Electrolytic copper foil for secondary batteries with excellent flex resistance and its manufacturing method

By incorporating TOC, cobalt, and arsenic in the copper electrolyte at specific ratios, the electrolytic copper foil achieves improved bending resistance and adhesion, addressing the deterioration of physical properties and enhancing battery life cycle performance.

JP7572129B2Active Publication Date: 2024-10-23LOTTE ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021210123
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-11-11
Filing Date
2021-12-24
Publication Date
2024-10-23
Estimated Expiration
2037-03-28

AI Technical Summary

Technical Problem

Existing electrolytic copper foils for secondary batteries face issues with deteriorating physical properties and bending resistance due to repeated charging and discharging cycles, leading to active material detachment and collector collapse.

Method used

The copper electrolyte contains Total Organic Carbon (TOC), cobalt, and arsenic at specific ratios to maintain consistent physical properties, enhancing bending resistance and adhesion, with controlled surface roughness and tensile strength.

Benefits of technology

The electrolytic copper foil exhibits excellent bending resistance, maintaining adhesion and improving battery life cycle characteristics by absorbing stress from active material volume changes during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572129000004
    Figure 0007572129000004
  • Figure 0007572129000005
    Figure 0007572129000005
  • Figure 0007572129000001
    Figure 0007572129000001
Patent Text Reader

Abstract

The present invention provides an electrolytic copper foil for secondary batteries having excellent flex resistance and a manufacturing method thereof, and more specifically, a manufacturing method that enables an electrolytic copper foil for secondary batteries having excellent flex resistance to be obtained without using a large number of additives in a copper electrolyte during copper foil production. [Solution] The electrolytic copper foil for secondary batteries is manufactured using a drum with a plating solution containing TOC, cobalt, and arsenic, and is coated with a cathode active material, and the ratio of TOC, cobalt, and arsenic contained in the electrolytic copper foil satisfies the following formula 1. Equation 1: TOC / (cobalt + arsenic) = 1.30-1.55
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrolytic copper foil for secondary batteries having excellent flex resistance and a manufacturing method thereof, and more particularly to an electrolytic copper foil for secondary batteries having excellent flex resistance even without using a large amount of additives in a copper electrolyte during copper foil production, and a manufacturing method thereof. [Background technology]

[0002] In general, electrolytic copper foil is widely used as a basic material for PCBs (Printed Circuit Boards) in the electrical / electronics industry, and demand is rapidly increasing, especially for small products such as slim notebook computers, personal digital assistants (PDAs), e-books, MP3 players, next-generation mobile phones, ultra-thin flat panel displays, etc. In addition, by improving the physical properties of electrolytic copper foil, it is also widely used as a cathode current collector for secondary batteries.

[0003] Typically, electrolytic copper foil is produced by electrolysis in an electrolytic cell that includes a cylindrical titanium cathode (also called a drum), a titanium anode coated with a lead alloy or iridium oxide that is spaced apart from the cathode, an electrolyte, and a current source. The electrolyte is made of sulfuric acid and / or copper sulfate, and when a direct current is passed between the cathode and the anode while the cylindrical cathode is rotated, copper is electrodeposited on the cathode, making it possible to continuously produce electrolytic copper foil. The process of reducing copper ions to metal by electrolysis in this way is called the foil-making process.

[0004] The copper foil obtained in the foil manufacturing process can then be subjected to additional surface treatment processes, such as a nodule treatment process to improve adhesion to the insulating substrate, a diffusion prevention process to prevent the diffusion of copper ions, an anti-rust treatment to prevent oxidation from the outside, and a chemical adhesion improvement process to complement adhesion to the insulating substrate, if necessary. If the surface treatment process is performed, it becomes copper foil for low-profile printed circuits, and if only the anti-rust treatment is performed among the surface treatment processes, it becomes copper foil for secondary batteries.

[0005] When electrodeposited copper foil is used for printed circuits, it is supplied to PCB processors in a laminated form with an insulating substrate after surface treatment, whereas when it is used for secondary batteries, it is supplied to secondary battery manufacturers after only undergoing anti-rust treatment.

[0006] Such secondary batteries have an anode and a cathode, and are configured such that an anode active material is bound to the surface of an anode current collector, and a cathode active material is bound to the surface of a cathode current collector. When such secondary batteries are repeatedly charged and discharged, the active material layer expands and contracts, causing stress between the current collector and the active material, which can cause the active material layer to fall off or the current collector to be destroyed, resulting in a problem of reduced cycle characteristics.

