Substrate processing method and substrate processing apparatus
A two-stage etching process with controlled gas flow rates addresses mask distortion issues, ensuring uniform hole shapes in silicon oxide films by protecting the organic mask during etching.
Patent Information
- Application Number
- JP2021012453
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-28
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-01-28
AI Technical Summary
Mask distortion during etching leads to abnormal shapes in underlying films, particularly in silicon oxide films etched through organic masks.
A substrate processing method involving two-stage etching with a first processing gas containing carbon and fluorine, and a lower flow rate of hydrogen and bromine, followed by a second processing gas to etch silicon oxide films, protecting the organic mask and maintaining film shape integrity.
The method effectively suppresses film shape abnormalities by reducing mask distortion and ensuring uniform, circular holes in silicon oxide films.
Smart Images

Figure 0007572123000001 
Figure 0007572123000002 
Figure 0007572123000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a substrate processing method and a substrate processing apparatus. [Background technology]
[0002] For example, Patent Document 1 proposes a plasma etching method for forming holes in a silicon oxide film by an etching process through a mask, in which the silicon oxide film is etched using an etching gas containing a fluorocarbon gas. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2006-278436 A Summary of the Invention [Problem to be solved by the invention]
[0004] If the mask is distorted, shape abnormalities will occur in the underlying film when the underlying film is etched through the mask.
[0005] The present disclosure provides a technique capable of suppressing shape abnormalities of a film during an etching process. [Means for solving the problem]
[0006] According to one aspect of the present disclosure, 1. A substrate processing method, comprising: (a) providing a substrate having a silicon-containing film and a mask of an organic film on the silicon-containing film in a chamber; (b) etching the silicon-containing film with plasma generated from a first process gas containing a carbon- and fluorine-containing gas and a hydrogen- and bromine-containing gas; and (c) further etching the silicon-containing film with plasma generated from a second process gas containing a carbon- and fluorine-containing gas, wherein a flow rate of the hydrogen- and bromine-containing gas contained in the first process gas is less than a flow rate of the carbon- and fluorine-containing gas. is provided. Effect of the Invention
[0007] According to one aspect, it is possible to suppress abnormal shape of the film in the etching process. [Brief description of the drawings]
[0008] [Figure 1]FIG. 1 is a schematic cross-sectional view showing an example of a substrate processing apparatus according to the present disclosure. [Diagram 2] FIG. 2 is a diagram showing an example of a film structure and a hole shape in the etching process according to the present disclosure. [Diagram 3] FIG. 3 is a diagram showing an example of the shape of a hole with or without addition of HBr gas according to the present disclosure. [Figure 4] FIG. 4 is a flow chart illustrating a first embodiment of a substrate processing method according to the present disclosure. [Diagram 5] FIG. 5 is a flow chart illustrating a second embodiment of a substrate processing method according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and duplicated descriptions may be omitted.
[0010] [Plasma processing system] An example of the configuration of a plasma processing system will be described below with reference to FIG. 1. The plasma processing system includes a capacitively coupled plasma processing device 1 and a control unit 2. The plasma processing device 1 is an example of a substrate processing device. The capacitively coupled plasma processing device 1 includes a plasma processing chamber 10, a gas supply unit 20, a power supply 30, and an exhaust system 40. The plasma processing device 1 also includes a substrate support 11 and a gas introduction unit. The gas introduction unit is configured to introduce at least one processing gas into the plasma processing chamber 10. The gas introduction unit includes a shower head 13. The substrate support 11 is disposed in the plasma processing chamber 10. The shower head 13 is disposed above the substrate support 11. In the present disclosure, the shower head 13 constitutes at least a part of the ceiling of the plasma processing chamber 10. The plasma processing chamber 10 has a plasma processing space 10s defined by the shower head 13, a sidewall 10a of the plasma processing chamber 10, and the substrate support 11. The plasma processing chamber 10 has at least one gas supply port for supplying at least one processing gas to the plasma processing space 10s and at least one gas exhaust port for exhausting gas from the plasma processing space. The sidewall 10a is grounded. The shower head 13 and the substrate support 11 are electrically insulated from the plasma processing chamber 10 housing.
