Method for producing water-decomposable cleaning article and method for modifying fibers

By dispersing and drying cellulose fibers from waste paper multiple times to reduce fibrillarity and using a water-soluble binder, the challenge of achieving high wet strength and water-disintegrability in cleaning products is addressed, resulting in an environmentally friendly and effective cleaning article.

JP7572387B2Active Publication Date: 2024-10-23KAO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022020889
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-02-14
Publication Date
2024-10-23
Estimated Expiration
2042-02-14

AI Technical Summary

Technical Problem

Cellulose fibers derived from waste paper have different physical properties from virgin pulp, making it challenging to achieve both high wet strength and water-disintegrability in water-disintegratable cleaning products.

Method used

A manufacturing process involving dispersing cellulose fibers from waste paper in water, heating, and drying them multiple times to reduce fibrillarity and improve surface smoothness, followed by forming a fiber sheet with a water-soluble binder to create a water-disintegratable cleaning article.

Benefits of technology

The process results in a water-disintegratable cleaning article with sufficient wet strength and water-disintegrability, using environmentally friendly waste paper as a raw material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572387000003
    Figure 0007572387000003
  • Figure 0007572387000001
    Figure 0007572387000001
  • Figure 0007572387000002
    Figure 0007572387000002
Patent Text Reader

Abstract

To provide a water-disintegrable cleaning article having wet strength and water-disintegrability sufficient in actual use and moreover, being environmentally-friendly by using waste papers.SOLUTION: A manufacturing method of a water-disintegrable cleaning article includes steps of: manufacturing a raw material fiber by dispersing a waste paper-derived cellulose fiber in water, followed by conducting heat dry treatment 2 or more times; manufacturing a substantially water-dispersible fiber sheet containing the raw material fiber and a water-soluble binder by wet type sheet-making using the raw material fiber; and maintaining an aqueous agent in the fiber sheet. Preferably, the treatment to the waste paper-derived cellulose fiber is run in a manner that a mean fiber length of the raw material fiber becomes 0.5 mm or over and 1.6 mm or under and a fibril degree becomes under 2.0%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a water-disintegrable cleaning article. The present invention also relates to a method for modifying fibers. [Background technology]

[0002] As a type of water-disintegrable cleaning article that is disposed of by flushing down the drain after use, a wet-type water-disintegrable cleaning article is known, which is made by impregnating a water-disintegrable sheet made of cellulose fibers such as wood pulp bound with a water-soluble binder with an aqueous chemical. This type of water-disintegrable cleaning article is required to have water disintegrability that allows it to disintegrate and disperse quickly when placed in a large amount of water, and wet strength sufficient for practical use.

[0003] From the viewpoint of achieving a balance between water-disintegrability and wet strength, virgin pulp has been used in the water-disintegrable cleaning article. However, in recent years, the idea of ​​product development based on the three viewpoints of environment, society, and governance, i.e., ESG viewpoint, has become popular in the management and growth of companies, and this idea also extends to the technological development of water-disintegrable cleaning articles. Therefore, the applicant previously proposed using cellulose fibers derived from waste paper as the raw fiber of the water-disintegrable sheet that constitutes the water-disintegrable cleaning article (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2021-069641 Summary of the Invention [Problem to be solved by the invention]

[0005] Because the physical properties of cellulose fibers derived from waste paper are different from those of virgin pulp, even if the technology related to conventional water-decomposable cleaning products that use virgin pulp as a raw material is directly applied to cellulose fibers derived from waste paper, it is not easy to achieve both water-decomposability and wet strength. Therefore, an object of the present invention is to provide a method for producing a water-disintegrable cleaning article which has sufficient wet strength and water-disintegrability for practical use and is environmentally friendly by using recycled paper. [Means for solving the problem]

[0006] The present invention relates to a process for producing raw fiber by dispersing cellulose fiber derived from waste paper in water and then performing a heat-drying treatment twice or more; A step of producing a substantially water-dispersible fiber sheet containing the raw fiber and a water-soluble binder by wet papermaking using the raw fiber; and and causing the fiber sheet to retain an aqueous chemical.

