Infrared reflective sheet

The use of a specific infrared-transmissive dark ink with a brown and phthalocyanine pigment composition addresses the temperature rise and appearance issues in solar cell modules, improving power generation efficiency by transmitting near-infrared rays and maintaining a dark appearance.

JP7571821B2Active Publication Date: 2024-10-23DAI NIPPON PRINTING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023092597
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-09-30
Filing Date
2023-06-05
Publication Date
2024-10-23
Estimated Expiration
2035-09-30

AI Technical Summary

Technical Problem

Existing solar cell modules face issues with increased temperature due to near-infrared ray absorption, leading to decreased power generation efficiency, and conventional infrared-transmissive dark inks do not provide a satisfactory black appearance and adequate infrared transmittance.

Method used

An infrared-transmissive dark ink containing a pigment component comprising a brown pigment and a phthalocyanine pigment, with a specific composition and content, is used to form a dark layer that transmits near-infrared rays, suppressing heat generation and maintaining a dark appearance.

Benefits of technology

The infrared-transmissive dark ink effectively reduces heat generation in solar cell modules by transmitting near-infrared rays, enhancing power generation efficiency while providing a desirable dark appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571821000009
    Figure 0007571821000009
  • Figure 0007571821000010
    Figure 0007571821000010
  • Figure 0007571821000011
    Figure 0007571821000011
Patent Text Reader

Abstract

To provide an infrared reflection sheet which also has sufficient infrared reflectivity in spite of having high design properties with black appearance.SOLUTION: Disclosed is an infrared ray reflective sheet formed by laminating an infrared ray transmitting dark color layer on the surface of a reflection layer reflecting near infrared rays. The infrared ray transmitting dark color layer contains a main resin having a hydroxyl group, a curing agent having an isocyanate group, and a pigment component. The pigment component contains a brown pigment and a dark pigment composed of a phthalocyanine pigment.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an infrared reflective sheet. [Background technology]

[0002] In recent years, solar cells have been attracting attention as a clean energy source due to the growing awareness of environmental issues. In general, a solar cell module constituting a solar cell is configured by laminating a transparent front substrate, a sealing material, a solar cell element, a sealing material, and a back protective sheet in this order from the light-receiving surface side, and has a function of generating electricity when sunlight is incident on the solar cell element.

[0003] For example, in the case of inks used in solar cell modules, etc., there are cases where inks with a black appearance are required from the viewpoint of design. One method for achieving a dark appearance is to use an ink containing carbon black, but carbon black absorbs near-infrared rays, which causes an increase in temperature, and therefore is not necessarily preferable when used in solar cell modules, etc.

[0004] When used as a back surface protective sheet for a solar cell module, it increases the temperature of the solar cell module during use, resulting in a decrease in the power generation efficiency of the solar cell module.

[0005] Therefore, in order to suppress heat generation in the dark layer and further improve power generation efficiency by allowing reflected light to enter the solar cell element, a back surface protection sheet for a solar cell module has been developed which is manufactured by bonding a plurality of layers with an adhesive or the like, and which includes a black resin layer containing an organic pigment such as an oxazine pigment having infrared transmissibility, a white resin layer having infrared reflectivity, and a weather-resistant back surface protection layer, etc. (Patent Document 1).

[0006] An infrared-transmitting dark ink containing an oxazine-based pigment and a curing agent is an infrared-transmitting dark ink with high adhesion durability (Patent Document 1

[0057] ). However, since the oxazine-based pigment transmits light with a wavelength of 700 to 800 nm, the oxazine-based pigment itself is a pigment closer to purple than black. Therefore, an infrared-transmitting dark ink containing an oxazine-based pigment in a resin is closer to purple, which is not necessarily preferable when a black appearance is required from the viewpoint of design.

[0007] In particular, when used as a back protective sheet for a solar cell module, the demand for power generation efficiency of the solar cell module is becoming stronger, so an infrared-transmitting dark ink that transmits and reflects infrared rays is required. This is because suppressing absorption of near-infrared rays suppresses the temperature rise of the solar cell module, and using infrared rays to generate power can further increase the power generation efficiency of the solar cell module. Therefore, it is important to use an infrared-transmitting dark ink that transmits infrared rays more. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2012-216689 A Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide an excellent infrared-transmitting dark ink that is capable of imparting a dark appearance to a rear protective sheet for a solar cell module and that has high near-infrared transmittance. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to solve the above problems. As a result, they have found that the above problems can be solved by an infrared-transmitting dark ink containing a pigment component that includes a specified brown pigment and a phthalocyanine pigment, and have completed the present invention. More specifically, the present invention provides the following.

[0011] (1) An infrared-transmitting dark ink that transmits near-infrared rays having a wavelength of 750 nm or more and 1500 nm or less, the ink contains a resin component and a pigment component, the pigment component contains a brown pigment and a dark pigment made of a phthalocyanine pigment, the brown pigment being selected from the group consisting of benzimidazolone pigments, 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide, 1-[(4-nitrophenyl)azo]-2-naphthalenol, bis[3-hydroxy-4-(phenylazo)-2-naphthalenecarboxylic acid] copper salt, CIPig An infrared-transmitting dark ink comprising at least one pigment selected from the group consisting of mentBrown7, N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl-4,4'-diamine, 3,4,9,10-perylenetetracarboxylic acid diimide, Δ2,2'(1H,1'H)-binaphtho[2,1-b]thiophene-1,1'-dione, and N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide).

[0012] (2) The content of the dark pigment in the pigment component is 80% by mass or more, The infrared-transmitting dark ink according to (1), wherein the transmittance of light having a wavelength of 425 nm is 5% or more and 30% or less, and the transmittance of light having a wavelength of 675 nm is 4% or more and 20% or less, in a light transmittance test of the infrared-transmitting dark ink.

[0013] (3) The infrared-transmitting dark ink according to (1) or (2), wherein the pigment component is contained in an amount of 20 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the resin component.

[0014] (4) An infrared reflective sheet comprising an infrared-transmitting dark layer laminated on the surface of a reflective layer that reflects near-infrared rays of 750 nm or more and 1500 nm or less, the infrared-transmitting dark layer containing a base resin having a hydroxyl group, a curing agent having an isocyanate group, and a pigment component, the pigment component containing a brown pigment and a dark pigment consisting of a phthalocyanine pigment, the brown pigment being selected from the group consisting of benzimidazolone pigment, 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide, 1-[(4-nitrophenyl)azo]-2-naphthalenol, bis[3-hydroxy-4-( An infrared reflective sheet comprising at least one pigment selected from the group consisting of N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl-4,4'-diamine, 3,4,9,10-perylenetetracarboxylic acid diimide, Δ2,2'(1H,1'H)-binaphtho[2,1-b]thiophene-1,1'-dione, and N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide).

[0015] (5) The infrared reflective sheet according to (4), further comprising a transparent adhesive layer laminated on the surface of the infrared reflective sheet on the side where the infrared transmissive dark layer is laminated.

[0016] (6) An infrared reflective sheet comprising an infrared-transmitting dark layer and a transparent resin layer laminated in this order on the surface of a reflective layer that reflects near-infrared rays of 750 nm or more and 1500 nm or less, the infrared-transmitting dark layer containing a base resin having a hydroxyl group, a curing agent having an isocyanate group, and a pigment component, the pigment component being 20 parts by mass or more and 40 parts by mass or less per 100 parts by mass of the base resin, the pigment component containing a brown pigment and a dark pigment consisting of a phthalocyanine pigment, the brown pigment being selected from the group consisting of benzimidazolone pigment, 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide, 1-[(4-nitrophenyl)azo] -2-naphthalenol, bis[3-hydroxy-4-(phenylazo)-2-naphthalenecarboxylic acid] copper salt, CI Pigment Brown 7, N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl-4,4'-diamine, 3,4,9,10-perylenetetracarboxylic acid diimide, Δ2,2'(1H,1'H)-binaphtho[2,1-b]thiophene-1,1'-dione, and N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide).

[0017] (7) The coating amount of the infrared-transmitting dark ink forming the infrared-transmitting dark layer is 5 g / m2 in terms of solid content. 2 More than 15g / m 2 The infrared reflective sheet according to (6) below.

[0018] (8) The color difference ΔE between the color tone of the infrared-transmitting dark layer and the color tone of carbon black measured under conditions of D65 light source and 10° viewing angle in accordance with JIS-Z8722 * The infrared reflective sheet according to any one of (4) to (7), wherein ab is 10 or less.

[0019] (9) A back surface protective sheet for a solar cell module, comprising a laminate of a plurality of layers including at least a transparent adhesive layer that transmits all light rays and a reflective layer that reflects near-infrared rays of 750 nm or more and 1500 nm or less, wherein two of the layers laminated between the transparent adhesive layer and the reflective layer are an infrared-transmitting dark layer and a transparent adhesive layer, the infrared-transmitting dark layer includes a base resin having a hydroxyl group, a curing agent having an isocyanate group, and a pigment component, the pigment component included in the infrared-transmitting dark layer is 20 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the base resin, the pigment component includes a brown pigment and a dark pigment consisting of a phthalocyanine pigment, the brown pigment being selected from the group consisting of a benzimidazolone pigment, 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide, and the like. imide, 1-[(4-nitrophenyl)azo]-2-naphthalenol, bis[3-hydroxy-4-(phenylazo)-2-naphthalenecarboxylic acid] copper salt, CI Pigment Brown 7, N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl-4,4'-diamine, 3,4,9,10-perylenetetracarboxylic diimide, Δ2,2'(1H,1'H)-binaphtho[2,1-b]thiazide An infrared reflective sheet comprising at least one pigment selected from the group consisting of 1,1'-phenylenedione and N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide), and having an NCO / OH ratio, which is the ratio of the NCO value of the curing agent to the OH value of the base resin, of 1.0 or more and 2.0 or less.

[0020] (10) The coating amount of the infrared-transmitting dark ink forming the infrared-transmitting dark layer is 3 g / m2 in terms of solid content. 2 More than 7g / m 2 The infrared reflective sheet according to (9) below.

[0021] (11) The infrared reflective sheet according to (9) or (10), wherein the curing agent having an isocyanate group is a diisocyanate compound.

[0022] (12) The infrared reflective sheet according to any one of (9) to (11), wherein the infrared-transmitting dark layer is laminated only on a part of the surface of the transparent adhesive layer and / or the reflective layer.

[0023] (13) An infrared reflective sheet according to any one of (4) to (12), further comprising an infrared-transmitting coating layer containing a dark-colored organic pigment laminated on the surface of the reflective layer opposite to the surface on which the infrared-transmitting dark layer is laminated, the infrared-transmitting coating layer transmitting near-infrared rays having a wavelength of 750 nm or more and 1500 nm or less.

[0024] (14) A solar cell module comprising the infrared reflective sheet according to any one of (4) to (13) laminated on the non-light-receiving side of a solar cell element. Effect of the Invention

[0025] The infrared-transmitting dark ink of the present invention can suppress heat generation caused by absorption of near-infrared rays even in an environment where it is irradiated with sunlight. Moreover, the infrared-reflective sheet of the present invention obtained by using the infrared-transmitting dark ink of the present invention in an infrared-reflective sheet (rear surface protective sheet) for a solar cell module is an excellent infrared-reflective sheet that suppresses heat generation caused by absorption of near-infrared rays while fully satisfying design requirements, and also contributes to increasing the power generation efficiency of the solar cell module when used as a rear surface protective sheet for the solar cell module. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of a solar cell module. [Diagram 2] This is a diagram provided for explaining the layer structure of the infrared reflective sheet, and is an enlarged schematic diagram of a cross section of the infrared reflective sheet integrated with a solar cell module when the infrared reflective sheet is used as a back surface protective sheet for a solar cell module. [Diagram 3] 1 is a graph showing infrared reflectance in Example 1 and Comparative Example 1. [Figure 4] FIG. 1 is a diagram showing color coordinates of Examples 2 to 4. [Diagram 5] FIG. 1 is a diagram showing color coordinates of Comparative Examples 2 to 6. [Figure 6] This is a diagram provided for explaining the layer structure of an infrared reflective sheet of another embodiment, and is an enlarged schematic diagram of a cross section of the infrared reflective sheet integrated with a solar cell module when the infrared reflective sheet is used as a back protective sheet for a solar cell module. [Figure 7] FIG. 1 is a diagram showing color coordinates of Examples 13 to 15. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The infrared-transmitting dark ink of the present invention will be described in detail below, but the present invention is not limited to the embodiments described below.