[0011] The substrate support 11 includes a main body 111 and a ring assembly 112. The main body 111 has a central region (substrate support surface) 111a for supporting a substrate (wafer) W, and an annular region (ring support surface) 111b for supporting the ring assembly 112. The annular region 111b of the main body 111 surrounds the central region 111a of the main body 111 in a plan view. The substrate W is disposed on the central region 111a of the main body 111, and the ring assembly 112 is disposed on the annular region 111b of the main body 111 so as to surround the substrate W on the central region 111a of the main body 111. In the present disclosure, the main body 111 includes a base and an electrostatic chuck. The base includes a conductive member. The conductive member of the base functions as a lower electrode. The electrostatic chuck is disposed on the base. The upper surface of the electrostatic chuck has a substrate support surface 111a. The ring assembly 112 includes one or more annular members. At least one of the one or more annular members is an edge ring. Although not shown, the substrate support 11 may include a temperature adjustment module configured to adjust at least one of the electrostatic chuck, the ring assembly 112, and the substrate to a target temperature. The temperature adjustment module may include a heater, a heat transfer medium, a flow path, or a combination thereof. A heat transfer fluid such as brine or gas flows through the flow path. The substrate support 11 may also include a heat transfer gas supply unit configured to supply a heat transfer gas between the back surface of the substrate W and the substrate support surface 111a.
[0012] The shower head 13 is configured to introduce at least one processing gas from the gas supply unit 20 into the plasma processing space 10s. The shower head 13 has at least one gas supply port 13a, at least one gas diffusion chamber 13b, and multiple gas inlets 13c. The processing gas supplied to the gas supply port 13a passes through the gas diffusion chamber 13b and is introduced into the plasma processing space 10s from the multiple gas inlets 13c. The shower head 13 also includes a conductive member. The conductive member of the shower head 13 functions as an upper electrode. In addition to the shower head 13, the gas introduction unit may include one or more side gas injectors (SGIs) attached to one or more openings formed in the side wall 10a.
[0013] The gas supply 20 may include at least one gas source 21 and at least one flow controller 22. In the present disclosure, the gas supply 20 is configured to supply at least one process gas from a respective gas source 21 through a respective flow controller 22 to the showerhead 13. Each flow controller 22 may include, for example, a mass flow controller or a pressure-controlled flow controller. Additionally, the gas supply 20 may include one or more flow modulation devices to modulate or pulse a flow rate of the at least one process gas.
[0014] The power source 30 includes an RF power source 31 coupled to the plasma processing chamber 10 via at least one impedance matching circuit. The RF power source 31 is configured to supply at least one RF signal (RF power), such as a source RF signal and a bias RF signal, to a conductive member of the substrate support 11 and / or a conductive member of the showerhead 13. This causes a plasma to be formed from at least one processing gas supplied to the plasma processing space 10s. Thus, the RF power source 31 can function as at least a part of a plasma generating unit configured to generate a plasma from one or more processing gases in the plasma processing chamber 10. In addition, by supplying a bias RF signal to the conductive member of the substrate support 11, a bias potential is generated on the substrate W, and ion components in the formed plasma can be attracted to the substrate W.
[0015] In the present disclosure, the RF power supply 31 includes a first RF generating unit 31a and a second RF generating unit 31b. The first RF generating unit 31a is coupled to the conductive member of the substrate support 11 and / or the conductive member of the shower head 13 via at least one impedance matching circuit, and is configured to generate a source RF signal (source RF power) for plasma generation. In the present disclosure, the source RF signal has a frequency in the range of 13 MHz to 150 MHz. In the present disclosure, the first RF generating unit 31a may be configured to generate a plurality of source RF signals having different frequencies. The generated one or more source RF signals are supplied to the conductive member of the substrate support 11 and / or the conductive member of the shower head 13. The second RF generating unit 31b is coupled to the conductive member of the substrate support 11 via at least one impedance matching circuit, and is configured to generate a bias RF signal (bias RF power). In the present disclosure, the bias RF signal has a lower frequency than the source RF signal. In the present disclosure, the bias RF signal has a frequency in the range of 400 kHz to 13.56 MHz. In the present disclosure, the second RF generator 31b may be configured to generate multiple bias RF signals having different frequencies. The generated bias RF signal or signals are provided to the conductive members of the substrate support 11. In various embodiments, at least one of the source RF signal and the bias RF signal may be pulsed.
[0016] The power supply 30 may also include a DC power supply 32 coupled to the plasma processing chamber 10. The DC power supply 32 includes a first DC generator 32a and a second DC generator 32b. In the present disclosure, the first DC generator 32a is connected to a conductive member of the substrate support 11 and configured to generate a first DC signal. The generated first bias DC signal is applied to the conductive member of the substrate support 11. In the present disclosure, the first DC signal may be applied to another electrode, such as an electrode in an electrostatic chuck. In the present disclosure, the second DC generator 32b is connected to a conductive member of the showerhead 13 and configured to generate a second DC signal. The generated second DC signal is applied to the conductive member of the showerhead 13. In various embodiments, at least one of the first and second DC signals may be pulsed. The first and second DC generating units 32a, 32b may be provided in addition to the RF power supply 31, or the first DC generating unit 32a may be provided in place of the second RF generating unit 31b.
