LAMINATE, METHOD FOR PRODUCING LAMINATE, FILM FOR LAMINATION, AND IMAGE DISPLAY DEVICE
The laminate with a plastic film and hard coat layer covering the adherend's main and side surfaces addresses the issue of fragment scattering by ensuring comprehensive coverage and adhesion, enhancing impact resistance in display devices.
Patent Information
- Application Number
- JP2021561481
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2020-11-26
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-11-26
AI Technical Summary
Existing laminates with functional films bonded to protective plates fail to prevent scattering of both large and fine fragments upon impact, as they primarily cover only the surface and not the side surfaces of the adherend.
A laminate structure is developed where the adherend's main surface and side surfaces are covered by an adjacent layer comprising a plastic film and a hard coat layer with specific softening point relationships (F1 < F2), ensuring comprehensive coverage and adhesion, using a method involving vacuum pressure forming.
The laminate effectively suppresses both large and fine fragment scattering upon impact, while enabling easy manufacturing and providing enhanced protection for display devices.
Smart Images

Figure 0007571734000004 
Figure 0007571734000005 
Figure 0007571734000006
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate, a method for producing a laminate, a film for lamination, and an image display device. [Background technology]
[0002] 2. Description of the Related Art On the surfaces of various display devices such as TVs, mobile terminals, in-vehicle center information displays, and in-vehicle meters, a protective plate such as a resin plate or a glass plate is often placed on the surface for the purpose of protecting the display elements.
[0003] In addition, a functional layer may be formed on the protective plate of a display device by applying a functional ink for the purpose of improving the visibility of information such as images and characters and preventing damage to the protective plate. However, simply forming a functional layer on the protective plate cannot prevent the protective plate from scattering into the surroundings when the protective plate receives a strong impact.
[0004] As a means for imparting a predetermined function to the protective plate and preventing the protective plate from shattering, a means for attaching a functional film having shatterproof properties to the protective plate has been proposed (eg, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-171770 A [Patent Document 2] JP 2013-178332 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the case of a laminate obtained by laminating a functional film having splash prevention properties on a protective plate as in Patent Documents 1 and 2, even though it is possible to suppress the scattering of large fragments when the protective plate cracks due to impact, it is not possible to suppress the scattering of fine powdery fragments.
Means for Solving the Problems
[0007] As a result of intensive research by the present inventors, it has been found that the fine powdery fragments are generated from the side surface of the protective plate which is the adherend of the functional film. And as a result of intensive research on means for sufficiently covering not only the surface but also the side surface of the adherend, the present disclosure has been completed.
[0008] The present disclosure provides the following [1] to [4]. [1] A laminate having an adherend and an adjacent layer, The adherend has a first main surface, a second main surface on the back of the first main surface, and a side surface connecting the end of the first main surface and the end of the second main surface, At least the first main surface and the side surface of the adherend are covered by the adjacent layer, The adjacent layer has, in this order from the adherend side, at least a plastic film and a hard coat layer containing a cured product of a curable resin composition, A laminate in which the softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship F1 < F2. [2] A method for manufacturing a laminate having the following steps (1) to (5). (1) A step of disposing an adherend in the lower vacuum chamber of a vacuum pressure machine having an upper vacuum chamber and a lower vacuum chamber so that the first main surface side faces upward. (2) A step of disposing the following laminate film between the upper vacuum chamber and the lower vacuum chamber so that the adhesive layer faces downward. <Laminate Film> A laminate film having, in this order, at least an adhesive layer, a plastic film, and a hard coat layer containing a cured product of a curable resin composition, and in which the softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship F1 < F2. (3) Process of evacuating the upper vacuum chamber and the lower vacuum chamber. (4) Process of pressing the adherend up to the upper vacuum chamber while heating the film for lamination, thereby pressing the first main surface of the adherend against the heated film for lamination. (5) Process of pressing the upper vacuum chamber while the film for lamination is heated, thereby causing the film for lamination to adhere to the exposed surface of the adherend. [3] A film for lamination having at least, in this order, an adhesive layer, a plastic film, and a hard coat layer including a cured product of a curable resin composition, wherein the softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship F1 < F2. [4] An image display device having the laminate according to [1] on a display element. [Advantages of the Invention]
[0009] The laminate and the image display device of the present disclosure can suppress not only the scattering of large fragments but also the scattering of powdery fine fragments when the adherend cracks due to impact. Further, the method for manufacturing the laminate of the present disclosure can easily manufacture the above-described laminate. Further, the film for lamination of the present disclosure is useful as a material for the above-described laminate. [Brief Description of the Drawings]
[0010] [Figure 1] It is a cross-sectional view showing an embodiment of the laminate of the present disclosure. [Diagram 2] It is a cross-sectional view showing another embodiment of the laminate of the present disclosure. [Diagram 3] It is a cross-sectional view showing an embodiment of the adherend included in the laminate of the present disclosure. [Figure 4] It is an enlarged view showing an embodiment of an end portion of the adherend included in the laminate of the present disclosure. [Diagram 5] It is a plan view for explaining a measurement location of in-plane retardation. [Figure 6] It is a cross-sectional view showing an embodiment of the film for lamination of the present disclosure. [Figure 7]A cross-sectional view showing another embodiment of the film for lamination of the present disclosure. [Figure 8] A process diagram showing an embodiment of a method for manufacturing a laminate of the present disclosure. [Figure 9] A schematic diagram of a four-point bending test. [Figure 10] A schematic cross-sectional view of an apparatus for measuring erosion rate. [Figure 11] An image diagram of a state where a laminate is worn by a test liquid containing pure water and spherical silica ejected from an ejection part.
Mode for Carrying Out the Invention
[0011] [Laminate] The laminate of the present disclosure has an adherend and an adjacent layer. The adherend has a first main surface, a second main surface on the back of the first main surface, and a side surface connecting an end of the first main surface and an end of the second main surface. At least the first main surface and the side surface of the adherend are covered by the adjacent layer. The adjacent layer has, in this order from the adherend side, at least a plastic film and a hard coat layer containing a cured product of a curable resin composition. The softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship F1 < F2.
[0012] FIGS. 1 to 2 are cross-sectional views showing embodiments of the laminate of the present disclosure. The laminate 100 in FIGS. 1 to 2 has an adherend 10 and an adjacent layer 20. In addition, the adherend 10 in FIGS. 1 to 2 has a first main surface 10a, a second main surface 10b on the back of the first main surface, and a side surface 10c connecting an end of the first main surface and an end of the second main surface. In FIGS. 1 to 2, the end of the first main surface is denoted by reference sign X1, and the end of the second main surface is denoted by reference sign X2. In addition, the first main surface 10a and the side surface 10c of the adherend 10 in FIGS. 1 to 2 are covered by the adjacent layer 20. In FIG. 2, the second main surface 10b of the adherend 10 is also covered by the adjacent layer 20. 1 and 2, the adjacent layer 20 has, from the adherend 10 side, an adhesive layer 21, a plastic film 22, and a hard coat layer 23 containing a cured product of a curable resin composition, in this order.
[0013] <Adherend> The shape of the adherend is not particularly limited, so long as it has a first main surface, a second main surface behind the first main surface, and a side surface connecting an end of the first main surface and an end of the second main surface. For example, the planar shape of the adherend may be a triangle, a quadrangle such as a square, a rectangle, a trapezoid, a parallelogram, etc., a polygon such as a pentagon, an ellipse, a circle, a star, an irregular shape, etc. Among these, a quadrangle is preferred for formability. The cross-sectional shape of the adherend may be flat, or may be partially or entirely curved. The end of the first principal surface and the end of the second principal surface can be identified, for example, at an inflection point where the direction of a tangent to the first principal surface or the second principal surface suddenly changes. When the outer peripheral edge of the first main surface is chamfered, the end of the first main surface means the start point of the chamfer. Similarly, when the outer peripheral edge of the second main surface is chamfered, the end of the second main surface means the start point of the chamfer. In the case of Figures 4(a) and (b), the position of the symbol X means the end of the first main surface or the end of the second main surface.
[0014] At least the first main surface and the side surface of the adherend must be covered with an adjacent layer, which will be described later. A typical shatterproof film covers only the first main surface of the adherend, and therefore cannot prevent powdery fine fragments from being generated from the side surface. The laminate of the present disclosure covers not only the first main surface of the adherend but also the side surface with an adjacent layer, thereby preventing powdery fine fragments from being generated from the side surface. In this specification, "the first main surface of the adherend is covered with an adjacent layer" means that 99% or more of the surface area of the first main surface of the adherend is covered with the adjacent layer. In addition, in this specification, "the side surface of the adherend is covered with the adjacent layer" means that 70% or more of the surface area of the side surface of the adherend is covered with the adjacent layer. It is preferable that 80% or more of the surface area of the side surface of the adherend is covered with the adjacent layer.
[0015] The side surface of the adherend is preferably covered with the adjacent layer on the side surface on the first principal surface side. Specifically, when focusing on a region that is 90% of the total surface area of the side surface from the first principal surface side, the proportion of the region that is covered with the adjacent layer is preferably 80% or more, and more preferably 90% or more. It is preferable that the first main surface and the side surface of the adherend are intimately covered by the adjacent layer. Whether or not the first main surface and the side surface of the adherend are intimately covered by the adjacent layer can be determined, for example, by the following (x1) and (x2). (x1) The laminate is cut to prepare a sample including the interface between the first main surface and side surface of the adherend and the adjacent layer. (x2) While observing the sample with a general-purpose means such as SEM or TEM, it is confirmed whether or not the interface is in close contact with no gaps.
[0016] It is preferable that the adherend is covered with the adjacent layer near the end of the second main surface. By adopting the above-mentioned configuration, it is possible to improve the adhesion stability between the side surface of the adherend and the adjacent layer when it is subjected to an impact, and it is possible to more easily suppress the generation of fine powdery fragments from the side surface. The vicinity of the end of the second main surface of the adherend is preferably intimately covered by the adjacent layer. Whether or not the second main surface of the adherend is intimately covered by the adjacent layer can be determined, for example, by the following (y1) and (y2). (y1) The laminate is cut to prepare a sample including the interface between the second main surface of the adherend and the adjacent layer. (y2) While observing the sample with a general-purpose means such as SEM or TEM, it is confirmed whether or not the interface is in close contact with no gaps.
[0017] The "region near the edge of the second main surface covered by the adjacent layer" refers to a region within 2 mm from the edge of the second main surface. The region is preferably within 3 mm, more preferably within 5 mm, and even more preferably within 10 mm from the edge of the second main surface. In this specification, "the vicinity of the end of the second main surface of the adherend is covered with the adjacent layer" means that 70% or more of the surface area of the adherend near the end is covered with the adjacent layer. It is preferable that 80% or more of the surface area of the adherend near the end is covered with the adjacent layer.
[0018] It is preferable that the first main surface of the adherend has a chamfered outer periphery over substantially the entire periphery. By adopting this configuration, it becomes easier to cover the side surface of the adherend with the adjacent layer. In addition, it is preferable that the outer periphery of the second main surface of the adherend is chamfered over substantially the entire periphery. By adopting this configuration, it becomes easier to cover a part of the second main surface of the adherend with the adjacent layer. In this specification, "substantially the entire circumference of the outer periphery of the first main surface" means 90% or more of the entire circumference of the outer periphery of the first main surface. "Substantially the entire circumference of the outer periphery of the first main surface" is preferably 95% or more of the entire circumference of the outer periphery of the first main surface, more preferably 97% or more, even more preferably 99% or more, and even more preferably 100%. In this specification, "substantially the entire circumference of the outer periphery of the second main surface" means 90% or more of the entire circumference of the outer periphery of the second main surface. "Substantially the entire circumference of the outer periphery of the second main surface" is preferably 95% or more, more preferably 97% or more, even more preferably 99% or more, and even more preferably 100% of the entire circumference of the outer periphery of the second main surface.
[0019] Fig. 3(a) is a plan view showing an embodiment of the adherend 10, and Fig. 3(b) is a cross-sectional view showing the embodiment of the adherend 10. In Fig. 3(a), the four corners of the outer periphery of the first main surface 10a when the adherend 10 is viewed in plan are chamfered. In Fig. 3(b), the outer periphery of the first main surface 10a and the outer periphery of the second main surface 10b when the adherend 10 is viewed in cross-section are chamfered.
