Polyimide-based binder for power storage device, electrode mixture paste, negative electrode active material layer, negative electrode sheet for power storage device, and power storage device
A high-retention polyimide binder addresses the volume change issues in power storage devices, improving cycle characteristics and mechanical properties for industrial applications.
Patent Information
- Application Number
- JP2021509622
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-27
- Filing Date
- 2020-03-27
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Conventional polyimide binders used in power storage devices, particularly those with high charge/discharge capacity materials like silicon, suffer from volume changes leading to interfacial peeling and poor cycle characteristics, making them unsuitable for industrial applications such as electric/hybrid vehicles and all-solid-state batteries.
A polyimide binder with a repeated breaking energy retention rate of 70% or more, formed by heating or chemically imidizing a polyamic acid solution containing specific repeating units, exhibits excellent mechanical properties and maintains functionality even under high volume changes.
The polyimide binder significantly improves the cycle characteristics and mechanical properties of power storage devices, enhancing their capacity and durability, especially in all-solid-state batteries.
Smart Images

Figure 0007572944000001 
Figure 0007572944000002 
Figure 0007572944000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyimide-based binder for an electricity storage device, an electrode mixture paste, a negative electrode active material layer, a negative electrode sheet for an electricity storage device, and an electricity storage device. [Background technology]
[0002] Electricity storage devices, such as lithium secondary batteries, have a high energy density and a high capacity, and are therefore widely used as the driving power source for mobile information terminals. In recent years, industrial applications, such as installation in electric and hybrid vehicles and unmanned aerial vehicles, have been considered, and efforts are being made to further increase the capacity of electricity storage devices. As an example of increasing capacity, in the case of the negative electrode that constitutes the electricity storage device, studies are being made to increase the charge and discharge capacity by using silicon or tin, which have a large amount of lithium occluded per unit volume, or alloys containing these.
[0003] However, it is known that electrode active materials with large charge / discharge capacities, such as silicon, tin, or alloys containing these, undergo a very large volume change during charging and discharging. Therefore, when these electrode active materials are used to form a negative electrode active material layer with a general-purpose binder such as polyvinylidene fluoride or a rubber-based resin, the negative electrode active material layer suffers from layer destruction or interfacial peeling between the current collector and the negative electrode active material layer due to the volume change of the electrode active material, resulting in a problem of reduced cycle characteristics of the electricity storage device.
[0004] To address these issues, a method has been proposed to improve the deterioration of cycle characteristics caused by volume changes during repeated charging and discharging, in which silicon-based particles with an average particle size of 1 to 10 microns are bound together using polyimide, which has excellent mechanical properties, and then subjected to thermal pressure treatment to form a negative electrode active material layer (Patent Documents 1 to 5).
[0005] It has been pointed out that in negative electrodes using the polyimides disclosed in these patent documents as binders, cracks occur in the negative electrode active material layer when the electrodes are charged and discharged, forming island-like structures with spaces that can absorb the volume expansion during charging, thereby improving the capacity retention rate during repeated charging and discharging (Non-Patent Document 1). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2004 / 004031 [Patent Document 2] JP 2004-235057 A [Patent Document 3] JP 2003-203637 A [Patent Document 4] JP 2004-288520 A [Patent Document 5] JP 2004-022433 A [Non-patent literature]
[0007] [Non-Patent Document 1] Proceedings of the 48th Battery Symposium, 2B23, p.238 (2007) (Yasuo Takano et al.) Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the previously disclosed power storage devices equipped with a negative electrode using polyimide as a binder, although some improvement in capacity and cycle characteristics was observed, it was not possible to realize high capacity and high cycle characteristics sufficient for practical use in industrial applications such as electric and hybrid vehicles and unmanned aerial vehicles.
[0009] In addition, since all-solid-state batteries do not have a liquid layer that acts as a buffer, it has been difficult for conventionally disclosed polyimides to fully exhibit the functions required for all-solid-state batteries, such as mechanical properties and battery properties.
[0010] Therefore, the present invention is intended to solve the above problems, and has an object to provide a polyimide-based binder for an electricity storage device that can further improve the battery capacity and cycle characteristics, and also to provide a polyimide-based binder for an electricity storage device that can achieve excellent high capacity, cycle characteristics, and mechanical characteristics even in an all-solid-state battery. [Means for solving the problem]
[0011] As a result of extensive investigations, the present inventors have found that the cycle characteristics and mechanical characteristics of a high-capacity electricity storage device are related to the fracture energy of a binder used in an electrode. Thus, the present invention particularly relates to the following items.
[0012] [1] A polyimide binder for power storage devices that has a repeated fracture energy retention rate of 70% or more.
[0013] [2] The polyimide-based binder for an electricity storage device according to item 1, wherein the melting point of the binder is higher than 300° C. or is substantially nonexistent.
[0014] [3] The polyimide-based binder for an electricity storage device according to item 1 or 2 above, obtained by heating or chemically imidizing a polyamic acid solution containing a repeating unit represented by the following general formula (I):
[0015] [ka] (In the formula, A is one or more tetravalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more. B is one or more divalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more.)
[0016] [4] The polyimide binder for an electricity storage device according to item 3, wherein in general formula (I), 50 mol % or more of the groups A and B are linear aliphatic groups.
[0017] [5] The polyimide-based binder for an electricity storage device according to item 3 or 4, wherein in general formula (I), 50 mol % or more of A are groups represented by the following general formula (II):
[0018] [ka] (In the formula, X is a single bond or an oxygen atom, n is an integer from 0 to 2, and when n is 1 or 2, X may be the same or different.)
[0019] [6] A resin composition for a binder, which contains a polyamic acid having a repeating unit represented by the following general formula (I) and a solvent, and which can form the polyimide-based binder for an electricity storage device according to any one of items 1 to 5 above through an imidization reaction:
[0020] [ka] (In the formula, A is one or more tetravalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more. B is one or more divalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more.) [7] A negative electrode active material layer comprising the binder resin composition according to item 6 above and an electrode active material.
[0021] [8] A negative electrode active material layer comprising the binder for an electricity storage device according to any one of items 1 to 5 above and an electrode active material.
