Supramolecular deep eutectic electrolyte with synergistic effect of hydrogen bonds and lithium bonds, preparation method and lithium air battery
The supramolecular deep eutectic electrolyte that synergizes with hydrogen bonds and lithium bonds solves the problem of insufficient performance of lithium air battery electrolytes in complex environments, improves capacity and cycling performance, and achieves a more stable electrochemical reaction.
Patent Information
- Application Number
- CN202411055096.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing lithium-air battery electrolytes are difficult to adapt to complex internal environments, resulting in low actual capacity and poor circulation and rate performance.
The supramolecular deep eutectic electrolyte that uses hydrogen bonds and lithium bonds to work synergistically, consists of lithium salts, amide-based solid solvents and additives. By regulating the solvation structure of the electrolyte, it assists the transport of interfacial substances and improves redox stability, and optimizes the supramolecular Components and proportions of ligands.
The capacity and circulation performance of lithium air batteries have been improved, the redox stability and electrochemical window of electrolytes have been improved, and the cycle life of the battery has been extended.
Smart Images

Figure CN118970295A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds, a preparation method and a lithium-air battery, belonging to the technical field of lithium-air batteries. Background Art
[0002] Lithium-air batteries have the advantages of high theoretical energy density, easy availability of raw materials, environmental friendliness and low cost, which brings unlimited possibilities for the development of the next generation of high-energy-density secondary batteries. The active substance of the positive electrode of lithium-air batteries is oxygen, and the negative electrode is metallic lithium with a relatively negative electrode potential. As a link between the positive and negative electrodes, the electrolyte must take into account the lithium ion / active oxygen conductivity, electrode / electrolyte interface compatibility and open system environmental adaptability. However, the electrolytes that have been developed so far are still difficult to adapt to the complex internal environment of lithium-air batteries, resulting in low actual capacity of lithium-air batteries, poor cycle performance and rate performance. Therefore, the development of high-performance electrolytes is of great significance to the research of lithium-air batteries.
[0003] Supramolecules are ubiquitous structures in nature. Deep eutectic electrolyte (DEE), as a supramolecular material, is a low-melting liquid mixture formed by non-covalent interactions such as lithium bonds, hydrogen bonds, and van der Waals forces between solid components. The anions and cations of lithium salts are lithium bond donors and hydrogen bond acceptors, respectively, and can be matched with hydrogen bond donor molecules and lithium bond acceptor molecules to obtain deep eutectic electrolytes: (1) This DEE has only a single cation (Li + ), and the hydrogen bonding between salt anions and solid solvent molecules is beneficial to Li + dissociation, high ionic conductivity; (2) Li + The lithium bond formed with the acceptor molecule can weaken the Li + Lewis acidity, thus promoting O2 - (3) The synergistic effect of lithium / hydrogen bonds is beneficial to reduce the free solvent molecules in the electrolyte and promote the formation of anion-derived SEI film, improving its interfacial compatibility with the electrode; (4) DEE has strong intermolecular interactions, low volatility and non-flammability. Therefore, supramolecular strategies are expected to prepare electrolytes suitable for lithium-air batteries and realize truly open-system lithium-air batteries. However, the variety of supramolecular ligands is complicated, and the experimental trial and error screening workload is large, making it difficult to achieve accurate preparation of lithium-air battery electrolytes. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds, a preparation method and a lithium-air battery. The synergistic effects of hydrogen bonds and lithium bonds between lithium salts, amide solid solvents and additives are used to regulate the electrolyte solvation structure, assist the transport of interfacial substances and improve the redox stability of the electrolyte, thereby achieving the improvement of the capacity and cycle performance of lithium-air batteries.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows.
[0006] A supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds, comprising a lithium salt, an amide solid solvent and an additive;
[0007] Wherein, the additive is one or more of boric acid, dicyandiamide, melamine, allantoin and glycine;
[0008] The molar ratio of lithium salt to amide solid solvent is 0.1-1:1; the concentration of additive in supramolecular deep eutectic electrolyte is 0.005-0.1 mol / L.
[0009] Preferably, the lithium salt is one or more of LiN(SO2CF3)2, LiN(SO2F)2, LiCF3SO3, LiC(SO2CF3)3 and LiClO4.
[0010] Preferably, the amide solid additive is one or more of acetamide, N-methylacetamide, N-ethylacetamide, propionamide, benzamide, urea and N,N-dimethylurea.