[0007] The present invention also provides a method for modifying fibers, which comprises dispersing cellulose fibers derived from waste paper in water and then drying them by heating, the process being carried out at least twice. Effect of the Invention

[0008] According to the production method of the present invention, there is provided a water-decomposable cleaning article which has sufficient wet strength and water-decomposability for practical use, and which is environmentally friendly since it uses recycled paper. [Brief description of the drawings]

[0009] [Figure 1] 1(a) to (d) are schematic diagrams showing the steps of producing raw fiber used in the method for producing a water-decomposable cleaning article of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will now be described based on its preferred embodiments. In the manufacturing method of the present invention, cellulose fibers derived from waste paper are used as the raw material for the water-decomposable cleaning article. The cellulose fibers derived from waste paper include cellulose fibers obtained by recycling paper manufactured using virgin pulp as the raw material, and cellulose fibers obtained by recycling waste paper, but do not include virgin pulp itself. The main reason for using cellulose fibers derived from waste paper as the raw material for the water-decomposable cleaning article in the present invention is to reduce the environmental load, and by actively using cellulose fibers derived from waste paper, we aim to contribute even a little to preventing and solving various environmental problems such as preventing global warming and reducing waste. In addition, by using cellulose fibers derived from waste paper as the raw material, it is expected that the manufacturing cost of the water-decomposable cleaning article can be reduced.

[0011] However, the conditions of use of cellulose fibers derived from waste paper before recycling are different, and the quality varies greatly depending on the conditions of use, so not all of them are suitable for recycling. Moreover, if cellulose fibers derived from waste paper are used as the main raw material for a water-decomposable cleaning product that has both high wet strength and high water decomposability, it is expected that the cellulose fibers derived from waste paper that can be selected will be very limited. Under such a background, the present inventor focused on the concept of fibrillation degree and conducted various studies, and found that cellulose fibers derived from waste paper have a higher fibrillation degree, a shorter average fiber length, and contain a large amount of fine fibers derived from chemical and mechanical treatments and impurities compared to virgin pulp, as shown in Table 1 below. The fibrillation degree is an index that indicates the degree of fibrillation of cellulose fibers (especially external fibrillation), and the higher the fibrillation degree value, the more advanced the fibrillation of cellulose fibers is.

[0012] [Table 1]

[0013] Cellulose fibers derived from waste paper, which have characteristics completely different from those of virgin pulp, such as short average fiber length, high fibrillation degree, and a large content of fine fibers, have low entanglement due to these characteristics, which results in a decrease in paper strength. In addition, the dense structure of the fibrillated fibers results in low water permeability into the paper, which in turn results in poor water disintegrability. In detail, cellulose fibers with a relatively high degree of fibrillation have more advanced external fibrillation than cellulose fibers with a relatively low degree of fibrillation, and the fibrils on the outside of the fibers are fluffy and have an increased specific surface area. This promotes physical entanglement by the fibrils and strengthens the bonds between the fibers, resulting in a decrease in the water-disintegrability of the paper, and the paper becomes difficult to disintegrate and disperse even when placed in a large amount of water.

[0014] As described above, the present inventors have conducted extensive research to enable waste paper-derived cellulose fibers, which have completely different properties from virgin pulp, to be used as a raw material for water-decomposable cleaning products. As a result, it has been discovered that by subjecting waste paper-derived cellulose fibers to a series of two processes, (i) dispersing them in water and (ii) drying them by heating, and repeating this process two or more times, the surface of the fibers becomes smoother and the degree of fibrillation of the fibers decreases.

[0015] In detail, as shown in Fig. 1(a), cellulose fibers derived from waste paper are dispersed in water to form a slurry 10. This slurry 10 is dehydrated and pressed to produce a wet paper web 11 as shown in Figs. 1(b) and (c). This paper web 11 is dried to obtain paper 12 as shown in Fig. 1(d). This series of operations constitutes one set, and this set is repeated two or more times. In the final set, the operation shown in Fig. 1(d) is performed to obtain paper 12, which is then disintegrated in water to obtain cellulose fibers, which are the raw material for the water-decomposable cleaning article to be manufactured in the present invention.