[0020] Examples of chamfering include C-chamfering, in which the outer peripheral edge is beveled, and R-chamfering, in which the outer peripheral edge is rounded. Of these, R-chamfering is preferred. FIG. 4(a) is an enlarged view showing an embodiment of C-chamfering, and FIG. 4(b) is an enlarged view showing an embodiment of R-chamfering.
[0021] In the case of C-chamfering, the length L of one side of a right triangle with the slope formed by the chamfer as the hypotenuse is preferably 0.5 mm or more and 5.0 mm or less, and more preferably 1.0 mm or more and 3.0 mm or less (FIG. 4(a)).
[0022] In the case of R-chamfering, the radius D of the curved surface formed by the chamfering is preferably 0.5 mm or more and 5.0 mm or less, and more preferably 1.0 mm or more and 4.0 mm or less (FIG. 4(b)).
[0023] The material of the adherend may be one or a mixture of glass, ceramics, and resin. Glass is preferred because it easily generates fine powder fragments from the side when it is impacted, making it easy to exhibit the effects of the present disclosure, and because it has good resistance to heat during molding of the laminate. In addition, glass is preferred because it usually has substantially no retardation, making it easy to set the in-plane retardation of the laminate to the range described below.
[0024] Examples of the glass include soda-lime glass, borosilicate glass, and quartz glass. The glass is preferably tempered glass. Examples of the ceramics include transparent ceramics such as YAG ceramics, such as yttrium aluminate and yttrium oxide. The resin may be one or a mixture selected from polystyrene resins, polyolefin resins, ABS resins, AS resins, AN resins, polyphenylene oxide resins, polycarbonate resins, polyacetal resins, acrylic resins, polyethylene terephthalate resins, polybutylene terephthalate resins, polysulfone resins, and polyphenylene sulfide resins. Among these, polycarbonate resins are more preferred.
[0025] The suitable thickness of the adherend varies depending on the material and cannot be generally stated, but is preferably 0.5 mm to 5.0 mm, more preferably 0.7 mm to 3.0 mm, and even more preferably 1.0 mm to 1.8 mm. By making the thickness of the adherend 0.5 mm or more, it is possible to improve the suitability for protecting display elements, etc. In addition, when the thickness of the adherend is 0.5 mm or more, fine powdery fragments are likely to be generated from the side, which is also preferable in that the effects of the present disclosure can be easily exhibited. By setting the thickness of the adherend to 5.0 mm or less, it becomes easier to realize a reduction in weight and thickness of an article to which the laminate of the present disclosure is applied, such as an image display device.
[0026] Furthermore, when the adherend is glass, the thickness is preferably 0.5 mm or more and 3.0 mm or less, more preferably 0.7 mm or more and 2.5 mm or less, and even more preferably 1.1 mm or more and 1.8 mm or less. Furthermore, when the adherend is a resin, the thickness is preferably 1.0 mm or more and 5.0 mm or less, more preferably 1.8 mm or more and 3.0 mm or less, and even more preferably 2.0 mm or more and 2.5 mm or less.
[0027] <Adjacent layer> The adjacent layer has at least a plastic film and a hard coat layer containing a cured product of a curable resin composition, in this order, from the adherend side. In order to improve adhesion to the adherend, the adjacent layer preferably has an adhesive layer on the adherend side of the plastic film.
[0028] In addition, for the plastic film and the hard coat layer that constitute the adjacent layer, it is necessary that the softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship of F1 < F2. When the relationship of F1 < F2 is not satisfied, during the molding of the laminate, the plastic film located on the adherend side does not soften earlier than the hard coat layer, so it becomes difficult to cover the first main surface and the side surface of the adherend with the adjacent layer, and it is impossible to suppress the generation of powdery fine fragments from the side surface.
[0029] F2 - F1 is preferably 30°C or higher, more preferably 60°C or higher, and even more preferably 85°C or higher. By setting F2 - F1 within the above range, it is possible to more easily cover the first main surface and the side surface of the adherend with the adjacent layer.
[0030] "Measurement of Softening Point" The softening point F1 of the plastic film and the softening point F2 of the hard coat layer can be measured, for example, by the following (z1) and (z2). (z1) Prepare a vertically cut sample of the laminate. (z2) After bringing the probe into contact with an arbitrary position on the cross-section of the sample, heat the minute region in contact with the probe. In this specification, the detection temperature of the peak top of "Deflection" measured under the following measurement conditions is defined as the softening point. Also, in this specification, for the layer where the softening point is measured, five measurements are performed, and the average value of the five measurement values is defined as the softening point of the layer.
[0031] In the present disclosure, the "hard coat layer" is a layer containing a cured product of a curable resin composition. The layer containing the cured product of the curable resin composition usually does not have a softening point of less than 33°C. Therefore, in this specification, a hard coat layer for which the softening point was not measured in the temperature range of 33°C or higher and 300°C or lower, which is the temperature range of the following measurement conditions, is regarded as having a softening point F2 exceeding 300°C. That is, in this specification, when the softening point F1 of the plastic film is measured in the temperature range of 33°C or higher and 300°C or lower, which is the temperature range of the following measurement conditions, while the softening point F2 of the hard coat layer is not measured, it is regarded as satisfying F1 < F2. Further, in the present disclosure, it is preferable that the "hard coat layer" does not have a softening point measured in the temperature range of 33°C or higher and 300°C or lower. Note that a hard coat layer for which the softening point is not measured in the range of 33°C or higher and 300°C or lower may not have a softening point itself, but the fact that the softening point does not exist can be regarded as the softening point being infinitely high. Therefore, when the softening point F1 of the plastic film is measured while the softening point F2 of the hard coat layer is not measured, there is no technical problem in regarding it as satisfying F1 < F2.
[0032] <Measurement conditions> · Heating rate: 5°C / second · Starting temperature for heating: 33°C · Upper limit temperature for measurement: 300°C · Measurement area: 20μm□
[0033] Examples of an apparatus capable of measuring the softening point from the cross-section of a sample include "Product name: Anasys nano IR", which is a nanoscale infrared spectroscopic analysis system manufactured by Bruker Nano Inc.
[0034] A sample with an exposed cross-section for softening point measurement can be produced, for example, by the following steps (A1) to (A2). (A1) The laminate is cut to a predetermined size to prepare a cut sample, and then the cut sample is embedded in a resin to prepare an embedded sample. If the adherend is hard and thick, the back surface of the adherend may be partially scraped before the cutting operation to facilitate the cutting operation. The embedding resin is preferably an epoxy resin. The embedded sample can be obtained, for example, by placing the cut sample in a recess in a silicon embedding plate, pouring an embedding resin into the recess, hardening the embedding resin, and then removing the cut sample and the embedding resin encasing it from the silicon embedding plate. The hardening conditions of the embedding resin can be appropriately adjusted depending on the type of resin. In the case of the epoxy resin manufactured by Struers AG shown below, it is preferable to leave it at room temperature for 12 hours to harden. The silicon embedding plate may be, for example, a silicon embedding plate manufactured by Dosaka EM Co., Ltd. The epoxy resin for embedding may be, for example, a mixture of "Epofix" manufactured by Struers and "Epofix Hardener" manufactured by the same company in a ratio of 10:1.2.
[0035] (A2) The embedded sample is cut vertically with a diamond knife to expose the cross section, thereby preparing a sample for softening point measurement. When cutting the embedded sample, it is preferable to cut it so as to pass through the center of the cut sample. An example of an apparatus for cutting an embedded sample is the product name "Ultramicrotome EM UC7" manufactured by Leica Microsystems.
[0036] 《Adhesive layer》 In order to improve adhesion to the adherend, the adjacent layer preferably has an adhesive layer closer to the adherend than the plastic film. The adhesive layer is preferably located closest to the adherend among the adjacent layers. The adhesive layer may be a pressure-sensitive adhesive layer or a heat-sensitive adhesive layer. A pressure-sensitive adhesive layer is also called a "sticky layer." A heat-sensitive adhesive layer is also called a "heat seal layer." The heat-sensitive adhesive layer is preferable in terms of easily increasing the surface hardness of the laminate and the adhesive layer being less likely to protrude from the end of the adjacent layer during the molding of the laminate.
[0037] The adhesive layer preferably contains a heat-sensitive or pressure-sensitive resin as a main component. The main component means 50 mass% or more of all the resins constituting the adhesive layer, preferably 70 mass% or more, more preferably 90 mass% or more, still more preferably 95 mass% or more, and even more preferably 100 mass%.
[0038] Also, the adhesive layer preferably contains a heat-sensitive or pressure-sensitive resin suitable for the material of the adherend as a main component. For example, when the adherend is glass, the adhesive layer preferably contains a resin having at least one functional group selected from a carboxyl group and a methoxy group. When the material of the adherend is an acrylic resin, it is preferable to use an acrylic resin. When the material of the adherend is a polyphenylene oxide resin, a polycarbonate resin, or a styrene resin, it is preferable to use an acrylic resin, a polystyrene resin, a polyamide resin, etc. having an affinity with these resins. Further, when the material of the adherend is a polypropylene resin, it is preferable to use a chlorinated polyolefin resin, a chlorinated ethylene-vinyl acetate copolymer resin, a cyclized rubber, or a coumarone-indene resin.
[0039] When the adhesive layer contains a heat-sensitive resin as a main component, the softening point F3 of the adhesive layer (heat-sensitive adhesive layer) is preferably lower than the softening point F1 of the plastic film. That is, it is preferable to satisfy the relationship of F3 < F1. By satisfying the said relationship, the adjacent layer can more easily cover the first main surface and the side surface of the adherend.
[0040] The softening point F3 of the heat-sensitive adhesive layer is preferably 30° C. or more and 140° C. or less, more preferably 60° C. or more and 120° C. or less, and even more preferably 90° C. or more and 110° C. or less. By setting F3 to 30° C. or more, it is easy to improve the hardness of the molded product. By setting F3 to 140° C. or less, it is easy to prevent the adhesion to the adherend from decreasing.
[0041] The absolute value of the difference between F1 and F3 is preferably 200° C. or less. By making the absolute value of the difference between F1 and F3 200° C. or less, it is possible to easily suppress a decrease in coverage due to the adhesive layer becoming more likely to flow during the molding process. The absolute value of the difference between F1 and F3 is preferably 100° C. or less, more preferably 50° C. or less.
[0042] The thickness of the adhesive layer is preferably 0.1 μm or more and 50 μm or less, and more preferably 0.5 μm or more and 30 μm or less. In the case of the pressure-sensitive adhesive layer, the thickness is preferably 1 μm or more and 50 μm or less, and more preferably 5 μm or more and 25 μm or less. In the case of a heat-sensitive adhesive layer, the thickness is preferably 0.1 μm or more and 30 μm or less, and more preferably 1 μm or more and 20 μm or less.
[0043] <Plastic Film> Examples of plastic films include plastic films containing one or more resins selected from polyolefin resins such as polyethylene and polypropylene; vinyl resins such as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, and ethylene-vinyl alcohol copolymer; polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; acrylic resins such as polymethyl(meth)acrylate and polyethyl(meth)acrylate; styrene resins such as polystyrene; polyamide resins represented by nylon 6 or nylon 66; polycarbonate resins; and amorphous olefin (abbreviation: COP). The plastic film may be single-layer or multi-layer such as a co-extruded film.
[0044] An acrylic film and a polycarbonate-acrylic co-extruded film preferably satisfy the relationship of F1 < F2, and it is easy to cover the side surface of the adherend with an adjacent layer. In addition, an acrylic film and a polycarbonate-acrylic co-extruded film are preferable because the average in-plane retardation can be easily made 100 nm or less, and the synergistic effect described later is easily exhibited. In particular, the acrylic film is more likely to exhibit the synergistic effect described later.
