Solar cell and its manufacturing method, photovoltaic module

The solar cell design with optimized passivation layers enhances light absorption and reduces reflection, addressing the absorption efficiency limitation in solar cells, achieving improved conversion efficiency and aesthetic versatility.

JP7573066B2Active Publication Date: 2024-10-24JINKOSOLAR MIDDLE EAST FZCO
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023082684
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-26
Filing Date
2023-05-19
Publication Date
2024-10-24
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

The absorption efficiency of sunlight in solar cells is a limiting factor for improving conversion efficiency, and optimizing the passivation structure parameters, particularly the thickness and composition of passivation layers, is crucial.

Method used

A solar cell design incorporating specific passivation layers with tailored atomic ratios and refractive indices, including a first silicon nitride layer, a second silicon oxynitride layer, and a third silicon oxynitride layer, optimized through atomic layer deposition and plasma-enhanced chemical vapor deposition processes, to enhance light absorption and reduce reflection.

Benefits of technology

The optimized passivation structure significantly improves absorption efficiency for both short and long wavelength light, reducing internal reflection and enhancing photoelectric conversion efficiency, resulting in a solar cell with a dull blue or black appearance suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573066000001
    Figure 0007573066000001
  • Figure 0007573066000002
    Figure 0007573066000002
  • Figure 0007573066000003
    Figure 0007573066000003
Patent Text Reader

Abstract

To provide a solar cell, a method for producing the same, and a photovoltaic module.SOLUTION: A solar cell includes: a base having a front surface and a rear surface opposite to each other; first, second and third passivation layers positioned on the front surface and formed sequentially in a direction away from the front surface, where the first passivation layer contains a dielectric material, the second passivation layer contains a first silicon nitride SimNn (0.5≤n / m≤1) material, the third passivation layer contains a silicon oxynitride SiOiNj (0.1≤j / i≤0.6) material; and a tunneling oxide layer and a doped conductive layer that are positioned on the rear surface and formed sequentially in a direction away from the rear surface, where the doped conductive layer has a dopant of the same conductivity type as the base. Embodiments of the present application are advantageous in improving the light absorption efficiency of a solar cell.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of photovoltaics, in particular to solar cells and methods for producing same, and photovoltaic modules. [Background technology]

[0002] With the development of solar cell technology, the solar light absorption efficiency has become one of the factors that limit the further improvement of the conversion efficiency of solar cells. Since the absorption efficiency of solar cells is related to the parameters of the passivation structure, optimizing the parameters of the passivation structure is the key to improving the conversion efficiency of solar cells, and the parameters of the passivation structure include but are not limited to the stack structure, the components of the film layer and the thickness of the film layer. Summary of the Invention [Problem to be solved by the invention]

[0003] The present application provides a solar cell, a manufacturing method thereof, and a photovoltaic module that are advantageous in improving the absorption efficiency of the solar cell and the photovoltaic module. [Means for solving the problem]

[0004] In order to solve the above problems, the solar cell provided in the embodiment of the present application includes a base having a front surface and a back surface opposite to each other, and a first passivation layer including a dielectric material, a first silicon nitride (Si), and a second silicon nitride (Si) disposed in sequence on the front surface and away from the front surface. m N n a second passivation layer comprising a (n / m ∈ [0.5, 1]) material, and silicon oxynitride SiO i N j a third passivation layer including a (j / i∈[0.1, 0.6]) material; and a tunnel oxide layer and a doped conductive layer having a dopant of the same conductivity type as the base, located on the back surface and disposed sequentially in a direction away from the back surface.

[0005] The dielectric material includes one or more of aluminum oxide, titanium oxide, gallium oxide, and hafnium oxide.

[0006] The dielectric material is aluminum oxide Al x O y material and y / x∈[1.1, 1.5].

[0007] Furthermore, the first passivation layer has a thickness in a direction perpendicular to the front surface of the substrate of 3 nm to 10 nm.

[0008] Furthermore, the second passivation layer has a thickness in a direction perpendicular to the front surface of the substrate of 40 nm to 60 nm.

[0009] Furthermore, the third passivation layer has a thickness in a direction perpendicular to the front surface of the substrate of 20 nm to 50 nm.

[0010] Moreover, the second refractive index of the second passivation layer is greater than the first refractive index of the first passivation layer and the third refractive index of the third passivation layer.

[0011] The first passivation layer has a refractive index of 1.6 to 1.7, the second passivation layer has a refractive index of 1.9 to 2.2, and the third passivation layer has a refractive index of 1.45 to 1.8.

[0012] The solar cell further comprises a fourth passivation layer located on the side of the doped conductive layer facing away from the base, the fourth passivation layer being made of a second silicon nitride (Si a N b (a / b∈[3.5, 6.8]) Includes material.

[0013] The fourth passivation layer has a refractive index of 2.04 to 2.2, and a thickness of the fourth passivation layer in a direction perpendicular to the rear surface is 60 nm to 100 nm.

[0014] Additionally, the first passivation layer further includes a silicon oxide material interposed between the base and the dielectric material.

[0015] Also, the base is an N-type semiconductor base, and the doped conductive layer is at least one of an N-type doped polysilicon layer, an N-type doped microcrystalline silicon layer, or an N-type doped amorphous silicon layer.

[0016] Accordingly, an embodiment of the present application further provides a photovoltaic module comprising a cell string formed by connecting a plurality of solar cells described in any one of the above claims, a sealant film for covering a surface of the cell string, and a cover plate for covering a surface of the sealant film facing away from the cell string.

[0017] Accordingly, embodiments of the present application include providing a base having opposing front and back surfaces, and, at said front surface and in a direction away from said front surface, a first passivation layer comprising a dielectric material, a first silicon nitride (Si m N n a second passivation layer comprising a (n / m ∈ [0.5, 1]) material, and silicon oxynitride SiO i N j The present invention further provides a method for manufacturing a solar cell, the method including, in order, providing a third passivation layer including a (j / i∈[0.1, 0.6]) material, and providing, in order on the back surface in a direction away from the back surface, a tunnel oxide layer and a doped conductive layer having a dopant of the same conductivity type as the base.

[0018] The dielectric material is aluminum oxide Al x O y The material is a silicon nitride film, and the first passivation layer is formed by an atomic layer deposition process, the precursors of the atomic layer deposition process include trimethylaluminum and water, and the deposition temperature is 150°C to 250°C.

[0019] The method further includes, after forming the first passivation layer, performing an annealing process on the first passivation layer at a process temperature of 450° C. to 550° C. for a process time of 10 minutes or more.