[0011] Preferably, the concentration of the additive is 0.01 to 0.05 mol / L.
[0012] Preferably, the molar ratio of the lithium salt to the amide solid solvent is 0.2-0.5:1.
[0013] A method for preparing the supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds according to the present invention, the method steps comprising:
[0014] The lithium salt, the amide solid solvent and the additive are mixed, heated to 60-100° C., and stirred for 12-24 hours to obtain a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds.
[0015] Preferably, the heating temperature is 75-85°C.
[0016] A lithium-air battery, wherein the electrolyte of the battery is a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds as described in the present invention.
[0017] Preferably, the positive electrode of the battery is commercial carbon, graphene, carbon fiber or carbon nanotube.
[0018] Beneficial Effects
[0019] The present invention prepares a low-melting-point, non-volatile liquid deep eutectic electrolyte through the synergistic effect of lithium bonds and hydrogen bonds between three solid supramolecular ligands, namely, lithium salt, amide solid solvent and additive. The electrolyte solvation structure is regulated by optimizing the composition and proportion of supramolecular ligands to assist the transport of interfacial substances. The interaction between supramolecular ligands is used to expand the band gap (such as HOMO) and LOMO) energy levels of the electrolyte. Figure 1 As shown), the redox stability of the electrolyte is improved, and the overall capacity and cycle performance of the lithium-air battery are improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The change of HOMO / LOMO energy levels of deep eutectic electrolyte after adding additives.
[0021] Figure 2 This is the electrochemical window diagram of the electrolyte in Example 1.
[0022] Figure 3 This is a graph showing the cycle performance of the lithium-air battery in Example 1.
[0023] Figure 4 This is a full discharge performance diagram of the lithium-air battery in Example 1.
[0024] Figure 5 This is the electrochemical window diagram of the electrolyte in Comparative Example 1.
[0025] Figure 6 This is the cycle performance diagram of the lithium-air battery in Comparative Example 1.
[0026] Figure 7 This is the full discharge performance diagram of the lithium-air battery in Comparative Example 1. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, rather than for limiting the scope of the present invention.
[0028] The experimental methods in the following examples and comparative examples are conventional methods unless otherwise specified. The materials and reagents used are all commercially available unless otherwise specified.
[0029] In the following examples and comparative examples:
[0030] (1) Assembly of button batteries:
[0031] The button battery is assembled from a negative electrode shell, a spring, a gasket, a lithium sheet, a glass fiber separator (Whatman, GF / D), an electrolyte, a positive electrode and a positive electrode shell, wherein the lithium sheet is the negative electrode, and the positive and negative electrode shells are 2032 battery shells, wherein the positive electrode shell has holes on its surface.
[0032] Preparation of the positive electrode: The active electrode material (commercial carbon, graphene, carbon fiber or carbon nanotube) is mixed with polyvinylidene fluoride (PVDF) in a mass ratio of 4:1, and then an appropriate amount of N-methylpyrrolidone (NMP) solution is added and ground into a uniform slurry. The prepared slurry is evenly coated on carbon paper and dried under vacuum conditions at 120°C for 24 hours, and then rolled and punched to obtain a prefabricated positive electrode.
[0033] Assemble the battery in an argon atmosphere, place the positive electrode sheet, gasket, lithium sheet, and separator into the negative electrode shell in sequence, drop 160 μL of electrolyte, add the positive electrode and positive electrode shell, and seal the battery to obtain a button battery.
[0034] (2) Electrochemical window test: A stainless steel symmetrical cell was assembled and tested using a 660D electrochemical workstation (Shanghai Chenhua) with a scan rate of 1 mV s -1
[0035] (3) Cyclic performance test: The instrument model used is: Land, Wuhan, test parameters: current density 200mA g -1 , limited capacity 500mAh g -1 .
[0036] (4) Full discharge performance test: The instrument model used is: Land, Wuhan, test parameters: current density 400mA g -1 , limiting the discharge voltage to 2.5V.
[0037] Example 1
[0038] Preparation of lithium-air battery electrolyte: In an argon glove box with water and oxygen contents less than 0.01 ppm, 3.45 g of LiN(SO2CF3)2 was mixed with 2.84 g of acetamide and 0.0031 g of boric acid, and the mixture was heated to 80°C and stirred for 12 h until a uniform and clear lithium-air battery electrolyte was obtained.
[0039] The above method was used to assemble a CR2032 button cell. The electrode active material used in this example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in Example 1.
