Dual Ion Battery

The dual ion battery design with carbonaceous and potassium/rubidium metal electrodes and electrolytes allows for high-voltage operation by optimizing anion and metal reactions, overcoming limitations in conventional lithium-based batteries.

JP7573307B2Active Publication Date: 2024-10-25NATIONAL INSTITUTE OF ADVANCED INDUSTRIAL SCIENCE & TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022533971
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-29
Filing Date
2021-06-28
Publication Date
2024-10-25
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

Conventional dual-ion batteries using lithium ions face limitations in achieving high voltage potential due to unlowerable negative electrode reactions, hindering the development of high-voltage dual-ion batteries.

Method used

A dual ion battery design incorporating a positive electrode with a carbonaceous material and a negative electrode containing potassium or rubidium metal, along with an electrolyte containing potassium or rubidium salts, enables high-voltage charging and discharging through anion insertion/extraction and metal precipitation/dissolution reactions.

Benefits of technology

The battery achieves high-voltage charging and discharging capabilities, with anion insertion at elevated potentials and metal precipitation/dissolution at lower potentials, enhancing the voltage range to approximately 5.0V.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573307000002
    Figure 0007573307000002
  • Figure 0007573307000003
    Figure 0007573307000003
  • Figure 0007573307000004
    Figure 0007573307000004
Patent Text Reader

Abstract

Provided is a dual-ion battery with a positive-electrode reaction that is an anion insertion–elimination reaction and a negative-electrode reaction that is a metal deposition and dissolution reaction, wherein: a positive electrode, a negative electrode, and an electrolyte are provided; the positive electrode contains a positive-electrode active substance that includes a carbonaceous material; the negative electrode contains a negative-electrode active substance that includes potassium metal or rubidium metal; and the dual-ion battery is capable of charging and discharging at a high voltage.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dual-ion battery. [Background technology]

[0002] Conventionally, secondary batteries are particularly well known as a technology for storing electrical energy. Examples of secondary batteries include lithium-ion secondary batteries. Lithium-ion secondary batteries have excellent energy density, but have issues with charging speed, output density, lifespan, and the like. For example, lithium-ion secondary batteries for automotive applications have high energy density, but high resistance, a short lifespan, and are difficult to charge and discharge at large currents. For this reason, for example, lithium-ion secondary batteries for hybrid vehicles are extended in service life by restricting their state of charge (SOC). With an SOC of 50%, half of the battery performance is not used, and the unused portion of the battery is wasted space and weight.

[0003] When a lithium-ion secondary battery is charged, lithium ions in the positive electrode are released and inserted between the layers of the negative electrode active material. At that time, a coating called SEI (Solid electrolyte interface) is formed at the entrance between the layers of the negative electrode active material, and the lithium ions are inserted through this SEI coating. Since the lithium ions move through a solid called SEI, the resistance to their movement becomes the electrode resistance. In addition, the electrolyte ions are solvated with a solvent, and this solvation is released and they move between the layers of the negative electrode active material through the SEI coating. Therefore, the resistance when the solvation is released also increases the electrode resistance.

[0004] Meanwhile, in recent years, as a secondary battery having a high energy density and suitable for high-speed charging and discharging, a dual ion battery has been reported, which is a so-called dual intercalation type nonaqueous electrolyte secondary battery in which carbon is used for both the positive electrode and the negative electrode, and a nonaqueous electrolyte solution obtained by dissolving a lithium salt in a nonaqueous solvent is used, and during charging, anions in the nonaqueous electrolyte solution are inserted into the positive electrode, and lithium ions are inserted into the negative electrode, and during discharging, the anions and lithium ions inserted into the positive electrode and negative electrode are released into the electrolyte, thereby performing charging and discharging (for example, see Patent Document 1).

[0005] When comparing a lithium-ion secondary battery with a dual-ion battery that uses lithium ions as cations, the dual-ion battery has higher output characteristics than a lithium-ion secondary battery in which only lithium ions move. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-024119 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in conventional dual-ion batteries using lithium ions, the potential of the negative electrode reaction (metal deposition and dissolution reaction) cannot be lowered any further, so the obtainable voltage cannot be improved and it is not possible to construct a high-voltage dual-ion battery.

[0008] In view of the above, an object of the present invention is to provide a dual ion battery that can be charged and discharged at high voltage. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to achieve the above-mentioned object. As a result, they have found that a dual ion battery capable of being charged and discharged at a high voltage can be obtained by combining a positive electrode active material containing a carbonaceous material with a negative electrode active material containing potassium metal or rubidium metal. The present invention has been completed as a result of further research based on such findings. That is, the present invention includes the following configurations.

[0010] Item 1. A dual ion battery in which the positive electrode reaction is an anion insertion / extraction reaction and the negative electrode reaction is a metal precipitation and dissolution reaction; A positive electrode, a negative electrode, and an electrolyte solution are provided, The positive electrode contains a positive electrode active material including a carbonaceous material, The dual-ion battery, wherein the negative electrode contains a negative electrode active material including potassium metal or rubidium metal.

