Multilayer film for use in flexible packaging materials

A multilayer polyethylene film structure addresses the challenge of maintaining optical properties and sustainability in flexible packaging by using a single-material composition without adhesives, achieving high gloss and stiffness.

JP7572349B2Active Publication Date: 2024-10-23DOW GLOBAL TECHNOLOGIES LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021504269
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-29
Filing Date
2019-08-22
Publication Date
2024-10-23
Estimated Expiration
2039-08-22

AI Technical Summary

Technical Problem

Conventional flexible packaging materials face challenges in achieving sustainability, recyclability, and maintaining optical properties due to the use of multiple polymer groups and adhesives, which create a trade-off in recyclability and optical performance.

Method used

A multilayer polyethylene film structure comprising a first layer with a density of 0.935-0.965 g/cc and a melt index of 0.3-2.0, and a second layer with a polyolefin plastomer density of 0.885-0.910 g/cc and a melt index of 4.0-20.0, without the use of adhesives, to achieve high gloss and stiffness.

Benefits of technology

The multilayer film maintains desired optical properties like gloss and stiffness while improving sustainability by using a single-material polyethylene composition, enhancing recyclability and reducing the need for adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572349000001
    Figure 0007572349000001
  • Figure 0007572349000002
    Figure 0007572349000002
  • Figure 0007572349000003
    Figure 0007572349000003
Patent Text Reader

Abstract

The multilayer film includes a first film having at least a first layer and a second layer, and a second film extrusion coated onto the first layer of the first film. The multilayer film does not include an adhesive. The first layer of the first film includes a first high-density polyethylene (HDPE) having a density of 0.935-0.965 g / cc and a melt index I2 of 0.3-2.0, and the second layer of the first film includes a polyolefin plastomer having a density of 0.885-0.910 g / cc. The second film includes a second high-density polyethylene (HDPE) having a density of 0.945-0.965 g / cc and a melt index I2 of 4.0-20.0. The second film has a gloss of 65%-95% at 60° according to ASTM D2457. [Selection diagram] None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of European Patent Application No. 18382630.4, filed August 29, 2018, which is incorporated herein by reference in its entirety.

[0002] The embodiments described herein relate generally to multilayer films for use in flexible packaging, and more specifically to adhesive-free multilayer films in which a polyethylene film is extrusion coated onto a second polyethylene film for use in flexible packaging. [Background technology]

[0003] Improving sustainability is an ongoing goal for manufacturers of flexible packaging. Flexible packaging materials, such as flexible pouches, are more easily recyclable when made from one polymer family, and mono-polymer packaging materials are being considered to achieve this goal.

[0004] Conventional flexible packaging materials include polymer substrates that use many polymer families, such as polyester (PET) as printing film and polyethylene (PE) for sealant film. Products that may require further improvement in barrier properties may include additional layers of aluminum foil, metallized film, or barrier resin. Conventional flexible packaging materials also include adhesives that may make recyclability difficult.

[0005] Furthermore, while maintaining or improving optical properties is a continuing goal for flexible packaging, tradeoffs in optical properties arise, particularly when moving to single-material packaging materials without the use of adhesives. Thus, a need exists for single-material polyethylene materials that maintain the desired optical properties while improving sustainability. Summary of the Invention

[0006] Various embodiments of the present disclosure are directed to polyethylene film constructions that meet these needs and achieve the desired sustainability, strength, and optical properties such as gloss without the use of adhesives.

[0007] According to at least one embodiment of the present disclosure, a multilayer film is provided. The multilayer film includes a first film including at least a first layer and a second layer, and a second film extrusion coated on the first layer of the first film, the multilayer film being adhesive-free. The first layer of the first film includes a first high density polyethylene (HDPE) having a density of 0.935-0.965 g / cc and a melt index I2 of 0.3-2.0, and the second layer of the first film includes a polyolefin plastomer having a density of 0.885-0.910 g / cc. The second film includes a second high density polyethylene (HDPE) having a density of 0.945-0.965 g / cc and a melt index I2 of 4.0-20.0. The second film has a gloss of 65%-95% at 60° according to ASTM D2457.

[0008] These and other embodiments are described in greater detail in the detailed description that follows. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Specific embodiments of the present application will now be described. However, the present disclosure may be embodied in different forms and should not be construed as being limited to the embodiments set forth in this disclosure. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present subject matter to those skilled in the art.