[0028] <Infrared-transmitting dark ink> The infrared-transmitting dark ink of the present invention can be used for applications such as coloring a back protective sheet for a solar cell module in a dark color from the viewpoint of design. In addition, since the infrared-transmitting dark ink of the present invention has a high transmittance of near-infrared rays, it is possible to suppress heat generation caused by absorption of near-infrared rays. For example, by forming an infrared-transmitting dark layer 60 using the infrared-transmitting dark ink of the present invention on the surface of a reflective sheet capable of reflecting near-infrared rays, it is possible to manufacture an infrared reflective sheet that can reflect near-infrared rays while having a dark appearance.

[0029] Furthermore, the infrared-transmitting dark ink of the present invention becomes an infrared-transmitting dark ink capable of bonding sheets together by containing a curing agent in the infrared-transmitting dark ink. For example, an infrared-transmitting dark layer can be formed by applying the infrared-transmitting dark ink containing a curing agent onto a sheet, laminating another sheet, and curing the infrared-transmitting dark ink.

[0030] Furthermore, an infrared reflective sheet 6 may be produced by sequentially laminating an infrared-transmitting dark layer 60 and a transparent adhesive layer 62 on the surface of a reflective layer 61 that reflects near-infrared rays. For example, the infrared reflective sheet 6 of the present invention can be used as a back surface protective sheet for a solar cell module by placing it on the non-light-receiving side of a solar cell element.

[0031] From the viewpoint of design, there are cases where the infrared reflective sheet 6 is required to be partially colored, for example, to provide a pattern such as a patterning, rather than having the entire surface of the infrared reflective sheet 6 dark. When the infrared reflective sheet 6 of the embodiment in Fig. 6 is used as a back surface protection sheet for a solar cell module, the back surface protection sheet is excellent in design and can maintain high power generation efficiency as in the past, becoming an excellent back surface protection sheet for a solar cell module. The infrared reflective sheet 6 of the embodiment in Fig. 6 will be described later.

[0032] 2 or 6, the infrared reflective sheet can be formed by laminating and curing an infrared-transmitting dark ink applied to the upper surface of the reflective layer 61 or the lower surface of the transparent adhesive layer 62 facing the upper surface. By forming the infrared-transmitting dark layer 60 at a position between the reflective layer 61 and the transparent adhesive layer 62, the infrared reflective sheet 6 can be made preferable in terms of design.

[0033] It is important that the infrared-transmitting dark ink that forms the infrared-transmitting dark layer 60 has a black or nearly black appearance, that is, has the property of absorbing visible light and transmitting near-infrared light.

[0034] Here, near-infrared radiation is the region of infrared radiation that is closest to the visible region, but the exact wavelength range varies depending on the literature. In the present invention, near-infrared radiation refers to electromagnetic waves in the wavelength range of 750 nm to 2200 nm. Of these, the wavelength that particularly promotes heat storage is 1000 nm to 1500 nm.

[0035] The infrared-transmitting dark ink used for forming the infrared-transmitting dark layer 60 has the property of transmitting light rays having wavelengths of 750 nm or more and 1500 nm or less in a cured state. Note that "transmitting light rays having wavelengths of 750 nm or more and 1500 nm or less" means that the infrared-transmitting dark layer 60 transmits 15% or more of light rays having wavelengths of 750 nm or more and 1500 nm or less, preferably transmits 50% or more, and more preferably transmits 60% or more.

[0036] The infrared-transmitting dark ink used in the infrared-transmitting dark layer 60 can be used to bond sheets together. When using the infrared-transmitting dark ink in this way, it is preferable that the ink is a two-liquid type consisting of a base agent and a curing agent. In addition, from the viewpoints of application and handling, the composition contains an appropriate solvent.

[0037] [Organic pigments] The pigment component contained in the infrared-transmitting dark ink of the present invention contains a dark pigment consisting of a brown pigment and a phthalocyanine pigment, the details of which will be described below. The infrared-transmitting dark ink of the present invention containing a pigment component containing such a dark pigment has a dark appearance and is an excellent ink with high infrared transmittance.

[0038] In this specification, brown pigments include benzimidazolone pigments, 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide, 1-[(4-nitrophenyl)azo]-2-naphthalenol, bis[3-hydroxy-4-(phenylazo)-2-naphthalenecarboxylic acid] copper salt, N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl, The term "brown pigment" refers to at least one pigment selected from the group consisting of 4,4'-diamine, 3,4,9,10-perylenetetracarboxylic acid diimide, Δ2,2'(1H,1'H)-binaphtho[2,1-b]thiophene-1,1'-dione, and N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide). The brown pigment is preferably a benzimidazolone pigment from the viewpoints of the dispersibility of the pigment in the adhesive layer and the adhesiveness of the adhesive layer. The benzimidazolone pigment is a pigment having a benzimidazolone skeleton represented by the following general formula (1). Specific examples include, but are not limited to, CI Pigment Yellow 120, CI Pigment Yellow 151, CI Pigment Yellow 154, CI Pigment Yellow 175, CI Pigment Yellow 180, CI Pigment Yellow 181, CI Pigment Yellow 194, CI Pigment Red 175, CI Pigment Red 176, CI Pigment Red 185, CI Pigment Red 208, CI Pigment Violet 32, CI Pigment Orange 36, CI Pigment Orange 62, CI Pigment Orange 72, and CI Pigment Brown 25. From the viewpoint of color gamut, CI Pigment Brown 25 is more preferable.

[0039] [ka]

[0040] The primary particle size of the benzimidazolone pigment is preferably from 0.01 μm to 0.20 μm, inclusive. By setting the primary particle size of the benzimidazolone pigment in this range, it is possible to improve the dispersibility of the pigment in the ink.

[0041] In addition, brown pigments other than benzimidazolone pigments will be described. 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide is specifically CI Pigment Brown 1. 1-[(4-nitrophenyl)azo]-2-naphthalenol is specifically CI Pigment Brown 2. Bis[3-hydroxy-4-(phenylazo)-2-naphthalenecarboxylic acid] copper salt is specifically CI Pigment Brown 5. N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl-4,4'-diamine is specifically CI Pigment Brown 22. 3,4,9,10-perylenetetracarboxylic acid diimide is specifically CI Pigment Brown 26. Specific examples of Δ2,2'(1H,1'H)-binaphtho[2,1-b]thiophene-1,1'-dione include CI Pigment Brown 27. Specific examples of N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide) include CI Pigment Brown 28. In addition to the above brown pigments, CI Pigment Brown 7 may also be used as the brown pigment.

[0042] The phthalocyanine pigment is a pigment having a phthalocyanine skeleton, and includes phthalocyanines coordinated with various metals. Specific examples include, but are not limited to, CI Pigment Green 7, CI Pigment Green 36, CI Pigment Green 37, CI Pigment Blue 16, CI Pigment Blue 75, and CI Pigment Blue 15. It is preferable to use an amorphous phthalocyanine pigment that is blue.

[0043] The primary particle size of the phthalocyanine pigment is preferably from 0.15 μm to 0.20 μm, in order to improve the dispersibility of the phthalocyanine pigment in the ink.

[0044] The content of the brown pigment in the infrared-transmitting dark ink is preferably 43 parts by mass or more and 233 parts by mass or less (the content ratio of the brown pigment to the phthalocyanine pigment is in the range of 30:70 to 70:30 by mass ratio) relative to 100 parts by mass of the phthalocyanine pigment, and more preferably 66 parts by mass or more and 150 parts by mass or less (the content ratio of the brown pigment to the phthalocyanine pigment is in the range of 40:60 to 60:40 by mass ratio). By setting the content ratio in such a range, the infrared-transmitting dark ink can be made preferable in terms of design and infrared transmittance.

[0045] The content of the brown pigment in the infrared-transmitting dark ink can be specified by the transmittance of light of a specific wavelength in a light transmittance test. In order to make the content of the brown pigment such as the benzimidazolone pigment and the content of the phthalocyanine pigment preferable in terms of design and infrared transmittance, the brown pigment such as the benzimidazolone pigment and the phthalocyanine pigment contained in the infrared-transmitting dark ink are 80 mass% or more of the total amount of pigment components, and the transmittance of light with a wavelength of 425 nm in the light transmittance test of the infrared-transmitting dark ink is preferably 5% to 30% and 4% to 20%. The phthalocyanine pigment has the property of transmitting a certain amount of light with a wavelength of 425 nm and not transmitting light with a wavelength of 675 nm. The brown pigment such as the benzimidazolone pigment has the property of transmitting a certain amount of light with a wavelength of 675 nm and not transmitting light with a wavelength of 425 nm. Therefore, by determining the transmittance of light having a wavelength of 425 nm and the transmittance of light having a wavelength of 675 nm in the light transmittance test, it is possible to determine the content ratio between the content of brown pigments such as benzimidazolone pigments and the content of phthalocyanine pigments.

[0046] The transmittance of the infrared-transmitting dark ink can be measured, for example, by the following method. 2The infrared reflective sheet is prepared by gravure coating the above-mentioned, laminating polyethylene (60 μm) thereon, and performing aging treatment at 45° C. to 55° C. for 168 hours to heat cure the sheet. The polyethylene and white PET of the infrared reflective sheet are then peeled off, and a measurement sample of the transmittance of a solution in which an infrared-transmitting dark layer (infrared-transmitting dark ink) is dissolved using methyl ethyl ketone is prepared (for example, the concentration of the pigment in the measurement sample is about 0.01 g to 0.5 g per 100 g of methyl ethyl ketone). The measurement sample is poured into a quartz glass cell, and the transmittance (%) of light with wavelengths of 300 nm to 1200 nm is measured using a spectrophotometer (for example, an ultraviolet spectrophotometer "V-670" manufactured by JASCO Corporation or "U-4100" manufactured by Hitachi High-Technologies Corporation). The transmittance (%) of light with wavelengths of 425 nm and 675 nm is calculated, and the content of the brown pigment in the infrared-transmitting dark ink can be estimated.

[0047] The transmittance of the infrared-transmitting dark layer formed by the infrared-transmitting dark ink can be measured by the following method. 2 A sample for measuring transmittance is prepared by gravure coating the above, laminating a similar fluorine film (100 μm) on top of it, dry laminating, and heat-curing the film by aging at 45° C. to 55° C. for 168 hours. The measurement sample is poured into a quartz glass cell, and the transmittance (%) of light with a wavelength of 300 nm to 1200 nm is measured using a spectrophotometer (for example, an ultraviolet spectrophotometer "V-670" manufactured by JASCO Corporation or "U-4100" manufactured by Hitachi High-Technologies Corporation), and the transmittance of light with a wavelength of 425 nm and light with a wavelength of 675 nm can be measured.

[0048] The infrared-transmitting dark ink of the present invention contains a pigment component. It is preferable that the infrared-transmitting dark ink contains 20 parts by mass or more and 40 parts by mass or less of the pigment component per 100 parts by mass of the resin component. Here, when the infrared-transmitting dark ink contains a pigment component containing an organic pigment such as an oxazine-based pigment, it is known that if the content of the pigment component is 30 parts by mass or more, it adversely affects the adhesiveness of the curing agent, and the adhesiveness of the infrared-transmitting dark layer 60 decreases. For this reason, it has been thought that it is difficult to use the infrared-transmitting dark ink, especially for bonding sheets together. However, brown pigments and phthalocyanine pigments have higher dispersibility than other pigments, and have a smaller effect on the adhesiveness of the curing agent. Therefore, even if the content ratio of the pigment component is 30 parts by mass or more per 100 parts by mass of the resin component, the decrease in the adhesiveness and adhesive durability of the infrared-transmitting dark layer 60 can be suppressed to a very small range. Furthermore, as described below, by increasing the blending ratio of the pigment component of the infrared-transmitting dark ink, the color tone of the infrared-transmitting dark layer 60 can be stabilized with a smaller coating amount. By setting the pigment component of the infrared-transmitting dark ink to 40 parts by mass or less per 100 parts by mass of the resin component, the infrared-transmitting dark layer 60 formed by the infrared-transmitting dark ink of the present invention can be an infrared-transmitting dark layer 60 having adhesiveness and adhesive stability.

[0049] The infrared-transmitting dark ink of the present invention may contain a curing agent as necessary. The infrared-transmitting dark ink of the present invention containing a curing agent can form an infrared-transmitting dark layer 60 that has good adhesion to a resin sheet. In addition, by adjusting the content of the curing agent contained in the infrared-transmitting dark ink, an infrared-transmitting dark layer 60 that can bond sheets together can be formed. Below, the base agent and the curing agent will be described as an embodiment that can constitute the resin component contained in the infrared-transmitting dark ink. Note that the resin component related to the present invention is not limited to the following embodiment.

