Laminate
The laminate with a UV-curable hard coat layer addresses issues of scratch resistance, curling, and UV absorber elution by using a specific polymerizable compound and triazine-based UV absorber, ensuring effective blue light blocking and UV protection for display applications.
Patent Information
- Application Number
- JP2023208461
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-12-11
AI Technical Summary
Existing laminates for display applications, such as those used in liquid crystal displays and organic electroluminescent displays, face issues with insufficient surface scratch resistance, curling, and inadequate blue light blocking, while also suffering from UV absorber elution during saponification treatments, leading to increased UV transmittance and contamination.
A laminate with a hard coat layer composed of a UV-curable composition containing a polymerizable compound with three or more (meth)acryloyl groups, a triazine-based UV absorber with naphthalene rings, and a photopolymerization initiator, achieving low curling properties, excellent scratch resistance, and effective blue light cutting, while suppressing yellowing and UV absorber elution.
The laminate exhibits enhanced surface hardness, reduced curling, improved blue light absorption, and maintained UV blocking capabilities, with minimal yellowing and UV absorber elution, making it suitable for display applications.
Smart Images

Figure 0007571855000001 
Figure 0007571855000002 
Figure 0007571855000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate. [Background technology]
[0002] Substrates made of plastics such as polyethylene terephthalate resin are excellent in transparency and impact resistance, are lightweight, and are easy to process, and therefore are being used in various applications in place of glass substrates.
[0003] However, plastic substrates can have inferior surface properties such as hardness and scratch resistance compared to glass substrates, and therefore a hard coat layer is provided on the surface of the plastic substrate to improve the surface properties such as hardness and scratch resistance.
[0004] Plastic substrates cannot adequately block ultraviolet rays contained in sunlight, and so ultraviolet absorbents are often blended in to prevent deterioration due to ultraviolet rays. For example, in display devices, it is common to add ultraviolet absorbents to optical films such as polarizing plate protective films to prevent discoloration of these optical films. In addition, various organic materials such as fluorescent materials and phosphorescent materials are used in the light-emitting elements of organic EL displays, and ultraviolet absorbents are added to the surface films of the displays to prevent deterioration of these organic materials due to ultraviolet rays. (Patent Document 1)
[0005] It has also been pointed out that light in the short wavelength region of visible light (approximately 380 to 495 nm) emitted from sunlight and image display devices such as smartphones, so-called blue light, can cause damage to the human body (especially the eyes).
[0006] Patent Document 2 proposes a hard coat layer containing a yellow pigment, and describes that the transmittance of light at 440 nm is 80% or less.
[0007] A method of incorporating a blue light blocking agent has also been proposed. Patent Document 3 proposes an ultraviolet-curable hard coat resin composition having blue light blocking properties, and describes that it absorbs light at around 440 nm.
[0008] However, the cured product obtained by curing a composition containing a compound that absorbs 440 nm light has a strong yellowish hue, which is the complementary color of that wavelength range, and is unsuitable for display applications, and there is a problem that the haze value is high in a hard coat layer containing a pigment or a blue light cut agent with low solvent solubility. In addition, for display applications, it is necessary for the ultraviolet absorbing ability to not change even when exposed to light for a long time, that is, light resistance.
[0009] Patent Document 4 proposes an optical film having a blue light blocking rate of 30% or more. However, the 410 nm transmittance is high, and the blue light blocking properties are not sufficient.
[0010] Furthermore, the inventions described in Documents 1 to 4 have a problem that UV curing is difficult because a material that absorbs UV light is mixed into a UV-curable compound such as an acrylate compound, and the surface hardness and scratch resistance of the resulting cured product are insufficient. That is, the optical films proposed so far have insufficient surface scratch resistance, and further hard coat properties are required for use in display applications.
[0011] In general, it is known to use a polyfunctional acrylate compound such as pentaerythritol triacrylate or dipentaerythritol hexaacrylate to improve scratch resistance, but the use of a polyfunctional acrylate compound results in a large amount of curl in the cured product, making it difficult to use the product for display purposes. Therefore, there is a demand for a laminate having a hard coat layer that has low curling properties that can be used for display purposes, excellent scratch resistance, and blue light blocking performance.
[0012] Meanwhile, in recent years, various displays have been developed for display applications in addition to the conventionally widely used liquid crystal displays (LCDs). For example, organic electroluminescence (EL) displays are rapidly becoming more and more popular.
[0013] A polarizing plate is laminated on a general organic EL display, and the polarizing plate is often made of water-soluble polyvinyl alcohol (PVA) because of its compatibility with liquid crystals, and is manufactured by stretching it into a film after dyeing it with iodine. Since PVA polarizing plates are hygroscopic, triacetyl cellulose (TAC) film, which has excellent flame resistance, appearance (transparency) and insulation properties, is used as a protective film.
[0014] When adhering a polarizing plate made from PVA to a TAC film, the surface of the TAC film must be saponified with caustic alkali to hydrolyze some of the acetyl groups (-O=COCH groups) on the surface of the TAC film into hydrophilic hydroxyl groups (-OH).
[0015] The saponification process for TAC film is carried out by immersing the TAC film in an alkaline aqueous solution such as sodium hydroxide (NaOH) or potassium hydroxide (KOH), etc. Therefore, when a laminate with a hard coat layer having blue light blocking function is saponified on the TAC film, the UV absorber may be eluted, which may cause an increase in UV transmittance and elution (contamination) of the UV blocking agent into the saponification solution. In addition, since TAC film has high moisture permeability, there is a problem that it deteriorates under high temperature and high humidity conditions. Therefore, polarizing plates made of resin films with lower moisture permeability than TAC film have also been proposed. However, because they are produced on the same production line as TAC film, there is a possibility that the UV-blocking agent will leach out (become contaminant) into the saponification treatment solution, just as in the case of TAC film.
[0016] There has not yet been a laminate that can be used for display applications (a laminate having a hard coat layer with low curl properties and blue light blocking performance), which has excellent surface hardness, scratch resistance, and low haze, and further has suppressed yellowing and excellent light fastness and elution resistance. [Prior art documents] [Patent documents]
[0017] [Patent Document 1] International Publication No. 2017 / 217178 [Patent Document 2] JP 2017-003884 A [Patent Document 3] International Publication No. 2014 / 208749 [Patent Document 4] JP 2022-160466 A Summary of the Invention [Problem to be solved by the invention]
[0018] The present invention aims to provide a laminate having low curling properties and excellent absorption of ultraviolet light and light in the short wavelength region of visible light of 400 nm or more, and having a hard coat layer which has excellent surface hardness, scratch resistance, and low haze, and further has suppressed yellowing and excellent light resistance and elution resistance. [Means for solving the problem]
[0019] As a result of extensive research into solving the above problems, the inventors have arrived at the following inventions [1] to [3].
[0020] [1] A laminate having a hard coat layer on a transparent substrate, the hard coat layer is a cured product of an ultraviolet-curable composition containing a polymerizable compound (A), an ultraviolet absorber (B), and a photopolymerization initiator (C); The polymerizable compound (A) contains a compound (a1) having three or more (meth)acryloyl groups and a (meth)acryloyl group equivalent of 115 or more, The ultraviolet absorber (B) is a triazine compound that absorbs light having a wavelength of 400 to 420 nm, the photopolymerization initiator (C) contains at least one of an oxime ester compound (C1) and a phosphine oxide compound (C2); A laminate comprising a polyethylene terephthalate substrate and a hard coat layer having a thickness of 5 μm, the laminate satisfying all of the following (1) to (5): (1) The spectral transmittance of light with a wavelength of 410 nm is 5% or less. (2) Spectral transmittance of light with a wavelength of 450 nm is 70% or more (3)b * Value is 20 or less (4) The elastic modulus of the hard coat layer is 3.0 GPa or more. (5) After being left in a high-temperature, high-humidity room at 23°C and 50% relative humidity for 6 hours, the distance between both ends of the long side of a test film measuring 100 mm in length and 50 mm in width is 45 mm or more.
[0021] [2] The laminate according to [1], wherein the compound (a1) contains a polyfunctional urethane (meth)acrylate (a1x) having 4 to 15 (meth)acryloyl groups and a weight average molecular weight of 500 to 15,000.
[0022] [3] The laminate according to [1] or [2], wherein the ultraviolet absorber (B) has 1 to 3 naphthalene rings directly bonded to a triazine ring, and at least one of the naphthalene rings has a hydroxyl group at the 2-position. Effect of the Invention
[0023] According to the present invention described above, it is possible to provide a laminate having a hard coat layer which is excellent in surface hardness, scratch resistance, and low curling properties, and which is excellent in absorption of ultraviolet light and light in the short wavelength region of visible light of 400 nm or more, and further suppresses yellowing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The present invention will be described in detail below. Needless to say, other embodiments are also included in the scope of the present invention as long as they are consistent with the gist of the present invention. In addition, in this specification, a numerical range specified using "~" includes the numerical values before and after "~" as the lower and upper limit values.
[0025] First, the terms used in this specification will be explained. In this specification, unless otherwise specified, the terms "(meth)acrylic", "(meth)acryloyl", and "(meth)acrylate" mean "acrylic or methacrylic", "acryloyl or methacryloyl", and "acrylate or methacrylate", respectively. In addition, the "polymerizable compound (A)" may be referred to as "compound (A)," and the "photopolymerization initiator (C)" may be referred to as "initiator (C)." Unless otherwise noted, the various components appearing in this specification may be used independently as a single type, or as a mixture of two or more types.
