Optical sheet, liquid crystal display device, and method for manufacturing optical sheet

The optical sheet design with a polyurethane resin adhesive layer addresses bending and adhesive leakage issues, ensuring even light transmission and manufacturing efficiency in liquid crystal display devices.

JP7573167B2Active Publication Date: 2024-10-25DAI NIPPON PRINTING CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023211798
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-10-25
Estimated Expiration
2040-02-13

AI Technical Summary

Technical Problem

Optical sheets in liquid crystal display devices, particularly in-vehicle displays, bend due to their weight, leading to uneven light transmission and adhesive leakage when bonded with conventional UV-curable acrylic adhesives, which can cause further light unevenness.

Method used

An optical sheet design with a first base layer, an optically functional layer, a second base layer, and an adhesive layer made of polyurethane resin, specifically a two-part curable acrylic polyol-polyurethane resin, with a storage modulus of 1×10^9 to 2×10^9 Pa at 85°C, to prevent adhesive extrusion and maintain even light transmission.

Benefits of technology

The design effectively prevents adhesive extrusion and light unevenness, ensuring consistent light transmission and improved manufacturing efficiency by using a polyurethane resin with a suitable storage modulus.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573167000002
    Figure 0007573167000002
  • Figure 0007573167000003
    Figure 0007573167000003
  • Figure 0007573167000004
    Figure 0007573167000004
Patent Text Reader

Abstract

To provide an optical sheet and a liquid crystal display device in which an adhesive between an optical function layer and a base material layer does not spread out of a cut surface of the optical sheet, and manufacture such an optical sheet.SOLUTION: An optical sheet is provided between a light source of a liquid crystal display device and a liquid crystal panel and includes: a first base material layer; an optical function layer stacked on the first base material layer and including a plurality of light transmission parts disposed with a predetermined space therebetween along the first base material layer and transmitting light, and a louver part disposed between the adjacent light transmission parts and reflecting or absorbing the light; a second base material layer disposed to face the first base material layer with the optical function layer held therebetween; and an adhesive layer disposed between the optical function layer and the second base material layer. The adhesive layer is formed of polyurethane resin.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical sheet arranged on the viewer's side of a light source, a liquid crystal display device using the optical sheet, and a method for manufacturing the optical sheet. [Background technology]

[0002] 2. Description of the Related Art Liquid crystal display devices such as in-vehicle displays and liquid crystal televisions are equipped with optical sheets having various functions in order to control light emitted from a light source and provide a viewer with high quality light.

[0003] Patent Document 1 discloses an optical sheet having a layer in which prism portions (referred to herein as light-transmitting portions) and light-absorbing portions (referred to herein as louver portions) are alternately arranged on one side of a base film layer, and which can suppress bending even when made thin. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-198735 A Summary of the Invention [Problem to be solved by the invention]

[0005] When an optical sheet such as that described in Patent Document 1 is used in a liquid crystal display device, each module of the liquid crystal display device and this optical sheet are combined and mounted on the housing of the liquid crystal display device. When mounting an optical sheet such as that described in Patent Document 1, it is fixed by adhesion or fastening with the frame of the housing, but depending on the fixing method, the optical sheet may bend due to its own weight, etc., and this bending may cause unevenness in the light transmitted through the optical sheet.

[0006] In order to suppress such unevenness of light, it is conceivable to increase the rigidity of the optical sheet so that the optical sheet is less likely to bend. In order to increase the rigidity, it is conceivable to further adhere a second base film layer onto the layer in which the prism parts and the light absorbing parts of the optical sheet are alternately arranged as described in Patent Document 1. However, when an ultraviolet-curing acrylic adhesive, which has been conventionally used for adhering such optical sheets, is used for adhering the second base film layer, the adhesive may overflow from the cut surface after the optical sheet is cut after adhering. Such overflow of the adhesive is not preferable when mounting the optical sheet. In order to prevent the adhesive from overflowing, it is conceivable to perform a concave end treatment on the end surface of the optical sheet in advance to provide a margin for the adhesive overflow, but depending on the type of optical sheet, such end treatment may not be possible. In addition, depending on the type of adhesive, the above-mentioned unevenness of light may occur after mounting the optical sheet on the liquid crystal display device, even though the second base film layer is adhered.

[0007] The present invention has been made to solve the above-mentioned problems, and aims to provide an optical sheet using an adhesive that is particularly suitable for use in liquid crystal display devices, particularly in-vehicle liquid crystal display devices, a liquid crystal display device using this optical sheet, and a method for manufacturing the optical sheet. [Means for solving the problem]

[0008] In order to achieve the above-mentioned object, the present invention provides an optical sheet provided between a light source and a liquid crystal panel of a liquid crystal display device, comprising: a first base material layer; an optical functional layer laminated on the first base material layer, the optical functional layer having a plurality of light-transmitting sections arranged at a predetermined interval from each other along the first base material layer and transmitting light, and a louver section arranged between adjacent light-transmitting sections and reflecting or absorbing light; a second base material layer arranged to face the first base material layer across the optical functional layer; and an adhesive layer arranged between the optical functional layer and the second base material layer, the adhesive layer being made of polyurethane resin.

[0009] The polyurethane resin may also be an acrylic polyol-polyurethane resin.

