Air electrode for air secondary battery and air secondary battery including said air electrode

The air electrode with a dual-function catalyst and fluororesin distribution enhances the output of air secondary batteries by optimizing water repellency and interface formation, addressing high overvoltage issues.

JP7572882B2Active Publication Date: 2024-10-24FDK CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021040123
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-12
Publication Date
2024-10-24
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

Air secondary batteries face high overvoltage during charging and discharging, limiting their output, and insufficient studies have been conducted on optimizing the water repellency of the air electrode to address this issue.

Method used

An air electrode comprising a base material with a catalyst layer containing a dual-function catalyst (oxygen generation and reduction), a conductive carbon material, and a fluororesin water repellent agent, with a specific standard deviation range (0.03≦σ≦0.05) for the F/C ratio, ensuring optimal two-phase and three-phase interfaces for efficient charge/discharge reactions.

Benefits of technology

The optimized air electrode reduces overvoltage and increases the output of air secondary batteries by promoting efficient charging and discharging reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572882000003
    Figure 0007572882000003
  • Figure 0007572882000004
    Figure 0007572882000004
  • Figure 0007572882000005
    Figure 0007572882000005
Patent Text Reader

Abstract

To provide an air electrode for an air secondary battery, which can lower an overvoltage in charge and discharge reactions, and an air secondary battery including such an air electrode.SOLUTION: An air electrode comprises: an air electrode 2 including a base material 6, and a catalyst layer 8 held by the base material 6. The catalyst layer 8 contains: a bifunctional catalyst capable of producing and reducing oxygen; an electrically-conductive material composed of a carbon material and serving to impart an electrically-conductive property to the catalyst layer 8; and a fluorine resin, serving to impart a water repellent agent to the catalyst layer 8. The ratio F / C of F to C, where C is a percentage of the number of atoms of carbon included in the carbon material, and F is a percentage of the number of atoms of fluorine in the fluorine resin, and atomic %, is measured at a plurality of analysis points randomly selected in a view field of an image of a surface of the catalyst layer 8 taken and enlarged by a scanning type electron microscope. Then, a standard deviation σ is determined on measurements of F / C at the plurality of analysis points; σ falls in a range of 0.03≤σ≤0.05.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an air electrode for an air secondary battery and an air secondary battery including the air electrode. [Background technology]

[0002] In recent years, air batteries, which use oxygen in the air as the positive electrode active material, have been attracting attention because of their high energy density, small size, and ease of weight reduction, etc. Among such air batteries, zinc-air primary batteries have been put to practical use as power sources for hearing aids.

[0003] Additionally, research is being conducted on rechargeable air batteries that use Li, Zn, Al, Mg, etc. as the negative electrode metal, and such air secondary batteries are expected to become new secondary batteries with energy densities that exceed those of lithium-ion secondary batteries.

[0004] As one type of such air secondary battery, an air-hydrogen secondary battery is known, which uses an alkaline aqueous solution (alkaline electrolyte) as the electrolyte and hydrogen as the negative electrode active material (see, for example, Patent Document 1). Air-hydrogen secondary batteries as typified by Patent Document 1 use a hydrogen storage alloy as the negative electrode metal, but the negative electrode active material in air-hydrogen secondary batteries is hydrogen that is absorbed and released by the above-mentioned hydrogen storage alloy, so that no dissolution or deposition reaction of the hydrogen storage alloy itself occurs during chemical reactions (hereinafter also referred to as battery reactions) during charging and discharging in the battery. For this reason, air-hydrogen secondary batteries have the advantage that they do not cause problems such as internal short circuit caused by so-called dendrite growth, in which the negative electrode metal precipitates in a dendritic form, or a decrease in battery capacity caused by shape change.

[0005] In an air secondary battery that uses an alkaline electrolyte, such as the above-mentioned air hydrogen secondary battery, the following charge and discharge reactions occur in the positive electrode (hereinafter also referred to as the air electrode).

[0006] Charging (oxygen generation reaction): 4OH - →O2+2H2O+4e - (I) Discharge (oxygen reduction reaction): O2 + 2H2O + 4e - →4OH - (II)

[0007] As shown in reaction formula (I), oxygen is generated at the air electrode during charging in an air secondary battery. This oxygen passes through the voids inside the air electrode and is released into the atmosphere from the part of the air electrode that is open to the atmosphere. On the other hand, during discharging, oxygen taken in from the atmosphere is reduced to produce water as shown in reaction formula (II). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 4568124 Summary of the Invention [Problem to be solved by the invention]

[0009] However, the above-mentioned air secondary battery has not yet achieved a sufficiently high output, and therefore, in order to put the air secondary battery into practical use, there is a demand for a further increase in output.

[0010] A major factor preventing the above-mentioned increase in output is the large overvoltage during charging and discharging.

[0011] Here, in an air secondary battery, the charging reaction proceeds at a two-phase interface formed by a solid (catalyst) and a liquid (electrolyte), and the discharging reaction proceeds only at a three-phase interface where a solid (catalyst), a liquid (electrolyte), and a gas (oxygen) are simultaneously present. Therefore, in a dry state where the air electrode is not in contact with the electrolyte or in a state where it is completely immersed in the electrolyte, the overvoltage in one or both of the charging and discharging reactions may become extremely high. Therefore, in order to efficiently proceed with the charging and discharging reaction to reduce the overvoltage and increase the output of the air secondary battery, it is considered necessary to optimize the water repellency of the air electrode. However, the current situation is that there has not yet been sufficient research into optimizing the water repellency of the air electrode in an air secondary battery.

