] (Examples 2 to 17, Comparative Examples 1 to 5) Samples were prepared and evaluated in the same manner as in Example 1, except that the polymer type, alkali metal salt type, kneading temperature, stretch ratio, pressure, and molar ratio of polymer to alkali metal salt were as shown in Table 1. The evaluation results are shown in Table 2. The mass ratio of each component of the mixed ionization assistant shown in Example 10 was EC(30):PC(30):EMC(40).

[0085] In the same manner as in the case of the example 1, the polymer electrolytes of the examples 2 to 17 can be molded at low temperatures and are excellent in productivity and ion conductivity. That is, the polymer electrolytes of these examples, like the polymer electrolyte of the example 1, exhibit good ion conductivity at room temperature and are excellent in moldability, productivity, and quality stability. In the example 18, the polymer and the alkali metal salt are formed into a film, and then the film is biaxially stretched, and the crystallinity is increased by the stretching. Due to the increase in crystallinity, the amount of impregnation of the ionization assistant is decreased, and the ion conductivity is slightly inferior. In the comparative example 1, there is no constitutional unit in which Ar is at least one structure selected from (B) to (G). Therefore, the molding must be performed at high temperatures. The alkali metal salt is deteriorated at high temperatures, and the ion conductivity is inferior. In the comparative examples 2 to 4, a polymer other than PAS is used, and the affinity with the alkali metal salt and the ionization assistant is lower than that of PAS, and therefore the ion conductivity is inferior. In the comparative example 5, since the ionization assistant is not contained, the dissociation and conduction of the alkali metal salt are insufficient, and the ion conductivity is inferior.

[0086] (Example 18) Polymer 1 was pulverized to an average particle size of 20 micrometers or less. The pulverized powder was then mixed with alkali metal salt 1. At this time, the mixture was prepared so that the molar ratio of the number of structural units contained in polymer 1 to alkali metal salt 1 was 100:5.1. Specifically, 13.53 g of alkali metal salt 1 was mixed with 100 g of polymer 1 powder.

[0087] The powder mixture was placed in a melt kneader under dry room conditions with a dew point of -40°C and kneaded at 260°C. The obtained sample was again pulverized to an average particle size of 20 micrometers or less. The obtained powder was pressed in a press heated to 260°C, and then sandwiched between stainless steel plates at a temperature of 15°C and quenched to obtain a film with a thickness of 30 micrometers. A small amount of the obtained film was sampled to measure the crystallinity and melting point.

[0088] Next, the obtained film and pure water with an electrical resistivity of 0.5 MΩ (megaohms) were placed in a container and treated in a thermo-hygrostat at 1.0 atm and 60°C for 1 hour to impregnate the film with pure water. The weight of the film before impregnation was measured, and after the impregnation treatment, the surface was wiped and the weight after impregnation was measured. From the change in weight before and after impregnation, it was found that the film was impregnated at a molar ratio of 5.1:71.7, where 1:alkali metal salt.

[0089] The ionic conductivity of the obtained polymer electrolyte film was measured at 25° C. The measurement results are shown in Table 2.

[0090] (Example 19) A solid electrolyte was obtained in the same manner as in Example 18, except that the impregnation treatment condition in the thermo-hygrostat was set to 70° C. From the change in weight before and after impregnation, it was found that the impregnation was performed at a molar ratio of 5.1:90.5 (alkali metal salt:pure water: 1).

[0091] The ionic conductivity of the resulting polymer electrolyte film was measured at 25° C. The results are shown in Table 2.

[0092] (Example 20) A solid electrolyte was obtained in the same manner as in Example 18, except that the impregnation treatment condition in the thermo-hygrostat was set to 80° C. From the change in weight before and after impregnation, it was found that the impregnation was performed at a molar ratio of 5.1:136.7 (alkali metal salt:pure water: 1).

[0093] The ionic conductivity of the resulting polymer electrolyte film was measured at 25° C. The results are shown in Table 2.

[0094] Comparative Example 6 In Comparative Example 6, the polymer was PI (Polymer 9), but the melting temperature was 400° C. or higher. On the other hand, since the decomposition temperature of lithium salt (Li salt) was 380° C. or lower, vaporization and decomposition of the Li salt occurred when mixed with the Li salt, and melt mixing was not possible.