[0010] In order to achieve the above-mentioned object, the present invention provides an optical sheet provided between a light source and a liquid crystal panel of a liquid crystal display device, the optical sheet comprising: a first base material layer; an optical functional layer laminated on the first base material layer, the optical functional layer having a plurality of light-transmitting sections arranged at predetermined intervals along the first base material layer and transmitting light; and a louver section arranged between adjacent light-transmitting sections and reflecting or absorbing light; a second base material layer arranged to face the first base material layer with the optical functional layer therebetween; and an adhesive layer arranged between the optical functional layer and the second base material layer, the adhesive layer having a storage modulus of 1×10 at 85° C. 9 Pa to 2 x 10 9 Pa, which is an optical sheet.

[0011] The second base layer may also include a reflective polarizing film on the side in contact with the adhesive layer.

[0012] In addition, in order to achieve the above-mentioned object, another aspect of the present invention is a liquid crystal display device comprising the above-mentioned optical sheet, and a liquid crystal display device and a light source arranged to face each other across the optical sheet.

[0013] In addition, in order to achieve the above-mentioned object, another aspect of the present invention is a method for manufacturing an optical sheet comprising: a first base material layer; an optical functional layer laminated on the first base material layer, the optical functional layer having a plurality of light-transmitting sections arranged at a predetermined interval from each other along the first base material layer and transmitting light, and a louver section arranged between adjacent light-transmitting sections and reflecting or absorbing light; a second base material layer arranged to face the first base material layer across the optical functional layer; and an adhesive layer arranged between the optical functional layer and the second base material layer, wherein a polyurethane resin is used as the adhesive layer.

[0014] The polyurethane resin may also be an acrylic polyol-polyurethane resin.

[0015] Further, in order to achieve the above-mentioned object, another aspect of the present invention is a method for producing an optical sheet comprising: a first base layer; an optical functional layer laminated on the first base layer, the optical functional layer having a plurality of light transmitting sections arranged at a predetermined interval from each other along the first base layer and transmitting light; and a louver section arranged between adjacent light transmitting sections and reflecting or absorbing light; a second base layer arranged to face the first base layer with the optical functional layer therebetween; and an adhesive layer arranged between the optical functional layer and the second base layer, the adhesive layer having a storage modulus of 1×10 at 85° C. after the optical sheet is completed. 9 Pa to 2 x 10 9 A method for producing an optical sheet using an adhesive layer having a thickness of 100 Pa.

[0016] The second base layer may also include a reflective polarizing film on the side in contact with the adhesive layer. Effect of the Invention

[0017] According to the present invention, it is possible to provide an optical sheet and a liquid crystal display device that prevent the adhesive from spilling out and suppress unevenness in light. It is also possible to manufacture such an optical sheet. [Brief description of the drawings]

[0018] [Figure 1] 1 is an exploded perspective view of a liquid crystal display device according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an exploded view of the liquid crystal display device of FIG. [Diagram 3] FIG. 2 is an exploded view of the liquid crystal display device of FIG. [Figure 4] FIG. 3 is an enlarged view focusing on the optical sheet in FIG. 2. [Diagram 5] 2A to 2C are explanatory diagrams of a manufacturing process of the optical sheet of FIG. 1. [Figure 6] 2A to 2C are explanatory diagrams of a manufacturing process of the optical sheet of FIG. 1. [Figure 7] 2A to 2C are explanatory diagrams of a manufacturing process of the optical sheet of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an optical sheet and a liquid crystal display device according to an embodiment will be described with reference to the accompanying drawings. In order to facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals as much as possible, and duplicated descriptions will be omitted.

[0020] [composition] First, the configuration of an optical sheet 30 according to an embodiment and a liquid crystal display device 10 including the same will be described with reference to FIG. 1 to FIG. 4. FIG. 1 is an exploded perspective view of the liquid crystal display device 10 according to the embodiment. FIG. 2 and FIG. 3 are exploded views of the liquid crystal display device 10. For ease of explanation, when the horizontal direction, thickness direction, and vertical direction are defined as shown in FIG. 1, FIG. 2 shows the liquid crystal display device 10 from the horizontal direction, and FIG. 3 shows the liquid crystal display device 10 from the vertical direction. FIG. 4 shows the optical sheet 30 shown in FIG. 2 rotated 90 degrees counterclockwise as viewed from the cross-sectional direction and enlarged in order to show the configuration of the optical sheet 30 shown in FIG. 2 and the like. Note that the thickness of each layer shown in the figure may differ from the actual dimensions, with priority given to ease of viewing the figure.

[0021] The liquid crystal display device 10 is housed in a housing (not shown) together with a power source, electronic circuits, etc. The liquid crystal display device 10 is provided in the interior of a vehicle (not shown) and operates as a part of a navigation device. The liquid crystal display device 10 includes a liquid crystal panel 15, a surface light source device 20, and a functional film 40.

[0022] The liquid crystal panel 15 has a liquid crystal layer 12, an upper polarizing plate 13, and a lower polarizing plate 14. The upper polarizing plate 13 is disposed on the viewer side, and the lower polarizing plate 14 is disposed on the surface light source device 20 side. The liquid crystal layer 12 is disposed between the upper polarizing plate 13 and the lower polarizing plate 14.