[0045] The softening point F1 of the plastic film is preferably 70°C or higher and 150°C or lower, more preferably 100°C or higher and 140°C or lower, and even more preferably 110°C or higher and 130°C or lower. By setting F1 to 70°C or higher, it is easy to improve the handleability of the adjacent layer during the molding of the laminate. Also, when the plastic film is excessively softened during the molding of the laminate, it becomes difficult to cover the side surface and the second major surface of the adherend with the adjacent layer. Therefore, in order to easily cover the side surface and the second major surface of the adherend with the adjacent layer, F1 is preferably 100°C or higher. By setting F1 to 150°C or lower, it is possible to suppress the temperature during the molding of the laminate from becoming too high, and it is easy to suppress the yellowing of the plastic film and the alteration of the hard coat layer. Also, by setting F1 to 150°C or lower, the plastic film is easily softened during the molding of the laminate. Therefore, by setting F1 to 150°C or lower, it is possible to more easily cover the first major surface, the side surface, and the second major surface of the adherend with the adjacent layer.
[0046] When the average in-plane retardation of the plastic film is defined as Re1, Re1 is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 10 nm or less. A plastic film with Re1 of 100 nm or less is preferable because, due to its low degree of orientation, it is less likely to develop defects such as cracks at bent portions such as the boundary between the bent portion's first main surface and side surface. Also, a plastic film with Re1 of 100 nm or less has a small anisotropy in the in-plane physical properties of the plastic film, so it is easy to make the elongation during molding uniform. Therefore, F1 < F2, and since the Re1 of the plastic film is 100 nm or less, a synergistic effect occurs, making it extremely easy to coat the first main surface and side surface of the adherend. Furthermore, a plastic film with Re1 of 100 nm or less is likely to make the elongation during molding uniform, so the variation in physical properties for each location of the plastic film constituting the laminate can be suppressed within the plane of the laminate. For this reason, a plastic film with Re1 of 100 nm or less can also stabilize the anti-scattering property of the laminate. The physical properties described above include, for example, the erosion rate described later.
[0047] Re1, which is the average in-plane retardation of the plastic film, and Re2, which is the average in-plane retardation of the laminate described later, are the average values of the in-plane retardations of a total of nine points: one point in region (i) near the center of the measurement sample, any four points selected from region (ii) near the edge of the measurement sample, and any four points selected from region (iii) other than near the center and edge of the measurement sample. The region (i) near the center means a region of 1 cm centered on the centroid of the measurement sample. 2 The region (ii) near the edge of the measurement sample means a region within 1 cm from the edge of the measurement sample. Fig. 5 is a diagram for explaining the measurement locations (region (i), region (ii), region (iii)) of the in-plane retardation when the measurement sample is viewed in plan view. It should be noted that it is preferable to select any four points selected from region (ii) and any four points selected from region (iii) without bias in location.
[0048] In addition, when the in-plane retardation of the region (i) of the plastic film is defined as Re1C, the in-plane retardation of the region (ii) of the plastic film is defined as Re1E, and the in-plane retardation of the region (iii) of the plastic film is defined as Re1O, the absolute value of the difference between Re1C and Re1E is preferably 10 nm or less. Similarly, the absolute value of the difference between Re1C and Re1O is preferably 10 nm or less. Similarly, the absolute value of the difference between Re1O and Re1E is preferably 10 nm or less. Re1E means the average value of the in-plane retardation at any four points. Similarly, Re1O means the average value of the in-plane retardation at any four points.
[0049] In this specification, the in-plane retardation can be expressed by the following formula (A) using the refractive index nx in the slow axis direction, which is the direction in the plane of the measurement sample that has the largest refractive index, the refractive index ny in the fast axis direction, which is the direction perpendicular to the slow axis direction in the plane, and the thickness T [nm] of the measurement sample. In-plane phase difference (Re)=(nx-ny)×T[nm] (A) The in-plane retardation can be measured, for example, by using a product called "RETS-100" manufactured by Otsuka Electronics Co., Ltd. In this specification, the in-plane retardation refers to the value at a wavelength of 589 nm.
[0050] When measuring the in-plane retardation using the product "RETS-100" manufactured by Otsuka Electronics Co., Ltd., it is preferable to prepare for the measurement according to the following steps (A1) to (A4). (A1) First, turn on the RETS-100 light source and leave it for 60 minutes or more to stabilize it. After that, select the rotating analyzer method and select θ mode (angle direction phase difference measurement and Rth calculation mode). By selecting this θ mode, the stage becomes a tilt rotation stage. (A2) Next, enter the following measurement conditions into the RETS-100. <Measurement conditions> Retardation measurement range: Rotating analyzer method Measurement spot diameter: φ5mm Tilt angle range: 0 degrees ·Measurement wavelength range: 400 nm or more and 800 nm or less ·Average refractive index of the measurement sample ·Thickness: Measured value of the thickness. For example, describe the thickness separately measured by SEM or optical microscope. (A3) Next, obtain background data without installing a sample in this apparatus. The apparatus is a closed system, and this is carried out every time the light source is turned on. (A4) Then, install the sample on the stage in the apparatus and perform the measurement. It is preferable to arrange and measure the sample so that the surface with high flatness faces the stage side.
[0051] The thickness of the plastic film is preferably 30 μm or more and 150 μm or less, more preferably 35 μm or more and 100 μm or less, and even more preferably 40 μm or more and 80 μm or less. By setting the thickness of the plastic film to 30 μm or more, the moldability of the adjacent layer satisfying the relationship of F1 < F2 can be made better, and the side surface of the adherend can be more easily covered with the adjacent layer. Further, by setting the thickness of the plastic film to 150 μm or less, thickening of the laminate can be suppressed.
[0052] 《Hard coat layer》 The hard coat layer needs to contain a cured product of a curable resin composition. When the hard coat layer does not contain a cured product of a curable resin composition, the moldability tends to be good, but the scratch resistance of the laminate cannot be improved.
[0053] The cured product of the curable resin composition becomes the resin component of the hard coat layer. The ratio of the cured product of the curable resin composition to all the resin components of the hard coat layer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more.
[0054] The curable resin composition includes a thermosetting resin composition and an ionizing radiation curable resin composition, and among these, an ionizing radiation curable resin composition is preferable.
[0055] The thermosetting resin composition is a composition containing at least a thermosetting resin, and is a resin composition that is cured by heating. Examples of the thermosetting resin include acrylic resin, urethane resin, phenol resin, urea melamine resin, epoxy resin, unsaturated polyester resin, silicone resin, etc. In the thermosetting resin composition, a curing agent such as an isocyanate-based curing agent is added to the curable resin as necessary.
[0056] The ionizing radiation curable resin composition is a composition containing a compound having an ionizing radiation curable functional group. Examples of the ionizing radiation curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl groups, vinyl groups, and allyl groups, as well as epoxy groups and oxetanyl groups. Hereinafter, the "compound having an ionizing radiation curable functional group" may also be referred to as the "ionizing radiation curable compound." The ionizing radiation curable resin is preferably a compound having an ethylenically unsaturated bond group. In addition, in order to prevent the hard coat layer from being damaged during the process of producing the lamination film, the ionizing radiation curable resin is more preferably a compound having two or more ethylenically unsaturated bond groups, and among them, a polyfunctional (meth)acrylate compound having two or more ethylenically unsaturated bond groups is even more preferable. As the polyfunctional (meth)acrylate compound, either a monomer or an oligomer can be used. The ionizing radiation means, among electromagnetic waves or charged particle beams, electromagnetic waves or charged particle beams having an energy quantum capable of polymerizing or crosslinking molecules. As the ionizing radiation, ultraviolet rays or electron beams are usually used, but electromagnetic waves such as X-rays and γ-rays, and charged particle beams such as α-rays and ion beams can also be used.
[0057] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxydiacrylate, bisphenol A tetrapropoxydiacrylate, and 1,6-hexanediol diacrylate. Examples of trifunctional or higher (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and isocyanuric acid-modified tri(meth)acrylate. The (meth)acrylate monomer may have a part of its molecular skeleton modified with, for example, ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, an alkyl group, a cyclic alkyl group, an aromatic group, or a bisphenol.
[0058] Examples of the polyfunctional (meth)acrylate oligomer include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, and polyether (meth)acrylate. The urethane (meth)acrylate can be obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate. In addition, preferred epoxy (meth)acrylates include (meth)acrylates obtained by reacting a trifunctional or higher aromatic epoxy resin, a trifunctional or higher alicyclic epoxy resin, a trifunctional or higher aliphatic epoxy resin, or the like, with (meth)acrylic acid; (meth)acrylates obtained by reacting a difunctional or higher aromatic epoxy resin, a difunctional or higher alicyclic epoxy resin, a difunctional or higher aliphatic epoxy resin, or the like, with a polybasic acid and (meth)acrylic acid; and (meth)acrylates obtained by reacting a difunctional or higher aromatic epoxy resin, a difunctional or higher alicyclic epoxy resin, a difunctional or higher aliphatic epoxy resin, or the like, with a phenol and (meth)acrylic acid. The above ionizing radiation curable resins may be used alone or in combination of two or more.
[0059] When the radiation-curable resin is an ultraviolet-curable resin, the coating liquid for forming the hard coat layer preferably contains additives such as a photopolymerization initiator and a photopolymerization accelerator. Examples of the photopolymerization initiator include one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyldimethylketal, benzoyl benzoate, α-acyl oxime ester, thioxanthones, and the like. The photopolymerization accelerator has a role of reducing the polymerization inhibition by air during curing and increasing the curing rate. Examples of the photopolymerization accelerator include one or more selected from isoamyl p-dimethylaminobenzoate, ethyl p-dimethylaminobenzoate, and the like.
[0060] The hard coat layer may contain a thermoplastic resin as a resin component.
[0061] The hard coat layer may contain additives such as particles, an ultraviolet absorber, a light stabilizer, an antistatic agent, and a leveling agent.
[0062] The thickness of the hard coat layer is preferably 1 μm or more and 20 μm or less, more preferably 2 μm or more and 18 μm or less, and even more preferably 5 μm or more and 15 μm or less. By setting the thickness of the hard coat layer to 1 μm or more, the scratch resistance of the laminate can be easily improved. Also, by setting the thickness of the hard coat layer to 20 μm or less, the moldability of the adjacent layer can be easily improved.
[0063] The softening point F2 of the hard coat layer is preferably 180 °C or more, more preferably 200 °C or more, even more preferably 250 °C or more, and still more preferably more than 300 °C in order to easily satisfy the relationship of F1 < F2.
[0064] 《Other Layers》 The adjacent layer may have an adhesive layer, a plastic film, and other layers other than the hard coat layer. Examples of the other layers include an antireflection layer, an antiglare layer, an antistatic layer, an anchor layer, etc. Hereinafter, an embodiment of the antireflection layer, which is a typical example of the other layers, will be described.
[0065] The adjacent layer preferably has an anti-reflection layer on the side opposite to the plastic film of the hard coat layer, and the anti-reflection layer is preferably disposed on the side farthest from the adherend among the layers constituting the adjacent layer.
[0066] The antireflection layer may have, for example, a single-layer structure of a low refractive index layer, a two-layer structure of a high refractive index layer and a low refractive index layer, or may be formed of three or more layers. In the case of a two-layer structure of a high refractive index layer and a low refractive index layer, the low refractive index layer is disposed on the surface side, and the high refractive index layer is disposed on the hard coat layer side.
[0067] -Low refractive index layer- The refractive index of the low refractive index layer is preferably 1.10 or more and 1.48 or less, more preferably 1.20 or more and 1.45 or less, more preferably 1.26 or more and 1.40 or less, still more preferably 1.28 or more and 1.38 or less, and particularly preferably 1.30 or more and 1.35 or less. below is more preferred. The thickness of the low refractive index layer is preferably 80 nm or more and 120 nm or less, more preferably 85 nm or more and 110 nm or less, and even more preferably 90 nm or more and 105 nm or less.
[0068] The method of forming a low refractive index layer can be roughly divided into a wet method and a dry method. The wet method includes a method of forming by a sol-gel method using metal alkoxide or the like, a method of forming by coating a resin with a low refractive index such as a fluororesin, and a method of forming by coating a coating liquid for forming a low refractive index layer in which low refractive index particles are contained in a resin composition. The dry method includes a method of selecting particles having a desired refractive index from the low refractive index particles described later and forming by a physical vapor deposition method or a chemical vapor deposition method. The wet method is excellent in terms of production efficiency. Among the wet methods, it is preferable to form the low refractive index layer using a coating liquid for forming the low refractive index layer, in which low refractive index particles are contained in a binder resin composition.