[0016] In the procedure shown in Fig. 1(a), the cellulose fibers dispersed in water are derived from waste paper. The meaning of cellulose fibers derived from waste paper is as described above. The slurry 10 has a basic composition containing cellulose fibers derived from waste paper and water, and optional components can be added as necessary. Examples of optional components include natural polysaccharides, polysaccharide derivatives, and synthetic polymers. Examples of natural polysaccharides include sodium alginate, trant gum, guar gum, xanthan gum, gum arabic, carrageenan, galactomannan, gelatin, casein, albumin, and pulpuran. Examples of polysaccharide derivatives include carboxymethyl cellulose, carboxyethyl cellulose, carboxymethylated starch or its salt, starch, methyl cellulose, and ethyl cellulose. Examples of synthetic polymers include polyvinyl alcohol, polyvinyl alcohol derivatives, salts of polymers or copolymers of unsaturated carboxylic acids, and salts of copolymers of unsaturated carboxylic acids and monomers copolymerizable with the unsaturated carboxylic acids. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic anhydride, maleic acid, and fumaric acid.

[0017] In preparing the slurry 10, a stirring device using a stirring blade is used to thoroughly disperse the cellulose fibers derived from waste paper in water. Depending on the properties of the cellulose fibers derived from waste paper, treatment with a device used in a general wet papermaking method, such as a beater or refiner, may be used in combination.

[0018] After the slurry 10 is prepared as described above, as shown in Fig. 1(b) and (c), the slurry 10 is dehydrated and pressed to obtain a paper web 11. The basis weight of the cellulose fibers in the paper web 11 is 20 g / m 2 More than 60g / m 2 It is preferable to set the value below in terms of the physical properties of the paper, namely, the compatibility between strength and water disintegrability, and in terms of the feel of the paper. For dewatering and pressing, a papermaking machine used in a general wet papermaking method, such as a cylinder papermaking machine or a Fourdrinier papermaking machine, can be used. The paper web formed by dewatering contains, for example, 80% to 90% by weight of water. The pressing is performed by, for example, compressing the paper web 11 formed by dehydration from both sides. For example, a thick felt can be used to compress the paper web 11. By pressing, the proportion of water contained in the paper web 11 can be reduced to 40% to 70% by mass.

[0019] The paper web 11 obtained by pressing is subjected to a drying process as shown in FIG. 1(d). The paper web 11 can be dried using a heating and drying device used in general wet papermaking methods, such as a Yankee dryer. When using a Yankee dryer, the heating and drying conditions are preferably set to a peripheral temperature of 90° C. or higher and 140° C. or lower. Paper 12 is obtained by drying the paper web 11. The moisture content of the obtained paper 12 is preferably 10% by mass or lower. In general paper manufacturing, the paper obtained by drying the paper web is often subjected to a calendering process as a post-process, but in the present invention, no calendering process is performed.

[0020] This completes the series of treatments shown in Fig. 1(a) to (d). The paper obtained by this treatment is disintegrated in water, and the series of treatments shown in Fig. 1(a) to (d) are carried out once or twice or more. The reason for carrying out the treatments twice or more in total is that the fibrillation degree of the cellulose fibers derived from the waste paper cannot be sufficiently reduced by only one set of treatments shown in Fig. 1(a) to (d). From this viewpoint, it is preferable to repeat the series of treatments shown in Fig. 1(a) to (d) at least twice or more, more preferably three times or more, and even more preferably five times or more. The more the treatments are repeated, the lower the fibrillation degree of the cellulose fibers and the lower the content ratio of fine fibers. As a result, when a water-decomposable cleaning article is manufactured using the cellulose fibers obtained by repeating the above treatments twice or more as a raw material, the water-decomposability is improved. The upper limit of the number of repetitions is preferably 5 times from the viewpoints of economy and sheet strength. The present inventors have confirmed that even if the series of treatments shown in Figs. 1(a) to (d) are repeated multiple times, no significant change is observed in the average fiber length of the cellulose fibers.