[0050] [Main ingredient] The base component of the resin component may be, for example, a polyurethane / polycarbonate diol system containing a mixture of polyurethane diol and aliphatic polycarbonate diol. The polyurethane diol and aliphatic polycarbonate diol constituting the base are both polyols having hydroxyl groups, and react with a curing agent having an isocyanate group to form an adhesive layer. In this embodiment, the base is a mixture of a specific polyurethane diol and an aliphatic polycarbonate diol in a predetermined amount, thereby improving the adhesion and weather resistance of the infrared-transmitting dark layer 60.

[0051] The polyurethane diol that can be used as the main component is a polyurethane having a urethane structure as a repeating unit and having hydroxyl groups at both ends. The number average molecular weight of the polyurethane diol is preferably 7000 or more and 13000 or less. If it is 7000 or more, it is preferable because it has good reactivity with the curing agent, and if it is 13000 or less, it is preferable because it improves solubility in a solvent.

[0052] The hydroxyl value of the polyurethane diol is preferably in the range of 10 mgKOH / g to 50 mgKOH / g. If the hydroxyl value of the polyurethane diol is 10 mgKOH / g or more, most of the added curing agent component reacts with the hydroxyl group contained in the main component, which is preferable, and if it is 50 mgKOH / g or less, the reaction with the curing agent proceeds more, which is preferable.

[0053] Polyurethane diol is a main component of adhesives, and is characterized by being obtained by reacting aliphatic polycarbonate diol, 1,6-hexanediol, and isophorone diisocyanate to improve its adhesiveness and weather resistance. The components of polyurethane diol, aliphatic polycarbonate diol, 1,6-hexanediol, and isophorone diisocyanate, are explained below.

[0054] Aliphatic polycarbonate diol is a component of polyurethane diol that can react with isophorone diisocyanate. Aliphatic polycarbonate diol has a carbonate structure as a repeating unit and has hydroxyl groups at both ends. The hydroxyl groups at both ends can react with isocyanate groups to harden the polymer.

[0055] The aliphatic polycarbonate diol can be produced by a production method using an alkylene carbonate and a diol as raw materials, or a production method using a dialkyl carbonate or diaryl carbonate and a diol, etc. The aliphatic polycarbonate diol used in the present embodiment can be produced by appropriately selecting the above production method according to the performance required for the main component.

[0056] Examples of alkylene carbonates that can be used in the production of aliphatic polycarbonate diols include ethylene carbonate, trimethylene carbonate, 1,2-propylene carbonate, 1,2-butylene carbonate, 1,3-butylene carbonate, 1,2-pentylene carbonate, etc. Examples of dialkyl carbonates include dimethyl carbonate, diethyl carbonate, dipropyl carbonate, etc., and examples of diaryl carbonates include diphenyl carbonate, etc.

[0057] Examples of diols include diols without side chains such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,7-heptanediol, diols with side chains such as 2-methyl-1,8-octanediol, neopentyl glycol, and 2-ethyl-1,6-hexanediol, and cyclic diols such as 1,3-cyclohexanediol and 1,4-cyclohexanediol. One type of diol may be used, or a copolymerized polycarbonate diol made from two or more types of diols may be used.

[0058] The number average molecular weight of the aliphatic polycarbonate diol is preferably 1000 or more and 2000 or less. If it is 1000 or more, it is preferable because the curing reaction with the diisocyanate easily occurs, and if it is 2000 or less, it is preferable because the solubility in the solvent, which is the adhesive component, is improved. In the production of polycarbonate diol, since the reactivity of the monomer is high and it is easy to increase the molecular weight, it is necessary to control the reaction rate, etc., in order to obtain a polycarbonate diol having a predetermined number average molecular weight.

[0059] The aliphatic polycarbonate diol may be a commercially available product. In order to obtain an adhesive having excellent durability, weather resistance, heat resistance, and hydrolysis resistance, for example, an aliphatic polycarbonate diol having a number average molecular weight of 1000 (manufactured by Asahi Kasei Chemicals Corporation, product name "Duranol T5651") or an aliphatic polycarbonate diol having a number average molecular weight of 2000 (manufactured by Asahi Kasei Chemicals Corporation, product name "Duranol T5662") may be suitably used.

[0060] 1,6-hexanediol is an aliphatic diol that can react with the following isophorone diisocyanate to form a polyurethane diol. 1,6-hexanediol is liquid at room temperature and can be dissolved in the solvent that is an adhesive component.

[0061] A polyester diol can be used together with 1,6-hexanediol. The polyester diol is a polyol having two or more hydroxyl groups, like 1,6-hexanediol, but it can also be esterified with a carboxylic acid having a bulky aromatic ring in its basic skeleton, so that the polyurethane diol obtained by reacting with isophorone diisocyanate can be given excellent curing speed and cohesive strength. An example of the polyester diol is an aromatic polyester diol produced using isophthalic acid. In this embodiment, the polyester diol can be produced by adopting a combination of a predetermined carboxylic acid compound and a diol according to a conventional method.

[0062] The number average molecular weight of the polyester diol is preferably 3000 or more and 4000 or less. When the number average molecular weight of the polyester diol is 3000 or more, the reactivity with the curing agent is improved, which is preferable, and when the number average molecular weight of the polyester diol is 4000 or less, the solubility in a solvent is improved, which is preferable.

[0063] Isophorone diisocyanate is a component of polyurethane diol and is an alicyclic polyisocyanate. Isophorone diisocyanate reacts with the hydroxyl groups of the aliphatic polycarbonate diol, 1,6-hexanediol, or polyester diol to form polyurethane diol, which is the main component.

[0064] The above-described aliphatic polycarbonate diol, aliphatic diol, and isophorone diisocyanate are dissolved in a solvent, mixed, and heated under reflux to react, thereby obtaining a solution of polyurethane diol, which is the main component. In the above reaction, the hydroxyl groups at both ends of the aliphatic polycarbonate diol and the aliphatic diol react with the isocyanate groups of the isophorone diisocyanate to form urethane bonds and harden.

[0065] The amount of 1,6-hexanediol in the reaction system for producing the polyurethane diol, which is the main component, is preferably 5 parts by mass or more and 15 parts by mass or less, and more preferably 2 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the aliphatic polycarbonate diol. If the amount of 1,6-hexanediol is 5 parts by mass or more, a durable adhesive component can be obtained, and if it is 15 parts by mass or less, solubility in a solvent is improved, which is preferable.

[0066] The amount of polyester diol in the reaction system for producing polyurethane diol is preferably 50 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of aliphatic polycarbonate diol. When the amount of polyester diol is 50 parts by mass or more, a durable adhesive component can be obtained, and when the amount is 100 parts by mass or less, solubility in a solvent is improved, which is preferable.

[0067] In addition, the solvent that can be used when reacting the aliphatic polycarbonate diol, the aliphatic diol, and isophorone diisocyanate is not particularly limited as long as it can dissolve these compounds and does not react with the solvent, but examples of the solvent include carboxylic acid ester solvents such as ethyl acetate from the viewpoints of compatibility with the solvent and processability during lamination.

[0068] The aliphatic polycarbonate diol, which is the main component, reacts with the curing agent component having an isocyanate group. The aliphatic polycarbonate diol may be the same as the aliphatic polycarbonate diol used in producing the polyurethane diol.

[0069] The main component is a mixture of the polyurethane diol and the aliphatic polycarbonate diol described above. The mass ratio of the polyurethane diol and the aliphatic polycarbonate diol in the mixture is preferably 10 parts by mass or more and 20 parts by mass or less of the aliphatic polycarbonate diol per 100 parts by mass of the polyurethane diol. If the amount of the aliphatic polycarbonate diol is 10 parts by mass or more, the adhesion is appropriately reduced, and if it is 20 parts by mass or less, the reaction between the polyurethane diol and the curing agent is easily caused, which is preferable.

[0070] In addition to the polyurethane diol and aliphatic polycarbonate diol, which are the main component, the main agent may contain additives such as a tackifier, a stabilizer, a filler, a plasticizer, a softening point improver, and a catalyst, as necessary. Examples of the tackifier include rosin-based resins and terpene-based resins. Examples of the stabilizer include antioxidants and ultraviolet inhibitors. Examples of the filler include inorganic fillers.

[0071] [Hardening agent] Curing agents that can be used in infrared-transmitting dark inks include, for example, those that contain a polyisocyanate compound as the main component. The polyisocyanate compound is a compound having two or more isocyanate groups in one molecule, and the isocyanate groups react with hydroxyl groups in the polyurethane diol compound of the main component to crosslink the polyurethane diol compound. Such polyisocyanate compounds are not particularly limited as long as they can crosslink the polyurethane diol compound of the main component, and examples thereof include polyurethane diisocyanate, hexamethylene diisocyanate (hereinafter, "HDI"), and isocyanurate-modified isophorone diisocyanate (hereinafter, "nurate-modified IPDI"). Among these polyisocyanate compounds, a mixture of HDI and nurate-modified IPDI is preferred from the viewpoint of improving reactivity to hydroxyl groups. When the curing agent is a mixture of HDI and nurate-modified IPDI, it is preferable to use HDI and nurate-modified IPDI in a range of 70:30 to 50:50 (mass ratio).

[0072] [Base and hardener blend] When the infrared-transmitting dark ink contains a curing agent and is intended to bond substrates together, the blending ratio of the base material to the curing agent is preferably in the range of 1.0 to 3.5, more preferably 1.2 to 3.0, where the ratio of the isocyanate group derived from the polyisocyanate compound to the hydroxyl group derived from the polyurethane diol compound is in the range above. By having the blending ratio of the polyurethane diol compound as the base material and the polyisocyanate compound as the curing agent in the above range, it is possible to obtain an infrared-transmitting dark ink that can firmly bond substrates together, which is preferable.

[0073] [Additives such as silane coupling agents] In addition to the above, silane coupling agents, tackifiers, stabilizers, fillers, plasticizers, softening point improvers, catalysts, etc. can be mixed as additives as necessary. Examples of silane coupling agents include silane monomers such as methyltrimethoxysilane and methyltriethoxysilane, vinyl silanes such as vinyltriethoxysilane and vinyltrimethoxysilane, methacryl silanes such as 3-methacryloxypropyltriethoxysilane and 3-methacryloxypropyltrimethoxysilane, and epoxy silanes such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Examples of tackifiers include rosin-based resins and terpene-based resins. Examples of stabilizers include antioxidants and ultraviolet inhibitors. Examples of fillers include inorganic fillers.

[0074] The amount of the silane coupling agent added is preferably 1% by mass or more and 3% by mass or less relative to 100 parts by mass of the total of the base agent and the curing agent of the infrared-transmitting dark ink. If the amount of the silane coupling agent added is 1% by mass or more, the adhesion is improved, and if it is 3% by mass or less, the durability is improved, which is preferable.

[0075] [solvent] In order to obtain good coating properties and handling properties, it is preferable to add a solvent component to the infrared-transmitting dark ink composition. Examples of such a solvent component include, but are not limited to, carboxylic acid esters such as ethyl acetate, methyl acetate, and methyl propionate. In addition, when the ink is configured as a two-liquid type consisting of a base agent and a hardener, the solvent component used in the base agent and the solvent component used in the hardener are independently selected and may be the same or different.

[0076] The composition of the infrared-transmitting dark ink is not limited to the above, and may be in any form of composition, such as aqueous type, solution type, emulsion type, dispersion type, etc. Also, the property may be in any form, such as film / sheet type, powder type, solid type, adhesive, etc. Furthermore, the adhesion mechanism may be in any form, such as chemical reaction type, solvent volatilization type, heat melting type, heat pressure type, etc.

[0077] <Infrared reflective sheet> By using the infrared-transmitting dark ink, an infrared reflective sheet can be manufactured. An example of an infrared reflective sheet is a laminate in which a transparent adhesive layer 62, an infrared-transmitting dark layer 60, and a reflective layer 61 are laminated, as in the infrared reflective sheet 6 in Fig. 2. Although the infrared reflective sheet 6 in Fig. 2 is used as a back protection sheet for a solar cell module, the use of the infrared reflective sheet of the present invention is not limited to a back protection sheet for a solar cell module. Each layer constituting the infrared reflective sheet will be described below.

[0078] [Infrared-transmitting dark layer] The infrared-transmitting dark layer 60 of this embodiment is a layer containing a base resin having a hydroxyl group, a curing agent having an isocyanate group, and a pigment component. The infrared-transmitting dark layer 60 of this embodiment contains a base resin having a hydroxyl group and a curing agent having an isocyanate group, and has the function of bonding sheets together.

