Formula and process method for producing PET (polyethylene terephthalate) nucleating master batch suitable for supercritical physical foaming

By using PTFE micropowder and nano-concave and concave rods as nucleation agents, combined with surface treatment agents and chain extenders, the problem of low chemical reaction and nucleation efficiency of PET foamed material nucleation agents is solved, and uniform nucleation and high mechanical properties are achieved The production of PET foamed materials reduces costs and improves the mechanical properties and yield of the materials.

CN118879043APending Publication Date: 2024-11-01WEISAI (JIANGSU) COMPOSITE MATERIALS TECH CO LTD

Patent Information

Application Number
CN202411212747.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The nucleating agents of existing PET foaming materials have problems such as molecular chain breakage, decreased mechanical properties, low nucleation efficiency and high cost, especially the use of organic acid salts and ionic polymer nucleating agents is not good. , Traditional inorganic nucleating agents need to be added excessively to achieve nucleation effect, affecting the mechanical properties and binding strength of the material.

Method used

PTFE powder is used as the main nucleation agent and nano-concave rods are used as auxiliary nucleation agents. A uniform nucleation masterbatch is obtained through double screw extrusion and granulation, avoiding reaction with PET molecular chains, controlling bubble size and improving melt viscoelasticity. Combined with surface treatment agents, anti-hydrolyzers and chain extenders to improve nucleation efficiency.

Benefits of technology

The uniform nucleation of PET is achieved, the cell diameter is significantly reduced, the shear performance and mechanical uniformity are improved, the yield and mechanical properties of foamed materials are improved, and the use of nucleating agents is reduced, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879043A_ABST
    Figure CN118879043A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of polymer foaming materials, in particular to a formula and a process method suitable for production of PET (polyethylene terephthalate) nucleating master batches for supercritical physical foaming, PTFE (polytetrafluoroethylene) micro powder is used as a main nucleating agent, nano attapulgite is used as an auxiliary nucleating agent, and the nucleating master batches with uniform components are obtained through twin-screw extrusion granulation; the master batch is prepared from the following raw materials in percentage by weight: 50-80% of bottle-grade PET (Polyethylene Terephthalate) slices; 5% to 10% of LDPE particles; 5%-10% of PTFE micro powder; 5%-10% of inorganic nano attapulgite; 0.5%-2% of a surface treating agent; 0.5%-2% of an anti-hydrolysis agent; 0.5%-2% of a chain extender; the PET master batch has the following beneficial effects: crystallization and nucleation of PET can be promoted, and uniformly dispersed nucleation master batch is obtained; the foam holes of the manufactured plate can be obviously reduced, the distribution of the foam holes is more uniform, the shearing performance is improved, and the mechanical uniformity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer foam material preparation, and in particular to a formula and a process method for producing PET nucleating master batches suitable for supercritical physical foaming. Background Art

[0002] Polyethylene terephthalate (PET) foam material is a closed-cell foam with low density and high strength. As a structural foam material, PET foam is widely used as the core material of sandwich structures. It can significantly increase the strength and stiffness without increasing the weight. It is used in wind power, rail transportation, ships and aerospace. Nucleating agents need to be added in the production of PET foam materials.

[0003] The nucleating agent of PET foaming material has two main functions. One is to promote the crystallization nucleation of PET molecular chain, increase the cold crystallization temperature or increase the crystallinity of PET macromolecules, so that it can obtain better mechanical properties. The working principle of the crystallization nucleating agent: adsorb the polymer chain segments to form a crystal nucleus by using external impurities, polymer crystals, artificially added small particles or high molecular compounds. The other is to promote the nucleation of bubbles. In the process of PET melt foaming, it provides a nucleation point for the vaporization of supercritical fluid, allowing the supercritical gas to adsorb and deposit on its surface to form bubbles.

[0004] The nucleating agents in the prior art are mainly the following:

[0005] 1. Chinese patent CN110563994A discloses a supercritical foaming nucleating agent and a manufacturing method, using an organic acid salt as a foaming nucleating agent.