[0012] Regarding the optimization of the water repellency of electrodes, a lot of research has been done from the viewpoint of improving discharge performance (oxygen reduction reaction) in the field of fuel cells, for example. However, in air secondary batteries, it is necessary to take into account the charging reaction (oxygen generation reaction), and the water repellency and effects required in the field of fuel cells are completely different, so knowledge in the field of fuel cells cannot be directly applied.

[0013] The present invention has been made based on the above circumstances, and an object of the present invention is to provide an air electrode for an air secondary battery that can reduce overvoltage in charge and discharge reactions, and an air secondary battery including this air electrode. [Means for solving the problem]

[0014] In order to achieve the above object, according to the present invention, there is provided an air electrode for an air secondary battery, comprising a substrate and a catalyst layer supported on the substrate, the catalyst layer including a catalyst having a dual function of oxygen generation and oxygen reduction, a conductive material made of a carbon material that imparts electrical conductivity to the catalyst layer, and a water repellent made of a fluororesin that imparts water repellency to the catalyst layer, wherein, when the atomic percentage of carbon contained in the carbon material measured at a plurality of analysis points randomly selected within a field of view when the surface of the catalyst layer is magnified with a scanning electron microscope is C, the atomic percentage of fluorine contained in the fluororesin is F, the ratio of F to C is F / C, and σ is the standard deviation calculated based on the F / C for the plurality of points, σ ​​is in the range of 0.03≦σ≦0.05. Effect of the Invention

[0015] The air electrode for an air secondary battery according to the present invention is an air electrode for an air secondary battery comprising a substrate and a catalyst layer supported on the substrate, the catalyst layer comprising a catalyst having a dual function of oxygen generation and oxygen reduction, a conductive material made of a carbon material that imparts electrical conductivity to the catalyst layer, and a water repellent made of a fluororesin that imparts water repellency to the catalyst layer, and the surface of the catalyst layer is magnified with a scanning electron microscope. When the atomic percentage of carbon contained in the carbon material measured at a plurality of analysis points randomly selected within the field of view is C, the atomic percentage of fluorine contained in the fluororesin is F, the ratio of F to C is F / C, and the standard deviation calculated based on the F / C at the plurality of points is σ, the σ is in the range of 0.03≦σ≦0.05. An air electrode in which the standard deviation σ of F / C is in the range of 0.03≦σ≦0.05 can obtain an appropriate bias of the fluororesin in the air electrode. If the fluororesin is appropriately distributed in the air electrode, the two-phase interface required for the charging reaction and the three-phase interface required for the discharging reaction can be sufficiently secured, and the charging and discharging reactions can proceed efficiently. As a result, the overvoltage can be reduced, and the output of the air secondary battery can be increased. Therefore, according to the present invention, it is possible to provide an air electrode for an air secondary battery that can reduce the overvoltage in the charging and discharging reactions, and an air secondary battery that includes this air electrode and has a high output. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic diagram illustrating an air secondary battery according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing a cyclic voltammogram on the oxygen generation side. [Diagram 3] 1 is a graph showing a cyclic voltammogram on the oxygen reduction side. [Figure 4] 1 is a graph showing the relationship between polarization characteristics and standard deviation σ of F / C ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an air electrode 2 for an air secondary battery according to this embodiment and an air secondary battery (hereinafter also referred to as battery) 4 including this air electrode 2 will be described with reference to the drawings.

[0018] The air electrode 2 includes a substrate 6 and a catalyst layer 8 supported on the substrate 6, as shown in an enlarged view in FIG.

[0019] The substrate 6 is not particularly limited as long as it is a material that does not impede gas diffusion and can support the catalyst layer 8. Suitable examples of the substrate 6 include carbon-based porous substrates such as carbon paper, carbon fiber woven fabric, carbon fiber nonwoven fabric, carbon felt, and carbon cloth, and metal-based porous substrates such as metal foam, metal mesh, and expanded metal. In addition, these substrates may be impregnated with a water repellent agent made of a fluororesin to the extent that gas diffusion is not impeded, thereby imparting leakage resistance to the electrolyte.

[0020] The catalyst layer 8 contains a catalyst, a conductive material made of a carbon material that imparts electrical conductivity to the catalyst layer 8, and a water repellent made of a fluororesin that imparts water repellency to the catalyst layer 8.

[0021] The catalyst used has the dual functions of oxygen generation and oxygen reduction. Such a dual-function catalyst contributes to reducing the overvoltage of the battery during both the charging and discharging processes. As such an oxidation-reduction catalyst, for example, a pyrochlore-type bismuth ruthenium composite oxide is preferably used. This bismuth ruthenium composite oxide has the composition formula Bi2Ru2O 7-z (where z satisfies the relationship 0≦z≦1.)

[0022] Next, a method for producing a pyrochlore-type bismuth ruthenium composite oxide as a catalyst will be specifically described below.