[0079] The infrared-transmitting dark color layer 60 according to this embodiment can be formed by applying or laminating the infrared-transmitting dark color ink containing the curing agent described above onto the reflective layer 61 and / or the transparent adhesive layer 62, and drying and curing it. The application method can be a roll coating method, a gravure roll coating method, a kiss coating method, or other coating methods, or a printing method, etc.

[0080] Here, when using an infrared-transmitting dark ink containing a conventional dark-colored organic pigment such as an oxazine-based compound, the coating amount should be 10 g / m2 in order to achieve both design, infrared transmittance, and the adhesiveness and adhesive stability required for the laminated member. 2 However, when using an infrared-transmitting dark ink containing the curing agent of this embodiment, the curing rate is 5 g / m or more. 2 More than 15g / m 2 The following range, preferably 5 g / m 2 More than 7g / m 2 Both of these can be sufficiently achieved with the coating amount in the following range. This is because, by setting the pigment component to 20 parts by mass or more and 40 parts by mass or less, preferably 30 parts by mass or more and 40 parts by mass or less, per 100 parts by mass of the resin component, the color tone can be sufficiently stabilized even with a coating amount smaller than that of the conventional method. This also leads to an increase in the yield of the infrared reflective sheet produced using the infrared-transmitting dark ink of the present invention, thereby improving productivity.

[0081] In addition, since brown pigments and phthalocyanine pigments have higher dispersibility than other pigments and have little effect on the adhesiveness of the curing agent, it is possible to suppress the deterioration of adhesiveness and adhesive stability due to the inclusion of pigments. The thickness of the infrared-transmitting dark layer 60 is preferably in the range of 5 μm to 15 μm, and more preferably in the range of 5 μm to 7 μm.

[0082] [Reflective layer] The reflective layer 61 is a white resin layer that reflects near-infrared rays, and is made of a resin sheet containing a white pigment or a resin sheet on which a coating layer (coating film or printing film) containing a white pigment is formed. The reflective layer 61 has a function of reflecting near-infrared rays that have passed through the infrared-transmitting dark layer 60. For this reason, for example, when the infrared reflective sheet 6 of this embodiment is used as a back surface protection sheet for a solar cell module, the infrared reflective sheet 6 of this embodiment becomes an infrared reflective sheet (back surface protection sheet) 6 that can sufficiently contribute to improving the power generation efficiency of the solar cell module 1. In this specification, the term "resin sheet" is used as the name of a resin processed into a sheet shape, but this term is used as a concept that also includes a resin film.

[0083] As the resin sheet constituting the reflective layer 61, a resin sheet such as a fluororesin such as PTFE (polytetrafluoroethylene) or ETFE (ethylene tetrafluoride-ethylene copolymer), a poly(meth)acrylic resin, or a polyester resin such as PET (polyethylene terephthalate) can be preferably used. Here, in this embodiment, the reflective layer 61 is disposed as the outermost layer in the solar cell module 1, and therefore is required to have high weather resistance, barrier properties, and hydrolysis resistance. From this viewpoint, it is particularly preferable to use a fluororesin such as ETFE or a polyester resin such as PET among the above.

[0084] The reflective layer 61 must have a function of reflecting near-infrared rays. For this purpose, it is preferable to use a white resin layer containing a white pigment having a particle size of 0.5 μm to 1.5 μm, and more preferably 0.8 μm to 1.2 μm. In addition, in the reflective layer 61, the particles of the white pigment having a particle size of 0.8 μm to 1.2 μm are preferably 80 mass % or more of the total particles of the white pigment. By setting the particle size and distribution ratio of the white pigment within the above range, the white resin layer can efficiently reflect near-infrared rays. In addition, when the infrared reflective sheet of the present invention is used as a back protection sheet for a solar cell module, the white pigment contributes to improving the power generation efficiency of the solar cell module. "Reflecting near-infrared rays" means a function of having an integrated reflectance of 85% or more in a wavelength range of approximately 750 nm to 2200 nm.

[0085] A representative example of a white pigment having a particle size of 0.5 μm or more and 1.5 μm or less is titanium oxide, and in the present invention, it is preferable to use titanium oxide as the white pigment. Here, titanium oxide also includes surface-treated titanium oxide. For example, when the white pigment having the above particle size range is titanium oxide, its production can be carried out as follows.

[0086] A white pigment having the above particle size range and consisting mainly of titanium oxide can be produced by using hydrous titanium oxide as the raw material, adding an aluminum compound having an amount of 0.1% by mass to 0.5% by mass, calculated as aluminum oxide, a potassium compound having an amount of 0.1% by mass to 0.5% by mass, calculated as potassium carbonate, and a zinc compound having an amount of 0.2% by mass to 1.0% by mass, calculated as zinc oxide, and then drying and roasting the mixture.

[0087] The method for producing the reflective layer 61 includes, for example, a method of forming a coating layer containing a white pigment on a resin sheet, and a method of kneading a white pigment into a resin sheet. Either method is not particularly limited and the reflective layer 61 can be produced by a conventionally known method.

[0088] When forming a coating layer (coating film or printing film) containing a white pigment on a resin sheet, a typical paint or ink vehicle is used as the main component, to which a white pigment is added. If necessary, a UV absorber, a crosslinking agent, and other additives are optionally added to prepare a paint or ink composition, which is then coated or printed on the surface of a substrate film by a typical coating method or printing method to form the coating film or printing film.

[0089] When the white pigment is kneaded into the resin sheet, the resin constituting the resin sheet is used as the main component, to which the white pigment is added. Furthermore, other additives may be added as necessary to prepare a resin composition, and a sheet can be produced by kneading the white pigment into the resin composition using a film forming method such as an extrusion method or a T-die method.

[0090] [Transparent adhesion layer] The transparent adhesive layer 62 in this embodiment is a layer that transmits near-infrared light and is disposed on the outermost layer of the infrared reflective sheet 6. The transparent adhesive layer 62 is also a layer that has adhesion to other resin layers, for example, a layer that has adhesion to a resin layer containing an ethylene-vinyl acetate copolymer resin (EVA resin) or a polyolefin such as polyethylene. Therefore, the rear sealing material layer 5 and the transparent adhesive layer 62 can be laminated and adhered to each other, as in the transparent adhesive layer 62 in FIG. 2.

[0091] The transparent adhesive layer 62 in this embodiment is required to transmit the near-infrared rays reflected by the reflective layer 61, and is required to be transparent or semi-transparent from the viewpoint of design. From this viewpoint, it is preferable to use a polyolefin resin such as a polyethylene resin or a polypropylene resin, or polyethylene terephthalate (PET) for the transparent adhesive layer 62.

[0092] [Other layers] The infrared reflective sheet 6 of this embodiment may be provided with other layers as long as they do not impair the effects of the present invention. For example, a weather-resistant layer (not shown) made of a fluorine-based resin, polyethylene terephthalate (PET), or the like may be further laminated on the outermost surface of the infrared reflective sheet 6, opposite to the lamination surface of the transparent adhesive layer 62 of the reflective layer 61. In this case, the weather-resistant layer may be dark in color to improve the design. Alternatively, another transparent reinforcing layer (not shown) may be provided between the reflective layer 61 and the transparent adhesive layer 62 to increase the strength of the back surface protective sheet 6, for example.

[0093] Furthermore, an infrared-transmitting coating layer containing a dark-colored organic pigment may be further laminated on the surface of the reflective layer 61 opposite to the surface on which the infrared-transmitting dark layer 60 is laminated. By laminating the infrared-transmitting dark layer and the infrared-transmitting coating layer, both sides of the infrared reflective sheet can be unified in dark colors. The infrared reflective sheet of this embodiment is an infrared reflective sheet unified in dark colors on both sides, which is preferable from the standpoint of design.

[0094] Furthermore, by making the infrared-transmitting coating layer of this embodiment a layer that transmits near-infrared rays with wavelengths of 750 nm or more and 1500 nm or less, like the infrared-transmitting dark layer 60, heat generation caused by absorption of near-infrared rays with wavelengths of 750 nm or more and 1500 nm or less can be suppressed.

[0095] Specific examples of dark-colored organic pigments contained in the infrared-transmitting coating layer include oxazines, benzimidazolones, pyrroles, quinacridones, azos, perylenes, dioxanes, isoindolinones, indanthrenes, quinophthalones, perinones, and phthalocyanines. From the viewpoint of UV resistance, oxazine-based organic pigments or benzimidazolone-based pigments, 4-[(2,5-dichlorophenyl)azo]-3-hydroxy-N-(2,5-dimethoxyphenyl)-2-naphthalenecarboxamide, 1-[(4-nitrophenyl)azo]-2-naphthalenol, bis[3-hydroxy-4-(phenylazo)-2-naphthalenecarboxylic acid] copper salt, CI Pigment Brown 7, N,N'-bis(2,4-dinitrophenyl)-3,3'-dimethoxy-1,1'-biphenyl-4 A dark pigment composed of at least one pigment selected from the group consisting of N,N'-(10,15,16,17-tetrahydro-5,10,15,17-tetraoxo-5H-dinaphtho[2,3-a:2',3'-i]carbazole-4,9-diyl)bis(benzamide) and a phthalocyanine pigment can be preferably used.

[0096] In addition, by kneading the pigment component contained in the infrared-transmitting dark ink into a base film, a dark film or sheet with high designability similar to the infrared-transmitting dark layer 60 can be manufactured. In addition, these dark films or sheets can be used as the infrared-transmitting dark layer in a multilayer sheet. In manufacturing a dark film or sheet by kneading into this base film, the content of the brown pigment in the pigment component is preferably 43 parts by mass or more and 233 parts by mass or less (the content ratio of the brown pigment to the phthalocyanine pigment is in the range of 30:70 to 70:30 by mass ratio) relative to 100 parts by mass of the phthalocyanine pigment, more preferably 66 parts by mass or more and 150 parts by mass or less (the content ratio of the brown pigment to the phthalocyanine pigment is in the range of 40:60 to 60:40 by mass ratio).

[0097] When the above-mentioned dark-colored film or sheet is formed by kneading the pigment component into the base film as described above, first, the thermoplastic resin constituting the base film is used as the main component, to which the above-mentioned pigment component is added, and further, if necessary, one or more additives such as ultraviolet absorbers, plasticizers, light stabilizers, antioxidants, antistatic agents, crosslinking agents, curing agents, fillers, lubricants, reinforcing agents, reinforcing agents, flame retardants, flame retardants, foaming agents, mildew inhibitors, colorants such as pigments and dyes, and others are added arbitrarily. Furthermore, if necessary, a solvent, a diluent, and the like are added, and the mixture is thoroughly kneaded to prepare a thermoplastic resin composition. The thermoplastic resin composition thus prepared is molded by a film molding method such as an extrusion method, a T-die method, a cast molding method, an inflation method, and others using, for example, an extruder, a T-die extruder, a cast molding machine, an inflation molding machine, and the like, to produce the above-mentioned dark-colored film or sheet. Furthermore, if necessary, these films or sheets can be produced by stretching in uniaxial or biaxial directions using, for example, a tenter system or a tubular system.

[0098] When other layers are provided on the infrared reflective sheet, adhesive layers for bonding each layer may be formed at multiple positions. In this case, if each layer disposed between the transparent adhesive layer 62 and the infrared transmissive dark layer 60 is transparent, any adhesive layer on the transparent adhesive layer side of the reflective layer 61 among the multiple adhesive layers may be made the infrared transmissive dark layer 60, thereby making it possible to obtain an infrared reflective sheet having a dark appearance and sufficient weather resistance and durability. In addition, if the infrared reflective sheet of this embodiment is converted into a back surface protection sheet for a solar cell module, it can be made into a back surface protection sheet that can sufficiently contribute to improving the power generation efficiency of the solar cell module. Such an infrared reflective sheet (back surface protection sheet) is also within the scope of the present invention.

[0099] [Back protection sheet for solar cell modules] A preferred use example of the infrared reflective sheet of this embodiment will be described. For example, the infrared reflective sheet 6 of this embodiment can be used as a back surface protective sheet for a solar cell module by arranging it on the non-light receiving side of a solar cell element of the solar cell module. FIG. 1 is a schematic cross-sectional view illustrating an example of the layer structure of a solar cell module. A solar cell module 1 constituting a solar cell has a structure in which a transparent front substrate 2, a front sealing material layer 3, a solar cell element 4, a rear sealing material layer 5, and a rear surface protective sheet (infrared reflective sheet) 6 are laminated in this order from the light receiving side of incident light 7 as shown in FIG. 1.