[0022] [9] A negative electrode sheet for an electricity storage device, comprising the negative electrode active material layer according to item 8 formed on a surface of a current collector.
[0023]
[10] An electricity storage device comprising the negative electrode sheet for an electricity storage device according to item 9 above. Effect of the Invention
[0024] According to the present invention, it is possible to provide a polyimide-based binder having a repeated breaking energy retention rate of 70% or more, which is useful for improving the characteristics of an electricity storage device. Since such a polyimide-based binder exhibits suitable physical behavior for an electricity storage device, it can be used as a binder for various members of the electricity storage device, such as a negative electrode active material layer and a negative electrode sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] <Polyimide binder> The polyimide binder of the present invention is characterized by having a repeated breaking energy retention of 70% or more.
[0026] The repeated breaking energy retention rate in the present invention refers to a value represented by the following formula. Repeated breaking energy retention rate = (TEB 200-10 ) / (TEB0) (Here, (TEB0) is the initial value of the tensile breaking energy calculated by performing a tensile breaking test according to a method conforming to ASTM D882, and (TEB 200-10) refers to the tensile breaking energy calculated by conducting a tensile breaking test after repeating 10% strain 200 times. It is also simply called the 10% repeated breaking energy retention. Similarly, the retention rate after repeating 20% strain 200 times is called the 20% repeated breaking energy retention, and (TEB 200-20 The retention rate after 200 cycles of 30% strain is called the 30% repeated breaking energy retention rate, (TEB 200-30 It can also be expressed as
[0027] The polyimide-based binder of the present invention has a repeated breaking energy retention rate of 70% or more, and therefore can improve the function as an electricity storage device while maintaining mechanical properties. In particular, the repeated breaking energy retention rate is preferably 75% or more, 80% or more, 85% or more, or 90% or more. In other words, the higher the repeated breaking energy retention rate, the higher the function such as high cycle characteristics can be expressed at a high level without impairing mechanical properties even when a negative electrode active material with a high volume change rate is used in large amounts. Depending on the use of the electricity storage device, a 20% repeated breaking energy retention rate of 60% or more, more preferably 70% or more, and particularly 80% or more may be an additional indicator. Depending on the use of the electricity storage device, a 30% repeated breaking energy retention rate of 50% or more, preferably 60% or more, and more preferably 70% or more may be an additional indicator.
[0028] In this way, by using the repeated fracture energy retention rate, the numerical values and standards of the elements of the test conditions, such as the strain value (e.g., whether to use a "10%" strain or a "20%" strain), the fracture energy value, the number of repetitions, and the retention rate, can be appropriately determined according to the purpose, and by using this as one of the indicators, it is possible to develop a polyimide-based binder that meets the required characteristics of an electricity storage device.
[0029] From another viewpoint, the polyimide-based binder of the present invention preferably has a melting point of more than 300° C. or is substantially free of melting point. In particular, it is more preferable that the melting point is more than 330° C. or is substantially free of melting point. By providing the polyimide-based binder with such properties, it can be suitably used even in industrial applications where it may be used in high-temperature environments.
[0030] The polyimide binder of the present invention refers to a polymeric compound in which the repeating units containing imide bonds account for 50 mol % or more of the total repeating units. Polymers capable of forming such polyimide binders include, for example, polymeric compounds having groups capable of forming imide bonds in the main chain by heating or chemical reaction, such as polyamic acids, particularly polyamic acids containing preferably 50 mol % or more, more preferably 70 mol % or more, and even more preferably 90 mol % or more of repeating units represented by the following formula (I):
[0031] [ka] (In the formula, A is one or more tetravalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more. B is one or more divalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more.)
[0032] The chemical structure of the polyimide binder is preferably such that the polyimide binder contains, for example, 50% or more, preferably 70% or more, and more preferably 90% or more of repeating units represented by the following general formula (III).
[0033] [ka] (In the formula, X1 is one or more tetravalent groups selected from groups having an aromatic ring, chain aliphatic groups, and groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more. Y1 is one or more divalent groups selected from groups having an aromatic ring, chain aliphatic groups, and groups having an alicyclic structure, which may be substituted with halogen, and these may be the same or two or more.)
[0034] Such polyimide-based binders can be prepared by using a known method from a tetracarboxylic acid component having the A structure of formula (I) or the X1 structure of formula (III) and a diamine component having the B structure of formula (I) or the Y1 structure of formula (III) as essential components, and other components as required.
[0035] The tetracarboxylic acid component is not particularly limited, but examples thereof include 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, diphenylsulfonetetracarboxylic dianhydride, p-terphenyltetracarboxylic dianhydride, m-terphenyltetracarboxylic dianhydride, and the like. aromatic tetracarboxylic dianhydrides such as cyclobutane-1,2,3,4-tetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, dicyclohexyl-3,3',4,4'-tetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, dicyclohexyl-1,2:4,5-dianhydride, bicyclo[2.2.2]oct-7-ene-2,3:5,6-tetracarboxylic dianhydride, and other alicyclic tetracarboxylic dianhydrides; 4,4'-(Hexafluoroisopropylidene)diphthalic anhydride, 3,3'-(Hexafluoroisopropylidene)diphthalic anhydride, 5,5'-[2,2,2-trifluoro-1-[3-(trifluoromethyl)phenyl]ethylidene]diphthalic anhydride, 5,5'-[2,2,3,3,3-pentafluoro-1-(trifluoromethyl)pyropyridene]diphthalic anhydride, 1H-difuro[3,4-b:3',4'-i]xanthene-1,3, Preferred examples of the halogen-substituted tetracarboxylic acid dianhydrides include 7,9(11H)-tetrone, 5,5'-oxybis[4,6,7-trifluoro-pyromellitic anhydride], 3,6-bis(trifluoromethyl)pyromellitic dianhydride, 4-(trifluoromethyl)pyromellitic dianhydride, 1,4-difluoropyromellitic dianhydride, and 1,4-bis(3,4-dicarboxytrifluorophenoxy)tetrafluorobenzene dianhydride. These may be used alone or in combination.
[0036] Depending on the application of the electricity storage device, it is preferable to use a polyimide-based binder in which A or X1 in formula (I) or formula (III) contains 50 mol % or more of a group represented by the following formula (II).