[0020] The second passivation layer is formed by a first plasma enhanced chemical vapor deposition process, a precursor of the first plasma enhanced chemical vapor deposition process includes silane and ammonia gas, a flow ratio of the ammonia gas to the silane is 4 to 15, and a pulse power per unit area is 30 to 40 mW / cm 2 It is.

[0021] The third passivation layer is formed by a second plasma enhanced chemical vapor deposition process, and the precursor of the second plasma enhanced chemical vapor deposition process contains silane, nitrous oxide and ammonia gas, the flow rate ratio of the silane to the nitrous oxide is 1 / 10 or more, and the pulse power per unit area is 25 to 40 mW / cm 2 It is.

[0022] Compared with the prior art, the technical solutions provided in the embodiments of the present application have the following advantages:

[0023] In the above technical solution, the third passivation layer containing silicon oxynitride material is provided on the side of the second passivation layer away from the base, which is advantageous for the solar cell to have good absorption efficiency for short-wavelength light, and the atomic ratio of the silicon oxynitride material is limited to give the third passivation layer a high refractive index, which is advantageous for external light to be incident into the base at a smaller incident angle. In addition, the atomic ratio of the first silicon nitride material in the second passivation layer is limited to make the second passivation layer have a higher refractive index than the third passivation layer, which is advantageous for reducing internal reflection and outgoing light, and the second passivation layer has a weak positive charging property, which is advantageous for avoiding the field passivation effect of the second passivation layer on the first passivation layer and not affecting the photoelectric effect of the base. [Brief description of the drawings]

[0024] One or more embodiments are illustratively illustrated in the accompanying drawing figures, which are not to scale unless specifically noted. [Figure 1] FIG. 1 is a diagram showing a cross-sectional structure of a solar cell according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram comparing wavelength and reflectance according to an embodiment of the present application. [Diagram 3] FIG. 3 is a diagram showing a surface of a solar cell according to an embodiment of the present application. [Figure 4] FIG. 4 is a diagram showing the structure of a photovoltaic module according to an embodiment of the present application. [Diagram 5] FIG. 5 is a diagram showing the structure of a photovoltaic module according to an embodiment of the present application. [Figure 6] FIG. 6 is a structural schematic diagram corresponding to each step of the method for manufacturing a solar cell according to an embodiment of the present application. [Figure 7] FIG. 7 is a structural schematic diagram corresponding to each step of the method for manufacturing a solar cell according to an embodiment of the present application. [Figure 8]FIG. 8 is a structural schematic diagram corresponding to each step of the method for manufacturing a solar cell according to an embodiment of the present application. [Figure 9] FIG. 9 is a structural schematic diagram corresponding to each step of the method for manufacturing a solar cell according to an embodiment of the present application. [Figure 10] FIG. 10 is a structural schematic diagram corresponding to each step of the method for manufacturing a solar cell according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] In order to clarify the purpose, technical solutions and advantages of the embodiments of the present application, the embodiments of the present application will be described in detail below in conjunction with the drawings. However, as will be understood by those skilled in the art, in order to allow the reader to better understand the present application, many technical details are proposed in the embodiments of the present application, but the technical solutions claimed for protection by the present application can be realized without these technical details and various changes and modifications based on the following embodiments.

[0026] The embodiments of the present application provide a solar cell, a manufacturing method thereof, and a photovoltaic module. The solar cell provided in the embodiments of the present application will be described in detail below with reference to the drawings. Fig. 1 is a diagram showing a cross-sectional structure of a solar cell according to an embodiment of the present application. Fig. 2 is a schematic diagram showing a comparison of wavelength and reflectance according to an embodiment of the present application. Fig. 3 is a diagram showing the surface of a solar cell according to an embodiment of the present application.

[0027] Referring to FIG. 1, the solar cell includes a base 10 having an opposing front surface 10a and a back surface 10b, a first passivation layer 111 including a dielectric material, a first silicon nitride (Si) layer 121, and a second silicon nitride (Si) layer 122, which are disposed on the front surface 10a and in a direction away from the front surface 10a. m N n A second passivation layer 112 comprising a (n / m ∈ [0.5, 1]) material, and silicon oxynitride SiO i N jThe semiconductor device further comprises a third passivation layer 113 including a (j / i∈[0.1, 0.6]) material, and a tunnel oxide layer 121 and a doped conductive layer 122 having a dopant of the same conductivity type as the base 10, which are located on the rear surface 10b and arranged in sequence in a direction away from the rear surface 10b.

[0028] It can be understood that y / x, n / m and j / i are the corresponding atomic number ratios.

[0029] In some embodiments, the atomic ratio in each film layer can be determined using X-ray energy spectroscopy (EDS) or electron energy loss spectroscopy (EELS). In some embodiments, the second passivation layer 112 is a silicon-rich layer, and the first silicon nitride material provided herein has a higher ratio of silicon atoms to nitrogen atoms compared to conventional silicon nitride materials. Accordingly, the third passivation layer 113 may also be a silicon-rich layer, i.e., the third passivation layer 113 has a higher ratio of silicon atoms to nitrogen atoms and a higher ratio of oxygen atoms.

[0030] Here, by providing the third passivation layer 113 containing a silicon oxynitride material on the side of the second passivation layer 112 facing away from the base 10, it is advantageous for the solar cell to have good absorption efficiency for short-wavelength light, and by limiting the atomic ratio of the silicon oxynitride material, it is advantageous for the third passivation layer 113 to have a high refractive index, thereby allowing external light to enter the base 10 at a smaller angle of incidence.

[0031] In addition, by limiting the proportion of the number of atoms of the first silicon nitride material in the second passivation layer 112, the second passivation layer 112 has a higher refractive index than the third passivation layer 113, which is advantageous for reducing the internal reflection and outgoing of light. In addition, the second passivation layer 112 has a weak positive charging property, which is advantageous for avoiding the influence of the second passivation layer 112 on the field passivation effect of the first passivation layer 111 and the photoelectric effect of the base 10. In addition, the second passivation layer 112 has an appropriate amount of hydrogen ions, which can efficiently saturate the dangling bonds of the front surface 10a by ion transfer and suppress the recombination of carriers with themselves, which is advantageous for ensuring the effective convergence of carriers to the corresponding electrode.

[0032] The solar cell shown in FIG. 1 will now be described in more detail with reference to the drawings.

