Method for manufacturing soft carbon and lithium ion secondary battery
The described method enhances soft carbon production by controlling temperature, particle size, and adding asphalt, resulting in improved capacity retention and rapid charging cycle life for lithium ion secondary batteries.
Patent Information
- Application Number
- JP2023077006
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-09
- Filing Date
- 2023-05-09
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-05-09
AI Technical Summary
Conventional soft carbon production methods for lithium ion secondary batteries do not adequately improve characteristics such as capacity retention rate and rapid charging cycle life.
A method involving specific temperature and heating rates, particle size control, and addition of asphalt to carbon powder, along with a smoothing treatment, to produce soft carbon for use in lithium ion secondary batteries.
Improves capacity retention rate and rapid charging cycle life of lithium ion secondary batteries by reducing fine powder content and modifying the carbon surface, enhancing the performance of the negative electrode.
Smart Images

Figure 0007572500000004 
Figure 0007572500000005 
Figure 0007572500000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing soft carbon and a lithium ion secondary battery including the soft carbon as a negative electrode. [Background technology]
[0002] In recent years, lithium-ion secondary batteries have been widely used in various electronic products due to their advantages of high operating voltage, fast charge / discharge rate, long life, etc. Generally, the positive electrode material of a lithium-ion secondary battery can be selected from lithium cobalt oxide, lithium iron phosphate, ternary lithium, lithium manganese oxide, etc., and the negative electrode material can be selected from soft carbon, etc.
[0003] Next, the method of producing soft carbon mainly includes a pre-process and a post-process. The pre-process refers to the process of converting heavy oil into a precursor structure (e.g. raw coke), and the post-process refers to the process of calcining and carbonizing the precursor structure, followed by crushing and classification, carbonization at high temperature, and modified carbonization to finally obtain the finished product of soft carbon.
[0004] For the specific content of the method for preparing the soft carbon, please refer to the applicant's earlier Taiwanese patent application, i.e., application number TW111142065. The entire text of the earlier application is incorporated herein by reference. In the earlier application, a specific preparation process is used to provide a soft carbon anode material that can improve the rapid charge / discharge capability and cycle life of a battery. Summary of the Invention [Problem to be solved by the invention]
[0005] However, the present inventors have discovered that there is still room for improvement in the conventional soft carbon manufacturing method in terms of further improving the characteristics of lithium ion secondary batteries, such as the capacity retention rate and the rapid charging cycle life. [Means for solving the problem]
[0006] In order to solve the above problems, the present invention provides A step (A) of heating heavy oil at a temperature of 480°C to 550°C to produce raw coke; (B) a step of heating the raw coke to obtain a carbon-containing material by increasing the temperature to 850° C. to 900° C. at a first heating rate of 3° C. / min to 5° C. / min and maintaining the temperature for 4 hours or more; The carbon-containing material is pulverized and classified to obtain a particle size distribution D 50 (C) obtaining a carbon-containing powder having a particle size of 8 μm to 12 μm and a cumulative amount of powder having a particle size of 5 μm or less of the total powder being 1.0 wt % or less; (D) a step of heating the carbon-containing powder to obtain a carbon powder by increasing the temperature to 1030° C. to 1220° C. at a second heating rate of 3° C. / min to 10° C. / min and maintaining the temperature for 4 hours or more; A step (E) of obtaining soft carbon by adding asphalt to the carbon powder, and then heating the mixture to 1030°C to 1220°C at a third heating rate of 0.90°C / min to 1.25°C / min and maintaining the mixture for 5 hours or more; The soft carbon is used in the manufacture of a first type lithium ion secondary battery.
[0007] In one embodiment of the present invention, the amount of the asphalt added in step (E) is 5-8% by weight of the carbon powder. The soft carbon of this embodiment is used for manufacturing a second-type lithium ion secondary battery.
[0008] In one embodiment of the present invention, the method further includes a step (F) of performing a smoothing treatment to reduce the BET specific surface area of the carbon-containing material by 20% or more before the step (C), or a step (F) of performing a smoothing treatment to reduce the BET specific surface area of the carbon-containing powder by 20% or more after the step (C). The soft carbon of this embodiment is used in the manufacture of a third-type lithium-ion secondary battery.
