Recovery of nickel and cobalt from Li-ion batteries or their waste
A slag composition with controlled MnO, CaO, and Li2O levels addresses the issue of refractory brick corrosion in Li-ion battery recycling, enhancing furnace longevity and economic efficiency by suppressing magnesia dissolution.
Patent Information
- Application Number
- JP2023572896
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-26
- Filing Date
- 2022-05-13
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2042-05-13
AI Technical Summary
Existing methods for recovering nickel and cobalt from Li-ion batteries result in increased corrosion of magnesia-containing refractory bricks due to high furnace temperatures, leading to high maintenance costs and reduced furnace lifetime.
A method involving a slag composition with specific ranges of MnO, CaO, Li2O, and other components that suppresses the dissolution of magnesia from refractory bricks, maintaining furnace integrity and improving the process economy by reducing wear and tear.
The method effectively minimizes the corrosion of magnesia-containing refractory bricks, extending furnace life and reducing maintenance costs while efficiently recovering nickel and cobalt from Li-ion batteries.
Smart Images

Figure 0007573125000001 
Figure 0007573125000002 
Figure 0007573125000003
Abstract
Description
[Technical field]
[0001] The present invention is in the field of pyrometallurgy, and more particularly, relates to the recovery of Ni and Co from Li-ion batteries or their waste materials. [Background technology]
[0002] Electric vehicles have experienced unprecedented growth in recent years, driven by new legislation, particularly in Europe and China, and are reducing overall vehicle CO 2 It is designed to gradually reduce the footprint and limit air pollution in cities. This growth is expected to continue for the next few decades. The adoption of electric vehicles depends heavily on the performance of the batteries used to store the electrical energy. To obtain the highest energy density while keeping costs down, rechargeable Li-ion batteries are currently the preferred choice. Many of these batteries contain cathodes based on the transition metals Ni, Mn, and Co, and are therefore also known as NMC batteries. With the growth of the electric mobility market, the demand for these metals is expected to increase significantly.
[0003] The demand for Ni and Co may even exceed the world's production capacity. Co is particularly important since it is currently only produced as a by-product of the Ni and Cu industries. The nickel market is significantly larger than the cobalt market. Most of the Ni is used in the production of stainless steels, where the purity of the Ni is less important. However, high-purity Ni and high-purity Co metal or compounds are already in short supply. In light of the above, the recovery of Ni and Co from used Li-ion batteries or their waste is therefore an attractive proposition.
[0004] There are several known methods for recycling Li-ion batteries, in which the oxides of nickel, cobalt, and copper are reduced to metals at high temperatures and concentrated in alloy phases.
[0005] WO2017121663 describes a slag composition produced in an industrial process and discloses the effect of MnO on slag viscosity and cobalt recovery. The main slag components described therein are CaO, SiO 2 , Al 2 O 3 , Li 2 O, and MnO (MnO 2 ). The disclosed MnO concentration in their slags is very low, and the above teaching is to limit the amount of MnO in the slags. Elwert et al. (Phase composition of high lithium slags from the recycling of lithium-ion batteries: World of Metallurgy-ERZMETALL, Vol. 65(3), 2012, pp. 163-171) analyzed the phase composition of three different slags with the aim of developing a potential slag beneficiation method for lithium recovery. Hu et al. (Recovery of Co, Ni, Mn, and Li from Li-ion batteries by smelting reduction-Part II: A pilot-scale demonstration: Journal of Power Sources, Vol. 483, 2021, pp. 229089) proposed a method for recycling Li-ion batteries by smelting them with fluxing agents at temperatures above 1500 °C to obtain slags and alloys containing Ni, Co, and Mn. Both Elwert and Hu describe slag compositions having MnO concentrations well below 10%.
[0006] On the other hand, modern Li-ion batteries typically have a higher Mn content. This makes the formation of slags containing small amounts of Mn more difficult, since it would require either diluting the Mn by adding large amounts of fluxing agents or choosing more reducing conditions in such processes to drive more Mn into the alloy phase rather than the slag phase. The former option would increase the consumption of fluxing agents and the total amount of slag obtained, while the latter option would increase the complexity of any subsequent hydrometallurgical processing of the alloy due to its higher Mn content. Both options would significantly reduce the economics of the process.