[0033] In some embodiments, the base 10 is a silicon-based material, such as one or more of monocrystalline silicon, polysilicon, amorphous silicon, or microcrystalline silicon. In other embodiments, the base material may be carbon, an organic material, or a polyvalent compound, including, but not limited to, perovskite, gallium arsenide, cadmium telluride, copper indium selenium, and the like. The front surface 10a is a light-receiving surface, and the back surface 10b is a back surface opposite to the light-receiving surface, and the front surface 10a may be provided with a pyramidal texture, which reduces the light reflection of the front surface 10a, improves the absorption utilization rate of the light, and improves the conversion efficiency of the solar cell. In some embodiments, the back surface 10b may be provided with a non-pyramidal texture, such as a stacked step pattern, which ensures that the tunnel oxide layer covering the back surface 10b has high density and uniformity, and ensures a good passivation effect of the tunnel oxide layer on the back surface 10b.

[0034] The base 10 is an N-type semiconductor base. The base 10 includes a base area 101 containing an N-type dopant such as phosphorus, arsenic, or antimony, and an emitter 102 containing a P-type dopant, and the emitter 102 forms a PN junction with the base area 101. In some embodiments, a first passivation layer 111 covers the emitter 102. The emitter 102 is obtained by performing diffusion doping of P-type ions (such as boron ions) on the surface layer of the base area 101, and the doped part of the base area 101 is converted into the emitter 102. The doping ion species in the doped conductive layer 122 is the same as the doping ion species in the base 10, which actually means that the doping ion species in the doped conductive layer 122 is the same as the doping ion species in the main body of the base 10, that is, the doping ion species in the doped conductive layer 122 is the same as the doping ion species in the base area 101.

[0035] Regarding the type of material of the first passivation layer 111, depending on whether the main passivation effect to be realized is field passivation or interface passivation, the material of the first passivation layer 111 can be divided into interface passivation material and field passivation material, where the interface passivation material includes at least one of silicon oxide or silicon oxynitride, and the field passivation material includes one or more of aluminum oxide, titanium oxide, gallium oxide, and hafnium oxide. In the following, the material of the first passivation layer 111 is mainly a field passivation material, specifically aluminum oxide Al X O y The material will be described as an example.

[0036] Regarding the characteristics of the material of the first passivation layer 111, in order to enhance the field passivation effect of the first passivation layer 111 and realize selective transport of carriers, the first passivation layer 111 must be provided to have a strong negative charge. In order to suppress the movement and intrusion of external positive ions into the base 10, the first passivation layer 111 must be provided to have a weak negative charge. In order to reduce the stress between the first passivation layer 111 and the adjacent film layer, the hardness of the first passivation layer 111 must be set low. In addition, in order to improve the efficiency of absorption of short-wavelength light by the solar cell, the absorption effect of short-wavelength light by the first passivation layer 111 must also be taken into consideration. From the above considerations, the aluminum oxide Al in the first passivation layer 111 is x O y The y / x ratio of the material can be, and is selectable from, 1.1 to 1.5, such as 1.2, 1.3, or 1.4, where y / x is greater than or equal to 1.1 and less than 1.5.

[0037] It can be seen that the thicker the first passivation layer 111 is, the stronger the field passivation effect is, since the difference in material properties between aluminum oxide and silicon is large. At the same time, the thicker the first passivation layer 111 is, the greater the stress the first passivation layer 111 exerts on the base 10. Furthermore, based on the barrier effect of any of the film layers themselves, it can be seen that the thicker the first passivation layer 111 is, the more difficult it is for hydrogen ions in the second passivation layer 112 to pass through the first passivation layer 111 and saturate the dangling bonds on the front surface 10a. From the above considerations, the thickness of the first passivation layer 111 can be set to 3 nm to 10 nm, for example, 5 nm, 7 nm, or 9 nm.

[0038] In some embodiments, the first passivation layer 111 further comprises a silicon oxide material, which covers the front surface 10a or is interposed between the N-type base 10 and a dielectric material, and the dielectric material is aluminum oxide Al. x O y The silicon oxide material may be formed by natural oxidation or by a thermal oxygen process to passivate the front surface. In a direction perpendicular to the front surface 10a, the thickness of the film layer made of the silicon oxide material may be 0.5 nm to 2 nm, for example, 0.8 nm, 1.1 nm, 1.4 nm, or 1.7 nm. If the film layer is too thick, carriers may not be able to pass through the thin film by the tunnel effect, and if the film layer is too thin, the passivation effect is poor.

[0039] In some embodiments, the second passivation layer 112 includes a first silicon nitride (Si m N nWhen the atomic ratio of the material is determined, the refractive index range of the second passivation layer 112 is also almost determined (the refractive index is also affected by other impurity elements in the second passivation layer 112), so that the thickness of the second passivation layer 112 in the direction perpendicular to the front surface 10a can be set to 40 nm to 60 nm, for example, 45 nm, 50 nm, or 55 nm, in order to ensure that the sunlight incident through the second passivation layer 112 is closer to the center of the base 10 and suppress the emission of light rays. If the thickness of the second passivation layer 112 is too thin, the refraction effect of the second passivation layer 112 on light rays is poor, and the incident light rays may be emitted through other passivation film layers or may be emitted through the base 10 before being absorbed by the base 10, which is disadvantageous to improving the incidence efficiency of the solar cell on light rays. In addition, the second passivation layer 112 only has a weak positive charging property, and the hydrogen ions in the second passivation layer 112 may not be enough to saturate the dangling bonds on the front surface 10a, and need to be replenished by the hydrogen ions in the third passivation layer 113. Therefore, if the second passivation layer 112 is too thick, it may block the transport of hydrogen ions and even cause a lot of interface defects on the front surface 10a, which is disadvantageous to suppressing the carrier recombination on the front surface 10a and reducing the contact resistance of the front surface 10a.

[0040] It is also understandable that the thickness of the second passivation layer 112 is also affected by the atomic ratio of the second passivation layer 112, and the two are matched with each other to mainly absorb light in a specific wavelength range, for example, mainly absorb long wavelength light. Furthermore, the thickness of the second passivation layer 112 is also limited by the total thickness of the solar cell, and if the total thickness of the solar cell is too thin, the solar cell is easily broken under the influence of external stress, and if the total thickness of the solar cell is too thick, it is disadvantageous to the overall sealing and the process cost is also high.

[0041] In some embodiments, in order to improve the absorption efficiency of the solar cell for both long and short wavelength light, the second passivation layer 112 primarily absorbs long wavelength light, and the third passivation layer 113 primarily absorbs short wavelength light. Meanwhile, since the refractive index of the silicon oxynitride material that primarily absorbs short wavelength light is relatively low, the refractive index of the second passivation layer 112 can be set to be higher than that of the third passivation layer 113 so that the refractive index for all light rays in different wavelength ranges is high, thereby improving the absorption efficiency of the solar cell for light.