[0009] In order to solve the above problems, the present invention provides a first type lithium ion secondary battery including a case, a negative electrode installed in the case and having soft carbon manufactured by the soft carbon manufacturing method, a positive electrode installed in the case and separated from the negative electrode, a separator film installed between the negative electrode and the positive electrode, and an electrolyte filled in the case.
[0010] In one embodiment of the present invention, the first cycle irreversible capacity of the first type lithium ion secondary battery is 40-45 mAh / g.
[0011] In order to solve the above problems, the present invention provides a second type lithium ion secondary battery including a case, a negative electrode placed in the case and having soft carbon produced by the soft carbon production method, a positive electrode placed in the case and separated from the negative electrode, a separator film placed between the negative electrode and the positive electrode, and an electrolyte filled in the case.
[0012] In one embodiment of the present invention, when fast-charged at 5C for 12 minutes, the capacity retention rate of the second type lithium ion secondary battery is 40% or more than that of the first type lithium ion secondary battery.
[0013] In one embodiment of the present invention, when fast-charged at 8C for 7.5 minutes, the capacity retention rate of the second type lithium ion secondary battery is 40% or more than that of the first type lithium ion secondary battery.
[0014] In order to solve the above problems, the present invention provides a third type lithium ion secondary battery including a case, a negative electrode installed in the case and having soft carbon produced by the soft carbon production method, a positive electrode installed in the case and separated from the negative electrode, a separator film installed between the negative electrode and the positive electrode, and an electrolyte filled in the case.
[0015] In one embodiment of the present invention, when fast charged at 5C for 12 minutes, the capacity retention rate of the third type lithium ion secondary battery is 10% or more higher than that of the first type lithium ion secondary battery or the second type lithium ion secondary battery.
[0016] In one embodiment of the present invention, when fast charged at 8C for 7.5 minutes, the capacity retention rate of the third type lithium ion secondary battery is 20% or more higher than that of the first type lithium ion secondary battery or the second type lithium ion secondary battery. Effect of the Invention
[0017] The present invention has been made in view of the above-mentioned problems in the prior art, and an object of the present invention is to provide a soft carbon material for use in the negative electrode of a lithium ion secondary battery. By using the soft carbon material as the negative electrode of a lithium ion secondary battery, it is possible to improve the characteristics of the lithium ion secondary battery, such as the capacity retention rate and the rapid charging cycle life. [Brief description of the drawings]
[0018] [Figure 1] 2 is a flow chart showing a method for producing soft carbon according to the present invention. [Figure 2a] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, (a) showing cycle life detection of the high-power half-cells of Example 1 and Comparative Example 1 under fast charging conditions of 5C for 12 minutes. [Figure 2b] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, and (b) shows the cycle life detection of the two high-power half-cells under fast charging conditions of 8C for 7.5 minutes. [Figure 3a] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, (a) showing cycle life detection of the high-energy type half cells of Example 1 and Comparative Example 1 under fast charging conditions of 5C for 12 minutes. [Figure 3b] 1 is a graph showing the capacity retention versus charge / discharge cycles, and (b) shows the cycle life detection of the two high-energy half-cells under fast charging conditions of 8C for 7.5 minutes. [Figure 4a] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, (a) showing cycle life detection of the high-power half-cells of Example 2 and Comparative Example 1 under fast charging conditions of 5C for 12 minutes. [Figure 4b] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, and (b) shows the cycle life detection of the two high-power half-cells under fast charging conditions of 8C for 7.5 minutes. [Figure 5a] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, (a) showing cycle life detection of the high-power half cells of Example 3 and Comparative Example 2 under fast charging conditions of 5C for 12 minutes. [Figure 5b] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, and (b) shows the cycle life detection of the two high-power half-cells under fast charging conditions of 8C for 7.5 minutes. [Figure 6a] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, (a) showing cycle life detection of the high-energy half-cells of Example 4 and Comparative Example 1 under fast charging conditions of 5C for 12 minutes; [Figure 6b] 1 is a graph showing the capacity retention versus charge / discharge cycles, and (b) shows the cycle life detection of the two high-energy half-cells under fast charging conditions of 8C for 7.5 minutes. [Figure 7a] 1 is a graph showing the relationship between capacity retention and charge / discharge cycles, (a) showing cycle life detection of the high energy type half cells of Example 5 and Example 4 under fast charging conditions of 5C for 12 minutes; [Figure 7b] 1 is a graph showing the capacity retention versus charge / discharge cycles, and (b) shows the cycle life detection of the two high-energy half-cells under fast charging conditions of 8C for 7.5 minutes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The following describes the implementation of the present invention through specific examples, and those skilled in the art can understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through different embodiments, and the details of the specification can be variously modified and changed based on different perspectives and applications without departing from the spirit of the present invention.
