Catalyst for air secondary battery, air electrode and air secondary battery

A bismuth ruthenium composite oxide with a specific lattice constant and sodium incorporation enhances catalytic activity, addressing overvoltage issues in air secondary batteries by facilitating easier oxygen ion movement within the crystal lattice, thereby improving charge/discharge efficiency.

JP7572881B2Active Publication Date: 2024-10-24FDK CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021037882
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-10
Publication Date
2024-10-24
Estimated Expiration
2041-03-10

AI Technical Summary

Technical Problem

Conventional pyrochlore-type bismuth ruthenium composite oxides do not adequately address the need for higher catalytic activity to reduce overvoltage in air secondary battery charge/discharge reactions.

Method used

A bismuth ruthenium composite oxide with a pyrochlore type crystal structure and a lattice constant of 10.33 Å to 10.47 Å, incorporating sodium, is used as a catalyst to enhance oxygen ion movement within the crystal lattice, thereby reducing overvoltage.

Benefits of technology

The catalyst exhibits higher catalytic activity, leading to reduced overvoltage in air secondary batteries, improving charge/discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572881000002
    Figure 0007572881000002
  • Figure 0007572881000003
    Figure 0007572881000003
  • Figure 0007572881000001
    Figure 0007572881000001
Patent Text Reader

Abstract

To provide a catalyst for an air secondary battery, having higher catalytic activity than conventional ones, an air electrode including the catalyst for an air secondary battery, and an air secondary battery including the air electrode.SOLUTION: A battery 2 includes: an electrode group 10 including, an air electrode 16 and a negative electrode 12 superimposed through a separator 14; and a container 4 accommodating the electrode group 10 together with an alkaline electrolyte 82 therein. The air electrode 16 includes a catalyst for an air secondary battery. The catalyst for an air secondary battery comprises a sodium-containing bismuth ruthenium composite oxide having a pyrochlore type crystal structure, a lattice constant in the crystal structure being 10.33Å or more and 10.47Å or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for an air secondary battery, an air electrode including this catalyst for an air secondary battery, and an air secondary battery including this air electrode. [Background technology]

[0002] In recent years, air batteries, which use oxygen in the air as the positive electrode active material, have been attracting attention because of their high energy density, small size, and ease of weight reduction, etc. Among such air batteries, zinc-air primary batteries have been put to practical use as power sources for hearing aids.

[0003] Additionally, research is being conducted on rechargeable air batteries that use Li, Zn, Al, Mg, etc. as the negative electrode metal, and such air secondary batteries are expected to become new secondary batteries that may have the potential to exceed the energy density of lithium-ion secondary batteries.

[0004] As one type of such air secondary battery, an air-hydrogen secondary battery is known, which uses an alkaline aqueous solution (hereinafter also referred to as an alkaline electrolyte) as the electrolyte and hydrogen as the negative electrode active material (see, for example, Patent Document 1). Air-hydrogen secondary batteries as typified by Patent Document 1 use a hydrogen storage alloy as the negative electrode metal, but the negative electrode active material in air-hydrogen secondary batteries is hydrogen that is absorbed and released by the above-mentioned hydrogen storage alloy, so that no dissolution or deposition reaction of the hydrogen storage alloy itself occurs during the chemical reaction (hereinafter also referred to as the battery reaction) during charging and discharging in the battery. For this reason, air-hydrogen secondary batteries have the advantage that they do not cause problems such as internal short circuit caused by so-called dendrite growth, in which the negative electrode metal precipitates in a dendritic form, or a decrease in battery capacity caused by shape change.

[0005] In an air secondary battery that uses an alkaline electrolyte, such as the above-mentioned air hydrogen secondary battery, the following charge and discharge reactions occur in the positive electrode (hereinafter also referred to as the air electrode).

[0006] Charging (oxygen generation reaction): 4OH -→O 2 +2H 2 O+4e - (I) Discharge (oxygen reduction reaction): O 2 +2H 2 O+4e - →4OH - (II)

[0007] As shown in reaction formula (I), oxygen is generated at the air electrode during charging in an air secondary battery. This oxygen passes through the voids inside the air electrode and is released into the atmosphere from the part of the air electrode that is open to the atmosphere. On the other hand, during discharging, oxygen taken in from the atmosphere is reduced to generate hydroxide ions as shown in reaction formula (II).

[0008] A catalyst that promotes the above-mentioned charge and discharge reaction is used for the air electrode, which is the positive electrode of the air secondary battery. In air secondary batteries, it is desired to reduce the overvoltage in the charge and discharge reaction of the air electrode in order to improve energy efficiency and increase output. For this reason, materials that are effective in reducing the overvoltage have been studied for the catalyst used in the air electrode. Materials that are effective in reducing such overvoltage include noble metals, metal oxides, and metal complexes. Among such materials, pyrochlore-type bismuth ruthenium composite oxides have the dual functions of oxygen reduction and oxygen generation, and can reduce the overvoltage during charging and discharging, making them promising catalysts for air secondary batteries.

[0009] In order to further reduce the overvoltage in the charge / discharge reaction, it is effective to increase the specific surface area of ​​the catalyst. As disclosed in Patent Document 1, a method for synthesizing a catalyst with a large specific surface area includes a method of obtaining a pyrochlore-type bismuth ruthenium composite oxide by heat-treating a catalyst precursor prepared by a coprecipitation method. In detail, a sodium hydroxide aqueous solution as a precipitant is added to a solution containing two or more types of metal ions to precipitate poorly soluble salts such as oxides as precipitate particles, and the obtained precipitate particles (precursor) are calcined in the air to obtain a bismuth ruthenium composite oxide (catalyst). According to the coprecipitation method, fine precipitate particles are obtained, so that the catalyst particles after calcination also become fine particles, and the specific surface area of ​​the catalyst is large. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2019-179592 A Summary of the Invention [Problem to be solved by the invention]

[0011] In order to further reduce the overvoltage in the charge / discharge reaction, it is necessary to increase the specific surface area of ​​the catalyst and to increase the activity of the catalyst itself (hereinafter, also referred to as catalytic activity). In other words, there is a demand for the development of a catalyst for air secondary batteries with higher catalytic activity than conventional catalysts. However, in the case of conventional pyrochlore-type bismuth ruthenium composite oxides, there has not been sufficient research into increasing the catalytic activity.