[0011] Item 2. The dual ion battery according to Item 1, wherein the positive electrode active material consists solely of the carbonaceous material.

[0012] Item 3. The dual ion battery according to item 1 or 2, wherein the positive electrode contains the carbonaceous material, a binder, and a thickener.

[0013] Item 4. The dual ion battery according to any one of Items 1 to 3, wherein the negative electrode active material consists of only the potassium metal or rubidium metal.

[0014] Item 5. The dual ion battery according to any one of Items 1 to 4, wherein the negative electrode is composed only of the potassium metal or rubidium metal.

[0015] Item 6. The dual ion battery according to any one of Items 1 to 5, wherein the electrolyte solution contains an electrolyte salt including a potassium salt and / or a rubidium salt.

[0016] Item 7. The dual ion battery according to any one of Items 1 to 6, wherein the electrolyte solution contains a solvent containing an ionic liquid. Effect of the Invention

[0017] According to the present invention, a dual ion battery capable of being charged and discharged at a high voltage can be provided. [Brief description of the drawings]

[0018] [Figure 1] 1 is a graph showing the results of Test Example 1 (cyclic voltammetry at 3.0 V or higher using the dual ion battery of Example 1). [Diagram 2] 1 is a graph showing the results of Test Example 1 (cyclic voltammetry at 3.0 V or higher using the dual ion battery of Example 3). [Diagram 3] 1 is a graph showing the results of Test Example 1 (cyclic voltammetry at 3.0 V or higher using the dual ion battery of Comparative Example 1). [Figure 4] 1 is a graph showing the results of Test Example 2 (cyclic voltammetry using four types of electrolyte solutions). [Diagram 5] 1 is a graph showing the results of Test Example 3 (cyclic voltammetry using the dual ion battery of Example 1). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] In this specification, "containing" is a concept that encompasses all of "comprise," "consist essentially of," and "consist only of." In addition, in this specification, when a numerical range is shown as "A to B," it means A or more and B or less.

[0020] The dual ion battery of the present invention is a dual ion battery in which the positive electrode reaction is an anion insertion / removal reaction and the negative electrode reaction is a metal precipitation and dissolution reaction, and comprises a positive electrode, a negative electrode, and an electrolyte, in which the positive electrode contains a positive electrode active material including a carbonaceous material, and the negative electrode contains a negative electrode active material including potassium metal or rubidium metal.

[0021] In the dual ion battery of the present invention, the positive electrode reaction is an anion insertion / desorption reaction, that is, the positive electrode reaction proceeds by insertion and desorption of anions in an electrolyte salt present in an electrolyte solution into and from a carbonaceous material that is a positive electrode active material.

[0022] In the dual ion battery of the present invention, the negative electrode reaction is a metal deposition and dissolution reaction, that is, the negative electrode reaction proceeds by deposition and dissolution of cations in the electrolyte salt present in the electrolyte solution at the negative electrode.

[0023] 1. Positive electrode In the dual ion battery of the present invention, the positive electrode contains a positive electrode active material that includes a carbonaceous material.

[0024] The positive electrode is not particularly limited as long as it contains a positive electrode active material (including a carbonaceous material), and can be appropriately selected depending on the purpose, and examples thereof include a positive electrode provided with a positive electrode material having a positive electrode active material on a positive electrode current collector. Note that the carbonaceous material can be used as the positive electrode without providing a positive electrode current collector.

[0025] The positive electrode material is not particularly limited and can be appropriately selected depending on the purpose, and for example, contains at least a positive electrode active material and can further contain a conductive assistant, a binder, a thickener, etc., as necessary. Note that the carbonaceous material can be used as it is as the positive electrode material without containing other components.

[0026] (1-1) Positive electrode active material Examples of carbonaceous materials contained as the positive electrode active material include graphite (natural graphite, artificial graphite, etc.), sinter-resistant carbon, activated carbon, coke, and pyrolysis products of organic matter. Among these, graphite is preferred from the viewpoints of anion insertion / extraction performance, the positive electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, and stability to an electrolyte (particularly an electrolyte using an ionic liquid). These carbonaceous materials can be used alone or in combination of two or more.

[0027] The average particle diameter (D90) of the carbonaceous material contained as the positive electrode active material is preferably 5 to 50 μm, more preferably 10 to 30 μm, from the viewpoints of anion insertion / desorption performance, the positive electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability to an electrolyte (particularly an electrolyte using an ionic liquid), etc. The average particle diameter (D90) of the carbonaceous material is measured by a particle size distribution measuring device using light scattering.

[0028] The specific surface area of ​​the carbonaceous material contained as the positive electrode active material is 1 to 1000 m from the viewpoints of the anion insertion / desorption performance, the positive electrode reaction potential of the resulting dual ion battery, the charge / discharge cycle characteristics, and the stability to the electrolyte (especially the electrolyte using an ionic liquid). 2 / g is preferable, and 5 to 100m 2 The specific surface area of ​​the carbonaceous material is measured by the BET method.

[0029] The shape of the carbonaceous material is not particularly limited, and various shapes such as powder, particles, and plates can be adopted.