[0037] [ka] (In the formula, X is a single bond or an oxygen atom, n is an integer from 0 to 2, and when n is 1 or 2, X may be the same or different.)
[0038] The diamine component is not particularly limited, but may be an aromatic diamine such as p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 2,4-toluenediamine, 3,3'-dihydroxy-4,4'-diaminobiphenyl, bis(4-amino-3-carboxyphenyl)methane, or 2,4-diaminotoluene; 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,3,5,6-tetrafluoro-1,4-diaminobenzene, 2,4,5,6-tetrafluoro-1,3-diaminobenzene, 2,3,5,6-tetrafluoro-1,4-benzene(dimethanamine), 2,2'-difluoro(1,1'-biphenyl)-4,4'-diamine, 4,4'-diaminooctafluorobiphenyl, or 2,2-bis(4-aminophenyl)hexafluoropropane. , 4,4'-oxybis(2,3,5,6-tetrafluoroaniline) and other halogen-substituted diamines; alicyclic diamines which may be substituted with halogen, such as trans-1,4-diaminocyclohexane, cis-1,4-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane; linear chain aliphatic diamines, such as 1,4-tetramethylenediamine, 1,5-pentamethylenediamine, 1,6-hexamethylenediamine, 1,7-heptamethylenediamine, 1,8-octamethylenediamine, 1,9-nonamethylenediamine, 1,10-decamethylenediamine, 1,11-undecamethylenediamine and 1,12-dodecamethylenediamine; and linear chain aliphatic diamines having a branched structure in which these linear aliphatic diamines are substituted with alkyl groups. These diamines may be used alone or in combination. In one embodiment of the present invention, the diamine component preferably contains a chain aliphatic diamine having a linear or branched structure, and can be contained in an amount of preferably 40 mol % or more, more preferably 50 mol % or more, even more preferably 60 mol % or more, and even more preferably 70 mol % or more, and may be 100 mol %.The number of carbon atoms in the chain aliphatic diamine is preferably 2 or more, more preferably 6 or more, and even more preferably 8 or more, and is, for example, 22 or less, preferably 18 or less. The chain aliphatic diamine is preferably linear, but in the case of a branched chain, it is preferable that the number of carbon atoms in the linear portion (i.e., the number of carbon atoms bonding two amino groups) is the above-mentioned carbon number.
[0039] Also, a known dicarboxylic acid component may be added in a ratio of less than 50 mol % per 1 mol of tetracarboxylic acid so as to form an ester bond, or various repeating units may be introduced using a diamine having a polyether structure, a diamine having a polysiloxane structure, a diamine having a carbonate structure, etc. Such a structure may be appropriately determined depending on the application, function, etc. of the electricity storage device.
[0040] <Binder Resin Composition> The resin composition for binder, which is one embodiment of the present invention, contains at least a polyamic acid capable of forming a polyimide-based binder and a solvent, and can form the above-mentioned polyimide-based binder. The polyamic acid is dissolved in a solvent, and the solid content concentration (polyimide-equivalent concentration) is preferably in the range of 5 to 45 mass %. The polyamic acid includes a polyamic acid containing a repeating unit represented by the above formula (I) at preferably 50 mol % or more, preferably 70 mol % or more, more preferably 90 mol % or more. The resin composition for binder can be prepared by reacting a tetracarboxylic acid component having the A structure of formula (I) and a diamine component having the B structure of formula (I) as essential components, and other components as necessary, in a solvent. Specific examples of the tetracarboxylic acid component and the diamine component are as described above in the section on <polyimide-based binder>. The reaction liquid may be used as it is as a resin composition for binder, or may be concentrated or diluted as necessary.
[0041] Examples of the solvent include aromatic hydrocarbons such as xylene, toluene, and ethylbenzene; aliphatic hydrocarbons such as pentane, hexane, and heptane; non-polar solvents such as benzoic acid esters such as methyl benzoate, ethyl benzoate, and propyl benzoate; water, methanol, ethanol, acetone, N,N-dimethylformamide, dimethylamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, and hexamethylphosphonic acid. Lotriamide, 1,2-dimethoxymethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, tetrahydrofuran, bis[2-(2-methoxyethoxy)ethyl]ether, 1,4-dioxane, dimethyl sulfoxide, dimethyl sulfone, diphenyl ether, sulfolane, diphenyl sulfone, tetramethylurea, anisole, m-cresol, phenol, and γ-butyrolactone are preferred, and water, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and γ-butyrolactone are particularly preferred.
[0042] The binder resin composition may contain additives other than the electrode active material, which will be described in the next section "Electrode Mixture Paste".
[0043] <Electrode mixture paste> The electrode mixture paste according to one embodiment of the present invention is a composition containing a polyamic acid, an electrode active material, and a solvent. The polyamic acid may be any polyamic acid capable of forming the polyimide-based binder of the present invention.
[0044] The electrode active material that can be used in the electrode mixture paste of the present invention can be suitably a known one. The polyimide-based binder of the present invention can be used in either the negative electrode or the positive electrode. Therefore, the electrode active material may be either the negative electrode active material or the positive electrode active material. Usually, the effect of using the polyimide-based binder of the present invention is greater in the negative electrode. In this case, the electrode active material includes a negative electrode active material. As the electrode active material, for example, a lithium-containing metal composite oxide, a carbon powder, a silicon powder, a tin powder, or an alloy powder containing silicon or tin is preferable. The amount of the electrode active material in the electrode mixture paste is not particularly limited, but is usually 0.1 to 1000 times, preferably 1 to 1000 times, more preferably 5 to 1000 times, and even more preferably 10 to 1000 times, based on the mass of the electrode binder resin composition. If the amount of the electrode active material is too large, the electrode active material is not sufficiently bound to the current collector and is likely to fall off. On the other hand, if the amount of the electrode active material is too small, the negative electrode active material layer formed on the current collector will have many inactive portions, which may result in an insufficient function as an electrode.