[0007] Therefore, there is a demand for an electrolytic copper foil for secondary batteries that has little change in physical properties and excellent flex resistance so that it can withstand changes due to expansion and contraction of the active material layer even when the charge and discharge are repeated. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention relates to an electrolytic copper foil for secondary batteries having high flex resistance and a manufacturing method thereof, which maintains constant physical properties of the copper foil by making TOC and metal additives, cobalt and arsenic, present in a copper electrolyte at a constant content.

[0009] The present invention also relates to an electrodeposited copper foil for secondary batteries, which has high flex resistance and thus provides an excellent battery life, and a method for producing the same. [Means for solving the problem]

[0010] According to one aspect of the present invention, an embodiment of the present invention provides an electrolytic copper foil for a secondary battery, which is manufactured using a drum with a plating solution containing TOC (total organic carbon), cobalt, and arsenic, and is coated with a negative electrode active material, and the ratio of TOC, cobalt, and arsenic contained in the electrolytic copper foil satisfies the following formula 1:

[0011] Equation 1: TOC / (cobalt + arsenic) = 1.30-1.55 The electrolytic copper foil is characterized in that it can be bent 110 times or more in the MIT bending test.

[0012] The plating solution is characterized in that the concentration of TOC contained therein is 100 ppm or more.

[0013] The electrolytic copper foil has one side that is in direct contact with the drum and another side that is the opposite side to the one side, and the Rz roughness of the one side and the other side is 2.0 μm or less.

[0014] The tensile strength of the electrolytic copper foil is 30 kgf / mm 2 ~51kgf / mm 2 It is characterized in that:

[0015] The electrolytic copper foil has a stretch ratio of 2% to 15%.

[0016] The electrolytic copper foil has a thickness of 4 μm to 10 μm.

[0017] According to one aspect of the present invention, an embodiment of the present invention is a method for manufacturing an electrolytic copper foil for a secondary battery, comprising the steps of: (1) preparing a plating solution containing copper, TOC, cobalt, and arsenic; (2) applying a current density of 30 ASD to 150 ASD under a condition of a temperature of 30° C. to 70° C., and performing electrolytic plating using a drum; (3) A method for producing the electrodeposited copper foil for a secondary battery, comprising: coating a negative electrode active material on the electrodeposited copper foil formed by the electrolytic plating; and wherein the ratio of TOC, cobalt, and arsenic contained in the electrodeposited copper foil satisfies the following formula 1:

[0018] Equation 1: TOC / (cobalt + arsenic) = 1.30-1.55 The electrolytic copper foil is characterized in that it can be bent 110 times or more in the MIT bending test.

[0019] The plating solution is characterized in that the concentration of TOC contained therein is 100 ppm or more. The electrolytic copper foil formed by electrolytic plating via the step (2) has one side in contact with the drum and another side opposite to the one side, and the Rz roughness of the one side and the other side is 2.0 μm or less.

[0020] The tensile strength of the electrolytic copper foil is 30 kgf / mm 2 ~51kgf / mm 2 It is characterized in that:

[0021] The electrolytic copper foil has a stretch ratio of 2% to 15%.

[0022] The electrolytic copper foil has a thickness of 4 μm to 10 μm. Effect of the Invention

[0023] According to the present invention, the TOC, cobalt and arsenic are present in the copper electrolyte at constant contents, so that the physical properties of the copper foil can be maintained constant and the flex resistance can be improved.

[0024] Moreover, according to the present invention, it is possible to provide an electrodeposited copper foil for a secondary battery having excellent flex resistance and improved life cycle characteristics of the battery. [Brief description of the drawings]

[0025] [Figure 1]1 is a flowchart showing a method for producing an electrolytic copper foil for a secondary battery according to an embodiment of the present invention. [Diagram 2] 1 is a diagram showing a process for manufacturing an electrolytic copper foil using a drum according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Further details of the embodiments are included in the detailed description and the drawings.

[0027] The advantages and features of the present invention, and the methods for achieving them, will become clear with reference to the following detailed description of the embodiments in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, and may be embodied in various different forms. In the following description, when a part is connected to another part, this includes not only a direct connection, but also a connection via another medium. In addition, in the drawings, parts that are not related to the present invention are omitted to clarify the description of the present invention, and similar parts are designated by the same reference numerals throughout the specification.