[0023] The upper polarizing plate 13 and the lower polarizing plate 14 have the function of decomposing the incident light into two orthogonal polarized components (P wave and S wave), transmitting the polarized component in one direction (parallel to the transmission axis) (e.g., P wave) and absorbing the polarized component in the other direction (parallel to the absorption axis) orthogonal to the one direction (e.g., S wave). The lower polarizing plate 14 is an example of a polarizing film.

[0024] In the liquid crystal layer 12, a plurality of pixels are arranged vertically and horizontally in a direction along the layer surface. By applying an electric field to each region forming one pixel, the orientation of the pixel in that region changes. As a result, the polarization direction of the polarized component (e.g., P wave) parallel to the transmission axis that has passed through the lower polarizing plate 14 arranged on the surface light source device 20 side (i.e., the light input side) rotates by 90° when passing through a pixel to which an electric field is applied, and on the other hand, maintains its polarization direction when passing through a pixel to which an electric field is not applied. Therefore, depending on whether or not an electric field is applied to the pixel, it is possible to control whether the polarized component (e.g., P wave) that has passed through the lower polarizing plate 14 is further transmitted through the upper polarizing plate 13 arranged on the light output side, or is absorbed and blocked by the upper polarizing plate 13.

[0025] In this way, the liquid crystal panel 15 is configured to control the transmission or blocking of light from the surface light source device 20 for each pixel, and to provide an image to the observer. Therefore, when light is irradiated from the rear side of the liquid crystal panel 15, by allowing a large amount of light having a polarization component parallel to the transmission axis of the lower polarizer 14 to reach the liquid crystal panel 15, the light can be transmitted through the lower polarizer 14 to increase the light utilization efficiency.

[0026] Furthermore, due to its nature, the liquid crystal panel 15 has excellent contrast and efficiency (transmittance) of emitted light for light incident from the normal direction of the liquid crystal panel 15. However, for light incident from an angle relative to the normal direction of the liquid crystal panel 15 and for observation by an observer from an oblique direction, problems arise in terms of reduced contrast and low efficiency (transmittance). In other words, in order to increase the light utilization efficiency, it is also effective to increase the amount of incident light from the normal direction of the liquid crystal panel 15.

[0027] There is no particular limitation on the type of liquid crystal panel 15, and any known type of liquid crystal panel can be used. For example, the liquid crystal panel 15 can be TN, STN, VA, MVA, IPS, OCB, etc.

[0028] The surface light source device 20 is an illumination device that emits planar light toward the liquid crystal panel 15. The surface light source device 20 is disposed on the opposite side of the liquid crystal panel 15 from the observer side. The surface light source device 20 is configured as an edge-light type surface light source device, and includes a light guide plate 21, a light source 25, a light diffusion plate 26, a prism layer 27, a reflective polarizing plate 28, an optical sheet 30, and a reflective sheet 39.

[0029] The light guide plate 21 has a base 22 and optical elements 23. The base 22 has a plate shape with a predetermined thickness. The base 22 guides light and is a base for the optical elements 23. Various materials can be used for the materials forming the base 22 and the optical elements 23. However, materials that are widely used as materials for optical sheets incorporated in display devices, have excellent mechanical properties, optical properties, stability, processability, and the like, and are inexpensively available can be used. Examples of such materials include thermoplastic resins such as polymer resins having an alicyclic structure, methacrylic resins, polycarbonate resins, polystyrene resins, acrylonitrile-styrene copolymers, methyl methacrylate-styrene copolymers, ABS resins, and polyethersulfones, and epoxy acrylate and urethane acrylate reactive resins (ionizing radiation curable resins, etc.).

[0030] The optical elements 23 are formed on the back side of the base 22 (the side opposite to the side where the reflective polarizing plate 28 is arranged). The optical elements 23 protrude from the base 22 and have a triangular prism shape. The optical elements 23 are formed so that the ridges of the protruding apexes extend in the horizontal direction. On the back side of the base 22, a plurality of optical elements 23 are arranged in the vertical direction at a predetermined pitch. The optical elements 23 have a triangular cross section, but this is not limited thereto, and may have any cross section such as a polygonal cross section, a hemispherical cross section, a part of a sphere, or a lens cross section. The arrangement direction of the plurality of optical elements 23 is preferably the light guide direction. That is, the optical elements 23 are arranged in a direction away from the light source 25, and the ridges of the optical elements 23 extend parallel to the direction in which the light source 25 is arranged, or in the case of one long light source, the direction in which the light source extends.

[0031] The light guide plate 21 having such a configuration can be manufactured by extrusion molding, or by molding the optical elements 23 on the base 22. In the light guide plate 21 manufactured by extrusion molding, the base 22 and the optical elements 23 can be integrally formed. In addition, when the light guide plate 21 is manufactured by molding, the optical elements 23 may be made of the same resin material as the base 22 or a different material.

[0032] The light source 25 is disposed on one of the side surfaces of the base 22 of the light guide plate 21 in the direction in which the multiple optical elements 23 are arranged. The light source 25 is made up of multiple LEDs (light emitting diodes). The light source 25 is configured so that the turning on and off of each LED and / or the brightness of each LED when lit can be individually and independently adjusted by a control device (not shown).

[0033] The light diffusion plate 26 has a function of diffusing and emitting incident light. The light diffusion plate 26 is provided on the light output side of the light guide plate 21. This can further improve the uniformity of the light emitted from the light guide plate 21 and make scratches on the light guide plate 21 less noticeable. The light diffusion plate 26 also functions as a support for the prism layer 27.

