Method for producing tantalum nitride
By controlling the nitrogen and ammonia gas ratio during tantalum nitride production, a small particle size and large specific surface area are achieved, addressing the limitations of existing methods and enabling high-purity tantalum nitride production suitable for photocatalytic applications.
Patent Information
- Application Number
- JP2020186768
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-14
- Filing Date
- 2020-11-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-11-09
AI Technical Summary
Existing methods for producing tantalum nitride as a photocatalyst material face challenges in achieving high photocatalytic activity due to limitations in particle size and specific surface area, with concerns about foreign matter contamination and oxidation during pulverization.
The production of tantalum nitride is conducted in a mixed gas atmosphere of nitrogen and ammonia, with a controlled volume ratio of 9 or less, at a temperature of 800 to 950°C, resulting in a small particle size and large specific surface area without the need for pulverization.
This method allows for the production of tantalum nitride with a BET specific surface area of 10.0 m²/g or more and an average particle diameter of 2 μm or less, maintaining high purity by minimizing impurities such as oxygen, iron, and chromium.
Smart Images

Figure 0007573417000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing tantalum nitride. [Background technology]
[0002] Tantalum nitride (Ta3N5) has attracted attention as a photocatalytic material, for example, as a photocatalyst for generating oxygen that can decompose water into hydrogen and oxygen. For example, it is produced by calcining tantalum oxide in an ammonia gas atmosphere (Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-156673 A [Patent Document 2] JP 2017-164732 A [Patent Document 3] JP 2002-233769 A Summary of the Invention [Problem to be solved by the invention]
[0004] When tantalum nitride is used as a photocatalytic material, it is required to have a higher photocatalytic activity. To meet such a requirement, it is advantageous to make the particle size of tantalum nitride smaller and the specific surface area larger. In Patent Document 1, tantalum nitride is crushed to reduce the particle size and increase the specific surface area of tantalum nitride, but there are concerns about the inclusion of foreign matter and oxidation during crushing. An object of the present invention is to provide tantalum nitride having a small particle size and a large specific surface area, and a method for producing the same. [Means for solving the problem]
[0005] As a result of investigations aimed at solving the above problems, the inventors have found that by using a mixed gas of nitrogen gas and ammonia gas in the atmosphere when producing tantalum nitride by firing a tantalum compound, and controlling the volume ratio of nitrogen gas to ammonia gas in the mixed gas to a specific value or less, it is possible to obtain tantalum nitride having a small particle size and a large specific surface area, without necessarily requiring pulverization.
[0006] That is, the present invention provides the following [1] to [8]. [1] A method for producing a tantalum compound, comprising the steps of: firing the tantalum compound in an atmosphere of a mixed gas of nitrogen gas and ammonia gas; The volume ratio of nitrogen gas to ammonia gas in the mixed gas (nitrogen / ammonia) is 9 or less. A method for producing tantalum nitride. [2] The method for producing tantalum nitride according to [1] above, wherein the tantalum compound is tantalum oxide. [3] The method for producing tantalum nitride according to [1] or [2] above, wherein the firing temperature is 800 to 950°C. [4] BET specific surface area is 10.0m 2 / g or more. [5] The tantalum nitride according to [4] above, having an average particle size of 2 μm or less. [6] The tantalum nitride according to [4] or [5] above, having an oxygen content of 2.0 mass% or less. [7] The tantalum nitride according to any one of [4] to [6] above, having an iron content of 30 ppm by mass or less. [8] The tantalum nitride according to any one of [4] to [7] above, having a chromium content of 10 ppm by mass or less. Effect of the Invention
[0007] According to the present invention, tantalum nitride having a small particle size and a large specific surface area can be produced industrially and advantageously. Moreover, according to the present invention, it is possible to obtain a small particle size and a large specific surface area of tantalum nitride even without pulverization, so that high-purity tantalum nitride can be obtained. Therefore, the tantalum nitride of the present invention is useful as a photocatalytic material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Method of producing tantalum nitride] The method for producing tantalum nitride of the present invention includes a step of firing a tantalum compound in an atmosphere of a mixed gas of nitrogen gas and ammonia gas, and is characterized in that the volume ratio of nitrogen gas to ammonia gas (nitrogen / ammonia) in the mixed gas is 9 or less.