[0028] The present invention will now be described with reference to the accompanying drawings.

[0029] Next, the electrolytic copper foil for a secondary battery having improved flex resistance according to an embodiment of the present invention will be described in more detail.

[0030] According to an embodiment of the present invention, there is provided an electrolytic copper foil for a secondary battery, which is manufactured using a drum and coated with a negative electrode active material, and the electrolytic copper foil includes an electrolytic copper foil for a secondary battery having a bending number of 110 times or more in an MIT bending test.

[0031] In the conventional manufacturing technology of electrolytic copper foil, a method of increasing the strength of copper foil and improving its flex resistance by using a large number of additives is used. However, when a large number of additives are used during the manufacturing of copper foil, the elongation rate decreases, making it difficult to maintain the physical properties during mass production of copper foil, and the charge / discharge cycle characteristics of secondary batteries decrease, which is undesirable.

[0032] In order to solve the above problems, the present invention provides an electrolytic copper foil for secondary batteries having excellent flex resistance without using a large number of additives in the copper electrolyte during the production of the copper foil, and a method for producing the same.

[0033] The electrolytic copper foil according to the present invention has a certain content of TOC in the copper electrolyte used for copper plating, thereby preventing the physical properties from changing during mass production of the copper foil and providing an electrolytic copper foil for secondary batteries with improved flex resistance. The electrolytic copper foil for secondary batteries according to the present invention is characterized by having a flex number of 110 or more in the MIT flex test. When the copper foil has excellent flexibility, it can effectively absorb the large stress applied to the foil due to the large volume change of the active material during charging and discharging of the battery, thereby preventing the phenomenon of the cycle characteristics being deteriorated or the current collector being destroyed.

[0034] In the present invention, by making the copper electrolyte contain 100 ppm or more of TOC during the production of electrolytic copper foil, the physical properties of the copper foil are maintained constant, the flex resistance is improved, the life cycle is improved, and cracks are prevented.

[0035] In addition, the electrolytic copper foil for secondary batteries according to the present invention includes one side directly contacting the drum and another side opposite to the one side, and the Rz roughness of the one side and the other side may be 2.0 μm or less. The active material in the secondary battery undergoes volumetric changes during charging and discharging, and therefore, in order to maintain an excellent battery life, it is very important to maintain a good adhesion state between the current collector, which is the copper foil, and the active material. Therefore, in order to improve the adhesion state, the surface roughness of the electrolytic copper foil must be flattened so that the spreadability of the solvent for the active material is improved and the binder is uniformly distributed to increase the adhesive force. If the surface roughness of the one side and the other side of the electrolytic copper foil exceeds 2.0 μm, the adhesive force between the current collector and the active material is reduced, and the performance of the battery may be reduced due to the volumetric changes during charging and discharging of the secondary battery.

[0036] FIG. 1 is a flow chart showing a method for producing an electrodeposited copper foil for a secondary battery according to an embodiment of the present invention. Referring to FIG. 1, the method for producing an electrodeposited copper foil for a secondary battery according to the present invention includes: (1) adding copper ions (Cu 2+ (1) preparing a plating solution containing 60 g / L to 140 g / L of cadmium, 70 g / L to 200 g / L of sulfuric acid, 10 ppm to 90 ppm of chlorine, 100 ppm or more of TOC, cobalt and arsenic (S100); (2) applying a current density of 30 ASD to 150 ASD under a condition of a temperature of 30° C. to 70° C. and performing electrolytic plating using a drum (S200); and (3) coating the electrolytic copper foil formed by the electrolytic plating with a negative electrode active material (S300).

[0037] In step (1) (S100), a plating solution is prepared by adding copper ions (Cu 2+ A plating solution containing 60g / L to 140g / L of copper, 70g / L to 200g / L of sulfuric acid, 10ppm to 90ppm of chlorine, 100ppm or more of TOC, cobalt and arsenic is prepared. In the plating solution, TOC plays a role in minimizing the change in grain size in the copper foil during electrolytic plating.