[0023] Bi(NO3)3·5H2O and RuCl3·3H2O are added to distilled water so that they have the same concentration, and the solution is stirred to prepare a mixed solution of Bi(NO3)3·5H2O and RuCl3·3H2O. The temperature of the distilled water is 60°C to 90°C. Then, a 1mol / L to 3mol / L NaOH solution is added to this mixed solution. The bath temperature is kept at 60°C to 90°C, and the solution is stirred while bubbling oxygen. The solution containing the precipitate generated by this operation is kept at 80°C to 100°C to evaporate some of the water and form a paste. The paste is transferred to an evaporating dish, heated at 100°C to 150°C, and dried by keeping it in that state for 10 hours to 20 hours to obtain a dried paste. The dried product is then placed in a mortar and crushed with a pestle, then heated to a temperature of 350°C to 650°C in an air atmosphere and held for 0.5 hours to 24 hours to obtain a fired product. The fired product is washed with distilled water at a temperature of 60°C to 90°C and then dried. This produces a pyrochlore-type bismuth ruthenium composite oxide.

[0024] Next, it is preferable to immerse the prepared bismuth ruthenium composite oxide in an aqueous nitric acid solution to perform an acid treatment. Specifically, the procedure is as follows.

[0025] First, prepare an aqueous solution of nitric acid. Here, the concentration of the aqueous solution of nitric acid to be prepared is set to 5 mol / L or less, the amount is set to 20 mL per 1 g of bismuth ruthenium composite oxide, and the temperature is preferably set to 20° C. or more and 25° C. or less.

[0026] Then, the bismuth ruthenium composite oxide is immersed in the prepared nitric acid aqueous solution and stirred for 6 hours or less. After a predetermined time has passed, the bismuth ruthenium composite oxide is suction filtered from the nitric acid aqueous solution. The filtered bismuth ruthenium composite oxide is placed in distilled water or ion-exchanged water set to 60°C or higher and 80°C or lower and washed.

[0027] The washed bismuth ruthenium composite oxide is subjected to a drying treatment by being maintained in an environment of 100° C. or higher and 120° C. or lower for 1 hour or longer and 2 hours or shorter.

[0028] In this manner, an acid-treated bismuth ruthenium composite oxide is obtained. By carrying out the acid treatment in this manner, by-products generated during the manufacturing process of the bismuth ruthenium composite oxide can be removed. The acidic aqueous solution used in the acid treatment is not limited to an aqueous nitric acid solution, and in addition to the aqueous nitric acid solution, an aqueous hydrochloric acid solution or an aqueous sulfuric acid solution can be used. The aqueous hydrochloric acid solution and the aqueous sulfuric acid solution also have the effect of removing by-products, similar to the aqueous nitric acid solution.

[0029] The bismuth ruthenium composite oxide obtained as described above is mechanically pulverized to obtain a powder of the bismuth ruthenium composite oxide which is an aggregate of particles having a predetermined particle size.

[0030] Next, the carbon material as the conductive material may be graphite, carbon black, graphene, carbon nanotubes, carbon nanofibers, etc. In particular, it is preferable to use graphite from the viewpoint of oxidation resistance.

[0031] Next, the fluororesin as the water repellent is not particularly limited as long as it has stability against charge and discharge reactions. Preferred fluororesins include FEP (perfluoroethylene propene copolymer), PTFE (polytetrafluoroethylene), PFA (perfluoroalkoxyalkane polymer), ETFE (ethylene-tetrafluoroethylene copolymer), PVDF (polyvinylidene fluoride), PVF (polyvinyl fluoride), etc. In addition, the fluororesin not only serves to impart appropriate water repellency to the air electrode 2, but also serves to bond the constituent materials of the air electrode, such as catalyst particles and conductive materials, together.

[0032] The air electrode 2 can be produced, for example, as follows. First, a catalyst powder which is an aggregate of catalyst particles (bismuth ruthenium composite oxide particles), a carbon material powder which is an aggregate of carbon material particles as a conductive material, a fluororesin as a water repellent, and water are prepared. Then, the catalyst powder, the carbon material powder, the fluororesin, and the water are kneaded to prepare a catalyst layer mixture slurry.

[0033] The obtained catalyst layer mixture slurry is applied, for example, to one side of carbon paper of a predetermined size using a bar coater. This results in a composite of the catalyst layer slurry and carbon paper. This composite is then heated to 50°C to 80°C and held for 10 hours to 24 hours for drying treatment. After drying treatment, the composite is compressed while being heated by a hot press and then fired. This results in an air electrode 2 in which the carbon paper and the catalyst layer are bonded and integrated.

[0034] The method for applying the catalyst layer slurry is not limited to the use of a bar coater, and for example, a dip coating method, a spray coating method, a doctor blade method, a spin coating method, a screen printing method, or the like can be appropriately selected.