[0012] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a catalyst for air secondary batteries having higher catalytic activity than conventional catalysts, an air electrode including this catalyst for air secondary batteries, and an air secondary battery including this air electrode. [Means for solving the problem]

[0013] In order to achieve the above object, the present invention provides a catalyst for an air secondary battery, which is a sodium-containing bismuth ruthenium composite oxide having a pyrochlore type crystal structure, and in which the lattice constant in the crystal structure is 10.33 Å or more and 10.47 Å or less. Effect of the Invention

[0014] The catalyst for air secondary batteries according to the present invention is a sodium-containing bismuth ruthenium composite oxide having a pyrochlore-type crystal structure, and the lattice constant in the crystal structure is 10.33 Å or more and 10.47 Å or less. When the lattice constant is in the range of 10.33 Å or more and 10.47 Å or less, the space in the pyrochlore-type crystal structure expands, facilitating the movement of oxygen ions, and is considered to have a dominant effect on the oxygen reduction catalytic reaction involving the movement of oxygen in the crystal lattice. Therefore, the catalyst for air secondary batteries according to the present invention has high catalytic activity, and an air secondary battery using this catalyst for air secondary batteries in the air electrode can reduce overvoltage in charge and discharge reactions more than conventional air secondary batteries. Therefore, according to the present invention, it is possible to provide an air secondary battery catalyst that has a higher catalytic activity than conventional ones and can reduce overvoltage in charge and discharge reactions, an air electrode including this catalyst for air secondary batteries, and an air secondary battery including this air electrode. [Brief description of the drawings]

[0015] [Figure 1] 1 is a cross-sectional view illustrating an air hydrogen secondary battery according to an embodiment of the present invention; [Diagram 2] 1 shows an XRD profile of a bismuth ruthenium composite oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an air hydrogen secondary battery (hereinafter also referred to as battery) 2 including an air electrode catalyst for an air secondary battery according to one embodiment will be described with reference to the drawings.

[0017] As shown in FIG. 1, the battery 2 includes a container 4 and an electrode group 10 placed in the container 4 together with an alkaline electrolyte 82 .

[0018] The electrode group 10 is formed by stacking a negative electrode 12 and an air electrode (positive electrode) 16 with a separator 14 interposed therebetween.

[0019] The negative electrode 12 includes a conductive negative electrode substrate having a porous structure and a large number of pores, and a negative electrode mixture supported in the pores and on the surface of the negative electrode substrate. For example, foamed nickel can be used as the negative electrode substrate.

[0020] The negative electrode mixture includes a hydrogen storage alloy powder, which is an aggregate of hydrogen storage alloy particles capable of absorbing and releasing hydrogen as a negative electrode active material, a conductive material, and a binder. Here, the conductive material may be graphite powder, carbon black powder, or the like.

[0021] The hydrogen storage alloy constituting the hydrogen storage alloy particles is not particularly limited, but for example, a rare earth-Mg-Ni based hydrogen storage alloy is preferably used. The composition of this rare earth-Mg-Ni based hydrogen storage alloy can be freely selected, but for example, General formula: Ln 1-a Mg a Ni b-c-d Al c M d (III) It is preferable to use one represented by the following formula:

[0022] In general formula (III), Ln represents at least one element selected from the group consisting of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc, Y, Zr, and Ti; M represents at least one element selected from the group consisting of V, Nb, Ta, Cr, Mo, Mn, Fe, Co, Ga, Zn, Sn, In, Cu, Si, P, and B; and the subscripts a, b, c, and d represent numbers satisfying the relationships 0.01≦a≦0.30, 2.8≦b≦3.9, 0.05≦c≦0.30, and 0≦d≦0.50, respectively.

[0023] Here, the hydrogen storage alloy particles can be obtained, for example, as follows. First, metal raw materials are weighed and mixed to obtain a desired composition, and the mixture is melted in an inert gas atmosphere, for example, in a high-frequency induction melting furnace, and then cooled to form an ingot. The resulting ingot is heated to 900 to 1200°C in an inert gas atmosphere, and is homogenized by heat treatment in which it is held at that temperature for 5 to 24 hours. The ingot is then crushed and sieved to obtain a hydrogen storage alloy powder, which is an aggregate of hydrogen storage alloy particles of a desired particle size.

[0024] As the binder, for example, sodium polyacrylate, carboxymethyl cellulose, styrene butadiene rubber, etc. are used.

[0025] Here, the negative electrode 12 can be produced, for example, as follows. First, a negative electrode mixture paste is prepared by kneading hydrogen storage alloy powder, which is an aggregate of hydrogen storage alloy particles, a conductive material, a binder, and water. The obtained negative electrode mixture paste is filled into a negative electrode base material, and then a drying process is performed. After drying, the negative electrode base material to which the hydrogen storage alloy particles and the like are attached is rolled to increase the amount of alloy per unit volume, and then cut, thereby obtaining a negative electrode 12. This negative electrode 12 has a plate shape as a whole. The negative electrode mixture layer included in the negative electrode 12 is formed by hydrogen storage alloy particles, conductive material particles, and the like, so that there are gaps between the particles and the negative electrode mixture layer has a porous structure as a whole.

[0026] Next, the air electrode 16 includes a conductive air electrode substrate having a mesh structure, and an air electrode mixture layer (cathode mixture layer) formed by the air electrode mixture (cathode mixture) held on the air electrode substrate. For example, a nickel mesh can be used as the air electrode substrate.

[0027] The air electrode mixture contains an oxidation-reduction catalyst (air electrode catalyst), a conductive material, and a binder. The redox catalyst used has a dual function of redox. Such a catalyst with dual function contributes to reducing the overvoltage of the battery during both the charging and discharging processes. For example, a pyrochlore-type bismuth ruthenium composite oxide is used as such a redox catalyst. This bismuth ruthenium composite oxide has the dual functions of oxygen generation and oxygen reduction.

[0028] In this embodiment, a bismuth ruthenium composite oxide containing sodium is used. This bismuth ruthenium composite oxide has the composition formula Bi 2-x Ru 2 O 7-z (where x satisfies the relationship 0≦x≦1, z satisfies the relationship 0≦z≦1), and sodium is incorporated into the above crystal structure. This sodium is inevitably included during the manufacturing process. The bismuth ruthenium composite oxide used has a lattice constant in the above crystal structure of 10.33 Å or more and 10.47 Å or less.

[0029] Here, the inventors of the present application have conducted extensive research into reducing the overvoltage of the charge and discharge reactions in air secondary batteries, and have found that the larger the lattice constant of the bismuth ruthenium composite oxide used as the air electrode catalyst, the greater the reduction in the overvoltage of the discharge reaction in particular. This is believed to be because, when the lattice constant of the pyrochlore crystal structure becomes larger, the space within the pyrochlore crystal structure expands, facilitating the movement of oxygen ions, which has a dominant effect on the oxygen reduction catalytic reaction involving the movement of oxygen within the crystal lattice, resulting in a reduction in the overvoltage of the discharge reaction. The effect of reducing the overvoltage of the discharge reaction becomes significant when the lattice constant is 10.33 Å or more. The lattice constant of a typical pyrochlore-type bismuth ruthenium composite oxide (Bi 2-x Ru 2 O 7-z ) has a lattice constant of 10.28 Å or more and 10.30 Å or less. The pyrochlore-type bismuth ruthenium composite oxide according to this embodiment is characterized in that its lattice constant is larger than that of the general pyrochlore-type bismuth ruthenium composite oxide described above.