[0038] In addition, in the present invention, in order to improve the flex resistance of the electrolytic copper foil for secondary batteries, cobalt and arsenic are further included as metal additives other than TOC. The electrolytic copper foil can be manufactured by electrolytic plating using a plating solution, in which TOC can be included at a certain content, cobalt can be included at 1 mg / L to 50 mg / L, and arsenic can be included at 10 mg / L to 80 mg / L.

[0039] The concentrations of TOC, cobalt, arsenic, etc. are not always the same as those of electrodeposited copper foil produced by electrolytic plating, but may be the same or less.

[0040] The cobalt and arsenic control the plating speed of copper during electrolytic plating, flatten the surface, and control the excessive increase in carbon content inside the electrodeposited copper foil. Therefore, when the ratio of cobalt, arsenic, and TOC in the electrodeposited copper foil is within the range of the following formula 1, the change in physical properties of the electrodeposited copper foil at low temperatures is minimized.

[0041] Equation 1: TOC / (cobalt + arsenic) = 1.30-1.55 If the ratio of TOC to cobalt and arsenic is less than 1.30, the content of cobalt and arsenic added to the plating solution increases, suppressing the effect of TOC in the plating solution in preventing abnormal grain growth, which is undesirable, and if the ratio exceeds 1.30, the excessive TOC content in the electrodeposited copper foil generates stress in the grains, causing abnormal grain growth in the electrodeposited copper foil after plating, preventing the formation of a crystal structure advantageous for bending resistance. Therefore, in order to improve the bending resistance of the electrodeposited copper foil for secondary batteries, it is preferable that the ratio of cobalt and arsenic to TOC is maintained in the range of 1.30 to 1.55 as shown in the above formula 1.

[0042] If the copper ions and sulfate ions in the plating solution are outside the above ranges, copper foil may not be properly deposited during subsequent electrolytic plating, or the hardness of the copper foil may be reduced.

[0043] In addition, the plating solution contains 10 ppm to 90 ppm of chlorine, and chlorine suppresses crystal growth of CuCl2 precipitates formed at grain boundary interfaces during electrolytic plating when heated to high temperatures, thereby improving thermal stability at high temperatures. If the chlorine concentration is out of the range of 10 ppm to 90 ppm, the tensile strength of the electrolytic copper foil may be reduced, and the thermal stability at high temperatures may be reduced.

[0044] In step (2) (S200), the plating solution prepared in step (1) is electroplated using a drum at a temperature of 30° C. to 70° C. and a current density of 30 ASD (Ampere per Square Decimal) to 150 ASD. FIG. 2 is a diagram showing the steps of manufacturing an electrolytic copper foil using a drum according to an embodiment of the present invention. If the plating temperature and current density are outside the above-mentioned ranges, plating may not be performed normally, the surface of the electrolytic copper foil may not be uniform, or the tensile strength and elongation rate may be reduced, which may cause a deterioration in battery performance.

[0045] Step (3) (S300) includes coating the electrolytic copper foil formed by electrolytic plating with a negative electrode active material, and the electrolytic copper foil coated with the negative electrode active material formed by step (3) (S300) has excellent flex resistance and can be flexed 110 times or more in the MIT flex test.

[0046] The electrolytic copper foil formed by electrolytic plating in step (2) may have one side in contact with the drum and another side opposite to the one side, and the Rz roughness of the one side and the other side may be 2.0 μm or less. If the surface roughness of the one side and the other side of the electrolytic copper foil exceeds 2.0 μm, the adhesive strength between the current collector and the active material is reduced, and the battery performance may be reduced due to the volume change during charging and discharging of the secondary battery, which is undesirable. Therefore, the Rz roughness of the one side and the other side of the electrolytic copper foil is preferably 2.0 μm or less.

[0047] The tensile strength of the electrolytic copper foil for secondary batteries according to the present invention is 30 kgf / mm 2~51kgf / mm 2 It is preferable that the tensile strength is 30 kgf / mm 2 If it is less than 100 kgf / mm, it may be deformed or broken during the press manufacturing process after coating the electrode active material. When the secondary battery is charged and discharged, the volume of the secondary battery expands or contracts as other active materials such as graphite exchange lithium ions. At this time, the active material layer is in close contact with the electrolytic copper foil, so stress is generated due to the expansion or contraction. Therefore, the tensile strength is 30 kgf / mm 2 If the thickness is less than 100 mm, the electrolytic copper foil cannot withstand the stress and is broken, making it impossible to maintain the battery performance, and the breakage may cause deformation, resulting in a short circuit between the anode and the cathode.