[0010] The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether the monomers are the same or different. Thus, the generic term polymer encompasses the term "homopolymer", which is commonly used to refer to a polymer prepared from only one type of monomer, as well as the term "copolymer", which refers to a polymer prepared from two or more different types of monomers. As used herein, the term "interpolymer" refers to a polymer prepared by polymerization of at least two different types of monomers. Thus, the generic term interpolymer includes copolymers and polymers prepared from three or more different types of monomers, such as terpolymers.

[0011] "Polyethylene" or "ethylene-based polymer" is intended to mean a polymer containing greater than 50 mole percent of units derived from ethylene monomers. This includes polyethylene homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of polyethylene known in the art include low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene (m-LLDPE) which includes both linear and substantially linear low density resins, medium density polyethylene (MDPE), and high density polyethylene (HDPE).

[0012] The term "ULDPE" is defined as a polyethylene-based copolymer having a density in the range of 0.895 to 0.915 g / cc.

[0013] The term "LDPE" may also be referred to as "high pressure ethylene polymer", or "highly branched polyethylene", and is defined to mean that the polymer is partially or fully homopolymerized or copolymerized in an autoclave or tubular reactor at pressures above 14,500 psi (100 MPa) using a free radical initiator such as peroxide (see, for example, U.S. Pat. No. 4,599,392, incorporated herein by reference). LDPE resins typically have a density in the range of 0.916 to 0.940 g / cc.

[0014] The term "LLDPE" includes both conventional Ziegler-Natta catalyst systems as well as resins made using single-site catalysts such as metallocenes (sometimes referred to as "m-LLDPE"). LLDPE contains less long chain branches than LDPE and includes substantially linear ethylene polymers as further defined in U.S. Pat. Nos. 5,272,236, 5,278,272, 5,582,923, and 5,733,155; homogeneous branched linear ethylene polymer compositions such as those prepared according to the process disclosed in U.S. Pat. No. 3,645,992; heterogeneous branched ethylene polymers such as those prepared according to the process disclosed in U.S. Pat. No. 4,076,698; and / or blends thereof (such as those disclosed in U.S. Pat. No. 3,914,342 or U.S. Pat. No. 5,854,045). Linear PE can be made via gas phase, liquid phase, or slurry polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art, including, but not limited to, gas phase and liquid phase reactors.

[0015] The term "HDPE" refers to polyethylene having a density greater than about 0.940 g / cc, and is generally prepared with Ziegler-Natta, chromium, or even metallocene catalysts.

[0016] As used herein, the term "propylene-based polymer" refers to a polymer that, in polymerized form, contains a majority amount of propylene monomer (based on the total weight of the polymer) and may optionally contain at least one polymerized comonomer.

[0017] The term "flexible packaging" or "flexible packaging material" encompasses a variety of non-rigid containers familiar to those skilled in the art. These can include pouches, stand-up pouches, pillow pouches, bulk bags, prefabricated packaging, and the like.

[0018] As used herein, the term "single material" means that the multilayer film consists essentially of polyethylene, where "substantially" means at least 95% by weight polyethylene, or at least 99% by weight polyethylene, or at least 99.5% by weight polyethylene, or at least 99.9% by weight, or 100% by weight polyethylene, based on the total moles of the multilayer film.

[0019] As used herein, the term "printed film" refers to the outer film of a multilayer film, which is the film on which printing is performed in the manufacture of flexible packaging. In some embodiments, the term "outer" should not be interpreted as the outermost layer, as additional layers disposed externally on the printed film are contemplated, such as a printed primer layer, a barrier layer, an overprint varnish layer, or other layers known to those skilled in the art of flexible packaging.

[0020] As used herein, the term "sealant film" refers to the inner film of a multi-layer film that includes a sealant layer disposed internally relative to the print film. In some embodiments, the sealant film is a single layer film, while in other embodiments, the sealant film includes multiple layers, one of which is a sealant layer. In embodiments in which the sealant film includes multiple layers, the sealant film may include one or more additional layers, such as a barrier layer, a structural layer, etc., disposed internally between the layer that contacts the extrusion coating and the sealant layer.

[0021] As used herein, "extrusion coating" refers to an extrusion coating layer of a multi-layer film disposed on a sealant film. In some embodiments, the extrusion coating is a print protective film. In other embodiments, a print can be applied to the outside of the extrusion coating after the extrusion coating is applied to the sealant film.

[0022] As used herein, "adhesive" refers to a polyurethane or acrylic based liquid adhesive that is applied between two film surfaces, for example, between an extrusion coating and a sealant film, and then undergoes curing to bond the two film surfaces together.