[0006] 2. Chinese patent CN112679921A discloses a PET extrusion foaming ionomer composite nucleating agent, which uses ethylene acrylic acid copolymer ionic salt composite talc as the foaming nucleating agent.

[0007] 3. Currently, many traditional nucleating agents are mainly inorganic powders, which is mainly considered from the perspective of cost, because traditional inorganic nucleating agents such as silica, talc, montmorillonite, etc. are highly available, but the effect of use is not good.

[0008] The prior art has the following defects:

[0009] 1. Organic acid salt nucleating agents easily react chemically with polyester molecules, breaking the molecular chains, reducing melt strength, and reducing molecular weight, thereby causing the mechanical properties of the foamed products to decrease and possibly affecting the foaming properties.

[0010] 2. First, the sources of ionomers are limited, and only a few foreign suppliers can produce them. Secondly, ionomers contain ionic salts, which are easily affected by water vapor in the environment and cause quality fluctuations. Thirdly, the extrusion foaming nucleation efficiency of ionomers is low. Both the chain extender and the ionomer need to react with the hydroxyl and carboxyl groups in the PET molecular chain, which affects the nucleation efficiency of the ionomer. It is necessary to add a large amount of nucleation aids to achieve the purpose of reducing the bubble size. From the results, the above three aspects have reduced the yield rate and increased the cost.

[0011] 3. Traditional inorganic nucleating agents have low nucleation efficiency. If you want to achieve the same nucleation effect, you need to add more than 2% or even 5% of nucleating agent, which will undoubtedly affect the mechanical properties of PET foamed sheets. At the same time, the use of excessive inorganic nucleating agents will reduce the bonding strength between the foamed sheet and the epoxy resin, affecting its application in sandwich structures. Summary of the invention

[0012] The invention aims to provide a formula for producing PET nucleation masterbatch suitable for supercritical physical foaming, which has the following characteristics: promoting the crystallization nucleation of PET; providing a center for bubble nucleation, allowing supercritical gas to be adsorbed to form gas nuclei; not reacting with ester bonds on PET molecular chains, not causing molecular chain breakage, not reducing the melt strength of polyester, and thus not causing the rupture of bubble walls between adjacent bubbles, thereby controlling the size of bubbles; containing a small amount of components that can undergo chain extension reactions with PET molecules, increasing melt viscoelasticity, limiting bubble growth, and playing a role in controlling bubble size.

[0013] The above technical purpose of the present invention is achieved through the following technical scheme: a formula suitable for the production of PET nucleation masterbatch for supercritical physical foaming, using PTFE micropowder as the main nucleating agent and nano-attapulgite as the auxiliary nucleating agent, and obtaining a nucleation masterbatch with uniform components through twin-screw extrusion granulation; the masterbatch is composed of the following raw materials in weight percentage: 50%-80% bottle-grade PET chips; 5%-10% LDPE particles; 5%-10% PTFE micropowder; 5%-10% inorganic nano-attapulgite; 0.5%-2% surface treatment agent; 0.5%-2% anti-hydrolysis agent; 0.5%-2% chain extender; 0.5%-3% lubricant.

[0014] Preferably, the particle size D50 of the PTFE powder is in the range of 1.0um-2.4um.

[0015] Preferably, the nano-concave-convex rod has a diameter range of 50nm-60nm and a length range of 300-500nm, and contains Si, Al, Mg, Ti, and C elements, wherein the content of silicon and silicon oxide is 55%-65%.

[0016] Preferably, the viscosity of the PET chips is in the range of 0.78-0.85 dl / g, which is bottle-grade chips.

[0017] Preferably, the density of LDPE is in the range of 0.91-0.94 g / cm 3 .

[0018] Preferably, the surface treatment agent is any one or more of a silane coupling agent, stearic acid, and aluminate.