[0045] Examples of negative electrode active materials for power storage devices, such as lithium secondary batteries, include lithium metal, lithium alloys, and carbon materials capable of absorbing and releasing lithium (e.g., graphitizable carbon, non-graphitizable carbon with a (002) plane spacing of 0.37 nm or more, and graphite with a (002) plane spacing of 0.34 nm or less), tin (simple element), tin compounds, silicon (simple element), silicon compounds, and Li4Ti5O 12 Lithium titanate compounds such as tin (single element), tin compounds, silicon (single element), or silicon compounds can be used alone or in combination. In the present invention, the negative electrode active material preferably contains at least a silicon-containing electrode active material such as tin (single element), tin compounds, silicon (single element), or silicon compounds. In particular, silicon-containing negative electrode active materials such as silicon (single element) or silicon compounds have a theoretical capacity that is extremely large compared to graphite, but also have a very large volume expansion rate of the electrode active material itself during charging.
[0046] When the polyimide-based binder for the power storage device of the present invention is used, deterioration of the electrode active material due to volume expansion can be significantly suppressed. Therefore, not only the characteristics during use such as cycle characteristics, but also the characteristics of the power storage device in a wide temperature range such as low temperature characteristics and gas generation after high temperature storage can be significantly improved.
[0047] The type of the silicon-containing negative electrode active material is not particularly limited, and examples thereof include silicon (single substance), silicon compounds, silicon partial substituents, silicon compound partial substituents, solid solutions of silicon compounds, and the like. Specific examples of the silicon compound include silicon oxides represented by SiOx (0.05 < x < 1.95), silicon carbides represented by the formula: SiCy (0 < y < 1), silicon nitrides represented by the formula: SiNz (0 < z < 4 / 3), and silicon alloys which are alloys of silicon and a different element M. In the silicon alloy, as the different element M1, at least one element selected from the group consisting of Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, and Ti is preferably exemplified.
[0048] Further, the silicon partial substituent is a compound in which a part of the silicon contained in silicon (single substance) and the silicon compound is substituted with a different element M2. Specific examples of the different element M2 include, for example, B, Mg, Ni, Ti, Mo, Co, Ca, Cr, Cu, Fe, Mn, Nb, Ta, V, W, Zn, C, N, and Sn. Among these silicon-containing active materials, silicon (single substance), silicon oxide, or silicon alloy is preferable, and silicon (single substance) or silicon oxide is more preferable.
[0049] Regarding the amount of the silicon-containing negative electrode active material, as the net mass of silicon in the negative electrode binder, in order to increase the capacity, 1% by mass or more is preferable, 5% by mass or more is more preferable, 10% by mass or more is further preferable, and from the viewpoint of improving the cycle characteristics, 95% by mass or less is preferable, 65% by mass or less is more preferable, and 45% by mass or less is further preferable.
[0050] In addition, examples of the electrode active material for the primary lithium battery, particularly the negative electrode active material, include lithium metal or a lithium alloy.
[0051] Solvents that can be used in the electrode mixture paste of the present invention include non-polar solvents such as aromatic hydrocarbons, such as xylene, toluene, and ethylbenzene; aliphatic hydrocarbons, such as pentane, hexane, and heptane; benzoic acid esters, such as methyl benzoate, ethyl benzoate, and propyl benzoate; water, methanol, ethanol, acetone, N,N-dimethylformamide, dimethylamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, heptane, and the like. Preferred are 1,2-hexamethylphosphorotriamide, 1,2-dimethoxymethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, tetrahydrofuran, bis[2-(2-methoxyethoxy)ethyl]ether, 1,4-dioxane, dimethyl sulfoxide, dimethyl sulfone, diphenyl ether, sulfolane, diphenyl sulfone, tetramethylurea, anisole, m-cresol, phenol, and γ-butyrolactone, and particularly preferred are water, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and γ-butyrolactone.
[0052] The solvent may be the same as that in the resin composition for binders, or may be concentrated or additional solvent may be added as necessary to obtain a suitable concentration for coating.
[0053] In the electrode mixture paste of the present invention, when the solvent system is an aqueous solvent system, it is preferable to contain a pyridine compound and an imidazole compound. This can reduce the swelling degree of the obtained polyimide in the electrolyte solution, and can increase the breaking elongation and breaking energy. In addition, the heat treatment temperature for obtaining the negative electrode active material layer can be kept low. The pyridine compound is a compound having a pyridine skeleton in the chemical structure, and examples of suitable compounds include pyridine, 3-pyridinol, quinoline, isoquinoline, quinoxaline, 6-tert-butylquinoline, acridine, 6-quinolinecarboxylic acid, 3,4-lutidine, and pyridazine. These pyridine compounds may be used alone or in combination. Examples of imidazole compounds include 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 4-ethyl-2-methylimidazole, and 1-methyl-4-ethylimidazole. The imidazoles used may be one type or a mixture of multiple types.
[0054] The amount of the pyridine compound is not limited, but is preferably 0.05 to 2.0 molar equivalents, more preferably 0.1 to 1.0 molar equivalents, relative to 1 mole of the amic acid repeating unit of the polyamic acid. If the amount added is outside this range, it may be difficult to make the solvent system water-based. The amount of the imidazole compound is not limited, but is 1.6 molar equivalents or more, more preferably 2.0 molar equivalents or more, and even more preferably 2.4 molar equivalents or more, relative to 1 mole of the amic acid repeating unit of the polyamic acid.
[0055] The electrode mixture paste of the present invention may contain known additives as necessary, such as a negative electrode conductive agent, a base, a surfactant, a viscosity modifier, a conductive auxiliary, a silane coupling agent, and a binder other than a polyimide, which may be used within a range that does not impair the effects of the present invention.
[0056] The negative electrode conductive agent is not particularly limited as long as it is an electronic conductive material that does not undergo chemical changes, but it is preferable to use metal powder such as copper, nickel, titanium, or aluminum, or a carbon material, etc. Suitable examples of carbon materials used as the conductive agent or negative electrode active material include graphite such as natural graphite (e.g., flake graphite) and artificial graphite; one or more types of carbon black selected from acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; and fibrous carbon powder such as carbon nanotubes and carbon fibers.