[0017] The exhaust system 40 may be connected to, for example, a gas exhaust port 10e provided at the bottom of the plasma processing chamber 10. The exhaust system 40 may include a pressure regulating valve and a vacuum pump. The pressure in the plasma processing space 10s is adjusted by the pressure regulating valve. The vacuum pump may include a turbomolecular pump, a dry pump, or a combination thereof.
[0018] The control unit 2 processes computer-executable instructions that cause the substrate processing apparatus, such as the plasma processing apparatus 1, to execute various steps described in the present disclosure. The control unit 2 may be configured to control each element of the substrate processing apparatus to execute various steps described herein. In the present disclosure, a part or all of the control unit 2 may be included in the substrate processing apparatus. The control unit 2 may include, for example, a computer 2a. The computer 2a may include, for example, a processing unit (CPU: Central Processing Unit) 2a1, a storage unit 2a2, and a communication interface 2a3. The processing unit 2a1 may be configured to perform various control operations based on a program stored in the storage unit 2a2. The storage unit 2a2 may include a random access memory (RAM), a read only memory (ROM), a hard disk drive (HDD), a solid state drive (SSD), or a combination thereof. The communication interface 2a3 may communicate with the substrate processing apparatus via a communication line such as a local area network (LAN).
[0019] [Etching process and hole shape] Next, the etching step performed in the substrate processing method according to the present disclosure will be described with reference to FIG. 2. FIG. 2 is a diagram showing a film structure that is the target of the etching step according to the present disclosure, and an example of an etching shape formed by this etching step. The substrate processing method including the etching step according to the present disclosure is performed in a substrate processing apparatus, an example of which is a plasma processing apparatus 1. Note that, although the following describes a case in which a hole H is formed by the etching step, the etching shape is not limited to this. The etching step according to the present disclosure can also be applied to a case in which, for example, a trench or the like is formed.
[0020] An example of a film structure in an initial state before etching is shown in the upper part of Fig. 2(a). On the substrate W, a polysilicon film 100, a silicon oxide film 101, an organic film 102, a Si-ARC (silicon-containing anti-reflective coating) 103, and a resist film 104 are laminated in this order from the bottom. The upper parts of Fig. 2(b) to (e) show examples of film structures during and after etching.
[0021] The lower parts of Figures 2(a) to (e) show the pattern of holes H when this film structure is viewed in plan. The lower part of Figure 2(a) shows the pattern of holes H when the film structure in an initial state is viewed in plan. A pattern of nearly circular holes H is formed at equal intervals in the resist film 104, and the Si-ARC 103 is exposed at the bottom of the holes H.
[0022] For the substrate W having the above-described film structure, the Si-ARC 103 is etched using the resist film 104 as a mask. This etching process is performed until the organic film 102 is exposed. Next, the organic film 102 is etched using the Si-ARC 103 as a mask. This etching process is performed until the silicon oxide film 101 is exposed.
[0023] 2(b) shows a film structure when the organic film 102 is etched until the silicon oxide film 101 is exposed, and holes H in the film structure when viewed from above. In the organic film 102, holes H of approximately perfect circles are formed at equal intervals.
[0024] Next, the silicon oxide film 101 is etched using the organic film 102 as a mask. This etching process is performed until the polysilicon film 100 is exposed.
[0025] 2(c) shows the film structure when the silicon oxide film 101 is etched until the polysilicon film 100 is exposed, and the holes H in the film structure when viewed in plan. When the organic film 102 is not distorted and substantially circular holes H are formed at equal intervals in the organic film 102, the silicon oxide film 101 etched through the organic film 102 will have substantially circular holes H formed at equal intervals, as shown in the lower part of FIG. 2(c).
[0026] After the above etching process is performed, the organic film 102 on the silicon oxide film 101 is removed by ashing. Figure 2(d) shows the film structure after ashing and the holes H in the film structure when viewed from above. As shown in the lower part of Figure 2(d), substantially circular holes H are formed at equal intervals in the silicon oxide film 101.
[0027] 2(e), if the size or shape of the organic film 102 is abnormal and distortion occurs in the organic film 102, then shape abnormalities will occur in the silicon oxide film 101 etched using the organic film 102 as a mask. In other words, the holes H formed in the silicon oxide film 101 will vary in size and shape, and the distance between adjacent holes H will vary.