[0048] In addition, the elongation rate of the electrolytic copper foil for secondary batteries according to the present invention is preferably 2% to 18%. When the elongation rate of the electrolytic copper foil is high, it has an advantage that it can withstand tension during coating of active materials in the electrode manufacturing process, and can prevent breakage during the process, and can prevent breakage due to stress received during the electrode winding process. In addition, it prevents efficiency reduction and breakage during the charge / discharge cycle of the battery, improving the performance of the battery. However, if the elongation rate exceeds 18%, the secondary battery may be severely deformed and short-circuited during charge / discharge, and if the elongation rate is less than 2%, the electrolytic copper foil may easily break.

[0049] The tensile strength and elongation ratio are inversely proportional to each other, that is, when the tensile strength increases, the elongation ratio decreases, and when the tensile strength decreases, the elongation ratio increases. Therefore, in order to manufacture an electrodeposited copper foil having high tensile strength while preventing breakage, it is important to maintain the tensile strength and elongation ratio within the appropriate range. Therefore, the tensile strength is 30 kgf / mm 2 ~51kgf / mm 2 It is preferable to maintain the stretch ratio in the range of 2% to 18%.

[0050] In addition, the thickness of the electrolytic copper foil for secondary batteries according to the present invention is preferably 4 μm to 10 μm. If the thickness of the electrolytic copper foil is less than 4 μm, the electrolytic copper foil may be easily broken due to its thin thickness, and if the thickness of the electrolytic copper foil is more than 10 μm, the volume and weight of the secondary battery to be manufactured increases, which is not preferable.

[0051] Hereinafter, examples and comparative examples of the present invention will be described. However, the following examples are only preferred examples of the present invention, and the scope of the present invention is not limited to the following examples.

[0052] Experiment 1. Battery life test based on TOC concentration and MIT count Example 1 A plating solution containing 100 g / L copper ions, 110 g / L sulfuric acid, 30 ppm chlorine, 340 ppm TOC, 0.025 g / L cobalt, and 0.045 g / L arsenic (the sum of cobalt and arsenic is 0.775 g / L) was prepared, and electrolytic plating was performed using a drum at 50° C. and a current density of 90 ASD, and the electrolytic copper foil formed by electrolytic plating was coated with a cathode active material.

[0053] (Examples 2 to 8) The plating solution was prepared in the same manner as in Example 1, except that the concentrations of TOC, cobalt and arsenic contained in the plating solution were as shown in Table 3 below.

[0054] (Comparative Examples 1 to 4) In Comparative Examples 1 to 4, electrolytic copper foils were manufactured under the same conditions as in Example 1, except that the concentrations of TOC, cobalt, and arsenic in the plating solution were as shown in Table 3 below.

[0055] The experimental conditions of Examples 1 to 8 and Comparative Examples 1 to 4 were the same as those described above. The room temperature tensile strength and elongation, the number of MIT tests, and the battery life after 300 cycles of each of the electrodeposited copper foils for secondary batteries prepared by the above methods were measured and are shown in Tables 2 and 3 below.

[0056] Tensile strength and elongation were measured by cutting tensile test pieces of 12.7 mm wide x 50 mm long gauge from the electrodeposited copper foils obtained in Examples 1 to 8 and Comparative Examples 1 to 4, and carrying out a tensile test at a crosshead speed of 50.8 mm / min according to the IPC-TM-6502.4.18B standard. The maximum load of the tensile strength was defined as the tensile strength, and the elongation at break was defined as the elongation. The tensile strength and the elongation were all measured at room temperature.

[0057] In addition, the percentage values ​​of TOC, cobalt, and arsenic after dissolving the copper foil were analyzed using inductively coupled plasma mass spectrometry (ICP) after dissolving the electrolytic copper foils obtained from Examples 1 to 8 and Comparative Examples 1 to 4 in 60 ml of hydrochloric acid (35%) and 40 ml of hydrogen peroxide (30%). The percentage values ​​of TOC, cobalt, and arsenic were calculated using Equation 1 above, and the results are shown in Table 3 below.