[0023] Reference will now be made in detail to various multilayer film embodiments of the present disclosure, particularly those used in articles such as flexible packaging materials. In one embodiment, the multilayer film comprises a first film including at least a first layer and a second layer, and a second film extrusion coated onto the first layer of the first film, where the multilayer film does not include an adhesive. The first layer of the first film comprises a first high density polyethylene (HDPE) having a density of 0.935-0.965 g / cc and a melt index I2 of 0.3-2.0, and the second layer of the first film comprises a polyolefin plastomer having a density of 0.885-0.910 g / cc. The second film comprises a second high density polyethylene (HDPE) having a density of 0.945-0.965 g / cc and a melt index I2 of 4.0-20.0. The second film has a gloss at 60° of 65% to 95% according to ASTM D2457.

[0024] Sealant Film

[0025] In one or more embodiments, the first film is a sealant film that includes at least a first layer and a second layer. In some embodiments, the sealant film includes at least three layers, specifically, a middle layer, an inner layer disposed between the second film and the middle layer, and an outer layer. The sealant film may include or consist of an ethylene-based polymer layer.

[0026] In various embodiments, the first layer of the sealant film is an ink layer and a print layer that undergoes extrusion coating. The first layer may include a polyethylene composition that provides stiffness and resists gelation during cast film or blown film extrusion processes. In one embodiment, the first layer includes at least 70 wt.% high density polyethylene (HDPE) having a density of 0.935-0.965 g / cc and a melt index (I2) of 0.3-2.0 g / 10 min, where I2 is measured at 190° C. and 2.16 kg load according to ASTM D1238.

[0027] Various methodologies are contemplated for producing polyethylene copolymers, HDPE, which are produced from the polymerization of ethylene and one or more α-olefin comonomers in the presence of one or more catalysts, such as Ziegler-Natta catalysts, Phillips catalysts, metallocene catalysts, post-metallocene catalysts, constrained geometry complex (CGC) catalysts, or biphenylphenol (BPP) complex catalysts. The α-olefin comonomers range from C3 to C 12 The olefin monomer may include, in one embodiment, the α-olefin comonomer in the HDPE is 1-octene.

[0028] In further embodiments, the first layer of the sealant film may comprise at least 95% by weight HDPE, or at least 99% by weight HDPE, or 100% by weight HDPE. Without being limited by theory, the HDPE of the first layer provides the multilayer film with stiffness to withstand the stretching of high speed printing processes. Additionally, the HDPE of the sealant film may have a density of 0.935-0.965 g / cc or 0.940-0.965 g / cc. In further embodiments, the melt index (I2) may be 0.3-4.0 g / 10 min, or 0.3-3.0 g / 10 min, or 0.3-2.0 g / 10 min, or 0.3-1.5 g / 10 min, or 0.5-1.0 g / 10 min. Various commercially available products are believed to be suitable, such as ELITE™ 5960G, ELITE™ 5940ST, DOWLEX™ 2740G from The Dow Chemical Company (Midland, MI), or other HDPE products having suitable density and melt index I2. Other suitable HDPEs include those described in PCT Publication No. WO2017 / 099915, which is incorporated herein by reference in its entirety.

[0029] The sealant film further comprises a second layer comprising a low density polyolefin plastomer which functions as a low temperature sealing layer. In various embodiments, the polyolefin plastomer can be a polyethylene plastomer or a polypropylene plastomer. The polyolefin plastomer can include resins made using single site catalysts such as metallocenes and constrained geometry catalysts. The polyolefin plastomer has a viscosity of 0.885 to 0.910 g / cm. 3 It has a density of 0.885g / cm 3 ~0.910g / cm 3 All individual values ​​and subranges are included herein and disclosed herein, for example, the density of a polyolefin plastomer may be 0.895, 0.900, or 0.905 g / cm 3from the lower limit of 0.905, 0.910, or 0.915 g / cm 3 In some embodiments, the polyolefin plastomer has a viscosity of 0.885 to 0.907 g / cm 3 or 0.885~0.902g / cm 3 has a density of

[0030] In some embodiments, the polyolefin plastomer has a melt index (I2) of up to 20 g / 10 min. All individual values ​​and subranges up to 20 g / 10 min are included herein and disclosed herein. For example, the polyolefin plastomer may have an upper melt index of 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 g / 10 min. In certain aspects of the present invention, the polyolefin plastomer has a lower I2 limit of 0.5 g / 10 min. One factor in specifying the melt index of the polyolefin plastomer is whether the second layer is produced as a blown film or a cast film.