[0028] To etch the silicon oxide film 101, fluorocarbon gases such as C4F8 gas and C4F6 gas (hereinafter also referred to as "CxFy gas") are used. The organic film 102 is damaged while the silicon oxide film 101 is being etched by the CxFy gas. As a result, the organic film 102 is scraped off, causing a selectivity ratio of the organic film 102 to the silicon oxide film 101 (hereinafter also referred to as "mask selectivity") to become insufficient, or distortion occurs in the organic film 102.
[0029] When the silicon oxide film 101 is etched using the distorted organic film 102 as a mask, a shape abnormality occurs in the hole H formed in the silicon oxide film 101, as shown in FIG. 2(e).
[0030] In response to this, it is possible to improve the mask selectivity by optimizing the gas species such as CxFy gas or hydrofluorocarbon gas (hereinafter also referred to as "CHzFy gas"), or to form a protective film on the mask. However, this method may cause a problem that the hole H of the mask of the organic film 102 is blocked.
[0031] Therefore, in the etching step included in the substrate processing method according to the present disclosure, a hydrogen (H)-containing gas is added to the CxFy gas to etch the silicon oxide film 101 in order to improve the shape of the organic film 102. Specifically, the etching of the silicon oxide film 101 is divided into two steps, and in the first etching step, a first processing gas containing a CxFy gas and an H-containing gas is supplied into the plasma processing chamber 10. Then, plasma is generated from the first processing gas to etch the silicon oxide film 101. In the first etching step, the flow rate of the H-containing gas included in the first processing gas is made smaller than the flow rate of the CxFy gas.
[0032] In the second etching step after the first etching step, a second processing gas containing a CxFy gas is supplied into the plasma processing chamber 10. Then, plasma is generated from the second processing gas to further etch the silicon oxide film 101 until the polysilicon film 100 is exposed.
[0033] FIG. 3 is a diagram showing an example of the effect when hydrogen bromide gas (HBr) is added as the H-containing gas in the first etching step.
[0034] The upper part of FIG. 3 shows an example of an etching result according to a comparative example (without addition of HBr gas). In the comparative example, HBr gas is not added to the CxFy gas in the first etching step. The second etching step of the comparative example has the same etching conditions as the second etching step of the present embodiment. That is, in the comparative example, C4F8 gas, C4F6 gas, argon (Ar) gas, and oxygen (O2) gas are supplied in the first and second etching steps, and the silicon oxide film 101 is etched by plasma generated from these gases using the organic film 102 as a mask.
[0035] 3, after etching of the silicon oxide film 101 and before ashing, the organic film 102 was damaged and distorted by the CxFy gas during etching of the silicon oxide film 101, and variations were observed in the size and shape of the holes H. As a result, in the upper right diagram after ashing of the organic film 102, shape abnormalities occurred in the holes H in the silicon oxide film 101, and the variations in the size and shape of the holes H and the distance between adjacent holes H became large.
[0036] In contrast to this, in this embodiment, in the first etching step, C4F8 gas, C4F6 gas, Ar gas, O2 gas, and HBr gas are supplied as examples of the first processing gas, and the silicon oxide film 101 is etched halfway by the plasma of these gases using the organic film 102 as a mask. Also, in the second etching step, C4F8 gas, C4F6 gas, Ar gas, and O2 gas are supplied as examples of the second processing gas, and the silicon oxide film 101 is etched by the plasma of these gases using the organic film 102 as a mask until the polysilicon film 100 is exposed.
[0037] 3, after etching of silicon oxide film 101 and before ashing, organic film 102 was protected by the action of HBr gas, which suppressed damage during etching and showed almost no distortion. Therefore, in the lower right diagram after ashing of organic film 102, the shape abnormality of holes H in silicon oxide film 101 has been improved and nearly perfect circular holes H have been formed at equal intervals in silicon oxide film 101.
[0038] 2(d), the CD (Critical Dimension) of the hole H at the top of the silicon oxide film 101 after the organic film 102 is removed by ashing is hereinafter referred to as "Hole CD." Also, the distance between adjacent holes H at the top of the silicon oxide film 101 after the organic film 102 is removed by ashing is hereinafter referred to as "Bar CD."
[0039] [Gas type] In the above example, C4F8 gas, C4F6 gas, Ar gas, O2 gas, and HBr gas are supplied as the first processing gas. However, the first processing gas may contain at least CxFy gas and an H-containing gas. The CxFy gas may be at least one of C4F8 gas and C4F6 gas, or may be another CxFy gas. The CxFy gas mainly contributes to etching the silicon oxide film 101.
[0040] HBr gas is an example of a H-containing gas, and is not limited thereto. The H-containing gas may be at least one of hydrogen (H2) gas, a gas containing H and Br, a gas containing H and C, a gas containing H, C and F, and a gas containing H and chlorine (Cl). The gas containing H and Br may be a mixed gas of H2 gas and Br2 gas, in addition to the above-mentioned HBr gas.