[0021] When the series of processes shown in FIGS. 1(a) to (d) is repeated multiple times, the conditions in each cycle may be the same as or different from the conditions in another cycle.

[0022] The series of treatments shown in Figures 1(a) to (d) is preferably repeated two or more times so that the fibrillation degree of the cellulose fibers is preferably less than 2.0%, more preferably 1.9% or less. By using raw fibers that have been subjected to such treatment, it is possible to manufacture a water-decomposable cleaning product that has both high levels of wet strength and water-decomposability. The fibrillation degree is preferably 1.2% or more, more preferably 1.3% or more, and even more preferably 1.5% or more.

[0023] 1(a) to (d) is preferably repeated two or more times so that the average fiber length of the cellulose fibers is preferably 0.5 mm to 1.6 mm, more preferably 0.6 mm to 1.4 mm, and even more preferably 0.65 mm to 1.2 mm. This also makes it possible to produce a water-disintegratable cleaning article that has both high wet strength and high water-disintegratability.

[0024] The method for measuring the fibrillation degree and average fiber length of cellulose fibers is as follows. The fibrillation degree is measured using a fiber image analysis analyzer. Specifically, a commercially available fiber image analysis analyzer (Valmet FS5 manufactured by Valmet Automation) is used and the measurement is performed according to the manual. The measurement principle is to prepare an aqueous dispersion of the fiber to be measured, inject this aqueous dispersion into a tube with an inner diameter of 0.5 mm and allow it to flow in one direction, and capture the flowing state with an imaging means such as a CCD camera in the presence of a light source. Based on the obtained image, the fibrillation part of each fiber is distinguished from the other parts. Then, the "ratio of the area of ​​the fibrillation part to the total area of ​​the fiber" (hereinafter also referred to as the "fibril area ratio") is measured. This fibrillation area ratio is the fibrillation degree. A small fibrillation degree means a small fibrillation area ratio, that is, external fibrillation has not progressed much. The average fiber length of the cellulose fibers can be measured using the measuring device (Valmet FS5) used in the above-mentioned measurement of the fibrillation degree, according to the manual.

[0025] As mentioned above, the cellulose fiber that is the raw material for the water-decomposable cleaning product is derived from waste paper. Waste paper that has been collected as a raw material for papermaking can be used. In Japan, waste paper is defined as follows in the implementation notice of the Resource Effective Utilization Promotion Law (enforced October 25, 1991). In the present invention, waste paper that meets the following definition can be used. Definition of waste paper: Paper, paper products, books, and other items that are entirely or partially made of paper, that have been used once or not and have been collected, or that have been discarded, but are useful and can be used as raw materials for paper (including those imported after collection), or have the potential to be used as raw materials for paper. However, this does not include those generated during the papermaking process at the factories or business premises (hereinafter referred to as "factories, etc.") of paper manufacturers, or those generated when processing is carried out at the factories, etc. of paper manufacturers (including cases where the paper manufacturers commission other businesses to process the products before shipping them), and that are not shipped as products and are used by the paper manufacturers as raw materials for paper.

[0026] Examples of waste paper that can be used in the present invention include newspapers, magazines, cardboard, "white and cardboard" (e.g. white, cream white and lined white), extra white, medium white, "imitation and colored" (e.g. imitation, colored, Kent, white art, flyers, beverage cartons, office paper), "ticket and medium-smooth paper" (e.g. special cut, separate cut, medium-smooth paper), brown imitation paper (e.g. cut brown, plain brown, miscellaneous bags, kraft cardboard), "mount paper, ground ticket, and cardboard" (e.g. wrap, upper mount paper, mount paper, miscellaneous paper), and the like. Among these waste papers, from the viewpoint of reliably imparting the desired properties (water-disintegrability, wet strength) to the water-disintegrable cleaning article, "imitation and colored" (inked wood-free paper and beverage cartons) are preferred, and beverage cartons such as milk cartons are more preferred.