[0034] The prism layer 27 is provided closer to the liquid crystal panel 15 than the light diffusion plate 26, and has a plurality of unit prisms 27a. The unit prisms 27a protrude toward the liquid crystal panel 15, and extend in a direction perpendicular to the light guide direction of the light guide plate 21. This allows the optical function layer 32 to collect light in a direction in which the light is controlled (the vertical direction in this embodiment), and the optical function layer 32 to efficiently totally reflect the light, thereby improving the light utilization efficiency.

[0035] The reflective polarizing plate 28 has a function of decomposing the incident light into two orthogonal polarized components (P wave and S wave), transmitting the polarized component in one direction (parallel to the transmission axis) (for example, P wave) and reflecting the polarized component in the other direction (parallel to the reflection axis) orthogonal to the one direction (for example, S wave). A publicly known structure can be used for such a reflective polarizing plate 28.

[0036] The optical sheet 30 comprises a first base material layer 31a formed in a sheet shape, an optical functional layer 32 laminated on one surface of the first base material layer 31a (in this embodiment, the surface on the light guide plate 21 side), and a second base material layer 31b arranged opposite the first base material layer 31a across the optical functional layer 32 and adhered to the optical functional layer 32 by an adhesive layer 37.

[0037] The first base material layer 31a and the second base material layer 31b are flat plate-shaped members that support the optical function layer 32. Various materials can be used to form the first base material layer 31a and the second base material layer 31b, but in the illustrated embodiment, both the first base material layer 31a and the second base material layer 31b are polyester films.

[0038] The optical function layer 32 has a light-transmitting portion 33 and a louver portion 34. The light-transmitting portion 33 is a portion whose main function is to transmit light, and has a substantially trapezoidal cross-sectional shape in the cross-sections shown in FIG. 1, FIG. 2, and FIG. 4. As shown enlarged in FIG. 4, the light-transmitting portions 33 extend horizontally while maintaining the cross-section along the layer surfaces of the first base material layer 31a and the second base material layer 31b, and are arranged at a predetermined interval in the vertical direction. Then, between adjacent light-transmitting portions 33, a groove 33a (see FIG. 6) having a substantially trapezoidal cross-section is initially formed, and the groove 33a is filled with a material described later to form the louver portion 34. Note that the structures shown in each figure, including FIG. 4, are schematic and do not necessarily correspond to the dimensions of the actual product. In various products, the thicknesses of the layers may differ from the dimensional relationship shown in the figures. A method for forming the louver portion 34 will be described later with reference to FIG. 6.

[0039] The light transmitting portions 33 extend in the front-rear direction of the paper surface of FIG. 4 while maintaining the cross section along the layer surface of the first base layer 31a, and are arranged at a predetermined interval (pitch: Pk) in a direction perpendicular to the cross section (horizontal direction in FIG. 4). Then, between adjacent light transmitting portions 33, a groove having a substantially trapezoidal cross section is initially formed, and the groove has a trapezoidal cross section having a long bottom base on the top bottom side (light guide plate 21 side) of the light transmitting portion 33 and a short top base on the bottom bottom side (liquid crystal panel side) of the light transmitting portion 33, and the louver portion 34 is formed by filling the groove with a necessary material described later. In this embodiment, the adjacent light transmitting portions 33 are connected at the long bottom base side. In order to specify the structure of the optical function layer 32, the following parameters are mainly used for the louver portion 34. Regarding the substantially trapezoidal shape of the louver portion 34 having a substantially trapezoidal cross section, the width of the short top base is We, and the width of the long bottom base is Wb. The thickness of the louver portion 34 (approximately equivalent to the height of the trapezoid) is designated as Dk.

[0040] The pitch Pk of the light transmitting portion 33 (that is, the pitch of the louver portion 34) is preferably 30 μm or more and 100 μm or less. Furthermore, the angle between the interface at the oblique side between the louver portion 34 and the light transmitting portion 33, indicated by θk in FIG. 4, and the normal line to the layer surface of the optical function layer 32 is preferably 1° or more and 10° or less. However, the angle may be outside this range, for example, 0° (that is, the oblique side coincides with the normal line to the layer surface of the optical function layer 32). The louver portion 34 shown in FIG. 4 has a shape of an approximately isosceles trapezoid, but the length of one leg and the length of the other leg may be different. The thickness Dk of the louver portion 34 is preferably 50 μm or more and 150 μm or less, and more preferably 60 μm or more and 150 μm or less. The width We of the upper base and the width Wb of the lower base of the approximately trapezoidal portion of the louver portion 34 are appropriately selected so as to satisfy the relationship between the thickness Dk of the louver portion 34, the pitch Pk, and the angle θk. Having these parameters within the preferred ranges often provides an appropriate balance between light transmission and light absorption.

[0041] The light transmitting portion 33 has a refractive index of Nt. Such a light transmitting portion 33 can be formed by curing a predetermined composition, as described later. The value of the refractive index Nt is not particularly limited, but materials with too high a refractive index are often prone to cracking, and from the viewpoint of appropriately reflecting light (including total reflection) at the interface with the louver portion 34 at the inclined surface of the trapezoidal cross section, the refractive index is preferably greater than 1.47 and less than 1.65, and more preferably greater than 1.49 and less than 1.57.