[0026] <Hard coat layer> The hard coat layer is a cured product of an ultraviolet-curable composition containing a polymerizable compound (A), an ultraviolet absorber (B), and a photopolymerization initiator (C).
[0027] The ultraviolet-curable composition for forming a hard coat layer contains a polymerizable compound (A), an ultraviolet absorber (B), and a photopolymerization initiator (C), and thus it is possible to form a laminate having a hard coat layer that is excellent in surface hardness, scratch resistance, and low curling properties, and that is excellent in absorption of ultraviolet rays and visible light in the short wavelength region of 400 nm or more, and further has suppressed yellowing.
[0028] In the present invention, the hard coat layer has a modulus of elasticity of 3.0 GPa or more. The elastic modulus of the hard coat layer is preferably 4.0 GPa or more, more preferably 4.5 GPa or more, and is preferably 8.0 GPa or less, more preferably 6.5 GPa or less. When the elastic modulus is equal to or higher than the above lower limit, the surface of the hard coat layer is less likely to be damaged even when it is subjected to impact or abrasion.
[0029] The elastic modulus of the hard coat layer can be measured by using a nanoindenter to indent the surface of the hard coat layer at a depth of 200 nm. Details of the measurement method will be described in the Examples section.
[0030] <Polymerizable compound (A)> The polymerizable compound (A) contains a compound (a1) having three or more (meth)acryloyl groups and a (meth)acryloyl group equivalent of 115 or more.
[0031] Here, the (meth)acryloyl group equivalent is calculated by the following formula. (Meth)acryloyl group equivalent = weight average molecular weight / number of (meth)acryloyl groups in one molecule
[0032] <Compound (a1)> Compound (a1) is not particularly limited as long as it has three or more (meth)acryloyl groups and has a (meth)acryloyl group equivalent of 115 or more. Examples include, but are not limited to, polyester (meth)acrylate, epoxy (meth)acrylate, and urethane (meth)acrylate. In view of the ease of balancing surface hardness, scratch resistance, and low curling properties, (a1) preferably contains urethane (meth)acrylate.
[0033] In order to obtain a hard coat layer excellent in surface hardness, scratch resistance, and low curling property, the content of compound (a1) in 100% by mass of compound (A) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. When the content of the compound (a1) is within the above range, excellent surface hardness, scratch resistance, and low curling properties can be achieved.
[0034] <Polyester (meth)acrylate> The polyester (meth)acrylate can be obtained, for example, by reacting a polyester polycarboxylic acid obtained by polycondensing a polybasic acid and a polyhydric alcohol with a hydroxyl group-containing (meth)acrylate or the like. The polybasic acid may be aliphatic, alicyclic, or aromatic, and may be used without any particular limitation.For example, the aliphatic polybasic acid may be oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, suberic acid, maleic acid, fumaric acid, dodecanedioic acid, pimelic acid, citraconic acid, glutaric acid, itaconic acid, succinic anhydride, or maleic anhydride, and these aliphatic dicarboxylic acids and their anhydrides may be used.In addition, derivatives of the acid anhydrides may also be used.
[0035] Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, dipropylene glycol, diethylene glycol, triethylene glycol, butylene glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-methyl-1,8-octanediol, 3,3'-dimethylolheptane, 2-butyl-2-ethyl-1,3-propanediol, polyoxyethylene glycol (addition mole number of 10 or less), and polyoxypropylene glycol. Examples of the diols include aliphatic or alicyclic diols such as (addition mole number 10 or less), propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, octanediol, butylethylpentanediol, 2-ethyl-1,3-hexanediol, cyclohexanediol, cyclohexanedimethanol, tricyclodecane dimethanol, cyclopentadiene dimethanol, and dimer diol.
[0036] Furthermore, polyols containing three or more hydroxyl groups, such as glycerin, trimethylolpropane, pentaerythritol, and dipentaerythritol, may also be used in part.
[0037] Among the above polyhydric alcohols, those in which two or more hydroxyl groups have been introduced into a branched alkane, such as neopentyl glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-methyl-1,8-octanediol, 3,3'-dimethylolheptane, 2-butyl-2-ethyl-1,3-propanediol, butylethylpentanediol, 2-ethyl-1,3-hexanediol, and trimethylolpropane, are preferred in terms of the adhesiveness, heat resistance, and the like of the oligomer.
[0038] Examples of the hydroxyl group-containing (meth)acrylate include the same as those mentioned above, and among them, those containing at least one selected from trimethylolpropane di(meth)acrylate, trimethylolethane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate are preferred.
[0039] <Epoxy (meth)acrylate> Examples of polyepoxy (meth)acrylate include those obtained by esterifying the glycidyl group of an epoxy resin with (meth)acrylic acid to form a (meth)acrylate group as a functional group.
[0040] <Urethane (meth)acrylate> Urethane (meth)acrylates include, for example, those obtained by reacting diisocyanate with (meth)acrylates having a hydroxyl group, those obtained by reacting isocyanurate (trimer) of diisocyanate with (meth)acrylates having a hydroxyl group, those obtained by reacting isocyanurate (trimer) of polyisocyanate with polyol and (meth)acrylates having a hydroxyl group, and those obtained by reacting an isocyanate group-containing urethane prepolymer obtained by reacting a polyol with a polyisocyanate under conditions of excess isocyanate groups with (meth)acrylates having a hydroxyl group. Alternatively, it can also be obtained by reacting a hydroxyl group-containing urethane prepolymer obtained by reacting a polyol with a polyisocyanate under conditions of excess hydroxyl groups with (meth)acrylates having an isocyanate group.
[0041] As the diisocyanate or polyisocyanate, known ones can be used, and examples thereof include aromatic diisocyanates, aliphatic diisocyanates, and alicyclic diisocyanates. Examples of aromatic diisocyanates include 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, tolylene diisocyanate, m-tetramethylxylylene diisocyanate, 4,4-diphenylmethane diisocyanate, xylylene diisocyanate, and 2,6-diisocyanate-benzyl chloride. Examples of the aliphatic diisocyanate include butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of alicyclic diisocyanates include cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, dimeryl diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, methylcyclohexane diisocyanate, norbornane diisocyanate, and dimer diisocyanate in which the carboxy group of a dimer acid is converted into an isocyanate group. Among these, aliphatic diisocyanates and alicyclic diisocyanates are preferred from the viewpoint of suppressing yellowing when optical applications are envisaged.
[0042] Examples of hydroxyl group-containing (meth)acrylates include trimethylolpropane di(meth)acrylate, trimethylolethane di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 1-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyethyl (meth)acrylate. Examples of the hydroxyl group-containing (meth)acrylic acid ester include hydroxyl group-containing (meth)acrylic acid esters such as octyl, cyclohexanedimethanol mono(meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, ethyl-α-(hydroxymethyl) (meth)acrylate, monofunctional glycerol (meth)acrylate, or (meth)acrylic acid esters having a hydroxyl group at the terminal obtained by ring-opening addition of these (meth)acrylates with ε-caprolactone lactone, and alkylene oxide-added (meth)acrylic acid esters obtained by repeatedly adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to the above-mentioned hydroxyl group-containing (meth)acrylates. From the viewpoint of increasing the crosslink density and suppressing scratches, curling, elution of the ultraviolet absorber (B), etc., a (meth)acrylic acid ester having 2 to 5 (meth)acrylolyl groups is preferred. Specifically, it is preferred to include at least one selected from trimethylolpropane di(meth)acrylate, trimethylolethane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.
[0043] The urethane (meth)acrylate is roughly classified into a multifunctional urethane (meth)acrylate (a1x) having 4 to 15 (meth)acryloyl groups and a weight average molecular weight of 500 to 15,000, and a multifunctional urethane (meth)acrylate (a1y) other than (a1x). Among these, a multifunctional urethane (meth)acrylate (a1x) having 4 to 15 (meth)acryloyl groups and a weight average molecular weight of 500 to 15,000 is preferred. By including (a1x), a laminate having a high elastic modulus of the hard coat layer of the laminate and excellent low curling properties can be formed.
[0044] In order to obtain a hard coat layer having particularly excellent surface hardness and scratch resistance, the content of compound (a1x) in 100 mass% of compound (a1) is preferably 60 mass% or more, more preferably 70 mass% or more, and even more preferably 85 mass% or more.
[0045] <Multifunctional urethane (meth)acrylate (a1x)> The polyfunctional urethane (meth)acrylate (a1x) is a polyfunctional urethane (meth)acrylate having 4 to 15 (meth)acryloyl groups and a weight average molecular weight of 500 to 15,000. The weight average molecular weight is preferably 1,000 to 5,000. By using (a1x) having a weight average molecular weight in the above range, a laminate having excellent surface hardness and scratch resistance, and further excellent low curling properties can be formed. The weight average molecular weight (Mw) is a polystyrene-equivalent weight average molecular weight determined by gel permeation chromatography (GPC) measurement. The weight average molecular weight can be measured by the method described in the [Examples] section.
[0046] The following describes a method for producing the polyfunctional urethane (meth)acrylate (a1x), but it is by way of example and is not limited thereto. For example, the polyfunctional urethane (meth)acrylate (a1x) can be obtained by stirring a polyisocyanate and a hydroxyl group-containing (meth)acrylate in the presence of a suitable urethane catalyst under an oxygen atmosphere at 60 to 100°C for 4 to 8 hours. Specific examples of urethanization catalysts include copper naphthenate, cobalt naphthenate, zinc naphthenate, dibutyltin dilaurate, triethylamine, 1,4-diazabicyclo[2.2.2]octane, 2,6,7-trimethyl-1,4-diazabicyclo[2.2.2]octane, etc. Among these, dibutyltin dilaurate is particularly preferred. The polyisocyanate and hydroxyl group-containing (meth)acrylate may be the same as those described in the explanation of the urethane (meth)acrylate.