[0030] The larger the lattice constant, the easier it is for oxygen ions to move, so it is expected that the overvoltage of the discharge reaction of an air secondary battery that contains such a pyrochlore-type bismuth ruthenium composite oxide as an air electrode catalyst can be further reduced. However, the lattice constant is subject to geometric constraints. Specifically, if the synthesis conditions are changed so that the lattice constant becomes larger, phase separation or other crystal structures will eventually be formed. Pyrochlore-type oxides consisting of cations of elements A and B are represented by the general formula A 2 B 2 O 7It is a cubic compound represented by the formula: Each atomic position can be substituted in various ways while maintaining the ionic radius and charge balance, and a certain degree of atomic deficiency can be tolerated, so there are many compound groups. The bismuth ruthenium composite oxide of this embodiment is characterized by containing Bi at the A site, Ru at the B site, and Na. Na, which has a large ionic radius, is thought to be substituted for part of the Bi at the A site, so the lattice constant is large. However, there have been no reports of a form in which Na is substituted and the lattice constant is as large as 10.33. On the other hand, in the case of bismuth ruthenium composite oxide, a form with a lattice constant of 10.47 Å was the highest value according to a survey by ICDD. This bismuth ruthenium oxide contains Bi 2 (Ru 1.45 Bi 0.55 )O 7 The composition is such that Bi is in excess of Ru. Since the pyrochlore type can also have a structure of 10.47 Å, the upper limit of the lattice constant is set to 10.47 Å.

[0031] In addition, in the pyrochlore-type bismuth ruthenium composite oxide of this embodiment, Na / Ru, which represents the ratio of sodium to ruthenium contained therein, is 0.11 or less. When Na / Ru is 0.11 or less, the amount of sodium incorporated in the crystal structure of the bismuth ruthenium composite oxide is small. When the amount of sodium is small, it has a favorable effect on the oxidation reaction in the catalyst, and the catalytic activity is higher. In order to increase the catalytic activity, it is effective to reduce the amount of sodium as much as possible, but there is a limit to the amount of sodium that can be reduced by the current manufacturing method of the bismuth ruthenium composite oxide. As a specific value of Na / Ru, the lower limit is 0.02.

[0032] The above-mentioned pyrochlore-type bismuth ruthenium composite oxide can be produced, for example, as follows.

[0033] Bi(NO 3 ) 3 5H 2 O and RuCl 3 3H 2Then, Bi(NO) was added to the mixture so that the molar ratio of Ru was 1.00 and Bi was 0.50 or more and less than 0.80. 3 ) 3 5H 2 O and RuCl 3 3H 2 O and the weighed Bi(NO 3 ) 3 5H 2 O and RuCl 3 3H 2 Add O to the specified solution and stir to obtain Bi(NO 3 ) 3 5H 2 O and RuCl 3 3H 2 A mixed aqueous solution of O is prepared. At this time, examples of the predetermined solution include distilled water and a dilute nitric acid aqueous solution, and the temperature of these solutions is set to 60°C or higher and 90°C or lower. Then, a 1 mol / L to 3 mol / L NaOH aqueous solution is added to this mixed aqueous solution to precipitate a precursor (coprecipitation process). After this precursor is precipitated, the mixed aqueous solution is stirred. This stirring operation is performed for 12 to 48 hours with oxygen bubbling. Here, during the stirring operation, the mixed aqueous solution is maintained so that the pH is 11, and the temperature is maintained so that the temperature is 60°C to 90°C or lower. After the stirring operation is completed, the mixed aqueous solution is left to stand for 12 to 48 hours. After being left to stand, the resulting precipitate is collected by suction filtration. The collected precipitate is kept at 80°C to 100°C to evaporate a part of the water, forming a paste. This paste is transferred to an evaporating dish, heated to 100°C to 150°C, and dried by keeping it in that state for 1 hour to 5 hours, to obtain a dried paste. The resulting dried paste is placed in a mortar and ground with a pestle to obtain a powder of the unwashed precursor.

[0034] Next, the unwashed precursor powder obtained as described above is washed (washing step). This washing operation is performed, for example, by pouring water held at 60°C to 90°C onto the unwashed precursor powder, or by immersing the precursor powder in water held at 60°C to 90°C and stirring for 3.0 hours or less. In this washing step, most of the impurities including sodium adhering to the precursor powder are removed. Here, distilled water, ion-exchanged water, etc. can be used as the water used for washing. It is preferable to perform acid washing prior to washing with water. By adding acid washing, impurities can be removed more reliably. An example of the acid used for acid washing is an aqueous solution of nitric acid.

[0035] The precursor powder is then collected by suction filtration, and the collected powder is heated to 60°C or higher and 130°C or lower, and is kept in that state for 1 hour or higher and 12 hours or lower to dry (drying step). This gives a washed precursor powder.

[0036] Next, the washed precursor powder is heated to a temperature of 400°C or higher and 700°C or lower in an air atmosphere and held for 0.5 hours or higher and 4 hours or lower, thereby carrying out a heat treatment (calcination process). After the heat treatment, the powder is washed with distilled water at a temperature of 60°C or higher and 90°C or lower, and then dried. This drying process is carried out by holding the washed powder at a temperature of 60°C or higher and 130°C or lower for 1 hour or higher and 12 hours or lower. This produces a pyrochlore-type bismuth ruthenium composite oxide (Bi 2-x Ru 2 O 7-z ) is obtained.

[0037] Next, it is preferable to immerse the obtained bismuth ruthenium composite oxide in an aqueous solution of nitric acid to perform an acid treatment. Specifically, the procedure is as follows.

[0038] First, prepare an aqueous solution of nitric acid. The concentration of the aqueous solution of nitric acid is preferably 5 mol / L or less. The amount of the aqueous solution of nitric acid is preferably 20 mL per 1 g of bismuth ruthenium composite oxide. The temperature of the aqueous solution of nitric acid is preferably set to 20°C or more and 25°C or less.

[0039] Then, the bismuth ruthenium composite oxide is immersed in the prepared nitric acid aqueous solution and stirred for 1 hour or more and 6 hours or less. After stirring for a predetermined time, the bismuth ruthenium composite oxide is suction filtered from the nitric acid aqueous solution. The filtered bismuth ruthenium composite oxide is put into distilled water set at 60°C or more and 80°C or less and washed.

[0040] The washed bismuth ruthenium composite oxide is subjected to a drying treatment by being kept at 60° C. or higher and 130° C. or lower for 1 hour or longer and 12 hours or shorter.

[0041] In this manner, an acid-treated bismuth ruthenium composite oxide is obtained. By carrying out the acid treatment in this manner, by-products, particularly amorphous by-products, generated in the firing process of the bismuth ruthenium composite oxide can be removed. The acidic aqueous solution used in the acid treatment is not limited to an aqueous nitric acid solution, and in addition to the aqueous nitric acid solution, an aqueous hydrochloric acid solution or an aqueous sulfuric acid solution can be used. The aqueous hydrochloric acid solution and the aqueous sulfuric acid solution also have the effect of removing by-products, similar to the aqueous nitric acid solution.