[0042] In some embodiments, the third passivation layer 113 is made of silicon oxynitride (SiO i N j When the atomic ratio of the materials is fixed, in order to enable the solar cell to have high absorption efficiency for short wavelength light and to enable the hydrogen ions in the third passivation layer 113 to complement the hydrogen ions in the second passivation layer 112, the thickness of the third passivation layer 113 in a direction perpendicular to the front surface 10a can be 20 nm to 50 nm, for example 25 nm, 30 nm, 35 nm, 40 nm, or 45 nm. In some cases, conventional solar cells are usually light blue in color, and the main reason for this is that they have a high reflectance of short-wavelength light (e.g., ultraviolet light wavelength range). In the embodiment of the present application, however, the thickness of the third passivation layer 113 is set to a specific range (e.g., 20 nm to 50 nm) to selectively absorb short-wavelength light, which is advantageous for making the cell exhibit a dull blue color or even black, and the photovoltaic module in which the cell is sealed exhibits a black color, has high power generation efficiency, and is expected to be suitable for multiple scenes (e.g., BIPV, building material-integrated photovoltaic power generation).

[0043] In some embodiments, if the thickness of the third passivation layer 113 is less than 20 nm, the battery may have a light blue color, and if the thickness of the third passivation layer 113 is greater than 50 nm, the battery may have a green color.

[0044] In addition, the second passivation layer 112 and the third passivation layer 113 may both be a laminated structure, in which the refractive indexes of different sub-layers in the laminated structure gradually decrease in the direction away from the front surface 10a of the base 10, which is advantageous in reducing internal reflection and outgoing reflection caused by too large difference in refractive index of adjacent film layers. Adjacent film layers include not only the film layers in the solar cell, but also the sealant film and cover plate in the photovoltaic module.

[0045] In some embodiments, the second refractive index of the second passivation layer 112 is greater than the first refractive index of the first passivation layer 111 and the third refractive index of the third passivation layer 113, in which the second refractive index is greater than the third refractive index, which is advantageous for reducing the reflection and emission of sunlight incident through the third passivation layer 113. Furthermore, in some embodiments, the first refractive index is greater than the third refractive index, which is advantageous for further reducing the reflection and emission of sunlight incident through the third passivation layer 113 and improving the absorption efficiency of the solar cell. When the above-mentioned film layer includes multiple sub-film layers, the refractive index corresponding to the film layer can be understood to be the average refractive index of the multiple sub-film layers.

[0046] Regarding the third passivation layer 113, from the viewpoint of reducing the angle of incidence of external light, it is necessary to set the third passivation layer 113 to have a high refractive index, and from the viewpoint of suppressing internal reflection and emission, it is necessary to set the third passivation layer 113 to have a small refractive index, and it is necessary that the difference between the refractive index of the third passivation layer 113 and the refractive index of the second passivation layer 112 is small. From the viewpoint of mainly absorbing short-wavelength light, it is necessary to set the ratio of the number of oxygen atoms in the third passivation layer 113 to be relatively large, and it can be seen that the refractive index of the third passivation layer 113 gradually decreases with an increase in the ratio of the number of atoms. In order for the solar cell to have a high absorption efficiency for short-wavelength light, the atomic ratio j / i of the third passivation layer 113 can be set to 0.43 to 0.46, for example, 0.44 or 0.45, and the refractive index of the third passivation layer 113 can be set to 1.45 to 1.8, for example, 1.55, 1.6, 1.65, 1.7 or 1.75.

[0047] The atomic ratio n / m of the second passivation layer 112 can be set to 0.56 to 0.7, for example, 0.60, 0.64, or 0.68, and the refractive index of the second passivation layer 112 can be set to 1.9 to 2.2, for example, 2.0, 2.05, or 2.1. At the same time, the refractive index of the first passivation layer 111 is set to 1.6 to 1.7, for example, 1.63, 1.65, or 1.68.

[0048] Referring to FIG. 2, compared with the conventional TOPCON cell (N-type TOPCON cell) and the PERC cell (P-type PERC cell), the solar cell provided in the embodiment of the present application has a lower reflectance in the short wavelength (e.g., ultraviolet light wavelength range) range, and the conventional TOPCON cell usually uses an aluminum oxide / silicon nitride laminate as a front passivation layer, and the conventional PERC cell usually uses a silicon nitride layer as a front passivation layer. Taking 400 nm and 450 nm as an example, at a wavelength of 400 nm, the reflectance of the conventional PERC cell is about 12.2%, and the reflectance of the conventional TOPCON cell is about 11.1%, but the reflectance of the solar cell provided in the embodiment of the present application is about 6.5%, which is about half. At a wavelength of 450 nm, the reflectance of the conventional PERC cell is about 5%, and the reflectance of the conventional TOPCON cell is about 4%, but the reflectance of the solar cell provided in the embodiment of the present application is about 2.4%, which is also about half. The solar cell provided in the embodiment of the present application has low light reflectance in the short wavelength region, and therefore can exhibit a dull blue or even black color, whereas conventional solar cells or photovoltaic modules exhibit blue color, thereby forming a black photovoltaic module. Referring to Fig. 3, the solar cell based on the structure shown in Fig. 1 exhibits a dull blue color and is close to black.

[0049] The average reflectance of the solar cell provided in the embodiment of the present application is also significantly lower in the wavelength range of 380 nm to 1050 nm. Specifically, in the entire range, the conventional PERC cell and the TOPCON cell have a reflectance of 2.1% to 2.3%, for example, the average reflectance of the conventional PERC cell is about 2.160%, and the average reflectance of the conventional TOPCON cell is about 2.237%, whereas the average reflectance of the solar cell provided in the embodiment of the present application is 1.4% to 1.7%, for example, about 1.552%, which is nearly 1 / 3 lower. Furthermore, in the wavelength range of 600 nm to 800 nm, the average reflectance of the solar cell provided in the embodiment of the present application is also less than 1%. When the above passivation layer stack (first passivation layer 111, second passivation layer 112, and third passivation layer 113) is applied to a TOPCON cell, the short-circuit current of the cell can be improved by 30 mA or more.

[0050] In some embodiments, a first intermediate layer may be provided between the first passivation layer 111 and the second passivation layer 112, the first passivation layer 111 being a field effect passivation layer, the second passivation layer 112 being a chemical effect passivation layer, and the first intermediate layer may be used to optimize the conductive performance or light absorption performance between them. For example, the first intermediate layer may affect the reflectivity (e.g., reflectance) of the short wavelength band incident light (e.g., ultraviolet light) across the front passivation layer. The material of the first intermediate layer may be a silicon oxide material, and the thickness of the first intermediate layer is 0.5 nm to 3 nm.