[0027] The cellulose fibers derived from waste paper may be natural cellulose fibers or non-natural cellulose fibers. Examples of natural cellulose fibers include wood pulps such as pulps derived from conifers, such as softwood bleached kraft pulp (NBKP), and hardwood bleached kraft pulp (LBKP); and non-wood pulps such as cotton pulp and hemp pulp. Examples of non-natural cellulose fibers include modified pulps, such as cationic pulp and mercerized pulp; and regenerated cellulose fibers, such as cupra and rayon. Cellulose fibers derived from waste paper are typically wood pulps (NBKP, LBKP, etc.).

[0028] In order to produce a water-decomposable cleaning article using cellulose fibers (hereinafter also referred to as "raw fibers") obtained by repeating the series of processes shown in Figs. 1(a) to (d) two or more times, it is preferable to carry out the following steps. For example, a wet sheet is produced from a dispersion containing raw material fibers by a known wet paper-making method, and the sheet is subjected to a press dehydration treatment and / or a heat treatment such as hot air blowing to dry or semi-dry the sheet. After that, a water-soluble binder is applied to one side of the sheet by spraying or coating, and the sheet is further dried to produce a substantially water-dispersible fiber sheet containing the raw material fibers and the water-soluble binder.

[0029] The dispersion containing the raw fiber may contain other fibers than the raw fiber. Examples of other fibers include cellulose fibers not derived from waste paper, biodegradable fibers made of polylactic acid, and synthetic fibers such as polypropylene fibers, polyvinyl alcohol fibers, polyester fibers, and polyacrylonitrile fibers. These fibers can be used alone or in combination of two or more. The proportion of fibers other than the raw fiber in all the fibers contained in the fiber sheet is preferably 50% by mass or less, and more preferably 20% by mass or less. On the other hand, the proportion of the raw fiber in all the fibers contained in the fiber sheet is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 100% by mass.

[0030] The fiber sheet preferably has a basis weight of 20 g / m2 in terms of the balance between softness and sufficient wet strength. 2 More preferably, 40 g / m 2 More than 120 g / m 2 Less than 60 g / m 2 The following is the result.

[0031] Water is added to the fiber sheet thus obtained as necessary, and the sheet is dried at the same time or immediately after the bulky embossing to form a concave-convex shape, to obtain a bulky fiber sheet having a large number of concave-convex parts. Such a manufacturing method is carried out, for example, by a heat embossing device capable of simultaneously drying and bulky concave-convex shaping, as shown in FIG. 4 of JP-A-2006-81883.

[0032] The fiber sheet thus obtained is allowed to retain the aqueous chemical, thereby obtaining the desired water-disintegrable cleaning article. This water-disintegrable cleaning article does not disintegrate when impregnated with the aqueous chemical, but disintegrates quickly and at the fiber level when discarded in a large amount of water. The degree of disintegration of the water-disintegrable cleaning article 1 is expressed by the ease of disintegration defined in JIS P 4501-1993 (toilet paper), and the lower this value, the better the water-disintegrability. As a guideline for the ease of disintegration, 100 seconds or less is preferable, and 60 seconds or less is more preferable.

[0033] The water-soluble binder used in the above-mentioned method for producing a water-disintegratable cleaning article not only contributes to the development of wet strength of the fibrous sheet in a wet state, but also can affect the water-disintegratability of the fibrous sheet.

[0034] The water-soluble binder contained in the fibrous sheet is preferably one that, when the fibrous sheet is in a wet state holding an aqueous chemical, temporarily becomes insoluble, thereby functioning as a binder that maintains the bonds between the constituent fibers of the fibrous sheet and plays a role in maintaining the strength of the water-decomposable cleaning article when it is in use, and examples of water-soluble binders having this function include natural polysaccharides, polysaccharide derivatives, and synthetic polymers. Note that the "temporary insolubilization of the water-soluble binder" is typically caused by the action of a binder insolubilizing component (e.g., a binder crosslinking agent) in the aqueous chemical held by the fibrous sheet.