[0007] WO12140951, WO13080266, and WO20013294 propose a method for recycling Li-ion battery scrap to recover Ni and Co while fixing impurities such as Fe and P in the slag phase. It is stated that Mn may be the main component of the resulting slag, but the preferred range or specific effect of MnO in such slag is not specified. Furthermore, the focus of WO12140951 and WO13080266 is on low melting point Fe-rich slag.
[0008] Vest et al. (Friedrich Slag design for lithium recovery from spent batteries: Int. Work. Met. Interact., Vol. 9(93), 2010, pp. 93-106) describe theoretical calculations for MnO-rich slags. Wittkowski et al. (Speciation of Manganese in a Synthetic Recycling Slag Relevant for Lithium Recycling from Lithium-Ion Batteries: Metals, Vol. 11(2), 2021, pp. 188) analyze the phase composition of various Li-containing slags from recycling Li-ion batteries.
[0009] In CN103924088 and EP3269832, alloys containing Co and / or Ni and SiO2 A bath smelting process for waste batteries is described, which produces a slag rich in MnO and MnO.
[0010] None of the above prior art teaches the slag composition according to the present invention.
[0011] Even when disclosing slags with a relatively higher MnO content, all the above documents do not teach the conditions of the present process and still do not mention any effect of the resulting MnO-rich slag composition on the walls of the furnace. Typically, the furnace walls are made of refractory bricks. The main component of such bricks is magnesia. Examples are magnesia bricks (magnesia content usually above 90%) or magnesia-chrome bricks (magnesia content usually 50-70%). It has been observed that the magnesia of the walls dissolves in the general slag during the operation of the furnace, resulting in wear or corrosion of the furnace walls over time. This is a recurring problem, leading to high maintenance costs, since the furnace needs to be shut down and the refractory bricks need to be replaced periodically. This problem is even more pronounced at higher operating temperatures, e.g. above 1550°C. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] WO2017121663 [Patent Document 2] WO12140951 [Patent Document 3] WO13080266 [Patent Document 4] WO20013294 [Patent Document 5] CN103924088 [Patent Document 6] EP3269832 [Non-patent literature]
[0013] [Non-Patent Document 1] Elwert et al., Phase composition of high lithium slags from the recycling of lithium-ion batteries: World of Metallurgy-ERZMETALL, Vol. 65(3), 2012, pp. 163-171 [Non-Patent Document 2] Hu et al., Recovery of Co, Ni, Mn, and Li from Li-ion batteries by smelting reduction-Part II: A pilot-scale demonstration: Journal of Power Sources, Vol. 483, 2021, p. 229089 [Non-Patent Document 3] Vest et al., Friedrich Slag design for lithium recovery from spent batteries: Int. Work. Met. Interact., 9(93), 2010, 93-106 [Non-Patent Document 4] Wittkowski et al., Specification of Manganese in a Synthetic Recycling Slag Relevant for Lithium Recycling from Lithium-Ion Batteries: Metals, vol. 11(2), 2021, p. 188 Summary of the Invention [Problem to be solved by the invention]
[0014] It is therefore an object of the present invention to provide a special MnO and Li refractory brick composition that is adapted to cause less corrosion during operation of the magnesia-containing refractory brick. 2 The objective of the present invention is to provide a process for the recovery of Ni and Co from Li-ion batteries, which simultaneously improves the life of the furnace by operating with a slag system rich in O. The reduction in wear achieved contributes favorably to the overall economics of the process of the present invention. [Means for solving the problem]
[0015] According to a first embodiment, a method for recovering Ni and Co from Li-ion batteries or waste thereof comprises: - providing a furnace lined with magnesia-containing refractory bricks; - providing a charge comprising a slag former and Li-ion batteries or waste materials thereof; - smelting the charge under reducing conditions, thereby obtaining an alloy containing a large proportion of Ni and Co, and a slag; The slag comprises: 10% <MnO<40%; (CaO+1.5*Li 2 O) / Al 2 O 3 >0.3; CaO+0.8*MnO+0.8*Li 2 O<60%; (CaO+2*Li 2 O+0.4*MnO) / SiO 2 ≥ 2.0; Li 2 O ≥ 1%; and Al 2 O 3 +SiO 2 +CaO+Li 2 O+MnO+FeO+MgO>85% It is characterized by having a mass percent composition according to:
[0016] "Slag forming agents" include, for example, CaO, Al 2 O 3 , and SiO 2 Other slag formers known to those skilled in the art may also be present. The slag forming compounds may be added as such or may be obtained in situ from easily oxidized metals, such as aluminum, present in the charge.