[0019] Preferably, the chain extender is a combination of an oxazoline and an epoxy chain extender.

[0020] Preferably, the oxazoline chain extender is one or a combination of 2,2'-bis(2-oxazoline) or 2,2'(-1,4-phenylene)bis(2-oxazoline).

[0021] Preferably, the epoxy chain extender is one or a combination of BGPM and TGDDM.

[0022] Glossary: ​​The above-mentioned PET stands for polyethylene terephthalate; LDPE stands for low-density polyethylene, also known as high-pressure polyethylene; PTFE stands for polytetrafluoroethylene, also known as Teflon, commonly known as the "King of Plastics"; BGPM stands for bisphenol A diglycidyl ether; TGDDM stands for 4,4-diaminodiphenylmethane tetraglycidylamine.

[0023] Another object of the present invention is to provide a process for producing PET nucleating masterbatch suitable for supercritical physical foaming, comprising the following steps:

[0024] Step 1: Powder preparation:

[0025] PET slices and nano-attapulgite are dried and dehumidified, and then mixed evenly with PTFE micropowder, surface treatment agent and anti-hydrolysis agent, and stirred in a mixing tank at ≤60°C and a speed of 10-30rpm for 20-40min to ensure even mixing, thereby forming a mixed material 1;

[0026] LDPE particles, chain extender and lubricant are mixed in a mixing tank at a speed of 10-30 rpm and stirred for 20-40 minutes to prepare mixed material 2;

[0027] Step 2: Mixing and granulation:

[0028] Mixed material 1 is first fed into the screw, melted at high temperature, and vacuumed by a vacuum pump to remove excess moisture, and then connected to the side feeding system, and mixed material 2 is fed into the screw through the side feeding system;

[0029] The parameters of the entire screw are set as follows: the twin-screw extruder includes zone 1-zone 10, and the temperatures thereof are: 190°C, 260°C, 255°C, 250°C, 240°C, 230°C, 200°C, 190°C, 190°C, 230°C, and the speed range is 400-500rpm.

[0030] In summary, the present invention has the following beneficial effects:

[0031] 1. It can promote the crystallization nucleation of PET and obtain uniformly dispersed nucleation masterbatch;

[0032] 2. The pores of the produced sheet can be significantly smaller, the pore distribution is more uniform, the shear performance is improved, and the mechanical uniformity is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is an optical microscope observation image of the foaming material to which the present nucleating agent is added in Example 1;

[0034] Figure 2 This is an optical microscope observation image of the foaming material to which the present nucleating agent is added in Example 2;

[0035] Figure 3 This is an optical microscope observation image of the foaming material to which the present nucleating agent is added in Example 3;

[0036] Figure 4 This is an optical microscope observation picture of the foaming material in Comparative Example 1 without adding the present nucleating agent;

[0037] Figure 5 This is an optical microscope observation picture of the foamed material in Comparative Example 2 without adding the present nucleating agent. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below in conjunction with the accompanying drawings.

[0039] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

[0040] Embodiment 1:

[0041] PTFE micropowder is used as the main nucleating agent, and nano-attapulgite is used as the auxiliary nucleating agent. At the same time, it is modified to be evenly distributed in the carrier resin to avoid agglomeration. The nucleating masterbatch with uniform components is obtained by twin-screw extrusion granulation.

[0042] The masterbatch is composed of the following raw materials in weight percentage: 50% of bottle-grade PET chips, 5% of LDPE particles, 5% of PTFE micropowder, 5% of inorganic nano-attapulgite, 0.5% of surface treatment agent, 0.5% of anti-hydrolysis agent, 0.5% of chain extender and 0.5% of lubricant, and the particle size D50 of the PTFE micropowder is 1.0um.

[0043] The nano-concave-convex rod has a diameter of 50 nm and a length of 300 nm, and contains elements such as Si, Al, Mg, Ti, and C, among which the content of silicon and silicon oxide is 55%.