[0030] The carbonaceous material does not only mean a material consisting of simple carbon, but also includes those having fluorine on the surface and carbon surface-modified with fluorine or a fluoride compound, as in Patent Document 1. However, from the viewpoints of anion insertion / desorption performance, the positive electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability to an electrolyte (particularly an electrolyte using an ionic liquid), etc., it is preferable that the carbon content is 95 to 100 atomic %, particularly 97 to 100 atomic %.

[0031] The positive electrode active material may be composed only of the carbonaceous material described above, but may also contain other positive electrode active materials. Examples of such other positive electrode active materials include coronene (C 24 H 12 ), Circumcoronen (C 54 H 20 ), dicoronylene (C 48 H 20 ), Hexabenzocoronene (C 42 H 18 ), Obalen (C32 H 14 ), circumtetracene (C 48 H 18 ), naphthalene (C 10 H 8 ), tetracene (C 18 H 12 ), methyl circumcoronene (C 55 H 20 ), Circum Circum Coronen (C 96 H 24 ), benzoanthracene (C 18 H 12 ), thymine (C 5 H 6 N 2 O 2 ), phenanthrene (C 4 H 10 ), anthracene (C 14 H 10 ), Perylene (C 20 H 12 However, from the viewpoints of anion insertion / extraction performance, the positive electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, and stability to an electrolyte (particularly an electrolyte using an ionic liquid), it is preferable that the content of these other positive electrode active materials is small. Specifically, it is preferable that the content of the carbonaceous material is 80 to 100 mass%, particularly 90 to 100 mass%, with the total amount of the positive electrode active materials being 100 mass%.

[0032] (1-2) Conductive additive Examples of the conductive assistant include metal materials such as copper and aluminum, amorphous carbon such as carbon black and acetylene black, etc. These conductive assistants can be used alone or in combination of two or more kinds.

[0033] When these conductive additives are contained, the content of the conductive additive is not particularly limited, but from the viewpoints of anion insertion / extraction performance, the positive electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability to the electrolyte (particularly the electrolyte using an ionic liquid), and the like, the content is preferably 1 to 20 mass%, and more preferably 2 to 10 mass%, relative to 100 mass% of the total amount of the positive electrode material.

[0034] (1-3) Binders and thickeners The binder and thickener are not particularly limited as long as they are stable to the solvent and electrolyte used in the production of the electrode and the applied potential, and can be appropriately selected according to the purpose, and examples thereof include fluorine-based binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE); ethylene-propylene-butadiene rubber (EPBR), styrene-butadiene rubber (SBR), isoprene rubber, acrylate-based latex, carboxymethylcellulose (CMC), methylcellulose, hydroxymethylcellulose, ethylcellulose, polyacrylic acid, polyvinyl alcohol, alginic acid, oxidized starch, starch phosphate, casein, etc. These binders and thickeners can be used alone or in combination of two or more.

[0035] When the binder and / or thickener is contained, the content of the binder and / or thickener is not particularly limited, but from the viewpoints of anion insertion / desorption performance, the positive electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability to the electrolyte (particularly the electrolyte using an ionic liquid), and the like, the content of the binder and / or thickener is preferably 1 to 20 mass%, and more preferably 2 to 10 mass%, relative to 100 mass% of the total amount of the positive electrode material.

[0036] (1-4) Positive electrode current collector The material of the positive electrode current collector is not particularly limited as long as it is made of a conductive material and is stable against the applied potential, and can be appropriately selected depending on the purpose. Examples of the material include stainless steel, nickel, aluminum, titanium, tantalum, tungsten, and titanium nitride.

[0037] The shape of the positive electrode current collector is not particularly limited and can be appropriately selected depending on the purpose. For example, a flat plate shape can be mentioned.

[0038] The size of the positive electrode current collector is not particularly limited as long as it is a size that can be used in a dual ion battery, and can be appropriately selected depending on the purpose.

[0039] (1-5) Manufacturing method of positive electrode The positive electrode can be manufactured by adding a conductive assistant, a binder, a thickener, a solvent, etc. to a positive electrode active material as necessary to form a slurry, applying the slurry onto a positive electrode current collector, and drying the slurry. The solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aqueous solvents and organic solvents. Examples of the aqueous solvent include water and alcohol. Examples of the organic solvent include N-methyl-2-pyrrolidone (NMP), toluene, etc.

[0040] The positive electrode active material may be directly rolled to form a sheet electrode, or may be compression molded to form a pellet electrode.

[0041] 2.Negative electrode In the dual ion battery of the present invention, the negative electrode contains a positive electrode active material that includes potassium metal or rubidium metal.

[0042] The negative electrode is not particularly limited as long as it contains a negative electrode active material (including potassium metal or rubidium metal), and can be appropriately selected depending on the purpose, and examples thereof include a negative electrode provided with a negative electrode material having a negative electrode active material on a negative electrode current collector. Note that potassium metal or rubidium metal can be used as the negative electrode without providing a negative electrode current collector.