[0069] The low refractive index particles can be any of particles made of an inorganic compound such as silica and magnesium fluoride, and particles made of an organic compound, without any restrictions. Since the anti-reflection properties are improved by reducing the refractive index, particles having a structure with voids are preferably used as the low refractive index particles. Particles having a structure with voids have fine voids inside. The voids are filled with a gas such as air having a refractive index of 1.0. Therefore, particles having a structure with voids have a low refractive index. Examples of such particles having voids include inorganic or organic porous particles and hollow particles. Examples of inorganic or organic porous particles and hollow particles include porous silica, hollow silica particles, porous polymer particles, and hollow polymer particles. Examples of the polymer of the porous polymer particles and hollow polymer particles include acrylic resin. The average particle size of the primary particles of the low refractive index particles is preferably 5 nm or more and 200 nm or less, more preferably 5 nm or more and 100 nm or less, and even more preferably 10 nm or more and 80 nm or less.
[0070] The content of the low refractive index particles is preferably from 50 parts by mass to 400 parts by mass, and more preferably from 100 parts by mass to 300 parts by mass, relative to 100 parts by mass of the binder component.
[0071] The binder resin composition is preferably a curable resin composition. The curable resin composition becomes a cured product in the low refractive index layer and serves as a binder component. Examples of the curable resin composition include a heat-curable resin composition and an ionizing radiation-curable resin composition, and among these, an ionizing radiation-curable resin composition is preferred. Examples of the heat-curable resin composition and ionizing radiation-curable resin composition for the low refractive index layer include the heat-curable resin compositions and ionizing radiation-curable resin compositions exemplified for the hard coat layer.
[0072] The low refractive index layer may contain additives such as an antifouling agent, a leveling agent, and an antistatic agent.
[0073] -High refractive index layer- The antireflection layer may further include a high refractive index layer. By including a high refractive index layer in addition to a low refractive index layer, the wavelength region with low reflectance can be expanded, and the antireflection properties can be improved. The high refractive index layer is disposed closer to the hard coat layer than the low refractive index layer.
[0074] The high refractive index layer preferably has a refractive index of 1.55 or more and 1.85 or less, and more preferably has a refractive index of 1.56 or more and 1.70 or less. The thickness of the high refractive index layer is preferably 200 nm or less, and more preferably 50 nm or more and 180 nm or less.
[0075] The high refractive index layer can be formed from a coating liquid for a high refractive index layer containing, for example, a binder resin composition and high refractive index particles. Examples of the binder resin composition include the curable resin compositions exemplified for the low refractive index layer.
[0076] Examples of high refractive index particles include antimony pentoxide (1.79), zinc oxide (1.90), titanium oxide (2.3 to 2.7), cerium oxide (1.95), tin-doped indium oxide (1.95 to 2.00), antimony-doped tin oxide (1.75 to 1.85), yttrium oxide (1.87), and zirconium oxide (2.10). For each high refractive index particle, the number in parentheses is the refractive index. The average particle size of the primary particles of the high refractive index particles is preferably 5 nm or more and 200 nm or less, more preferably 5 nm or more and 100 nm or less, and even more preferably 10 nm or more and 80 nm or less.
[0077] <Physical properties of laminate> <Total light transmittance, haze> The laminate preferably has a total light transmittance of 50% or more, more preferably 70% or more, and even more preferably 90% or more. The total light transmittance means the total light transmittance as defined in JIS K7361-1:1997.
[0078] When antiglare properties are imparted to the laminate, the haze of the laminate is preferably 5% or more and 25% or less. When antiglare properties are not imparted to the laminate, the haze of the laminate is preferably 1.0% or less, more preferably 0.5% or less, and even more preferably 0.3% or less. The haze refers to the haze specified in JIS K7136:2000. When measuring the total light transmittance and haze of the laminate, the light incident surface is the adherend side.
[0079] 《Reflectance》 When the adjacent layer of the laminate has an antireflection layer, the reflectance of the surface of the laminate on the antireflection layer side is preferably 1.0% or less, and more preferably 0.5% or less. In this specification, reflectance refers to the luminous reflectance Y value of the CIE 1931 standard color system.
[0080] In this specification, the reflectance of the surface of the laminate is measured by preparing a sample by attaching a black plate to the adherend side of the laminate via a transparent adhesive layer, and then irradiating light from the anti-reflection layer side of the sample at an incident angle of 5°. The light source used for measuring the reflectance is preferably D65. The refractive index difference between the sample adherend and the transparent adhesive layer is preferably within 0.15, more preferably within 0.10, and even more preferably within 0.05. The black plate preferably has a total light transmittance of 1% or less, more preferably 0%, according to JIS K7361-1:1997. The refractive index difference between the resin constituting the black plate and the transparent adhesive layer is preferably within 0.15, more preferably within 0.10, and even more preferably within 0.05.
[0081] 《In-plane phase difference》 Furthermore, when the average in-plane retardation of the laminate of the present disclosure is defined as Re2, Re2 is preferably 100 nm or less, more preferably 50 nm or less, and even more preferably 10 nm or less. When the state of polarization is disturbed, rainbow stripes may appear. By setting Re2 to 100 nm or less, the appearance of rainbow stripes can be easily suppressed.
[0082] In addition, when the in-plane retardation of the laminate in region (i) is defined as Re2C, the in-plane retardation of the laminate in region (ii) is defined as Re2E, and the in-plane retardation of the laminate in region (iii) is defined as Re2O, the absolute value of the difference between Re2C and Re2E is preferably 10 nm or less. By satisfying the above-mentioned configuration, the visibility of the laminate itself and the visibility of an image observed through the laminate can be easily made uniform in the plane. Similarly, the absolute value of the difference between Re2C and Re2O is preferably 10 nm or less.Similarly, the absolute value of the difference between Re2O and Re2E is preferably 10 nm or less. The regions (i), (ii) and (iii) are as described in the section on the in-plane retardation of the plastic film. That is, the region (i) is a 1 cm 2 Region (i) refers to the region within 1 cm from the edge of the measurement sample, and region (ii) refers to the rest of the region (see FIG. 5).
[0083] In order to set the in-plane retardation of the laminate within the above-mentioned range, it is preferable to use an adherend and adjacent layers having small in-plane retardation, and to produce the laminate by vacuum and pressure forming, which will be described later.
[0084] Shape parameters, scale parameters In the laminate of the present disclosure, the following shape parameter is preferably 16.0 or less, more preferably 15.0 or less, and even more preferably 12.0 or less. <Calculation of shape parameters and scale parameters by four-point bending test> The laminate is cut into 20 samples having a width of 130 mm. The second main surface of the adherend is placed on a support span. Support SpanAfter placing the samples so that the sample faces the side, a four-point bending test is performed on each sample to measure the breaking stress of each sample. The test conditions are a load span distance of 20 mm, a support span distance of 40 mm, and a loading speed of 5 mm / min. The shape parameters and scale parameters of the laminate are calculated by performing a Weibull distribution analysis on the 20 measured values of the breaking stress.
[0085] Weibull distribution analysis is a probability distribution used to statistically represent the strength of an object. In this disclosure, strength is measured as the breaking stress. The probability density function of the Weibull distribution can be expressed by the following formula (B). In formula (B), "x" is a random variable, "m" is a shape parameter, and "η" is a scale parameter. It can be said that the smaller the shape parameter, the more resistant to stress. It can be said that the larger the scale parameter, the more resistant to stress. Both the shape parameter and the scale parameter are dimensionless values. In this embodiment, the random variable x is the breaking stress, and the shape parameter m is also called the Weibull modulus.
number
[0086] By setting the shape parameter of the laminate to 16.0 or less, it is possible to easily prevent the laminate from cracking due to stress.
[0087] The laminate of the present disclosure preferably has a scale parameter of 3000 or more, more preferably 3200 or more, and even more preferably 3400 or more. By making the scale parameter of the laminate 3000 or more, it is possible to easily prevent the laminate from cracking due to stress. The shape and scale parameters of the laminate can be facilitated within the above ranges, for example, by covering the first major surface and the side surfaces of the adherend with an adjacent layer. In addition, when a 1.3 mm thick tempered glass is used as an adherend, the laminate of the present disclosure more preferably has shape parameters and scale parameters in the above ranges. The thickness of the tempered glass having a thickness of 1.3 mm is preferably 6 μm or more and 20 μm or less, more preferably 6 μm or more and 10 μm or less.
[0088] FIG. 9 is a schematic diagram of the four-point bending test. In Fig. 9, L1 is the distance between the supports of the load span, L2 is the distance between the supports of the support span, and L3 is the length of the sample in the long direction. In this disclosure, L1 is 20 mm, L2 is 40 mm, and L3 is 220 mm. In this disclosure, the length of the sample in the short direction is 130 mm. 9, the laminate 100 as a sample is placed on a support span 300. At this time, the sample is placed so that the top, bottom, left and right sides are even on the support span. Although not shown, the sample is placed so that the second main surface side of the adherend faces the support span side. In the four-point bending test, a load span 200 moves downward and a load pin 201 of the load span contacts the laminate 100 as a sample, thereby applying stress to the laminate 100. The application of stress to the laminate 100 continues until the laminate 100 breaks. In the present disclosure, the loading speed is 5 mm / min. The load pins 201 of the load span are preferably 3mm in diameter. The support pins 301 of the support span are preferably 3mm in diameter. An example of a measuring device for the four-point bending test is Shimadzu Corporation's product name "Autograph AGX-50kN." An example of analysis software for the four-point bending test is Shimadzu Corporation's product name "TRAPEZIUM X version 1.2.1b."
[0089] Erosion rate In the laminate of the present disclosure, when the erosion rate of the central part in the in-plane direction of the plastic film is defined as E1 and the erosion rate near the end part in the in-plane direction of the plastic film is defined as E2, E1 / E2 is preferably 0.80 or more and 1.20 or less, more preferably 0.85 or more and 1.15 or less, and even more preferably 0.90 or more and 1.10 or less. By setting E1 / E2 in the above range, the variation in the erosion rate in the in-plane direction of the plastic film is suppressed, and the shatterproof property of the laminate can be easily stabilized. By setting the average in-plane retardation of the plastic film to 100 nm or less, E1 / E2 can be easily set in the above range.
[0090] The vicinity of the end in the in-plane direction of the plastic film means a region within 3 mm from the end in the in-plane direction of the plastic film. Also, the end in the in-plane direction of the plastic film means a portion that overlaps with the end of the first main surface of the adherend in the in-plane direction of the plastic film when the laminate is viewed in plan. When the shape of the plastic film in plan view is a rectangle, it is preferable to select four corners as the end portions. That is, when the shape of the plastic film in plan view is a rectangle, it is preferable to measure the erosion rate in an area within 3 mm from the four corners, and then set the average value of the four erosion rates as E2.
[0091] In the laminate of the present disclosure, when the erosion rate of the central part in the in-plane direction of the hard coat layer is defined as E3 and the erosion rate of the vicinity of the end part in the in-plane direction of the hard coat layer is defined as E4, E3 / E4 is preferably 0.80 or more and 1.20 or less, more preferably 0.85 or more and 1.15 or less, even more preferably 0.90 or more and 1.10 or less, and even more preferably 0.95 or more and 1.05 or less. By setting E3 / E4 within the above range, variations in the erosion rate in the in-plane direction of the hard coat layer can be suppressed, and it becomes easier to stabilize the anti-scattering property of the laminate. By satisfying the relationship of F1 < F2 to improve the moldability, it becomes easier to set E3 / E4 within the above range.
[0092] The vicinity of the end in the in-plane direction of the hard coat layer means a region within 3 mm from the end in the in-plane direction of the hard coat layer. When the planar shape of the hard coat layer is a rectangle, it is preferable to select four corner portions as the ends. That is, when the planar shape of the hard coat layer is a rectangle, after measuring the erosion rate in the region within 3 mm from the four corner portions, it is preferable to set the average value of the four erosion rates as E4.