[0035] Examples of natural polysaccharides include sodium alginate, trant gum, guar gum, xanthan gum, gum arabic, carrageenan, galactomannan, gelatin, casein, albumin, and purpuran. Examples of polysaccharide derivatives include carboxymethyl cellulose, carboxyethyl cellulose, carboxymethylated starch or a salt thereof, starch, methyl cellulose, and ethyl cellulose. Examples of synthetic polymers include polyvinyl alcohol, polyvinyl alcohol derivatives, salts of polymers or copolymers of unsaturated carboxylic acids, and salts of copolymers of unsaturated carboxylic acids and monomers copolymerizable with the unsaturated carboxylic acids. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic anhydride, maleic acid, and fumaric acid.

[0036] Among the above-mentioned water-soluble binders, water-soluble binders having a carboxyl group are preferred because they have good performance as a binder and good affinity with a crosslinking agent described below. Examples of water-soluble binders having a carboxyl group include carboxymethyl cellulose (CMC), carboxyethyl cellulose, and salts thereof.

[0037] The aqueous chemical applied to the fiber sheet containing the water-soluble binder typically contains a binder insolubilizing component that insolubilizes the water-soluble binder contained in the fiber sheet. The reason is as follows. Since the fiber sheet is water-decomposable, it may easily disintegrate when impregnated with an aqueous liquid such as an aqueous chemical. Therefore, in order to improve the shape retention of the fiber sheet and prevent the fiber sheet from disintegrating in the presence of a small amount of water, the aqueous chemical held in the fiber sheet contains a binder insolubilizing component to promote the insolubilization of the water-soluble binder contained in the fiber sheet. For example, when a crosslinking agent is contained in the aqueous chemical held in the fiber sheet as a binder insolubilizing component, the water-soluble binder is crosslinked and insolubilized by the crosslinking agent, so that the water-soluble binder is no longer dissolved by a small amount of water. As a result, the shape retention of the fiber sheet is improved and the fiber sheet is less likely to disintegrate even when a small amount of water is poured on it. However, when the fiber sheet is immersed in a large amount of water, the water-soluble binder, whose insolubilization was temporarily suppressed, becomes soluble in water again, and the fiber sheet can quickly disintegrate at the fiber level.

[0038] The crosslinking agent (binder insolubilizing component) may be selected appropriately depending on the type of water-soluble binder used, and is not particularly limited. For example, when a water-soluble binder having a carboxyl group, such as the above-mentioned CMC, is contained in the fiber sheet, it is preferable to use a polyvalent metal ion as the crosslinking agent. In particular, it is preferable to use one or more divalent metal ions selected from the group consisting of alkaline earth metals, manganese, zinc, cobalt, and nickel, because the fibers in the fiber sheet are sufficiently bonded to each other to develop a strength that can withstand use, and the fiber sheet has sufficient water disintegratability. Among these divalent metal ions, it is particularly preferable to use ions of calcium, strontium, barium, zinc, cobalt, and nickel. The divalent metal ions are added to the aqueous agent in the form of water-soluble metal salts, such as hydroxides, chlorides, sulfates, nitrates, carbonates, formates, and acetates.

[0039] The aqueous agent preferably contains a water-soluble organic solvent in addition to the crosslinking agent as a binder insolubilizing component. This significantly increases the generation of a crosslinked complex between the water-soluble binder and the crosslinking agent, and the complex exists in an insolubilized state, so that even if the amount of aqueous liquid in the aqueous agent held by the fiber sheet is large, sufficient strength to withstand use can be developed. Examples of the water-soluble organic solvent include monohydric alcohols such as ethanol, methanol, and isopropyl alcohol; glycols such as ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, and hexylene glycol; mono- or di-ethers of the glycols and lower alcohols such as methanol, ethanol, propanol, and butanol; esters of the glycols and lower fatty acids; and polyhydric alcohols such as glycerin and sorbitol, and the like. These can be used alone or in combination of two or more.