[0100] The back surface protective sheet will be described with reference to Fig. 2. The back surface protective sheet 6 has an infrared-transmitting dark layer 60, a reflective layer 61, and a transparent adhesive layer 62. The reflective layer 61 and the transparent adhesive layer 62 are bonded via the infrared-transmitting dark layer 60. In the solar cell module 1, the reflective layer 61 is disposed on the outermost layer side of the module, and the transparent adhesive layer 62 is disposed on the inner layer side of the module, i.e., on the side of the back surface sealing material layer 5.

[0101] Generally, most of the sealing materials for solar cell modules are transparent or semi-transparent. Therefore, when the solar cell module 1 is viewed from the transparent front substrate 2 side, the color of the infrared-transmitting dark layer 60 is visible through the transparent adhesive layer 62 in the gaps where the solar cell elements 4 are not arranged. In addition, the solar cell elements 4 often have a black or similar dark color on the surface. In particular, the thin-film solar cell elements, which have been in increasing demand in recent years, have a black or similar dark color on the surface in most products. Since the infrared-transmitting dark layer 60 of the back protective sheet 6 is black or similar dark, the appearance of many solar cell modules, particularly thin-film solar cell modules equipped with thin-film solar cell elements, can be unified in black or similar dark color, which is preferable in terms of design.

[0102] In order to unify the appearance of the back protective sheet (infrared reflective sheet) 6 to black or a dark color close to black, for example, the color difference ΔE between the color tone of the infrared-transmitting dark layer 60 and the color tone of carbon black measured under conditions of a D65 light source and a 10° viewing angle in accordance with JIS-Z8722 is * It is preferable that ab is 10 or less, and more preferably 7 or less.

[0103] In the back surface protective sheet 6, sunlight that has not been absorbed by the solar cell element 4 is incident from the transparent adhesive layer 62 side. Most of the near-infrared rays contained in the incident light are transmitted through the infrared-transmitting dark layer 60 without being absorbed, and reach the reflective layer 61. Since the reflective layer 61 reflects near-infrared rays, most of the infrared rays that reach the reflective layer 61 are reflected back to the infrared-transmitting dark layer 60. The reflected infrared rays are transmitted through the infrared-transmitting dark layer 60 and are further reflected and absorbed by the solar cell element 4. Since the infrared-transmitting dark layer 60 does not absorb infrared rays, heat generation due to absorption of near-infrared rays can be suppressed. As a result, a decrease in power generation efficiency due to heat generation of the solar cell module 1 can be prevented.

[0104] Furthermore, the infrared-transmitting dark ink of the present invention contains a brown pigment and a phthalocyanine pigment in a predetermined ratio. Therefore, the transmittance of near-infrared rays is higher than when a conventional infrared-transmitting dark ink is used. This makes it possible to suppress the absorption of near-infrared rays and thereby suppress the temperature rise of the solar cell module, and to further increase the power generation efficiency of the solar cell module by utilizing infrared rays for power generation. Therefore, a solar cell module using the infrared reflective sheet of this embodiment as a back surface protective sheet has improved power generation efficiency.

[0105] In addition, in a thin-film solar cell module, suppressing heat generation from all components in the module does not necessarily contribute to improving power generation efficiency, and it is preferable to raise the surface temperature of the black or dark-colored solar cell element to 50°C or more and 70°C or less in relation to the annealing effect. When the infrared reflective sheet of this embodiment is used as a back surface protective sheet, the near-infrared rays reflected by the reflective layer 61 can be absorbed into the solar cell element 4 without loss, without storing heat inside the back surface protective sheet 6, while limiting the appearance to black or a dark color similar to black in order to meet the requirements for design. This makes it possible to efficiently raise the surface temperature of the black or dark-colored thin-film solar cell element to the above temperature. From this point of view, the infrared reflective sheet of the present invention can be particularly preferably used as a back surface protective sheet for a thin-film solar cell module.

[0106] [Method of manufacturing a back protection sheet for a solar cell module] The back surface protective sheet 6 can be produced by dry lamination processing with an infrared-transmitting dark layer 60 provided between a reflective layer 61 and a transparent adhesive layer 62. Even if the adhesive layer is made up of multiple layers by providing other layers, the layers can be laminated by adhering them to each other in a similar manner.

[0107] [Solar cell module manufacturing method] An example of a method for manufacturing the solar cell module 1 that constitutes the solar cell is a method in which each member that constitutes the solar cell is sequentially laminated and integrated by vacuum thermal lamination. The lamination temperature at this time is preferably within a range of 130°C to 190°C. The lamination time is preferably within a range of 5 minutes to 60 minutes, and more preferably within a range of 8 minutes to 40 minutes. In this manner, each member that constitutes the solar cell is thermocompression molded into an integrally molded body, and the solar cell module 1 can be manufactured.

[0108] <Other embodiments of the infrared reflective sheet> Another embodiment of the infrared reflective sheet of the present invention will be described with reference to Fig. 6. (Note that, as necessary, in order to distinguish from the infrared reflective sheet 6 of this embodiment in Fig. 6, an infrared reflective sheet in which an infrared reflective sheet having an infrared reflective dark layer 60 having a function of bonding sheets together, as in the infrared reflective sheet 6 of Fig. 2, is laminated, may be referred to as "the infrared reflective sheet of the above embodiment".) The infrared reflective sheet of this embodiment has an infrared reflective dark layer 60 that does not have a function of bonding sheets together, and two layers among the layers laminated between the transparent adhesive layer 62 and the reflective layer 61 are the infrared reflective dark layer 60 and the transparent adhesive layer 63. From the viewpoint of design, there are cases where an infrared reflective sheet that is partially colored is required, for example, to apply a pattern such as patterning, without making the entire surface of the sheet dark. When manufacturing such an infrared reflective sheet, for example, an infrared-transmitting dark ink having infrared transparency is first partially applied to a resin sheet such as a transparent adhesive layer and / or a reflective layer, and the infrared-transmitting dark layer 60 is formed by hardening the partially applied infrared-transmitting dark ink, and then a transparent adhesive that does not contain pigment is applied and hardened to form a transparent adhesive layer, and the reflective layer and the transparent adhesive layer are laminated to produce an infrared reflective sheet that is partially colored and has a pattern-like design, etc.

[0109] Furthermore, even if an infrared reflective sheet is formed by laminating an infrared-transmitting dark layer and a transparent easy-adhesive layer that transmits all light on the surface of the reflective layer in this order instead of the transparent adhesive layer 62 and the transparent adhesive layer 63, an infrared reflective sheet having a pattern-like pattern or the like can be manufactured by partially applying an infrared-transmitting dark ink to the reflective layer and curing the infrared-transmitting dark ink to form the infrared-transmitting dark layer 60. By laminating a transparent easy-adhesive layer instead of the transparent adhesive layer and the transparent adhesive layer, it is possible to reduce the layers of the infrared reflective sheet, which is preferable from the viewpoint of productivity.

[0110] The infrared-transmitting dark layer 60 is formed of an infrared-transmitting dark ink, and therefore transmits near-infrared rays. The transparent adhesive layer also transmits near-infrared rays, since it does not contain a pigment that absorbs infrared rays. The reflective layer that reflects near-infrared rays with wavelengths of 750 nm or more and 1500 nm or less can reflect near-infrared rays that have transmitted through the infrared-transmitting dark layer 60 and the transparent adhesive layer. Therefore, even when the infrared reflective sheet of this embodiment is used as a back surface protection sheet for a solar cell module, the near-infrared rays that have transmitted through the infrared reflective dark layer 60 and the transparent adhesive layer can still be reused for power generation (see FIG. 6). When the infrared reflective sheet of this embodiment is used as a back surface protection sheet for a solar cell module, the back surface protection sheet is excellent in design and can maintain high power generation efficiency as in the past, making it an excellent back surface protection sheet for a solar cell module.

[0111] [Infrared-transmitting dark layer] The infrared reflective sheet in this embodiment will be described below, focusing on the parts unique to this embodiment. The infrared reflective sheet 60 is mainly disposed as a laminate between the reflective layer 61 and the transparent adhesive layer 62. The infrared reflective layer 60 may be laminated on the entire surface of the transparent adhesive layer and / or the reflective layer, or may be laminated only on a part of the transparent adhesive layer and / or the reflective layer. An infrared reflective sheet in which the infrared reflective layer 60 is laminated only on a part of the transparent adhesive layer and / or the reflective layer is an infrared reflective sheet with high designability. The infrared reflective layer 60 may be bonded to the transparent adhesive layer 62 as shown in FIG. 6, for example, as long as it is on the light receiving surface side of the reflective layer 61, or may be laminated on the inside of the reflective layer 61 in a form in contact with the reflective layer 61 other than that shown in FIG. 6.

[0112] In the infrared reflective sheet of this embodiment, the infrared-transmitting dark layer 60 is made of a crosslinked resin in which a base resin having a hydroxyl group (hereinafter also simply referred to as "base resin") is crosslinked with an isocyanate-based curing agent, as in the infrared reflective sheet of the above embodiment. The infrared-transmitting dark layer 60 can be formed by applying an infrared-transmitting dark ink made of a base resin, a curing agent, a solvent, and a pigment component containing a brown pigment and a phthalocyanine pigment to the surface of a resin sheet, and then drying and curing the applied infrared-transmitting dark ink.

[0113] In the case of an infrared-transmitting dark ink that forms an infrared-transmitting dark layer on the transparent adhesive layer and / or reflective layer surface, as in the infrared-transmitting dark ink of this embodiment, the pigment component is preferably 20 parts by mass or more and 50 parts by mass or less, more preferably 35 parts by mass or more and 45 parts by mass or less, relative to 100 parts by mass of the main resin component. By setting the content of the pigment component within this range, the color tone can be stabilized. In addition, since the infrared-transmitting dark layer 60 can be formed with a small amount of infrared-transmitting dark ink, even if the infrared-transmitting dark layer 60 is laminated only on a part of the surface of the resin sheet, the step between the surface on which the infrared-transmitting dark layer 60 is laminated and the surface on which the infrared-transmitting dark layer 60 is not laminated is small. Therefore, it is possible to laminate the transparent adhesive layer 62 and the reflective layer 61 via the transparent adhesive layer 63 with a small amount of transparent adhesive, and the infrared reflective sheet can be manufactured at low cost. Furthermore, even if an infrared reflective sheet is formed by laminating, in that order, an infrared-transmitting dark layer and a transparent easy-adhesive layer that transmits all light on the surface of the reflective layer instead of the transparent adhesive layer 62 and the transparent adhesive layer 63, it is possible to laminate the reflective layer 61 and other layers such as the back sealing material layer 5 via a small amount of primer agent, and the infrared reflective sheet can be manufactured at low cost.

[0114] In the manufacturing process of the infrared reflective sheet of this embodiment, the resin sheet on which the infrared-transmitting dark layer is formed is exposed once to the outermost surface in a previous process of applying a transparent adhesive or a primer agent. Therefore, the infrared-transmitting dark layer of this embodiment, which does not have the function of adhering sheets together, is required to have blocking resistance.

[0115] The blending ratio of the base resin and the curing agent in the infrared reflective sheet of this embodiment is preferably such that the NCO / OH ratio, which is the ratio of the NCO value of the curing agent to the OH value of the base resin, is in the range of 1.0 to 2.0. By making the NCO / OH ratio 2.0 or less, the blocking resistance of the infrared-transmitting dark layer 60 can be improved. By making the NCO / OH ratio 1.0 or more, the adhesion between the infrared-transmitting dark layer 60 and the resin sheet can be improved.

[0116] In addition, in terms of adhesion between the infrared-transmitting dark layer 60 and the resin sheet and blocking resistance of the infrared-transmitting dark layer 60, when a polyurethane / polycarbonate diol system is used as the main component of the resin component, it is preferable that the number average molecular weight of the polyurethane diol is 6000 or more and 8000 or less, and the hydroxyl value of the polyurethane diol is 15 mgKOH / g. In addition, it is preferable to use, as the curing agent, a mixture of an isocyanurate modified product of hexamethylene diisocyanate (HDI nurate product) and a TMP adduct modified product of isophorone diisocyanate (IPDI) in a 1:1 (mass ratio).

[0117] The coating amount of infrared-transmitting dark ink in the infrared reflective sheet of this embodiment is 3 g / m 2 More than 7g / m 2 The following range is preferable: The coating amount of infrared-transmitting dark ink is 3 g / m 2 By setting the amount of the infrared-transmitting dark ink to 7 g / m or more, the color of the infrared-transmitting dark layer 60 can be made sufficient. 2or less, there is a small difference in level between the surface on which the infrared-transmitting dark layer 60 is laminated and the surface on which the infrared-transmitting dark layer 60 is not laminated. Therefore, it is possible to laminate the reflective layer 61 and the transparent adhesive layer 62 via the transparent adhesive layer 63 using a small amount of transparent adhesive, and the infrared reflective sheet can be manufactured at low cost.