[0093] The erosion rates of the plastic film and the hard coat layer can be measured, for example, under the following measurement conditions. <Measurement conditions> A test liquid obtained by mixing pure water, a dispersion liquid, and spherical silica having an average particle diameter within ±8% based on 5.0 μm is stored in a container. The test liquid in the container is sent to a nozzle. Compressed air is sent into the nozzle to accelerate the test liquid in the nozzle, and a predetermined amount of the test liquid is ejected perpendicularly to the laminate of the present disclosure from the ejection hole at the tip of the nozzle, thereby causing the spherical silica in the test liquid to collide with the laminate. The laminate is installed such that the first main surface side of the adherend faces the nozzle side. The cross-sectional shape of the nozzle is a square of 1 mm × 1 mm, and the distance between the ejection hole and the laminate is 4 mm. Also, the flow rates of the test liquid and the compressed air supplied to the nozzle, the pressure of the compressed air, and the pressure of the test liquid in the nozzle are set to predetermined values adjusted by calibration described later. After ejecting a predetermined amount of the test liquid, the ejection of the test liquid is temporarily stopped. After temporarily stopping the ejection of the test liquid, the cross-sectional profile is measured at the location where the spherical silica in the test liquid of the laminate has collided. The operation of spraying a predetermined amount of the test liquid from the spray nozzle, stopping the spray of the test liquid after spraying the predetermined amount of the test liquid, and measuring the cross-sectional profile after stopping the spray of the test liquid is performed until the adherend is reached. Then, in each cycle, an erosion rate (μm / g) is calculated by dividing the depth (μm) of the cross-sectional profile progressed in each cycle by the amount (g) of the test liquid sprayed in each cycle. The E3 or E4 can be calculated by averaging the erosion rates of each cycle in the region of the hard coat layer in the cross-sectional profile. The E1 or E2 can be calculated by averaging the erosion rates of each cycle in the region of the plastic film in the cross-sectional profile.
[0094] <Calibration> The test liquid is placed in the container. The test liquid in the container is sent to the nozzle. Compressed air is sent into the nozzle to accelerate the test liquid in the nozzle, and an arbitrary amount of the test liquid is sprayed perpendicularly from the spray hole at the tip of the nozzle onto an acrylic plate with a thickness of 2 mm, causing the spherical silica in the test liquid to collide with the acrylic plate. The cross-sectional shape of the nozzle is a square of 1 mm x 1 mm, and the distance between the spray hole and the acrylic plate is 4 mm. After a given amount of the test liquid is sprayed, the spraying of the test liquid is stopped temporarily. After the spraying of the test liquid is stopped temporarily, a cross-sectional profile is measured at the point on the acrylic plate where the spherical silica in the test liquid collided. The erosion rate (μm / g) of the acrylic plate is calculated by dividing the depth (μm) of the cross-sectional profile by the arbitrary amount (g) mentioned above. The erosion rate of the acrylic plate is set to a range of ±5% based on 0.17 (μm / g) as the standard, and the flow rates of the test liquid and the compressed air, the pressure of the compressed air, and the pressure of the test liquid in the nozzle are adjusted and calibrated so that the erosion rate of the acrylic plate is within this range.
[0095] The measurement conditions for the erosion rate will be described below with reference to Fig. 10. An example of an apparatus for measuring the erosion rate as shown in Fig. 10 is an MSE test apparatus manufactured by Palmeso, product number "MSE-A203".
[0096] In the measurement conditions for the erosion rate of the present disclosure, first, a test liquid obtained by mixing pure water, a dispersant, and spherical silica having an average particle size of 5.0 μm within ±8% at a mass ratio of 968:2:30 is placed in a container (1100). It is preferable to stir the test liquid in the container (1100). The dispersant is not particularly limited as long as it can disperse spherical silica. An example of the dispersant is "Demol N" manufactured by Wako Pure Chemical Industries, Ltd. "The average particle size is within ±8% of 5.0 μm as the standard" means, in other words, that the average particle size is 4.6 μm or more and 5.4 μm or less. In addition, in the measurement conditions of the erosion rate in this specification, the "average particle size of spherical silica" is measured as the volume average value d50 in particle size distribution measurement by laser light diffraction method (the so-called "median size"). In the particle size distribution measurement, the spherical silica preferably has a particle size width with a frequency of 50 within ±10% of 5.0 μm when the frequency of the particle size with the maximum frequency is normalized to 100. The "particle size width with a frequency of 50" is expressed as "XY (μm)" when "X is a particle size with a frequency of 50 and located in the positive direction of the particle size with a frequency of 100" and "Y is a particle size with a frequency of 50 and located in the negative direction of the particle size with a frequency of 100". In this specification, the "particle size width with a frequency of 50" may be referred to as the "full width at half maximum of the particle size distribution".
[0097] An example of spherical silica with an average particle size of 5.0 μm within ±8% is the model number "MSE-BS-5-3" specified by Palmeso. An example of spherical silica that corresponds to the model number "MSE-BS-5-3" specified by Palmeso is the product number "BS5-3" of Potters Ballotini.
[0098] The test liquid in the container is sent to the nozzle (5100). The test liquid can be sent to the nozzle, for example, through a test liquid pipe (21). A flow meter (3100) for measuring the flow rate of the test liquid is preferably disposed between the container (1100) and the nozzle (5100). The flow rate of the test liquid is the value adjusted by the above calibration. In FIG. 10, the nozzle (5100) is disposed in a housing (5200) that constitutes the ejection unit (5000).
[0099] Compressed air is fed into the nozzle (5100). The compressed air is fed to the nozzle, for example, through a compressed air pipe (2200). In the nozzle, the position to which the compressed air is fed is preferably upstream of the position to which the test liquid is fed. The upstream side refers to the side farther from the nozzle injection hole. It is preferable that a flow meter (3200) for measuring the flow rate of the compressed air and a pressure meter (4200) for measuring the pressure of the compressed air are disposed before the compressed air reaches the nozzle (5100). The compressed air can be supplied by an air compressor (not shown) or the like. The flow rate and pressure of the compressed air are adjusted by the above calibration.
[0100] When compressed air is sent into the nozzle (5100), the test liquid is accelerated while being mixed by the compressed air. The accelerated test liquid is then sprayed from the spray hole at the tip of the nozzle (5100) and collides perpendicularly with the laminate (100). The laminate is primarily worn by the spherical silica particles in the test liquid. The laminate is placed so that the first main surface of the adherend faces the nozzle. It is preferable that a pressure gauge (4100) for measuring the pressure of the test liquid in the nozzle is disposed in the nozzle (5100). The pressure gauge (4100) is preferably located downstream of the position where the compressed air is fed and the position where the test liquid is fed. The pressure of the test liquid in the nozzle (5100) is adjusted by the above calibration.
[0101] The test liquid injected from the injection hole at the tip of the nozzle (5100) is mixed with air and injected in the form of a mist. This makes it possible to reduce the impact pressure on the laminate of spherical silica particles. This makes it possible to minimize the amount of wear on the laminate caused by a single spherical silica particle. FIG. 11 is an image of the laminate (100) being worn away by the test liquid containing pure water (A1) and spherical silica (A2) injected from the injection part (5000). In FIG. 11, symbol A3 indicates air, and symbol A4 indicates the worn laminate. In addition, since the test liquid contains water, which has an excellent cooling effect, deformation and deterioration of the laminate caused by heat during collision can be substantially eliminated. In other words, abnormal wear of the laminate can be substantially eliminated. Water also plays a role in cleaning the surface of the worn laminate and realizing stable wear. Water also plays a role in accelerating the spherical silica particles and controlling the fluid of the test liquid. In addition, since a huge number of spherical silica particles collide with the laminate, the influence of subtle differences in the physical properties of individual spherical silica particles can be eliminated. Furthermore, the measurement conditions of the present disclosure are the flow rate of the test liquid supplied to the nozzle, the flow rate of the compressed air supplied to the nozzle, the pressure of the compressed air supplied to the nozzle, and the pressure of the test liquid in the nozzle, adjusted by the above calibration, and the cross-sectional shape of the nozzle is specified to be a square of 1 mm x 1 mm, and the distance between the injection hole and the laminate is specified to be 4 mm, thereby specifying the factors that affect the amount of wear of the laminate. Note that the above distance is the distance indicated by "d" in Figure 10, and means the vertical distance between the injection hole at the tip of the nozzle and the laminate. From the above, it can be said that the measurement conditions disclosed herein are measurement conditions that can form statistically stable wear marks on the laminate.
[0102] The laminate (100) may be attached to a sample mounting stage (8100) of a measuring device (10000). It is preferable to prepare a laminate 1 by bonding the laminate to a support (8200) such as a stainless steel plate, and attach the laminate 1 to the sample mounting stage (8100). The laminate is placed so that the first main surface of the adherend faces the nozzle.
[0103] The test liquid sprayed onto the laminate (100) is preferably collected in a receiver (1200) and returned to the container (1100) through a return pipe (2300).
[0104] The measurement conditions disclosed herein require that after a predetermined amount of test liquid has been sprayed, spraying of the test liquid is stopped temporarily, and that after spraying of the test liquid is stopped temporarily, the cross-sectional profile of the laminate at the point where the spherical silica in the test liquid collided is measured. The cross-sectional profile refers to the cross-sectional shape of the laminate abraded by the test liquid. The laminate is abraded mainly by the spherical silica particles in the test liquid. The cross-sectional profile can be measured by a cross-sectional profile acquisition unit (6000) such as a stylus-type surface shape measuring device or a laser interference-type surface shape measuring device. The cross-sectional profile acquisition unit (6000) is usually disposed at a position away from the laminate (100) when the test liquid is sprayed. For this reason, it is preferable that at least one of the laminate (100) and the cross-sectional profile acquisition unit (6000) is movable. Palmeso's MSE test equipment, model number "MSE-A203," uses a stylus to measure cross-sectional profiles.
[0105] In this specification, the erosion rate of each cycle can be expressed by the following [Formula C]. Erosion rate in each cycle (μm / g) = Depth of cross-sectional profile progressed in each cycle (μm) / Amount of test liquid sprayed in each cycle (g) [Formula C]
[0106] In formula C, "depth (μm) of the cross-sectional profile progressed in each cycle" means a value represented by "yx" when the depth of the cross-sectional profile in the nth cycle is defined as x (μm) and the depth of the cross-sectional profile in the (n+1)th cycle is defined as y (μm). In addition, for the first cycle, the depth (μm) of the cross-sectional profile in the first cycle corresponds to "depth (μm) of the cross-sectional profile progressed in each cycle." In this specification, the depth of the cross-sectional profile in the nth cycle means the depth of the deepest position of the cross-sectional profile in the nth cycle (n is an integer of 1 or more).
[0107] In formula C, the "amount of test liquid sprayed in each cycle (g)" is, in principle, a "fixed amount," but slight variations from cycle to cycle are acceptable. The amount of test liquid sprayed in each cycle is not particularly limited, but the lower limit is preferably 0.3 g or more, more preferably 0.5 g or more, and the upper limit is preferably 3.0 g or less, more preferably 2.0 g or less.
[0108] Before measuring the above-mentioned erosion rate, the above-mentioned calibration is carried out.
[0109] The test liquid used for calibration shall be the same as the test liquid used under the measurement conditions to be carried out later. In addition, the measurement device used in the calibration is the same as the measurement conditions used later. Measuring Equipment shall be considered the same as The difference between the calibration and the measurement conditions to be carried out later is, for example, that the calibration uses a 2 mm thick acrylic plate as a standard sample, whereas the measurement conditions use a laminate as a sample.
[0110] The 2 mm thick acrylic plate serving as the standard sample is preferably a polymethyl methacrylate plate. In addition, when the average erosion rate of the acrylic plate measured under the following measurement condition A is defined as AcE, the 2 mm thick acrylic plate serving as the standard sample is preferably one having an AcE of 0.1615 μm / g or more and 0.1785 μm / g or less. In addition, an example of the spherical silica under the following measurement condition A is the model number "MSE-BS-5-3" specified by Palmeso. An example of the spherical silica corresponding to the model number "MSE-BS-5-3" specified by Palmeso is the product number "BS5-3" by Potters Ballotini.