[0057] It is more preferable to use a suitable mixture of graphite and carbon black, graphite and fibrous carbon powder, or carbon black and fibrous carbon powder as the negative electrode conductive agent. In particular, the use of fibrous carbon powder is preferable because it ensures electrical conductivity and therefore requires less use of a conductive agent with a large specific surface area. Carbon materials are used as conductive agents or negative electrode active materials, and the amount of the carbon material added to the negative electrode mixture is preferably 1 to 90% by mass, more preferably 10 to 70% by mass.
[0058] When a carbon material is used as a negative electrode conductive agent by mixing it with a silicon-containing negative electrode active material, the ratio of the silicon-containing negative electrode active material to the carbon material is preferably 10% by mass or more, more preferably 20% by mass or more, based on the total mass of the net silicon of the silicon-containing negative electrode active material in the negative electrode mixture, from the viewpoint of cycle improvement based on the effect of improving electronic conductivity by mixing with the carbon material. In addition, if the ratio of the carbon material mixed with the silicon-containing negative electrode active material is too high, the amount of the silicon-containing negative electrode active material in the negative electrode mixture layer decreases, and there is a risk that the effect of increasing capacity is reduced. Therefore, the net mass of silicon of the silicon-containing negative electrode active material is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, based on the total mass of the carbon material. In addition, it is more preferable that the conductive agent is a composite obtained by mixing it with the silicon-containing active material in advance and appropriately heat-treating it.
[0059] When graphite is used, it is more preferable to use a carbon material having a graphite type crystal structure in which the lattice spacing (d002) of the graphite lattice plane (002) is 0.340 nm (nanometers) or less, particularly 0.335 to 0.337 nm. In particular, it is preferable to use artificial graphite particles having a block structure in which a plurality of flat graphitic fine particles are aggregated or bonded in a non-parallel manner, or particles obtained by repeatedly applying mechanical actions such as compression force, friction force, and shear force to spheroidize scaly natural graphite.
[0060] The density of the negative electrode, excluding the current collector, is 1.5 g / cm 3 When the negative electrode sheet is pressed to a density of 1000 or more, the ratio I(110) / I(004) of the peak intensity I(110) of the (110) plane of the graphite crystals to the peak intensity I(004) of the (004) plane obtained by X-ray diffraction measurement of the negative electrode sheet is preferably 0.01 or more, since the electrochemical characteristics are improved over a wider temperature range, more preferably 0.05 or more, and even more preferably 0.1 or more. In addition, since excessive processing may reduce the crystallinity and reduce the discharge capacity of the battery, the upper limit of the peak intensity ratio I(110) / I(004) is preferably 0.5 or less, more preferably 0.3 or less.
[0061] In addition, it is preferable that the highly crystalline carbon material (core material) is coated with a carbon material having a lower crystallinity than the core material, since the electrochemical properties over a wide temperature range are further improved. The crystallinity of the carbon material of the coating can be confirmed by TEM. When a highly crystalline carbon material is used, it reacts with the non-aqueous electrolyte during charging, and the interface resistance increases, which tends to deteriorate the properties of the electricity storage device over a wide temperature range, such as low-temperature properties after high-temperature storage and gas generation, but when the polyimide binder for electricity storage devices according to the present invention is used, the properties of these electricity storage devices are improved.
[0062] The polyimide binder for an electricity storage device of the present invention is used as a binder for a negative electrode. When the polyimide binder for an electricity storage device of the present invention is used in combination with another binder, the ratio of the mass of the other binder to the total mass of the binders is preferably 1 to 95 mass%, more preferably 5 to 45 mass%.
[0063] Examples of binders other than the polyimide-based binder for an electricity storage device of the present invention include polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, butadiene rubber, nitrile rubber, polyacrylonitrile, ethylene-vinyl alcohol copolymer resin, ethylene-propylene-diene rubber, polyurethane, polyacrylic acid, polyamide, polyacrylate, polyvinyl ether, fluororubber, carboxymethylcellulose, and sodium carboxymethylcellulose.
[0064] The electrode mixture paste of the present invention may further contain a solid electrolyte. The solid electrolyte may be, for example, La2O3 having a perovskite crystal structure. 0.51 Li 0.34 TiO 2.94 , garnet-type crystal Li7La3Zr2O 12 , NASICON type crystal Li 1.3 Al 0.3 Ti 1.7 (PO4)3, amorphous LIPON(Li 2.9 PO 3.3 N 0.46 ) and sulfide-based solid electrolytes such as Li2S-SiS2 and Li2S-P2S5.
[0065] The electrode mixture paste of the present invention can be produced as a uniform composition by applying a known production method to the above-mentioned components and adding, stirring, mixing, etc. For example, the electrode mixture paste may be produced by producing a solution or dispersion by mixing a polyimide-based binder with a solvent, and then adding and mixing various additives.
[0066] <Negative electrode active material layer> The negative electrode active material layer, which is one embodiment of the present invention, can be produced by forming a film from an electrode mixture paste by a known method. Although not particularly limited, as an example, an electrode mixture paste containing a polyimide binder, a solvent, and a negative electrode active material is prepared, and the electrode mixture paste is cast or applied onto a metal foil or a plastic film, and the solvent is removed by heat treatment, and if necessary, an imidization reaction is performed to form the layer. In particular, a negative electrode sheet for a power storage device can be produced by forming a negative electrode active material layer on a conductive current collector made of a metal foil such as aluminum foil.
[0067] The thickness of the negative electrode active material layer of the present invention may be appropriately determined depending on the application and desired capacity of the electricity storage device. Although not limited, it is preferable to use it in the range of 0.1 μm to 500 μm, for example. In particular, it is more preferable to use it in the range of 1 μm or more, 10 μm or more, or 20 μm or more, and more preferably 300 μm or less, 100 μm or less, or 50 μm or less.
[0068] <Negative electrode sheet for power storage devices> The negative electrode sheet for an electricity storage device, which is one embodiment of the present invention, is obtained by casting or applying an electrode mixture paste, which is a mixture of the polyimide-based binder for an electricity storage device of the present invention, a negative electrode active material, and any optional components such as a conductive agent, onto a current collector to form an active material layer. Preferably, the negative electrode sheet for an electricity storage device of the present invention is a negative electrode sheet obtained by casting or applying an anode mixture containing the polyimide-based binder for an electricity storage device of the present invention, a silicon-containing negative electrode active material, and a carbon material onto the surface of a copper current collector to form a negative electrode active material layer.