[0042] The bismuth ruthenium composite oxide obtained as described above is mechanically pulverized as necessary to adjust the particle size to a predetermined size, thereby obtaining a powder of the bismuth ruthenium composite oxide which is an aggregate of particles having the predetermined particle size.

[0043] In the method for producing the bismuth ruthenium composite oxide of this embodiment, a sodium hydroxide solution is used as a precipitant in the coprecipitation step, so that the precipitate particles become fine, but sodium inevitably remains. This remaining sodium is sufficiently removed in the washing step, so that the subsequent firing step can be performed in a state of low sodium. Therefore, the amount of sodium incorporated in the crystal structure of the obtained bismuth ruthenium composite oxide is kept low.

[0044] Next, the conductive material will be described. The conductive material is used to reduce the internal resistance so as to increase the output of the air secondary battery, and is used as a support for the above-mentioned oxidation-reduction catalyst.

[0045] As such a conductive material, for example, nickel powder made of nickel particles is preferably used. The average particle size of the nickel particles is not particularly limited, and it is preferable that the nickel particles have a size that can impart the desired conductivity to the air electrode.

[0046] The nickel powder is preferably contained in the air electrode mixture in an amount of 60% by mass or more. The upper limit of the content of the nickel powder is preferably 80% by mass or less in relation to other constituent materials in the air electrode mixture. In addition, it is preferable to use filamentary nickel powder as the nickel powder.

[0047] The binder binds the constituent materials of the air electrode mixture and also serves to impart appropriate water repellency to the air electrode 16. The binder is not particularly limited, and may be, for example, a fluororesin. A preferred example of the fluororesin is polytetrafluoroethylene (hereinafter, also referred to as PTFE).

[0048] The air electrode 16 can be manufactured, for example, as follows. First, a catalyst powder which is an aggregate of bismuth ruthenium composite oxide particles, a conductive powder which is an aggregate of Ni particles as a conductive material, a binder, and water are prepared. Then, the catalyst powder, conductive powder, binder, and water are kneaded to prepare an air electrode mixture paste.

[0049] The obtained air electrode mixture paste is formed into a sheet by, for example, roller pressing, and dried at room temperature of about 25° C. This produces an air electrode mixture sheet, which is then press-bonded to a nickel mesh (air electrode substrate), thereby producing an intermediate air electrode product.

[0050] Next, the obtained intermediate product is put into a heat treatment furnace and subjected to heat treatment (firing). This heat treatment is performed in an inert gas atmosphere. For example, nitrogen gas or argon gas is used as the inert gas. The heat treatment conditions are to heat the intermediate product to a temperature of 200°C or more and 400°C or less, and to hold the product in this state for 10 minutes or more and 40 minutes or less. After that, the intermediate product is naturally cooled in the heat treatment furnace, and when the temperature of the intermediate product becomes 150°C or less, the intermediate product is taken out into the air. In this way, a heat-treated intermediate product is obtained. The heat-treated intermediate product is cut into a predetermined shape to obtain an air electrode 16. This air electrode 16 includes an air electrode mixture layer formed from an air electrode mixture. Since the air electrode mixture contains particles of bismuth ruthenium composite oxide, the air electrode mixture layer formed from the air electrode mixture has a porous structure including a large number of pores as a whole, and has excellent gas diffusion properties.

[0051] The air electrode 16 and the negative electrode 12 obtained as described above are stacked with a separator 14 interposed therebetween, thereby forming an electrode group 10. This separator 14 is disposed to prevent a short circuit between the air electrode 16 and the negative electrode 12, and an electrically insulating material is used for it. Examples of materials that can be used for this separator 14 include a polyamide fiber nonwoven fabric to which a hydrophilic functional group has been imparted, and a polyolefin fiber nonwoven fabric such as polyethylene or polypropylene to which a hydrophilic functional group has been imparted.

[0052] The formed electrode group 10 is placed in a container 4 together with an alkaline electrolyte. The container 4 is not particularly limited as long as it can accommodate the electrode group 10 and the alkaline electrolyte, and for example, an acrylic box-shaped container 4 is used. For example, as shown in FIG. 1, the container 4 includes a container body 6 and a lid 8.

[0053] The container body 6 is shaped like a box and has a bottom wall 18 and side walls 20 extending upward from the peripheral portion of the bottom wall 18. The portion surrounded by the upper edge 21 of the side wall 20 is open. In other words, an opening 22 is provided on the opposite side of the bottom wall 18. Furthermore, the side wall 20 has through holes at predetermined positions on the right side wall 20R and the left side wall 20L, respectively, and these through holes become outlets 24, 26 for lead wires, which will be described later.

[0054] Furthermore, an electrolyte storage unit 80 is attached to the container body 6. The electrolyte storage unit 80 is a container that stores an alkaline electrolyte 82, and is attached, for example, via a connection unit 84 that communicates with a through-hole 19 provided in the bottom wall 18. The connection unit 84 is a flow path for the alkaline electrolyte 82 that communicates between the inside of the container 4 and the electrolyte storage unit 80. Since the inside of the container 4 and the electrolyte storage unit 80 are thus communicated with each other, the alkaline electrolyte 82 can move between the inside of the container 4 and the electrolyte storage unit 80.

[0055] The lid 8 has the same shape as the container body 6 in a plan view, and is placed on the upper part of the container body 6 to close the opening 22. The gap between the lid 8 and the upper edge 21 of the side wall 20 is liquid-tightly sealed.

[0056] The lid 8 has an air passage 30 on the inner surface 28 facing the inside of the container body 6. The air passage 30 is open at the portion facing the inside of the container body 6, and has a serpentine shape as a whole. Furthermore, the lid 8 has an inlet air hole 32 and an outlet air hole 34 penetrating in the thickness direction at a predetermined position. The inlet air hole 32 communicates with one end of the air passage 30, and the outlet air hole 34 communicates with the other end of the air passage 30. That is, the air passage 30 is open to the atmosphere through the inlet air hole 32 and the outlet air hole 34. It is preferable to attach a pressure pump (not shown) to the inlet air hole 32. By driving this pressure pump, air can be sent from the inlet air hole 32 to the air passage 30.

[0057] If necessary, an adjustment member 36 is placed on the bottom wall 18 of the container body 6. The adjustment member 36 is used to align the electrode group 10 in the height direction inside the container 4. As the adjustment member 36, for example, a foamed nickel sheet is used.

[0058] The electrode group 10 is disposed on the adjustment member 36. At this time, the negative electrode 12 of the electrode group 10 is disposed so as to be in contact with the adjustment member 36.

[0059] On the other hand, a water-repellent ventilation member 40 is disposed on the air electrode 16 side of the electrode group 10 so as to contact the air electrode 16. This water-repellent ventilation member 40 is a combination of a PTFE porous membrane 42 and a nonwoven diffusion paper 44. The water-repellent ventilation member 40 exhibits a water-repellent effect due to the PTFE and allows gas to pass through. The water-repellent ventilation member 40 is interposed between the lid 8 and the air electrode 16 and is in close contact with both the lid 8 and the air electrode 16. This water-repellent ventilation member 40 has a size sufficient to cover the entire ventilation path 30, the inlet ventilation hole 32, and the outlet ventilation hole 34 of the lid 8.