[0035] Here, the inventors have conducted intensive research to develop an air electrode for an air secondary battery that can reduce overvoltage in charge and discharge reactions. In the course of the research, a catalyst made of bismuth ruthenium composite oxide, a conductive material made of carbon material, and a water repellent made of fluororesin were kneaded to obtain a mixture slurry, which was applied onto carbon paper, and then the mixture was hot-pressed under different firing conditions to produce an air electrode. The composition of the surface of the obtained air electrode was analyzed, and a cyclic voltammetry (hereinafter also referred to as CV) evaluation of a battery incorporating the air electrode was performed to investigate the relationship between the bias of the fluororesin and the polarization characteristics. Conventionally, it was thought that the smaller the standard deviation of F / C, which is the ratio of the carbon concentration to the fluorine concentration, the better the CV polarization characteristics. However, as a result of the above investigation, it was found that the CV polarization characteristics deteriorate conversely when the standard deviation of F / C, which is the ratio of the carbon concentration to the fluorine concentration, falls below a certain value. This is thought to be because applying the fluororesin too uniformly reduces the two-phase interface required for the charge reaction or the three-phase interface required for the discharge reaction. From these results, it was discovered that a moderate bias in the fluororesin is necessary to obtain good charge / discharge characteristics.

[0036] Based on this knowledge, the air electrode of this embodiment is characterized in that the standard deviation σ is calculated based on the value of F / C, which is the ratio of the carbon concentration to the fluorine concentration on the surface of the catalyst layer, and this standard deviation σ is 0.03≦σ≦0.05. More specifically, in the air electrode of this embodiment, the atomic percentage of carbon contained in the carbon material and the atomic percentage of fluorine contained in the fluororesin are measured by analysis using energy dispersive X-ray spectroscopy (EDS) for multiple analysis points randomly selected within the field of view when the surface of the catalyst layer is enlarged with a scanning electron microscope (SEM). The atomic percentage of carbon obtained at this time is C, and the atomic percentage of fluorine obtained is F. The ratio of F to C is F / C, and the standard deviation σ is calculated based on the values ​​of F / C for the multiple points. In the air electrode of this embodiment, this standard deviation σ is within the range of 0.03≦σ≦0.05.

[0037] In the air electrode of this embodiment, if the standard deviation σ is less than 0.03, the fluororesin will be present in the catalyst layer excessively uniformly, reducing the two-phase interface required for the charge reaction or the three-phase interface required for the discharge reaction, and inhibiting the progress of good charge and discharge reactions. On the other hand, if the standard deviation σ is 0.03 or more, the fluororesin will be present in a moderately biased manner in the catalyst layer, increasing the two-phase interface required for the charge reaction and the three-phase interface required for the discharge reaction, and promoting the progress of good charge and discharge reactions. However, it is difficult to bias the fluororesin in the catalyst layer to such an extent that the standard deviation σ exceeds 0.05 in the current manufacturing method. Therefore, the upper limit of the standard deviation σ is set to 0.05.

[0038] Here, if the amount of fluororesin added to the catalyst layer is too small, it cannot provide good water repellency to the catalyst layer. On the other hand, if the amount of fluororesin added is too large, the value of σ drops drastically, and furthermore, it causes a drop in electrical conductivity and an obstruction of gas diffusion, so it is preferable that the amount of fluororesin is 10% by weight or more and 30% by weight or less of the entire catalyst layer. Also, if the amount of carbon material added to the catalyst layer is too small, it cannot provide good electrical conductivity to the catalyst layer. For this reason, it is preferable to add 20% by weight or more of the carbon material to the entire catalyst layer in order to ensure good electrical conductivity. However, if the amount of carbon material added is too large, the amount of catalyst is relatively reduced, making it difficult to proceed with good charge and discharge reactions. Therefore, it is preferable that the amount of carbon material added is 50% by weight or less of the entire catalyst layer.

[0039] Next, a three-electrode battery 4 that can be used for electrochemical measurements will be described below as an example of an air secondary battery incorporating the air electrode of this embodiment.

[0040] As shown in FIG. 1, the battery 4 includes a working electrode container 10, a reference electrode container 14 connected to the working electrode container 10 via a liquid junction 12, an air electrode 2 and a counter electrode 30 disposed in the working electrode container 10, and a reference electrode 16 disposed in the reference electrode container 14.

[0041] The working electrode container 10 is in the shape of an acrylic box, and a side wall opening 20 is provided in a part of the side wall 18. The side wall opening 20 has a shape similar to that of the air electrode 2 in a plan view, and is slightly smaller than the air electrode 2. The air electrode 2 is disposed so as to cover the side wall opening 20 from the outside of the side wall 18. In other words, the side wall opening 20 is closed by the air electrode 2. The periphery of the air electrode 2 is fixed by an acrylic frame member 22 from the outside of the working electrode container 10. The frame member 22 has an opening 24 in the center that has the same shape as the side wall opening 20, and is fixed to the side wall 18 of the working electrode container 10 by a screw 26. The base material 6 side of the air electrode 2 is positioned outside the working electrode container 10, and the catalyst layer 8 side is positioned inside the working electrode container 10. In other words, the catalyst layer 8 of the air electrode 2 is exposed inside the working electrode container 10, and the base material 6 is open to the atmosphere. In addition, a rubber gasket (not shown) is provided in the area where the air electrode 2 and the side wall 18 overlap, so that the catalyst layer 8 of the air electrode 2 is in close contact with the side wall 18 around the side wall opening 20, ensuring liquid-tightness.