[0040] The water-decomposable cleaning article obtained by the manufacturing method of the present invention is suitable for use as an object cleaning agent for toilets, washrooms, kitchens, and other wet areas, and as an object wipe, a care wipe, or a makeup remover sheet. After use, the water-decomposable cleaning article 1 can be disposed of by simply flushing it down the drain, and as it quickly decomposes when flushed down the drain, it will not clog drain pipes. Specifically, the water-disintegrable cleaning article obtained by the manufacturing method of the present invention preferably has a water-disintegration time of 100 seconds or less as measured by the method described in the Examples below, because a water-disintegrable cleaning article having a water-disintegration time of 100 seconds or less can be quickly disintegrated and dispersed when placed in a large amount of water. Furthermore, the water-decomposable cleaning article obtained by the manufacturing method of the present invention preferably has a wet tensile strength of 300 cN / 25 mm or more as measured by the method described in the Examples below. A water-decomposable cleaning article having a wet tensile strength of 300 cN / 25 mm or more is unlikely to be damaged during normal cleaning or wiping work and is therefore suitable for practical use.

[0041] According to the present invention, in addition to the above-mentioned method for producing a water-decomposable cleaning article, a method for modifying cellulose fibers derived from waste paper is also provided. In this modification method, cellulose fibers derived from waste paper are dispersed in water and then heated and dried at least twice. By adopting this method, the fibrillation degree of cellulose fibers derived from waste paper, which have a high fibrillation degree, can be reduced, and the surface of the fibers can be made closer to a smooth state. The steps performed in this modification method are the same as those in the method for producing fibers used in the production of the above-mentioned water-decomposable cleaning article, so a repeated explanation will be omitted here. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0043] Example 1 General-purpose recycled paper (fibrillation degree 1.97%, average fiber length 0.762 mm) was dispersed in water and hand-made to obtain a paper web. This paper web was dried in a Yankee dryer heated to 130°C to obtain a paper web with a basis weight of 40 g / m2. 2 The paper was disintegrated in water, and the same procedure was repeated once more (a total of two times), and the paper thus obtained was disintegrated in water to obtain raw fiber. The fibrillation degree and average fiber length of the raw fiber were as shown in Table 2 below.

[0044] A specified amount of CMC was added as a water-soluble binder to a slurry (fiber concentration of about 0.3%) in which the raw material fibers were dispersed in water, and the slurry was wet-formed into a paper with a basis weight of 40 g / m. 2 The fiber sheet thus obtained had a raw fiber content of 95% and a CMC content of 5% in terms of solid content. The fiber sheet was immersed in an aqueous chemical to allow the fiber sheet to retain the aqueous chemical. The aqueous chemical used had the following formula. The amount of aqueous chemical retained (impregnated amount) in the fiber sheet was 210%. Thus, a water-decomposable cleaning article containing the fiber sheet and the aqueous chemical was produced. [Aqueous drug formulations] Alkyl glucoside 0.2% Zinc sulfate 3% Propylene glycol monomethyl ether 13% 1,2-Propanediol 7% Water balance (total 100%)

[0045] Example 2 The process from dispersing general-purpose waste paper in water to drying by heating was repeated three times in total in Example 1. A water-decomposable cleaning article was produced in the same manner as in Example 1 except for the above.

[0046] Example 3 The process from dispersing general-purpose waste paper in water to drying by heating was repeated five times in total in Example 1. A water-decomposable cleaning article was produced in the same manner as in Example 1 except for the above.

[0047] Comparative Example 1 A water-decomposable cleaning article was produced in the same manner as in Example 1, except that the general-purpose waste paper used in Example 1 was used as it was.

[0048] 〔evaluation〕 The wet tensile strength and water disintegration time of the water-disintegrable cleaning articles obtained in the Examples and Comparative Examples were measured by the following method. The results are shown in Table 2 below.

[0049] <Wet tensile strength measurement method> Based on JIS P8113, the wet tensile strength of the water-disintegrable cleaning article in the flow direction at the time of its manufacture is measured. A rectangular shape in plan view, 70 mm in the flow direction and 25 mm in the width direction, is cut out from the water-disintegrable cleaning article to prepare a test piece. This test piece is attached to the chuck of a tensile tester (Shimadzu Corporation Autograph AG-1kN) without tension so that the flow direction of the test piece is the tensile direction. The distance between the chucks is 50 mm. The test piece attached to the chuck is pulled at a tensile speed of 300 mm / min, and the maximum strength (unit: cN / 25 mm) until the test piece breaks is measured. The above measurement is performed 10 times for one type of water-disintegrable cleaning article, and the average of these measured values ​​is regarded as the wet tensile strength of the water-disintegrable cleaning article. The higher the wet tensile strength value, the stronger the wet strength and the less likely it is to break under normal use.