[0060] The container body 6 housing the electrode group 10, the adjusting member 36, and the water-repellent and breathable member 40 as described above is covered with the lid 8. Then, as illustrated diagrammatically in Fig. 1, peripheral edge portions 46, 48 of the container 4 (container body 6 and lid 8) are sandwiched from above and below by connectors 50, 52. Thereafter, a predetermined amount of alkaline electrolyte 82 is injected from the electrolyte reservoir 80, and the container 4 is filled with the alkaline electrolyte 82. In this manner, the battery 2 is formed.

[0061] As the alkaline electrolyte 82, a typical alkaline electrolyte used in alkaline secondary batteries is suitably used, and specifically, an aqueous solution containing at least one of NaOH, KOH, and LiOH as a solute is used.

[0062] Here, in the battery 2, the ventilation passage 30 of the lid 8 faces the water-repellent ventilation member 40. The water-repellent ventilation member 40 allows gas to pass but blocks moisture, so the air electrode 16 is open to the atmosphere via the water-repellent ventilation member 40, the ventilation passage 30, the inlet ventilation hole 32, and the outlet ventilation hole 34. In other words, the air electrode 16 comes into contact with the atmosphere through the water-repellent ventilation member 40.

[0063] In the battery 2, an air electrode lead (positive electrode lead) 54 is electrically connected to the air electrode (positive electrode) 16, and a negative electrode lead 56 is electrically connected to the negative electrode 12. The air electrode lead 54 and the negative electrode lead 56 are drawn generally in FIG. 1, but are drawn out of the container 4 from the outlets 24, 26 while maintaining airtightness and liquid tightness. An air electrode terminal (positive electrode terminal) 58 is provided at the tip of the air electrode lead 54, and a negative electrode terminal 60 is provided at the tip of the negative electrode lead 56. In the battery 2, the air electrode terminal 58 and the negative electrode terminal 60 are used to input and output current during charging and discharging.

[0064] [Example] 1. Battery manufacturing Example 1 (1) Synthesis of air electrode catalyst 1) Co-precipitation process Bi(NO3 ) 3 5H 2 O and RuCl 3 3H 2 Then, Bi(NO) was added to the mixture so that the molar concentration ratio of Ru was 1.00 and Bi was 0.75. 3 ) 3 5H 2 O and RuCl 3 3H 2 O and Bi(NO 3 ) 3 5H 2 O and RuCl 3 3H 2 O were added to a dilute aqueous solution of nitric acid at 75°C and stirred to obtain Bi(NO 3 ) 3 5H 2 O and RuCl 3 3H 2 A mixed aqueous solution of O was prepared. Then, a 2 mol / L NaOH aqueous solution was gradually added to the obtained mixed aqueous solution to precipitate the precursor. After the precursor precipitated, the mixed aqueous solution was stirred. This stirring operation was performed for 24 hours while oxygen bubbling was performed. During this stirring operation, the pH of the mixed aqueous solution was maintained at 11 and the temperature was maintained at 75°C. After the stirring operation was completed, the mixed aqueous solution was left to stand for 24 hours. After standing, the resulting precipitate was collected by filtration. The collected precipitate was kept at 85°C to evaporate part of the water and make it into a paste. The obtained paste was transferred to an evaporating dish, heated to 120°C, and kept in that state for 3 hours to perform a drying process, and a dried product of the precursor was obtained. The obtained dried product of the precursor was placed in a mortar and crushed with a pestle to be powdered. In this way, a powder of an unwashed precursor was obtained.

[0065] 2) Cleaning process The unwashed precursor powder obtained as described above was immersed in ion-exchanged water kept at 75° C., stirred for 1 hour, and then filtered, thereby carrying out a washing process.

[0066] 3)Drying process The washed precursor powder was collected by suction filtration, and the collected powder was heated to 60° C. and kept for 12 hours to dry, thereby obtaining a washed precursor powder.

[0067] Here, X-ray diffraction (XRD) analysis was performed on the unwashed precursor powder set aside in advance and the washed precursor powder obtained as described above. A parallel beam X-ray diffractometer was used for the XRD analysis. The analysis conditions were as follows: X-ray source: CuKα, tube voltage: 15 kV, tube current: 15 mA, scan speed: 1 degree / min, step width: 0.01 degree. As a result of the analysis, the diffraction chart pattern for the unwashed precursor powder showed NaNO 3 On the other hand, the diffraction chart pattern of the washed precursor powder showed peaks of impurities such as NaNO 3 It was confirmed that the peaks of impurities such as NaCl and NaCl had almost completely disappeared. This analysis result showed that the above-mentioned washing process removed most of the impurities, including sodium, that had adhered to the precursor powder.

[0068] 4) Firing process The obtained precursor powder was subjected to a heat treatment in which it was heated to 500°C in an air atmosphere and held there for 3 hours. After the heat treatment, the precursor powder was washed with distilled water at 70°C, suction filtered, and dried at 120°C for 3 hours. This resulted in a sintered powder. The obtained powder was subjected to an XRD analysis. A parallel beam X-ray diffractometer was used for the XRD analysis. The analysis conditions were as follows: X-ray source: CuKα, tube voltage: 15 kV, tube current: 15 mA, scan speed: 1 degree / min, step width: 0.01 degree. The diffraction chart pattern obtained as a result of the analysis is shown in Figure 2. From the obtained diffraction chart pattern, it was found that the main phase of the sintered powder was Bi 2-x Ru 2 O 7-z It was confirmed that the pyrochlore crystal was RuO, which was not present before the calcination. 2 It was confirmed that a subphase of

[0069] In other words, it was confirmed that a pyrochlore-type bismuth ruthenium composite oxide (air electrode catalyst) was obtained by this firing process. The amount of the pyrochlore-type bismuth ruthenium composite oxide obtained was approximately 12 g.

[0070] Furthermore, the positions of the peaks originating from the (222) plane, the (440) plane, and the (622) plane were read, and the lattice constant of the pyrochlore-type bismuth ruthenium composite oxide was calculated from the read peak positions. Specifically, the spacing d of the crystal planes was calculated using the Bragg equation 2dsinθ=nλ (d is the spacing of the crystal planes, θ is the angle between the crystal planes and the X-rays, λ is the wavelength of the X-rays (λ=1.54 Å in this embodiment), and n is a natural number) and the equation of the (hkl) plane. Here, the equation of the (hkl) plane is generally hx+ky+lz-a=0, and the distance from the origin is equal to the spacing d of the crystal planes of the (hkl) plane, d=a*(h^2+k^2+l^2)^(-1 / 2). The obtained value of d was input into the analysis software "CellCalc" to calculate the lattice constant. As a result, the Bi of Example 1 was 2-x Ru 2 O 7-z The lattice parameter of the catalyst was 10.33 Å.