[0043] The negative electrode material is not particularly limited and can be appropriately selected depending on the purpose, and for example, contains at least a negative electrode active material, and can further contain a conductive assistant, a binder, a thickener, etc., as necessary. Note that potassium metal or rubidium metal can be used as it is as the negative electrode material without containing other components.

[0044] (2-1) Negative electrode active material The negative electrode active material contains potassium metal or rubidium metal. By using potassium metal or rubidium metal as the negative electrode active material, the negative electrode potential can be sufficiently lowered, and as a result, the difference between the negative electrode potential and the positive electrode potential can be increased, and a dual ion battery capable of being charged and discharged at a high voltage can be provided. In addition, when lithium metal and sodium metal are used as the negative electrode active material, the negative electrode potential becomes high, and as a result, the difference between the negative electrode potential and the positive electrode potential becomes small, and it is not possible to provide a dual ion battery capable of being charged and discharged at a high voltage.

[0045] The shape of the potassium metal or rubidium metal is not particularly limited, and various shapes such as powder, particles, and plates can be used.

[0046] (2-2) Conductive additive Examples of the conductive assistant include metal materials such as copper and aluminum, amorphous carbon such as carbon black and acetylene black, etc. These conductive assistants can be used alone or in combination of two or more kinds.

[0047] When these conductive additives are contained, the content of the conductive additive is not particularly limited. However, from the viewpoints of metal deposition and dissolution performance, the negative electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, and stability to the electrolyte (particularly the electrolyte using an ionic liquid), the content is preferably 1 to 20 mass%, and more preferably 2 to 10 mass%, relative to 100 mass% of the total amount of the negative electrode material.

[0048] (2-3) Binders and thickeners The binder and thickener are not particularly limited as long as they are stable to the solvent and electrolyte used in the production of the electrode and the applied potential, and can be appropriately selected according to the purpose, and examples thereof include fluorine-based binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE); ethylene-propylene-butadiene rubber (EPBR), styrene-butadiene rubber (SBR), isoprene rubber, acrylate-based latex, carboxymethylcellulose (CMC), methylcellulose, hydroxymethylcellulose, ethylcellulose, polyacrylic acid, polyvinyl alcohol, alginic acid, oxidized starch, starch phosphate, casein, etc. These binders and thickeners can be used alone or in combination of two or more.

[0049] When these binders and / or thickeners are contained, the content of the binders and / or thickeners is not particularly limited, but from the viewpoints of metal deposition and dissolution performance, the negative electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability to the electrolyte (particularly the electrolyte using an ionic liquid), and the like, the content of the binders and / or thickeners is preferably 1 to 20 mass%, and more preferably 2 to 10 mass%, based on 100 mass% of the total amount of the negative electrode material.

[0050] (2-4) Negative electrode current collector The material of the negative electrode current collector is not particularly limited as long as it is made of a conductive material and is stable against the applied potential, and can be appropriately selected depending on the purpose. Examples of the material include stainless steel, nickel, aluminum, copper, etc.

[0051] The shape of the negative electrode current collector is not particularly limited and can be appropriately selected depending on the purpose. For example, it may be in a flat plate shape.

[0052] The size of the negative electrode current collector is not particularly limited as long as it is a size that can be used in a dual ion battery, and can be appropriately selected depending on the purpose.

[0053] (2-5) Method for manufacturing negative electrode The negative electrode can be manufactured by adding a conductive assistant, a binder, a thickener, a solvent, etc. to a negative electrode active material as necessary to form a slurry, applying the slurry onto a negative electrode current collector, and drying the slurry. The solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples of the solvent include organic solvents. Examples of the organic solvent include N-methyl-2-pyrrolidone (NMP), toluene, etc.

[0054] The negative electrode active material may be directly rolled to form a sheet electrode, or may be compression molded to form a pellet electrode.

[0055] 3. Electrolyte In the dual ion battery of the present invention, the negative electrode reaction is a metal precipitation and dissolution reaction, and since potassium metal or rubidium metal is used as the negative electrode active material, it is preferable to adopt the same cationic species of the electrolyte salt in the electrolyte as that of the negative electrode active material. In other words, it is preferable that the electrolyte contains an electrolyte salt containing a potassium salt and / or a rubidium salt.