[0047] The (meth)acryloyl number and weight average molecular weight can be adjusted by the combination of polyol, polyisocyanate, and hydroxyl group-containing mono(meth)acrylate or poly(meth)acrylate.
[0048] Specific examples of polyfunctional urethane (meth)acrylates (a1x) whose weight average molecular weight and number of acryloyl groups are published in catalogs, etc., include Shiko UV1700B (weight average molecular weight 2000, number of acryloyl groups 10), UV7600B (weight average molecular weight 1400, number of acryloyl groups 6), UV7605B (weight average molecular weight 1100, number of acryloyl groups 6), UV7610B (weight average molecular weight 1100, number of acryloyl groups 9), U V7629EA (weight average molecular weight 4100, number of acryloyl groups 9, volatile content 35%), UV7640B (weight average molecular weight 1500, number of acryloyl groups 6-7), and UV7650B (weight average molecular weight 2300, number of acryloyl groups 4-5); MIWON Co., Ltd.: Miramer PU610 (weight average molecular weight 1800, number of acryloyl groups 6), and MU9500 (weight average molecular weight 3200, number of acryloyl groups 10); Nippon Kayaku Co., Ltd.: KAYARAD DPHA-40H (weight average molecular weight 2000, number of acryloyl groups 10), UX-5000 (weight average molecular weight 1500, number of acryloyl groups 6), UX-5102D-M20 (weight average molecular weight 3500, number of acryloyl groups 6) Examples of the resins include, but are not limited to, Art Resin UN-3320HA (weight average molecular weight 1500, number of acryloyl groups 6), UN-3320HC (weight average molecular weight 1500, number of acryloyl groups 15, volatile content 5%), UN-904 (weight average molecular weight 4900, number of acryloyl groups 10), UN-906S (weight average molecular weight 1000, number of acryloyl groups 6), UN-901T (weight average molecular weight 4000, number of acryloyl groups 9, volatile content 20%), and UN-952 (weight average molecular weight 6500 to 11000, number of acryloyl groups 10), manufactured by Negami Chemical Industries, Ltd.
[0049] The hard coat agent of the present invention may contain a polymerizable compound other than the compound (a1) as the compound (A) as necessary. Examples include a compound (a2) having three or more (meth)acryloyl groups and a (meth)acryloyl group equivalent of less than 115, and a compound (a3) having one or two (meth)acryloyl groups.
[0050] Specific examples of the compound (a2) having three or more (meth)acryloyl groups and a (meth)acryloyl group equivalent of less than 115 include: Polyol poly(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, pentaerythritol tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; Other examples include polyacrylates of polymer polyols having three or more (meth)acryloyl groups, such as polyacryl poly(meth)acrylate, polyurethane poly(meth)acrylate, and polyester (meth)acrylate; Polyepoxy(meth)acrylate; These include, but are not limited to, the following.
[0051] Examples of commercially available products of compound (a2) include polyol poly(meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate (Miramer M300 manufactured by MIWON Co., Ltd., etc.), glycerin tri(meth)acrylate (Aronix M-930 manufactured by Toagosei Co., Ltd., etc.), dipentaerythritol penta(meth)acrylate (SR399 manufactured by Sartomer Co., Ltd., etc.), dipentaerythritol hexa(meth)acrylate (Miramer M600 manufactured by MIWON Co., Ltd., etc.), pentaerythritol tri(meth)acrylate (Miramer M340 manufactured by MIWON Co., Ltd., etc.), and pentaerythritol tetra(meth)acrylate (Light Acrylate PE-4A manufactured by Kyoeisha Chemical Co., Ltd., etc.), but are not limited thereto.
[0052] Examples of the compound (a3) having one or two (meth)acryloyl groups include, but are not limited to, di(meth)acrylates such as 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, and ethylene oxide-modified di(meth)acrylate of bisphenol A, oligomers such as polyurethane poly(meth)acrylate and polyester poly(meth)acrylate, and mono(meth)acrylates such as 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, isooctyl (meth)acrylate, benzyl (meth)acrylate, cyclopentanyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and isobornyl (meth)acrylate.
[0053] <Ultraviolet absorber (B)> The ultraviolet absorber (B) is a triazine compound that absorbs light with a wavelength of 400 to 420 nm, and preferably has an absorbance of 0.1 or more over the entire wavelength range of 400 to 420 nm. Further, it is more preferable that the triazine ring has one to three naphthalene rings directly bonded to the triazine ring, and at least one of the naphthalene rings has a hydroxyl group at the 2-position. It is preferable because the action of the naphthalene ring directly bonded to the triazine ring allows the absorption of light in the visible light short wavelength region of about 400 to 420 nm in addition to the ultraviolet region of less than 400 nm. In addition, an ultraviolet absorber having 1 to 3 naphthalene rings directly bonded to the triazine ring and having a hydroxyl group at the 2-position of at least one of the naphthalene rings has an unexpected effect of enabling the desired wavelength absorption with a smaller amount of addition than before, and a cured product with suppressed yellowing can be obtained.
[0054] In order to obtain a hard coat layer that is excellent in absorbing ultraviolet light and light in the short wavelength region of visible light of 400 nm or more, the content of the ultraviolet absorber (B) relative to 100 mass% of the compound (A) is preferably 3 mass% or more, more preferably 5 mass% or more, and even more preferably 7 mass% or more. In order to obtain a hard coat layer with suppressed yellowing, the content of the ultraviolet absorber (B) is preferably 20% by mass or less, and more preferably 15% by mass or less, based on 100% by mass of the compound (A).
[0055] The ultraviolet absorber (B) is preferably a compound selected from the group consisting of the following general formulae (1), (2) and (3).
[0056] General formula (1) TIFF0007571855000001.tif87162 General formula (2) TIFF0007571855000002.tif76164 General formula (3) TIFF0007571855000003.tif68149
[0057] (In general formulas (1) to (3), R 1b ~R 1g , R 2a ~R 2g , R 3a ~R 3g are each independently a hydrogen atom, a hydroxyl group, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a nitrile group, a nitro group, a sulfo group, R7, Ar1, or a group represented by the following general formulas (4-1) to (4-3). R7 is an alkyl group having 1 to 20 carbon atoms which may have a branched chain, an alkenyl group having 1 to 20 carbon atoms which may have a branched chain, an alkoxy group having 1 to 20 carbon atoms which may have a branched chain, or an alkenyloxy group having 1 to 20 carbon atoms which may have a branched chain, which may have a hydroxyl group, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a nitrile group, a nitro group, a carboxyl group, or a sulfo group, and one or more -O-, -CO-, -COO-, -OCO-, -CONH-, or -NHCO- may be bonded between carbon atoms of the alkyl group having 1 to 20 carbon atoms which may have a branched chain, the alkenyl group having 1 to 20 carbon atoms which may have a branched chain, the alkoxy group having 1 to 20 carbon atoms which may have a branched chain, or the alkenyloxy group having 1 to 20 carbon atoms which may have a branched chain. Ar1 is an aryl group having 6 to 20 carbon atoms, an aryloxy group having 6 to 20 carbon atoms, or a biphenyl group, which may have a substituent selected from the group consisting of a hydroxyl group, an alkyl group having 1 to 20 carbon atoms which may have a branched chain, an alkenyl group having 1 to 20 carbon atoms which may have a branched chain, an aryl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms which may have a branched chain, an alkenyloxy group having 1 to 20 carbon atoms which may have a branched chain, an aryloxy group having 6 to 20 carbon atoms, a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a nitrile group, a nitro group, a carboxyl group, and a sulfo group. In addition, in the general formulae (2) to (3), R4, R5, and R6 are a hydroxyl group, R7, or Ar1. General formula (4-1) [ka]
[0058] In the general formula (4-1), X1 is -CO-, -COO-, -OCO-, -CONH-, or -NHCO-. R8 is a hydrogen atom, a hydroxyl group, R7, or Ar1. However, * in the general formula (4-1) represents a bonding site with the naphthalene ring of the general formulae (1) to (3). General formula (4-2) [ka]
[0059] In the general formula (4-2), X2 and X3 are each independently -CO-, -COO-, -OCO-, -CONH-, or -NHCO-. R9 is an arylene group having 6 to 20 carbon atoms. 10 is R7 or Ar1, provided that * in general formula (4-2) represents the bonding site with the naphthalene ring of general formulae (1) to (3). General formula (4-3) [ka]
[0060] In the general formula (4-3), X4 and X5 are each independently -CO-, -COO-, -OCO-, -CONH-, or -NHCO-. 11 R is a linear or branched alkylene group having 1 to 20 carbon atoms, or an arylene group having 6 to 20 carbon atoms. 12 is R7 or Ar1. n is 1 to 20. In addition, * in general formula (4-3) represents a bonding site with the naphthalene ring of general formulas (1) to (3).
[0061] In addition, the general formula (4-1) is preferably a group containing the general formula (4).
[0062] General formula (4) [ka]
[0063] In the general formula (4), Y is -NH- or -O-. 13is a hydrogen atom, a hydroxyl group, an alkyl group having 1 to 20 carbon atoms which may have a branched chain, an alkenyl group having 1 to 20 carbon atoms which may have a branched chain, an aryl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms which may have a branched chain, an alkenyloxy group having 1 to 20 carbon atoms which may have a branched chain, an aryloxy group having 6 to 20 carbon atoms, an alkyl group having 1 to 20 carbon atoms which may have a branched chain or an aryl group having 6 to 20 carbon atoms which may have a substituent such as a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, a nitrile group, a nitro group, a carboxyl group, or a sulfo group. However, the mark * in general formula (4) represents the bonding site with the naphthalene ring in general formulas (1) to (3).