[0069] <Cathode active material> As a positive electrode active material for an electricity storage device, particularly for a lithium secondary battery, a composite metal oxide containing one or more selected from cobalt, manganese, and nickel and lithium is used. These positive electrode active materials can be used alone or in combination of two or more. Examples of such lithium composite metal oxides include LiCoO2, LiMn2O4, LiNiO2, and LiCo 1-x Nix O2(0.01 <x<1)、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, LiNi 1 / 2 Mn 3 / 2 O4 and LiCo 0.98 Mg 0.02 LiCoO2 and LiMn2O4, LiCoO2 and LiNiO2, or LiMn2O4 and LiNiO2 may be used in combination.
[0070] In addition, a part of the lithium composite metal oxide may be replaced with other elements in order to improve safety and cycle characteristics during overcharging, and to enable use at a charging potential of 4.3 V or higher. For example, a part of the cobalt, manganese, and nickel may be replaced with at least one element such as Sn, Mg, Fe, Ti, Al, Zr, Cr, V, Ga, Zn, Cu, Bi, Mo, and La, a part of the O may be replaced with S or F, or the lithium composite metal oxide may be coated with a compound containing these other elements. Among these, lithium composite metal oxides such as LiCoO2, LiMn2O4, and LiNiO2, which can be used at a positive electrode charge potential of 4.3 V or more based on Li in a fully charged state, are preferred. 1-x M x Lithium cobalt oxide substituted with different elements such as LiNiO2 (wherein M is one or more elements selected from Sn, Mg, Fe, Ti, Al, Zr, Cr, V, Ga, Zn, and Cu, and 0.001≦x≦0.05) 1 / 3 Mn 1 / 3 Co 1 / 3 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 1 / 2 Mn 3 / 2More preferred are lithium composite metal oxides that can be used at 4.4 V or higher, such as lithium composite metal oxides in which the ratio of nickel atoms and manganese atoms to all metal elements other than lithium atoms is 50 atomic % or more and 100 atomic % or less, such as a solid solution of Li2MnO3 and LiMO2 (M is a transition metal such as Co, Ni, Mn, or Fe).When a lithium composite metal oxide that operates at a high charging voltage is used, the characteristics of the electricity storage device tend to deteriorate when used over a wide temperature range due to a reaction with the electrolyte during charging, but the use of the polyimide binder for electricity storage devices according to the present invention makes it possible to suppress the deterioration of the characteristics of these electricity storage devices.
[0071] Furthermore, a lithium-containing olivine-type phosphate can be used as the positive electrode active material. In particular, a lithium-containing olivine-type phosphate containing one or more selected from iron, cobalt, nickel, and manganese is preferable. Specific examples thereof include one or more selected from LiFePO4, LiCoPO4, LiNiPO4, and LiMnPO4. These lithium-containing olivine-type phosphates may be partially substituted with other elements, and part of the iron, cobalt, nickel, and manganese may be substituted with one or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W, and Zr, or may be coated with a compound or carbon material containing these other elements. Of these, LiFePO4 or LiMnPO4 is preferred. The lithium-containing olivine-type phosphate can also be used by mixing with, for example, the above-mentioned positive electrode active material.
[0072] In addition, the positive electrodes for lithium primary batteries include CuO, Cu2O, Ag2O, Ag2CrO4, CuS, CuSO4, TiO2, TiS2, SiO2, SnO, V2O5, and V6O. 12 , V.O. x, Nb2O5, Bi2O3, Bi2Pb2O5, Sb2O3, CrO3, Cr2O3, MoO3, WO3, SeO2, MnO2, Mn2O3, Fe2O3, FeO, Fe3O4, Ni2O3, NiO, CoO3, CoO, etc., oxides or chalcogen compounds of one or more metal elements, sulfur compounds such as SO2 and SOCl2, or compounds represented by the general formula (CF x ) n Among them, MnO2, V2O5, graphite fluoride, etc. are preferable.
[0073] <Positive electrode conductive material> The conductive agent for the positive electrode is not particularly limited as long as it is an electron conductive material that does not undergo chemical changes. For example, graphite such as natural graphite (e.g., flake graphite), artificial graphite, one or more carbon blacks selected from acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, and fibrous carbon powder such as carbon nanotubes and carbon fibers are preferably used. In addition, it is more preferable to use a suitable mixture such as graphite and carbon black, graphite and fibrous carbon powder, or carbon black and fibrous carbon powder. The amount of the conductive agent added to the positive electrode mixture is preferably 1 to 10 mass%, and particularly preferably 2 to 5 mass%.
[0074] <Positive electrode binder> As the positive electrode binder, the polyimide binder for an electricity storage device of the present invention can be used, but other binders such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), a styrene-butadiene copolymer (SBR), an acrylonitrile-butadiene copolymer (NBR), carboxymethyl cellulose (CMC), or an ethylene propylene diene terpolymer can also be used. The polyimide binder for an electricity storage device of the present invention can be used in combination with other binders, and the preferred embodiments in this case are the same as those described in the section on negative electrode binders.
[0075] <Positive electrode sheet for power storage devices> The positive electrode sheet for an electricity storage device is obtained by casting or applying an electrode mixture paste, which is a mixture of a positive electrode binder, a positive electrode active material, and any other components such as a conductive agent, onto a current collector to form an active material layer.
[0076] <Electricity storage device> The electricity storage device according to one embodiment of the present invention includes the above-mentioned negative electrode sheet for electricity storage devices, and other components may be any known components necessary for electricity storage devices. The electricity storage device of the present invention includes lithium batteries, electric double layer capacitors, lithium ion capacitors, etc. In another embodiment, the negative electrode sheet for electricity storage devices can be made high-capacity and formed into a sheet, and has excellent mechanical properties, so that it can also be suitably used in all-solid-state batteries, etc. EXAMPLES
[0077] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0078] The methods for measuring the properties used in the following examples are as follows. <Tensile breaking energy> A tensile break test was carried out in accordance with ASTM D882 to calculate the tensile break energy.