[0050] <Method of measuring dissolution time> A 300 ml beaker containing 300 ml of water (water temperature 20±5°C) and a rotor (disk-shaped with a diameter of 35 mm and a thickness of 12 mm) is placed on a magnetic stirrer, and the rotor's rotation speed is set to 600±10 rotations / min. A water-disintegrable cleaning article having a rectangular shape in plan view of 70 mm×60 mm is placed in the beaker, and a stopwatch is started. The rotation speed of the rotor is reduced to about 500 rotations at one time due to the resistance of the test piece present in the water, but increases as the disintegration and dispersion of the test piece progresses. When the rotation speed of the rotor recovers to 540 rotations, the stopwatch is stopped, and the time is measured in 1-second units. The above measurement is performed five times for one type of water-disintegrable cleaning article, and the average of these measured values ​​is regarded as the water disintegration time of the water-disintegrable cleaning article. The shorter the water disintegration time, the better the water disintegration and the easier it is to disintegrate and disperse in water.

[0051] [Table 2]

[0052] As is clear from the results shown in Table 2, the water-disintegrable cleaning articles obtained in the Examples had shorter water-disintegration times and higher wet tensile strengths than the water-disintegrable cleaning articles of the Comparative Examples. [Explanation of symbols]

[0053] 10 Slurry 11 paper animals 12. Paper

Claims

1. A process for producing raw fiber by dispersing cellulose fiber derived from waste paper in water and then heat-drying the same at least twice; A step of producing a substantially water-dispersible fiber sheet containing the raw fiber and a water-soluble binder by wet papermaking using the raw fiber; and A method for producing a water-decomposable cleaning article, comprising a step of retaining an aqueous chemical on the fiber sheet, A Yankee dryer is used for the treatment, the temperature of the peripheral surface of the Yankee dryer is set to 90° C. or more and 140° C. or less, and the mixture is dried until the moisture content becomes 10% by mass or less. The conditions in each round of the treatment may be the same as or different from the conditions in other rounds; The method for producing a water-decomposable cleaning article comprises the step of treating the cellulose fibers derived from waste paper so that the average fiber length of the raw fibers is 0.5 mm or more and 1.6 mm or less and the fibrillation degree is less than 2.0%.

2. The method according to claim 1 , wherein the treatment is performed on the cellulose fibers derived from waste paper so that the fibrillation degree of the raw fiber is 1.0 or more and 1.9 or less.

3. A method for modifying fibers, comprising dispersing cellulose fibers derived from waste paper in water and then heating and drying the fibers at least twice, A Yankee dryer is used for the treatment, the temperature of the peripheral surface of the Yankee dryer is set to 90° C. or more and 140° C. or less, and the mixture is dried until the moisture content becomes 10% by mass or less. The conditions in each round of the treatment may be the same as or different from the conditions in other rounds; The fiber modifying method comprises subjecting the waste paper-derived cellulose fibers to the treatment so that the fibers have an average fiber length of 0.5 mm or more and 1.6 mm or less and a fibrillation degree of less than 2.0%.

4. The method for modifying waste paper according to claim 3 , wherein the treatment is performed on the waste paper-derived cellulose fibers so that the fibrillation degree is 1.0% or more and 1.6% or less.

Citation Information

Patent Citations

  • Regeneration of waste paper of corrugated board by rising-floating and enzyme treatment

    JP2000027083A

  • Method for producing liner

    JP2003268699A

  • Bulky water disintegrative cleaning article

    JP2006081883A

  • Paper durability promoters, paper obtained by the same and manufacturing method of paper

    JP2015052194A

  • Cleaning sheet and method for manufacturing cleaning sheet

    JP2020117821A