[0064] Examples of the compound represented by the general formula (1) include the following compounds. (B1) TIFF0007571855000008.tif57116(B2) TIFF0007571855000009.tif62132(B3) TIFF0007571855000010.tif57116(B4) TIFF0007571855000011.tif66147(B5) TIFF0007571855000012.tif64168(B6) TIFF0007571855000013.tif46114 (B7) TIFF0007571855000014.tif64166 (B8) TIFF0007571855000015.tif53120
[0065] Examples of the compound represented by the general formula (2) include the following compounds. (B9) TIFF0007571855000016.tif53113
[0066] Examples of the compound represented by the general formula (3) include the following compounds. (B10) TIFF0007571855000017.tif57120
[0067] The above triazine-based compound can be synthesized by using a known synthesis method for a compound having a triazine structure. For example, a method of adding naphthol or a naphthol derivative to cyanuric chloride using aluminum trichloride can be mentioned. In addition, a method of condensing methyl 2-hydroxy-1-naphthoate and benzamidine hydrochloride using sodium methoxide can be mentioned. The naphthalene ring connected to the triazine ring by a single bond and the substituents of R4, R5, and R6 may be introduced after the triazine structure is formed, or before the triazine structure is formed.
[0068] <Photopolymerization initiator (C)> The photopolymerization initiator (C) contains at least one of an oxime ester compound (C1) and a phosphine oxide compound (C2). The oxime ester compound (C1) and the phosphine oxide compound (C2) have absorption at wavelengths of 400 nm or more, so that even if the ultraviolet light required for photoexcitation of the photopolymerization initiator is cut off by the ultraviolet absorber (B), they can efficiently generate radicals with a small amount of ultraviolet light. Of these, it is preferable to use the oxime ester compound (C1), which can provide a hard coat layer with excellent surface curing properties.
[0069] Examples of the oxime ester compound (C1) include, but are not limited to, Irgacure OXE01, Irgacure OXE02, and Irgacure OXE03 manufactured by BASF Ltd.
[0070] Examples of the phosphine oxide compound (C2) include, but are not limited to, 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 4-n-propylphenyl-di(2,6-dichlorobenzoyl)phosphine oxide.
[0071] The amount of the photopolymerization initiator (C) is preferably 0.1 to 30% by mass, more preferably 3 to 20% by mass, and even more preferably 5 to 10% by mass, based on 100% by mass of the polymerizable compound (A). Within this range, a sufficient polymerization initiation effect is obtained, and it is effective in improving the surface hardness and scratch resistance.
[0072] In addition, a photopolymerization initiator (C3) other than the oxime ester compound (C1) and the phosphine oxide compound (C2) may be used in combination. As (C3), for example, a monocarbonyl photopolymerization initiator, a dicarbonyl photopolymerization initiator, an acetophenone photopolymerization initiator, a benzoin ether photopolymerization initiator, an aminocarbonyl photopolymerization initiator, etc. can be used.
[0073] Specific examples of such photopolymerization initiators include monocarbonyl-based photopolymerization initiators such as benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, methyl-o-benzoylbenzoate, 4-phenylbenzophenone, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 2- / 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, and 1-chloro-4-propoxythioxanthone; Dicarbonyl photoinitiators such as 2-ethylanthraquinone, 9,10-phenanthrenequinone, and methyl-α-oxobenzeneacetate; acetophenone-based photopolymerization initiators such as 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxy-cyclohexyl phenyl ketone, diethoxyacetophenone, dibutoxyacetophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2,2-diethoxy-1,2-diphenylethan-1-one, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, and 1-phenyl-1,2-propanedione-2-(o-ethoxycarbonyl)oxime; Benzoin ether-based photopolymerization initiators such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, and benzoin normal butyl ether; and aminocarbonyl photopolymerization initiators such as ethyl-4-(dimethylamino)benzoate, 2-n-butoxyethyl-4-(dimethylamino)benzoate, isoamyl-4-(dimethylamino)benzoate, 2-(dimethylamino)ethyl benzoate, 4,4'-bis-4-dimethylaminobenzophenone, 4,4'-bis-4-diethylaminobenzophenone, and 2,5'-bis(4-diethylaminobenzal)cyclopentanone; etc.
[0074] Commercially available photopolymerization initiators (C3) include Omnirad 184, 651, 500, 907, 127, 369, 784, 2959, and Esacure One manufactured by IGM-Resins BV.
[0075] <Sensitizer (D)> The ultraviolet-curable composition may contain a photopolymerization initiator (C) and a sensitizer (D) in combination. Examples of the sensitizer (D) include amine-based sensitizers, anthracene-based sensitizers, and thioxanthone-based sensitizers. The sensitizers may be used alone or in combination of two or more.
[0076] Examples of the amine sensitizer include trimethylamine, methyldimethanolamine, triethanolamine, p-diethylaminoacetophenone, ethyl p-dimethylaminobenzoate (EPA), isoamyl p-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, N,N-dimethylbenzylamine, and 4'-bis(diethylamino)benzophenone. Examples of the anthracene sensitizer include 9,10-dibutoxyanthracene (DBA), 9,10-diethoxyanthracene (DEA), 9,10-dipropoxyanthracene, and 9,10-bis(2-ethylhexyloxy)anthracene.
[0077] Examples of the thioxanthone sensitizer include 2,4-diethylthioxanthone (DETX), 2-isopropylthioxanthone (ITX), and 4-isopropylthioxanthone.
[0078] Representative examples of commercially available products include amine-based sensitizers such as KAYACURE KAYACURE EPA manufactured by Nippon Kayaku Co., Ltd., anthracene-based sensitizers such as Anthracure UVS-1331 (DBA) and UVS-1101 (DEA) manufactured by Air Water Performance Chemical Inc., and thioxanthone-based sensitizers such as Omnirad DETX and ITX manufactured by IGM Resins BV.
[0079] Sensitizers having absorption up to about 420 nm, which is longer than the ultraviolet ray cutoff range, are preferred, and thioxanthone sensitizers or a combination of an amine sensitizer and a thioxanthone sensitizer are preferred.
[0080] When a sensitizer is used, the content thereof is preferably from 1 to 15% by mass relative to 100% by mass of the polymerizable compound (A).
[0081] <Other ingredients> The ultraviolet-curable composition may contain other components such as an organic solvent (E) and additives, if necessary. Examples of the additives include a thermosetting resin, a polymerization inhibitor, a leveling agent (F), a slip agent, an antifoaming agent, a surfactant, an antibacterial agent, an antiblocking agent, a plasticizer, an infrared absorbing agent, an antioxidant, a silane coupling agent, a conductive agent, an inorganic filler, a pigment, and a dye.
[0082] <Organic solvent (E)> The ultraviolet-curable composition may contain an organic solvent (E). As the organic solvent (E), known organic solvents can be used, such as aromatic organic solvents such as toluene and xylene; ketone-based organic solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester-based organic solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, and isobutyl acetate; alcohol-based organic solvents such as methanol, ethanol, n-propanol, isopropanol, and n-butanol; and glycoether-based organic solvents such as propylene glycol monomethyl ether.
[0083] When the organic solvent (E) is contained, the content of the organic solvent (E) is preferably in a range such that the non-volatile concentration of the coating composition of the present invention is 1 to 60 mass %, from the viewpoints of coatability and film-formability.
[0084] <Leveling agent (F)> The ultraviolet-curable composition may contain a leveling agent (F) depending on the performance to be imparted to the hard coat layer to be formed. The leveling agent is not particularly limited as long as it has a desired leveling effect, that is, an effect of suppressing coating defects such as cissing during coating and an effect of smoothing the surface of the coating layer to be formed. Examples of such leveling agents include silicone-based leveling agents, fluorine-based leveling agents, acrylic-based leveling agents, siloxane-modified acrylic-based leveling agents, and vinyl-based leveling agents.
[0085] As the silicone-based leveling agent, a copolymer of polyoxyalkylene and polydimethylsiloxane can be used. Commercially available silicone-based leveling agents include, for example, FZ-2118, FZ-77, FZ-2161, etc. manufactured by Toray Dow Corning Co., Ltd., KP321, KP323, KP324, KP326, KP340, KP341, etc. manufactured by Shin-Etsu Chemical Co., Ltd., and TSF4440, TSF4441, TSF4445, TSF4450, TSF4446, TSF4452, TSF445 manufactured by Momentive Performance Materials Japan, LLC. 3, TSF4460, and polyester modified silicone oils such as BYK-300, BYK-302, BYK-306, BYK-307, BYK-320, BYK-325, BYK-330, BYK-331, BYK-333, BYK-337, BYK-341, BYK-344, BYK-345, BYK-346, BYK-348, BYK-377, BYK-378, BYK-UV3500, BYK-UV3510, and BYK-UV3570 manufactured by BYK-Chemie Japan.
[0086] Fluorine-based leveling agents include copolymers of polyoxyalkylene and fluorocarbon. As a commercially available fluorine-based leveling agent, for example, Examples include the Megafack series manufactured by Epson and the FC series manufactured by Sumitomo 3M.
[0087] Commercially available acrylic leveling agents include, for example, BYK-350, BYK-352, BYK-354, BYK-355, BYK-358N, BYK-361N, BYK-380N, BYK-381, and BYK-392 manufactured by BYK Japan.