[0017] By "Li-ion batteries or waste materials" is meant electrode materials or pre-processed battery materials, including, for example, new or waste Li-ion batteries, used or end-of-life batteries, manufacturing or battery scrap, e.g., after shredding or sorting, so-called "black mass", however these should still contain significant amounts of Co and / or Ni.
[0018] A "major portion" of an element or compound means greater than 50% by weight of the corresponding amount present in the charge, which may also include a range having a lower value selected from 55%, 60%, 65%, 70%, and 75% and an upper value selected from 80%, 85%, 90%, 95%, and 100%.
[0019] The content of MnO in the slag plays an important role in the present invention. A minimum of about 10% in the slag is required to see an effect in inhibiting the dissolution of MgO from the magnesia-containing refractory bricks lining the furnace into the slag. It is preferable to have at least 15% MnO. Furthermore, it is beneficial to have a MnO content of 10-40% in a relatively small amount of slag, since the reduction in the volume of the slag helps to inhibit MgO dissolution. On the other hand, if more fluxing agent is added, which increases the overall volume of the slag and dilutes the proportion of MnO, the amount of MgO that dissolves from the refractory bricks increases, thus having a negative effect.
[0020] Also, the upper limit of MnO in the slag is important because it helps to keep the melting temperature of the slag low enough. Slags containing up to 40% MnO according to the invention melt below 1500°C. The lower temperature, in combination with the amount of MnO, is beneficial in suppressing the dissolution of MgO from the magnesia-containing refractory brick. Amounts of MnO greater than 40% increase the melting point of the slag above 1500°C, so it is particularly important when the slag contains a relatively higher amount of Al. 2 O 3 , e.g., more than 50% Al 2 O 3 It is not very preferable if it also contains
[0021] According to a further embodiment, the content of MnO in the slag is less than or equal to 30%.
[0022] The percentage of Mn in slags is standardized as "percent MnO". However, the exact oxidation state of Mn in such slags is not always clear. Thus, manganese oxide ("MnO") may consist of the monoxide species MnO and manganese dioxide MnO. 2 However, it is expected that the occupancy of the monoxide species MnO will be much higher than 95%, especially under the selected reduction reaction conditions.
[0023] MnO typically has a green color, while MnO 2 It typically has a dark brown or dark grey color, hence the name "manganese black". Only if the monoxide content is high enough will the green color be visible.
[0024] According to a further embodiment, the content of CaO in the slag is greater than or equal to 15%, preferably greater than or equal to 20%.
[0025] According to a further embodiment, the content of CaO in the slag is less than or equal to 50%, preferably less than or equal to 30%.
[0026] A minimum of 15% CaO ensures that the slag remains sufficiently fluid and easy to handle. Since Ca and Mg share similar chemical sites in the slag, CaO helps to inhibit dissolution of Mg from the magnesia-containing refractory bricks, so a larger amount of CaO, e.g. 20% or more, is preferred. Operating the process with the preferred upper limit of 30% CaO helps to maintain the melting temperature of the slag below 1600°C. Too much CaO, e.g. more than 50%, should be avoided as it significantly increases the melting temperature of the slag.
[0027] In addition to MnO and CaO, Li 2 O also inhibits the dissolution of Mg from magnesia-containing refractory bricks, but SiO 2It was further observed that increasing the amount of CaO had a negative effect. This can be seen in the formula (CaO+2*Li 2 O+0.4*MnO) / SiO 2 ≧2.0. When recycling Li-ion batteries, the Li in the slag 2 The amount of O is expected to be important.
[0028] According to a further embodiment, too much Al 2 O 3 The Al in the slag increases the melting point of the slag. 2 O 3 The content is <50%, preferably <40%.
[0029] According to a further embodiment, the content of Fe in the slag is less than or equal to 25%, preferably less than or equal to 10%.
[0030] According to a further embodiment, Al 2 O 3 , SiO 2 , CaO, Li 2 The total content of O, MnO, FeO, and MgO is 90% or more, and preferably 95% or more.
[0031] According to a further embodiment, (CaO+2*Li 2 O+0.4*MnO) / (SiO 2 +0.2*Al 2 O 3 ) is >1.5.
[0032] The composition of the slag and the operating temperature are important considerations for the methods described herein. The present invention uses compounds that protect the furnace walls (e.g., MnO, CaO, Li 2 O) will inevitably have a negative effect on the furnace wall (e.g., Al from Al in the feed material). 2 O 3 ) or is otherwise necessary (e.g., SiO 2 required to lower the melting point of the slag). 2) compounds. Furthermore, the slag composition region allows for suitable fluidity of the slag at the desired operating temperature and minimal overheating of the slag. The lowest possible temperature is preferred while still remaining above the melting point of the alloy.