[0042] An alkaline electrolyte 28 is stored inside the working electrode container 10. As described above, the catalyst layer 8 of the air electrode 2 is exposed to the inside of the working electrode container 10, and therefore the catalyst layer 8 of the air electrode 2 is in contact with the alkaline electrolyte 28.

[0043] In addition, a counter electrode 30 made of a nickel plate having an area sufficiently larger than that of the air electrode 2 is disposed in the working electrode container 10 at a position facing the air electrode 2. The counter electrode 30 is in a state where it is completely immersed in the alkaline electrolyte 28.

[0044] An air electrode lead 32 is electrically connected to the air electrode 2, and a counter electrode lead 34 is electrically connected to the counter electrode 30.

[0045] The reference electrode container 14 is a box-shaped container made of acrylic, and a lid 38 is fitted into an opening 36 at the top. An alkaline electrolyte 28 is stored inside the reference electrode container 14. The reference electrode 16 is disposed at a predetermined position on the lid 38. The reference electrode 16 is an Hg / HgO electrode, and approximately half of it is immersed in the alkaline electrolyte 28. The reference electrode container 14 is connected to the working electrode container 10 via a liquid junction 12 to eliminate the influence of a liquid junction potential difference. A reference electrode lead 40 is electrically connected to the reference electrode 16.

[0046] As the alkaline electrolyte 28, a typical alkaline electrolyte used in alkaline secondary batteries is suitably used, and specifically, an aqueous solution containing at least one of NaOH, KOH, and LiOH as a solute is used.

[0047] In the battery 4, oxygen is generated at the air electrode 2 by charging via the air electrode lead 32 and the counter electrode lead 34, and this oxygen is released into the atmosphere from the part of the substrate 6 that is open to the atmosphere through the inside of the air electrode 2. On the other hand, during discharge, oxygen taken in from the atmosphere via the part of the substrate 6 is reduced, causing a discharge reaction, and a discharge current can be output via the air electrode lead 32 and the counter electrode lead 34.

[0048] Here, the battery 4 of this embodiment is not limited to the above-mentioned three-electrode battery, and may be another air secondary battery having two electrodes, a positive electrode and a negative electrode. An example of such an air secondary battery is an air secondary battery that includes a container and an electrode group housed in the container together with an alkaline electrolyte, the electrode group including a positive electrode and a negative electrode stacked together with a separator interposed therebetween, and the positive electrode is the air electrode according to this embodiment. It is also possible to form an air hydrogen secondary battery that employs a negative electrode containing a hydrogen storage alloy as the negative electrode.

[0049] [Example] 1. Battery manufacturing Example 1 (1) Synthesis of air electrode catalyst 1) Co-precipitation process A certain amount of Bi(NO3)3·5H2O and RuCl3·3H2O was prepared, and these Bi(NO3)3·5H2O and RuCl3·3H2O were put into distilled water at 75°C so that the concentrations of these were the same, and stirred to prepare a mixed aqueous solution of Bi(NO3)3·5H2O and RuCl3·3H2O. Then, 2mol / L NaOH aqueous solution was added to this mixed aqueous solution. The bath temperature was 75°C, and the mixture was stirred while bubbling oxygen. The solution containing the precipitate generated by this operation was kept at 85°C to evaporate some of the water and form a paste. This paste was transferred to an evaporating dish, heated to 120°C, and kept in that state for 12 hours to dry, obtaining a dried paste (precursor).

[0050] 2) Firing process The dried product was placed in a mortar and crushed with a pestle, then heated to 600°C in an air atmosphere and held for 1 hour to obtain a fired product. The fired product was washed with distilled water at 70°C, filtered by suction, and dried at 120°C. This produced a pyrochlore-type bismuth ruthenium composite oxide.

[0051] The obtained bismuth ruthenium composite oxide was placed in a mortar and pulverized with a pestle to obtain a powder of bismuth ruthenium composite oxide, which is an aggregate of particles having a predetermined particle size. When the secondary electron image of this bismuth ruthenium composite oxide powder was observed with a scanning electron microscope, the particle size of the bismuth ruthenium composite oxide was found to be 0.1 μm or less.

[0052] 3) Acid treatment process A nitric acid aqueous solution adjusted to a concentration of 2 mol / L and a powder of bismuth ruthenium composite oxide were placed in a stirring tank of a stirrer, and stirred for 1 hour while maintaining the temperature of the nitric acid aqueous solution at 25° C. At this time, the amount of the nitric acid aqueous solution was adjusted so that the ratio of the nitric acid aqueous solution was 20 mL per 1 g of the bismuth ruthenium composite oxide powder.

[0053] After the stirring was completed, the bismuth ruthenium composite oxide powder was taken out from the nitric acid aqueous solution by suction filtration. The taken out bismuth ruthenium composite oxide powder was washed with 1 liter of distilled water heated to 70°C. After washing, the bismuth ruthenium composite oxide powder was dried by heating to 120°C.

[0054] In this manner, a powder of acid-treated bismuth ruthenium composite oxide (Bi2Ru2O7) was obtained.