[0071] 5) Acid treatment process 1 g of the bismuth ruthenium composite oxide powder was placed in a stirring tank with a stirrer together with 20 mL of an aqueous nitric acid solution, and acid treatment was performed by stirring for 1 hour while maintaining the temperature of the aqueous nitric acid solution at 25° C. Here, the concentration of the aqueous nitric acid solution was 2 mol / L.

[0072] After the stirring was completed, the powder of the bismuth ruthenium composite oxide was taken out from the nitric acid aqueous solution by suction filtration. The taken out powder of the bismuth ruthenium composite oxide was washed with 1 liter of distilled water heated to 75°C. After washing, the powder of the bismuth ruthenium composite oxide was dried by keeping it in an atmosphere of 120°C for 3 hours.

[0073] In the above manner, the acid-treated bismuth ruthenium composite oxide powder, i.e., the air electrode catalyst (Bi 2-x Ru2 O 7-z The resulting air electrode catalyst was subjected to the acid treatment as described above to remove the amorphous by-products generated in the manufacturing process of the bismuth ruthenium composite oxide.

[0074] Regarding the obtained powder of bismuth ruthenium composite oxide, secondary electron images were observed under a scanning electron microscope, and it was found that the particle size of the bismuth ruthenium composite oxide was 0.1 μm or less.

[0075] Furthermore, the obtained bismuth ruthenium composite oxide powder was observed by a scanning electron microscope and subjected to elemental analysis by energy dispersive X-ray spectroscopy, that is, a composition analysis was performed by so-called SEM / EDS. The analysis conditions at this time were an acceleration voltage of 15 keV, a measurement magnification of 2000 times, and an accumulation number of 50 times. Specifically, particles close to the average particle size were selected and used as the analysis object. Then, the analysis object was spot-irradiated with an electron beam. The characteristic X-rays generated at this time were dispersed to calculate the molar ratios of Na, Bi, and Ru in the spot-irradiated area, and the elemental concentrations of these elements were obtained. As a result of the analysis, the molar ratio of each element was Na:Bi:Ru=6.3:36.9:56.8. And, Na / Ru, which represents the ratio of Na to Ru, was Na / Ru=0.11. Furthermore, Na / (Bi+Ru), which represents the ratio of Na to the sum of Bi and Ru, was Na / (Bi+Ru)=0.07.

[0076] (2) Manufacturing of air electrodes Ni powder was prepared as an aggregate of Ni particles. The Ni particles were filament-shaped and had an average particle size of 10 to 20 μm.

[0077] Furthermore, a polytetrafluoroethylene (PTFE) dispersion and ion-exchanged water were prepared.

[0078] Nickel powder, polytetrafluoroethylene (PTFE) dispersion, and ion-exchanged water were added to the bismuth ruthenium composite oxide powder (air electrode catalyst) obtained as described above and mixed. At this time, the bismuth ruthenium composite oxide powder was 20 parts by weight, the nickel powder was 70 parts by weight, the PTFE dispersion was 10 parts by weight, and the ion-exchanged water was 10 parts by weight, and mixed uniformly to produce an air electrode mixture paste.

[0079] The obtained air electrode mixture paste was formed into a sheet, and this sheet-shaped air electrode mixture paste was dried at room temperature of 25°C, and then pressed onto a nickel mesh with a mesh number of 60, a wire diameter of 0.08 mm, and an opening ratio of 60%, thereby obtaining an intermediate air electrode product.

[0080] Next, the obtained intermediate product was heat-treated (sintered). The heat treatment conditions were that the intermediate product was heated to a heat treatment temperature of 340°C in a nitrogen gas atmosphere and held at this temperature for 13 minutes. The heat-treated intermediate product was cut into a length of 40 mm and a width of 40 mm, thereby obtaining an air electrode 16. The thickness of this air electrode 16 was 0.23 mm. In the obtained air electrode 16, the amount of bismuth ruthenium composite oxide powder (air electrode catalyst) was 0.25 g.

[0081] (3) Manufacturing of negative electrodes The metallic materials Nd, Mg, Ni, and Al were mixed to a predetermined molar ratio, then placed in a high-frequency induction melting furnace and melted under an argon gas atmosphere. The resulting molten metal was poured into a mold and cooled to room temperature of 25°C to produce an ingot.

[0082] Next, this ingot was subjected to a heat treatment in which it was held in an argon gas atmosphere at a temperature of 1000°C for 10 hours, and then cooled to room temperature of 25°C. After cooling, the ingot was mechanically pulverized in an argon gas atmosphere to obtain a rare earth-Mg-Ni based hydrogen storage alloy powder. The volume average particle size (MV) of the obtained rare earth-Mg-Ni based hydrogen storage alloy powder was measured by a laser diffraction / scattering type particle size distribution measuring device. As a result, the volume average particle size (MV) was 60 μm.

[0083] The composition of this hydrogen storage alloy powder was analyzed by inductively coupled plasma spectrometry (ICP), and found to be Nd 0.89 Mg 0.11 Ni 3.33 Al 0.17 It was.

[0084] To 100 parts by weight of the obtained hydrogen storage alloy powder, 0.2 parts by weight of sodium polyacrylate powder, 0.04 parts by weight of carboxymethyl cellulose powder, 3.0 parts by weight of a styrene butadiene rubber dispersion, 0.5 parts by weight of carbon black powder, and 22.4 parts by weight of water were added and kneaded in an environment of 25°C to prepare a negative electrode mixture paste.

[0085] This negative electrode mixture paste is applied to a substrate with a surface density (weight) of approximately 250 g / m 2 The mixture was then filled into a foamed nickel sheet having a thickness of about 0.6 mm. The negative electrode mixture paste was then dried to obtain a foamed nickel sheet filled with the negative electrode mixture. The obtained sheet was rolled to increase the amount of alloy per unit volume, and then cut into a length of 40 mm and a width of 40 mm. In this manner, the negative electrode 12 was obtained. The thickness of the negative electrode 12 was 0.77 mm.

[0086] Next, an activation treatment was performed on the obtained negative electrode 12. The procedure of this activation treatment is as follows. First, a typical sintered nickel hydroxide positive electrode was prepared. The nickel hydroxide positive electrode had a positive electrode capacity sufficiently larger than the negative electrode capacity of the negative electrode 12. The nickel hydroxide positive electrode and the obtained negative electrode 12 were then stacked together with a separator made of polyethylene nonwoven fabric interposed therebetween to form an electrode group for activation treatment. The electrode group for activation treatment was placed in an acrylic resin container together with a predetermined amount of alkaline electrolyte. In this way, a single-pole cell of a nickel-hydrogen secondary battery with a negative electrode capacity regulation was formed.