[0033] This balance is reflected in the conditions of the presented method as well as the composition of the slag itself.
[0034] According to a further embodiment, the step of smelting the charge is carried out at a temperature of at least 1400° C. to ensure complete melting of the metallurgical charge and at a maximum of 300° C. above the liquidus point of the slag, preferably at a maximum of 100° C. above the liquidus point of the slag. A lower limit is preferred to avoid even partial solidification of the produced alloy and slag. An upper limit is preferred to avoid overheating of the slag. Higher temperatures promote dissolution of Mg from the magnesia-containing refractory bricks. Therefore, lower temperatures are generally preferred for energy savings as well as reduced wear. Overheating the slag has a negative effect on the dissolution of the magnesia-containing refractory bricks by the slag.
[0035] CaO and Li in the described slags 2 O'Al 2 O 3 to aid in maintaining the melting point of the slag sufficiently low, preferably below 1700°C, more preferably below 1650°C, even more preferably below 1600°C, and most preferably below 1550°C.
[0036] Despite their beneficial effects on the life of magnesia-containing refractory bricks, CaO, MnO, and Li in the slag 2 It is also important to limit the amount of O in the combination, because CaO+0.8*MnO+0.8*Li 2 This is because it is believed that if O exceeds 60%, the melting point of the slag becomes too high.
[0037] According to a further embodiment, the smelting step comprises: - sampling the slag; - cooling the slag sample and evaluating its color; and - terminating the smelting process if the slag sample is green, or - If the slag sample is not green, pO 2 The process of adjusting the levels to achieve more reducing conditions and then continuing the smelting process. The method includes the further step of:
[0038] "Sampling the slag" means taking a small sample of the slag and evaluating its color while the process continues under selected conditions.
[0039] Color assessment can be easily performed visually. Compared to chemical analysis of the slag, monitoring the color change quickly and efficiently provides an indication that the slag contains a certain minimum percentage of MnO. As described in more detail below, it has been further observed that the green color of the slag also indicates that a significant portion of the Co contained in the feed material has been reduced and transferred to the alloy. Without wishing to be bound by theory, it is believed that the color change to green is due to the reduction of MnO. 2 to MnO, but is actually believed to result from the reduction of the typically darker oxides of, for example, Ni and Co.
[0040] Visual inspection is a quick and easy way to know if process conditions should be adjusted, optimized, and / or terminated, which can save time and operating costs. Color confirmation is therefore a reliable indicator of the progress of metallurgical operations.
[0041] In this context, "green" refers to the following range according to the ASTM D1535-14(2018) standard: - Hues from 5GY to 5BG; - Lightness: ≥ 3; and - Saturation: ≥ 3 A color is defined as a color having a hue, lightness, and saturation of 100%.
[0042] An example of the color green is shown in the "Geological Rock-Color Chart with Genuine Munsell Color Chips" created by Munsell Color in 2009.
[0043] The operating conditions are selected to oxidize most of the Mn to slag and reduce most of the Co and Ni to the alloy. Preferably, >90%, more preferably >95%, and most preferably >98% of the Co and Ni are collected in the alloy to make the process most economical. 2 Levels are easily adjusted to achieve these favorable yields.
[0044] According to a further embodiment, pO 2 Level is 10 -7 >pO 2 >10 -12 , preferably pO 2 <10 -8 , more preferably pO 2 <10 -8.5 , most preferably pO 2 <10 -9 Adjust to.
[0045] Therefore, 10 -8 , 10 -8.5 , and 10 -9 Preferred pO 2 Level, as well as 10 -12 The limit value of is 10 -7 pO 2 This indicates more reducing conditions compared to the levels.
[0046] According to a further embodiment, the slag is green in color. During smelting of the charge at reducing conditions, the color of the slag typically changes from dark gray or dark brown to green as the process progresses.
[0047] According to a further embodiment, the furnace is an electric furnace. By using an electric furnace or electric arc furnace (EAF), there is more flexibility when higher operating temperatures are desired or required. Another advantage is the possibility to benefit from off-peak electricity prices or electricity produced by environmentally friendly green sources, for example local wind farms.