[0111] <Measurement condition A> A test liquid obtained by mixing pure water, a dispersant, and spherical silica with an average particle size of 5.0 μm within ±8% at a mass ratio of 968:2:30 is placed in a container. The test liquid in the container is sent to a nozzle. Compressed air is sent into the nozzle to accelerate the test liquid in the nozzle, and a predetermined amount of the test liquid is sprayed perpendicularly to the acrylic plate from the spray hole at the tip of the nozzle, causing the spherical silica in the test liquid to collide with the acrylic plate. The cross-sectional shape of the nozzle is a square of 1 mm x 1 mm, and the distance between the spray hole and the acrylic plate is 4 mm. In addition, the flow rates of the test liquid and the compressed air supplied to the nozzle, the pressure of the compressed air, and the pressure of the test liquid in the nozzle are as follows: flow rate of test liquid is 125 ml / min or more and 128 ml / min or less, flow rate of compressed air is 4.5 L / min or more and 4.8 L / min or less, pressure of compressed air is 0.174 MPa or more and 0.180 Pa or less, and pressure of test liquid in the nozzle is 0.155 MPa or more and 0.160 MPa or less. After 4 g of the test liquid was sprayed, the spraying of the test liquid was temporarily stopped. After the spraying of the test liquid is temporarily stopped, a cross-sectional profile is measured at the point on the acrylic plate where the spherical silica in the test liquid collided. Then, the erosion rate of the acrylic plate, AcE (unit: μm / g), is calculated by dividing the depth (μm) of the cross-sectional profile by the amount of the test liquid sprayed (4 g).
[0112] In the calibration, with the erosion rate of the acrylic plate being within the range of ±5% based on 0.17 (μm / g) as the pass condition, the operation of adjusting the flow rates of the test liquid and the compressed air, the pressure of the compressed air, and the pressure of the test liquid in the nozzle is carried out so that the erosion rate of the acrylic plate falls within the above range. Note that "the erosion rate is within the range of ±5% based on 0.17 (μm / g)" means, in other words, that the erosion rate is 0.1615 (μm / g) or more and 0.1785 (μm / g) or less.
[0113] [Film for Lamination] The film for lamination of the present disclosure has at least an adhesive layer, a plastic film, and a hard coat layer including a cured product of a curable resin composition in this order, and the softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship F1 < F2.
[0114] Figs. 6 to 7 are cross-sectional views showing embodiments of the film for lamination of the present disclosure. The film for lamination 20A in Figs. 6 to 7 has an adhesive layer 21, a plastic film 22, and a hard coat layer 23 including a cured product of a curable resin composition in this order. Further, the film for lamination 20A in Fig. 7 has an antireflection layer 24 on the side opposite to the plastic film 22 of the hard coat layer 23.
[0115] Embodiments of the layer configuration of the film for lamination of the present disclosure include embodiments similar to the layer configuration of the adjacent layers constituting the laminate of the present disclosure described above. Also, as embodiments of the adhesive layer, the plastic film, the hard coat layer, and other layers included as necessary that constitute the film for lamination of the present disclosure, there are embodiments of the adhesive layer, the plastic film, the hard coat layer, and other layers included as necessary that constitute the adjacent layers described above. In addition, the film for lamination of the present disclosure may have a separator on the side opposite to the plastic film of the adhesive layer. The separator only needs to be peelable and removable during the molding of the laminate, and may be a paper separator or a film separator.
[0116] [Method for manufacturing laminate] The laminate of the present disclosure is preferably manufactured by vacuum pressure air molding. Vacuum pressure air molding has, for example, the following steps (1) to (5). (1) A step of arranging an adherend in the lower vacuum chamber of a vacuum pressure air machine having an upper vacuum chamber and a lower vacuum chamber so that the first main surface side faces upward. (2) A step of arranging the following film for lamination between the upper vacuum chamber and the lower vacuum chamber so that the adhesive layer faces downward. [Film for lamination] A film for lamination having at least an adhesive layer, a plastic film, and a hard coat layer containing a cured product of a curable resin composition in this order, and satisfying the relationship F1 < F2 between the softening point F1 of the plastic film and the softening point F2 of the hard coat layer. (3) A step of evacuating the upper vacuum chamber and the lower vacuum chamber. (4) A step of pressing the first main surface of the adherend against the heated film for lamination by pushing up the adherend to the upper vacuum chamber while heating the film for lamination. (5) A step of closely adhering the film for lamination to the exposed surface of the adherend by pressurizing the upper vacuum chamber while the film for lamination is heated.
[0117] Hereinafter, embodiments of each step will be described with reference to FIG. 8. Step (1) is a step of arranging the adherend 10 in the lower vacuum chamber 31 of a vacuum pressure air machine having an upper vacuum chamber 32 and a lower vacuum chamber 31 so that the first main surface side faces upward (see FIG. 8(a)).
[0118] As shown in Fig. 8(a), a general-purpose vacuum laminating machine has two upper and lower vacuum chambers, an upper vacuum chamber 32 and a lower vacuum chamber 31. Further, in the lower vacuum chamber 31 of the general-purpose vacuum laminating machine, a table 33 that can move up and down is installed. In step (1), the adherend 10 is placed on the table 33, for example, with the first main surface side facing upward.
[0119] Step (2) is a step of disposing the following laminating film 20A between the upper vacuum chamber 32 and the lower vacuum chamber 31 with the adhesive layer facing downward (see Fig. 8(a)). <Laminating film> A laminating film having at least an adhesive layer, a plastic film, and a hard coat layer containing a cured product of a curable resin composition in this order, and the softening point F1 of the plastic film and the softening point F2 of the hard coat layer satisfy the relationship F1 < F2.
[0120] The general-purpose vacuum laminating machine is provided with a jig for setting a laminating film that covers the adherend between the upper and lower vacuum chambers. In step (2), the laminating film 20A is disposed, for example, by the jig with the adhesive layer facing downward. In steps (1) and (2), the upper and lower vacuum chambers are in a state of being open to atmospheric pressure.
[0121] Step (3) is a step of evacuating the upper vacuum chamber 32 and the lower vacuum chamber 31 (see Fig. 8(b)). During evacuation, after closing the upper and lower vacuum chambers respectively, the upper and lower vacuum chambers are evacuated respectively to make the inside vacuum (for example, a vacuum pressure of 0.1 Pa or more and 100 Pa or less).
[0122] Step (4) is a step of pressing the first main surface of the adherend 10 against the heated laminating film 20A by pushing up the adherend 10 to the upper vacuum chamber while heating the laminating film 20A (see Fig. 8(c)).
[0123] In step (4), the means for pushing up the adherend to the upper vacuum chamber includes, for example, means for raising the table of the lower vacuum chamber.
[0124] In steps (4) and (5), the lamination film is preferably heated so that the surface temperature of the hard coat layer side of the lamination film relative to the plastic film exceeds the softening point F1 of the plastic film. By setting such temperature conditions, the moldability becomes better, and the side surface of the adherend can be easily covered with the lamination film as an adjacent layer. In steps (4) and (5), the surface temperature of the hard coat layer side of the lamination film based on the plastic film is preferably 160°C or less, more preferably 150°C or less, and even more preferably 140°C or less.
[0125] In steps (4) and (5), the heat treatment can be performed, for example, by using a lamp heater installed in the ceiling of the upper vacuum chamber. In steps (4) and (5), the upper and lower vacuum chambers are separated by a partition plate 34 or the like.
[0126] Step (5) is a step of adhering the lamination film to the exposed surface of the adherend by pressurizing the upper vacuum chamber while the lamination film is heated (see FIG. 8(d)).
[0127] In step (5), the upper vacuum chamber is pressurized to, for example, 2 MPa or more and atmospheric pressure or less. In step (5), the lamination film as the adjacent layer adheres to the exposed surface of the adherend, and further stretches following the shape of the exposed surface of the adherend, thereby obtaining a laminate in which the exposed surface of the adherend is covered with the lamination film as the adjacent layer. That is, if the first main surface and side surface of the adherend are exposed, a laminate in which the first main surface and side surface of the adherend are covered with the lamination film as the adjacent layer can be obtained. Also, if the first main surface and side surface of the adherend are exposed, and further, if a part of the second main surface of the adherend is exposed, a laminate in which the first main surface and side surface of the adherend and a part of the second main surface of the adherend are covered with the lamination film as the adjacent layer can be obtained.
[0128] After the step (5), it is preferable to further carry out the following steps (6) and (7) (see FIG. 8(e)). (6) A step of opening the upper and lower vacuum chambers to return the pressure to atmospheric pressure, and then removing the laminate. (7) A step of trimming off unnecessary portions of the lamination film adhered to the surface of the adherend 10.
[0129] [Image display device] The image display device according to the present disclosure has the above-described laminate according to the present disclosure on a display element. The laminate is preferably disposed such that the surface of the laminate facing the adherend faces the display element.
[0130] Examples of display elements include liquid crystal display elements; EL display elements such as organic EL display elements and inorganic EL display elements; plasma display elements; LED display elements such as mini LED display elements and micro LED display elements; and display elements using quantum dots. When the display element of the display device is a liquid crystal display element, a backlight is required on the surface of the liquid crystal display element opposite to the laminate.
[0131] The image display device may be an image display device equipped with a touch panel function. Examples of touch panels include resistive, capacitive, electromagnetic induction, infrared, and ultrasonic touch panels. The touch panel function may be provided within a display element, such as an in-cell touch panel liquid crystal display element, or a touch panel may be placed on the display element. EXAMPLES
[0132] The present disclosure will be specifically described below with reference to examples and comparative examples. Note that the present disclosure is not limited to the embodiments described in the examples.
[0133] 1. Measurement and Evaluation The laminates of the examples and comparative examples were subjected to the following measurements and evaluations. The results are shown in Tables 1 and 2.
[0134] 1-1. Softening point According to the steps (A1) to (A2) in the specification, samples for softening point measurement in which the cross sections of the laminates of the examples and comparative examples were exposed were prepared. The softening point F1 of the plastic film and the softening point F2 of the hard coat layer of the sample were measured using a nanoscale infrared spectroscopic analysis system "Anasys nano IR (product name)" manufactured by Bruker Nano Inc. and the following probe under the following measurement conditions. For Examples 2 to 8 and Comparative Example 2, the softening point F3 of the heat-sensitive adhesive layer was also measured. The softening points are shown in Tables 1 and 2. As described in the specification, the softening point F2 of the hard coat layer whose softening point was not measured between 33°C and 300°C was considered to be "over 300°C". <Measurement conditions> Heating rate: 5℃ / sec Start temperature: 33℃ ·Measurement upper limit temperature: 300℃ Measurement area: 20μm <Probe> -ThermaLever Probes, product name manufactured by Bruker Nano Inc. <<Probe Details>> Probe model numbers:AN2-300 Cantilever material:Si ·Resistor material: Doped Silicon ·Length: 300μm or less ·Thickness: 2μm or less ·Tip height: 3μm or more and 6μm or less ·Spring constant: 0.1 N / m or more and 0.6 N / m or less Resonant frequency: 15 kHz to 30 kHz Tip radius: <30nm ·Max.controllable temperature:400℃ Contact:Yes ·Intermittent contact: No
[0135] 1-2. Coating condition For the laminates of the Examples and Comparative Examples, whether the first main surface, side surface, and second main surface of the adherend were covered with the lamination film as an adjacent layer was visually confirmed, and the laminates were evaluated according to the following criteria. Comparative Examples 4 and 5 did not use the lamination film and were made of tempered glass alone, and therefore were marked with "-". <Evaluation of the first principal surface> A: The percentage of the first main surface covered with the lamination film is 99% or more. B: The percentage of the first main surface covered with the lamination film is 90% or more and less than 99%. C: The proportion of the first main surface covered with the lamination film is less than 90%. <Aspect evaluation> (Hereinafter, the "side surface on the first main surface side" refers to 90% of the total surface area of the side surface from the first main surface side.) A: The ratio of the side surface of the first main surface covered with the lamination film is 90% or more. A-: The percentage of the side surface of the first principal surface that is covered with the lamination film is 80% or more and less than 90%. B: The proportion of the side surface on the first principal surface side that is covered with the lamination film is 50% or more and less than 80%. C: The proportion of the side surface on the first principal surface side that is covered with the lamination film is 5% or more and less than 50%. D: The proportion of the side surface on the first principal surface side covered with the lamination film is less than 5%. <Evaluation of the second principal surface> A: The percentage of the area within 2 mm from the edge of the second main surface that is covered with the lamination film is 80% or more. A-: The percentage of the area within 2 mm from the edge of the second main surface that is covered with the lamination film is 70% or more and less than 80%. B: The percentage of the area within 2 mm from the edge of the second main surface that is covered with the lamination film is 50% or more and less than 70%. C: The percentage of the area within 2 mm from the edge of the second main surface that is covered with the lamination film is 5% or more and less than 50%. D: The percentage of the area within 2 mm from the edge of the second main surface that is covered with the lamination film is less than 5%.