[0020] Unless otherwise specified in the text, the term "A to B" used in the specification and claims includes the meaning of "A or more and B or less." For example, the term "10 to 40% by weight" includes the meaning of "10% by weight or more and 40% by weight or less."
[0021] First, please refer to Fig. 1. Fig. 1 is a flow chart showing a method for producing soft carbon according to the present invention. As shown in Fig. 1, the method for producing soft carbon according to the present invention includes steps (A) to (E) and may further include step (F) (not shown). Each step will be described in detail below.
[0022] "Process (A)" Step (A) is a step for heating heavy oil to produce green coke at a temperature of 480° C. to 550° C. Specifically, the heavy oil is transported to a reaction vessel and heated at a coking temperature of 480° C. to 550° C. and a pressure of 0.2 MPa to 4 MPa for 1 to 16 hours, causing the heavy oil to undergo a cracking reaction and a polycondensation reaction to produce green coke.
[0023] "Process (B)" Step (B) is a step for obtaining a carbon-containing material by heating the raw coke obtained from step (A) to 850°C to 900°C at a first heating rate of 3°C / min to 5°C / min and maintaining the temperature for 4 hours or more. By step (B), the raw coke can undergo at least one of a polycondensation reaction, a dehydrogenation reaction, and a cracking reaction, and the raw coke can be converted into a carbon-containing material by the sp 2 This starts the trend towards forming carbon-containing materials with mixed orbitals.
[0024] "Process (C)" Step (C) is a step for pulverizing and classifying the carbon-containing material obtained in step (B) to obtain a carbon-containing powder. 50 The cumulative amount of powder having a particle size of 8 μm to 12 μm and a particle size of 5 μm or less is 1.0% by weight or less of the total carbon-containing powder. The pulverization in step (C) can be performed using a high-pressure air pulverizer, a collision plate pulverizer, an impact pulverizer, or the like, and the classification in step (C) can be performed using a cyclone classifier, a vibration classifier, or the like, and is not particularly limited.
[0025] Compared with the conventional technology, the first technical feature of the present invention is that the soft carbon material of the present invention can reduce the weight of the solid electrolyte membrane (SEI) formed on the surface of the negative electrode in the subsequent production of the negative electrode of a lithium ion secondary battery by reducing the proportion of fine powder (powder with a median particle size of 5 μm or less) in the carbon-containing powder through step (C), thereby improving the capacity retention rate and rapid charging cycle life of the lithium ion secondary battery.
[0026] "Process (D)" Step (D) is a step for obtaining carbon powder by heating the carbon-containing powder obtained from step (C) by increasing the temperature to 1030°C to 1220°C at a second heating rate of 3°C / min to 10°C / min and maintaining the temperature for 4 hours or more. By step (D), the raw coke remaining in the carbon-containing powder can undergo at least one of a polycondensation reaction, a cracking reaction, and a dehydrogenation reaction, and the carbon in the remaining raw coke can be converted into sp 2 It is rearranged into a mixed orbital and becomes carbon powder.
[0027] "Process (E)" Step (E) is a step for obtaining soft carbon by adding asphalt to the carbon powder obtained from step (D), and then heating the mixture to 1030°C to 1220°C at a third heating rate of 0.90°C / min to 1.25°C / min and maintaining the temperature for 5 hours or more. In step (E), the carbon powder to which asphalt has been added reaches the softening point of asphalt during the heating process of step (E) by utilizing the softening point of asphalt, thereby reducing the viscosity of the asphalt. The asphalt with reduced viscosity can modify the micropores on the surface of the carbon powder, and also reduces the specific surface area of the carbon powder, thereby obtaining the soft carbon of the present invention.