[0055] (2) Manufacturing of air electrodes 50 parts by mass of the bismuth ruthenium composite oxide powder obtained as described above, 30 parts by mass of high-purity natural graphite powder (SNO-1T manufactured by SEC Carbon Co., Ltd., average particle size 1 to 2 μm) as a carbon material, 20 parts by mass of FEP dispersion (perfluoroethylene propene copolymer 120-JRB manufactured by Mitsui-Chemours Fluoro Products Co., Ltd., average particle size 0.2 μm) as a fluororesin converted into solid content ratio, 10 parts by mass of ethanol, and 70 parts by mass of ion-exchanged water were prepared and charged into the stirring vessel of a planetary centrifugal mixer. Then, the planetary centrifugal mixer was driven to mix and stir the mixture to obtain a catalyst layer mixture slurry with a solid content ratio of 50%.

[0056] Next, the catalyst layer mixture slurry obtained as described above was applied to a carbon paper substrate (GDL29BA manufactured by SGL Carbon Co., Ltd., basis weight: 36 g / m 2 A composite of the catalyst layer slurry and carbon paper was formed by applying the slurry to a carbon paper (thickness: 173 μm) using a bar coater with a wire diameter of 50 μm. The composite was then dried at 60°C for 12 hours, and then compressed while being heated by a hot press, and subjected to a firing treatment. At this time, the pressing pressure was 15 kgf / cm. 2 The carbon paper and the catalyst layer were bonded and integrated to obtain an air electrode 2. The resulting air electrode 2 had an electrode area of ​​40 mm length, 40 mm width, and 0.15 mm thickness, and the catalyst amount was 2.7 mg / cm. 2Two air electrodes 2 were prepared, one for analysis and the other for battery assembly.

[0057] (3) Battery assembly A working electrode container 10 made of acrylic and having a side wall opening 20 in a part of a side wall 18, and an air electrode 2 for assembling a battery were prepared. The side wall opening 20 was a square shape of 35 mm in length and 35 mm in width. The air electrode 2 was then attached to cover the side wall opening 20. At this time, the air electrode 2 was arranged so that the catalyst layer 8 side faces the inside of the working electrode container 10 and the substrate 6 side faces the outside of the working electrode container 10, closing the side wall opening 20. The periphery of the air electrode 2 was then fixed from the outside of the working electrode container 10 by an acrylic frame member 22. The frame member 22 had an opening 24 in the center that was the same shape as the side wall opening 20, and was fixed to the side wall 18 of the working electrode container 10 by screws 26. In addition, a rubber gasket (not shown) is provided in the area where the side wall 18 of the working electrode container 10 and the air electrode 2 overlap, so that the catalyst layer 8 of the air electrode 2 is in close contact with the side wall 18 around the side wall opening 20, ensuring liquid-tightness.

[0058] Furthermore, inside the working electrode container 10, a counter electrode 30 made of a nickel plate and having a rectangular shape of 100 mm in length and 100 mm in width was disposed at a position facing the air electrode 2.

[0059] Thereafter, a predetermined amount of alkaline electrolyte 28 was poured into the working electrode container 10. A 5 mol / L KOH aqueous solution was used as the alkaline electrolyte 28. The counter electrode 30 was in a state of being completely immersed in the alkaline electrolyte 28. In addition, since the catalyst layer 8 of the air electrode 2 was exposed to the inside of the working electrode container 10, the catalyst layer 8 of the air electrode 2 was in contact with the alkaline electrolyte 28. On the other hand, the substrate 6 side of the air electrode 2 was exposed to the atmosphere.

[0060] An air electrode lead 32 was electrically connected to the air electrode 2, and a counter electrode lead 34 was electrically connected to the counter electrode 30, respectively.

[0061] Next, an acrylic box-shaped reference electrode container 14 was prepared. The reference electrode container 14 had an opening 36 at the top, and a predetermined amount of alkaline electrolyte 28 was poured into the reference electrode container 14 through the opening 36. A 5 mol / L KOH aqueous solution was used as the alkaline electrolyte 28. The opening 36 was closed with a lid 38. A reference electrode 16 was disposed at a predetermined position on the lid 38. The reference electrode 16 was an Hg / HgO electrode, and was in a state where almost half of it was immersed in the alkaline electrolyte 28. The reference electrode container 14 was connected to the working electrode container 10 via a liquid junction 12 in order to eliminate the influence of the liquid junction potential difference. A reference electrode lead 40 was electrically connected to the reference electrode 16. In this manner, the battery 4 shown in FIG. 1 was manufactured.

[0062] Example 2 An air electrode and a battery were produced in the same manner as in Example 1, except that the sintering temperature in the hot press was 200°C.

[0063] Example 3 An air electrode and a battery were produced in the same manner as in Example 1, except that the firing conditions in the hot press were changed to 200° C. and 1 minute.

[0064] Comparative Example 1 An air electrode and a battery were produced in the same manner as in Example 1, except that the sintering temperature in the hot press was 250°C.

[0065] Comparative Example 2 An air electrode and a battery were produced in the same manner as in Example 1, except that the firing conditions in the hot press were 300° C. and 1 minute.

[0066] Comparative Example 3 An air electrode and a battery were produced in the same manner as in Example 1, except that the firing time in the hot press was 1 minute.