[0087] This single-electrode cell was left to stand for 5 hours in an environment at a temperature of 25°C, charged for 2.8 hours at 0.5 It, and then discharged at 0.5 It until the battery voltage reached 0.70 V. This charge-discharge cycle was repeated five times to activate the negative electrode 12. The capacity of the single-electrode cell was determined in each charge-discharge cycle. The maximum capacity obtained was taken as the negative electrode capacity. The negative electrode capacity was 2500 mAh.

[0088] Thereafter, charging was performed at 0.5 It for 2.8 hours, and then the negative electrode 12 was removed from the single-electrode cell. In this manner, the negative electrode 12 that had been activated and charged was obtained.

[0089] (4) Manufacturing of air hydrogen secondary batteries The obtained air electrode 16 and negative electrode 12 were stacked with a separator 14 sandwiched between them to produce an electrode group 10. The separator 14 used in the production of this electrode group 10 was formed of a nonwoven fabric made of polypropylene fibers having sulfonic groups, and had a thickness of 0.1 mm (basis weight 53 g / m 2 ) was.

[0090] Next, the container body 6 was prepared, and the above-mentioned electrode group 10 was housed in this container body 6. At this time, a foamed nickel sheet serving as the adjustment member 36 was placed on the bottom wall 18 of the container body 6, and the electrode group 10 was placed on this adjustment member 36. Here, the foamed nickel sheet serving as the adjustment member 36 had a thickness of 1 mm and was in the shape of a square measuring 40 mm in length and 40 mm in width.

[0091] Next, the water-repellent and ventilation member 40 was disposed on the electrode group 10 (on the air electrode 16). Here, the water-repellent and ventilation member 40 was formed by combining a PTFE porous membrane 42 having a length of 45 mm, a width of 45 mm, and a thickness of 0.1 mm, and a nonwoven fabric diffusion paper 44 having a length of 40 mm, a width of 40 mm, and a thickness of 0.2 mm.

[0092] Next, the lid 8 was placed on the container body 6 to close the opening 22. At this time, the water-repellent ventilation member 40 was brought into close contact with the inner surface 28 of the lid 8 so that the area including the ventilation passage 30, the inlet ventilation hole 32, and the outlet ventilation hole 34 was entirely covered with the water-repellent ventilation member 40. Here, the ventilation passage 30 has a single serpentine shape as a whole. The cross section of the ventilation passage 30 is rectangular, with the vertical dimension of the rectangle being 1 mm and the horizontal dimension of the rectangle being 1 mm. The ventilation passage 30 is open on the water-repellent ventilation member 40 side.

[0093] The container 4 is formed by combining the container body 6 and the lid 8, and its peripheral edges 46, 48 are sandwiched from above and below by connectors 50, 52. A resin packing (not shown) is provided at the contact area between the container body 6 and the lid 8 to prevent leakage of the alkaline electrolyte.

[0094] Next, a 5 mol / L KOH aqueous solution was injected as the alkaline electrolyte 82 into the electrolyte reservoir 80. The amount of the KOH aqueous solution injected at this time was 50 mL. In this manner, a battery 2 as shown in FIG. 1 was produced.

[0095] An air electrode lead 54 is electrically connected to the air electrode 16, and an anode lead 56 is electrically connected to the anode 12, and these air electrode lead 54 and anode lead 56 appropriately extend from the lead wire outlets 24, 26 to the outside of the container 4 while maintaining the airtightness and liquid-tightness of the container 4. An air electrode terminal 58 is attached to the tip of the air electrode lead 54, and an anode terminal 60 is attached to the tip of the anode lead 56.

[0096] Example 2 An air-hydrogen secondary battery was manufactured in the same manner as in Example 1, except that in the washing step, the unwashed precursor powder was put into a 2 mol / L nitric acid aqueous solution, stirred for 1 hour for acid washing, and then the precursor powder filtered out from the nitric acid aqueous solution was washed with ion-exchanged water maintained at 75° C. The bismuth ruthenium composite oxide (air electrode catalyst) of Example 2 has a main phase of Bi 2-xRu 2 O 7-z It was confirmed that the crystal was a pyrochlore type crystal with a lattice constant of 10.33 Å. In addition, the molar ratio of each element in the bismuth ruthenium composite oxide after firing was Na:Bi:Ru = 1.9:39.7:58.5. The Na / Ru ratio was 0.03, and Na / (Bi+Ru) = 0.04.

[0097] Comparative Example 1 An air hydrogen secondary battery was manufactured in the same manner as in Example 1, except that the washing and drying steps were omitted and the firing step was carried out on the unwashed precursor powder. 2-x Ru 2 O 7-z The lattice constant of the catalyst was 10.24 Å. Here, the bismuth ruthenium composite oxide (air electrode catalyst) of Comparative Example 1 has a main phase of Bi 2-x Ru 2 O 7-z It was confirmed that the crystal was a pyrochlore type crystal with a lattice constant of 10.24 Å. In addition, the molar ratio of each element in the bismuth ruthenium composite oxide after firing was Na:Bi:Ru = 12.4:38.2:49.4. The Na / Ru ratio was 0.25, and Na / (Bi+Ru) = 0.14.

[0098] Comparative Example 2 In the coprecipitation process, Bi(NO 3 ) 3 5H 2 O and RuCl 3 3H 2 An air-hydrogen secondary battery was manufactured in the same manner as in Example 1, except that 1,0 and 1,0-tetrafluoroethylene were weighed, the washing and drying steps were omitted, and the firing step was performed on the unwashed precursor powder. 2-x Ru 2 O 7-zIt was confirmed that the crystal was a pyrochlore type crystal with a lattice constant of 10.27 Å. In addition, the molar ratio of each element in the bismuth ruthenium composite oxide after firing was Na:Bi:Ru = 9.5:41.7:48.8. The Na / Ru ratio was 0.19, and Na / (Bi+Ru) = 0.10.

[0099] 2. Evaluation of air hydrogen secondary batteries

[0100] (1) Battery characteristic evaluation The air hydrogen secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2 were repeatedly charged and discharged in an atmosphere of 25° C. via the air electrode terminal 58 and the negative electrode terminal 60 at 0.1 It for 10 hours, and then discharged at 0.2 It until the battery voltage reached 0.4 V. This cycle was repeated. 2000 mAh, which corresponds to 80% of the negative electrode capacity, was defined as 1.0 It.

[0101] In the above-mentioned charge / discharge operation, a rest period of 10 minutes was provided between charge and discharge, and between discharge and charge, respectively, and the discharge capacity and battery voltage were measured in each cycle.

[0102] The discharge capacity in the first cycle when the discharge voltage was stable was taken as the reference discharge capacity, and the battery voltage when the discharge capacity became half of the reference discharge capacity in the second cycle and after was recorded as the discharge intermediate voltage. The obtained data are shown in Table 1.

[0103] During the above-mentioned charging and discharging operations, regardless of charging and discharging, air was constantly supplied to the ventilation passage 30 at a rate of 33 mL / min by introducing air through the inlet vent 32 and discharging air through the outlet vent 34.