[0009] (Tantalum compounds) As the tantalum compound, for example, tantalum oxide, tantalum halide, tantalic acid or its salt, and tantalum complex can be used. Among them, tantalum oxide is preferable from the viewpoint of production efficiency. The tantalum compound may be chemically synthesized or may be a commercially available product.
[0010] The tantalum compound may be in bulk or powder, but is preferably in powder from the viewpoint of small particle size and high specific surface area. The size of the tantalum compound can be appropriately selected according to the particle size of the desired tantalum nitride, but for example, from the viewpoint of further small particle size and high specific surface area, the average particle size is preferably 2 μm or less, more preferably 1.8 μm or less, and even more preferably 1.5 μm or less. The lower limit of the average particle size is not particularly limited and can be appropriately selected, but is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. Here, in this specification, the "average particle size" means the particle size (D50) corresponding to 50% of the cumulative distribution curve when the particle size distribution of the sample is created on a volume basis in accordance with JIS R 1629 "Method of measuring particle size distribution by laser diffraction and scattering method for fine ceramic raw materials". As a particle size distribution measuring device by the laser diffraction and scattering method, for example, Microtrac MT3300EX II (manufactured by Microtrac Bell Co., Ltd.) can be used. In order to obtain a tantalum compound having a desired particle size, the tantalum compound may be pulverized using a media pulverizer, such as a planetary ball mill, a ball mill, or a disk mill.
[0011] (mixed gas) The mixed gas is composed of nitrogen gas and ammonia gas. As the nitrogen gas, for example, nitrogen cylinder gas or liquefied nitrogen with a purity of 99.9% by volume or more can be used, and as the ammonia gas, for example, liquefied ammonia with a purity of 99.8% by mass or more can be used.
[0012] The volume ratio of nitrogen gas to ammonia gas in the mixed gas (nitrogen / ammonia) is 9 or less, but from the viewpoint of reducing particle size and increasing the specific surface area, it is preferably 0.1 to 9, more preferably 0.2 to 8.5, even more preferably 0.2 to 8, and still more preferably 0.2 to 7.
[0013] As a method for supplying the mixed gas, a predetermined amount of nitrogen gas and a predetermined amount of ammonia gas may be mixed and supplied to the calcination apparatus, or both may be supplied to the calcination apparatus through separate pipes. The supply rates of the nitrogen gas and ammonia gas are controlled usually within the range of 0.01 to 100 L / min, preferably 0.05 to 10 L / min, and more preferably 0.1 to 5 L / min so that the volume ratio of the two gases is within the above range.
[0014] (Firing) The apparatus used for firing is not particularly limited as long as it can withstand the firing temperature, and examples thereof include a tubular furnace, an electric furnace, a batch kiln, and a rotary kiln. The firing may be performed under a mixed gas atmosphere, either in a mixed gas atmosphere or in a closed space replaced with the mixed gas. Among these, from the viewpoint of promoting the nitriding reaction, it is preferable to perform the firing under a mixed gas atmosphere.
[0015] The firing may be carried out at normal pressure, and there is no need to apply pressure or a vacuum. The firing temperature is usually 800 to 950°C, and preferably 800 to 900°C, from the viewpoint of promoting the nitriding reaction. The calcination time varies depending on the reaction scale, but is usually 1 to 60 hours, preferably 5 to 40 hours, and more preferably 10 to 30 hours.
[0016] After the tantalum compound is fired, the fired product may be cooled, for example, to room temperature (20±15° C.).
[0017] Tantalum nitride can be produced in this manner, and the resulting tantalum nitride is a single phase Ta3N5. In addition, in the present invention, since it is possible to reduce the particle size and increase the specific surface area even without pulverization, high-purity tantalum nitride can be obtained. Specifically, the tantalum nitride produced by the method of the present invention can have the physical properties described below. If it is desired to further reduce the particle size of tantalum nitride, it may be pulverized, but it is preferable to use a pulverization medium that can prevent foreign matter from being mixed in. In addition, from the viewpoint of preventing oxidation, it is preferable to perform the pulverization, for example, under an inert gas atmosphere at room temperature (20°C ± 15°C). The pulverization conditions can be appropriately set depending on the type of pulverization device, the production scale, and the like.