[0040] Electrochemical window test: test results such as Figure 2 As shown, the solid line represents the electrolyte electrochemical window, and it is found that the electrolyte electrochemical window can reach 4.50V.
[0041] Cycle performance test: Test results are as follows Figure 3 As shown, the solid line represents the charge and discharge of the battery in the first week, the dotted line represents the charge and discharge of the battery in the 80th week, and the dotted horizontal line represents the charge and discharge of the battery in the 196th week, indicating that the battery can be cycled stably for 196 weeks.
[0042] Full discharge performance test: Test results are as follows Figure 4 As shown, the solid line is the battery at 200mAg -1 The full discharge performance at the current density shows that the battery can discharge 12952.3mAh g -1 capacity.
[0043] Comparative Example 1
[0044] Preparation of lithium-air battery electrolyte: In an argon glove box with water and oxygen contents less than 0.01 ppm, 3.45 g of LiN(SO2CF3)2 was mixed with 2.84 g of acetamide, and the mixture was heated to 80°C and stirred for 12 h until a uniform and clear lithium-air battery electrolyte was obtained.
[0045] The above method was used to assemble a CR2032 button battery. The electrode active material used in this comparative example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in this comparative example 1.
[0046] Electrochemical window test: test results such as Figure 5 As shown, the solid line represents the electrolyte electrochemical window, and it is found that the electrolyte electrochemical window can reach 3.70V.
[0047] Cycle performance test: Test results are as follows Figure 6 As shown, the solid line represents the charge and discharge of the battery in the first week, the dotted line represents the charge and discharge of the battery in the 80th week, and the dotted horizontal line represents the charge and discharge of the battery in the 120th week, indicating that the battery can be cycled stably for 120 weeks.
[0048] Full discharge performance test: Test results are as follows Figure 7 As shown, the solid line is the battery at 200mA g -1 The full discharge performance at the current density shows that the battery can discharge 6049.5 mAh g -1 capacity.
[0049] Comparative Example 2
[0050] Preparation of lithium-air battery electrolyte: In an argon glove box with water and oxygen contents less than 0.01 ppm, mix 2.87 g of LiN(SO2CF3)2 and 3.54 g of acetamide, heat to 80°C and stir for 12 hours until a uniform and clear lithium-air battery electrolyte is obtained.
[0051] The above method was used to assemble a CR2032 button cell. The electrode active material used in this comparative example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in comparative example 2.
[0052] Electrochemical window test: The electrolyte electrochemical window can reach 3.53V.
[0053] Cycle performance test: The battery can cycle stably for 67 weeks.
[0054] Full discharge performance test: The battery can discharge 5093.3mAh g -1 capacity.
[0055] Comparative Example 3
[0056] Preparation of lithium-air battery electrolyte: In an argon glove box with water and oxygen contents less than 0.01 ppm, mix 2.87 g of LiN(SO2CF3)2 and 1.18 g of acetamide, heat to 80°C and stir for 12 hours until a uniform and clear lithium-air battery electrolyte is obtained.
[0057] The above method was used to assemble a CR2032 button battery. The electrode active material used in this comparative example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in Comparative Example 3.
[0058] Electrochemical window test: The electrolyte electrochemical window can reach 4.71V.
[0059] Cycle performance test: The battery can cycle stably for 3 weeks.
[0060] Full discharge performance test: The battery can discharge 3843.3mAh g -1 capacity.
[0061] Example 2
[0062] Preparation of lithium-air battery electrolyte: In an argon glove box with water and oxygen contents less than 0.01 ppm, 3.45 g of LiN(SO2CF3)2 was mixed with 2.84 g of acetamide and 0.0062 g of boric acid, and the mixture was heated to 80°C and stirred for 12 h until a uniform and clear lithium-air battery electrolyte was obtained.
[0063] The above method was used to assemble a CR2032 button cell. The electrode active material used in this example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in Example 2.
[0064] Electrochemical window test: The electrolyte electrochemical window can reach 4.46V.
[0065] Cycle performance test: The battery can be cycled stably for 135 weeks.
[0066] Full discharge performance test: The battery can discharge 9498.6mAh g -1 capacity.
[0067] Example 3
[0068] Preparation of lithium-air battery electrolyte: In an argon glove box with water and oxygen contents less than 0.01 ppm, 1.87 g of LiN(SO2F)2 was mixed with 3.49 g of N-ethylacetamide and 0.0053 g of melamine, and the mixture was heated to 80°C and stirred for 12 h until a uniform and clear lithium-air battery electrolyte was obtained.