[0088] An example of a commercially available siloxane-modified acrylic leveling agent is BYK-3550 manufactured by BYK Japan.
[0089] The above leveling agents may be used alone or in combination of two or more kinds.
[0090] <Laminate> The laminate of the present invention is not particularly limited as long as it has a hard coat layer, which is a cured product of the ultraviolet-curable composition, on a transparent substrate.
[0091] <Transparent base material> The transparent substrate used in the present invention is not particularly limited, and examples thereof include glass, synthetic resin moldings, films, etc. Examples of synthetic resin moldings include moldings of synthetic resins such as polymethyl methacrylate resin, copolymer resins mainly composed of methyl methacrylate, polystyrene resins, styrene-methyl methacrylate copolymer resins, styrene-acrylonitrile copolymer resins, polycarbonate resins, cellulose acetate butyrate resins, polyallyl diglycol carbonate resins, polyvinyl chloride resins, and polyester resins.
[0092] Examples of films include polyester films, polyethylene films, polyethylene terephthalate films, polypropylene films, cellophane films, diacetyl cellulose films, triacetyl cellulose (TAC) films, acetyl cellulose butyrate films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, ethylene vinyl alcohol films, polyolefin films, polystyrene films, polycarbonate films, polymethylpentel films, polysulfone films, polyether ether ketone films, polyether sulfone films, polyether imide films, polyimide films, fluororesin films, nylon films, and acrylic films.
[0093] The film substrate used in the present invention may be of an optically transparent grade, and the thickness of the film substrate is not particularly limited, but is generally about 10 to 500 μm in terms of strength, workability such as handling, thinness, etc. In particular, 20 to 250 μm is preferred.
[0094] <Hard coat layer> The thickness of the hard coat layer is not particularly limited as long as it has hard coat properties, and is usually 1 to 20 μm, preferably 2 to 15 μm. The thickness of the laminate is not particularly limited, but is preferably from 15 to 300 μm, more preferably from 20 to 100 μm, and further preferably from 25 to 75 μm.
[0095] The laminate of the present invention, which has a hard coat layer having a thickness of 5 μm on a polyethylene terephthalate substrate, satisfies all of the following (1) to (5). (1) The spectral transmittance of light with a wavelength of 410 nm is 5% or less. (2) Spectral transmittance of light with a wavelength of 450 nm is 70% or more (3)b * Value is 20 or less (4) The elastic modulus of the hard coat layer is 3.0 GPa or more. (5) After being left in a high-temperature, high-humidity room at 23°C and 50% relative humidity for 6 hours, the distance between both ends of the long side of a test film measuring 100 mm in length and 50 mm in width is 45 mm or more. From the viewpoint of blocking blue light, the spectral transmittance of light with a wavelength of 410 nm is preferably 4% or less, and more preferably 3% or less. In order to suppress yellowing of the laminate, the spectral transmittance of light with a wavelength of 450 nm is preferably 75% or more, more preferably 80% or more, and the b* value is preferably 15 or less, more preferably 10 or less.
[0096] <Manufacture of Laminate> The method for producing the laminate is not particularly limited, and the laminate can be produced by a conventionally known method, such as coating an ultraviolet-curable composition on a transparent substrate. For example, the ultraviolet-curable composition of the present invention is applied to a polyethylene terephthalate substrate, and the solvent is dried as necessary. The applied ultraviolet-curable composition is crosslinked and cured by irradiating the composition with active energy rays, thereby obtaining a laminate having a polyethylene terephthalate substrate and a hard coat layer.
[0097] Examples of the coating method include bar coating, blade coating, spin coating, reverse coating, die coating, spray coating, roll coating, gravure coating, microgravure coating, lip coating, air knife coating, and dipping.
[0098] Examples of active energy rays that can be used include electron beams and ultraviolet rays emitted from light sources such as xenon lamps, low-pressure mercury lamps, high-pressure mercury lamps, extra-high-pressure mercury lamps, metal halide lamps, carbon arc lamps, and tungsten lamps. EXAMPLES
[0099] The present invention will be described in more detail below. The present invention is not limited to the examples. In addition, "parts by mass" is expressed as "parts" and "% by mass" is expressed as "%".
[0100] The ultraviolet absorbent (B) used in the examples was prepared as follows.
[0101] <Ultraviolet absorber (B1)> In a 300mL Erlenmeyer flask, 170 parts of chlorobenzene, 43.4 mmol of cyanuric chloride, and 65.1 mmol of aluminum chloride were charged and suspended by stirring. Next, while cooling with ice water, 151.8 mmol of 2-naphthol was added little by little. After that, the mixture was gradually returned to room temperature and stirred overnight. Meanwhile, 38.1 parts of water, 10.0 parts of 35% hydrochloric acid, and 45.0 parts of methanol were charged into a 500mL beaker, and the reaction solution was gradually added dropwise. Furthermore, 45.0 parts of methanol were added to the Erlenmeyer flask in several portions and added to the 500mL beaker while washing. The precipitate was filtered and washed by sprinkling with a mixed solvent of water / methanol = 75 parts / 75 parts. The obtained wet cake was returned to 150 parts of water, reslurried at room temperature for 30 minutes, and filtered. Then, it was washed by sprinkling with 150 parts of water. The obtained wet cake was dried overnight at 80° C. to obtain an ultraviolet absorber (B1).
[0102] The NMR measurement of the ultraviolet absorber (B1) gave results supporting the above structure. The measurement conditions were as follows: <Measurement conditions> Equipment:BRUKER AVANCE400 Resonance frequency: 400MHz (1H-NMR) Solvent: Dimethylsulfoxide-d8 Tetramethylsilane was used as the internal standard for 1H-NMR, and the chemical shift values were expressed in δ values (ppm), and the coupling constants in Hertz. s stands for singlet, d for doublet, and m for multiplet. The contents of the obtained NMR spectrum are as follows. δ=12.05(s,3H),8.70(d,J=8.4Hz,3H),8.07(d,J=8.8Hz,3H),7.93(d,J=8.0Hz,3H),7.46-7.50(m,3H),7.38-7.42(m,3H),7.34(d,J=9.2Hz,3H)
[0103] As described above, in this specification, the structure of the ultraviolet absorbent (B1) was identified by NMR as an example. The structure of the other ultraviolet absorbents was also identified by NMR in the same manner as above, but the data is omitted.
[0104] <Ultraviolet absorber (B2)> In a 200 mL Erlenmeyer flask, 100 g of N-methyl-2-pyrrolidone, 20.0 mmol of ultraviolet absorber (B1), and 40.0 mmol of potassium carbonate were charged, and the mixture was heated to 90 ° C. while stirring. Next, 40.0 mmol of 1-bromo-2-ethylhexane was charged, and the mixture was stirred at 90 ° C. for 4 hours. Meanwhile, 500 g of water was charged in a 1 L beaker, and the reaction solution was dripped little by little. The precipitate was filtered, and washed by sprinkling with 500 g of water. The obtained wet cake was returned to 500 g of water, reslurried at room temperature for 30 minutes, and filtered. Then, 500 g of water was sprinkled and washed. The obtained wet cake was dried overnight at 80 ° C. to obtain ultraviolet absorber (B2).
[0105] <Ultraviolet absorber (B3)> In a 200 mL Erlenmeyer flask, 100 g of N-methyl-2-pyrrolidone, 20.0 mmol of ultraviolet absorber (B1), and 20.0 mmol of potassium carbonate were charged, and the mixture was heated to 90 ° C. while stirring. Next, 20.0 mmol of 1-bromobutane was charged, and the mixture was stirred at 90 ° C. for 4 hours. Meanwhile, 500 g of water was charged in a 1 L beaker, and the reaction solution was dripped little by little. The precipitate was filtered, and washed by sprinkling with 500 g of water. The obtained wet cake was returned to 500 g of water, reslurried at room temperature for 30 minutes, and filtered. Then, 500 g of water was sprinkled and washed. The obtained wet cake was dried overnight at 80 ° C. to obtain ultraviolet absorber (B3).
[0106] <Ultraviolet absorber (B4)> In a 200 mL Erlenmeyer flask, 100 parts of N-methyl-2-pyrrolidone and 20.0 mmol of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS (N), manufactured by Kyoeisha Chemical) were charged and stirred while cooling with ice. 20 mmol of thionyl chloride was dropped and stirred for 2 hours while cooling with ice. Then, 20.0 mmol of ultraviolet absorber (B1) was charged and stirred at room temperature for 4 hours. Meanwhile, 500 parts of water were charged in a 1 L beaker and the previous reaction solution was dropped little by little. The precipitate was filtered and washed by sprinkling with 500 parts of water. The obtained wet cake was returned to 500 parts of water and reslurried at room temperature for 30 minutes, and filtered. Then, 500 parts of water was sprinkled and washed. The obtained wet cake was dried overnight at 80 ° C. to obtain ultraviolet absorber (B4).
[0107] <Ultraviolet absorber (B5)> In a 200 mL Erlenmeyer flask, 100 parts of N-methyl-2-pyrrolidone and 40.0 mmol of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS (N), manufactured by Kyoeisha Chemical) were charged and stirred while cooling with ice. 40 mmol of thionyl chloride was dropped and stirred for 2 hours while cooling with ice. Then, 20.0 mmol of ultraviolet absorber (B1) was charged and stirred at room temperature for 4 hours. Meanwhile, 500 parts of water were charged in a 1 L beaker and the previous reaction solution was dropped little by little. The precipitate was filtered and washed by sprinkling with 500 parts of water. The obtained wet cake was returned to 500 parts of water and reslurried at room temperature for 30 minutes, and filtered. Then, 500 parts of water was sprinkled and washed. The obtained wet cake was dried overnight at 80 ° C. to obtain ultraviolet absorber (B5).