[0031] Examples of polyolefin plastomers that can be used in the second layer include those commercially available from The Dow Chemical Company under the name AFFINITY™, including, for example, AFFINITY™ PL1881G and AFFINITY™ PF1140G.

[0032] In some embodiments, the sealant film may include additional layers between the first layer and the second layer. For example, in embodiments, the sealant film may include a third layer comprising one or more ethylene-based polymers. The third layer may include HDPE, LDPE, a combination of HDPE and LDPE, and the like. In some embodiments, the sealant film may include three additional layers between the first layer and the second layer, two of which are tie layers that bond the barrier layer (e.g., EVOH layer) to the first layer and the second layer. Although additional layers are contemplated, it should be understood that such additional layers are optional in some embodiments.

[0033] Extrusion Coating

[0034] In various embodiments, the second film, sometimes referred to herein as extrusion coating layer or extrusion coating film, is extrusion coated onto the first layer of the first film. The second film, which may be considered a print protection film in some embodiments, provides aesthetic benefits (e.g., gloss and transparency) to the multilayer film. In one or more embodiments, the second film may enable the multilayer film to achieve a gloss value of at least 65%, where gloss is measured at 60° according to ASTM D2457.

[0035] The second film comprises a second high density polyethylene (HDPE) having a density of 0.945 g / cc to 0.965 g / cc and a melt index I2 of 4.0 to 20.0 g / 10 min, where I2 is measured at 190° C. and 2.16 kg load according to ASTM D1238. As noted above, various methodologies are contemplated for producing the HDPE of the second film.

[0036] In various embodiments, the second film includes an inner layer and an outer layer that may have the same or different formulations. In one or more embodiments, the inner layer is in contact with the first layer of the sealant film. In some embodiments, the outer layer includes the second HDPE. In one or more embodiments, the outer layer includes or consists of 100% by weight of the second HDPE. However, in other embodiments, the outer layer may include the second HDPE and LDPE or other polyethylene-based polymers. In such embodiments, the outer layer may include 50% to 99%, 55% to 95%, 60% to 90%, 65% to 85%, or 75% to 95% by weight of the second HDPE. In embodiments, the inner layer has a thickness of 5 μm to 10 μm or 7 μm to 9 μm. The outer layer may have a thickness of 1 μm to 5 μm or 2 μm to 4 μm. The thickness of the second film may vary depending on the particular embodiment. However, in various embodiments, the second film may be 9 g / m 2 ~20g / m 2 , 10g / m 2 ~18g / m 2 , or 11 g / m 2 ~15g / m 2 In some embodiments, the second film has a coat weight of 12 g / m 2 Such a coat weight allows the second film to protect the ink while maintaining good transparency.

[0037] The inner layer of various embodiments includes HDPE and low density polyethylene (LDPE). The HDPE of the inner layer has a density of 0.935-0.965 g / cc or 0.940-0.965 g / cc. In further embodiments, the melt index (I2) can be 4.0-15.0 g / 10 min or 5.0-15.0 g / 10 min. The HDPE and LDPE of the inner layer can be blended together to form the inner layer, or the HDPE and LDPE can be coextruded to form the inner layer.

[0038] In one or more embodiments, the LDPE of the inner layer of the second film can have a density of 0.915 to 0.930 g / cc or 0.915 g / cc to 0.925 g / cc. Further, the melt index (I2) of the LDPE can be 1.0 to 15.0 g / 10 min, or 1.0 to 10.0 g / 10 min, or 2.5 to 10.0 g / 10 min.

[0039] In one or more embodiments, the LDPE composition may include an antiblocking agent, a slip agent, or both. Various commercially available LDPE products are believed to be suitable for the inner layer of the second film, such as AGILITY™ EC7000, AGILITY™ EC7220, DOW™ LDPE7008, and DOW™ LDPE7004, all of which are available from The Dow Chemical Company (Midland, MI).

[0040] In embodiments in which the second film comprises LDPE, the second film may comprise up to 30% by weight LDPE or up to 25% by weight LDPE. In one embodiment, the inner layer may comprise 5-30% by weight LDPE. In a further embodiment, the inner layer may comprise 5-25% by weight LDPE. In yet another embodiment, the inner layer may comprise 5-10% by weight LDPE. In an embodiment, the LDPE may improve optical properties such as gloss and clarity while also improving processability for extrusion coating.

[0041] Although described in various embodiments as a multi-layer film (e.g., including outer and inner layers), in embodiments the extrusion coating may be a monolayer film. For example, HDPE and LDPE may be blended together to form a single layer rather than being co-extruded as multiple layers.