[0018] [Tantalum nitride] The tantalum nitride of the present invention is characterized by having a larger BET specific surface area than conventional tantalum nitrides. Specifically, the BET specific surface area of the tantalum nitride is 10.0 m 2 / g or more, but 10.3m 2 / g or more is preferable, and 10.5m 2 / g or more is more preferable, and 10.7m 2 The upper limit of the BET specific surface area is not particularly limited, but from the viewpoint of production efficiency, it is preferably 100 m 2 / g or less is preferable, and 50m 2 / g or less is more preferable, and 30m 2 In this specification, the term "BET specific surface area" refers to a surface area measured by the BET method (a method for measuring surface area by utilizing the adsorption of gas molecules), and can be measured, for example, by using an automatic flow type specific surface area measuring device (Flowsorb III2305, manufactured by Shimadzu Corporation).
[0019] The tantalum nitride of the present invention has a small particle size. Specifically, the average particle size of tantalum nitride is usually 2 μm or less, more preferably 1.8 μm or less, and even more preferably 1.5 μm or less. The lower limit of the average particle size is not particularly limited, but from the viewpoint of production efficiency, it is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more. The "average particle size" here is as explained above.
[0020] Furthermore, the tantalum nitride of the present invention is characterized by its high purity, for example, the content of impurities such as oxygen, iron and chromium in the tantalum nitride of the present invention is extremely low. The oxygen content in the tantalum nitride of the present invention is usually 2.0 mass%, preferably 1.8 mass% or less, and more preferably 1.5 mass% or less. The lower limit of the oxygen content in the tantalum nitride is not particularly limited, and may be 0 mass%. The iron content in the tantalum nitride of the present invention is usually 30 ppm by mass or less, preferably 20 ppm by mass or less, more preferably 15 ppm by mass or less, and further preferably 12 ppm by mass or less. The lower limit of the iron content in the tantalum nitride is not particularly limited, and may be 0 ppm by mass. Furthermore, the chromium content in the tantalum nitride of the present invention is usually 10 mass ppm or less, preferably 5 mass ppm or less, more preferably 3 mass ppm or less, and even more preferably 1 mass ppm or less. The lower limit of the chromium content in the tantalum nitride is not particularly limited, and may be 0 mass ppm. The oxygen, iron and chromium contents in tantalum nitride are measured by the method described in the Examples below.
[0021] The tantalum nitride of the present invention can be produced by any appropriate method as long as it has the above-mentioned BET specific surface area, etc., but the production method of the present invention is useful in that it can easily produce the desired tantalum nitride. EXAMPLES
[0022] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0023] 1. Identification of mineral phases Measurements were performed using a powder X-ray diffractometer (Bruker D8 advance, manufactured by Bruker AXS Co., Ltd.), and the mineral phases were identified from the obtained X-ray diffraction patterns.
[0024] 2. Measurement of BET specific surface area The BET specific surface area of tantalum nitride was measured using an automatic flow type specific surface area measuring device (Flowsorb III2305, manufactured by Shimadzu Corporation).
[0025] 3. Measurement of average particle size The particle size distribution of tantalum nitride was created on a volume basis in accordance with JIS R 1629 "Method for measuring particle size distribution of fine ceramic raw materials by laser diffraction and scattering method," and the particle size (D50) corresponding to 50% of the cumulative distribution curve was calculated. The particle size distribution measuring device used by the laser diffraction and scattering method was Microtrac MT3300EX II (Microtrac Bell).
[0026] 4. Analysis of impurities (1) Oxygen Analysis The tantalum nitride powder was packed into a sample capsule in a glove box, and the oxygen content was measured using an oxygen and nitrogen simultaneous analyzer (TCH-600, manufactured by LECO Japan).
[0027] (2) Analysis of iron and chromium 0.1 g of tantalum nitride powder was placed in a container together with 1 mL of hydrofluoric acid (a 1:1 mixture of hydrofluoric acid (ultra-pure reagent) and ultra-pure water) and 1 mL of hydrogen peroxide (for atomic absorption spectrometry), and microwave decomposition was performed for 5 hours at 180 °C using a microwave decomposition system (MARS6, CEM Japan). 10 mL of 4% boric acid solution (prepared using boric acid (EDM Millipore Corporation)) and 2.5 mL of nitric acid 1.38 (Kanto Chemical) were added to the resulting solution, and the volume was then adjusted to 50 mL. This solution was measured using an ICP mass spectrometer (Agilent 7900ICP-MS, Agilent Technologies) to calculate the iron and chromium contents.