[0118] [Transparent adhesive layer] The transparent adhesive layer 63 is an adhesive layer provided mainly for bonding the reflective layer 61 and the transparent adhesive layer 62. In this embodiment, the transparent adhesive layer 63 is formed by laminating and curing a transparent adhesive applied to the upper surface of the reflective layer 61 or the lower surface of the transparent adhesive layer 62 facing the upper surface.

[0119] The transparent adhesive layer 63 is required to have sufficient adhesiveness and adhesive durability, and is preferably one that has the property of transmitting near-infrared rays in order to reflect the near-infrared rays.

[0120] The transparent adhesive that forms the transparent adhesive layer 63 is preferably a transparent adhesive that, like the infrared-transmitting dark ink of this embodiment, has the property of transmitting light having a wavelength of 750 nm or more and 1500 nm or less when hardened.

[0121] The adhesive composition used for the transparent adhesive layer 63 is preferably a two-component type consisting of a base agent and a curing agent, similar to the infrared-transmitting dark ink of this embodiment, and from the viewpoints of application and handling, the composition appropriately contains a solvent.

[0122] The main resin component of the transparent adhesive used in the transparent adhesive layer is preferably a polyurethane / polycarbonate diol system containing a mixture of polyurethane diol and aliphatic polycarbonate diol, as in the infrared-transmitting dark ink of this embodiment. By using a mixture of a specific polyurethane diol and an aliphatic polycarbonate diol in a predetermined amount as the main resin, the adhesiveness and weather resistance of the transparent adhesive layer are improved.

[0123] The adhesive composition used for the transparent adhesive layer 63 in this embodiment is mainly composed of a base agent and a curing agent, and the blending ratio of the base agent and the curing agent may be the same as that of the infrared-transmitting dark ink used in the infrared reflective sheet of the above embodiment. It is preferable that the blending ratio of the polyurethane diol compound of the base agent component and the polyisocyanate compound of the curing agent component is within the above range, since it is possible to obtain an adhesive that can firmly bond each substrate. In addition to the above, silane coupling agents, tackifiers, stabilizers, fillers, plasticizers, softening point improvers, catalysts, etc. can be mixed as additives as necessary.

[0124] In order to obtain good coating property and handling property, it is preferable to add a solvent component to the transparent adhesive composition. Such a solvent component can include, but is not limited to, carboxylic acid esters such as ethyl acetate, methyl acetate, and methyl propionate. As mentioned above, the adhesive is configured as a two-liquid type of a base agent and a hardener, but the solvent component used in the base agent and the solvent component used in the hardener are independently selected and may be the same or different.

[0125] However, the transparent adhesive composition is not limited thereto, and may be in any composition form, such as an aqueous type, a solution type, an emulsion type, or a dispersion type, and the properties may be in any form, such as a film / sheet type, a powder type, or a solid type, and further, the adhesion mechanism may be in any form, such as a chemical reaction type, a solvent evaporation type, a thermal melting type, or a thermal pressure type.

[0126] The transparent adhesive layer 63 can be formed by applying or laminating the adhesive composition described above onto, for example, the reflective layer 61 and / or the transparent adhesive layer 62, and drying and curing it.

[0127] [Transparent adhesion layer] The transparent adhesive layer of this embodiment may be the same as the transparent adhesive layer used in the infrared reflective sheet of the above embodiment. The transparent adhesive layer of this embodiment may be a film or sheet produced by a film forming method such as an extrusion method or a T-die method.

[0128] [Transparent adhesive layer] Also, instead of the transparent adhesive layer and the transparent adhesive layer, a transparent easy-adhesive layer may be formed between the rear sealing material layer 5 and the infrared-transmitting dark layer 60. The transparent easy-adhesive layer is a so-called primer layer, and a primer composition constituting the transparent easy-adhesive layer, for example, a primer composition containing an olefin resin and an aqueous medium and substantially not containing an organic solvent, can be used. By laminating a transparent easy-adhesive layer instead of the transparent adhesive layer and the transparent adhesive layer, it is possible to reduce the layers of the infrared reflective sheet, which is preferable from the viewpoint of productivity.

[0129] The olefin resin contained in the primer composition (hereinafter, also simply referred to as "primer composition") used to form the transparent adhesive layer is preferably an acid-modified polyolefin resin containing an olefin component and an unsaturated carboxylic acid component. The acid-modified polyolefin resin preferably has an MFR of 0.01 g / 10 min or more and less than 100 g / 10 min at 190° C. and a load of 2.16 kg measured in accordance with JIS K7210. This allows the formation of a transparent adhesive layer 62 that maintains good dispersibility in an aqueous medium at the primer composition stage and has excellent adhesion to the olefin resin that forms the back sealing material layer 5.

[0130] The primer composition may be, for example, the primer composition described in JP 2013-74172 A. Strong adhesion can be achieved between the rear sealing material layer 5 and the infrared-transmitting dark color layer.

[0131] [Other layers] The infrared reflective sheet of this embodiment may be provided with other layers as long as the effects of the present invention are not impaired, similarly to the infrared reflective sheet of the above embodiment.

[0132] [Back protection sheet for solar cell modules] The infrared reflective sheet of this embodiment can be manufactured by dry lamination using, for example, a reflective layer 61 or a transparent adhesive layer 62, on which an infrared-transmitting dark color layer 60 has been laminated in advance, with a transparent adhesive layer 63 interposed therebetween. Even if other layers are provided to form a transparent adhesive layer having a plurality of layers, each layer can be laminated by adhering them in a similar manner.

[0133] [Solar cell module] The infrared reflective sheet of this embodiment can be manufactured by sequentially stacking the members constituting the solar cell and integrating them by, for example, vacuum thermal lamination, in the same manner as in the manufacturing method of the solar cell module described above.

[0134] An example of use of an infrared reflective sheet capable of partially coloring the surface of the infrared reflective sheet as in the present embodiment, as a back protection sheet for a solar cell module, will be described. Since most sealing materials for solar cell modules are transparent or semi-transparent, the color of the back protection sheet 6 for the solar cell module can be seen in the gap portion (non-element region) where the solar cell element 4 is not arranged in a plan view from the surface side where the solar cell element is arranged. By using the infrared reflective sheet of this embodiment, the gap portion (non-element region) where the solar cell element 4 is arranged in a plan view can be colored to form a dark color region with an average reflectance of 10% or less at wavelengths from 400 nm to 700 nm. In addition, by not coloring the cell region where the solar cell element is arranged, a reflection region with an average reflectance of 80% or more at wavelengths from 1000 nm to 1200 nm can be formed. EXAMPLES

[0135] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0136] In order to evaluate the near-infrared transmittance, color coordinate-application amount dependency, high temperature discoloration, adhesion, and adhesion durability of the infrared-transmitting dark ink according to this embodiment, each ink was manufactured by the method described below, and an infrared reflective sheet and a pseudo module sample were made using the ink.

[0137] [Main ingredient] Under a nitrogen atmosphere, ethylene glycol (32.3 parts by mass), 2,2-dimethyl-1,3-propanediol (270.8 parts by mass), 1,6-hexanediol (122.9 parts by mass), adipic acid (228.1 parts by mass), and isophthalic acid (664 parts by mass) were added to a flask equipped with a stirrer and a nitrogen gas inlet tube, and the mixture was bubbled with nitrogen at 180°C to 220°C to react until the acid value reached 2 mgKOH / g. Ethyl acetate (860 parts by mass) was added to obtain a 50% solution of polyester diol H. The hydroxyl value of the obtained resin was 32 mgKOH / g, and the number average molecular weight was about 3500.

[0138] In a nitrogen atmosphere, 100 parts by mass of aliphatic polycarbonate diol with a number average molecular weight of 1000 (manufactured by Asahi Kasei Chemicals Corporation, trade name "Duranol T5651" hereinafter abbreviated as "PDC1000"), the above polyester diol H (50 parts by mass), 1,6-hexanediol (2 parts by mass), isophorone diisocyanate (23.8 parts by mass), and ethyl acetate (175.8 parts by mass) were added to a flask equipped with a stirrer, and the mixture was heated under reflux until the absorption of isocyanate at 2270 cm-1 disappeared in the infrared absorption spectrum, thereby obtaining a 50% solution of polyurethane diol. The hydroxyl value of the obtained resin was 14 mgKOH / g, and the number average molecular weight was about 8000.

[0139] A base resin was prepared by mixing 100 parts by mass of the above polyurethane diol and 15 parts by mass of the aliphatic polycarbonate diol (B) (PDC1000).

[0140] [Hardening agent] A mixture of hexamethylene diisocyanate (HDI adduct: bifunctional) and isocyanurate-modified isophorone diisocyanate (nurate-modified IPDI) was used. The mixing ratio of the adduct-modified HDI and nurate-modified IPDI (HDI adduct) / (nurate-modified IPDI) was 6:4 (mass ratio).

[0141] [Infrared-transmitting dark ink (Ink 1)] Pigments: Brown pigments (benzimidazolone pigments (Pigment Brown 25, particle size 0.08 μm)), phthalocyanine pigments (amorphous phthalocyanine pigment blue (Pigment Blue 15, particle size 0.15 to 0.20 μm)) Solvent: Ethyl acetate The base resin (solid content 50% by mass), the curing agent (solid content 10% by mass), the brown pigment (benzimidazolone pigment), and the phthalocyanine pigment (amorphous phthalocyanine pigment) (benzimidazolone pigment to phthalocyanine pigment content ratio of 52.5:47.5, 35 parts by mass of pigment component per 100 parts by mass of resin component) were dissolved in the solvent to prepare the resin composition.

[0142] [Dark Ink (Ink 2)] The organic pigment is as follows, and the solid coating amount is 10g / m 2 More than 20g / m 2 It was prepared in the same manner as Ink 1, except that it was adjusted to the following thickness (thickness after curing: 10 μm to 20 μm). Pigment: 16.7% by mass of dioxazine compound (20 parts by mass of pigment component per 100 parts by mass of resin component)

[0143] (Spectral transmittance measurement) In order to evaluate the near-infrared reflectivity (transmittance) of the infrared-transmitting dark ink according to this embodiment, samples for measuring transmittance were prepared as examples and comparative examples by the method described below.

[0144] The following resin was used as the resin substrate that would become the reflective layer. Reflective layer: Toray, white PET, 188μm The following resin was used as the resin substrate that would become the transparent adhesive layer. Transparent adhesive layer: polyethylene, 60μm

[0145] <Sample Creation> [Example 1]: Ink 1 was gravure-coated onto the sheet made of the above-mentioned reflective layer (coating amount: 5 g / m 2 ) an adhesive layer having a thickness of 5 μm (in a dry state), on top of which the above-mentioned transparent adhesive layer was laminated, and then the adhesive layer was aged at 45°C or higher and 55°C or lower for 168 hours to heat-set the adhesive layer, thereby producing an infrared reflective sheet.

[0146] [Comparative Example 1]: Ink 2 was gravure-coated onto the sheet made of the above-mentioned reflective layer (coating amount: 12 g / m 2 ) and a 12 μm thick (dry state) adhesive layer was laminated on top of that, followed by a transparent adhesive layer. The infrared reflective sheet was then produced by aging for 168 hours at 45°C to 55°C and then heat-curing it.

[0147] <Evaluation> A spectrophotometer ("U-4100" manufactured by Hitachi High-Technologies Corporation) was used to evaluate the reflectance (%) of light with wavelengths of 300 nm to 1200 nm when light was incident on the infrared reflective sheet samples of Example 1 and Comparative Example 1. The evaluation results are shown in FIG.

[0148] 3, the infrared reflective sheet of Example 1 has an infrared-transmitting dark layer 60 containing a predetermined amount of a brown pigment (benzimidazolone pigment) and a phthalocyanine pigment, and thereby has improved infrared transmittance in the vicinity of wavelengths of about 800 nm to 900 nm, which are higher in energy than 1000 nm or more. Therefore, it is found that this is an infrared-transmitting dark ink with a higher transmittance in the vicinity of wavelengths of about 800 nm to 900 nm, compared to when a conventional organic black pigment is added.