[0042] The louver portion 34 is formed by filling the grooves 33a that were originally provided between the adjacent light transmitting portions 33 with a material described later, and finally has a cross-sectional shape similar to the cross-sectional shape of the grooves 33a before filling. The louver portion 34 has a refractive index of Nr and is configured to absorb light. Specifically, light absorbing particles are dispersed in a transparent resin having a refractive index of Nr. The refractive index Nr is set to a refractive index lower than the refractive index Nt of the light transmitting portion 33. In this way, by making the refractive index of the louver portion 34 smaller than the refractive index of the light transmitting portion 33, light that enters the light transmitting portion 33 under a specified condition can be appropriately totally reflected at the interface with the louver portion 34. Also, even if the total reflection condition is not satisfied, some light is reflected at the interface. The value of the refractive index Nr is not particularly limited, but a material with a too high refractive index is often prone to cracking, and from the viewpoint of appropriately performing the total reflection, it is preferably 1.47 or more and less than 1.65, more preferably 1.49 or more and less than 1.57.

[0043] The difference between the refractive index Nt of the light transmitting portion 33 and the refractive index Nr of the louver portion 34 is not particularly limited, but is preferably greater than 0 and equal to or less than 0.14, and more preferably greater than or equal to 0.05 and equal to or less than 0.14. By increasing the refractive index difference, more light can be totally reflected.

[0044] The optical function layer 32 having such a configuration and the second base material layer 31b are bonded together by an adhesive layer 37. This process will be described later with reference to Fig. 7. The adhesive 370 constituting the adhesive layer 37 is a polyurethane resin, in particular a two-component curing acrylic polyol-polyurethane resin.

[0045] When the optical sheet 30 including the optical functional layer 32 having such a configuration is bent, unevenness of light may occur when viewed by a user (observer). Specifically, in the optical sheet 30 shown in Figs. 2 and 3, bending in a direction perpendicular to the surface of the optical sheet 30, i.e., in the direction shown as the thickness direction in Figs. 2 and 3, affects the occurrence of unevenness of light when viewed by a user (observer). Among the bending directions of the optical sheet 30, bending in the thickness direction of the optical sheet 30 shown in Fig. 2, i.e., bending in a direction perpendicular to the direction in which the multiple light transmitting parts 33 and the louver parts 34 of the optical functional layer 32 are alternately arranged (the direction shown as the "vertical direction" in Fig. 2) in the plane of Fig. 2, changes the orientation of the louver parts, and therefore greatly affects the occurrence of unevenness of light when viewed by a user (observer).

[0046] The configuration of the liquid crystal display device 10 will be further described with reference to Fig. 1 to Fig. 3. The functional film 40 is provided on the light output side of the liquid crystal panel 15, and has the functions of improving the quality of the image light and protecting the liquid crystal display device 10. For example, the functional film 40 may be an anti-reflection film, an anti-glare film, a hard coat film, a color tone correction film, a light diffusion film, or the like. The functional film 40 may also be configured by using a combination of a plurality of these films.

[0047] [How to make optical sheets] Next, a method for producing the optical sheet 30 will be described with reference to Fig. 5 to Fig. 7. Fig. 5 to Fig. 7 are explanatory diagrams of the process for producing the optical sheet 30. Note that these explanatory diagrams show an outline of the production process, and therefore may differ in size and scale from the actual configuration, particularly in the thickness dimensions of the optical sheet 30 and other films.

[0048] As described above, the first base layer 31a and the optional second base layer 31b of the optical sheet 30 are both polyester films. The polyester film can be obtained by condensing any dicarboxylic acid and a diol. Examples of dicarboxylic acids that can be used include terephthalic acid, isophthalic acid, orthophthalic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, diphenylcarboxylic acid, diphenoxyethanedicarboxylic acid, diphenylsulfonecarboxylic acid, anthracenedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, malonic acid, dimethylmalonic acid, succinic acid, 3,3-diethylsuccinic acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, azelaic acid, dimer acid, sebacic acid, suberic acid, and dodecadicarboxylic acid.

[0049] As the diol, for example, ethylene glycol, propylene glycol, hexamethylene glycol, neopentyl glycol, 1,2-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, decamethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexadiol, 2,2-bis(4-hydroxyphenyl)propane, bis(4-hydroxyphenyl)sulfone, etc. can be used.

[0050] The dicarboxylic acid component and the diol component constituting the polyester film may each be one or more. For example, polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc. may be used as the polyester resin constituting the polyester film, and preferably polyethylene terephthalate and polyethylene naphthalate are used, and preferably polyethylene terephthalate can be used. The polyester resin may contain other copolymerization components. From the viewpoint of mechanical strength, the ratio of the copolymerization components is preferably 3 mol% or less, preferably 2 mol% or less, and more preferably 1.5 mol% or less. These resins are excellent in transparency and also in thermal and mechanical properties. In addition, the retardation Re of these resins can be easily controlled by stretching.