[0041] An example of a gas containing H and C is CH4 gas, an example of a gas containing H, C and F is CH3F gas, and an example of a gas containing H and Cl is HCl gas. The gas containing H mainly contributes to protecting the mask of the organic film 102 and improving its shape.
[0042] In the above substrate processing method, C4F8 gas, C4F6 gas, Ar gas, and O2 gas are supplied as the second processing gas. However, the second processing gas may contain at least CxFy gas. The CxFy gas may be at least one of C4F8 gas and C4F6 gas, or may be another CxFy gas. The CxFy gas of the second processing gas may be the same CxFy gas as the CxFy gas of the first processing gas, or may be a different CxFy gas.
[0043] As described above, the first processing gas and the second processing gas may further include Ar gas and / or O2 gas. Ar gas is an example of a dilution gas, and contributes to ignition of plasma. Inert gas such as He gas and N2 gas may be supplied instead of Ar gas.
[0044] Moreover, O2 gas is an example of an oxygen (O)-containing gas, and is used to mainly contribute to removing reaction products attached to the mask of the organic film 102, etc., and to prevent clogging of the mask, etc. As the O-containing gas, CO gas or CO2 gas can be used in addition to O2 gas.
[0045] The second processing gas may contain H-containing gas, similarly to the first processing gas. When the second processing gas contains H-containing gas, the ratio (flow rate ratio) of the flow rate of H-containing gas to the flow rate of CxFy gas in the second processing gas may be smaller than the ratio of the flow rate of H-containing gas to the flow rate of CxFy gas in the first processing gas. Alternatively, an O-containing gas may be added to the second processing gas according to the flow rate of H-containing gas. When both the first processing gas and the second processing gas contain H-containing gas and O-containing gas, the ratio of H-containing gas to O-containing gas in the second processing gas may be larger than the ratio of H-containing gas to O-containing gas in the first processing gas. In this way, by adjusting the H-containing gas or the flow rate ratio of H-containing gas and O-containing gas in the second processing gas, the blockage of holes H due to the addition of H-containing gas can be suppressed.
[0046] [Time for first and second etching] The time of the first etching and the time of the second etching are appropriately adjusted depending on the etching conditions such as the depth (or aspect ratio) of the hole H to be formed in the silicon oxide film 101 and the magnitude of the RF power. In one example, the ratio of the time of the first etching step to the total time of the first etching step and the second etching step is set in the range of 0.4 to 0.8 or 0.5 to 0.8. If the ratio of the first etching step is large, the hole H is easily blocked by the addition of the H-containing gas. In such a case, the flow rate of the O-containing gas may be adjusted to suppress the blocking of the hole H.
[0047] [Substrate processing method] (First embodiment) Next, a first embodiment of a substrate processing method according to the present disclosure will be described with reference to Fig. 4. Fig. 4 is a flowchart showing the first embodiment of the substrate processing method according to the present disclosure. The substrate processing method of the first embodiment is controlled by a control unit 2.
[0048] When this process is started, first, the substrate W having the film structure of FIG. 2(a) including the silicon oxide film 101 and the organic film 102 mask is provided in the plasma processing chamber 10 (step S10). Next, the Si-ARC 103 is etched using the resist film 104 as a mask until the organic film 102 is exposed (step S11). Next, the organic film 102 is etched using the Si-ARC 103 as a mask until the silicon oxide film 101 is exposed (step S12).
[0049] Next, the silicon oxide film 101 is partially etched by plasma generated from a first process gas obtained by adding H-containing gas to CxFy gas (step S13: first etching process). In the first etching process, the flow rate of the H-containing gas contained in the first process gas is controlled to be smaller than the flow rate of the CxFy gas.
[0050] Next, the silicon oxide film 101 is etched with CxFy gas until the polysilicon film 100 is exposed (step S14: second etching step). Next, the polysilicon film 100 is over-etched with CxFy gas to remove residues at the bottom of the silicon oxide film 101 (step S15). Note that the over-etching process performed in step S15 is a process for forming a slight recess in the surface of the polysilicon film 100 by over-etching, so as to prevent residues of the silicon oxide film 101 from remaining on the exposed polysilicon film 100, and can be omitted.
[0051] Next, the organic film 102 is removed by ashing (step S16), and the substrate W is unloaded from the plasma processing chamber 10 (step S17), thereby completing this process.
[0052] Second embodiment Next, a second embodiment of the substrate processing method according to the present disclosure will be described with reference to Fig. 5. Fig. 5 is a flow chart showing the second embodiment of the substrate processing method according to the present disclosure. The substrate processing method of the first embodiment is controlled by a control unit 2. The same steps as those in the first embodiment of the substrate processing method of Fig. 4 are denoted by the same step numbers.