[0042] In various embodiments described herein, the second film has a gloss value at 60° of 65% to 95% according to ASTM D2457. In some specific embodiments, the second film has a gloss value of 70% to 90% or 80% to 85%.

[0043] The second film may further have a melting point (highest differential scanning calorimetry (DSC) melting peak temperature) of 110°C to 135°C.

[0044] In addition to the components of the sealant film and extrusion coating film described above, other polymer additives such as UV absorbers, antistatic agents, pigments, dyes, nucleating agents, fillers, slip agents, flame retardants, plasticizers, processing aids, lubricants, stabilizers, smoke suppressants, viscosity modifiers and antiblocking agents may be included. In certain embodiments, slip agents, antiblocking agents, or both are included with one or more of the polymers of the sealant film and / or extrusion coating film. However, in various embodiments, the multilayer film comprises more than 95 wt% ethylene-based polymer based on the total weight of the multilayer film. In some embodiments, the multilayer film comprises more than 98 wt% ethylene-based polymer based on the total weight of the multilayer film, or even more than 99 wt% ethylene-based polymer based on the total weight of the multilayer film.

[0045] Although the above discussion focuses on multilayer films with a total thickness of less than 150 μm, various additional thicknesses and layer configurations are also suitable. For example, it is contemplated that the multilayer film may include more than the first and second layers previously described herein. For example, the multilayer film may include an ink layer between the first and second films. The ink layer may be in the form of, for example, an image or words. In such an embodiment, the ink layer may be printed on the first film and the second layer may be extruded onto the ink layer, as described in more detail below.

[0046] As noted above, the multilayer film is endowed with a unique combination of high gloss and high stiffness without the use of adhesives. In one embodiment, the multilayer film has a stiffness of 0.014 N / mm, as measured according to ASTM D747, for multilayer films having a thickness of less than 150 μm. 2 The material may have an apparent flexural modulus of greater than 0.1.

[0047] Method for manufacturing flexible packaging

[0048] Various methodologies are contemplated for producing the sealant films and extrusion coated films. For example, multi-layer sealant films can be prepared by cast film extrusion or blown film extrusion. Multi-layer extrusion coated films can be prepared by flat die film extrusion.

[0049] After the sealant film is blown or cast, it can be subjected to a printing process. Various printing processes are believed to be suitable for cast or blown printing films. These printing processes include, but are not limited to, rotogravure, flexography, and offset printing. In certain embodiments, the sealant film can be subjected to rotogravure printing. In certain embodiments, the sealant film is printed in reverse rotogravure at the printing speed typically utilized for conventional PET / PE laminates. The tension between the rollers of a rotogravure press can cause conventional films to overstretch, resulting in poor print registration. Without being bound by theory, it is believed that the sealant film has the necessary stiffness to prevent overstretching and thereby achieve the desired print performance. In one or more embodiments, the sealant film can stretch less than 2 mm in a rotogravure press, whereas conventional polyethylene printing films can stretch about 6 mm.

[0050] In other embodiments, an extrusion coating film may be coated directly onto the sealant film and the multilayer film is subjected to a printing process such that the print is applied onto the extrusion coating film. However, in such embodiments, the extrusion coating film may not provide protection to the ink layer.

[0051] Alternatively, various additional processes may be used to produce flexible packaging from the laminate structure. These may include heat sealing or other processes well known to those skilled in the art.

[0052] Test Method The test methods include the following:

[0053] Melt Index (I2) The melt index (I2) was measured at 190° C. and 2.16 kg according to ASTM D-1238. 10 ) was measured at 190° C., 10 kg according to ASTM D-1238. Values ​​are reported in g / 10 min, which corresponds to grams dissolved per 10 minutes.

[0054] density Samples for density measurements were prepared according to ASTM D4703 and measured in grams per cubic centimeter (g / cc or g / cm 3 ) Measurements were performed within 1 hour of specimen compression using ASTM D792, Method B.

[0055] Glossiness Gloss was measured at 60° according to the method of ASTM D2457, and the reported value is the average of the gloss measured for five samples.