[0051] In some embodiments, a second intermediate layer may also be provided between the second passivation layer 112 and the third passivation layer 113, and the second intermediate layer may be used to affect the reflective performance of the entire front passivation layer. For example, the second intermediate layer may affect the reflective performance (e.g., reflectance) of the short-wavelength band incident light (e.g., ultraviolet light) of the entire front passivation layer. The material of the second intermediate layer may be a silicon oxycarbonitride material, and the thickness of the second intermediate layer is less than 10 nm. In some embodiments, the back surface 10b is also provided with a passivation contact structure, which includes at least a tunnel oxide layer 121 and a doped conductive layer 122, which are sequentially arranged in a direction away from the base 10. Among them, the material of the tunnel oxide layer 121 is a dielectric material such as silicon oxide, and is used to realize the interface passivation of the back surface 10b. The material of the doped conductive layer 122 is used to form a field passivation, for example, doped silicon, and the doped conductive layer 122 has the same conductive type dopant as the base 10, and the doped silicon can be one or more of N-type doped polysilicon, N-type doped microcrystalline silicon, or N-type doped amorphous silicon, and the doped conductive layer 122 contains N-type doping ions. In some embodiments, the doped conductive layer 122 is a doped polysilicon layer, and the thickness range of the doped conductive layer 122 in the direction perpendicular to the back surface 10b is 80 nm to 160 nm, for example, 100 nm, 120 nm, or 140 nm, and the refractive index range of the doped conductive layer 122 is 3.5 to 4.5, for example, 3.75, 4, or 4.25.

[0052] In some embodiments, the doped conductive layer 122 is further provided with a fourth passivation layer 123 to enhance the reflection effect of the incident light on the back of the cell. Here, the fourth passivation layer 123 may include multiple sub-layers, and the refractive indexes of different sub-layers gradually decrease in the direction of the back surface 10b toward the doped conductive layer 122, thus favoring the enhancement of the reflection effect of the incident light on the back of the cell through internal reflection. When the material of the fourth passivation layer 123 is silicon nitride, the silicon nitride sub-layer with a higher refractive index has more hydrogen ions, and the hydrogen ions can migrate to the back surface 10b under the diffusion force formed by the concentration difference or the thermal force formed by the heat treatment process to passivate the interface defects between the base 10 and the passivation contact structure, inhibit the recombination of carriers, and improve the photoelectric conversion efficiency.

[0053] Specifically, the fourth passivation layer 123 may include a lower passivation layer, an intermediate passivation layer, and an upper passivation layer, which are arranged in sequence, and the lower passivation layer covers the surface of the doped conductive layer 122, and the refractive index of the lower passivation layer may be 2.12 to 2.2, for example, 2.14, 2.16, or 2.18, and the thickness in the direction perpendicular to the back surface 10b is 10 nm to 20 nm, for example, 13 nm, 15 nm, or 18 nm. The refractive index of the intermediate passivation layer may be 2.10 to 2.12, for example, 2.13, 2.15, or 2.18, and the thickness is 20 nm to 30 nm, for example, 23 nm, 25 nm, or 28 nm. The refractive index of the upper passivation layer may be 2.09 to 2.10, and the thickness is 30 nm to 50 nm, for example, 35 nm, 40 nm, or 45 nm. In short, the fourth passivation layer 123 is a second silicon nitride Si a N bThe fourth passivation layer 123 may have an overall refractive index of 2.04 to 2.2, such as 2.08, 2.12, or 2.16, and a thickness of the fourth passivation layer 123 in a direction perpendicular to the back surface 10b may be 60 nm to 100 nm, such as 70 nm, 80 nm, or 90 nm.

[0054] The solar cell further includes a first electrode 114 electrically connected to the emitter 102 and a second electrode 124 electrically connected to the doped conductive layer 122 through the fourth passivation layer 123. In some embodiments, the first electrode 114 and / or the second electrode 124 may be printed and fired using a conductive paste (silver paste, aluminum paste, or silver-aluminum paste).

[0055] In the embodiment of the present application, the third passivation layer containing the silicon oxynitride material is provided on the side of the second passivation layer away from the base, which is advantageous for providing the solar cell with good absorption efficiency for short wavelength light, and the atomic ratio of the silicon oxynitride material is limited to provide the third passivation layer with a high refractive index, which is advantageous for allowing external light to enter the base at a smaller incident angle. In addition, the atomic ratio of the first silicon nitride material in the second passivation layer is limited to allow the second passivation layer to have a higher refractive index than the third passivation layer, which is advantageous for reducing internal reflection and emission of light. At the same time, the second passivation layer is provided with a weak positive charging property, which is advantageous for avoiding the influence of the second passivation layer on the field passivation effect of the first passivation layer and the photoelectric effect of the base.

[0056] In addition, the embodiment of the present application further provides a photovoltaic module that converts received light energy into electrical energy. Referring to FIG. 4, the photovoltaic module includes a cell string (not shown), a sealant film 2, and a cover plate 3. The cell string is formed by connecting a plurality of solar cells 1, and the solar cells 1 may be any of the solar cells described above (including but not limited to the solar cell in FIG. 1), and adjacent solar cells 1 are electrically connected to each other by a conductive tape (not shown), and the positional relationship between adjacent solar cells 1 may be partially laminated or connected to each other. The sealant film 2 may be an organic sealant film such as an ethylene vinyl acetate copolymer (EVA) adhesive film, a polyethylene octene co-elastomer (POE) adhesive film, or a polyethylene terephthalate (PET) adhesive film, and the sealant film 2 covers and seals the surface of the cell string. The cover plate 3 may be a transparent or translucent cover plate such as a glass cover plate or a plastic cover plate, and the cover plate 3 covers the surface of the sealant film 2 that is away from the cell string. In some embodiments, the cover plate 3 is provided with a light trapping structure to improve the utilization efficiency of the incident light, and the light trapping structures of different cover plates 3 may be different. The photovoltaic module has a relatively high current collection ability and a relatively low carrier recombination rate, and can achieve a high photoelectric conversion efficiency. At the same time, the front surface of the photovoltaic module exhibits a dull blue or even black color, which can be applied to more scenes.

[0057] In some embodiments, the sealant film 2 and the cover plate 3 are located only on the front surface of the solar cell 1, to avoid the sealant film 2 and the cover plate 3 located on the back surface from further blocking and attenuating the relatively weak light. The photovoltaic module may also use a side full-enclosure type sealing, that is, the side of the photovoltaic module is completely covered with the sealant film 2, to prevent the phenomenon of lamination slippage during lamination, and to prevent the external environment such as water intrusion from affecting the performance of the solar cell through the side of the photovoltaic module.