[0053] When this process is started, first, the substrate W is provided in the plasma processing chamber 10 (step S10), the Si-ARC 103 is etched (step S11), and then the organic film 102 is etched (step S12).
[0054] Next, the silicon oxide film 101 is etched for a predetermined time (hereinafter, referred to as "predetermined time 1") by adding H-containing gas to the CxFy gas (step S20: first etching step). In the first etching step, the flow rate of the H-containing gas contained in the first processing gas is controlled to be less than the flow rate of the CxFy gas. Next, the silicon oxide film 101 is etched for a predetermined time (hereinafter, referred to as "predetermined time 2") by the CxFy gas (step S21: second etching step).
[0055] Next, it is determined whether the processes of steps S20 and S21 have been performed a predetermined number of times (hereinafter referred to as the "predetermined number of times") (step S22). While it is determined in step S22 that the processes have not been performed the predetermined number of times, the processes of steps S20 to S22 are repeatedly performed. If it is determined in step S22 that the processes have been performed the predetermined number of times, the polysilicon film 100 is over-etched with CxFy gas to remove residues at the bottom of the silicon oxide film 101 (step S15). The over-etching process performed in step S15 can be omitted.
[0056] Next, the organic film 102 is removed by ashing (step S16), and the substrate W is carried out from the plasma processing chamber 10 (step S17), thereby completing this process. Note that, although the number of repetitions is determined in step S22, it may be determined whether the polysilicon film 100 is sufficiently exposed, and when the polysilicon film 100 is sufficiently exposed, the process may proceed to the next step S15.
[0057] In the first and second embodiments of the substrate processing method described above, the organic film 102 is protected by adding an H-containing gas to the CxFy gas in the first etching step, and the shape of the organic film 102 can be improved. For example, when HBr gas is added, it is presumed that C-Br and / or Si-Br are formed as a protective film on the mask of the organic film 102. Since a protective film is formed on the organic film 102 in the first etching step, even if the silicon oxide film 101 is etched in the second etching step without adding an H-containing gas to the CxFy gas, no shape abnormality occurs in the organic film 102. This makes it possible to improve the shape abnormality of the silicon oxide film 101. However, in the second etching step, an H-containing gas may also be added to the CxFy gas following the first etching step.
[0058] [Example of substrate processing method] Next, an example of the result of an etching process performed by the substrate processing method according to the present disclosure will be described.
[0059] (Example 1: Improvement of the shape of organic films by adding HBr) First, the shape improvement of the organic film 102 by adding HBr gas will be described with reference to Example 1 of the substrate processing method according to the present disclosure. In Example 1, in the first etching step, C4F8 gas, C4F6 gas, Ar gas, O2 gas, and HBr gas were supplied as examples of the first processing gas, and the silicon oxide film 101 was etched by plasma of these gases using the organic film 102 as a mask.
[0060] Next, in the second etching step, C4F8 gas, C4F6 gas, Ar gas, and O2 gas were supplied as an example of a second processing gas, and the silicon oxide film 101 was etched by plasma of these gases using the organic film 102 as a mask.
[0061] In the first etching process, the ratio (HBr / CxFy) of the flow rate of HBr gas to the flow rate of CxFy gas (total flow rate of C4F8 gas and C4F6 gas) was controlled to 1 / 3, and the ratio (HBr / O2) of the flow rate of HBr gas to the flow rate of O2 gas was controlled to 1 / 2. As a result, the variation in hole CD (3σ of hole CD) of the top of the silicon oxide film 101 after ashing the organic film 102 was 2.4 nm, and the variation in bar CD (3σ of bar CD) was 3.1 nm. Note that the 3σ of hole CD and the 3σ of bar CD become larger when the mask shape of the organic film 102 is distorted. On the other hand, when HBr gas is not added to the first processing gas in the first etching process, the 3σ of hole CD was 2.8 nm, and the 3σ of bar CD was 5.1 nm.
[0062] From the above, it was found that when the H-containing gas was added to the first process gas and the flow rate of the H-containing gas was set to be lower than the flow rate of the CxFy gas, the 3σ of the Hole CD and the 3σ of the Bar CD could be improved and the distortion of the organic film 102 could be suppressed. As a result, the variation in the size and shape of the holes H could be suppressed, and the holes H having almost perfect circles could be formed at equal intervals in the silicon oxide film 101.
[0063] (Example 2: HBr Addition Amount) Next, the amount of HBr gas added and the improvement in the shape of the organic film 102 will be described with reference to Example 2 of the substrate processing method according to the present disclosure. The gas species of the first and second processing gases supplied in the first and second etching steps are the same as those described in Example 1.