[0056] Melting point Differential scanning calorimetry (DSC) is used to measure the melting and crystallization behavior of polymers over a wide range of temperatures. For example, a TA Instruments Q1000 DSC equipped with an RCS (refrigerated cooling system) and an autosampler is used to perform this analysis. The instrument is first calibrated using the software calibration wizard. A baseline is obtained by heating the cell from -80°C to 280°C without any sample in the aluminum DSC pan. A sapphire standard is then used as instructed by the calibration wizard. Next, 1-2 milligrams (mg) of fresh indium sample is analyzed by heating the standard sample to 180°C, cooling it to 120°C at a cooling rate of 10°C / min, and then holding the standard sample isothermal at 120°C for 1 minute. The standard sample is then heated from 120°C to 180°C at a heating rate of 10°C / min. The indium standard is then determined to have a heat of fusion (Hf) = 28.71 ± 0.50 Joules per gram (J / g), and an onset of melting = 156.6 ° C. ± 0.5 ° C. The test sample is then analyzed with a DSC instrument.

[0057] A nitrogen purge gas flow rate of 50 ml / min is used during testing. Each sample is melt pressed into a thin film at approximately 175°C, and then the molten sample is air cooled to room temperature (approximately 25°C). Film samples are formed by pressing 0.1-0.2 grams of sample at 175°C, 1,500 psi, and 30 seconds to form a 0.1-0.2 mil thick film. A 3-10 mg, 6 mm diameter specimen is extracted from the cooled polymer, weighed, placed in a light aluminum pan (approximately 50 mg), and crimped shut. Analysis is then performed to determine its thermal properties.

[0058] The thermal behavior of the sample is determined by ramping the sample temperature to generate a heat flow vs. temperature profile. First, the sample is rapidly heated to 180°C to remove its thermal history and held isothermal for 5 minutes. Next, the sample is cooled to -40°C at a cooling rate of 10°C / min and held isothermal at -40°C for 5 minutes. The sample is then heated to 150°C (this is the "second heat" gradient) at a heating rate of 10°C / min. The cooling and second heating curves are recorded. The cooling curve is analyzed by setting a baseline end point from the onset of crystallization to -20°C. The heat curve is analyzed by setting a baseline end point from -20°C to the melting end point. The determined value is the peak melting temperature (T m ), peak crystallization temperature (T c ), onset crystallization temperature (Tc onset), heat of fusion (H f ) (grams per joule), and the % crystallinity calculated for the polyethylene samples using % crystallinity PE = ((Hf) / (292 J / g)) x 100, and the % crystallinity calculated for the polypropylene samples using % crystallinity PP = ((Hf) / 165 J / g)) x 100. f ) and peak melt temperature are reported from the second heat curve. The peak crystallization temperature and onset crystallization temperature are determined from the cooling curve.

[0059] Oxygen permeability Oxygen transmission rate is measured according to ASTM D3985 at 23° C. and 75% RH.

[0060] Water Vapor Transmission Rate Water vapor transmission rate is measured at 38° C. and 90% RH according to ASTM E-398.

[0061] Apparent bending modulus Apparent flexural modulus is measured in accordance with ASTM D747. EXAMPLES

[0062] The following examples are illustrative of the features of the present disclosure and are not intended to limit the scope of the present disclosure. All parts and percentages are by weight unless otherwise indicated. Approximate properties, characteristics, parameters, etc. are provided below for various examples, comparative examples, and materials used in the examples and comparative examples. In addition, the description of the raw materials used in the examples is as follows:

[0063] HDPE1 is 0.950g / cm 3 and a melt index (I2) of 1.5 g / 10 min, prepared as described for Resin 1 of the invention in WO 2017 / 099915.

[0064] POLYBATCH® AMF705HF is a processing aid available from A. Schulman.

[0065] POLYBATCH® VLA55 is an antistatic additive available from A. Schulman.

[0066] POLYBATCH® NG8160 is an additive available from A. Schulman.

[0067] AFFINITY™ 1881G is an ethylene / octene plastomer available from The Dow Chemical Company (Midland, MI).

[0068] DOW™ LDPE310E is an LDPE available from The Dow Chemical Company (Midland, MI).

[0069] ADCOTE™ L719A is a solvent-based polyurethane adhesive available from The Dow Chemical Company (Midland, MI).

[0070] MORFREE™ LPLUS 1 is a solvent-free adhesive available from The Dow Chemical Company (Midland, MI).