[0058] In some embodiments, referring to FIG. 5, the photovoltaic module further includes an edge sealing member 6 fixedly sealed at least to the side of the photovoltaic module. Furthermore, the edge sealing member 6 is fixedly sealed at least to the side near the corner of the photovoltaic module. The edge sealing member 6 may be a high-temperature resistant tape, and the high-temperature resistant property of the high-temperature resistant tape is advantageous for ensuring reliable sealing of the solar cell to the photovoltaic module without disassembling or falling off during lamination and use. In some embodiments, the high-temperature resistant tape is attached not only to the side of the photovoltaic module but also to the front and back of the photovoltaic module, which is advantageous for suppressing the occurrence of lamination misalignment of the photovoltaic module during lamination and the occurrence of stress distortion of the photovoltaic module due to stress.

[0059] An embodiment of the present application further provides a method for manufacturing a solar cell. With reference to Figures 6 to 10 and 1, Figures 6 to 10 and 1 are structural schematic diagrams corresponding to each step of the method for manufacturing a solar cell according to an embodiment of the present application.

[0060] Referring to FIG. 6, a base area 101 is provided for double sided texturing.

[0061] Specifically, the base area 101 is cleaned and a pyramid texture is created by wet chemical etching, and the pyramid texture can reduce the reflection of light on the surface of the base area 100, increase the absorption utilization rate of the light in the base area 100, and improve the conversion efficiency of the solar cell. In some embodiments, the material of the base area 101 is single crystal silicon, the thickness of the base area 101 is 60 μm to 240 μm, specifically, it may be 60 μm, 80 μm, 90 μm, 100 μm, 120 μm, 150 μm, 200 μm, or 240 μm, etc., and the resistivity range of the base area 101 is 0.3 to 2 ohm.cm. In addition, the base area 101 may be an N-type semiconductor or a P-type semiconductor, and the following description will be given taking the base area 101 as an N-type semiconductor as an example.

[0062] However, the present application does not limit the specific operation method of texturing. For example, the texturing can be performed by selecting a wet texturing process, but is not limited thereto. When the base area 101 is N-type single crystal silicon, the texturing can be performed by using an alkaline solution such as potassium hydroxide, and the corrosion of the NaOH solution is anisotropic, which is advantageous for manufacturing a pyramidal microstructure. The pyramidal microstructure can be a tetrahedron, a near-tetrahedron, a pentahedron, a near-pentahedron, etc. structure. In addition, the texturing process can be chemical etching, laser etching, mechanical etching, plasma etching, etc., and the pyramidal microstructure can better fill the microstructure when the metal paste is screen-printed to form the electrode, and can obtain a better electrode contact, and can effectively reduce the series resistance of the battery and improve the fill factor. By controlling the pattern of the pyramidal microstructure, the overall refractive index of the solar cell can be less than 10%.

[0063] Referring to FIG. 7, a P-type emitter 102 is formed.

[0064] After double-sided texturing, a boron diffusion process is performed on the front surface 10a of the base area 101 to form a P-type emitter 102, which occupies a portion of the surface space of the base area 101 facing sunlight, and the P-type emitter 102 and the N-type base area 101 form the base 10. The diffusion sheet resistance of the P-type emitter 102 is in the range of 130Ω to 150Ω, and the surface diffusion concentration is E18 to E19.

[0065] In addition, the boron diffusion process also simultaneously generates unnecessary borosilicate glass on the front surface (i.e., the front surface 10a), back surface and side surfaces of the base area 101, and the borosilicate glass has a certain protective effect on the base area 101, and can prevent damage to the surface of the base area 101 caused by some manufacturing processes, that is, the unnecessary borosilicate glass can be used as a mask layer for the base area 101. Among them, the boron source used in the boron diffusion process contains liquid boron tribromide, and when the boron diffusion process is performed, the microcrystalline silicon phase is converted into a polysilicon phase.

[0066] Referring to FIG. 8, the rear surface of the base area 101 is subjected to a planarization process (eg, alkaline polishing).

[0067] The back surface is the surface of the solar cell facing away from sunlight, and the planarization process can form a back surface 10b that is a flat surface required for deposition of back surface film layers. During the planarization process, the borosilicate glass on the back surface is simultaneously removed.

[0068] In some embodiments, the method further includes the following steps before performing the polishing process: Remove the borosilicate glass on the back surface 10b of the base area 101 using the prepared mixed acid, which contains a hydrofluoric acid solution with a mass fraction of 0.1% to 10%, a sulfuric acid solution with a mass fraction of 10% to 20%, and a nitric acid solution with a mass fraction of 25% to 50%, the pickling time is 10 s to 180 s, and the pickling temperature is 7°C to 20°C. The back surface 10b after the pickling is washed with water and dried. Note that a porous structure appears on the back surface 10b of the base 10 after the pickling.

[0069] In some embodiments, the rear surface 10b may be polished using an alkaline solution. Specifically, the rear surface 10b is washed with an alkaline solution having a mass fraction of 5% to 15% to remove the porous silicon. Fine droplets of the alkaline solution are sprayed onto the rear surface 10b to roughen it, and the rear surface 10b is pre-cleaned with hydrofluoric acid having a mass fraction of 5% to 10%. The rear surface 10b is polished using a polishing solution at a polishing temperature of 70°C to 80°C and for a polishing time of less than 260 s, in which the polishing solution contains NaOH having a mass fraction of 1% to 15%, KOH having a mass fraction of 1% to 15%, and an additive having a mass fraction of 0.5% to 2.5%. The organic components in the etching solution are removed using a mixture of potassium hydroxide having a mass fraction of 5% to 15% and hydrogen peroxide having a mass fraction of 15% to 40%. The polished base 10 is washed with water and dried.

[0070] In some embodiments, because the boron concentration of the back surface 10b is low, etching with an alkaline solution can effectively improve the etching efficiency. The alkaline solution includes an organic base and / or an inorganic base, the inorganic base may be NaOH, KOH, Ga(OH)2, NH3.H2O, and the organic base may be triethylamine, nitrophenol, pyridine, quinine, colchicine, etc. The additive in the polishing solution may be a buffer solution consisting of sodium sulfonate, maleic anhydride, alkyl glycoside, etc. In some embodiments, the polishing loss of the base 10 is less than 0.3 g, and the back surface 10b can have a preset structure by controlling the polishing time and polishing temperature.

[0071] In some embodiments, the structure of the back surface 10b is different from that of the front surface 10a so as to enhance the solar absorption by different levels of structure. For example, the front surface 10a may have a pyramidal structure to mainly improve the anti-reflection ability. The back surface 10b may have a stacked stepped structure to maintain high density and uniformity of the tunnel oxide layer covering the back surface 10b and good passivation effect of the tunnel oxide layer on the back surface 10b.