[0028] Compared with the conventional technology, the second technical feature of the present invention is that the amount of asphalt added in step (E) is 5 to 8% by weight of the carbon powder. In general, as described above, the addition of asphalt reduces the specific surface area of the carbon powder, and the charge capacity per unit time of the lithium ion secondary battery decreases. However, the present inventors have discovered that when the amount of asphalt in step (E) is 5 to 8% by weight (particularly 5% by weight) of the carbon powder, the charge capacity increases rather than decreases, and the capacity retention rate and rapid charge cycle life of the lithium ion secondary battery can be improved, compared with the amount of asphalt added of 4% by weight.
[0029] In step (E), it is preferable to add asphalt in an amount of 5 to 8% by weight of the carbon powder content, raise the temperature to 1100° C. at a rate of 1.22° C. per minute, and maintain the temperature for 5 hours or more.
[0030] "Process (F)" Compared with the prior art, a third technical feature of the present invention is that it further includes a step (F), which is a smoothing treatment performed before the step (C) to reduce the BET specific surface area of the carbon-containing material by 20% or more, or a smoothing treatment performed after the step (C) to reduce the BET specific surface area of the carbon-containing powder by 20% or more.
[0031] Specifically, in step (F), a jet mill (STJ200, manufactured by SEISHIN) is used to pulverize the carbon-containing material or carbon-containing powder, smoothing the surface of the carbon-containing material or carbon-containing powder and reducing the BET specific surface area by 20% or more. In addition, in step (F), step (C) may be repeated 5 to 10 times to repeatedly collide the carbon-containing material or carbon-containing powder against the wall surface of a pulverizer and / or classifier, or to collide carbon-containing materials or carbon-containing powders with each other, thereby reducing the BET specific surface area by 20% or more and achieving the effect of the smoothing treatment.
[0032] By carrying out the step (F), the capacity retention rate and the rapid charging cycle life of the lithium ion secondary battery can be further improved. EXAMPLES
[0033] The present invention will be further described below through examples and comparative examples, but the present invention is not limited to these examples and comparative examples.
[0034] <Comparative Example 1 and Examples 1 to 2> According to the above steps (A) to (E), the soft carbons of Comparative Example 1 and Examples 1 and 2 are produced under the conditions shown in the following Table 1. In addition, in step (C) of Comparative Example 1 and Examples 1 and 2, a high-pressure air pulverizer and a cyclone classifier are used.
[0035] [Table 1]
[0036] <Comparative Example 2 and Example 3> Comparative Example 2 is the same as Comparative Example 1 except that a collision plate polishing machine is used. Example 3 is the same as Example 2 except that a collision plate polishing machine is used. In this manner, the soft carbons of Comparative Example 2 and Example 3 are produced.
[0037] <Examples 4 to 5> Example 4 is the same as Comparative Example 1, except that step (C) is repeated five times as step (F) after step (C). Example 5 is the same as Example 4, except that the cumulative amount of powder having a particle size of 5 μm or less is reduced to 0.75 wt %. In this manner, the soft carbons of Examples 4 and 5 are produced.
[0038] <Production of soft carbon anode> A soft carbon negative electrode is manufactured according to the conventional technology. Specifically, the soft carbon negative electrode can be manufactured by referring to the method disclosed in Taiwan Patent Application No. TW111142065. First, each of the above soft carbons is crushed using a crusher, and then sieved with a sieve (mesh size: 38 μm) to obtain a soft carbon negative electrode material. Next, 9.1 g of the soft carbon negative electrode material, 0.5 g of PVDF, 0.4 g of conductive carbon black, and 12 g to 15 g of N-methylpyrrolidone (NMP) are uniformly mixed to form a mixed solution, and this mixed solution is applied to a copper foil having a thickness of 14 μm. Then, the mixture is dried at 85° C. for 0.5 hours to remove NMP and moisture, thereby forming the soft carbon negative electrodes of Comparative Examples 1 to 2 and Examples 1 to 5.