[0051] The polyester film can be obtained according to a general manufacturing method. Specifically, a polyester resin is melted, and the non-oriented polyester extruded into a sheet is stretched in the longitudinal direction by utilizing the speed difference between rolls at a temperature equal to or higher than the glass transition temperature, and then stretched in the transverse direction by a tenter, and heat-treated and, if necessary, relaxed to obtain a stretched polyester film. The stretched polyester film may be a uniaxially stretched film or a biaxially stretched film. For example, the polyester film used in Example 1 described later is stretched in the longitudinal direction at a temperature of 90 to 120°C, and then stretched in the transverse direction, with a stretch ratio of 2.0 times in the longitudinal direction and 4.5 times in the transverse direction. It is also known that the greater the stretch ratio, the stronger the breaking strength in that direction.

[0052] The thickness of the polyester film is not limited and can be appropriately set within the range of, for example, 15 to 300 μm, preferably 30 to 200 μm.

[0053] The light-transmitting portion 33 is formed on one side of the first base layer 31a, which is the polyester film formed as described above. As shown in FIG. 5, a polyester film 310 to be the first base layer 31a is inserted between a mold roll R1 having a shape (groove) on its surface to which the shape of the light-transmitting portion 33 can be transferred, and a nip roll R2 arranged to face the mold roll R1. At this time, the mold roll R1 and the nip roll R2 are rotated in the direction indicated by the arrow in FIG. 5 while supplying a composition 330 constituting the light-transmitting portion 33 (see FIG. 1, FIG. 4, etc.) between the polyester film 310 and the mold roll R1. As a result, the composition 330 is filled into the groove (a shape that is an inverted shape of the light-transmitting portion 33) formed on the surface of the mold roll R1, and the composition 330 conforms to the surface shape of the mold roll R1.

[0054] The composition 330 constituting the light transmitting portion 33 may be, for example, an ionizing radiation curable resin such as an epoxy acrylate, a urethane acrylate, a polyether acrylate, a polyester acrylate, or a polythiol.

[0055] The composition 330, which is sandwiched between the mold roll R1 and the polyester film 310 and filled therein, is irradiated with light (ultraviolet rays, etc.) from the polyester film 310 side by a light irradiation device 61. This cures the composition 330. Then, the pre-filling sheet 36a, which is made up of the polyester film 310 and the molded light transmitting portion 33, is released from the mold roll R1 by a release roll R3.

[0056] Next, the louver portion 34 is formed. To form the louver portion 34, as shown in FIG. 6, an excess of the composition 340 constituting the louver portion 34 is supplied to the grooves 33a between the adjacent light transmitting portions 33 of the pre-filled sheet 36a. The excess composition 340 is then scraped off with a blade 62 or the like. Then, the remaining composition 340 that filled the grooves 33a is irradiated with light (such as ultraviolet light) from a light source (not shown). This causes the composition 340 to harden, forming the louver portion 34 and obtaining the intermediate sheet 36b.

[0057] For example, photocurable resins such as urethane (meth)acrylate, polyester (meth)acrylate, epoxy (meth)acrylate, and butadiene (meth)acrylate can be used as the composition 340 constituting the louver portion 34. Furthermore, these resins in which colored light absorbing particles are dispersed can also be used.

[0058] Instead of dispersing light-absorbing particles, the entire louver portion can be colored with pigments or dyes. When light-absorbing particles are used, light-absorbing colored particles such as carbon black are preferably used, but are not limited to these, and colored particles that selectively absorb specific wavelengths in accordance with the characteristics of the image light may be used. Specifically, organic fine particles colored with metal salts such as carbon black, graphite, and black iron oxide, dyes, pigments, etc., and colored glass beads can be mentioned. In particular, colored organic fine particles are preferably used from the viewpoints of cost, quality, ease of availability, etc. The average particle size of the colored particles is preferably 1.0 μm or more and 20 μm or less.

[0059] The second base layer 31b is further bonded to the intermediate sheet 36b manufactured in this way using an adhesive 370. Specifically, as shown in FIG. 7, the intermediate sheet 36b is fed from the roll R4, and the polyester film 310 to become the second base layer 31b is fed from the roll R5 in the same direction. At this time, by bonding the first base layer 31a included in the intermediate sheet 36b and the second base layer 31b (polyester film 310) in the same flow direction, it is possible to prevent the disturbance of polarization due to the phase difference, the occurrence of color unevenness and the decrease in transmittance caused thereby. The intermediate sheet 36b and the polyester film 310 are guided by the roller 380 so as to approach each other and are integrated. At this time, the polyester film 310 is arranged so as to face the first base layer 31a with the light transmission portion 33 and the louver portion 34 sandwiched therebetween. Then, a mixed two-component curing acrylic polyol-polyurethane resin adhesive 370 is introduced from an adhesive supply unit (not shown) between the intermediate sheet 36b and the polyester film 310, and the two are bonded together. The optical sheet 30 completed by this bonding is then taken up on a roll R6. When a predetermined length has been taken up, the optical sheet 30 is cut, and the taken-up roll R6 is replaced with a new roll R6, and the next winding begins.

[0060] In the process shown in FIG. 7, before the polyester film 310 is fed from the roll R5, a reflective polarizing film may be attached in advance to the surface of the polyester film 310 facing the intermediate sheet 36b, that is, the surface that will come into contact with the adhesive layer of the adhesive 370. In this case, the second base layer 31b includes the polyester film 310 and a reflective polarizing film (not shown). With such a configuration, it is possible to make the optical sheet function as the reflective polarizing plate 28. Therefore, it is not necessary to use the reflective polarizing plate 28 as a separate member, and therefore the number of components of the liquid crystal display device can be reduced, and the overall thickness can be reduced, making it possible to reduce the weight and thickness of the components while suppressing the occurrence of uneven light.