[0072] Referring to FIG. 9, a tunnel oxide layer 121 and a doped conductive layer 122 are formed.

[0073] In some embodiments, the tunnel oxide layer 121 is formed by a deposition process, specifically, the material of the tunnel oxide layer 121 includes silicon oxide, the deposition process includes a chemical vapor deposition process, and the thickness of the tunnel oxide layer 121 in the direction perpendicular to the back surface 10b is 1 nm to 2 nm, for example, 1.2 nm, 1.4 nm, 1.6 nm, or 1.8 nm. In other embodiments, the tunnel oxide layer can also be formed by an in-situ generation process, specifically, in addition to silicon-based, the tunnel oxide layer can be generated in-situ by a process such as thermal oxidation process and nitric acid passivation.

[0074] In some embodiments, the tunnel oxide layer 121 is deposited on the back surface 10b using a variable temperature process and chemical vapor deposition. During the deposition process, the temperature ramp rate is controlled to be 0.5°C / min to 3°C / min, e.g., 1.0°C / min, 1.5°C / min, 2.0°C / min, or 2.5°C / min, the deposition temperature is controlled to be 560°C to 620°C, e.g., 570°C, 590°C, or 610°C, and the deposition time is controlled to be 3 min to 10 min, e.g., 4 min, 6 min, or 8 min.

[0075] In some embodiments, after the formation of the tunnel oxide layer 121, intrinsic polysilicon is deposited to form a polysilicon layer, and phosphorus ions are doped by ion implantation and source diffusion to form an N-type doped polysilicon layer, which is the doped conductive layer 122. In a direction perpendicular to the back surface 10b, the thickness of the doped conductive layer 122 can be 80 nm to 160 nm, for example, 100 nm, 120 nm, or 140 nm. In other embodiments, the doped conductive layer 122 has a dopant of the same conductivity type as the base 10, and when the base 10 is an N-type semiconductor, the doped conductive layer 122 is at least one of an N-type doped polysilicon layer, an N-type doped microcrystalline silicon layer, or an N-type doped amorphous silicon layer.

[0076] When the tunnel oxide layer 121 and the doped conductive layer 122 are formed by a deposition process, the borosilicate glass serves as a mask layer to protect the front surface 10a of the base area 101, so there is no need to limit the deposition area to the back surface by a mask during the deposition process, and the borosilicate glass on the front surface and the silicon oxide and polysilicon deposited on the front surface can be removed at the same time later by the same process. In this way, there is no need to provide a separate mask, which is advantageous for reducing process steps, shortening the process flow, and reducing process costs. In another embodiment, when the interface passivation layer is formed by an in-situ generation process, only polysilicon is deposited on the surface of the borosilicate glass on the front surface of the base.

[0077] In some embodiments, the deposition of the tunnel oxide layer 121 and the polysilicon layer, and the doping of the polysilicon layer are all formed in a low pressure chemical vapor deposition apparatus. The specific process includes the following: First, the base 10 after alkali polishing is placed in the deposition apparatus, 20L to 60L of oxygen source (e.g., oxygen, nitrous oxide, ozone) is introduced, the temperature in the deposition apparatus is heated to 560°C to 620°C at a heating rate of 0.5°C / min to 3°C / min, and the deposition time is 3min to 10min to form the tunnel oxide layer 121. After the introduction of oxygen is completed, a constant temperature stage is performed, and then an appropriate amount of silane gas is introduced to form the polysilicon layer. Finally, the polysilicon layer is in-situ doped to form the doped conductive layer 122.

[0078] Referring to FIG. 10, a first passivation layer 111, a second passivation layer 112, and a third passivation layer 113 are formed on the front surface 10a.

[0079] In some embodiments, before forming the first passivation layer, it is necessary to remove excess borosilicate glass, silicon oxide, and polysilicon that has been roll-plated onto the front surface 10a of the base 10. In other embodiments, before forming the first passivation layer, it is necessary to remove excess borosilicate glass and polysilicon that has been roll-plated onto the front surface of the base.

[0080] In addition, in another embodiment, after removing excess material, a thin silicon oxide layer is also grown on the front surface of the base. The formation process of the thin silicon oxide layer includes processes such as natural oxidation, thermal oxidation, wet oxidation, atomic layer deposition, plasma enhanced chemical vapor deposition, etc., and in a direction perpendicular to the surface of the base, the thin silicon oxide layer has a thickness of 0-3 nm, for example 1 nm, 1.5 nm or 2 nm.

[0081] In some embodiments, the first passivation layer 111, the second passivation layer 112 and the third passivation layer 113 can be formed using, but not limited to, chemical vapor deposition, low pressure chemical vapor deposition processes, plasma enhanced chemical vapor deposition (including direct plasma deposition and indirect plasma deposition), magnetron sputtering processes, etc., where the first passivation layer 111 comprises a dielectric material and the second passivation layer 112 comprises a first silicon nitride (Si m N n material (n / m ∈ [0.5, 1]), the third passivation layer 113 being silicon oxynitride SiO i N j Materials (j / i∈[0.1, 0.6]) are included. In the following, the combination of atomic layer deposition and tubular plasma enhanced chemical vapor deposition processes is described as an exemplary fabrication route.

[0082] Regarding the type of material of the first passivation layer 111, depending on whether the main passivation effect to be realized is field passivation or interface passivation, the material of the first passivation layer 111 can be divided into interface passivation material and field passivation material, where the interface passivation material includes at least one of silicon oxide or silicon oxynitride, and the field passivation material includes one or more of aluminum oxide, titanium oxide, gallium oxide, and hafnium oxide. In the following, the material of the first passivation layer 111 is mainly a field passivation material, specifically aluminum oxide Al X O y The material will be described as an example.

[0083] In some embodiments, the first passivation layer 111 is formed by an atomic layer deposition process, the reactants of which include trimethylaluminum and water, the deposition temperature is 150°C to 250°C, for example 175°C, 200°C or 225°C, the refractive index of the first passivation layer 111 at a wavelength of 632 nm is 1.6 to 1.7, for example 1.63, 1.65 or 1.67, and the thickness of the first passivation layer 111 in a direction perpendicular to the front surface 10a is 3 nm to 10 nm, for example 5 nm, 7 nm or 9 nm.

[0084] After forming the first passivation layer 111, the first passivation layer 111 is placed in a shielding gas atmosphere and subjected to high-temperature annealing to remove residual water molecules and organic functional groups. The annealing temperature is 450°C to 550°C, for example, 475°C, 500°C, or 525°C, and the annealing time is more than 10 minutes, for example, 12 minutes, 14 minutes, or 16 minutes. The above "shielding gas" may be any gas that does not participate in the reaction, for example, an inert gas, and in some embodiments, nitrogen gas may be used as the shielding gas.