[0039] The soft carbon negative electrode includes a copper foil and a conductive film formed on the copper foil, and when the conductive film has a thickness of 20 to 30 μm, the negative electrode is a high-power type that can be used as a high-power half cell, and when the conductive film has a thickness of 50 μm, the negative electrode is a high-energy type that can be used as a high-energy half cell.
[0040] <Making a half cell> Fabricate half-cells according to the prior art. Specifically, the fabrication of half-cells can be carried out by referring to the method disclosed in Taiwan Patent Application No. TW111142065. First, soft carbon anodes in Comparative Examples 1-2 and Examples 1-5 (hereinafter simply referred to as the anodes of Comparative Examples 1-2 and Examples 1-5), lithium metal sheets as cathodes, electrolytes, and separator films [manufacturer: Celgard, material: polypropylene (PP) and polyethylene (PE)] are combined to form half-cells (hereinafter simply referred to as the half-cells of Comparative Examples 1-2 and Examples 1-5). The electrolyte contains 99 wt% of 1M LiPF6 solution and 1 wt% of vinylene carbonate. The LiPF6 solution contains LiPF6, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC), and the volume ratio of EC:EMC:DMC is 1:1:1.
[0041] In Comparative Example 1 and Example 1, high-power half-cells and high-energy half-cells are fabricated. In Comparative Example 2, high-power half-cells are fabricated. In Examples 2-3, high-power half-cells are fabricated. In Examples 4-5, high-energy half-cells are fabricated, respectively.
[0042] <Performance Test of Half-Cells> Using a charge-discharge machine (manufacturer: Arbin, model: BT2043), measure the charge capacity and discharge capacity of the first cycle of the half-cells in Comparative Examples 1-2 and Examples 1, 4-5. The measurement conditions are a temperature of 25°C, a charge-discharge rate (C-rate) of 0.2C, a charge termination voltage of 0V, and a discharge termination voltage of 1.8V. The irreversible capacity of the first cycle of the half-cell is calculated by the formula: irreversible capacity of the first cycle = (charge capacity of the first cycle - discharge capacity of the first cycle). Also, summarize the above measurement results in Table 2 below.
[0043] <BET Specific Surface Area> The BET specific surface areas of the soft carbons in Comparative Examples 1-2 and Examples 1, 4-5 were measured using a BET specific surface area measuring device (model: ASAP2020plus, brand: Micromeritics), and the measurement results are summarized in Table 2 below.
[0044] [Table 2]
[0045] <Thermogravimetric analysis (TGA) test> A TGA test is performed on the high-energy half-cell of Comparative Example 1 and the high-energy half-cell of Example 1. Specifically, after the cycle life of each of the half-cell of Comparative Example 1 and the half-cell of Example 1, 7.76 mg and 10.58 mg of the negative electrode material of the electrode sheet of the half-cell of Comparative Example 1 and the negative electrode material of the electrode sheet of the half-cell of Example 1 are scraped off and a TGA test is performed, and the negative electrode material is heated at 1100°C for 1 hour in an oxygen atmosphere to incinerate the carbon. From Table 3 below, it can be seen that the remaining weight (i.e., the weight of the SEI) of Comparative Example 1 after the TGA test was 0.29 mg, while the remaining weight (i.e., the weight of the SEI) of Example 1 after the test was 0.20 mg. From this, it can be seen that by making the cumulative amount of the powder having a particle size of 5 μm or less in step (C) 1.0 wt% or less of the entire carbon-containing powder, the weight of the high-resistance SEI is reduced and the rapid charging cycle life is improved.
[0046] [Table 3]
[0047] <Quick charging performance test> Using a charger (manufacturer: Maccor, model: Series 4000), the capacity retention rates for different charge / discharge cycles are measured for the half-cells in Comparative Examples 1-2 and Examples 1, 4-5 when the charge / discharge rates are 5C / 5C (charge / discharge time is 12 minutes) and 8C / 8C (charge / discharge time is 7.5 minutes). In addition, when the charge / discharge rate is 5C / 5C and the charge / discharge time is 12 minutes, it is abbreviated as "12 minutes rapid charge at 5C", and when the charge / discharge rate is 8C / 8C and the charge / discharge time is 7.5 minutes, it is abbreviated as "7.5 minutes rapid charge at 8C". The test results of the rapid charge performance of the half-cells in Comparative Examples 1-2 and Examples 1, 4-5 are shown in Figures 2-7.