[0048] According to a further embodiment, the Li-containing metallurgical slag comprises: 10% <MnO<40%; (CaO+1.5*Li 2 O) / Al 2 O 3 >0.3; CaO+0.8*MnO+0.8*Li 2 O<60%; (CaO+2*Li 2 O+0.4*MnO) / SiO 2 ≥ 2.0; Li 2 O ≥ 1%; and Al 2 O 3 +SiO 2 +CaO+Li 2 O+MnO+FeO+MgO>85% The mass percent composition according to
[0049] According to a further embodiment, the Li-containing metallurgical slag has a green color.
[0050] According to a further embodiment, the content of MnO in the Li-containing metallurgical slag is less than or equal to 30%.
[0051] According to a further embodiment, the content of CaO in the Li-containing metallurgical slag is greater than or equal to 15%, preferably greater than or equal to 20%.
[0052] According to a further embodiment, the content of CaO in the Li-containing metallurgical slag is less than or equal to 50%, preferably less than or equal to 30%.
[0053] According to a further embodiment, Al in the Li-containing metallurgical slag 2O 3 The content is 50% or less, preferably 40% or less.
[0054] According to a further embodiment, the content of Fe in the Li-containing metallurgical slag is not more than 25%, preferably not more than 10%. In FeO-rich slags containing more than 10% FeO, or even more than 20% FeO, respectively, it is not possible to reduce CoO to metallic Co without also transferring relatively large amounts of metallic Fe to the alloy phase, which is less desirable since it significantly increases the cost of any hydrometallurgical post-treatment of the resulting alloy.
[0055] According to a further embodiment, the Li-containing metallurgical slag is used as a slag former in a pyrometallurgical recycling process. The resulting metallurgical slag contains CaO and SiO 2 can be used as a slag former in new operations.
[0056] According to a further embodiment, the Li-containing metallurgical slag is used as a slag former in the method according to the first embodiment, thereby partially or completely replacing the slag former in the step of providing a charge comprising the slag former.
[0057] By recycling the generated metallurgical slag in new operations, the operating conditions of the process, e.g. pO 2 This allows for more flexibility in the selection of levels: for example, if more oxidizing conditions are used, thereby sending more Co and / or Ni to the slag, it is conceivable that these valuable metals would not be lost, but rather would be recovered in a new work cycle, where perhaps more reducing conditions would be used to recover more of the Co and / or Ni.
[0058] If this metallurgical slag is reused as a slag former in a new process or as starting slag in the same process, it should be taken into account that the incoming battery or its waste may contain additional amounts of compounds such as Al, Mn, or Li, which will be present in the slag after its oxidation. 2 O 3 , MnO, or Li 2 The amount of each of Li 2 The amount of O is not considered to be very important, but Al 2 O 3 And the amount of MnO has a more direct effect on the melting temperature. In a further embodiment, the preferred upper limit of MnO is 30% to allow for a margin for fresh MnO coming in from the new charge.
[0059] Due to the incoming new compounds, metallurgical slag according to the present invention can only be reused for a limited number of cycles. To determine whether the slag can be subsequently reused, the slag composition should be analyzed and compared to the compositional specifications set forth herein. Bleeding at least a portion of the metallurgical slag and diluting it with fresh slag formers for reuse can be utilized as a viable long-term option.
[0060] As mentioned above, the slag of the present invention helps to significantly suppress the dissolution of MgO from the refractory bricks. However, this cannot be avoided completely. This leads to another positive side effect when recycling the slag. The dissolved MgO from the refractory bricks (resulting from the dissolution of a small amount of MgO during the previous smelting process) accumulates in the slag, which is then converted into MnO, Li 2 In combination with O and CaO, this tends to inhibit further corrosion of the refractory brick, making reuse of the resulting slag particularly attractive.
[0061] The following examples are provided to further illustrate embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS EXAMPLES
[0062] Example 1 The dissolution of MgO from the walls of a magnesia-containing crucible was measured using several different slag compositions. Various compounds contained in Li-ion batteries or their waste products, and their respective oxides, e.g., FeO, Al 2 O 3 , Li 2 O, and MnO as fluxing agents, CaO and SiO 2 The total mass of the oxides added was 1000 g. 2 O 3 , Li 2 The ratio of O, MnO, and MnO was chosen to represent a typical composition of existing Li-ion batteries.
[0063] The crucibles were gradually heated at a heating rate of 150° C. / h using an induction furnace. When the slag was completely melted, the crucibles were maintained at a temperature of 1400, 1450, or 1500° C. After 2 hours of heating, the molten slag was removed from the crucibles and quenched with water. Table 1 lists the compositions of the slags obtained in this example.