[0149] The polyethylene and white PET of the infrared reflective sheet of Example 1 were peeled off, and the infrared-transmitting dark layer was dissolved using methyl ethyl ketone to prepare a sample for measuring transmittance. The measurement sample was poured into a quartz glass cell, and the transmittance (%) of light with a wavelength of 300 nm to 1200 nm was measured using a spectrophotometer (for example, an ultraviolet spectrophotometer "V-670" manufactured by JASCO Corporation or "U-4100" manufactured by Hitachi High-Technologies Corporation). As a result, the transmittance of light with a wavelength of 425 nm was 11.6%, and the transmittance of light with a wavelength of 675 nm was 10.0%.

[0150] Moreover, the infrared reflective sheet of Example 1 absorbs almost all of the light in the visible region (wavelengths of 380 nm to 780 nm), whereas the infrared reflective sheet of Comparative Example 1 reflects light in the visible region with wavelengths of around 700 nm to 750 nm. Therefore, the ink of Example 1 has a black appearance and is excellent in design properties, whereas the ink of Comparative Example 1 transmits light in the visible region with wavelengths of around 700 nm to 750 nm, and therefore has a dark appearance that is more purplish than black, and it is found to be an ink with poor design properties.

[0151] (Color coordinate-coating amount dependency test 1) <Sample Creation> [Examples 2 to 4]: Infrared reflective sheets were prepared by gravure coating Ink 1 in various coating amounts in the same manner as in Example 1. After that, new pseudo modules were prepared using each infrared reflective sheet as a back surface protective sheet.

[0152] The pseudo module was created by laminating glass as a transparent front substrate, 450 μm of ethylene-vinyl acetate copolymer resin (EVA) as a sealing material layer, and a sample according to this embodiment as an infrared reflective sheet (rear protective sheet) in the order of transparent front substrate / front sealing material layer / rear sealing material layer / infrared reflective sheet (rear protective sheet), followed by vacuum lamination (vacuum lamination conditions: temperature 150° C., vacuum time 5 minutes, pressing time 9 minutes).

[0153] [Comparative Examples 2 to 6]: Infrared reflective sheets were prepared by gravure coating dark ink 2 in various application amounts instead of dark ink 1 in Examples 2 to 4. After that, pseudo modules were newly prepared in the same manner as in Examples 2 to 4, using each infrared reflective sheet as a back surface protective sheet.

[0154] <Evaluation> In accordance with JIS Z8722, measurements were performed using a KONICA MINOLTA spectrophotometer CM-700d under conditions of D65 light source and 10° viewing angle, with the light source shining on the transparent resin layer side of each sample. The color coordinate results obtained from this test are shown in Table 1, Figures 4 and 5.

[0155] [Table 1]

[0156] From Table 1 and Figures 4 and 5, the coating amount of the comparative sample was 10 to 20 g / m 2 A * and b * In comparison with the variation in the coating amount, the variation in the color tone of the sample in the embodiment is small. 2 Comparative Example 4 and coating amount 5g / m 2 Example 2 of L * The values ​​of are almost equal. From these results, the infrared-transmitting dark ink of the example has a color tone close to that of carbon black, and the variation in color coordinates with respect to the amount of solid adhesive applied is small. Therefore, it is found to be an infrared-transmitting dark ink with high yield and high productivity. Furthermore, compared to the sample of the comparative example, it is found to be an infrared-transmitting dark ink that can exhibit sufficient design properties even with a small amount applied.

[0157] (Color coordinate-coating amount dependency test 2) The ink was coated at a rate of 5 g / m2, with the brown pigment (benzimidazolone pigment (shown as brown in Table 2)) and phthalocyanine pigment (shown as blue in Table 2) content ratios changed to those shown in Table 2. 2A pseudo module was created in the same manner as in the above color coordinate-coating amount dependency test 1, and measurements were performed by shining a light source on each sample from the transparent resin layer side using a KONICA MINOLTA spectrophotometer CM-700d under the conditions of D65 light source and 10° viewing angle in accordance with JIS Z8722. In addition, the color difference with carbon black (ΔE * The color coordinates obtained in this test and the color difference with carbon black (ΔE * ab) are shown in Table 2. In addition, the description of "content of brown pigment" in Table 2 means the content of brown pigment relative to 100 parts by mass of phthalocyanine pigment.

[0158] The transmittance (%) of light having a wavelength of 425 nm and light having a wavelength of 675 nm was also determined for each of the inks according to Examples 5 to 9, 16, and 17, and Comparative Examples 11 and 12 in Table 2. Specifically, each of the inks according to Examples 5 to 9 and Test Examples 1 to 4 was applied at 5 g / m2 to a fluorofilm (fluorofilm Aflex 100 μm, manufactured by Asahi Glass Co., Ltd.) which is a transparent substrate. 2 A sample for measuring transmittance was prepared by gravure coating the above-mentioned, laminating a similar transparent substrate thereon, dry laminating the resultant, and heat-curing the resultant by aging at 45° C. to 55° C. for 168 hours. Then, using a spectrophotometer (Hitachi High-Technologies Corporation, "U-4100"), the transmittance of light with a wavelength of 425 nm and the transmittance of light with a wavelength of 675 nm were determined from the transmittance (%) of light with wavelengths of 300 nm to 1200 nm.

[0159] [Table 2]

[0160] From the results of this test, it was found that an infrared-transmitting dark ink in which the content of the brown pigment is in the range of 43 to 233 parts by mass (the content ratio of the brown pigment to the phthalocyanine pigment is in the range of 30:70 to 70:30 by mass), preferably in the range of 66 to 150 parts by mass (the content ratio of the brown pigment to the phthalocyanine pigment is in the range of 40:60 to 60:40 by mass), relative to 100 parts by mass of the phthalocyanine pigment, has a lower color difference (ΔE * Therefore, compared with the inks of Examples 16 and 17 and Comparative Examples 11 and 12, the infrared-transmitting dark inks of Examples 5 to 9 are closer to the color tone of carbon black, and therefore are infrared-transmitting dark inks that can exhibit sufficient design properties.

[0161] (High temperature discoloration test) <Sample Creation> [Example 10]: The coating amount of ink 1 was 7 g / m as in Example 1. 2 Then, an infrared reflective sheet was prepared by gravure coating. After that, a pseudo module was newly prepared in the same manner as in Examples 2 to 4, using each infrared reflective sheet as a back surface protective sheet.

[0162] [Comparative Example 12]: The coating amount of ink 2 was 7 g / m, similar to ink 1. 2 Then, a pseudo module was newly prepared from each sheet sample in the same manner as in Examples 2 to 4.

[0163] <Evaluation> The above samples were stored at 170°C for 14 hours, and the color tone after storage was measured. The color tone was measured by measuring the color coordinates of each sample of the examples and comparative examples under conditions of a D65 light source and a 10° viewing angle in accordance with JIS Z8722. Each sample was measured using a KONICA MINOLTA spectrophotometer CM-700d.

[0164] The color change in each of the Examples and Comparative Examples before and after storage was measured three times, and the average change is shown in Table 3.

[0165] [Table 3]

[0166] From Table 3, the color difference of the sample of Example 10 is smaller than that of the sample of Comparative Example 7. From this, it can be seen that the laminate produced using the infrared-transmitting dark ink of this embodiment does not discolor the other layers even in an environment exposed to a poor environment of 170°C. Therefore, it can be seen that the laminate in which the infrared-transmitting dark ink of this embodiment is laminated is an excellent laminate with no change in design even in a high-temperature environment. In particular, when the infrared reflective sheet of this embodiment is used as a back protective sheet for a solar cell module, the dark pigment contained in the infrared-transmitting dark layer 60 of the back protective sheet does not migrate to the sealing layer, causing discoloration of the sealing layer. Therefore, it can be seen that a solar cell module with excellent storage stability can be manufactured without a decrease in power generation efficiency due to discoloration of the sealing layer.

[0167] (Interlaminar strength-durability test) <Sample Creation> Adhesion was performed using ink 1 and ink 2 to prepare samples for measuring adhesion in Example 11 and Reference Example, respectively. In Example 11, an infrared reflective sheet was prepared by gravure coating ink 1 in the same manner as in Example 1 (the amount of ink 1 applied was 5 g / m 2 , thickness 5 μm (dry state)). In the reference example, an infrared reflective sheet was prepared by gravure coating with Ink 2 in the same manner as in Comparative Example 1 (the coating amount of Ink 2 was 10 g / m 2 , thickness 10 μm (dry state).

[0168] The samples of Example 11 and Reference Example were subjected to adhesiveness tests by the following method, and the adhesiveness was evaluated based on the measurement results. All test pieces were 15 mm wide. (Adhesion Test) In accordance with JIS K6854-2, the peel strength (N) of each sample of Example 11 and Reference Example was measured by measuring the initial value and the value after each of the durability tests described below using a 180-degree peel test method. Each sample was measured using a peel tester (manufactured by A&D Co., Ltd., product name "TENSILON RTA-1150-H") at 23°C under peel conditions of 50 mm / min.

[0169] (Damp Heat Durability (PCT) test) The conditions were set to 120°C, 85% RH, and 1.6 atm in a pressure cooker tester (HASTTEST, manufactured by Hirayama Seisakusho), and each of the above samples was placed in the tester for a certain period of time (in Table 4, before placement is indicated as 0h, after placement for 24 hours is indicated as 24h, etc.). The above peel test was then carried out three times. The average values ​​of each measurement result before placement and after placement for a certain period of time are shown in Table 4.

[0170] [Table 4]

[0171] From Table 4, it can be seen that the infrared-transparent dark ink of Example 11 has adhesion properties and adhesion durability similar to those of the dark ink of the Reference Example which contains a dioxazine compound having high adhesion durability.

[0172] From the above results, it can be seen that the infrared-transmitting dark ink of this embodiment has the same adhesion and adhesion durability as dark inks containing a dioxazine compound, but has higher infrared transparency, and has good design properties even in an extremely small amount of application, and is an infrared-transmitting dark ink with good yield and extremely high productivity.

[0173] Therefore, for example, a back protective sheet for a solar cell module using an infrared reflective sheet produced with the infrared-transmitting dark ink according to the present invention can suppress heat generation caused by absorbing infrared rays due to its high infrared transmittance, and can utilize more near-infrared rays for power generation. Therefore, the solar cell module using the infrared-transmitting dark ink according to this embodiment is an extremely excellent solar cell module that can improve the power generation efficiency of the solar cell module compared to conventional ones.

[0174] <Examples of other embodiments> In order to evaluate the adhesiveness, adhesive durability, blocking resistance, adhesion, and color coordinate-application amount dependency of the back surface protective sheet according to this embodiment, an adhesive was manufactured by the method described below, and a sample for measuring adhesiveness was created using the adhesive.

[0175] [Manufacture of infrared-transmitting dark ink (ink 3)] [Main ingredient] In a round-bottom flask equipped with a stirrer, a thermometer, and a nitrogen gas inlet tube, an aliphatic polycarbonate diol having a number average molecular weight of 1000 (50 parts by mass), 1,6-hexanediol (70 parts by mass), 1,8-octanediol (30 parts by mass), isophorone diisocyanate (IPDI) (176.6 parts by mass), a trimethylolpropane (TMP) adduct modified product of isophorone diisocyanate (IPDI) (10 parts by mass), and ethyl acetate (333.6 parts by mass) were charged, and the mixture was subjected to an infrared absorption spectrum with a peak at 2270 cm under nitrogen gas introduction. -1The mixture was heated under reflux until the absorption of the isocyanate disappeared, to prepare a base resin of Example 1 having a glycol modification amount of 10% and an IPDI modification amount of 2%. In this example, the glycol modification amount refers to the mass (mass ratio %) of the alkylene diol compound (in this example, a mixture of 1,6-hexanediol and 1,8-octanediol) relative to the total component mass of the base resin component, and the IPDI modification amount refers to the mass (mass ratio %) of the modified isocyanate compound (in this example, a trimethylolpropane (TMP) adduct modified product of isophorone diisocyanate (IPDI)) relative to the total component mass of the base resin component.

[0176] The total amount of 1,6-hexanediol and 1,8-octanediol added, and the amount of the modified adduct of isophorone diisocyanate (IPDI) with trimethylolpropane (TMP) added were appropriately adjusted so that the amount of glycol modification was 10% and the amount of IPDI modification was 3%.