[0108] <Ultraviolet absorber (B6)> An ultraviolet absorber (B6) was obtained in the same manner as in the production of the ultraviolet absorber (B5), except that ω-carboxy-polycaprolactone (n≒2) monoacrylate (Aronix M-5300, manufactured by Toa Gosei Co., Ltd.) was added instead of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS (N), manufactured by Kyoeisha Chemical Co., Ltd.).
[0109] <Ultraviolet absorber (B7)> An ultraviolet absorber (B7) was obtained in the same manner as in the production of ultraviolet absorber (B5), except that monohydroxyethyl phthalate acrylate (Aronix M-5400, manufactured by Toa Gosei Co., Ltd.) was added instead of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS (N), manufactured by Kyoeisha Chemical Co., Ltd.).
[0110] <Ultraviolet absorber (B8)> In a 300mL Erlenmeyer flask, 170 parts of chlorobenzene, 43.4 mmol of 2-chloro-4,6-di(naphthalene-1-yl)-1,3,5-triazine, and 65.1 mmol of aluminum chloride were charged and suspended by stirring. Next, while cooling with ice water, 65.1 mmol of 2-naphthol was added little by little. After that, the mixture was gradually returned to room temperature and stirred overnight. Meanwhile, 38.1 parts of water, 10.0 parts of 35% hydrochloric acid, and 45.0 parts of methanol were charged in a 500mL beaker, and the reaction solution was gradually added dropwise. Furthermore, 45.0 parts of methanol were added to the Erlenmeyer flask in several portions and added to the 500mL beaker while washing. The precipitate was filtered and washed by sprinkling with a mixed solvent of water / methanol = 75 parts / 75 parts. The obtained wet cake was returned to 150 parts of water, reslurried at room temperature for 30 minutes, and filtered. Thereafter, 150 parts of water was sprinkled on the cake for washing. The resulting wet cake was dried overnight at 80° C. to obtain an ultraviolet absorber (B8).
[0111] <Ultraviolet absorber (B9)> In a 300mL Erlenmeyer flask, 170 parts of chlorobenzene, 43.4 mmol of 2,4-dichloro-6-phenyl-1,3,5-triazine, and 65.1 mmol of aluminum chloride were charged and suspended by stirring. Next, 108.5 mmol of 2-naphthol was gradually added while cooling with ice water. After that, the mixture was gradually returned to room temperature and stirred overnight. Meanwhile, 38.1 parts of water, 10.0 parts of 35% hydrochloric acid, and 45.0 parts of methanol were charged in a 500mL beaker, and the reaction solution was gradually added dropwise. Furthermore, 45.0 parts of methanol were added to the Erlenmeyer flask in several portions and added to the 500mL beaker while washing. The precipitate was filtered and washed by sprinkling with a mixed solvent of water / methanol = 75 parts / 75 parts. The obtained wet cake was returned to 150 parts of water, reslurried at room temperature for 30 minutes, and filtered. Then, 150 parts of water was sprinkled and washed. The obtained wet cake was dried overnight at 80° C. to obtain an ultraviolet absorber (B9).
[0112] <Ultraviolet absorber (B10-1)> An ultraviolet absorber (B10-1) was obtained in the same manner as in the production of the ultraviolet absorber (B8), except that 2-chloro-4,6-di(naphthalen-1-yl)-1,3,5-triazine was used instead of 2-chloro-4,6-diphenyl-1,3,5-triazine.
[0113] <Ultraviolet absorber (B10-2)> 420mmol of 2-hydroxy-1-naphthoic acid methyl ester was charged into a 500mL Erlenmeyer flask and heated to 90℃ with stirring. Next, 128mmol of benzamidine hydrochloride and 26 parts of 30% sodium methylate solution were charged and stirred at 90℃ for 22 hours. After this, 200 parts of methanol were charged, cooled to room temperature, and filtered. The obtained wet cake was returned to 150 parts of methanol, reslurried at room temperature for 30 minutes, and filtered. Then, 150 parts of methanol was sprinkled and washed. The obtained wet cake was dried overnight at 80℃ to obtain ultraviolet absorber (B10-2). The ultraviolet absorber (B10-2) is the same compound as the ultraviolet absorber (B10-1) but synthesized by a different synthetic route.
[0114] <Ultraviolet absorber (B11)>: BASF Tinvin 477 <Ultraviolet absorber (B12)>: BASF Tinvin 460 <Ultraviolet absorber (B13)>: ADEKA LA-F70 <Ultraviolet absorber (B'1)>: BASF Tinvin 400
[0115] <Absorbance measurement of UV absorber (B)> The absorbance of the ultraviolet absorber (B) was measured as follows.
[0116] <Solution preparation method> 1 part of the ultraviolet absorber (B1) and 1000 parts of tetrahydrofuran were mixed and completely dissolved, and then 1 part of the above solution and 99 parts of tetrahydrofuran were uniformly mixed to prepare a solution with a concentration of 10 ppm.
[0117] <Measurement conditions> Equipment: U-3500 (Hitachi) Measurement wavelength: 260~700nm Solvent: Tetrahydrofuran Concentration: See Table 1
[0118] The evaluation criteria for the ultraviolet to visible absorption spectrum are as follows: ◎: The absorbance is 0.3 or more over the entire wavelength range of 400 to 420 nm. ○: The absorbance at wavelengths of 400 to 420 nm is 0.1 or more over the entire range △: Some absorbances at wavelengths of 400 to 420 nm are 0.1 or more, others are less than 0.1 ×: The absorbance at wavelengths of 400 to 420 nm is greater than 0 and less than 0.1 over the entire range. ××: The absorbance is 0 over the entire wavelength range of 400 to 420 nm.
[0119] [Table 1]
[0120] As shown in Table 1, it was found that the ultraviolet absorbent of the present invention has a higher absorbance per unit weight in the short wavelength visible light region of 400 to 420 nm compared to conventional ultraviolet absorbents.
[0121] (B11) Tinuvin 477 (manufactured by BASF Japan Ltd.), (B12) Tinuvin 460 (manufactured by BASF Japan Ltd.), (B13) LA-F70 (manufactured by ADEKA Corporation), and (B'1) Tinuvin 400 (manufactured by BASF Japan Ltd.) are triazine-based ultraviolet absorbents but do not have a naphthalene ring. (B11), (B12), and (B13) have an absorbance of more than 0 and less than 0.1 at wavelengths of 400 to 420 nm over the entire range, and (B'1) has an absorbance of 0 at wavelengths of 400 to 420 nm over the entire range.
[0122] The raw materials used in the synthesis examples, working examples, and comparative examples are shown in Table 2, and the blends and compositions of the synthesis examples are shown in Tables 3 and 4.
[0123] <Weight average molecular weight (Mw)> The weight average molecular weight is the polystyrene equivalent weight average molecular weight measured at a flow rate of 0.6 ml / min using a gel permeation chromatography "HLC-8220GPC" manufactured by Tosoh Corporation, with four separation columns "TSK-GEL SUPER H5000," "TSK-GEL SUPER H4000," "TSK-GELSUPER H3000," and "TSK-GEL SUPER H2000" manufactured by Tosoh Corporation connected in series, and using tetrahydrofuran at a temperature of 40°C as the mobile phase.
[0124] <Production of urethane acrylate compound (a1x-1) (1)> (Synthesis Example 1): Urethane acrylate mixed solution (A1): Into a four-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, a thermometer, and a dropping funnel, 1049.0 parts by mass of Purchase DPPA (manufactured by Molekula, dipentaerythritol pentaacrylate (a4)) and 0.1 parts by mass of Neostan U-810 (manufactured by Nitto Kasei, tin catalyst) were placed, and the liquid temperature was raised to 50°C. After that, 223.2 parts by mass of VESTANAT IPDI (manufactured by EVONIK, isophorone diisocyanate) was dropped from the dropping funnel over a period of 30 minutes. After the temperature rise subsided, the mixture was heated to 80°C and reacted for 3 hours. After confirming that the isocyanate group peak had disappeared by Fourier transform infrared spectroscopy (FT-IR), the temperature was lowered to room temperature to obtain a urethane acrylate mixed solution (A1) with a non-volatile content of 100.0% by mass, which contained 99.9% by mass of a urethane acrylate compound (a1x-1) having 10 acryloyl groups and a weight average molecular weight of 1,300 in the non-volatile content.
[0125] <Production of urethane acrylate compound (a1x-2) and compound (a1x-3)> (Synthesis Example 2) and (Synthesis Example 3): Urethane acrylate mixed solution (A2) and (A3): In the same manner as in (Synthesis Example 1), a urethane acrylate mixed solution (A2) and a mixed solution (A3) containing a urethane acrylate compound (a1x-2) and a compound (a1x-3) were obtained according to the formulations in Table 3.
[0126] <Production of urethane acrylate compound (a1x-4)> (Synthesis Example 4): Urethane acrylate mixed solution (A4): A four-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, a thermometer, and a dropping funnel was charged with 455.4 parts by mass of VESTANAT IPDI 2, 1442.1 parts by mass of CHDM (cyclohexyl dimethanol, manufactured by SK Chemicals), and 0.1 parts by mass of Neostan U-810, and the mixture was heated to 80° C. and reacted for 3 hours. After confirming that the peak intensity of the isocyanate group in FT-IR was reduced to 50% of that before the reaction, PE-3A (pentaerythritol triacrylate, manufactured by Thermo FS) was added. 596.5 parts by mass of the urethane acrylate mixture was added and reacted at 80°C for a further 3 hours. After confirming that the isocyanate group peak had disappeared in FT-IR, the temperature was lowered to room temperature to obtain a urethane acrylate mixture (A4) with a non-volatile content of 100.0% by mass, including 99.8% by mass of a urethane acrylate compound (a1x-4) having 6 acryloyl groups and a weight average molecular weight of 4,500 in the non-volatile content.