[0136] 1-3. Shatterproof A DuPont impact test was carried out in accordance with JIS K5600-5-3. Specifically, a DuPont impact tester (model number: No. 451 DuPont impact tester (for coating film) manufactured by Toyo Seiki Seisakusho Co., Ltd.) was used, and a shot mold with a hemispherical tip with a radius of 15 mm was placed on the surface of the laminated film side of the laminated bodies of Examples 1 to 10 and Comparative Examples 1 to 3, and a weight of 600 g was dropped onto the shot mold from a height of 250 mm. The laminated bodies made of tempered glass alone of Comparative Examples 4 to 5 were also evaluated in the same manner. The surface of the laminated film side of the laminated bodies of Examples 1 to 10 and Comparative Examples 1 to 3 means the surface of the laminated bodies of Examples 1 to 10 and Comparative Examples 1 to 3 on the adjacent layer side. Thereafter, the state of scattering of glass fragments, which is the adherend, was visually confirmed and evaluated according to the following criteria. The evaluation of shatter resistance and the measurement of the in-plane phase, erosion rate, shape parameters, and scale parameters described below were performed in an atmosphere with a temperature of 23±5° C. and a humidity of 40% RH to 65% RH. In addition, before the start of the measurement or evaluation, the target sample was exposed to the above atmosphere for 30 minutes or more. A: Neither large fragments nor fine powder-like fragments were observed. B: No large fragments are observed, but a small amount of fine powder fragments are observed. C: No large fragments are observed, but a large amount of fine powder fragments are observed. D: Large debris observed, extremely dangerous.
[0137] 1-4. In-plane retardation of laminate Using an Otsuka Electronics Co., Ltd. product name "RETS-100," in accordance with the procedures described in the specification, the in-plane retardation Re2C of the region (i) near the center, the in-plane retardation Re2E of the region (ii) near the ends, and the in-plane retardation Re2O of the region (iii) other than near the center and near the ends of the laminates of Examples 1 to 10 and Comparative Examples 1 and 2 were measured.
[0138] 1-5. Measurement of erosion rate Using Palmeso's MSE tester, part number "MSE-A203", the erosion rates of the laminates in Examples 1 and 2 were measured at the following locations. The method for measuring the erosion rates was in accordance with the description in the main text of the specification. E1 / E2 and E3 / E4 are shown in Table 1. Erosion rate (E1) at the center of the laminate in the in-plane direction of the plastic film. Erosion rate (E2) near the edge in the in-plane direction of the plastic film of the laminate. The erosion rate was measured in an area within 3 mm from each of the four corners when the plastic film was viewed in a plan view, and the average of the four erosion rates was taken as E2. Erosion rate (E3) of the center of the hard coat layer of the laminate in the in-plane direction. Erosion rate (E4) near the edge of the hard coat layer of the laminate in the in-plane direction. The erosion rate was measured in an area within 3 mm from each of the four corners when the hard coat layer was viewed in plan, and the average of the four erosion rates was taken as E4.
[0139] 1-6.4-point bending test Using Shimadzu Corporation's product name "Autograph AGX-50kN", the shape parameters and scale parameters of the laminates of Examples 9 to 10 and Comparative Examples 3 to 5 were measured. The method for measuring the shape parameters and scale parameters was in accordance with the description in the specification.
[0140] 2. Preparation of Coating Solution The following coating solutions were prepared. Note that "parts" and "%" are by weight.
[0141] <Coating solution for hard coat layer 1> Urethane acrylate oligomer A 20.6 parts (Manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name "New Frontier R-1403M(70)-LM") (70% solids, MEK solvent) Monofunctional methacrylate monomer 18.8 parts (100% solids, benzyl methacrylate) Conductive polymer 7.5 parts (Polymer having quaternary ammonium base and acryloyl group) (50% solids, MEK / n-BuOH mixed solvent) (Mitsubishi Chemical Corporation, product name "Upimer UV H-6500") Photopolymerization initiator 0.9 parts (IGM Resins BV, product name "Omnirad 184") Leveling agent 0.1 parts (active ingredient: 0.005 parts) (Manufactured by DIC, product name "Megafac F-568") Dilution solvent 52.1 parts (MIBK / PGME / n-BuOH=85 / 7 / 8 mixture)
[0142] <Coating solution 2 for hard coat layer> Urethane acrylate oligomer A 13.3 parts (45% solids, MEK solvent) Monofunctional acrylate monomer 17.8 parts (100% solids, phenoxyethyl acrylate) Conductive polymer 6.7 parts (Polymer having quaternary ammonium base and acryloyl group) (50% solids, MEK / n-BuOH mixed solvent) (Mitsubishi Chemical Corporation, product name "Upimer UV H-6500") Trifunctional acrylate monomer 6.7 parts (Pentaerythritol triacrylate) (Nippon Kayaku Co., Ltd., solids content 100%) Photopolymerization initiator 0.9 parts (IGM Resins BV, product name "Omnirad 184") Leveling agent 0.1 parts (active ingredient: 0.005 parts) (Manufactured by DIC, product name "Megafac F-568") Dilution solvent 54.5 parts (MIBK / PGME / n-BuOH=85 / 8 / 7 mixture)
[0143] <Coating solution 3 for hard coat layer> Urethane acrylate oligomer A 49.6 parts (45% solids, MEK solvent) Photopolymerization initiator 1.0 parts (IGM Resins BV, product name "Omnirad 184") Leveling agent 0.1 parts (active ingredient: 0.005 parts) (Manufactured by DIC, product name "Megafac F-568") Dilution solvent 49.3 parts (MIBK / PGME / n-BuOH=80 / 17 / 13 mixture)
[0144] <Double-sided adhesive film for forming pressure-sensitive adhesive layer 1> A double-sided adhesive film (manufactured by PANAC Corporation, product name: PDS1-15HU75) having a 15 μm-thick transparent adhesive layer and separators on both sides was prepared.
[0145] <Coating solution for heat-sensitive adhesive layer 1> ·Thermoplastic resin 64.8 parts (Polyester resin, manufactured by Toyobo Co., Ltd., product name "Vylon 63SS") (30% solids, toluene / MEK solvent = 75 / 25) Photoinitiator 1.3 parts (IGM Resins BV, product name "Omnirad 184") Leveling agent 0.1 parts (active ingredient: 0.005 parts) (Manufactured by DIC, product name "Megafac F-568") Dilution solvent 33.8 parts (PGMEA / MEK=71 / 29 mixed liquid)
[0146] <Coating solution for heat-sensitive adhesive layer 2> ·Thermoplastic resin 41.4 parts (Polyester-based urethane resin, manufactured by Toyobo Co., Ltd., product name "Vylon UR4800") (32% solids, toluene / MEK solvent = 50 / 50) Polyfunctional monomer 4.6 parts Photopolymerization initiator 0.9 parts (IGM Resins BV, product name "Omnirad 184") Leveling agent 0.1 parts (active ingredient: 0.005 parts) (Manufactured by DIC, product name "Megafac F-568") Dilution solvent 53.0 parts (Toluene / MEK=90 / 10 mixture)
[0147] <Low refractive index layer coating solution 1> ·UV curable compound 2.1 parts (3-4 functional alkoxylated pentaerythritol acrylate, manufactured by Shin-Nakamura Chemical Co., Ltd., product name "NK Ester ATM-4PL") Photopolymerization initiator 0.2 parts (IGM Resins BV, product name "Omnirad 127") Hollow silica 3.7 parts (Average particle size 60nm) Solid Silica 0.5 parts (Average particle size 12nm) Fluorine-based antifouling agent 0.8 parts (active ingredient: 0.2 parts) Dilution solvent 92.7 parts (90 / 10 mixture of methyl isobutyl ketone and propylene glycol monomethyl ether acetate)
[0148] 3. Preparation of lamination film and laminate [Example 1] <Preparation of lamination film> A hard coat layer was formed by applying the hard coat coating solution 1 onto an acrylic film having a thickness of 40 μm (manufactured by Toyo Kohan Co., Ltd., product name: HX40-UF) so that the thickness after drying was 9 μm, drying, and irradiating with ultraviolet light. The acrylic film had an in-plane retardation Re1C of 3 nm in the region (i) near the center, an in-plane retardation Re1E of 4 nm in the region (ii) near the edge, and an in-plane retardation Re1O of 5 nm in the region (iii) other than the region near the center and the edge. Next, coating solution 1 for low refractive index layer was applied onto the hard coat layer so that the thickness after drying would be 100 nm, followed by drying and irradiating with ultraviolet light, thereby forming a single antireflection layer of a low refractive index layer. Next, one of the separators of the double-sided adhesive film 1 for forming the pressure-sensitive adhesive layer was peeled off to expose the adhesive side, and then the adhesive side was attached to the side of the acrylic film opposite the hard coat layer to obtain a lamination film of Example 1 having a separator, pressure-sensitive adhesive layer, acrylic film, hard coat layer and low refractive index layer in that order.
[0149] <Preparation of Laminate> The adherend was placed in the lower vacuum chamber of a vacuum pressurized machine having an upper vacuum chamber and a lower vacuum chamber, with the first main surface side facing upward. More specifically, the adherend was placed on a lifting platform in the lower vacuum chamber, with the first main surface side facing upward. The second main surface of the adherend was placed so that a region 3 mm from the end was exposed to the atmosphere. The adherend was a soda glass measuring 100 mm in length, 100 mm in width, and 1.8 mm in thickness, with R-chamfered ends of the first and second main surfaces. Next, the separator of the lamination film of Example 1 was peeled off, and then the lamination film was placed between the upper vacuum chamber and the lower vacuum chamber with the pressure-sensitive adhesive layer facing downward, and the lamination film was further fixed with a jig. Next, the upper and lower vacuum chambers were evacuated to 100 Pa or less. Next, while heating the lamination film, the adherend was pushed up to the upper vacuum chamber, and the first main surface of the adherend was pressed against the heated lamination film. Next, while the lamination film was heated, the upper vacuum chamber was pressurized at atmospheric pressure, so that the lamination film was adhered to the exposed surface of the adherend. In these steps, heating was performed from the ceiling of the upper vacuum chamber. Moreover, heating was performed under conditions where the surface temperature of the lamination film was stabilized at 140°C. Thereafter, the upper and lower vacuum chambers were opened to cool the laminate to room temperature, and the laminate was then taken out. Furthermore, the edges were trimmed to obtain the laminate of Example 1.
[0150] [Example 2] <Preparation of lamination film> A lamination film of Example 2 was obtained in the same manner as in Example 1, except that a heat-sensitive adhesive layer having a thickness of 8 μm was formed by applying and drying the heat-sensitive adhesive layer coating solution 1 on the surface of the acrylic film opposite to the hard coat layer. The lamination film of Example 2 has a heat-sensitive adhesive layer, an acrylic film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> The laminate of Example 2 was obtained in the same manner as Example 1, except that the lamination film of Example 1 was changed to the lamination film of Example 2, and further, the heat-sensitive adhesive layer of the lamination film of Example 2 was placed between the upper vacuum chamber and the lower vacuum chamber so that it faced downward.
[0151] [Example 3] <Preparation of lamination film> A lamination film of Example 3 was obtained in the same manner as in Example 2, except that the hard coat coating liquid 1 was changed to the hard coat coating liquid 2. The lamination film of Example 3 has a heat-sensitive adhesive layer, an acrylic film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> A laminate of Example 3 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Example 3.
[0152] [Example 4] <Preparation of lamination film> The same procedure as in Example 2 was repeated except that a low refractive index layer was not formed on the hard coat layer and the heat-sensitive adhesive layer coating liquid 1 was changed to the heat-sensitive adhesive layer coating liquid 2. Lamination Film The lamination film of Example 4 had a heat-sensitive adhesive layer, an acrylic film, and a hard coat layer in this order. <Preparation of Laminate> A laminate of Example 4 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Example 4.