[0064] In the first etching step, HBr / CxFy was controlled to 1 / 3, 2 / 5, and 1 / 2. Also, HBr / O2 was controlled to 1 / 2, 1 / 3, and 4 / 5, respectively. As a result of performing the first and second etching steps under these conditions, the 3σ of the hole CD of the silicon oxide film 101 after etching was 2.4 to 2.7 nm, and the 3σ of the bar CD was 3.6 to 4.1 nm.
[0065] From the above, it was found that when HBr / CxHy was controlled to 1 / 2 or less, the 3σ of Hole CD and the 3σ of Bar CD could be improved and the distortion of the organic film 102 could be suppressed. As a result, the variation in size and shape of the holes H could be suppressed, and nearly perfect circular holes H could be formed at equal intervals in the silicon oxide film 101. However, when HBr / CxFy was 1 / 2, the holes H in the organic film 102 tended to become blocked. Therefore, this tendency was improved by finely adjusting the flow rate of O2 gas.
[0066] Example 3: HBr Addition Time Next, the addition time of HBr gas and the shape improvement of the organic film 102 will be described with reference to Example 3 of the substrate processing method according to the present disclosure. The gas species of the first and second processing gases supplied in the first and second etching steps are the same as those described in Example 1.
[0067] In the first etching step, the flow rate ratio of HBr / CxFy was controlled to 1 / 3, and the flow rate ratio of HBr / O2 was controlled to 1 / 2, and the time of the first etching step, i.e., the time of adding HBr gas, was gradually increased. The first and second etching steps were performed under these conditions. As a result, when the ratio of the time of the first etching step to the total etching time (the sum of the time of the first etching step and the time of the second etching step) was in the range of 0.4 to 0.8, the 3σ of the Hole CD was 2.3 to 2.4 nm, and the 3σ of the Bar CD was 2.9 to 4.1 nm. It can be seen from these values that the shape of the organic film 102 was improved. This is presumably because the addition of HBr gas allowed the organic film 102 to be protected by a carbon-based or silicon-based protective film during etching. However, if the ratio of the time of the first etching step to the total etching time becomes large, there is a risk that the hole H in the organic film 102 may be blocked. In this case, the blockage of the hole H can be suppressed by finely adjusting the flow rate of the O2 gas.
[0068] 5, the effect of improving the shape of the organic film 102 was also confirmed. Specifically, a cycle of performing a first etching step and then a second etching step for the same time as the first etching step was repeated four times. As a result, the 3σ of the Hole CD was 2.3 nm, and the 3σ of the Bar CD was 3.4 nm. From these values, it can be seen that the second embodiment can also suppress shape abnormalities in the organic film 102 and improve the shape of the hole H in the silicon oxide film 101.
[0069] As described above, the substrate processing method according to this embodiment includes a first etching step of supplying a first processing gas containing a fluorocarbon gas and an H-containing gas into the plasma processing chamber 10 and generating plasma from the first processing gas to etch the silicon oxide film 101, and a step of supplying a second processing gas containing a fluorocarbon gas into the plasma processing chamber 10 and generating plasma from the second processing gas to further etch the silicon oxide film 101. In the first etching step, the flow rate of the H-containing gas contained in the first processing gas is controlled to be less than the flow rate of the fluorocarbon gas.
[0070] This allows the mask of the organic film 102 to be protected by the carbon-based or silicon-based protective film during etching of the silicon oxide film 101. As a result, by correcting the distortion of the organic film 102, it is possible to suppress variations in size and shape of the holes H formed in the silicon oxide film 101, and also to suppress variations in the distance between adjacent holes H. As a result, it is possible to form approximately circular holes H at equal intervals in the silicon oxide film 101.
[0071] In the embodiment described above, the silicon oxide film 101 is etched using the organic film 102 as a mask, but this is not limiting. As a modified example of the substrate processing method according to this embodiment, the method can be applied to an etching process in which a H- and Br-containing gas is added to a C- and F-containing gas, and a silicon-containing film is etched through a mask of the organic film 102.
[0072] In a modified example of the substrate processing method according to the above embodiment, the method includes the steps of providing a substrate having a silicon-containing film and an organic film mask on the silicon-containing film in a plasma processing chamber 10, a first etching step of etching the silicon-containing film with plasma generated from a first processing gas containing a C- and F-containing gas and a H- and Br-containing gas, and a second etching step of further etching the silicon-containing film with plasma generated from a second processing gas containing a C- and F-containing gas. In the first etching step, the flow rate of the H- and Br-containing gas contained in the first processing gas is controlled to be less than the flow rate of the C- and F-containing gas.