[0056] The potassium salt is not particularly limited, and examples thereof include potassium hexafluorophosphate (KPF 6 ), potassium perchlorate (KClO 4 ), potassium chloride (KCl), potassium tetrafluoroborate (KBF 4 ), potassium hexafluoroarsenate (KAsF 6 ), potassium trifluoromethanesulfonate (KCF 3 SO 3 ), potassium bisfluorosulfonylimide (KN(FSO 2 ) 2 ;KFSI), potassium bistrifluoromethanesulfonylimide (KN(CF 3 SO 2 ) 2 ;KTFSI), potassium bispentafluoroethanesulfonylimide (KN(C 2 F 5 SO 2 ) 2), potassium fluorosulfonyl trifluorosulfonimide (KNFSO 2 (CF 3 SO 2 )) and the rubidium salt is not particularly limited, and examples thereof include rubidium hexafluorophosphate (RbPF 6 ), rubidium perchlorate (RbClO 4 ), rubidium chloride (RbCl), rubidium tetrafluoroborate (RbBF 4 ), rubidium hexafluoroarsenate (RbAsF 6 ), rubidium trifluoromethanesulfonate (RbCF 3 SO 3 ), rubidium bisfluorosulfonyl imide (RbN(FSO 2 ) 2 ;RbFSI), rubidium bistrifluoromethanesulfonylimide (RbN(CF 3 SO 2 ) 2 ;RbTFSI), rubidium bispentafluoroethanesulfonylimide (RbN(C 2 F 5 SO 2 ) 2 ), rubidium fluorosulfonyl trifluorosulfonimide (RbNFSO 2 (CF 3 SO 2 )) and the like. These electrolyte salts can be used alone or in combination of two or more. Among them, potassium bisfluorosulfonylimide (KN(FSO 2 ) 2 ;KFSI), potassium bistrifluoromethanesulfonylimide (KN(CF 3 SO 2 ) 2 ;KTFSI), potassium bispentafluoroethanesulfonylimide (KN(C 2 F 5 SO 2 ) 2 ), rubidium bisfluorosulfonyl imide (RbN(FSO 2 ) 2;RbFSI), rubidium bistrifluoromethanesulfonylimide (RbN(CF 3 SO 2 ) 2 ;RbTFSI), rubidium bispentafluoroethanesulfonylimide (RbN(C 2 F 5 SO 2 ) 2 ) etc. are preferred.

[0057] In the present invention, the electrolyte salt may be composed only of the potassium salt and / or rubidium salt described above, but may also contain other electrolyte salts. Examples of such other electrolyte salts include lithium salts and sodium salts, and examples of the above potassium salts in which K is replaced with Li or Na. However, from the viewpoints of anion insertion and desorption performance at the positive electrode, metal deposition and dissolution performance at the negative electrode, positive electrode reaction potential and negative electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability against the electrolyte, etc., it is preferable that the content of these other electrolyte salts is small. Specifically, it is preferable that the content of the potassium salt and / or rubidium salt is 80 to 100 mol%, particularly 90 to 100 mol%, with the total amount of the electrolyte salt being 100 mol%.

[0058] The concentration of the electrolyte salt is not particularly limited and can be appropriately selected, but from the viewpoints of the operating potential, capacity, output, etc., it is preferably 0.1 to 1.5 mol / L, more preferably 0.3 to 0.6 mol / L.

[0059] In the present invention, in order to operate the dual ion battery at a higher potential, the solvent constituting the electrolyte is preferably an ionic liquid. As such an ionic liquid, it is preferable to use an ionic liquid composed of a cationic component, such as a nitrogen-containing cation (e.g., pyrrolidinium cation, piperidinium cation, imidazolium cation, quaternary ammonium cation) or a phosphorus-containing cation (e.g., quaternary phosphonium cation), and an anionic component.

[0060] Examples of pyrrolidinium cations include N-methylpyrrolidinium cation, N-ethylpyrrolidinium cation, Nn-propylpyrrolidinium cation, N,N-dimethylpyrrolidinium cation, N-ethyl-N-methylpyrrolidinium cation, and N-methyl-Nn-propylpyrrolidinium cation (Pyr 13 ), N-methyl-Nn-butylpyrrolidinium cation (Pyr 14 ) etc.

[0061] Examples of the piperidinium cation include N-methylpiperidinium cation, N-ethylpiperidinium cation, Nn-propylpiperidinium cation, N,N-dimethylpiperidinium cation, 1-ethyl-1-methylpiperidinium cation, and 1-methyl-1-n-propylpiperidinium cation.

[0062] Examples of the imidazolium cation include a 1,3-dimethylimidazolium cation, a 1-ethyl-3-methylimidazolium cation, a 1-methyl-3-n-propylimidazolium cation, and a 1-methyl-3-n-butylimidazolium cation.

[0063] Examples of the quaternary ammonium cation include an ethyltrimethylammonium cation, a triethylmethylammonium cation, an ethyltri-n-propylammonium cation, a triethyl-n-propylammonium cation, and a tetra-n-propylammonium cation.

[0064] Examples of the quaternary phosphonium cation include a tetramethylphosphonium cation, a triethylmethylphosphonium cation, a tetraethylphosphonium cation, an ethyltri-n-propylphosphonium cation, and a tetra-n-propylphosphonium cation.

[0065] The anion component may be, for example, hexafluorophosphate anion (PF 6 -), tetrafluoroborate anion (BF 4 - ), arsenic hexafluoride anion (AsF 6 - ), trifluoromethanesulfonate anion (CF 3 SO 3 - ), bisfluorosulfonylimide anion (N(FSO 2 ) 2 - ;FSI), bistrifluoromethanesulfonylimide anion (N(CF 3 SO 2 ) 2 - TFSI), bispentafluoroethanesulfonylimide anion (N(C 2 F 5 SO 2 ) 2 - ), Fluorosulfonyltrifluorosulfonimide (NFSO 2 (CF 3 SO 2 ) - ) etc.