[0061] In this manner, in manufacturing the optical sheet, the optical sheet is transferred between a plurality of rolls, that is, a roll-to-roll process is performed, and the optical sheet is finally wound up again on a roll.

[0062] (Example) The specific shapes of the optical sheets according to the examples are as follows.

[0063] <First Base Layer> Material: Polyester film Thickness: 80μm <Optical functional layer> Pitch (see Figure 4): Pk = 39 μm - Width of upper bottom of louver: 4μm (Wa in Figure 4) Bottom width of louver: 10μm (Wb in Figure 4) Slope angle: one is 0°, the other is 3° (θk in Figure 4) Thickness of louver part (see Figure 4): Dk = 102 μm Optical function layer thickness: 125μm Material and refractive index of light-transmitting part: UV-curable urethane acrylate with a refractive index of 1.57 Louver material and refractive index: UV-curable urethane acrylate with a refractive index of 1.49, with 20% dispersion of black beads made of acrylic beads with an average particle size of 4 μm that contain carbon black on the surface. <Second Base Layer> A second base layer, which will be described later, was further attached to the surface of the optical functional layer opposite to the first base layer with an adhesive, as described below. Material: Polyester film Thickness: 80μm <Adhesive> As an example of the polyurethane resin, the following two-component curing type acrylic polyol-polyurethane resin was used as an adhesive for bonding the optical functional layer and the second base layer. Base agent: Seikadyne TS241 Primer (Dainichi Seika Chemicals Co., Ltd.) Hardener: Seikadyne TS241 hardener (Dainichi Seika Chemicals Co., Ltd.) The base agent and hardener were mixed in a ratio of base agent:hardener = 20:1. The thickness of the adhesive layer is 25 μm.

[0064] Comparative Example 1 An optical sheet according to Comparative Example 1 was produced by changing the adhesive material used to bond the optical functional layer and the second base layer in the optical sheet according to the example to an acrylic adhesive (PD-S1 manufactured by PANAC).

[0065] Comparative Example 2 In the optical sheet of the example, the adhesive material used to bond the optical functional layer and the second base material layer was changed to an acrylic adhesive (CS9861US manufactured by Nitto Denko) different from that in Comparative Example 1, to produce the optical sheet of Comparative Example 2.

[0066] In order to confirm the storage modulus of the adhesive layer of the optical sheet, the protrusion of adhesive from the cut surface when the optical sheet is cut, and the occurrence of uneven light after the optical sheet is mounted on a liquid crystal display device, the optical sheets of the above-mentioned Example, Comparative Example 1, and Comparative Example 2 were each subjected to the following confirmation and tests.

[0067] [Storage modulus test] The samples of Example, Comparative Example 1, and Comparative Example 2 were each subjected to cross-section adjustment using a microtome (REM-710 manufactured by Yamato Koki Kogyo Co., Ltd.) and then fixed to a stage. Nano-viscoelasticity measurements of the adhesive layer were performed using the following evaluation method to obtain the storage modulus. Equipment: Environmentally controlled nanoindentation equipment manufactured by Nissan Arc Indenter used: Spherical indenter (tip radius 1μm) Measurement atmosphere: vacuum (10 -3 Pa or less) Measurement temperature: 85℃ Measurement frequency: 250 to 1Hz

[0068] [Check for adhesive overflow] The samples of Example, Comparative Example 1, and Comparative Example 2 were punched using a press cutter (Thomson cutter) and tested at 95°C for 1000 hours, after which the presence or absence of adhesive protrusion from the edges of the cut surfaces was visually confirmed using a microscope.

[0069] [Check for uneven lighting] Regarding the occurrence of uneven light, the optical sheets of each of the examples and comparative examples were mounted on a 12.3-inch IPS LCD display, and reliability tests were conducted for 1000 hours in an environment at a temperature of 95°C, 1000 hours in an environment at a temperature of 65°C and humidity of 95%, and 1000 hours in an environment at a temperature of -45°C. The presence or absence of uneven light was visually confirmed when the LCD display was operated.

[0070] Table 1 shows the results of measuring the storage modulus, the results of checking for adhesive extrusion, and the results of checking for light unevenness for each of the examples and comparative examples.

[0071] [Table 1]

[0072] As described above, it was found that, for the optical sheets using acrylic adhesives such as those in Comparative Examples 1 and 2, adhesive overflow and uneven light occurred, whereas, for the optical sheets using polyurethane resin as the adhesive, no adhesive overflow or uneven light occurred.

[0073] When using an acrylic adhesive as in Comparative Examples 1 and 2, the storage modulus of the adhesive layer is 0.8 to 1.0 × 10 5 Pa, and it was found that the adhesive overflowed in these comparative examples. Thus, a low storage modulus of the adhesive layer suggests that the adhesive constituting the adhesive layer is easily mobile and easily overflows from the edge of the cut surface of the optical sheet.