[0153] [Example 5] <Preparation of lamination film> A lamination film of Example 5 was obtained in the same manner as in Example 2, except that the hard coat coating liquid 1 was changed to the hard coat coating liquid 2, and the heat-sensitive adhesive layer coating liquid 1 was changed to the heat-sensitive adhesive layer coating liquid 2. The lamination film of Example 5 has a heat-sensitive adhesive layer, an acrylic film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> A laminate of Example 5 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Example 5.
[0154] [Example 6] <Preparation of lamination film> A lamination film of Example 6 was obtained in the same manner as in Example 2, except that the hard coat coating liquid 1 was changed to the hard coat coating liquid 3 and the heat-sensitive adhesive layer coating liquid 1 was changed to the heat-sensitive adhesive layer coating liquid 2. The lamination film of Example 6 has a heat-sensitive adhesive layer, an acrylic film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> A laminate of Example 6 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Example 6.
[0155] [Example 7] <Preparation of lamination film> A lamination film of Example 7 was obtained in the same manner as in Example 2, except that the acrylic film was changed to an acrylic film having a thickness of 80 μm (manufactured by Sumitomo Chemical Co., Ltd., product name: W001GU80) and the heat-sensitive adhesive layer coating liquid 1 was changed to the heat-sensitive adhesive layer coating liquid 2. The acrylic film had an in-plane retardation Re1C of 2 nm in the region (i) near the center, an in-plane retardation Re1E of 6 nm in the region (ii) near the end, and an in-plane retardation Re1O of 7 nm in the region (iii) other than the center and end. The lamination film of Example 7 has a heat-sensitive adhesive layer, an acrylic film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> A laminate of Example 7 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Example 7.
[0156] [Example 8] <Preparation of lamination film> A lamination film of Example 8 was obtained in the same manner as in Example 2, except that the acrylic film was changed to a biaxially stretched polyethylene terephthalate film having a thickness of 80 μm. The polyethylene terephthalate film had an in-plane retardation Re1C of 850 nm in the region (i) near the center, an in-plane retardation Re1E of 891 nm in the region (ii) near the end, and an in-plane retardation Re1O of 884 nm in the region (iii) other than the region near the center and the region near the end. The lamination film of Example 8 has a heat-sensitive adhesive layer, a polyethylene terephthalate film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> A laminate of Example 8 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Example 8.
[0157] [Example 9] <Preparation of lamination film> The lamination film of Example 9 was the same as that of Example 1. <Preparation of Laminate> The laminate of Example 9 was obtained in the same manner as in Example 1, except that the adherend was changed to 1.3 mm thick tempered glass (130 mm long, 220 mm wide, reinforced layer thickness: 6 μm, tempered glass with R-chamfered edges on the first and second main surfaces).
[0158] [Example 10] <Preparation of lamination film> The lamination film of Example 10 was the same as that of Example 1. <Preparation of Laminate> The laminate of Example 10 was obtained in the same manner as in Example 1, except that the adherend was changed to 1.3 mm thick tempered glass (130 mm long, 220 mm wide, reinforced layer thickness: 10 μm, tempered glass with R-chamfered edges on the first and second main surfaces).
[0159] [Comparative Example 1] <Preparation of lamination film> Except for changing the acrylic film to a triacetyl cellulose film (Konica Minolta, Inc., product name KC8UA), a lamination film of Comparative Example 1 was obtained in the same manner as in Example 1. The lamination film of Comparative Example 1 has a separator, a pressure-sensitive adhesive layer, a triacetyl cellulose film, a hard coat layer, and a low refractive index layer in this order. In addition, the triacetyl cellulose film had an in-plane retardation Re1C of 1 nm in the region (i) near the center, an in-plane retardation Re1E of 1 nm in the region (ii) near the ends, and an in-plane retardation Re1O of 1 nm in the region (iii) other than near the center and near the ends. <Preparation of Laminate> The laminate of Comparative Example 1 was obtained in the same manner as Example 1, except that the lamination film of Example 1 was changed to the lamination film of Comparative Example 1 and the heating conditions were changed to conditions such that the surface temperature of the lamination film became 180°C.
[0160] [Comparative Example 2] <Preparation of lamination film> A lamination film of Comparative Example 2 was obtained in the same manner as in Example 2, except that the acrylic film was changed to a biaxially stretched polyethylene terephthalate film having a thickness of 80 μm, and the hard coat coating liquid 1 was changed to the hard coat coating liquid 3. The polyethylene terephthalate film had an in-plane retardation Re1C of 850 nm in the region (i) near the center, an in-plane retardation Re1E of 891 nm in the region (ii) near the end, and an in-plane retardation Re1O of 884 nm in the region (iii) other than the center and end. The lamination film of Comparative Example 2 has a heat-sensitive adhesive layer, a polyethylene terephthalate film, a hard coat layer, and a low refractive index layer in this order. <Preparation of Laminate> A laminate of Comparative Example 2 was obtained in the same manner as in Example 2, except that the lamination film of Example 2 was changed to the lamination film of Comparative Example 2.
[0161] [Comparative Example 3] By peeling off the separator of the film for lamination in Example 1, the pressure-sensitive adhesive layer was exposed. The surface of the film for lamination on the exposed pressure-sensitive adhesive layer side was laminated on a tempered glass with a thickness of 1.3 mm (130 mm in length, 220 mm in width, thickness of the reinforcing layer: 6 μm, and the edges of the first main surface and the second main surface being R chamfered) to obtain the laminate of Comparative Example 3.
[0162] [Comparative Example 4] As the laminate of Comparative Example 4, a single piece of tempered glass with a thickness of 1.3 mm was prepared (130 mm in length, 220 mm in width, thickness of the reinforcing layer: 6 μm, and the edges of the first main surface and the second main surface being R chamfered).
[0163] [Comparative Example 5] As the laminate of Comparative Example 5, a single piece of tempered glass with a thickness of 1.3 mm was prepared (130 mm in length, 220 mm in width, thickness of the reinforcing layer: 10 μm, and the edges of the first main surface and the second main surface being R chamfered).
[0164]
Table 1
[0165]
Table 2
[0166] As is clear from Tables 1 and 2, it can be confirmed that the laminate of the example can suppress not only the scattering of large fragments but also the scattering of powdery fine fragments when the protective plate cracks due to impact. Further, from the comparison between Examples 1 to 7 and Example 8, since F1 < F2 and the Re1 of the plastic film is 100 nm or less, a synergistic effect is produced, and it can be confirmed that the first main surface and the side surface of the adherend can be extremely easily coated and the scattering prevention property can be improved. Further, from the comparison between Examples 9 to 10 and Comparative Examples 3 to 5, it can be confirmed that the laminate with a shape parameter of 16.0 or less can improve the scattering prevention property.
Explanation of Reference Signs
[0167] 10: Adherent 10a: First principal surface 10b: Second principal surface 10c: Side 20: Adjacent layer 20A: Lamination film 21: Adhesive layer 22: Plastic film 23: Hard coat layer 24: Anti-reflection layer 30: Vacuum pressure machine 31, 32: Vacuum chamber 33: stand 34: Partition plate 100: Laminate 200: Load span 201: Load pin 202: Foundation 300: Support span 301: Support pin 302: Foundation 1100: Container 1200: Receptor 2100: Test liquid piping 2200: Compressed air piping 2300: Return piping 3100, 3200: Flowmeter 4100, 4200: Pressure gauge 5000: Injection part 5100: Nozzle 5200: Chassis 6000: Cross-sectional profile acquisition section 8100: Sample mounting stand 8200: Support 100: Erosion rate measuring device A1: Water A2: Spherical silica A3: Air A4: Abraded laminate
Claims
1. A laminate having an adherend and an adjacent layer, The adherend has a first main surface, a second main surface on a back surface of the first main surface, and a side surface connecting an end portion of the first main surface and an end portion of the second main surface, the first main surface and the side surface of the adherend are covered with the adjacent layer, and a vicinity of an end portion of the second main surface of the adherend is covered with the adjacent layer; the adjacent layer is formed continuously over the first main surface, the side surface, and the vicinity of an end portion of the second main surface; the adjacent layer is a lamination film having, from the adherend side, at least an adhesive layer, a plastic film, and a hard coat layer including a cured product of a curable resin composition, in this order; A laminate, wherein a softening point F1 of the plastic film and a softening point F2 of the hard coat layer satisfy the relationship F1<F2.
2. The laminate according to claim 1 , wherein the adherend is glass.
3. The laminate according to claim 1 or 2, wherein the outer peripheral edge of the first main surface of the adherend is chamfered over substantially the entire periphery.
4. The laminate according to any one of claims 1 to 3, wherein the softening point F1 of the plastic film is 70°C or higher and 150°C or lower.
5. 5. The laminate according to claim 1, wherein, when the average in-plane retardation of the plastic film is defined as Re1, Re1 is 100 nm or less.
6. 6. The laminate according to claim 1, wherein, when an average in-plane retardation of the laminate is defined as Re2, Re2 is 100 nm or less.
7. 7. The laminate according to claim 6, wherein, when an in-plane retardation near a center of the laminate is defined as Re2C and an in-plane retardation near an end of the laminate is defined as Re2E, an absolute value of a difference between Re2C and Re2E is 10 nm or less.
8. The laminate according to any one of claims 1 to 7, wherein the hard coat layer has a thickness of 1 µm or more and 20 µm or less.
9. The laminate of claim 1, wherein the adhesive layer is a heat-sensitive adhesive layer.
10. 10. The laminate according to claim 1, wherein the adjacent layer is a lamination film having an anti-reflection layer on the side of the hard coat layer opposite to the plastic film.
11. The laminate according to any one of claims 1 to 10, wherein the following shape parameter is 16.0 or less. <Calculation of shape parameters and scale parameters by four-point bending test> The laminate is cut into 20 samples with a width of 130 mm. The samples are placed on a support span so that the second main surface of the adherend faces the support span, and then a four-point bending test is performed on each sample to measure the breaking stress of each sample. The test conditions are a support distance of 20 mm in the load span, a support distance of 40 mm in the support span, and a loading speed of 5 mm / min. The shape parameters and scale parameters of the laminate are calculated by performing a Weibull distribution analysis on the 20 measured values of the breaking stress.
12. A method for producing a laminate having an adherend and an adjacent layer, comprising: The adherend has a first main surface, a second main surface on a back surface of the first main surface, and a side surface connecting an end portion of the first main surface and an end portion of the second main surface, A method for producing a laminate, comprising the following steps (1) to (5): (1) A step of placing an adherend in a lower vacuum chamber of a vacuum pressurized air machine having an upper vacuum chamber and a lower vacuum chamber, with a first main surface facing upward. (2) A step of placing the lamination film described below between the upper vacuum chamber and the lower vacuum chamber with the adhesive layer facing downward. <Lamination film> A lamination film having at least an adhesive layer, a plastic film, and a hard coat layer containing a cured product of a curable resin composition, in that order, wherein a softening point F1 of the plastic film and a softening point F2 of the hard coat layer satisfy the relationship F1<F2. (3) A step of drawing a vacuum in the upper and lower vacuum chambers. (4) A step of pressing a first main surface of the adherend against the heated lamination film by pushing the adherend up to the upper vacuum chamber while heating the lamination film. (5) A step of adhering the lamination film to the exposed surface of the adherend by applying pressure to the upper vacuum chamber while the lamination film is heated, thereby forming a continuous adjacent layer over the first main surface, the side surface, and the vicinity of the end of the second main surface.
13. 13. The method for producing a laminate according to claim 12, wherein in the steps (4) and (5), the lamination film is heated so that a surface temperature of the hard coat layer side of the lamination film relative to the plastic film exceeds a softening point F1 of the plastic film.
14. A lamination film having at least a heat-sensitive adhesive layer, a plastic film, and a hard coat layer containing a cured product of a curable resin composition, in that order, wherein a softening point F1 of the plastic film and a softening point F2 of the hard coat layer satisfy the relationship F1<F2.
15. An image display device comprising the laminate according to any one of claims 1 to 11 on a display element.
Citation Information
Patent Citations
Method for manufacturing display panel and transparent tacky adhesive sheet
JP2005309021A
Decorative scattering prevention film for image display panel, and image display panel
JP2013178332A
Glass with scattering prevention performance
JP2015171770A
Protective cover and manufacturing method therefor
JP2019029845A
Glass sheet with antifouling layer
WO2017026318A1