[0079] <10% repeated breaking energy retention rate> The initial value of the tensile breaking energy is (TEB0), and the tensile breaking energy calculated by performing a tensile breaking test after repeating 10% strain 200 times is (TEB 200-10 ) was calculated using the following formula: 10% repeated breaking energy retention rate = (TEB 200-10 ) / (TEB0)
[0080] <20% repeated breaking energy retention rate> The initial value of the tensile breaking energy is (TEB0), and the tensile breaking energy calculated by performing a tensile breaking test after repeating 200 times of 20% strain is (TEB 200-20) was calculated using the following formula: 20% repeated breaking energy retention rate = (TEB 200-20 ) / (TEB0)
[0081] <30% repeated breaking energy retention rate> The initial value of the tensile breaking energy is (TEB0), and the tensile breaking energy calculated by performing a tensile breaking test after repeating 30% strain 200 times is (TEB 200-30 ) was calculated using the following formula: 30% repeated breaking energy retention rate = (TEB 200-30 ) / (TEB0)
[0082] The abbreviations of the compounds used in the following examples are explained below. s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride, ODPA: 4,4'-oxydiphthalic dianhydride, PMDA: pyromellitic dianhydride; ODA: 4,4'-diaminodiphenyl ether; PPD: p-phenylenediamine, DMD: decamethylenediamine; NMP: N-methyl-2-pyrrolidone
[0083] Example 1 400 g of NMP was added as a solvent to a 500 mL glass reaction vessel equipped with a stirrer and nitrogen gas inlet / outlet tubes, and 40.49 g (0.202 mol) of ODA and 59.51 g (0.202 mol) of s-BPDA were added thereto and stirred at 50° C. for 10 hours to obtain a polyimide precursor for electricity storage devices with a solids concentration of 18.2 mass% and a solution viscosity of 5.0 Pa s. The obtained polyimide precursor for electricity storage devices was used as it is as a binder resin composition.
[0084] The obtained polyimide precursor for an electricity storage device was applied onto a glass plate substrate using a bar coater, and the coating film was degassed and pre-dried under reduced pressure at 25°C for 30 minutes. After that, the coating film was placed in a hot air dryer under normal pressure and a nitrogen gas atmosphere and heat-treated at 120°C for 30 minutes, 150°C for 10 minutes, 200°C for 10 minutes, 250°C for 10 minutes, and 350°C for 10 minutes to form a binder resin film with a thickness of 30 μm.
[0085] The (TEB0) of the obtained film is 163MJ / m 3 , (TEB 200-10 ) is 151 MJ / m 3 The 10% repeated fracture energy retention was 93%.
[0086] Example 2 A 500 mL glass reaction vessel equipped with a stirrer and nitrogen gas inlet / outlet tubes was charged with 425 g of NMP as a solvent, to which 13.45 g (0.078 mol) of DMD, 15.63 g (0.078 mol) of ODA, and 45.92 g (0.156 mol) of s-BPDA were added and stirred at 50°C for 10 hours to obtain a polyimide precursor for use in electricity storage devices with a solids concentration of 13.3 mass% and a solution viscosity of 3.4 Pa s.
[0087] The obtained polyimide precursor for an electricity storage device was applied onto a glass plate substrate using a bar coater, and the coating film was degassed and pre-dried under reduced pressure at 25°C for 30 minutes. Thereafter, the coating film was placed in a hot air dryer under normal pressure and a nitrogen gas atmosphere and heat-treated at 120°C for 30 minutes, 150°C for 10 minutes, and 200°C for 120 minutes to form a binder resin film with a thickness of 30 μm.
[0088] The (TEB0) of the obtained film is 181MJ / m 3 , (TEB 200-10 ) is 179 MJ / m 3 , (TEB 200-20 ) is 159 MJ / m 3 , (TEB 200-30 ) is 132 MJ / m 3The 10% repeated fracture energy retention was 99%, the 20% repeated fracture energy retention was 88%, and the 30% repeated fracture energy retention was 73%.
[0089] Example 3 400 g of NMP was added as a solvent to a 500 mL glass reaction vessel equipped with a stirrer and nitrogen gas inlet / outlet tubes, and 17.35 g (0.101 mol) of DMD, 20.17 g (0.101 mol) of ODA, and 62.48 g (0.201 mol) of ODPA were added thereto and stirred at 50°C for 10 hours to obtain a polyimide precursor for electricity storage devices with a solid concentration of 18.0 mass% and a solution viscosity of 5.7 Pa s.
[0090] The obtained polyimide precursor for an electricity storage device was applied onto a glass plate substrate using a bar coater, and the coating film was degassed and pre-dried under reduced pressure at 25°C for 30 minutes. Thereafter, the coating film was placed in a hot air dryer under normal pressure and a nitrogen gas atmosphere and heat-treated at 120°C for 30 minutes, 150°C for 10 minutes, and 200°C for 120 minutes to form a binder resin film with a thickness of 30 μm.
[0091] The (TEB0) of the obtained film is 147MJ / m 3 , (TEB 200-10 ) is 140MJ / m 3 The 10% repeated fracture energy retention was 96%.
[0092] Example 4 A 500 mL glass reaction vessel equipped with a stirrer and nitrogen gas inlet / outlet tubes was charged with 400 g of NMP as a solvent, to which 32.56 g (0.163 mol) of ODA, 4.40 g (0.041 mol) of PPD, and 63.05 g (0.203 mol) of ODPA were added and stirred at 50°C for 10 hours to obtain a polyimide precursor for electricity storage devices with a solid concentration of 18.1 mass% and a solution viscosity of 6.3 Pa s.
[0093] The obtained polyimide precursor for an electricity storage device was applied onto a glass plate substrate using a bar coater, and the coating film was degassed and pre-dried under reduced pressure at 25°C for 30 minutes. Thereafter, the coating film was placed in a hot air dryer under normal pressure and a nitrogen gas atmosphere and heat-treated at 120°C for 30 minutes, 150°C for 10 minutes, and 200°C for 120 minutes to form a binder resin film with a thickness of 30 μm.
[0094] The TEB0 of the obtained film was 140MJ / m 3 , T.E.B. 200-10 is 139MJ / m 3 The 10% repeated fracture energy retention rate was 99%.