[0127] <Production of urethane acrylates (a1x-5) to (a1x-7), (a1y-1), and (Ax1-8) to (Ax1-12)> Synthesis Example 5 to Synthesis Example 8, and Synthesis Example 10 to Synthesis Example 14: In the same manner as Synthesis Example 4, urethane acrylate mixed solutions (A5) to (A8), and mixed solutions (A10) to (A14), containing urethane acrylate compounds (a1x1-5) to (a1x-7), compound (a1y-1), and compounds (a1x-8) to (a1x-12), were obtained according to the formulations in Tables 3 and 4.
[0128] <Production of urethane acrylate compound (a1y-2)> (Synthesis Example 9) Urethane acrylate mixed solution (A9): 432.5 parts by mass of 4-HBA (4-hydroxybutyl acrylate manufactured by Mitsubishi Chemical Corporation) and 0.1 parts by mass of Neostan U-810 (manufactured by Nitto Kasei Corporation, tin catalyst) were placed in a four-neck flask equipped with a stirrer, a reflux condenser, a nitrogen inlet tube, a thermometer, and a dropping funnel, and the liquid temperature was raised to 50°C. After that, 545.7 parts by mass of DURANATE TPA-100 (manufactured by Asahi Kasei Corporation, hexamethylene diisocyanate trimer) was added dropwise from the dropping funnel over a period of 30 minutes. After the temperature rise subsided, the mixture was heated to 80°C and reacted for 3 hours. After confirming that the isocyanate group peak had disappeared by Fourier transform infrared spectroscopy (FT-IR), the temperature was lowered to room temperature to obtain a urethane acrylate mixed solution (A9) with a non-volatile content of 100.0 mass%, which contained 95.8 mass% of a urethane acrylate compound (a1y-2) having three acryloyl groups and a weight average molecular weight of 950 in the non-volatile content.
[0129] As the polyacrylate mixture (A15), ARONIX M-315 (manufactured by Toagosei Co., Ltd., a mixture of 92 mass % isocyanuric acid EO-modified triacrylate (a1y-3) and 8 mass % isocyanuric acid EO-modified diacrylate (a3)) was used.
[0130] As the polyacrylate mixture (A16), ARONIX M-405 (manufactured by Toagosei Co., Ltd., a mixture of 85 mass % of dipentaerythritol hexaacrylate (a2-1) and 15 mass % of dipentaerythritol pentaacrylate (a2-2)) was used.
[0131] [Table 2]
[0132] [Table 3]
[0133] [Table 4]
[0134] Example 1: 100.07 parts by mass of the urethane acrylate mixed solution (A1), 10 parts by mass of an ultraviolet absorber (B3), and 10 parts by mass of Irgacure OXE01 (BASF, photopolymerization initiator) were added to a flask equipped with a stirrer and mixed with stirring, and 51.46 parts by mass of propylene glycol monomethyl ether (PGME) was further added and mixed with stirring to prepare a composition for forming a hard coat layer with a non-volatile content of 70% by mass.
[0135] (Example 2) to (Example 43) and (Comparative Example 1) to (Comparative Example 7): A composition for forming a hard coat layer having a nonvolatile content of 70 mass % was prepared in the same manner as in (Example 1), and the results shown in Tables 5 to 8 were obtained.
[0136] The materials used in the examples and comparative examples are described below.
[0137] Mixture (A1): A urethane acrylate mixture containing 99.93% by mass of compound (a1x-1) and 100% by mass of non-volatile matter. Mixture (A2): A urethane acrylate mixture containing 81.35% by mass of compound (a1x-2) and 83.98% by mass of non-volatile matter. Mixture (A3): A urethane acrylate mixture containing 99.89% by mass of compound (a1x-3) and 100% by mass of non-volatile matter. Mixture (A4): A urethane acrylate mixture containing 99.77% by mass of compound (a1x-4) and 100% by mass of non-volatile matter. Mixture (A5): A urethane acrylate mixture containing 99.79% by mass of compound (a1x-5) and 100% by mass of non-volatile matter. Mixture (A6): A urethane acrylate mixture containing 99.92% by mass of compound (a1x-6) and 100% by mass of non-volatile matter. Mixture (A7): A urethane acrylate mixture containing 99.92% by mass of compound (a1x-7) and 100% by mass of non-volatile matter. Mixture (A8): A urethane acrylate mixture containing 99.92% by mass of compound (a1y-1) and 100% by mass of non-volatile matter. Mixture (A9): A urethane acrylate mixture containing 95.79% by mass of compound (a1y-2) and 100% by mass of non-volatile matter. Mixture (A10): A urethane acrylate mixture containing 95.89% by mass of compound (a1x-8) and 100% by mass of non-volatile matter. Mixture (A11): A urethane acrylate mixture containing 95.92% by mass of compound (a1x-9) and 100% by mass of non-volatile matter. Mixture (A12): A urethane acrylate mixture containing 95.93% by mass of compound (a1x-10) and 100% by mass of non-volatile matter. Mixture (A13): A urethane acrylate mixture containing 95.93% by mass of compound (a1x-11) and 100% by mass of non-volatile matter. Mixture (A14): A urethane acrylate mixture containing 95.91% by mass of compound (a1x-12) and 100% by mass of non-volatile matter. As the mixed solution (A15), ARONIX M-315 (manufactured by Toagosei Co., Ltd., a mixture of 92 mass% isocyanuric acid EO modified triacrylate (a1y-3) and 8 mass% isocyanuric acid EO modified diacrylate (a3)) was used.
[0138] As the mixed solution (A16), ARONIX M-405 (manufactured by Toagosei Co., Ltd., a mixture of 85 mass % of dipentaerythritol hexaacrylate (a2-1) and 15 mass % of dipentaerythritol pentaacrylate (a2-2)) was used.
[0139] <Polyfunctional urethane (meth)acrylate compound (a1x) having 4 to 15 (meth)acryloyl groups and a weight average molecular weight of 500 to 15,000> Compound (a1x-1): weight average molecular weight 1300, number of acryloyl groups 10, acryloyl group equivalent 130, urethane acrylate (having an isophorone ring) Compound (a1x-2): Weight average molecular weight 1600, number of acryloyl groups 9, acryloyl group equivalent 178, urethane acrylate (having isophorone ring and nurate ring) Compound (a1x-3): Weight average molecular weight 800, number of acryloyl groups 6, acryloyl group equivalent 133, urethane acrylate (having an isophorone ring) Compound (a1x-4): weight average molecular weight 4500, number of acryloyl groups 6, acryloyl group equivalent 750, urethane acrylate (having isophorone ring and cyclohexyl ring) Compound (a1x-5): weight average molecular weight 5000, number of acryloyl groups 10, acryloyl group equivalent 500, urethane acrylate (having an isophorone ring and a cyclohexyl ring) Compound (a1x-6): weight average molecular weight 10,000, number of acryloyl groups 10, acryloyl group equivalent 1,000, urethane acrylate (having a polycarbonate chain having an isophorone ring and a cyclohexyl ring) Compound (a1x-7): weight average molecular weight 15,000, number of acryloyl groups 10, acryloyl group equivalent 1,500, urethane acrylate (having a polycarbonate chain having an isophorone ring and a cyclohexyl ring) Compound (a1x-8): weight average molecular weight 1600, number of acryloyl groups 10, acryloyl group equivalent 160, urethane acrylate (having isophorone ring and cyclohexyl ring) Compound (a1x-9): Weight average molecular weight 2400, number of acryloyl groups 10, acryloyl group equivalent 240, urethane acrylate (having a polycarbonate chain having an isophorone ring and a cyclohexyl ring) Compound (a1x-10): weight average molecular weight 2500, number of acryloyl groups 10, acryloyl group equivalent 250, urethane acrylate (having an isophorone ring and an aliphatic polyester chain) Compound (a1x-11): weight average molecular weight 2500, number of acryloyl groups 10, acryloyl group equivalent 250, urethane acrylate (having an isophorone ring and an aliphatic polyether chain) Compound (a1x-12): Weight average molecular weight 3200, number of acryloyl groups 15, acryloyl group equivalent 213, urethane acrylate (having an isophorone ring and an aliphatic polyether chain)
[0140] <Compound (a1y) other than compound (a1x) having 3 or more (meth)acryloyl groups and having a (meth)acryloyl group equivalent of 115 or more> Compound (a1y-1): weight average molecular weight 18000, number of acryloyl groups 10, acryloyl group equivalent 1800, urethane acrylate (having a polycarbonate chain having an isophorone ring and a cyclohexyl ring) Compound (a1y-2): Weight average molecular weight 950, number of acryloyl groups 3, acryloyl group equivalent 317, urethane acrylate (having a nurate ring) Compound (a1y-3): Weight average molecular weight 423, number of acryloyl groups 3, acryloyl group equivalent 141, isocyanuric acid EO modified triacrylate (having a nurate ring)
[0141] <Polyacrylate compound (a2) and compound (a3) other than compound (a1)> (a3) Weight average molecular weight 369, number of acryloyl groups 2, acryloyl group equivalent 185, isocyanuric acid EO modified diacrylate (having nurate ring) (a2-1) Weight average molecular weight 579, number of acryloyl groups 6, acryloyl group equivalent 96, dipentaerythritol hexaacrylate (a2-2) Weight average molecular weight 524, number of acryloyl groups 5, acryloyl group equivalent 105, dipentaerythritol pentaacrylate
[0142] <Photopolymerization initiator (C)> Photopolymerization initiator (C1-1): BASF Irugacure OXE01, oxime ester type Photopolymerization initiator (C1-2): BASF Irugacure OXE03, oxime ester type Photopolymerization initiator (C1-3): ADEKA Adeka Cruise NCI-831, oxime ester type Photopolymerization initiator (C2-1): Ormnirad TPOH, phosphine oxide type manufactured by IGM Resins Photoinitiator (C3-1): Omnirad 184, manufactured by IGM Resins, acetophenone-based Photopolymerization initiator (C3-2): ESCURE ONE manufactured by IGM Resins <Volatile matter (organic solvents)> Butyl acetate: an organic solvent derived from the polyisocyanate used in Synthesis Example 2 of (a1x-2) · Propylene glycol monomethyl ether (PGME): An organic solvent used to adjust the non-volatile content of the composition for forming the hard coat layer.