[0048] <Comparison of experimental results> "Example 1 and Comparative Example 1" First, please refer to Figure 2. As shown in Figure 2(a), when the high-power half-cell of Example 1 (the conductive film of the negative electrode is 20 to 30 μm thick) is charged and discharged 100 times under the condition of 12 minutes of rapid charging at 5C, the capacity retention rate is still about 90%, whereas the capacity retention rate of the high-power half-cell of Comparative Example 1 under the same condition is only about 40%. This shows that the capacity retention rate of the high-power half-cell of Example 1 is improved by about 50% compared to that of Comparative Example 1.
[0049] 2(a), when the state in which the capacity retention rate is maintained at 80% or more is used as the standard for the rapid charging cycle life, when the number of charge / discharge cycles is about 60 in Comparative Example 1, the capacity retention rate falls to 80% or less, whereas when the number of charge / discharge cycles is 100 in Example 1, the capacity retention rate is maintained at 80% or more. In other words, compared to Comparative Example 1, the rapid charging cycle life of Example 1 is improved by 60% or more (100 / 60=about 67% improvement).
[0050] 2(b), when the number of charge / discharge cycles is 100 under fast charging conditions of 8C for 7.5 minutes, the capacity retention rate of the high-power half-cell of Example 1 is still about 90%, whereas the capacity retention rate of the high-power half-cell of Comparative Example 1 under the same conditions is only about 40%. This shows that the capacity retention rate of the high-power half-cell of Example 1 is improved by about 50% compared to that of Comparative Example 1.
[0051] In view of the above, under either the condition of 12 minutes of rapid charging at 5C or 7.5 minutes of rapid charging at 8C, the first technical feature of the present invention, "by step (C) in the carbon-containing powder, D 50 "Reducing the cumulative amount of powder having a particle size of 5 μm or less to 1.0% by weight or less of the total carbon-containing powder" can improve the capacity retention rate and the rapid charging cycle life of a lithium-ion secondary battery.
[0052] Furthermore, please refer to Figure 3. When the soft carbon of the present invention is applied to a high-energy half cell (negative electrode conductive film thickness is 50 μm), if the same comparison as in Figure 2 is made, the following can be seen from Figures 3(a) and 3(b).
[0053] (1) Under the condition of 12 minutes of rapid charging at 5 C and 100 charge / discharge cycles, Example 1 has a capacity retention rate improved by 20% or more and a rapid charging cycle life improved by approximately 20% compared to Comparative Example 1.
[0054] (2) Under the condition of 7.5 minutes of rapid charging at 8 C, when the number of charge / discharge cycles is 100, the capacity retention rate of Example 1 is improved by 30% or more and the rapid charging cycle life is improved by approximately 100% compared to Comparative Example 1.
[0055] The first cycle irreversible capacity of the high energy half cell of Example 1 was 43 mAh / g, which is still within the acceptable range (40 to 45 mAh / g). In addition, the results of Figures 2 and 3 show that the soft carbon of the present invention has the effect of improving the capacity retention rate and the rapid charging cycle life when applied to various types of half cells. That is, Example 1 has the effect of improving the capacity retention rate and the rapid charging cycle life while maintaining other characteristics (for example, when the first cycle irreversible capacity is in the range of 40 to 45 mAh / g).
[0056] "Example 2 and Comparative Example 1" First, the difference between Example 2 and Comparative Example 1 is that the amount of asphalt added in step (E) is increased from 4% by weight of the carbon powder to 5% by weight of the carbon powder (the second technical feature of the present invention). Next, please refer to Figure 4. When the same comparison as in Figure 2 is made, the following can be seen from Figure 4(a) and Figure 4(b).
[0057] (1) Under the condition of 12 minutes of rapid charging at 5C and 100 charge / discharge cycles, Example 2 has a capacity retention rate improved by 40% or more and a rapid charging cycle life improved by approximately 80% compared to Comparative Example 1.