[0044] The viscosity of PET chips is 0.78dl / g, which is bottle-grade chips; the density of LDPE is 0.91g / cm 3 ; The surface treatment agent is a silane coupling agent; the chain extender is a combination of oxazoline and epoxy chain extenders, the oxazoline is specifically 2,2'-bis(2-oxazoline), and the epoxy is specifically bisphenol A diglycidyl ether (BGPM).

[0045] The production process is as follows:

[0046] Step 1: Powder preparation: PET slices and nano-attapulgite are dried and dehumidified, then mixed with PTFE micropowder, surface treatment agent and anti-hydrolysis agent, and stirred in a mixing tank at 60 degrees Celsius and 10 rpm for 20 minutes. Ensure that the mixture is evenly mixed to form a mixed material 1;

[0047] LDPE particles, chain extender and lubricant are mixed in a mixing tank at a speed of 10 rpm and stirred for 20 minutes to prepare mixed material 2;

[0048] Step 2: Mixing and granulation, the mixed material 1 is first fed into the screw, melted at high temperature, and vacuumed by a vacuum pump to remove excess moisture, and then connected to the side feeding system. The mixed material 2 is fed into the screw through the side feeding system;

[0049] The parameters of the entire screw are set as follows: the twin-screw extruder includes zone 1-zone 10, and the temperatures thereof are: 190°C, 260°C, 255°C, 250°C, 240°C, 230°C, 200°C, 190°C, 190°C, 230°C, and the speed range is 400rpm.

[0050] The obtained PET nucleating masterbatch was used to make a foamed board, and the foamed board was observed using an optical microscope. The results are as follows Figure 1 shown.

[0051] Embodiment 2:

[0052] PTFE micropowder is used as the main nucleating agent, and nano-attapulgite is used as the auxiliary nucleating agent. At the same time, it is modified to be evenly distributed in the carrier resin to avoid agglomeration. The nucleating masterbatch with uniform components is obtained by twin-screw extrusion granulation.

[0053] The masterbatch is composed of the following raw materials in weight percentage: 65% of bottle-grade PET chips, 7.5% of LDPE particles, 7.5% of PTFE micropowder, 7.5% of inorganic nano-attapulgite, 1.25% of surface treatment agent, 1.25% of anti-hydrolysis agent, 1.25% of chain extender and 1.75% of lubricant, and the particle size D50 of the PTFE micropowder is 1.7um.

[0054] The nano-concave-convex rod has a diameter of 55nm and a length of 400nm, and contains elements such as Si, Al, Mg, Ti, and C, among which the content of silicon and silicon oxide is 60%.

[0055] The viscosity of PET chips is 0.815dl / g, which is bottle-grade chips; the density of LDPE is 0.925g / cm 3 ; The surface treatment agent is stearic acid; the chain extender is a combination of oxazoline and epoxy chain extenders, the oxazoline is specifically 2,2'(-1,4-phenylene)bis(2-oxazoline), and the epoxy is specifically 4,4-diaminodiphenylmethane tetraglycidylamine (TGDDM).

[0056] The production process is as follows:

[0057] Step 1: Powder preparation: PET slices and nano-attapulgite are dried and dehumidified, then mixed evenly with PTFE micropowder, surface treatment agent and anti-hydrolysis agent, and stirred in a mixing tank at 50 degrees Celsius and 20 rpm for 30 minutes. Ensure that the mixture is evenly mixed to form a mixed material 1;

[0058] LDPE particles, chain extender and lubricant are mixed in a mixing tank at a speed of 20 rpm and stirred for 30 minutes to prepare mixed material 2;

[0059] Step 2: Mixing and granulation, the mixed material 1 is first fed into the screw, melted at high temperature, and vacuumed by a vacuum pump to remove excess moisture, and then connected to the side feeding system. The mixed material 2 is fed into the screw through the side feeding system;

[0060] The parameters of the entire screw are set as follows: the twin-screw extruder includes zone 1-zone 10, and the temperatures thereof are: 190°C, 260°C, 255°C, 250°C, 240°C, 230°C, 200°C, 190°C, 190°C, 230°C, and the speed range is 450rpm.