[0095] Comparative Example 7 In Comparative Example 7, LiTFSI and PI (polymer 9) were dissolved in an NMP solution so that the molar ratio was 1:2. The LiTFSI and PI solution was then cast onto a PET substrate and dried in a vacuum oven at 120°C for 3 hours. The residual NMP was 4 wt%. The ionic conductivity and moisture absorption of the obtained electrolyte film were measured. Although this comparative example achieved an initial ionic conductivity at the same level as the examples, the moisture absorption was high, and therefore electrolysis of moisture was likely to occur.

[0096] (Polymer manufacturing method) [Reference example 1] An autoclave equipped with a stirrer was charged with 6.005 kg (25 mol) of sodium sulfide nonahydrate, 0.787 kg (9.6 mol) of sodium acetate, and 5 kg of NMP (N-methylpyrrolidone), and the temperature was gradually raised to 205°C while nitrogen was passed through, and 3.6 liters of water was distilled off. Next, the reaction vessel was cooled to 180°C, and then 3.712 kg (25.25 mol) of 1,4-dichlorobenzene and 2.4 kg of NMP were added, sealed under nitrogen, and heated to 270°C, and reacted at 270°C for 2.5 hours. Next, the mixture was poured into 10 kg of NMP heated to 100°C, and stirred for about 1 hour, and then filtered, and washed with hot water at 80°C for 30 minutes three times. This was filtered, added to 25 L of an aqueous solution containing 10.4 g of calcium acetate, and stirred at 192°C for about 1 hour in a sealed autoclave. Then, it was filtered, washed with ion-exchanged water at about 90°C until the pH of the filtrate reached 7, and then dried under reduced pressure at 80°C for 24 hours to obtain Polymer 3.

[0097] [Reference example 2] With reference to Reference Example 1, 3.155 kg (21.46 mol) of 1,4-dichlorobenzene and 0.557 kg (3.79 mol) of 1,3-dichlorobenzene were added simultaneously to obtain Polymer 1.

[0098] [Reference example 3] With reference to Reference Example 1, 3.341 kg (22.72 mol) of 1,4-dichlorobenzene and 0.371 kg (2.53 mol) of 1,3-dichlorobenzene were also added at the same time to obtain Polymer 2.

[0099] [Reference example 4] With reference to Reference Example 1, 3.155 kg (21.46 mol) of 1,4-dichlorobenzene, 0.557 kg (3.79 mol) of 1,3-dichlorobenzene and 0.048 kg (0.26 mol) of 1,2,4-trichlorobenzene were also added at the same time to obtain Polymer 4.

[0100] [Table 1]

[0101]

Table 2

Claims

1. A polymer electrolyte comprising an alkali metal salt, an ionization assistant, and a polyarylene sulfide, The polyarylene sulfide is a polyarylene sulfide copolymer having a structural unit represented by the formula -(Ar-S)-, A polymer electrolyte, wherein Ar has a constitutional unit represented by (A) in chemical formula (1) and at least one constitutional unit selected from the group consisting of (B) to (G) in chemical formula (1). [Formula 1] (R1 and R2 are substituents selected from an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R1 and R2 may be the same or different. R3 and R4 are substituents selected from a hydrogen atom, an alkyl group, an alkoxy group, an amino group, a carboxyl group, and a hydroxyl group, and R3 and R4 may be the same or different. Y is an alkylene group, O, CO, SO, or SO 2 are selected from.)

2. The ionization assistant agent has a solvent, 2. The polymer electrolyte according to claim 1, wherein the solvent has a degree of ionic dissociation (1-ξ) at 25° C. obtained by the formula (1) of 0.1 or more and a solvent diffusion coefficient obtained by the formula (2) of 15 or less. [0010] [0025]

3. The polymer electrolyte according to claim 1 or 2, wherein the ionization assistant comprises one or more selected from the group consisting of water, gamma-butyrolactone, N-methylpyrrolidone, butylene carbonate (BC), ethylene carbonate (EC), propylene carbonate (PC), methyl-gamma-butyrolactone (GVL), triglyme (TG), diglyme (DG), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC).

4. 4. The polymer electrolyte according to claim 1, wherein the alkali metal salt comprises at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethane)sulfonimide.

5. A battery comprising the polymer electrolyte according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Polymer composite solid electrolyte and preparation method and application thereof

    CN106450424A

  • Electrically-conductive organic thermoplastic composition

    JP1984157151A

  • Electrochemical cells with solid ionically conductive polymer materials

    JP2019517712A

  • Polymer solid electrolyte and lithium secondary battery containing the same

    JP2019530166A

  • Solid polymer matrix electrolyte (PME) for rechargeable lithium batteries and batteries made therewith

    TW202015279A