[0028] 5.Raw materials used In the following examples and comparative examples, tantalum oxide (Ta2O5, manufactured by Mitsui Kinzoku Co., Ltd.) was used as a raw material. The average particle size (D50) was 1.1 μm.
[0029] Example 1 5 g of tantalum oxide was weighed out and placed in a tubular furnace. A mixed gas of nitrogen gas and ammonia gas, mixed in the ratio shown in Table 1, was circulated in the tubular furnace, and the temperature was raised to 850°C in 2 hours, and the mixture was held for 20 hours to obtain a mineral. The obtained mineral was measured using a powder X-ray diffractometer, and the mineral phase was identified from the obtained X-ray diffraction pattern, and it was confirmed to be a single Ta3N5 phase. In addition, the BET specific surface area and average particle size of the tantalum nitride were measured, and impurities were analyzed. The results are shown in Table 1.
[0030] Examples 2 to 5 A mineral was obtained by the same operation as in Example 1, except that a mixed gas having the ratio shown in Table 1 was passed through. The mineral phase of the obtained mineral was identified in the same manner as in Example 1, and it was confirmed to be a Ta3N5 single phase. In addition, the BET specific surface area and average particle size of the tantalum nitride were measured, and impurities were analyzed. The results are shown in Table 1.
[0031] Comparative Example 1 A mineral was obtained by the same operation as in Example 1, except that only ammonia gas was used. The mineral phase of the obtained mineral was identified in the same manner as in Example 1, and it was confirmed to be a Ta3N5 single phase. In addition, the BET specific surface area and average particle size of the tantalum nitride were measured, and impurities were analyzed. The results are shown in Table 1.
[0032] Comparative Example 2 A mineral was obtained by the same operation as in Example 1, except that a mixed gas having the ratio shown in Table 1 was passed through. The mineral phase of the obtained mineral was identified in the same manner as in Example 1, and it was confirmed to be TaON. Therefore, the measurement of the BET specific surface area and the average particle size was abandoned.
[0033] [Table 1]
[0034] It can be seen from Comparative Example 1 that when an atmosphere containing only ammonia gas and no nitrogen gas is used, even if tantalum nitride is obtained, the particle size is large and the BET specific surface area is small. It is clear from Comparative Example 2 that even in an atmosphere of a mixed gas of nitrogen gas and ammonia gas, if the volume ratio of nitrogen gas to ammonia gas in the mixed gas exceeds 9, tantalum nitride cannot be obtained. In contrast, in Examples 1 to 5, by using a mixed gas atmosphere of nitrogen gas and ammonia gas and controlling the volume ratio of nitrogen gas to ammonia gas in the mixed gas to 9 or less, it was possible to obtain a small particle size of 2 μm or less and a particle size of 10.0 m without the need for pulverization. 2 It can be seen that the tantalum nitride obtained has a high specific surface area of 1000 nm or more and is of high purity with little impurities such as oxygen, iron and chromium.
Claims
1. A method for producing a ceramic ceramic ceramic, comprising the steps of: firing Ta2O5 in an atmosphere of a mixed gas of nitrogen gas and ammonia gas; The volume ratio of nitrogen gas to ammonia gas in the mixed gas (nitrogen / ammonia) is 0.2 to 8. A method for producing tantalum nitride (Ta 3 N 5 ).
2. 2. The method for producing tantalum nitride (Ta 3 N 5 ) according to claim 1, wherein the firing temperature is 800 to 950°C.
3. A powder having an average particle size of 2 μm or less and a BET specific surface area of 10.0 to 30 m 2 / g, tantalum nitride (Ta 3 N 5 ).
4. The tantalum nitride (Ta 3 N 5 ) according to claim 3 , having an oxygen content of 2.0 mass % or less.
5. 5. Tantalum nitride (Ta 3 N 5 ) according to claim 3 or 4, having an iron content of 30 ppm by mass or less.
6. The tantalum nitride (Ta 3 N 5 ) according to any one of claims 3 to 5, wherein the chromium content is 10 ppm by mass or less.
Citation Information
Patent Citations
Photolysis catalyst for water decomposition by visible light
JP2002233769A
Nitride having pore structure and method for manufacturing the same
JP2007022858A
METHOD FOR PRODUCING TANTALUM NITRIDE (Ta3 N5)
JP2017164732A
Method for producing tantalum nitride
JP2018162190A
Tantalum nitride crystal
JP2019156673A