[0058] The MIT bending test was performed using an MIT bending tester. The bending test involved repeated bending under the following conditions, and the number of bending cycles until the test piece broke was calculated. The results are shown in Table 3. 1) Condition: Original foil 2) Bending radius (R): 0.38mm 3) Bending angle: 135° 4)Bending speed: 175 times / min 5) Load: 500g The battery evaluation conditions were set as follows, and the cell design, anode, cathode, separator, and electrolyte conditions were set as shown in Table 1 below. 1) Constant current charging: current value 1C, charge end voltage 4.2V 2) Rest for 20 minutes 3) Constant current discharge: current value 1C, charge cut-off voltage: 2.5V cut off 4) 1C=487mAh 5) Cycle: 300 cycles, Temperature: 55℃

[0059] [Table 1] JPEG0007572129000002.jpg8997JPEG0007572129000003.jpg118111Referring to Tables 2 and 3, it can be seen that Comparative Example 1 to Comparative Example 4, in which the TOC concentration is less than 100 ppm, all show MIT bending times of less than 90, while it can be seen that Examples 1 to 8, in which the TOC concentration is all 100 ppm or more, all show MIT bending times of 110 or more.When the TOC is contained in the plating solution at 100 ppm or more during the production of electrolytic copper foil, the grain size and crystal structure in the copper foil can be prevented from changing during electrolytic plating, and the tensile strength and bending resistance of the copper foil are improved.

[0060] In addition, in Comparative Examples 1 to 4, in which the TOC / (cobalt + arsenic) ratio is less than 1.30, the MIT bending times are all less than 90, and the battery life is also short after 300 cycles. When the TOC / (cobalt + arsenic) ratio is less than 1.30, the contents of cobalt and arsenic in the metal additives increase, which causes a problem in that the TOC in the plating solution does not prevent abnormal grain growth, and the physical properties of the electrolytic copper foil change significantly at low temperatures.

[0061] In addition, the batteries according to Examples 1 to 8 and Comparative Examples 1 to 4, whose capacities after 300 cycles were confirmed from Table 3, were disassembled to check the state of the electrolytic copper foil (which acted as a negative electrode plate). At this time, it was confirmed that the electrolytic copper foils according to Examples 1 to 8 had no defective appearance and were the same as the original. On the other hand, in the cases of Comparative Examples 1 to 4, it was confirmed that not only was the life of the battery reduced, but also that a part of the electrolytic copper foil was broken or peeled off, and in the case of Comparative Example 1, it was confirmed that there was a part where the negative electrode active material was peeled off from the electrolytic copper foil, and in Comparative Examples 2 and 4, it was confirmed that a broken part was formed on the outer part of the electrolytic copper foil.

[0062] Those skilled in the art will understand that the present invention can be implemented in other specific forms without changing its technical idea or essential features. Therefore, it should be understood that the above-described embodiments are illustrative in all respects and not limiting. The scope of the present invention is indicated by the claims below rather than the above detailed description, and all modifications or alterations derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

Claims

1. An electrolytic copper foil for a secondary battery, comprising TOC (total organic carbon), cobalt, and arsenic, and coated with a negative electrode active material, The ratio of TOC, cobalt, and arsenic contained in the electrolytic copper foil measured after dissolving the electrolytic copper foil was calculated based on the following formula 1: Equation 1: TOC / (cobalt + arsenic)=1.30-1.55 (In the formula, the TOC, cobalt, and arsenic are in mass ratios.) An electrolytic copper foil for a secondary battery according to the present invention, The TOC, cobalt and arsenic are derived from the plating solution, The electrolytic copper foil for a secondary battery contains the TOC of 100 ppm or more, the cobalt of 1 mg / L to 50 mg / L, and the arsenic of 10 mg / L to 80 mg / L.

2. The electrolytic copper foil has a bending resistance of 110 or more times in an MIT bending test. The electrolytic copper foil for a secondary battery according to claim 1.

3. The electrolytic copper foil has one side that is in direct contact with the drum and another side that is opposite to the one side, The Rz roughness of the one surface and the other surface is 2.0 μm or less. The electrolytic copper foil for a secondary battery according to claim 1.

4. The tensile strength of the electrolytic copper foil is 30 kgf / mm 2 ~51kgf / mm 2 That is, The electrolytic copper foil for a secondary battery according to claim 1.

5. The elongation rate of the electrolytic copper foil is 2% to 15%. The electrolytic copper foil for a secondary battery according to claim 1.