[0058] (2) Under the condition of 7.5 minutes of rapid charging at 8 C and 100 charge / discharge cycles, the capacity retention rate of Example 2 is improved by 40% or more and the rapid charging cycle life is improved by approximately 80% compared to Comparative Example 1.
[0059] Furthermore, the charge capacity per unit time in Comparative Example 1 was 59% (5C rapid charge) and 50% (8C rapid charge), while the charge capacity per unit time in Example 2 was 60% (5C rapid charge) and 50% (8C rapid charge). This shows that the second technical feature of the present invention can further improve the capacity retention rate and rapid charge cycle life of a lithium ion secondary battery without reducing the charge capacity.
[0060] "Example 3 and Comparative Example 2" Example 3 and Comparative Example 2 show that the method of the present invention (e.g., the second technical feature) can also be applied to soft carbon materials with deteriorated properties. First, as shown in Table 2, the irreversible capacity of the first cycle of Comparative Example 2 is 51 mAh / g, which is slightly higher than the allowable range (40-45 mAh / g). Next, refer to FIG. 5. When the same comparison as FIG. 2 is made, the following can be seen from FIG. 5(a) and FIG. 5(b).
[0061] (1) Under the condition of 12 minutes of rapid charging at 5 C, when the number of charge / discharge cycles is 100, compared with Comparative Example 2, Example 3 has a capacity retention rate improved by 10% or more.
[0062] (2) When the number of charge / discharge cycles is 100 under the condition of 7.5 minutes of rapid charging at 8 C, Example 3 has a capacity retention rate improved by 20% or more compared to Comparative Example 2.
[0063] Furthermore, the charge capacities per unit time in Comparative Example 2 were 62% (5C rapid charge) and 58% (8C rapid charge), while the charge capacities per unit time in Example 3 were 65% (5C rapid charge) and 62% (8C rapid charge). This shows that the capacity retention rate of a lithium ion secondary battery can be improved according to the present invention, even if the characteristics of the soft carbon material deteriorate.
[0064] "Example 4 and Comparative Example 1" First, Example 4 differs from Comparative Example 1 in that a smoothing step (F) is further performed (the third technical feature of the present invention). Also, as shown in Table 2, the BET specific surface area of Comparative Example 1 is 2.3 m 2 / g, whereas the BET specific surface area of Example 4 is 1.5 m 2 / g, that is, the smoothing treatment reduced the BET specific surface area of Comparative Example 1 by about 30%. Next, refer to Figure 6. When the same comparison as in Figure 2 is made, the following can be seen from Figures 6(a) and 6(b).
[0065] (1) Under the condition of 12 minutes of rapid charging at 5C and 100 charge / discharge cycles, Example 4 has a capacity retention rate improved by 10% or more and a rapid charging cycle life improved by approximately 10% compared to Comparative Example 1.
[0066] (2) Under the condition of 8C, 7.5 minutes of rapid charging, and 100 charge / discharge cycles, Example 4 has a capacity retention rate improved by 20% or more and a rapid charging cycle life improved by approximately 100% compared to Comparative Example 1.
[0067] From this, it can be seen that the third technical feature of the present invention also makes it possible to further improve the capacity retention rate and the rapid charging cycle life of a lithium ion secondary battery.
[0068] "Example 5 and Example 4" First, the difference between Example 5 and Example 4 is that Example 5 is based on Example 4, and performs pulverization and classification so that the cumulative amount of powder with a particle size of 5 μm or less is 0.75% by weight or less (the first technical feature of the present invention). That is, Example 5 performs the first and third technical features of the present invention, whereas Example 4 performs only the third technical feature. Next, please refer to FIG. 7. When making the same comparison as FIG. 2, the following can be seen from FIG. 7(a) and FIG. 7(b).
[0069] (1) When the number of charge / discharge cycles is 100 under the condition of 12 minutes of rapid charging at 5 C, Example 5 has a capacity retention rate improved by 25% or more compared to Example 4.
[0070] (2) When the number of charge / discharge cycles is 100 under the condition of 7.5 minutes of rapid charging at 8 C, the capacity retention rate of Example 5 is improved by 45% or more compared to Example 4.