[0177] [Hardening agent] A curing agent was prepared consisting of hexamethylene diisocyanate (HDI) nurate (40 parts by mass) and isophorone diisocyanate (IPDI) trimethylolpropane (TMP) adduct modified product (60 parts by mass). In addition, they were mixed so that the NCO / OH ratio, which is the ratio of the NCO value of the polyisocyanate compound to the OH value of the crosslinkable base resin, would be as shown in Table 5. Pigments: Brown pigments (benzimidazolone pigments (Pigment Brown 25, particle size 0.08 μm)), phthalocyanine pigments (amorphous phthalocyanine pigment blue (Pigment Blue 15, particle size 0.15 to 0.20 μm)) Solvent: Ethyl acetate The above-mentioned base resin, the above-mentioned curing agent, the above-mentioned brown pigment (benzimidazolone pigment) and the above-mentioned phthalocyanine pigment (the content ratio of brown pigment to phthalocyanine pigment was 52.5:47.5, and the pigment component was 40 parts by mass per 100 parts by mass of the base resin component) were dissolved in the above-mentioned solvent to obtain ink 3.

[0178] [Manufacturing transparent adhesives] [Main ingredient] Under a nitrogen atmosphere, ethylene glycol (32.3 parts by mass), 2,2-dimethyl-1,3-propanediol (270.8 parts by mass), 1,6-hexanediol (122.9 parts by mass), adipic acid (228.1 parts by mass), and isophthalic acid (664 parts by mass) were added to a flask equipped with a stirrer and a nitrogen inlet tube, and the mixture was bubbled with nitrogen at 180°C to 220°C to react until the acid value reached 2 mgKOH / g. Ethyl acetate (860 parts by mass) was added to obtain a 50% solution of polyester diol H. The OH value of the obtained resin was 32 mgKOH / g, and the number average molecular weight was about 3500.

[0179] In a nitrogen atmosphere, 100 parts by mass of an aliphatic polycarbonate diol having a number average molecular weight of 1000 (manufactured by Asahi Kasei Chemicals Corporation, product name "Duranol T5651" hereinafter abbreviated as "PDC1000"), the above polyester diol H (50 parts by mass), 1,6-hexanediol (2 parts by mass), isophorone diisocyanate (23.8 parts by mass), and ethyl acetate (175.8 parts by mass) were added to a flask equipped with a stirrer. -1 The mixture was heated under reflux until the absorption of isocyanate disappeared, and a 50% solution of polyurethane diol was obtained. The OH value of the obtained resin was 14 mgKOH / g, and the number average molecular weight was about 8000.

[0180] A base resin was prepared by mixing 100 parts by mass of the polyurethane diol and 15 parts by mass of the aliphatic polycarbonate diol (B) (PDC1000). The curing agent used was the same as that used in ink 3. Solvent: Ethyl acetate The above base agent (solid content 50% by mass), the above curing agent (solid content 10% by mass), 16.7% by mass of dioxazine compound (20 parts by mass of pigment component per 100 parts by mass of base resin component)

[0181] The base agent of the transparent adhesive, the hardener of the transparent adhesive, and the solvent were prepared in a mass ratio of 18:3.4:5.4.

[0182] (Blocking resistance test) The samples of Examples 12 to 15 and Comparative Examples 8 to 10 were subjected to a test for blocking resistance by the following method, and the blocking resistance was evaluated based on the measurement results. All test pieces were 15 mm wide.

[0183] An infrared-transmitting dark ink was applied to the surface of a white PET (white PET, 188 μm, manufactured by Toray Industries, Inc.) film using a bar coater, and the applied ink was dried at 120° C. for 2 minutes to form a dark ink layer on the surface of the substrate. Then, a white PET (white PET, 188 μm, manufactured by Toray Industries, Inc.) was placed on top of the surface of the dark ink layer immediately after drying and cured at 50° C. for 3 days in this state to form a sample for evaluating blocking resistance. A blocking resistance test was performed by peeling off the overlapped parts of each sample for evaluating blocking resistance to evaluate the blocking state, and the results were evaluated according to the following criteria. The evaluation results are shown in Table 5. The NCO / OH ratio in Table 5 is the ratio of the NCO value of the curing agent to the OH value of the base resin.

[0184] [Evaluation Criteria] ○: The sheets peel off naturally without any transfer of the dark ink layer. △: No transfer of the dark ink layer, slight adhesion when peeling the sheets apart ×: dark ink layer transfers and / or there is a feeling of adhesion when the sheets are peeled off

[0185] (Adhesion test) The samples of Examples 12 to 15 and Comparative Examples 8 to 10 were subjected to a test for blocking resistance by the following method, and the blocking resistance was evaluated based on the measurement results. All test pieces were 15 mm wide.

[0186] Adhesion tests were conducted according to ASTM D3359 and JIS 5400, and the adhesion was evaluated according to the following criteria. The results are shown in Table 5 below as "Adhesion."

[0187] [Evaluation Criteria] ○: 0% coating peeling △: Over 0% and 15% or less of coating peeling ×: More than 15% of the coating peeled off

[0188] [Table 5]

[0189] From Table 5, it can be seen that the samples of this embodiment in which the NCO / OH ratio of the infrared-transmitting dark ink is 1.0 or more and 2.0 or less have high blocking resistance and adhesion. Therefore, it can be seen that the infrared-transmitting dark ink used in the present invention has good blocking resistance and adhesion, and is therefore preferable for producing the solar cell module back surface protective sheet of the present invention.

[0190] (Color coordinate-coating amount dependency test) <Sample Creation> [Examples 13 to 15]: An infrared-transmitting dark ink was applied to the surface of a white PET film (white PET manufactured by Toray Industries, Inc., thickness 188 μm) using a bar coater (the amount applied is shown in Table 6), and the applied ink was dried at 120° C. for 2 minutes to form a dark ink layer on the surface of the substrate. Then, immediately after drying, a transparent adhesive was gravure-coated on the surface of the dark ink layer (the amount applied was 5.0 g / m 2 ), a 5.0 μm thick (dry state) adhesive layer was layered on top of which was polyethylene resin (60 μm thick), and then aged at 45°C to 55°C for 168 hours to heat harden it to create a back protection sheet, and a new pseudo-module was created from the back protection sheet.

[0191] The pseudo module was created by laminating glass as a transparent front substrate, 450 μm of ethylene-vinyl acetate copolymer resin (EVA) as a sealing material layer, and a sample according to this embodiment as a back surface protective sheet in the order of transparent front substrate / front sealing material layer / rear sealing material layer / rear surface protective sheet, followed by vacuum lamination (vacuum lamination conditions: temperature 150° C., vacuum time 5 minutes, press time 9 minutes).

[0192] <Evaluation> In accordance with JIS-Z8722, measurements were performed using a KONICA MINOLTA spectrophotometer CM-700d under conditions of D65 light source and 10° viewing angle, with the light source shining on the transparent resin layer side of each sample. The color coordinates obtained from this test are shown in Table 6.

[0193] [Table 6]

[0194] From Table 6, Figure 5, and Figure 7, in the sample of the comparative example, the a * and b * The a in the example sample fluctuates greatly, whereas the a in the example sample fluctuates greatly with the change in the amount of adhesive (ink) applied. * and b * From these results, it can be seen that the infrared-transmitting dark ink of the embodiment has little dependence on the color coordinates for the solid coating amount of the adhesive (ink). * The L of the sample of Comparative Example 5, in which the amount of adhesive (ink) applied is larger than that of the Examples, is * and is equivalent to the L* of carbon black. From the results of this experiment, it is understood that an infrared-transmitting dark layer formed by an infrared-transmitting dark ink containing a pigment component including a brown pigment and a phthalocyanine pigment component has sufficient designability even when its thickness is small. Therefore, even when an infrared-transmitting dark layer is laminated for the purpose of partially coloring a transparent adhesive layer and / or a reflective layer from the viewpoint of design, it is possible to reduce the amount of transparent adhesive used. Therefore, it is understood that the infrared reflective sheet of the present invention is an excellent infrared reflective sheet that can reduce costs and improve productivity.

[0195] (Adhesion test) <Sample Creation> An infrared-transmitting dark ink was applied to the surface of a white PET film (Toray white PET, 188 μm) using a bar coater (application amount 4 g / m 2), and the applied ink liquid was dried at 120°C for 2 minutes to form an infrared-transmitting dark layer on the surface of the substrate. Then, the above-mentioned transparent adhesive was gravure-coated on the surface of the infrared-transmitting dark layer (amount of application was 5.0 g / m 2 ), a transparent adhesive layer 5.0 μm thick (in a dry state), was laminated with polyethylene resin (60 μm) on top of that, and then aged at 45°C to 55°C for 168 hours to heat-set the layer, thereby creating a sample infrared reflective sheet.

[0196] A pressure cooker tester (HASTTEST, manufactured by Hirayama Seisakusho) was set at 120°C, 85% RH, and 1.6 atm, and each of the above samples was placed in the test for a fixed time (in Table 7, before placement is indicated as 0h, after 24 hours placement is indicated as 24h, etc.). The above peel test was then carried out three times. The average values ​​of each measurement result before placement and after placement for a fixed time are shown in Table 7. The NCO / OH ratio in Table 7 is the ratio of the NCO value of the curing agent to the OH value of the base resin.

[0197] [Table 7]

[0198] From Table 7, it can be seen that the sample of Example 12 having an NCO / OH ratio of 1.0 or more and 2.0 or less is a sample having higher adhesiveness and adhesive durability than the sample of Comparative Example 10. [Explanation of symbols]

[0199] 1. Solar cell module 2 Transparent front board 3 Front sealing material layer 4. Solar cell elements 5 Back sealing material layer 6 Infrared reflective sheet (back protection sheet) 7 Incident light 60 Infrared-transmitting dark layer 61 Reflective layer 62 Transparent adhesive layer 63 Transparent adhesive layer

Claims

1. An infrared reflective sheet having a multi-layer structure including an infrared-transmitting dark layer and a reflective layer, When light is incident from the infrared-transmitting dark layer side, the infrared reflective sheet has an average reflectance of 10% or less for light having a wavelength of 380 nm or more and 750 nm or less, an average reflectance of 10% or less for light having a wavelength of 650 nm or more and 750 nm or less, and an average reflectance of 750 nm or more and 2200 nm or less is greater than the average reflectance of light having a wavelength of 380 nm or more and 750 nm or less, The infrared reflective sheet has only one layer being the infrared transmissive dark layer, the infrared-transmitting dark layer has a resin component and a pigment component, the content of the pigment component is 20 parts by mass or more and 40 parts by mass or less when the content of the resin component is 100 parts by mass, and the infrared-transmitting dark layer has a thickness of 15 μm or less, The infrared reflective sheet was measured in accordance with JIS-Z8722 under conditions of a D65 light source and a 10° viewing angle, and the color tone of the infrared reflective sheet and the amount of carbon black (a * is 0.15, b * -0.48, L * The color difference ΔE between the color tone of * ab is 10 or less; Infrared reflective sheet.

2. An infrared reflective sheet having a multi-layer structure including an infrared-transmitting dark layer and a reflective layer, When light is incident from the infrared-transmitting dark layer side, the infrared reflective sheet has an average reflectance of 10% or less for light having a wavelength of 380 nm or more and 750 nm or less, an average reflectance of 10% or less for light having a wavelength of 650 nm or more and 750 nm or less, and an average reflectance of 750 nm or more and 2200 nm or less is greater than the average reflectance of light having a wavelength of 380 nm or more and 750 nm or less, The infrared reflective sheet has only one layer which is the infrared transmissive dark layer, and the coating amount of the infrared transmissive dark ink which forms the infrared transmissive dark layer is 15 g / m 2 is as follows: The infrared reflective sheet was measured in accordance with JIS-Z8722 under conditions of a D65 light source and a 10° viewing angle, and the color tone of the infrared reflective sheet and the amount of carbon black (a * is 0.15, b * -0.48, L * The color difference ΔE between the color tone of * ab is 10 or less; Infrared reflective sheet.

3. An infrared reflective sheet as described in claim 1 or 2, wherein a transparent adhesion layer or a transparent easy-adhesive layer is arranged on the outermost surface of the infrared reflective sheet on the side of the infrared-transmitting dark layer.

4. A transparent reinforcing layer is provided between the reflective layer and the transparent adhesive layer or the transparent easy-adhesive layer. The infrared reflective sheet according to claim 3 .

5. the infrared transmissive dark layer is cured; 5. The infrared reflective sheet according to claim 1.

6. The infrared reflective sheet according to any one of claims 1 to 5, A back protection sheet for solar cell modules.

7. The back protective sheet according to claim 6, Solar cell module.

Citation Information

Patent Citations

  • Rear surface protective sheet for solar cell module

    JP2012216689A

  • Back sheet for solar cell and solar cell module

    JP2013093410A

  • Black pigment composition for heat shield coating material, heat shield coating material using the same, and using of the same for color matching and coating

    JP2014091788A

  • Black pigment composition

    JP2014156501A

  • Polyester film for solar battery back sheet

    JP2014192180A