[0071] In the following experiments, a multilayer film according to the present disclosure (Example 1) was compared to a conventional PET / PE laminate having a conventional PE film adhered to a conventional PE printed film (Comparative Example 1), a PE / PE laminate having a conventional PE film adhered to a conventional PE printed film (Comparative Example 2), and a lacquer coated conventional PET printed film (Comparative Example 3). Table 1 lists the compositions of these multilayer films investigated herein as follows:

[0072] In the case of Example 1, Comparative Example 2, and Comparative Example 3, the sealant layer includes three layers, A, B, and C, where layer C is a low-temperature sealing layer. Layer A includes 98.5% HDPE1, 1% POLYBATCH AMF705HF, and 0.5% POLYBATCH VLA55. Layer B includes 84% ​​HDPE1 and 16% POLYBATCH NG8160. Layer C includes 84% ​​AFFINITY 1881G, 14.5% LDPE 310E, 1% POLYBATCH AMF705HF, and 0.5% POLYBATCH VLA55. The sealant layer of Comparative Example 1 is a film including a low-temperature sealing layer and a layer including LLDPE and / or LDPE. The lacquer of Comparative Example 3 is a commercial lacquer for providing heat resistance.

[0073] [Table 1]

[0074] For Example 1, the extrusion coating was 20% by weight of AGILITY™ EC7220 (0.918 g / cm as measured according to ASTM D792). 3and a melt index I2 of 1.5 g / 10 min as measured at 190° C. and 2.16 kg according to ASTM D1238) and DOWLEX™ 2006 (0.961 g / cm3 as measured according to ASTM D792). 3 and a melt index I2 of 8.0 g / 10 min measured at 190° C. and 2.16 kg according to ASTM D1238).

[0075] Synthesis of multilayer films

[0076] The film extrusion process used to make the multilayer films in Table 1 was carried out on a blown film line in Kaschier, Germany, which had the following properties as set forth in Table 2 below.

[0077] [Table 2]

[0078] Table 3 shows the temperature profile of the blown film line, i.e., the temperatures at various locations in the blown film line.

[0079] [Table 3]

[0080] For Example 1, an extrusion coating having the composition listed in Table 1 was applied to a blown film using the following conditions: SML extrusion coating line; coating melt temperature 309°C; air gap 280 mm; chill roll temperature -16 to 18°C.

[0081] Experimental Results

[0082] In this experiment, the gloss, oxygen transmission rate (OTR), water vapor transmission rate (WVTR), and stiffness were measured for Example 1 and Comparative Examples 1 to 3. The results are shown in Table 4 as follows.

[0083] [Table 4]

[0084] As shown by the data in Table 4, Example 1, which includes an extrusion coating, exhibits improved gloss at 60° compared to Comparative Examples 2 and 3, while maintaining similar OTR or WVTR. The extrusion coating also exhibits similar apparent flexural modulus as each of the comparative examples.

[0085] Thus, various embodiments described herein provide multi-layer polyethylene film structures that achieve desirable durability, strength, and optical properties such as gloss without the use of adhesives.

[0086] It will be apparent that modifications and variations are possible without departing from the scope of the present disclosure, as defined in the appended claims. More specifically, although certain aspects of the present disclosure are identified herein as preferred or particularly advantageous, it is not intended that the present disclosure be necessarily limited to those aspects.

[0087] In claims and drawing combinations using the singular, it will be apparent that the plural possibilities are also included. For example, a reference to an oil barrier layer implicitly includes a reference to at least one oil barrier layer as well. The present application also relates to the following aspects: (1) A first film including at least a first layer and a second layer, The first layer has a density of 0.935 to 0.965 g / cc and a melt index I of 0.3 to 2.0 g / 10 min. 2 A first high density polyethylene (HDPE) having I 2 is measured according to ASTM D1238 at 190°C and a load of 2.16 kg; and A first film, the second layer comprising a polyolefin plastomer having a density of 0.885 to 0.910 g / cc; A second film extrusion coated onto the first layer of the first film, the second film having a density of 0.945 to 0.965 g / cc and a melt index I of 4.0 to 20.0 g / 10 min. 2 and a second film comprising a second high density polyethylene (HDPE) having the multilayer film does not contain an adhesive; and The second film has a gloss at 60° of 65% to 95% according to ASTM D2457. (2) The second film is an inner layer comprising a blend of low density polyethylene (LDPE) having a density of 0.915 to 0.930 g / cc and high density polyethylene (HDPE) having a density of 0.935 to 0.965 g / cc; A multilayer film as described in (1) above, comprising a second outer layer comprising HDPE. (3) The multilayer film described in (2) above, wherein the outer layer contains 100% by weight of the second HDPE. (4) The multilayer film according to any one of (1) to (3) above, wherein the second film contains 30% by weight or less of low-density polyethylene (LDPE) having a density of 0.915 to 0.930 g / cc. (5) The multilayer film according to any one of (1) to (4) above, wherein the multilayer film contains more than 95% by weight of an ethylene-based polymer, based on the total weight of the multilayer film. (6) The multilayer film according to any one of (1) to (5) above, wherein the multilayer film contains more than 98% by weight of an ethylene-based polymer, based on the total weight of the multilayer film. (7) The multilayer film according to any one of (1) to (6) above, wherein the multilayer film has a total thickness of less than 150 μm and a bending stiffness, measured according to ASTM D790, of more than 0.014 Nmm. (8) Extrusion coating: 9 g / m 2 ~20g / m 2 The multilayer film according to any one of the above (1) to (7), having a coat weight of (9) The multilayer film according to any one of (1) to (8) above, wherein the extrusion coated film has a maximum differential scanning calorimetry (DSC) melting peak temperature of 110°C to 135°C. (10) The multilayer film according to any one of (1) to (9) above, further comprising an ink layer between the first film and the second film. (11) An article comprising the multilayer film according to any one of (1) to (10) above, wherein the article is a flexible packaging material. (12) The article according to (11) above, wherein the flexible packaging material is a stand-up pouch.