[0085] In some embodiments, the second passivation layer 112 is formed by a plasma enhanced chemical vapor deposition process, in which the reactants are silane and ammonia gas, the flow ratio of silane to ammonia gas is 1 / 4 to 1 / 15, for example, 1 / 6, 1 / 9, or 1 / 12, and the pulse power per unit area is 30 to 40 mW / cm. 2 , e.g. 33mW / cm 2 , 35mW / cm 2 , or 37 mW / cm 2 By controlling the flow rate ratio and the pulse power per unit area, the first silicon nitride Si in the second passivation layer 112 can be m N n It is advantageous to have a preset level of atomic fraction of the material and thus a preset refractive index for the second passivation layer 112. Exemplarily, the first silicon nitride Si m N n The second passivation layer 112 including the material has an overall refractive index of 1.9 to 2.2, for example 2.0, 2.05 or 2.1 at a wavelength of 632 nm, while the second passivation layer 112 has a thickness of 40 nm to 60 nm, for example 45 nm, 50 nm or 55 nm, in a direction perpendicular to the front surface 10a.

[0086] In some embodiments, the third passivation layer 113 is formed by a plasma enhanced chemical vapor deposition process, in which the reactants are silane, nitrous oxide (laughing gas) and ammonia gas, the flow ratio of silane to nitrous oxide is 1 / 10 or more, e.g., 1 / 4, 1 / 6 or 1 / 8, and the pulse power per unit area is 25-40 mW / cm. 2 , e.g. 28mW / cm 2 , 30mW / cm 2 , 33mW / cm 2 , or 36 mW / cm 2 By controlling the flow rate ratio and the pulse power per unit area, the silicon oxynitride (SiO ) in the third passivation layer 113 can be reduced. i N jIt is advantageous to have a preset level of atomic ratio of the material, so that the third passivation layer 113 has a preset refractive index. Exemplarily, the third passivation layer 113 has an overall refractive index at a wavelength of 632 nm of 1.45 to 1.8, for example 1.5, 1.6 or 1.7, while the third passivation layer 113 has a thickness in the direction perpendicular to the front surface 10a of 20 nm to 50 nm, for example 25 nm, 30 nm, 35 nm, 40 nm or 45 nm.

[0087] Referring to FIG. 1, a fourth passivation layer 123, a first electrode 114 and a second electrode 124 are formed on the doped conductive layer 122.

[0088] If the fourth passivation layer 123 is a silicon nitride layer, it can be provided as 2-4 graded refractive index layers according to actual needs, that is, the refractive index of different silicon nitride sub-layers gradually decreases in the direction away from the base 10. Also, the reactant can be silane and ammonia gas, the ratio of the number of silicon atoms to the number of nitrogen atoms in the fourth passivation layer 123 can be 3.5-6.8, such as 4.2, 4.9, 5.7 or 6.3, the refractive index range can be 2.04-2.2, such as 2.08, 2.12 or 2.16, and the thickness range can be 60nm-100nm, such as 70nm, 80nm or 90nm.

[0089] After forming the fourth passivation layer 123, the first electrode 114 and the second electrode 124 can be formed by processes such as metallization, screen printing and high-temperature baking. In addition, after forming the electrodes, it is necessary to further perform a light annealing treatment, that is, the solar cell is heated at a temperature of 400°C to 700°C for 1 min to 6 min, for example, at 500°C or 600°C for 2 min, 3 min, 4 min or 5 min, and then simultaneously treated for 1 min to 6 min at a temperature of 150°C to 400°C and 1 to 6 solar irradiation intensities, for example, 200°C, 250°C, 300°C and 350°C, and for example, 1, 2, 3, 4 or 5 solar intensities.

[0090] Those skilled in the art will understand that the above embodiments are specific examples for realizing the present application, but various changes in form and details are possible in practice without departing from the spirit and scope of the present application. Since any person skilled in the art can make changes and modifications without departing from the spirit and scope of the present application, the scope of protection of the present application should be based on the scope limited by the claims.

Claims

1. a base having opposing front and back surfaces; a first passivation layer, a second passivation layer, and a third passivation layer located on the front surface and arranged in sequence in a direction away from the front surface; wherein the first passivation layer has a thickness of 3 nm to 10 nm, the second passivation layer has a thickness of 40 nm to 60 nm, and the third passivation layer has a thickness of 20 nm to 50 nm; The first passivation layer has a refractive index of 1.6 to 1.7, the second passivation layer has a refractive index of 1.9 to 2.2, and the third passivation layer has a refractive index of 1.45 to 1.8; the first passivation layer comprises a dielectric material, the second passivation layer comprises a first silicon nitride Si m N n material, where n / m ∈ [0.5, 1], and the third passivation layer comprises a silicon oxynitride SiO i N j material, where j / i ∈ [0.1, 0.6]; A solar cell characterized by:

2. The dielectric material includes one or more of aluminum oxide, titanium oxide, gallium oxide, and hafnium oxide; The solar cell according to claim 1 .

3. The dielectric material is aluminum oxide Al x O y material and y / x∈[1.1, 1.5], The solar cell according to claim 2 .

4. The solar cell further comprises a tunnel oxide layer and a doped conductive layer having a dopant of the same conductivity type as the base, the tunnel oxide layer and the doped conductive layer being located on the back surface and disposed in a direction away from the back surface. The solar cell according to claim 1 .

5. the first passivation layer further comprises a silicon oxide material interposed between the base and the dielectric material. The solar cell according to claim 1 .

6. A first intermediate layer is provided between the first passivation layer and the second passivation layer, the material of the first intermediate layer is a silicon oxide material, and the thickness of the first intermediate layer is 0.5 nm to 3 nm; The solar cell according to claim 1 .

7. A second intermediate layer is provided between the second passivation layer and the third passivation layer, the material of the second intermediate layer is a silicon oxycarbonitride material, and the thickness of the second intermediate layer is less than 10 nm; The solar cell according to claim 1 .

8. A cell string formed by connecting a plurality of solar cells according to any one of claims 1 to 7; a sealant film for covering a surface of the cell string; a cover plate for covering a surface of the sealant film that faces away from the cell string; A photovoltaic module comprising:

Citation Information

Patent Citations

  • Anti-reflective film and preparation method thereof

    CN101866956A

  • A bifacial PERC solar cell structure and its fabrication process

    CN109087956B

  • PECVD technology-based preparation method of high-efficiency and low-cost N-type TOPCon battery

    CN112349816A

  • Solar cell and preparation method thereof

    CN112447863A

  • Method for manufacturing solar cell

    JP2014045187A