[0069] The above method was used to assemble a CR2032 button cell. The electrode active material used in this example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in Example 3.
[0070] Electrochemical window test: The electrolyte electrochemical window is higher than 4.4V.
[0071] Cycle performance test: The battery can be cycled stably for more than 80 weeks.
[0072] Full discharge performance test: The battery can discharge more than 5000mAh g -1 capacity.
[0073] Example 4
[0074] Preparation of lithium-air battery electrolyte: In an argon glove box with a water content and an oxygen content of less than 0.01 ppm, 2.87 g of LiN(SO2CF3)2 was mixed with 2.40 g of urea and 0.0031 g of glycine, and the mixture was heated to 80°C and stirred thoroughly until a uniform and clear lithium-air battery electrolyte was obtained.
[0075] The above method was used to assemble a CR2032 button cell. The electrode active material used in this example was carbon nanotubes with a loading of 0.2 mg. The electrolyte was the lithium-air battery electrolyte prepared in Example 4.
[0076] Electrochemical window test: The electrolyte electrochemical window is higher than 4.5V.
Claims
1. A supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds, characterized in that: It is composed of lithium salt, amide solid solvent and additives; Wherein, the additive is one or more of boric acid, dicyandiamide, melamine, allantoin and glycine; The molar ratio of lithium salt to amide solid solvent is 0.1-1:1; the concentration of additive in supramolecular deep eutectic electrolyte is 0.005-0.1 mol / L.
2. The supramolecular deep eutectic electrolyte with synergistic hydrogen bonds and lithium bonds according to claim 1, characterized in that: The lithium salt is one or more of LiN(SO2CF3)2, LiN(SO2F)2, LiCF3SO3, LiC(SO2CF3)3 and LiClO4.
3. The supramolecular deep eutectic electrolyte with synergistic hydrogen bonds and lithium bonds according to claim 1, characterized in that: The amide solid additive is one or more of acetamide, N-methylacetamide, N-ethylacetamide, propionamide, benzamide, urea and N,N-dimethylurea.
4. The supramolecular deep eutectic electrolyte with synergistic hydrogen bonds and lithium bonds according to claim 1, characterized in that: The concentration of the additive is 0.01-0.05 mol / L.
5. The supramolecular deep eutectic electrolyte with synergistic hydrogen bonds and lithium bonds according to claim 1, characterized in that: The molar ratio of the lithium salt to the amide solid solvent is 0.2-0.5:
1.
6. The supramolecular deep eutectic electrolyte with synergistic hydrogen bonds and lithium bonds according to claim 1, characterized in that: The lithium salt is one or more of LiN(SO2CF3)2, LiN(SO2F)2, LiCF3SO3, LiC(SO2CF3)3 and LiClO4; The amide solid additive is one or more of acetamide, N-methylacetamide, N-ethylacetamide, propionamide, benzamide, urea and N,N-dimethylurea; The concentration of the additive is 0.01 to 0.05 mol / L; The molar ratio of the lithium salt to the amide solid solvent is 0.2-0.5:
1.
7. A method for preparing a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds as claimed in any one of claims 1 to 6, characterized in that: The method steps include: The lithium salt, the amide solid solvent and the additive are mixed, heated to 60-100° C., and stirred for 12-24 hours to obtain a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds.
8. The method for preparing a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds according to claim 7, characterized in that: The heating temperature is 75-85°C.
9. A lithium-air battery, characterized in that: The electrolyte of the battery is a supramolecular deep eutectic electrolyte with synergistic effects of hydrogen bonds and lithium bonds as described in any one of claims 1 to 6.
10. A lithium-air battery as claimed in claim 9, characterized in that: The positive electrode of the battery is commercial carbon, graphene, carbon fiber or carbon nanotube.
Citation Information
Patent Citations
Electrolyte
CN102185156A
Solid-state lithium battery polymer electrolyte and preparation method and application thereof
CN107069084A
Lithium battery low-temperature electrolyte and lithium battery
CN115986211A
Modified deep eutectic electrolyte, preparation method thereof and application of modified deep eutectic electrolyte in lithium oxygen battery
CN117691263A
Wide-temperature-range electrolyte and preparation method and application thereof
CN118315677A
Cited By
Acyl deep eutectic electrolyte and preparation method and application thereof
CN120073062A
Method for measuring eutectic compound formed between two electrolyte molecules
CN121122481A