[0095] Comparative Example 1 A 500 mL glass reaction vessel equipped with a stirrer and nitrogen gas inlet / outlet tubes was charged with 400 g of NMP as a solvent, to which 47.85 g (0.239 mol) of ODA and 52.15 g (0.239 mol) of PMDA were added, and the mixture was stirred at 50°C for 10 hours to obtain a polyimide precursor with a solids concentration of 18.0 mass% and a solution viscosity of 4.8 Pa s.
[0096] The obtained polyimide precursor was applied onto a glass plate substrate using a bar coater, and the coating film was degassed and pre-dried under reduced pressure at 25°C for 30 minutes. Thereafter, the coating film was placed in a hot air dryer under normal pressure and a nitrogen gas atmosphere, and heat-treated at 120°C for 30 minutes, 150°C for 10 minutes, 200°C for 10 minutes, 250°C for 10 minutes, and then 350°C for 10 minutes to form a resin film having a thickness of 30 μm.
[0097] The (TEB0) of the obtained film is 138MJ / m 3 , (TEB 200-10 ) is 84MJ / m 3 The 10% repeated fracture energy retention was 61%.
[0098] [Preparation of Lithium-Ion Secondary Battery] LiNi 0.5 Mn 0.3 Co 0.2A mixture of 93% by mass of O2 and 3% by mass of acetylene black (conductive agent) was added to a solution in which 4% by mass of polyvinylidene fluoride (binder) had been dissolved in 1-methyl-2-pyrrolidone, and mixed to prepare a positive electrode mixture paste. This positive electrode mixture paste was applied to one side of an aluminum foil (current collector), dried, pressed, and punched to a specified size to prepare a positive electrode sheet for positive electrode No. 1. In addition, a negative electrode mixture paste was prepared using 15% by mass (as solid content) of the binder resin composition obtained in the examples and comparative examples, 60% by mass of silicon (Si), 20% by mass of artificial graphite (d002 = 0.335 nm), and 5% by mass of fibrous carbon powder (diameter: 12 nm, fiber length: 114 nm). This negative electrode mixture paste was applied to one side of a copper foil (current collector), heated, dried, and pressed to prepare a negative electrode sheet punched to a predetermined size. Then, a positive electrode sheet, a microporous polyethylene film separator, and a negative electrode sheet were laminated in this order, and a nonaqueous electrolyte was added to prepare a 2032-type coin battery. The non-aqueous electrolyte had a composition of 1M LiPF6 + 0.05M LiPO2F2 dissolved in ethylene carbonate / methyl ethyl carbonate / diethyl carbonate / 4-fluoro-1,3-dioxolan-2-one (volume ratio 25 / 30 / 40 / 5).
[0099] The prepared coin battery was charged in a thermostatic chamber at 25° C. for 3 hours at a constant current and voltage of 1 C to a cut-off voltage of 4.2 V, and then discharged at a constant current of 1 C to a cut-off voltage of 2.75 V. This cycle was repeated 200 times, and the capacity retention rate was calculated from the first and 200th discharge capacities.
[0100] It was found that the polyimide-based binders obtained from the resin composition for binders of Examples 1 to 4 had a large capacity retention rate compared to conventional polyimides (for example, the polyimide-based binder obtained from the resin composition for binders of Comparative Example 1). Therefore, it was confirmed that the use of the polyimide-based binder for electricity storage devices of the present invention can significantly improve the characteristics of electricity storage devices equipped with negative electrodes using Si or SiO as an electrode active material for increasing capacity in particular.
Claims
1. A polyimide-based binder for an electricity storage device having a repeated breaking energy retention rate of 80% or more (provided that the binder satisfies the following condition (a): (a) The binder is not composed solely of a polyimide obtained from 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-diaminodiphenyl ether and / or p-phenylenediamine.
2. 2. The polyimide-based binder for an electricity storage device according to claim 1, wherein the melting point of the binder is higher than 300°C or is substantially nonexistent.
3. 3. The polyimide-based binder for an electricity storage device according to claim 1, which is obtained by subjecting a polyamic acid solution containing a repeating unit represented by the following general formula (I) to an imidization reaction: 【Chemistry 1】 (In the formula, A is one or more tetravalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with a halogen, and these may be the same or two or more. B is one or more divalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with a halogen, and these may be the same or two or more.)
4. 4. The polyimide binder for an electricity storage device according to claim 3, wherein in said general formula (I), 50 mol % or more of either the groups A or B are linear aliphatic groups.
5. 5. The polyimide binder for an electricity storage device according to claim 3, wherein in said general formula (I), 50 mol % or more of A are groups represented by the following general formula (II): 【Chemistry 2】 (In the formula, X is a single bond or an oxygen atom, n is an integer of 0 to 2, and when n is 1 or 2, X may be the same or different.)
6. A resin composition for binders, comprising a polyamic acid including a repeating unit represented by the following general formula (I) and a solvent, and capable of forming the polyimide-based binder for an electricity storage device according to any one of claims 1 to 5 by an imidization reaction: 【Chemistry 3】 (In the formula, A is one or more tetravalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with a halogen, and these may be the same or two or more. B is one or more divalent groups selected from groups having an aromatic ring, chain aliphatic groups, or groups having an alicyclic structure, which may be substituted with a halogen, and these may be the same or two or more.)
7. An electrode mixture paste comprising the binder resin composition according to claim 6 and an electrode active material.
8. A negative electrode active material layer comprising the binder for an electricity storage device according to any one of claims 1 to 5 and an electrode active material.
9. A negative electrode sheet for an electricity storage device, comprising: a current collector on the surface of which the negative electrode active material layer according to claim 8 is formed.
10. An electricity storage device comprising the negative electrode sheet for an electricity storage device according to claim 9 .
Citation Information
Patent Citations
Lithium secondary battery negative electrode and lithium secondary battery
JP2003203637A
Negative electrode for lithium secondary battery, and lithium secondary battery
JP2004022433A
Negative electrode for lithium secondary battery, and the battery
JP2004235057A
Negative electrode for lithium secondary battery and lithium secondary battery
JP2004288520A
Negative electrode for lithium secondary cell and lithium secondary cell
WO2004004031A1