[0104] [Table 1]

[0105] (2) Consideration From Table 1, a negative correlation is seen between the lattice constant and the proportion of sodium in the catalyst. 2―x Ru 2 O 7-z It can be seen that the lattice constant of the bismuth alloy is high when it is outside the range of 10.28 Å to 10.30 Å, and is particularly high at 10.33 Å in Example 2. 2-x Ru 2 O 7-z It can be assumed that by shifting the lattice constant from the lattice constant, lattice distortion and oxygen vacancies are induced, and the catalytic activity involving the movement of oxygen within the crystal lattice is improved. In this example, it can be assumed that the increased lattice constant makes it easier for oxygen ions to move.

[0106] <Aspects of the present invention> A first aspect of the present invention is a catalyst for an air secondary battery, comprising a bismuth ruthenium composite oxide containing sodium, the bismuth ruthenium composite oxide having a pyrochlore type crystal structure, the lattice constant of the crystal structure being 10.33 Å or more and 10.47 Å or less.

[0107] According to the first aspect, since the lattice constant is larger than that of the conventional one, the space in the pyrochlore crystal structure is expanded, facilitating the movement of oxygen ions, and the catalytic activity related to the movement of oxygen ions in the crystal structure can be improved. As a result, the overvoltage in the charge and discharge reaction of the air secondary battery can be reduced more than that of the conventional one.

[0108] A second aspect of the present invention relates to the catalyst for an air secondary battery according to the above-mentioned first aspect of the present invention, wherein Na / Ru, which represents the ratio of sodium to ruthenium contained in the bismuth ruthenium composite oxide, is 0.11 or less.

[0109] According to the second aspect, the amount of sodium incorporated in the crystal structure of the bismuth ruthenium composite oxide is reduced, which has a favorable effect on the oxidation reaction and results in higher catalytic activity.

[0110] A third aspect of the present invention relates to an air electrode comprising an air electrode substrate and an air electrode mixture held on the air electrode substrate, the air electrode mixture including the air secondary cell catalyst according to the first or second aspect of the present invention described above, and a catalyst-supporting conductive material that supports the air secondary cell catalyst.

[0111] According to the third aspect, since the battery contains a catalyst for an air secondary battery having high catalytic activity, it is possible to further reduce overvoltage during charge and discharge reactions.

[0112] A fourth aspect of the present invention relates to the air electrode according to the above-mentioned third aspect of the present invention, wherein the catalyst-supporting conductive material is nickel.

[0113] According to the fourth aspect, the conductivity of the air electrode is improved.

[0114] A fifth aspect of the present invention relates to an air electrode according to the third or fourth aspect of the present invention, wherein the air electrode mixture further contains a water repellent agent.

[0115] According to the fifth aspect, the water repellency of the air electrode is improved, a three-phase interface is easily formed, and charge / discharge reactions proceed smoothly.

[0116] A sixth aspect of the present invention relates to the air electrode according to the above-mentioned fifth aspect of the present invention, wherein the water repellent is a fluororesin.

[0117] According to the sixth aspect, the fluororesin used as the water repellent is easily available, which contributes to reducing the manufacturing costs of the air electrode.

[0118] A seventh aspect of the present invention relates to the air electrode according to the above-mentioned sixth aspect of the present invention, wherein the fluororesin is polytetrafluoroethylene.

[0119] According to the seventh aspect, polytetrafluoroethylene is fibrous when subjected to mechanical stress, so that the binding property of the air electrode mixture is improved, which contributes to improving the strength of the air electrode.

[0120] An eighth aspect of the present invention relates to an air secondary battery comprising a container, an electrode group disposed in the container, and an alkaline electrolyte injected into the container, the electrode group including an air electrode and a negative electrode stacked together with a separator interposed therebetween, and the air electrode being the air electrode according to any one of the third to seventh aspects of the present invention described above.

[0121] According to the eighth aspect, an air secondary battery is obtained in which the overvoltage during charging and discharging is reduced compared to conventional air secondary batteries.

[0122] A ninth aspect of the present invention is the air secondary battery according to the third aspect, wherein the negative electrode contains a hydrogen storage alloy.

[0123] According to the ninth aspect, an air-hydrogen secondary battery in which overvoltage during charging and discharging is reduced can be obtained.

[0124] The present invention is not limited to the above-mentioned embodiment and examples. For example, the present invention is not limited to the air hydrogen secondary battery, and may be other air secondary batteries using Zn, Al, Mg, Li, etc. as the metal used in the negative electrode. In these other air secondary batteries, the reaction at the air electrode is the same as that of the air hydrogen secondary battery of this embodiment, and the effect of reducing the overvoltage of the battery is similarly obtained. [Explanation of symbols]

[0125] 2. Battery (air hydrogen secondary battery) 4 containers 6 Container body 8 Lid 10 electrode groups 12 Negative electrode 14 Separator 16 Air electrode (positive electrode) 30 Ventilation Channel 40 Water-repellent and breathable materials

Claims

1. A catalyst for an air secondary battery comprising a bismuth ruthenium composite oxide containing sodium, the bismuth ruthenium composite oxide having a pyrochlore type crystal structure, the lattice constant of the crystal structure being 10.33 Å or more and 10.47 Å or less.

2. 2. The catalyst for an air secondary battery according to claim 1, wherein a ratio Na / Ru of sodium to ruthenium contained in the bismuth ruthenium composite oxide is 0.11 or less.

3. A cathode substrate; and an air electrode mixture held on the air electrode substrate, 3. An air electrode, wherein the air electrode mixture comprises the catalyst for an air secondary cell according to claim 1 or 2, and a catalyst-supporting conductive material that supports the catalyst for an air secondary cell.

4. 4. The air electrode according to claim 3, wherein the catalyst-supporting conductive material is nickel.

5. The air electrode according to claim 3 or 4, wherein the air electrode mixture further contains a water repellent.

6. The air electrode according to claim 5 , wherein the water repellent is a fluororesin.

7. The air electrode according to claim 6 , wherein the fluororesin is polytetrafluoroethylene.

8. A container; An electrode group disposed in the container; and an alkaline electrolyte injected into the container; The electrode group includes an air electrode and a negative electrode stacked with a separator interposed therebetween, An air secondary battery, wherein the air electrode is the air electrode according to any one of claims 3 to 7.

9. The air secondary battery according to claim 8 , wherein the negative electrode contains a hydrogen storage alloy.

Citation Information

Patent Citations

  • Manufacturing method of catalyst for air secondary battery, manufacturing method of air secondary battery, catalyst for air secondary battery, and air secondary battery

    JP2019179592A

  • Air electrode catalyst for air secondary battery and air secondary battery

    JP2020126754A

  • Air electrode catalyst for air secondary battery, manufacturing method thereof, and air secondary battery

    JP2021099914A

  • Oxygen catalyst, electrode using oxygen catalyst, and electrochemical measurement method

    JP2021184340A

  • Air secondary battery catalyst and air secondary battery

    JP2022118881A