[0061] The obtained PET nucleating masterbatch was used to make a foamed board, and the foamed board was observed using an optical microscope. The results are as follows Figure 2shown.

[0062] Embodiment 3:

[0063] PTFE micropowder is used as the main nucleating agent, and nano-attapulgite is used as the auxiliary nucleating agent. At the same time, it is modified to be evenly distributed in the carrier resin to avoid agglomeration. The nucleating masterbatch with uniform components is obtained by twin-screw extrusion granulation.

[0064] The masterbatch is composed of the following raw materials in weight percentage: 80% of bottle-grade PET chips, 10% of LDPE particles, 10% of PTFE micropowder, 10% of inorganic nano-attapulgite, 2% of surface treatment agent, 2% of anti-hydrolysis agent, 2% of chain extender and 3% of lubricant, and the particle size D50 of the PTFE micropowder is 2.4um.

[0065] The nano-concave-convex rod has a diameter of 60nm and a length of 500nm, and contains elements such as Si, Al, Mg, Ti, and C, among which the content of silicon and silicon oxide is 65%.

[0066] The viscosity of PET chips is 0.85dl / g, which is bottle-grade chips; the density of LDPE is 0.94g / cm 3 ; The surface treatment agent is aluminate; the chain extender is a combination of oxazoline and epoxy chain extenders, the oxazoline is specifically a combination of 2,2'-bis(2-oxazoline) and 2,2'(-1,4-phenylene)bis(2-oxazoline), and the epoxy is specifically a combination of bisphenol A diglycidyl ether (BGPM) and 4,4-diaminodiphenylmethane tetraglycidylamine (TGDDM).

[0067] The production process is as follows:

[0068] Step 1: Powder preparation: PET slices and nano-attapulgite are dried and dehumidified, then mixed with PTFE micropowder, surface treatment agent and anti-hydrolysis agent, and stirred in a mixing tank at 40 degrees Celsius and 30 rpm for 40 minutes. Ensure that the mixture is evenly mixed to form a mixed material 1;

[0069] LDPE particles, chain extender and lubricant are mixed in a mixing tank at a speed of 30 rpm and stirred for 40 minutes to prepare mixed material 2;

[0070] Step 2: Mixing and granulation, the mixed material 1 is first fed into the screw, melted at high temperature, and vacuumed by a vacuum pump to remove excess moisture, and then connected to the side feeding system. The mixed material 2 is fed into the screw through the side feeding system;

[0071] The parameters of the entire screw are set as follows: the twin-screw extruder includes zone 1-zone 10, and the temperatures thereof are: 190°C, 260°C, 255°C, 250°C, 240°C, 230°C, 200°C, 190°C, 190°C, 230°C, and the speed range is 500rpm.

[0072] The obtained PET nucleating masterbatch was used to make a foamed board, and the foamed board was observed using an optical microscope. The results are as follows Figure 3 shown.

[0073] Comparative Example 1:

[0074] The foamed sheet was prepared without adding the PET nucleating masterbatch in the present invention, and the foamed sheet was observed using an optical microscope. Figure 4 shown.

[0075] Comparative Example 2:

[0076] The foamed sheet was prepared without adding the PET nucleating masterbatch in the present invention, and the foamed sheet was observed using an optical microscope. Figure 5 shown.

[0077] The foamed boards prepared in the above-mentioned Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 were analyzed to obtain the following data:

[0078]

[0079]

[0080] Through testing and comparison, for PET foam with a foaming ratio of 10, the diameter of the pores was 300-400um before the implementation of the solution, and it was reduced to 200-300um after the implementation of the solution. The average diameter decreased by more than 20%.