[0073] The silicon-containing film may be any one of a silicon oxide film, a silicon nitride film, and a silicon oxynitride film, or may be a laminated film containing two or more of these. The C and F-containing gas may be a fluorocarbon gas or a hydrofluorocarbon gas. The H and Br-containing gas may be HBr gas or a mixed gas of H2 gas and Br2 gas.
[0074] In the substrate processing methods according to the above embodiments and their modifications, the aspect ratios of the shapes formed in the silicon oxide film and the silicon-containing film by the first etching step and the second etching step are 5-20.
[0075] The substrate processing method and substrate processing apparatus according to the presently disclosed embodiments should be considered as illustrative and not restrictive in all respects. The embodiments can be modified and improved in various ways without departing from the scope and spirit of the appended claims. The matters described in the above embodiments can be configured in other ways without contradiction, and can be combined without contradiction.
[0076] The substrate processing apparatus of the present disclosure can be any of the following types of apparatus: Atomic Layer Deposition (ALD) apparatus, Capacitively Coupled Plasma (CCP), Inductively Coupled Plasma (ICP), Radial Line Slot Antenna (RLSA), Electron Cyclotron Resonance Plasma (ECR), and Helicon Wave Plasma (HWP). The substrate processing apparatus of the present disclosure may be an apparatus that processes a substrate using plasma, or an apparatus that processes a substrate without using plasma. [Explanation of symbols]
[0077] 1. Plasma processing equipment 2. Control section 2a Computer 2a1 Processing section 2a2 Storage section 2a3 Communication Interface 10 Plasma Processing Chamber 11 Substrate support 13. Shower Head 21 Gas Source 20 Gas supply section 30 power supply 31 RF power supply 31a First RF generation unit 31b Second RF generation unit 32a First DC generation unit 32b Second DC generation section 40 Exhaust system 100 Polysilicon film 101 Silicon oxide film 102 Organic film 103 Si-ARC 104 Resist film 111 Main body 112 Ring Assembly
Claims
1. (a) providing a substrate having a silicon-containing film and a mask of an organic film on the silicon-containing film in a chamber; (b) etching the silicon-containing film with a plasma generated from a first process gas comprising a carbon- and fluorine-containing gas and a hydrogen- and bromine-containing gas; (c) further etching the silicon-containing film with a plasma generated from a second process gas comprising a carbon- and fluorine-containing gas; having The flow rate of the hydrogen- and bromine-containing gas contained in the first process gas is less than the flow rate of the carbon- and fluorine-containing gas. A method for processing a substrate.
2. The hydrogen and bromine-containing gas is hydrogen bromide gas or a mixture of hydrogen gas and bromine gas. The method for processing a substrate according to claim 1 .
3. Repeating the steps (b) and (c); The substrate processing method according to claim 1 or 2.
4. The ratio of the time of the step (b) to the total time of the step (b) and the step (c) is 0.4 to 0.8; The substrate processing method according to claim 1 .
5. The silicon-containing film is a silicon oxide film. The substrate processing method according to claim 1 .
6. A substrate processing apparatus having a chamber in which a substrate is etched and a control unit, The control unit is (a) providing a substrate having a silicon-containing film and a mask of an organic film on the silicon-containing film in a chamber; (b) etching the silicon-containing film with a plasma generated from a first process gas comprising a carbon- and fluorine-containing gas and a hydrogen- and bromine-containing gas; (c) further etching the silicon-containing film with a plasma generated from a second process gas comprising a carbon- and fluorine-containing gas; Control the controlling a flow rate of a hydrogen- and bromine-containing gas contained in the first process gas to be lower than a flow rate of the carbon- and fluorine-containing gas; Substrate processing equipment.
7. The hydrogen and bromine-containing gas is hydrogen bromide gas or a mixed gas of hydrogen gas and bromine gas. The substrate processing apparatus according to claim 6 .
8. Repeating the steps (b) and (c). The substrate processing apparatus according to claim 6 or 7.
9. The ratio of the time of the step (b) to the total time of the step (b) and the step (c) is 0.4 to 0.
8. The substrate processing apparatus according to claim 6 .
10. The silicon-containing film, wherein the silicon-containing film is a silicon oxide film. The substrate processing apparatus according to claim 6 .
Citation Information
Patent Citations
Plasma etching method, plasma etching apparatus, control program, computer recording medium, and recording medium recorded with treatment recipe
JP2006278436A
Method of manufacturing semiconductor device
JP2012028431A
Plasma processing method and plasma processing apparatus
JP2014017406A
Etching method
JP2016225437A