[0067] Comparative Example 4 An air electrode and a battery were produced in the same manner as in Example 1, except that the firing conditions in the hot press were 250° C. and 1 minute.

[0068] 2. Evaluation of air electrodes and air secondary batteries (1) SEM / EDS analysis of the air electrode The air electrodes for analysis were observed with a scanning electron microscope (SEM) and subjected to elemental analysis by energy dispersive X-ray spectroscopy (EDS), a so-called SEM / EDS analysis, in which a scanning electron microscope (JSM-6510) and an energy dispersive X-ray analyzer (JED-2300) manufactured by JEOL Ltd. were used as the analytical equipment for the SEM / EDS analysis.

[0069] As a specific analysis procedure, first, a rectangular sample with a length of 1 cm and a width of 1 cm was cut out from the air electrodes for analysis of Examples 1 to 3 and Comparative Examples 1 to 4. Then, this sample was fixed on a carbon tape, and the surface morphology was observed by magnifying it up to 1000 times at an acceleration voltage of 15 keV using a scanning electron microscope (SEM). Then, 20 analysis points randomly selected within the field of view at a magnification of 1000 times were analyzed. Quantitative analysis was performed at each analysis point by dispersing the characteristic X-rays generated at that time. Note that, when an electron beam is irradiated to each analysis point, the range that is effectively analyzed is estimated to be a range of about 3 μm in diameter from the analysis point based on the experimental conditions. The ratios of fluorine and carbon when the abundance of all atoms obtained by the quantitative analysis was taken as 100% were converted to the number of atoms to obtain the atomic percentage of fluorine and the atomic percentage of carbon. Then, the ratio represented by F / C, where the atomic percentage of fluorine is F and the atomic percentage of carbon is C, was obtained for each analysis point 1 to 20. The results are shown in Table 1.

[0070] Next, the standard deviation σ was calculated from the F / C values ​​of analysis points 1 to 20. The results are shown in Tables 1 and 2.

[0071] [Table 1]

[0072] (2) Electrochemical measurements Electrochemical measurements were carried out by cyclic voltammetry using the air secondary batteries of Examples 1 to 3. The oxygen reduction reaction was evaluated with a sweep potential of -0.35 to 0.1 V and a sweep rate of 5 mV / sec, and the oxygen evolution reaction was evaluated with a sweep potential of 0.1 to 0.65 V and a sweep rate of 5 mV / sec. In a cyclic voltammogram with the applied potential on the horizontal axis and the current density in response on the vertical axis, the maximum current density was 10 mA / cm. 2 The positive electrode potential corresponding to the current value is the oxygen evolution potential (E OER ), -10mA / cm 2 The positive electrode potential corresponding to the current value is the oxygen reduction potential (E ORR ) and E OER and E ORR The polarization characteristic (ΔE) was calculated from the difference between the two. The smaller the polarization characteristic value, the more efficiently the charge and discharge reaction is progressing.

[0073] Electrochemical measurements were also performed by cyclic voltammetry on the air secondary batteries of Comparative Examples 1 to 4. However, for the air secondary batteries of Comparative Examples 1 to 4, electrochemical measurements were performed in the same manner as in Example 1, except that the sweep potential in the evaluation of the oxygen reduction reaction was changed to -0.5 to 0.1 V.

[0074] [Table 2]

[0075] (3) Results and Discussion The F / C ratio and standard deviation σ of each analysis point calculated from the quantitative analysis results by EDS are summarized in Table 1. Here, the standard deviation σ of the F / C ratio indicates the degree of uneven distribution of F, and it can be seen that the σ values ​​are higher than 0.03 in Examples 1 to 3, while the σ values ​​are smaller than 0.03 in Comparative Examples 1 to 4.

[0076] Figures 2 and 3 show cyclic voltammograms for the oxygen evolution side and the oxygen reduction side, respectively. In Figure 2, a response current is seen when the air electrode potential is applied in the noble direction; this is a reaction current associated with oxygen evolution; the higher the current value at a lower potential, the more efficiently the oxidation reaction is progressing. On the other hand, in Figure 3, a response current is seen when the air electrode potential is applied in the noble direction; this is a reaction current associated with oxygen reduction. The current value shows a negative value, but this is due to the reduction reaction. This shows that the higher the current value at a higher potential, the more efficiently the reduction reaction is progressing.

[0077] Table 2 shows the oxygen evolution potential (E OER ), oxygen reduction potential (E ORR ), polarization characteristics (ΔE), and standard deviation σ of the F / C ratio are summarized. The relationship between the standard deviation σ of the F / C ratio and ΔE is also shown in FIG. 4. It can be seen that Examples 1 to 3, which showed good polarization characteristics, had σ values ​​higher than 0.03, while Comparative Examples 1 to 4, which showed high ΔE, had σ values ​​lower than 0.03. From this, it is considered that a moderate bias in the fluororesin is necessary to obtain good polarization characteristics, and that if fluorine is applied excessively uniformly, the two-phase interface required for the charge reaction or the three-phase interface required for the discharge reaction will decrease.