[0066] The combination of the above-mentioned cation component and anion component is not particularly limited. In particular, from the viewpoints of anion insertion and desorption performance at the positive electrode, metal deposition and dissolution performance at the negative electrode, the positive electrode reaction potential and the negative electrode reaction potential of the resulting dual ion battery, charge / discharge cycle characteristics, stability against the electrolyte, etc., N-methyl-Nn-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr 13 TFSI), N-methyl-Nn-butylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr 14 TFSI), N-methyl-Nn-propylpyrrolidinium bisfluoromethanesulfonylimide (Pyr 13 FSI), N-methyl-Nn-butylpyrrolidinium bisfluoromethanesulfonylimide (Pyr 14FSI), N-methyl-Nn-propyl piperidinium bistrifluoromethanesulfonylimide, N-methyl-Nn-butyl piperidinium bistrifluoromethanesulfonylimide, N-methyl-Nn-propyl piperidinium bisfluoromethanesulfonylimide, N-methyl-Nn-butyl piperidinium bisfluoromethanesulfonylimide, 1-ethyl-3-methylimidazolium bisfluoromethanesulfonylimide, 1-butyl-3-methylimidazolium bisfluoromethanesulfonylimide, etc. are preferred. These ionic liquids can be used alone or in combination of two or more.

[0067] In the present invention, the solvent may be composed only of the ionic liquid described above, but may also contain other solvents. Examples of such other solvents include chain esters such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and methyl propyl carbonate; cyclic esters such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate; and ethers such as dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether. However, from the viewpoints of anion insertion and desorption performance at the positive electrode, metal deposition and dissolution performance at the negative electrode, the positive electrode reaction potential and negative electrode reaction potential of the resulting dual ion battery, charge and discharge cycle characteristics, and stability against the electrolyte, it is preferable that the content of these other solvents is small. Specifically, it is preferable that the total amount of the solvent is 100 mol%, and the content of the ionic liquid is 80 to 100 mol%, particularly 90 to 100 mol%.

[0068] The content of the solvent may be an excess amount, and specifically, the content can be adjusted so that the concentration of the electrolyte salt falls within the above range.

[0069] The electrolytic solution is usually in a liquid state, but a gel electrolyte obtained by gelling the electrolytic solution with a gelling agent made of a polymer or the like can also be used.

[0070] 4. Separator A separator may be provided between the positive and negative electrodes to prevent short circuits between the positive and negative electrodes.

[0071] Examples of materials for the separator include paper such as kraft paper, vinylon-mixed paper, and synthetic pulp-mixed paper, cellophane, polyethylene graft membrane, polyolefin nonwoven fabric such as polypropylene melt-blown nonwoven fabric, polyamide nonwoven fabric, glass fiber nonwoven fabric, and micropore membrane.

[0072] The separator may be in the form of a thin film having micropores or a nonwoven fabric having a high porosity.

[0073] The thickness of the separator is preferably 20 μm or more from the viewpoints of preventing short circuits and retaining the electrolyte.

[0074] The size of the separator is not particularly limited as long as it is a size that can be used in a dual ion battery, and can be appropriately selected depending on the purpose.

[0075] The separator may have a single-layer structure or a laminate structure.

[0076] 5. Manufacturing method of dual-ion battery The dual ion battery of the present invention can be manufactured by assembling the positive electrode, the negative electrode, the electrolyte, and the separator, which is used as necessary, into an appropriate shape. Furthermore, other components such as an outer can can be used as necessary. There is no particular limitation on the method for assembling the dual ion battery, and it can be appropriately selected from methods that are commonly used in known secondary batteries such as lithium ion secondary batteries.

[0077] The shape of the dual ion battery of the present invention is not particularly limited, and can be appropriately selected according to the application from various shapes generally adopted in known secondary batteries such as lithium ion secondary batteries. Examples of the shape include a cylinder type in which a sheet electrode and a separator are spirally wound, a cylinder type with an inside-out structure in which a pellet electrode and a separator are combined, and a coin type in which a pellet electrode and a separator are laminated. EXAMPLES

[0078] The present invention will be described in detail below based on examples, although the present invention is not limited to the following examples.

[0079] In the examples, the following materials were used as the carbonaceous material serving as the positive electrode active material, the metal material serving as the negative electrode active material, the constituent materials of the electrolyte, and the separator. Carbonaceous material: KS-6L (graphite; average particle size D90: 13.9 μm, specific surface area: 13.0 m 2 / g) Potassium metal: Sigma-Aldrich Rubidium metal: Sigma-Aldrich Lithium metal: Honjo Metal Industry Co., Ltd. Sodium metal: Sigma-Aldrich Potassium bistrifluoromethanesulfonylimide (KN(CF 3 SO 2 ) 2 ;KTFSI): Kanto Chemical Co., Ltd. Rubidium bistrifluoromethanesulfonylimide (RbN(CF 3 SO 2 ) 2 ;RbTFSI) Lithium bistrifluoromethanesulfonylimide (LiN(CF 3 SO 2 ) 2 ; LiTFSI): Kanto Chemical Co., Ltd. Sodium trifluoromethanesulfonylimide (NaN(CF 3 SO2 ) 2 ;NaTFSI): Tokyo Chemical Industry Co., Ltd. Potassium bisfluoromethanesulfonyl imide (KN(FSO 2 ) 2 ;KFSI): Kanto Chemical Co., Ltd. 1-Methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr 13 TFSI): Kanto Chemical Co., Ltd. 1-Methyl-1-n-propylpyrrolidinium bisfluoromethanesulfonylimide (Pyr 13 FSI): Kanto Chemical Co., Ltd. Separator: Polyethylene separator, glass filter.