[0064] [Table 1]
[0065] The MgO concentrations in the above slags were relatively low (0.9%–3.9%). This result indicates that the dissolution of MgO from the crucible walls was sufficiently suppressed under the selected conditions.
[0066] Experiments were performed with slag compositions having neither Ni, Co nor Cu, since the amounts of these metals in the final slag are typically very small and therefore do not essentially affect the slag properties.
[0067] Comparative Example 2 The dissolution of MgO from the walls of a magnesia-containing crucible when different slag compositions were used was measured. Various compounds contained in Li-ion batteries or their waste products, respectively, their oxides, e.g. FeO, Al 2 O 3 , and MnO as fluxing agents, CaO and SiO 2 The total mass of the oxides added was 1000 g.
[0068] The crucible was gradually heated at a heating rate of 150° C. / h using an induction furnace. When the slag was completely melted, the crucible was maintained at a temperature of 1400 or 1450° C. for 2 hours. After 2 hours of heating, the molten slag was removed from the crucible and quenched with water. Table 2 lists the composition of the slag obtained in this example.
[0069] [Table 2]
[0070] In comparison with slags 1-1 to 1-3 used in Example 1, the SiO 2 Adjust the content to be higher, CaO, Li 2 The O and / or MnO contents were adjusted to be lower. The measured MgO concentrations in the slags were relatively high (8.7%-13.2%), indicating that a relatively large amount of MgO was dissolved from the crucible into each slag.
[0071] As in Example 1, the slag contained neither Ni, Co, nor Cu.
[0072] Discussion of Examples 1 and 2 The slag obtained in Example 1 contained less MgO than the slag obtained in Comparative Example 2. Under the conditions of Example 1, no visible deterioration of the MgO crucible was observed, whereas under the conditions of Example 2, the walls of the crucible became thinner. As shown in Example 1, the relatively low concentration of SiO 2 , as well as relatively high combined concentrations of Li2 The slag containing O, CaO, and / or MnO suppressed the dissolution of MgO. More specifically, the dissolution of MgO in the slag was suppressed by the reaction of (CaO + 2Li 2 O+0.4MnO) / SiO 2 was efficiently inhibited when the ratio of
[0073] Example 3 500 kg of spent rechargeable Li-ion batteries were fed into a 1 m diameter furnace freshly lined with 200 mm chrome-magnesia refractory bricks. 80 kg of limestone and 20 kg of sand were added along with the Li-ion batteries. A bath temperature of 1450-1500 °C was maintained, which is suitable to keep both the slag and alloy sufficiently fluid for easy tapping and handling. 2 Injection was used to provide heat by oxidation of Al and C in the cell. The injection rate was set to strongly reducing conditions, i.e., 10 -9 pO 2 The temperature was selected to ensure a high temperature. Natural gas was added to compensate for the heat losses in the furnace. After 1 hour of heating, the resulting alloy and slag were separated by tapping. Table 3 shows the analysis of the input and production phases of the process.
[0074] [Table 3]
[0075] No visible deterioration of the magnesia-containing refractory bricks was observed during the treatment of the batteries. The concentration of MgO in the resulting slag was only 1.2%, which corresponds to a loss of 2.3 kg of MgO from the refractory bricks, which is considered low. (CaO+2Li 2 O+0.4MnO) / SiO 2 The ratio of slag to furnace wall was 4.3. Therefore, this slag effectively suppressed the wear of furnace wall.
[0076] Comparative Example 4 500 kg of spent rechargeable Li-ion batteries were fed into a 1 m diameter furnace freshly lined with 200 mm chrome-magnesia refractory bricks. 50 kg of limestone and 50 kg of sand were added along with the Li-ion batteries. A bath temperature of 1450-1500 °C was maintained, which is suitable to keep both the slag and alloy sufficiently fluid for easy tapping and handling. 2 Injection was used to provide heat by oxidation of Al and C in the cell. The injection rate was set to strongly reducing conditions, i.e., 10 -9 pO 2 The temperature was selected to ensure a high temperature. Natural gas was added to compensate for the heat losses in the furnace. After 1 hour of heating, the resulting alloy and slag were separated by tapping. Table 4 shows the analysis of the input and production phases of the process.