[0078] On the other hand, if the degree of uneven distribution of fluorine is too high, the water repellency will be insufficient in some places, and the electrolyte will seep into the substrate side, blocking the pores and reducing gas diffusion, resulting in a decrease in discharge performance. For this reason, it is considered appropriate for the σ value to be 0.03 or more and 0.05 or less. Also, if too much fluororesin is added, the σ value will drop drastically, and it will also cause a decrease in conductivity and inhibition of gas diffusion, so it is considered appropriate for the fluororesin to be 10 to 30% by weight of the entire catalyst layer. Also, in order to ensure the conductivity of the catalyst layer, it is considered appropriate for the carbon material to be 20% by weight or more of the entire catalyst layer.

[0079] <Aspects of the present invention> A first aspect of the present invention is an air electrode for an air secondary battery comprising a substrate and a catalyst layer supported on the substrate, the catalyst layer including a catalyst having a dual function of oxygen generation and oxygen reduction, a conductive material made of a carbon material that imparts electrical conductivity to the catalyst layer, and a water repellent made of a fluororesin that imparts water repellency to the catalyst layer, wherein, when the surface of the catalyst layer is magnified with a scanning electron microscope, the atomic percentage of carbon contained in the carbon material measured at a plurality of analysis points randomly selected within a field of view is taken as C, the atomic percentage of fluorine contained in the fluororesin is taken as F, the ratio of F to C is taken as F / C, and σ is the standard deviation calculated based on the F / C for the plurality of points, σ ​​is in the range of 0.03≦σ≦0.05.

[0080] According to the first aspect, an appropriate bias of the fluororesin can be obtained in the air electrode. If the fluororesin is appropriately biased in the air electrode, a two-phase interface required for the charge reaction and a three-phase interface required for the discharge reaction can be sufficiently secured, and the charge and discharge reactions can be efficiently promoted.

[0081] A second aspect of the present invention relates to an air electrode for an air secondary battery, wherein the catalyst layer in the first aspect of the present invention contains 10% by weight or more and 30% by weight or less of the fluororesin and 20% by weight or more of the carbon material.

[0082] According to the second aspect, it is possible to prevent the conductivity of the air electrode from decreasing and the gas diffusion from being hindered.

[0083] A third aspect of the present invention relates to an air electrode for an air secondary battery, in which the catalyst is a pyrochlore-type bismuth ruthenium composite oxide in the first or second aspect of the present invention described above.

[0084] According to the third aspect, the pyrochlore-type bismuth ruthenium composite oxide has the dual functions of oxygen generation and oxygen reduction, which contributes to reducing the overvoltage of the battery both during the charging and discharging processes and can contribute to increasing the output of air secondary batteries.

[0085] A fourth aspect of the present invention relates to an air secondary battery comprising a container, an electrolytic solution stored in the container, a negative electrode disposed in the electrolytic solution, and a positive electrode having one surface exposed to the outside of the container and open to the atmosphere and having another surface opposite to the one surface positioned inside the container and in contact with the electrolytic solution, wherein the positive electrode is an air electrode for the air secondary battery of any of the first to third aspects of the present invention.

[0086] According to the fourth aspect, it is possible to obtain an air secondary battery having a high output, which includes an air electrode for an air secondary battery capable of reducing overvoltage in charge / discharge reactions. [Explanation of symbols]

[0087] 2 Air electrode 4. Batteries (secondary air batteries) 6 Base material 8 Catalyst layer 10 Working electrode container 12 Liquid junction 14 Reference electrode container 16 Reference pole 28 Alkaline electrolyte 30 Opposite

Claims

1. An air electrode for an air secondary battery comprising a substrate and a catalyst layer supported on the substrate, the catalyst layer includes a catalyst having a dual function of oxygen generation and oxygen reduction, a conductive material made of a carbon material that imparts electrical conductivity to the catalyst layer, and a water repellent made of a fluororesin that imparts water repellency to the catalyst layer; an air electrode for an air secondary battery, wherein C is the atomic percentage of carbon contained in the carbon material, F is the atomic percentage of fluorine contained in the fluororesin, and F / C is the ratio of F to C, as measured at a plurality of analysis points randomly selected within a field of view when the surface of the catalyst layer is magnified with a scanning electron microscope, and σ is the standard deviation calculated based on the F / C at the plurality of points, where σ is in the range of 0.03≦σ≦0.

05.

2. 2. The air electrode for an air secondary battery according to claim 1, wherein the catalyst layer contains 10% by weight to 30% by weight of the fluororesin and 20% by weight or more of the carbon material.

3. 3. The air electrode for an air secondary battery according to claim 1, wherein the catalyst is a pyrochlore-type bismuth ruthenium composite oxide.

4. A container; An electrolyte solution stored in the container; a negative electrode disposed in the electrolyte; a positive electrode having one surface exposed to the outside of the container and open to the atmosphere, and another surface located opposite to the one surface, positioned inside the container and in contact with the electrolyte; The positive electrode is an air electrode for an air secondary battery according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Controlling the polymer surface distribution on the diffusion medium for improved fuel cell performance

    JP2007508677A

  • Hydrogen / air secondary battery

    JP2012064477A

  • Air magnesium battery

    JP2015125830A

  • Air electrode and metal-air battery

    JP2021048025A

  • Air electrode and air secondary battery using the air electrode

    JP4568124B2