Claims

1. A first film comprising at least a first layer and a second layer, The first layer has a density of 0.935 to 0.965 g / cc and a melt index I of 0.3 to 2.0 g / 10 min. 2 A first high density polyethylene (HDPE) having I 2 is measured according to ASTM D1238 at 190° C. and a load of 2.16 kg; and a first film, the second layer comprising a polyolefin plastomer having a density of 0.885 to 0.910 g / cc; A second film extrusion coated onto the first layer of the first film, the second film having a density of 0.945 to 0.965 g / cc and a melt index I of 4.0 to 20.0 g / 10 min. 2 and a second film comprising a second high density polyethylene (HDPE) having the multilayer film does not contain an adhesive; and 1. A multilayer film, wherein the second film has a gloss at 60° of 65% to 95% according to ASTM D2457, and the second film comprises up to 30% by weight of low density polyethylene (LDPE) having a density of 0.915 to 0.930 g / cc.

2. The second film comprises: an inner layer comprising a blend of a low density polyethylene (LDPE) having a density of 0.915 to 0.930 g / cc and a high density polyethylene (HDPE) having a density of 0.935 to 0.965 g / cc; and a second outer layer comprising HDPE.

3. 3. The multilayer film of claim 2, wherein the outer layer comprises 100% by weight of the second HDPE.

4. The multilayer film of any of claims 1 to 3, wherein the multilayer film comprises greater than 95 weight percent ethylene-based polymer, based on the total weight of the multilayer film.

5. The multilayer film of any of claims 1 to 4, wherein the multilayer film comprises greater than 98 weight percent ethylene-based polymer, based on the total weight of the multilayer film.

6. 6. The multilayer film according to any one of claims 1 to 5, wherein the multilayer film has a total thickness of less than 150 μm and a bending stiffness, measured according to ASTM D790, of more than 0.014 Nmm.

7. Extrusion coating: 9 g / m 2 ~20g / m 2 The multilayer film of any one of claims 1 to 6, having a coat weight of

8. The multilayer film according to any one of claims 1 to 7, wherein the extrusion coated film has a maximum differential scanning calorimetry (DSC) melting peak temperature of 110°C to 135°C.

9. The multilayer film of any one of claims 1 to 8, further comprising an ink layer between the first film and the second film.

10. The multilayer film of any of claims 1 to 9, wherein the second film comprises an inner layer and an outer layer, the outer layer comprising 65% to 100% by weight of the second HDPE.

11. The multilayer film of any of claims 1 to 10, wherein the second film comprises 5% to 30% by weight of low density polyethylene (LDPE) having a density of 0.915 to 0.930 g / cc.

12. 12. The multilayer film of claim 1, wherein the second film comprises an inner layer and an outer layer, and the inner layer of the second film comprises 5% to 30% by weight of low density polyethylene (LDPE) having a density of 0.915 to 0.930 g / cc.

13. An article comprising the multilayer film of any one of claims 1 to 12, wherein the article is a flexible packaging material.

14. The article of claim 13 , wherein the flexible packaging material is a stand-up pouch.

Citation Information

Patent Citations

  • Low density polyethylene film, polyethylene mixture, and its film

    JP1998237192A

  • Inflation multilayered film

    JP1999058635A

  • Extrusion-laminated laminate

    JP2006272587A

  • Laminated structure and stand-up pouch produced therefrom

    JP2018511504A

  • Coated film and packages formed therefrom

    JP2018522757A