[0143] <Production of Laminate Having a Hard Coat Layer> The above ultraviolet-curable composition was applied to a polyethylene terephthalate substrate having a thickness of 50 μm using a bar coater so that the dry film thickness was 5 μm. The resulting coating layer was dried at 100° C. for 1 minute, and then irradiated with 400 mJ / cm 2 using a high-pressure mercury lamp. 2 The coating was cured by exposure to ultraviolet light of 100 .ANG. to prepare a laminate having a hard coat layer.
[0144] b) Transmittance at 410 nm and 450 nm of the laminate having the hard coat layer prepared above * The value, elastic modulus, and warpage (curl property) were measured.
[0145] [Transmittance measurement] The laminate having the hard coat layer prepared above was measured for transmittance at 410 nm and 450 nm using a Hitachi High-Tech spectrophotometer "U-4100" placed in a constant temperature and humidity chamber at 23°C and a relative humidity of 50% (hereinafter referred to as 50% RH). [410nm transmittance level classification] 3: Less than 3% 2: 3~5% 1: More than 5% [450nm transmittance level classification] 3: 75% or more 2: 70% to less than 75% 1: Less than 70%
[0146] [b * Measurement of The laminate with the hard coat layer prepared above was placed in a constant temperature and humidity room at 23°C and 50% RH, and the average value of n=3 measurements was measured under a D65 light source using a spectroscopic haze meter "SH 7000" manufactured by Nippon Denshoku Industries Co., Ltd. * It was decided. [b * Level Classification 3:15 or less 2:15 to 20 More than 1:20
[0147] [Measurement of elastic modulus] The elastic modulus of the hard coat layer of the laminate having the hard coat layer prepared above was measured at an indentation depth of 200 nm under the following conditions using a nano-indenter.
[0148] Nanoindenter: Bruker "TI Premier" Indenter: Berkovich (triangular pyramid type) Measurement mode: Single indentation Measurement temperature: room temperature (25℃) Indentation depth: 200 nm Loading (unloading) speed: 40nm / s Holding time: 2s
[0149] [Warpage measurement] The laminate having the hard coat layer prepared above was cut into a length of 100 mm and a width of 50 mm to prepare a test film, which was then left in a constant temperature and humidity chamber at 23° C. and 50% RH for 6 hours. The test film was placed on a horizontal plane, and the distance between both ends in the width direction was measured at both ends of the long sides and at three points in the center using a microgauge, and the average value was calculated. [Warpage level classification] 4: 49mm or more 3: 47mm or more and less than 49mm 2: 45mm or more and less than 47mm 1: Less than 45mm
[0150] The laminates having the hard coat layer prepared as above were evaluated for haze value, scratch resistance, pencil hardness, elution resistance and light resistance by the following methods.
[0151] [HZ[%]; Haze value evaluation] The laminate with the hard coat layer prepared above was placed in a constant temperature and humidity room at 23°C and 50% RH, and the average value of n=3 measurements was taken with a Haze Meter SH7000 manufactured by Nippon Denshoku Industries Co., Ltd. under a D65 light source to determine the haze value (HZ). If it is less than 1.0%, there is no problem in practical use. [Evaluation Criteria] 3: Less than 0.8%: Very good 2: 0.8-1.0%: No practical problems -Over 1:1.0: Not practical
[0152] [Evaluation of scratch resistance] The laminate having the hard coat layer prepared as above was evaluated for scratch resistance using a Gakushin-type friction fastness tester manufactured by Tester Sangyo Co., Ltd. A friction element (surface area 1 cm2) with a load of 1000 g was attached. 2 ) was attached with steel wool #0000, and the surface of the hard coat layer (1 cm x 15 cm) was reciprocated 10 times. After that, the number of scratches on the surface of the hard coat layer was counted and evaluated according to the following criteria. The fewer the number of scratches, the better, and if there are three or less scratches, it can be used without any problems in practical use. [Evaluation Criteria] 3: No scratches (0 pieces): Very good 2: 1-3 scratches: No problems with use 1: 4 or more scratches: Unusable
[0153] [Evaluation of pencil hardness] The laminate having the hard coat layer prepared above was measured using pencils of different hardness according to a test method in accordance with JIS K5400 (1990). If the pencil hardness is "H" or higher, there is no problem in practical use.
[0154] [Evaluation of resistance to elution] The laminate provided with the hard coat layer prepared above was cut into a test film having a length of 100 mm and a width of 50 mm. This test film was immersed in a 9% by mass aqueous solution of sodium hydroxide heated to 50° C. for 5 minutes, and then the test film was taken out, washed with water, and dried in a box oven at 100° C. for 2 minutes. The transmittance (ta) and (tc) shown below were measured using a Hitachi High-Technologies Corporation spectrophotometer "U-4100." (ta): Transmittance at a wavelength of 380 nm of a hard coat film not immersed in a sodium hydroxide aqueous solution (tc): Transmittance of the hard coat film at a wavelength of 380 nm after immersion in an aqueous solution of sodium hydroxide, washing with water and drying. From the obtained (ta) and (tc), the amount of change in transmittance ((tc)-(ta)) was calculated, and the elution resistance was evaluated according to the following criteria. Note that Comparative Example 2, which did not contain the ultraviolet absorber (B), was marked as "-" since it was not possible to evaluate the elution resistance. [Evaluation Criteria] 3: The change in transmittance is 1% or less: Good 2: The change in transmittance is greater than 1% and less than 2%: No problem in practical use 1: Transmittance change exceeds 2%: Not practical
[0155] [Lightfastness evaluation] The laminate provided with the hard coat layer thus prepared was measured using a xenon weather meter to measure 60 W / m 2 After 100 hours of exposure to an illuminance of 100 nm, the absorbances Aa and Ac at the maximum absorption wavelengths shown below were measured using a Hitachi High-Tech Corporation spectrophotometer "U-4100," and the rate of decrease in absorbance was calculated using the following formula. Absorbance decrease rate (%) = {(Aa-Ac) / Aa} x 100 Aa: Before evaluation of xenon weather meter Ac: Xenon weather meter after 100 hours exposure [Evaluation Criteria] 3: The decrease in absorbance at the maximum absorption wavelength is less than 5%: Good 2: The decrease in absorbance at the maximum absorption wavelength is 5% or more and less than 20%: no practical problems 1: The decrease in absorbance at the maximum absorption wavelength is 20% or more: Not practical
[0156]
Table 5
[0157]
Table 6
[0158]
Table 7
[0159]
Table 8
Claims
1. A laminate having a hard coat layer on a transparent substrate, the hard coat layer is a cured product of an ultraviolet-curable composition containing a polymerizable compound (A), an ultraviolet absorber (B), and a photopolymerization initiator (C); The polymerizable compound (A) includes a compound (a1) having three or more (meth)acryloyl groups and a (meth)acryloyl group equivalent of 115 or more, The ultraviolet absorber (B) is a triazine compound that absorbs light having a wavelength of 400 to 420 nm, the photopolymerization initiator (C) contains at least one of an oxime ester compound (C1) and a phosphine oxide compound (C2); A laminate comprising a transparent substrate and a hard coat layer having a thickness of 5 μm, the laminate satisfying all of the following (1) to (4): (1) Spectral transmittance of light with a wavelength of 410 nm is 5% or less (2) Spectral transmittance of light with a wavelength of 450 nm is 70% or more (3) b * Value is 20 or less (4) The elastic modulus of the hard coat layer is 3.0 GPa or more.
2. The laminate according to claim 1, characterized in that the compound (a1) contains a polyfunctional urethane (meth)acrylate (a1x) having 4 to 15 (meth)acryloyl groups and a weight average molecular weight of 500 to 15,000.
3. 3. The laminate according to claim 1, wherein the ultraviolet absorber (B) has 1 to 3 naphthalene rings directly bonded to a triazine ring, and at least one of the naphthalene rings has a hydroxyl group at the 2-position.
Citation Information
Patent Citations
Optical film, and polarizing plate and liquid crystal display device using optical film
JP2008233882A
Active energy ray-curable resin composition, cured film for hard coat, and layered product
JP2010121013A
Laminate
JP2012081742A
Coating for lower layer formation used as groundwork of hard coat layer, and laminate formed by applying the coating for lower layer formation
JP2013119553A
UV curable coating composition excellent in hot water resistance, coating film formation method and coating article
JP2015067775A