[0077] [Table 4]
[0078] The concentration of MgO in the resulting slag was 9.0%, which corresponds to a loss of 19.8 kg of MgO from the refractory bricks and thus a significant wear and tear on the furnace walls.
[0079] (CaO+2Li 2 O+0.4MnO) / SiO 2 The ratio was 1.7.
[0080] Example 5 500 kg of spent rechargeable Li-ion batteries were fed into a 1 m diameter furnace freshly lined with 200 mm chrome-magnesia refractory bricks. 50 kg of limestone and 50 kg of sand were added along with the Li-ion batteries. A bath temperature of 1450-1500 °C was maintained, which is suitable to keep both the slag and alloy sufficiently fluid for easy tapping and handling. 2 Injection was used to provide heat by oxidation of Al and C in the cell. The injection rate was set to strongly reducing conditions, i.e., 10 -9 pO 2The temperature was selected to ensure a high temperature. Natural gas was added to compensate for the heat loss in the furnace. After 1 hour of heating, the resulting alloy and slag were separated by tapping. Table 5 shows the analysis of the input and production phases of the process.
[0081] [Table 5]
[0082] The concentration of MgO in the resulting slag was 2.8%, which corresponds to a loss of 7.4 kg of MgO from the refractory bricks. (CaO + 2Li 2 O+0.4MnO) / SiO 2 The ratio was 2.8.
[0083] Consideration of Examples 3, 4, and 5 In Example 3 and Comparative Example 4, the same amount and composition of cells were charged into the furnace, but with different ratios of limestone and sand. The resulting slag 3 had a higher concentration of CaO and a lower concentration of SiO than slag 4. 2 It contained.
[0084] (CaO+2Li 2 O+0.4MnO) / SiO 2 The ratios were 4.3 and 1.7 for slag 3 and 4, respectively. Only 2.3 kg of MgO was dissolved in slag 3, whereas a significantly larger amount of 19.8 kg of MgO was dissolved in slag 4.
[0085] In Example 5, the same limestone to sand ratio as in Comparative Example 4 was kept, but cells containing higher concentrations of Mn and Li were fed to the furnace. The resulting slag 5 had higher concentrations of MnO and Li than slag 4. 2 It contained O.
[0086] In slag 5, (CaO + 2Li 2 O+0.4MnO) / SiO 2 The ratio of MgO to Li was 2.8, and 7.4 kg of MgO was dissolved. Therefore, this example shows the effect of the combined MnO and Li 2These results show a beneficial effect of O.
[0087] As shown in Examples 3 and 5, lower concentrations of SiO 2 , as well as higher combined concentrations of Li 2 Slags containing O, CaO, and MnO are better suited to inhibit the dissolution of MgO.
[0088] Example 6 500 kg of spent rechargeable Li-ion batteries were fed into a 1 m diameter furnace freshly lined with 200 mm chrome-magnesia refractory bricks. 189 kg of slag produced in Example 3 was added along with the Li-ion batteries. The bath temperature was maintained at 1450-1500°C, which is suitable to keep both the slag and the alloy sufficiently fluid for easy tapping and handling. 2 Injection was used to provide heat by oxidation of Al and C in the cell. The injection rate was set to strongly reducing conditions, i.e., 10 -9 pO 2 The temperature was selected to ensure a high temperature. Natural gas was added to compensate for the heat loss in the furnace. After 1 hour of heating, the resulting alloy and slag were separated by tapping. Table 6 shows the analysis of the input and production phases of the process.
[0089] [Table 6]
[0090] No visible degradation of the magnesia-containing refractory brick was observed during the treatment of the battery. The concentration of MgO in the resulting slag was only 1.2%, corresponding to a loss of 1.4 kg of MgO from the refractory brick, which is even less degradation than in Example 3. (CaO+2Li 2 O+0.4MnO) / SiO 2 The ratio of β-magnesia to β-magnesia was 6.8. Therefore, this slag effectively suppressed the wear of the furnace wall made of magnesia-containing refractory bricks.
[0091] Overall conclusion The metallurgical slag according to the invention is suitable for recovering valuable metals, such as Ni and Co, from Li-ion batteries or their waste, while minimizing deterioration of the magnesia-containing refractory bricks of the furnace.