[0081] For foam products, the integrity of the cells can also be characterized by testing the open and closed cell ratio. Before the implementation of the solution, the open and closed cell ratio was between 88% and 90%, and after the implementation of the solution, the open and closed cell ratio was between 90% and 92%.

Claims

1. A formula suitable for the production of PET nucleating masterbatch for supercritical physical foaming, characterized in that: PTFE micropowder is used as a main nucleating agent, and nano-attapulgite is used as an auxiliary nucleating agent. A nucleating masterbatch with uniform components is obtained through twin-screw extrusion granulation; the masterbatch is composed of the following raw materials in weight percentage: 50%-80% of bottle-grade PET chips; 5%-10% of LDPE particles; 5%-10% of PTFE micropowder; 5%-10% of inorganic nano-attapulgite; 0.5%-2% of surface treatment agent; 0.5%-2% of anti-hydrolysis agent; 0.5%-2% of chain extender; and 0.5%-3% of lubricant.

2. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 1, characterized in that: The particle size D50 of the PTFE micropowder is in the range of 1.0um-2.4um.

3. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 1, characterized in that: The nano-concave-convex rod has a diameter range of 50nm-60nm and a length range of 300-500nm, and contains Si, Al, Mg, Ti, and C elements, wherein the content of silicon and silicon oxide is 55%-65%.

4. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 1, characterized in that: The viscosity of PET chips ranges from 0.78 to 0.85 dl / g, which is bottle-grade chips.

5. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 1, characterized in that: LDPE density range is 0.91-0.94g / cm 3 .

6. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 1, characterized in that: The surface treatment agent is any one or more of a silane coupling agent, stearic acid, and aluminate.

7. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 1, characterized in that: The chain extender is a combination of oxazoline and epoxy chain extenders.

8. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 7, characterized in that: The oxazoline chain extender is one or a combination of 2,2'-bis(2-oxazoline) or 2,2'(-1,4-phenylene)bis(2-oxazoline).

9. The formula for producing PET nucleating masterbatch suitable for supercritical physical foaming according to claim 7, characterized in that: The epoxy chain extender is one or a combination of BGPM and TGDDM.

10. A process for producing PET nucleating masterbatch suitable for supercritical physical foaming, characterized in that: The following steps are involved: Step 1: Powder preparation: PET slices and nano-attapulgite are dried and dehumidified, and then mixed evenly with PTFE micropowder, surface treatment agent and anti-hydrolysis agent, and stirred in a mixing tank at ≤60°C and a speed of 10-30rpm for 20-40min to ensure even mixing, thereby forming a mixed material 1; LDPE particles, chain extender and lubricant are mixed in a mixing tank at a speed of 10-30 rpm and stirred for 20-40 minutes to prepare mixed material 2; Step 2: Mixing and granulation: Mixed material 1 is first fed into the screw, melted at high temperature, and vacuumed by a vacuum pump to remove excess moisture, and then connected to the side feeding system, and mixed material 2 is fed into the screw through the side feeding system; The parameters of the entire screw are set as follows: the twin-screw extruder includes zone 1-zone 10, and the temperatures thereof are: 190°C, 260°C, 255°C, 250°C, 240°C, 230°C, 200°C, 190°C, 190°C, 230°C, and the speed range is 400-500rpm.

Citation Information

Patent Citations

  • High-thermoplasticity foam polyester

    CN109852009A

  • Supercritical foaming PET (Polyethylene Terephthalate) material and preparation method thereof

    CN116041917A

  • High-strength modified PET foam as well as preparation method and application thereof

    CN117603563A

  • Flame-retardant synergistic nucleation master batch for PET foam board and preparation method of flame-retardant synergistic nucleation master batch

    CN117777678A

  • Supercritical foaming nucleating agent master batch as well as preparation method and application thereof

    CN118459971A

Cited By

  • Foaming master batch and preparation method thereof

    CN119431923A

  • Particle, composition, molded article, and low dielectric material

    JP2026094015A

  • Particles, composition, molded article, and low-dielectric material

    WO2026116463A1