[0080] Example 1 A 2032-type coin-type dual ion battery was constructed with the cell configuration shown in Table 1 below. Specifically, a slurry containing 92% by mass of a carbonaceous material (KS-6L) and 8% by mass of polyvinylidene fluoride as a binder was applied to an aluminum foil (thickness 20 μm) as a positive electrode current collector, and the resulting dried positive electrode material (thickness 18 μm) was formed to form the positive electrode. A sheet of potassium metal was used as the negative electrode. The electrolyte was a mixture of ionic liquid 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) and 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) as a solvent. 13 Potassium bistrifluoromethanesulfonylimide (KN(CF 3 SO 2 ) 2 ;KTFSI) was dissolved in the electrolyte. A polyethylene separator and a glass filter were used as separators. Specifically, a polyethylene separator was impregnated with the electrolyte and placed between the positive and negative electrodes to construct a dual ion battery.

[0081] Example 2 The ionic liquid 1-methyl-1-n-propylpyrrolidinium bisfluoromethanesulfonylimide (Pyr) was used as a solvent. 13Potassium bisfluoromethanesulfonylimide (KN(FSO 2 ) 2 A dual ion battery was constructed in the same manner as in Example 1, except that an electrolyte solution in which KFSI (KFeO2) was dissolved was used.

[0082] Example 3 A 2032-type coin-type dual ion battery was constructed with the cell configuration shown in Table 1 below. Specifically, a slurry containing 92% by mass of a carbonaceous material (KS-6L) and 8% by mass of polyvinylidene fluoride as a binder was applied to an aluminum foil (thickness 20 μm) as a positive electrode current collector, and the slurry was dried to form a positive electrode material (thickness 18 μm) to form the positive electrode. A sheet of rubidium metal was used as the negative electrode. The electrolyte was a mixture of ionic liquid 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) and 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) as a solvent. 13 Rubidium bistrifluoromethanesulfonylimide (RbN(CF 3 SO 2 ) 2 ;RbTFSI) was dissolved in the electrolyte. One polyethylene separator and one glass filter were used. Specifically, a polyethylene separator was soaked in the electrolyte and placed between the positive and negative electrodes to construct a dual-ion battery.

[0083] Comparative Example 1 A 2032-type coin-type dual ion battery was constructed with the cell configuration shown in Table 1 below. Specifically, a slurry containing 92% by mass of a carbonaceous material (KS-6L) and 8% by mass of polyvinylidene fluoride as a binder was applied to an aluminum foil (thickness 20 μm) as a positive electrode current collector, and the slurry was dried to form a positive electrode material (thickness 18 μm) to form the positive electrode. A sheet-shaped lithium metal (thickness 400 μm) was used as the negative electrode. The electrolyte was a mixture of ionic liquid 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) and 1,2-dichlorophenyl ether (DMSO) as a solvent. 13Lithium bistrifluoromethanesulfonylimide (LiN(CF)) was added to TFSI at a concentration of 0.5 mol / L. 3 SO 2 ) 2 ;LiTFSI) was dissolved in the electrolyte. One polyethylene separator and one glass filter were used. Specifically, the polyethylene separator was impregnated with the electrolyte and placed between the positive and negative electrodes to construct a dual ion battery.

[0084] Comparative Example 2 A 2032-type coin-type dual ion battery was constructed with the cell configuration shown in Table 1 below. Specifically, a slurry containing 92% by mass of a carbonaceous material (KS-6L) and 8% by mass of polyvinylidene fluoride as a binder was applied to an aluminum foil (thickness 20 μm) as a positive electrode current collector, and the resulting dried positive electrode material (thickness 18 μm) was formed to form the positive electrode. A sheet of sodium metal was used as the negative electrode. The electrolyte was a mixture of ionic liquid 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) and 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr) as a solvent. 13 Sodium bistrifluoromethanesulfonylimide (NaN(CF 3 SO 2 ) 2 ;NaTFSI) was dissolved in the electrolyte. A polyethylene separator and a glass filter were used as separators. Specifically, a polyethylene separator was impregnated with the electrolyte and placed between the positive and negative electrodes to construct a dual ion battery.