Claims
1. A method for recovering Ni and Co from Li-ion batteries or waste thereof, comprising: providing a furnace lined with magnesia-containing refractory bricks; - providing a charge comprising a slag former and Li-ion batteries or waste materials thereof; - smelting the charge under reducing conditions, thereby obtaining an alloy containing a large proportion of Ni and Co, as well as a slag; The slag comprises: 10%<MnO<40%; (CaO+1.5*Li 2 O) / Al 2 O 3 >0.3; CaO+0.8*MnO+0.8*Li 2 O<60%; (CaO + 2*Li 2 O+0.4*MnO) / SiO 2 ≧2.0; Li 2 O≧1%; and A 2 O 3 +SiO 2 +CaO+Li 2 O+MnO+FeO+MgO>85% The method of claim 1, characterized in that the composition has a weight percent composition according to:
2. 2. The method according to claim 1, wherein the content of MnO in the slag is less than or equal to 30%.
3. 2. The method of claim 1, wherein the content of CaO in the slag is 15% or more, or 20% or more, and the content of CaO in the slag is 50% or less, or 30% or less.
4. Al in slag 2 O 3 The method according to claim 1 , wherein the content of is 50% or less, or 40% or less.
5. The method of claim 1, wherein the Fe content in the slag is 25% or less, or 10% or less.
6. A 2 O 3 , SiO 2 , CaO, Li 2 2. The method of claim 1 , wherein the sum of O, MnO, FeO, and MgO is 90% or more, or 95% or more.
7. (CaO + 2*Li 2 O+0.4*MnO) / (SiO 2 +0.2*Al 2 O 3 2. The method of claim 1 , wherein R 1 is >1.
5.
8. 2. The method of claim 1, wherein the step of smelting the charge is carried out at a temperature of at least 1400° C. and up to 300° C. above the liquidus point of the slag, or up to 100° C. above the liquidus point of the slag, thereby avoiding overheating.
9. The smelting process is - sampling the slag; - cooling the slag sample and evaluating its color; and - terminating the smelting process if the slag sample is green, or - If the slag sample is not green, the pO 2 and continuing the smelting process after adjusting the levels to achieve more reducing conditions, thereby obtaining an alloy and slag containing a majority of Ni and Co. comprising the further step of The green color ranges according to ASTM D1535-14 (2018) standard: - 5GY to 5BG hues; - Lightness: ≧3; and - Saturation: ≧3 The method of claim 1 , wherein the color is defined as a color having a hue, a lightness, and a saturation of 100%.
10. pO 2 Level 10 -7 >pO 2 >10 -12 , or pO 2 <10 -8, or pO 2 <10 -8.5 , or pO 2 <10 -9 The method of claim 1 , wherein the
11. 10. The method of claim 9, wherein the charge is smelted until the slag sample is green in color.
12. The method of claim 1 , wherein the furnace is an electric furnace.
13. 10%<MnO<40%; (CaO+1.5*Li 2 O) / Al 2 O 3 >0.3; CaO+0.8*MnO+0.8*Li 2 O<60%; (CaO + 2*Li 2 O+0.4*MnO) / SiO 2 ≧2.0; Li 2 O≧1%; and A 2 O 3 +SiO 2 +CaO+Li 2 O+MnO+FeO+MgO>85% Li-containing metallurgical slag having a mass percent composition according to
14. 14. The Li-containing metallurgical slag of claim 13, having a green color.
15. The Li-containing metallurgical slag according to claim 13, wherein the content of MnO in the slag is 30% or less.
16. 14. The Li-containing metallurgical slag according to claim 13, wherein the CaO content in the slag is 15% or more, or 20% or more, and the CaO content in the slag is 50% or less, or 30% or less.
17. Al in slag 2 O 3 The Li-containing metallurgical slag according to claim 13, wherein the content of is 50% or less, or 40% or less.
18. 14. The Li-containing metallurgical slag according to claim 13, wherein the content of Fe in the slag is 25% or less, or 10% or less.
19. 14. Use of the Li-containing metallurgical slag according to claim 13 as a slag-forming agent in a dry metallurgical recycling process for Li-ion batteries.
20. 19. Use of a Li-containing metallurgical slag according to any one of claims 13 to 18 as a slag-forming agent in the method according to any one of claims 1 to 12, thereby partially or completely replacing the slag-forming agent in the step of providing a charge comprising the slag-forming agent.
Citation Information
Patent Citations
Method for recovering and treating waste batteries or materials containing Co and / or Ni
CN103924088A
Method of recycling and processing waste battery
EP3269832A1
Method for recovering manganese alloy from manganese oxide waste
JP2012193424A
Lithium-rich metallurgical slag
JP2019502826A
Process for recovering valuable metal
JP2021031760A