[0071] As described above with reference to FIG. 3, in the high energy type half cell, due to the first technical feature of the present invention, in the case of a 12 minute fast charge condition of 5C, Example 1 shows a capacity retention rate improvement of 20% or more compared to Comparative Example 1. Meanwhile, in the case of a 7.5 minute fast charge condition of 8C, Example 1 shows a capacity retention rate improvement of 30% or more compared to Comparative Example 1. From this, it can be seen that the improvement effect of the capacity retention rate of Example 1 compared to Comparative Example 1 under the two fast charge conditions is close to the improvement effect of the capacity retention rate of Example 5 compared to Example 4 under the two fast charge conditions.
[0072] In other words, when one of the technical features of the present invention has already been implemented (Example 4), and another technical feature is further implemented (Example 5), the same improvement in capacity retention rate is obtained as "the improvement in capacity retention rate when one of the technical features of the present invention is implemented (Example 1) compared to when the technical feature of the present invention is not implemented (Comparative Example 1)."
[0073] In summary, the present invention can be applied to various lithium ion secondary batteries such as high-power lithium batteries or high-energy lithium batteries, and can also be applied to soft carbon materials with deteriorated characteristics. In addition, each technical feature of the present invention has the effect of improving the capacity retention rate and the rapid charging cycle life, and when one of the technical features of the present invention has already been implemented, when the other technical features are further implemented, the effect of further improving the capacity retention rate can be obtained.
[0074] According to the manufacturing method of the present invention, a soft carbon material for use in the negative electrode of a lithium ion secondary battery can be provided. In addition, by using the soft carbon material as the negative electrode of a lithium ion secondary battery, the capacity retention rate and the rapid charging cycle life of the lithium ion secondary battery can be improved.
[0075] The present invention is not limited to the above-described embodiments, and various modifications can be made within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included within the technical scope of the present invention. [Explanation of symbols]
[0076] (A)~(E) Process
Claims
1. A step (A) of heating heavy oil at a temperature of 480°C to 550°C to produce green coke; (B) heating the raw coke to obtain a carbon-containing material by increasing the temperature to 850° C. to 900° C. at a first heating rate of 3° C. / min to 5° C. / min and maintaining the temperature for 4 hours or more; The carbon-containing material is pulverized and classified to obtain a particle size distribution D 50 (C) obtaining a carbon-containing powder having a particle size of 8 μm to 12 μm and a cumulative amount of powder having a particle size of 5 μm or less of 1.0 wt % or less of the total powder; (D) a step of heating the carbon-containing powder to obtain a carbon powder by increasing the temperature to 1030° C. to 1220° C. at a second heating rate of 3° C. / min to 10° C. / min and maintaining the temperature for 4 hours or more; Step (E) of adding asphalt to the carbon powder, and then heating the carbon powder to 1030°C to 1220°C at a third heating rate of 0.90°C / min to 1.25°C / min and maintaining the temperature for 5 hours or more to obtain soft carbon, the amount of the asphalt being 4 to 8% by weight of the carbon powder; A method for producing soft carbon, including:
2. The method for producing soft carbon according to claim 1, wherein in the step (E), the amount of the asphalt added is 5 to 8% by weight of the carbon powder.
3. 2. The method for producing soft carbon according to claim 1, further comprising a step (F) of performing a smoothing treatment before the step (C) to reduce the BET specific surface area of the carbon-containing material by 20% or more, or a smoothing treatment after the step (C) to reduce the BET specific surface area of the carbon-containing powder by 20% or more.
4. 3. The method for producing soft carbon according to claim 2, further comprising a step (F) of performing a smoothing treatment before the step (C) to reduce the BET specific surface area of the carbon-containing material by 20% or more, or a smoothing treatment after the step (C) to reduce the BET specific surface area of the carbon-containing powder by 20% or more.
Citation Information
Patent Citations
Lithium ion battery soft carbon negative electrode material and preparation method thereof
CN108448114A
Performance improvement method of coal-based sodium ion battery negative electrode material and application thereof
CN111293309A
Preparation method of artificial graphite material special for lithium ion battery negative electrode
CN111825088A
Artificial graphite composite negative electrode material for lithium ion battery as well as preparation method and application of artificial graphite composite negative electrode material
CN114597361A
Negative electrode active material for lithium ion secondary battery and negative electrode