[0085] [Table 1]

[0086] Test Example 1: Evaluation of anion insertion and desorption reactions on the positive electrode Cyclic voltammetry was performed using the dual ion batteries of Examples 1 and 3 and Comparative Example 1. The measurement conditions were 25° C., the scan rate was 0.2 mV / s, and the scan range was 3.0 V or more. The results are shown in FIGS. 1 to 3. As a result, in Examples 1 and 3, there was a peak due to the anion insertion reaction at around 4.95 V, which was confirmed to be higher than the peak at around 4.55 V in Comparative Example 1, and the insertion and desorption of anions at the positive electrode were performed at a higher potential. In other words, by using potassium metal or rubidium metal as the negative electrode, the anion insertion potential was shifted to the higher potential side by about 0.4 V.

[0087] Test Example 2: Evaluation of metal deposition and dissolution reactions on the negative electrode The deposition and dissolution reactions of metals on the negative electrodes of the dual ion batteries of Examples 1 and 3 and Comparative Examples 1 and 2 were simply evaluated. 13 Potassium bistrifluoromethanesulfonylimide (KN(CF 3 SO 2 ) 2 ;KTFSI), rubidium bistrifluoromethanesulfonylimide (RbN(CF 3 SO 2 ) 2 ;RbTFSI), lithium bistrifluoromethanesulfonylimide (LiN(CF 3 SO 2 ) 2 ;LiTFSI) or sodium bistrifluoromethanesulfonylimide (NaN(CF 3 SO 2 ) 2 The electrolyte used was a nickel metal working electrode and a platinum metal counter electrode, and silver trifluoromethanesulfonate was diluted with 1-methyl-1-n-propylpyrrolidinium bistrifluoromethanesulfonylimide (Pyr;NaTFSI) to a concentration of 0.1 mol / L. 13Cyclic voltammetry was performed using a silver wire immersed in a solution of 1,2-dichlorophenyl tetrahydrofuran (TFSI) as a reference electrode. After the measurement, ferrocene was dissolved in the electrolyte and the redox potential was measured to calibrate the potential. The measurement conditions were 25°C and the scan rate was 1 mV / s. The results are shown in FIG. 4. As a result, in the electrolytes of Examples 1 and 3, there was a peak due to the anode reaction at around -3.5 V, and compared to the peaks at around -3.2 V in Comparative Example 1 and around -3.1 V in Comparative Example 2, it was confirmed that metal deposition and dissolution at the anode occurred at a lower potential. This result suggests that the deposition and dissolution of potassium and rubidium on the anode side are used for the anode reaction, which results in a higher voltage dual battery compared to the case of using lithium or sodium.

[0088] Test example 3: Evaluation of potential window Cyclic voltammetry was performed using the dual ion battery of Example 1. The measurement conditions were 25° C. and the scan rate was 0.2 mV / s. The results are shown in FIG. 5. As a result, the voltage from the peak caused by metal deposition and dissolution of the negative electrode to the peak caused by the anion insertion reaction of the positive electrode was about 5.0 V, suggesting that a dual ion battery exhibiting a high potential of about 5.0 V was constructed.

[0089] Test example 4: Constant current charge / discharge test Using the dual ion batteries of Examples 1 to 3, the following conditions were used: Charge / discharge conditions 3.0~5.0V Charge / discharge rate 0.05C Test temperature: 25℃ The battery was charged and discharged 30 times.

[0090] As a result, in all dual ion batteries, it was possible to repeatedly charge and discharge at a high voltage of about 5.0 V. In addition, the charge and discharge cycle characteristics (discharge capacity at the 30th cycle / discharge capacity at the 2nd cycle) were 100% in Example 1, 100% in Example 2, and 90% in Example 3. In Examples 1 and 2, the discharge capacity gradually increased with repeated cycles, so the capacity retention rate exceeded 100% in calculation, but here, for convenience, the capacity retention rate is set to 100%.

Claims

1. A dual ion battery in which the positive electrode reaction is an anion insertion / extraction reaction and the negative electrode reaction is a metal deposition and dissolution reaction, A positive electrode, a negative electrode, and an electrolyte solution are provided, The positive electrode contains a positive electrode active material including a carbonaceous material, the negative electrode contains a negative electrode active material including rubidium metal, The dual ion battery, wherein the electrolyte contains a solvent including an ionic liquid.

2. 2. The dual ion battery of claim 1, wherein the positive electrode active material consists solely of the carbonaceous material.

3. 3. The dual ion battery of claim 1, wherein the positive electrode contains the carbonaceous material, a binder, and a thickener.

4. The dual ion battery according to any one of claims 1 to 3, wherein the negative electrode active material consists solely of the rubidium metal.

5. The dual ion battery according to any one of claims 1 to 4, wherein the negative electrode consists solely of rubidium metal.

6. The dual ion battery according to any one of claims 1 to 5, wherein the electrolyte solution contains an electrolyte salt including a rubidium salt.

Citation Information

Patent Citations

  • Application of expanded graphite in potassium ion battery negative electrode material

    CN107331866A

  • Preparation method of potassium double ion battery with double carbon electrodes

    CN108630939A

  • Anion pre-embedding method and total battery

    CN109560339A

  • Power storage device

    JP2015153700A

  • Nonaqueous electrolyte power storage element

    JP2017220311A