[0074] When using an acrylic adhesive as in Comparative Examples 1 and 2, the storage modulus of the adhesive layer is 0.8 to 1.0 × 10 5The compressive strength was 1.0 Pa, and the occurrence of uneven light was observed in these comparative examples, suggesting that the ease of movement of the adhesive constituting the adhesive layer causes optical effects. In other words, the light-transmitting parts and the louver parts are usually arranged regularly in the optical function layer, but the arrangement of the light-transmitting parts and the louver parts becomes disordered as if dragged by the movement (shift) of the adhesive constituting the adhesive layer, and the viewing angle changes, making uneven light more likely to occur. In particular, since the amount of movement (shift) of the adhesive differs between the center and the outer periphery of the optical sheet, the slope angle of the louver parts changes depending on the location, which is thought to further cause uneven light. Therefore, it is considered that the storage modulus of the adhesive layer is 0.8 to 1.0 × 10 as in the comparative examples. 5 A low value of 0.1 Pa is not preferable.

[0075] On the other hand, the storage modulus of the adhesive layer is 1 to 2 × 10 9 If an adhesive agent that greatly exceeds the range of 100 Pa is used, the rigidity of the adhesive layer increases, and as a result, the rigidity of the entire optical sheet is expected to increase. If the rigidity of the entire optical sheet becomes too high, the optical sheet may crack when it is wound around a roll in the manufacture of the optical sheet as described above. Since this leads to a decrease in manufacturing efficiency, it is also undesirable that the storage modulus of the adhesive layer is too large. In the above-mentioned embodiment, there is no problem with the roll-to-roll characteristics, and the processing speed is 10 m / min, so there is no problem from the viewpoint of manufacturing efficiency.

[0076] In other words, the optical sheet of the above-mentioned embodiment and the liquid crystal display device using this optical sheet make it possible to suppress the adhesive layer from overflowing and the occurrence of uneven light, and also to prevent a decrease in manufacturing efficiency.

[0077] The two-component curing acrylic polyol-polyurethane resin used as the adhesive in the above-mentioned examples requires mixing of the base agent and the curing agent before use. Therefore, the number of steps required for use increases compared to the acrylic adhesive used in each comparative example. However, the use of the two-component curing acrylic polyol-polyurethane resin brings about a great advantage in that it prevents the adhesive layer from sticking out and the occurrence of uneven light while preventing a decrease in manufacturing efficiency.

[0078] In the above-described embodiment, a two-component curing acrylic polyol-polyurethane resin was used as the polyurethane resin. However, various other polyurethane resins such as polyether polyol-polyurethane resin, polyester polyol-polyurethane resin, and polycarbonate-polyurethane resin can also be used as the adhesive.

[0079] Also, other adhesives may be used as long as they are capable of forming an adhesive layer having a storage modulus similar to that of the adhesive layer in the above-described embodiment.

[0080] Moreover, according to the manufacturing method of the above-mentioned embodiment, it is possible to manufacture an optical sheet suitable for use in a liquid crystal display device, particularly an in-vehicle liquid crystal display device. [Explanation of symbols]

[0081] 10 LCD display device 14 Lower polarizing plate (polarizing film) 30 Optical Sheet 31a First base material layer 31b Second base layer 32 Optical functional layer 33 Light transmission part 34 Louver section 37 Adhesive layer

Claims

1. An optical sheet provided between a light source and a liquid crystal panel of a liquid crystal display device, A first substrate layer; an optical functional layer laminated on the first base layer, the optical functional layer having a plurality of light transmitting sections arranged at predetermined intervals along the first base layer to transmit light, and a louver section disposed between adjacent light transmitting sections to reflect or absorb light; a second base material layer disposed opposite to the first base material layer with the optical functional layer interposed therebetween; an adhesive layer disposed between the optical functional layer and the second base material layer; Equipped with The adhesive layer has a storage modulus of 1×10 over the entire frequency range of 1 to 250 Hz at 85° C. 9 Pa to 2 x 10 9 Pa, the optical sheet.

2. The optical sheet according to claim 1 , wherein the second base layer is provided with a reflective polarizing film on a side in contact with the adhesive layer.

3. The optical sheet according to claim 1 or 2; a light source and a liquid crystal panel arranged to face each other with the optical sheet interposed therebetween.

4. A first substrate layer; an optical functional layer laminated on the first base layer, the optical functional layer having a plurality of light transmitting sections arranged at predetermined intervals along the first base layer to transmit light, and a louver section disposed between adjacent light transmitting sections to reflect or absorb light; a second base material layer disposed opposite to the first base material layer with the optical functional layer interposed therebetween; a bonding layer disposed between the optical functional layer and the second base layer, The adhesive layer has a storage elastic modulus of 1×10 or less at 85° C. over the entire frequency range of 1 to 250 Hz after the optical sheet is completed. 9 Pa to 2 x 10 9 A method for producing an optical sheet using an adhesive layer having a thickness of 100 mm or less.

5. The method for producing an optical sheet according to claim 4 , wherein the second base layer is provided with a reflective polarizing film on a side in contact with the adhesive layer.

Citation Information

Patent Citations

  • Optical sheet, surface light source device, image source unit, and display unit

    JP2016033663A

  • Video source unit and display device

    JP2017111349A

  • Optical sheet, video source unit, and liquid crystal display

    JP2017198735A

  • Optical sheet, image source unit, and liquid crystal display device

    JP2018205640A

  • Optical sheet, surface light source device, image source unit and display device

    JP2019066622A