Cup-shaped container

The cup-shaped container with a laminate structure of metal foil and heat-fusible resin layers with varying melting points addresses the issues of barrier properties and sterilization, offering low-cost, long-term storage and aseptic capabilities.

JP7573435B2Active Publication Date: 2024-10-25LISSENOK PACKAGING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020212244
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-12-22
Publication Date
2024-10-25
Estimated Expiration
2040-12-22

AI Technical Summary

Technical Problem

Paper cups have low barrier properties and are not suitable for long-term storage, while plastic containers are costly and unsuitable for long-term storage, and both types face issues with delamination and corrosion during sterilization.

Method used

A cup-shaped container with a laminate structure comprising a metal foil layer and a heat-fusible resin layer, where the resin layers have different melting points to prevent delamination and corrosion, allowing for aseptic and retort sterilization.

Benefits of technology

The container provides excellent long-term storage stability, can be manufactured at low cost using paper cup equipment, and prevents delamination and corrosion, ensuring sanitary conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573435000001
    Figure 0007573435000001
  • Figure 0007573435000002
    Figure 0007573435000002
  • Figure 0007573435000003
    Figure 0007573435000003
Patent Text Reader

Abstract

To provide a cuplike container capable of being produced at a cheap price with the use of production facility of paper cups, being excellent in long-life nature of the content, and being aseptic sterilizable and retort sterilizable, in which the container may control degradation due to contact with the content.SOLUTION: A cuplike container comprises two or more layers of heat welding resin layers 202, 203 of a trunk blank 20A, and a heat welding resin configuring a laminate-side heat welding resin layer laminated on a metal foil layer 201 has a lower melting point compared to the heat welding resin configuring other layers. A portion of the metal foil layer 201 of an inner edge face 204 of the trunk blank 20A and an interface portion of the metal foil layer 201 and the heat welding resin layers 202, 203 are coated with a protective coating film M1 formed by fusion and solidification of the heat welding resin which configures the laminate-side heat welding resin layer at the time of heat welding.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cup-shaped container for containing food or beverages such as ice cream or yogurt. [Background technology]

[0002] 2. Description of the Related Art Paper cup-shaped containers, that is, paper cups, are commonly used as containers for filling and packaging semi-solid dairy products such as ice cream and yogurt. A paper cup is usually formed by joining together a body and a bottom, each of which is made of a paper blank cut to a predetermined shape. More specifically, the body is formed into a cylindrical shape by overlapping and joining both end edges of a substantially sector-shaped body blank, with a folded-back portion folded inward at the bottom opening edge and a flange portion curled outward at the top opening edge. The bottom has a substantially inverted U-shaped cross section, formed by skirt-molding a substantially circular bottom blank so that a hanging portion is formed on its outer periphery. The hanging portion of the bottom is wrapped around and joined to the folded-back portion of the body, thereby integrating the body and the bottom. Each blank for the body and bottom body is made of a laminate having, for example, a paper layer made of general base paper, acid-resistant paper, coated paper, etc., and a polyethylene (PE) layer laminated on one or both sides of the paper layer (see, for example, Patent Document 1 below).

[0003] Also known is a paper cup that uses a laminate formed by laminating a barrier layer made of aluminum foil or the like in addition to a paper layer and a polyethylene (PE) layer as the material for each of the above blanks (see, for example, Patent Document 2 below).

[0004] Additionally, containers for ice cream, yogurt, etc., made of plastic molded bodies such as polypropylene (PP) are also known (see, for example, Patent Document 3 below). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 58-30955 [Patent Document 2] JP 2007-210639 A [Patent Document 3] JP 2007-176505 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, while paper cups have excellent productivity and can be manufactured at low cost, they have poor barrier properties and are not suitable for long-term storage of contents. Paper cups with a barrier layer such as aluminum foil improve the long-term storage of the contents, but water easily penetrates through the edges of the paper layer, making retort sterilization impossible. In addition, plastic containers are expensive to manufacture and are not suitable for long-term storage of the contents.

[0007] In order to solve the above problems, the present inventor previously proposed a cup-shaped container using a laminate consisting of a metal foil layer and a heat-fusible resin layer laminated on at least one of its two sides as the material for each of the body blank and the bottom blank (Patent Application No. 2019-106125). The above-mentioned cup-shaped container can be produced inexpensively using paper cup manufacturing equipment, has excellent long-term storage properties for the contents, and can also be subjected to aseptic sterilization or retort sterilization.

[0008] Here, in the case of the above-mentioned cup-shaped container, the inner end face of the body blank located on the inside of the container is exposed to the contents at the overlapping portion of the body. Depending on the type of contents, etc., there is a risk that the inner end face may deteriorate due to delamination (peel-off between layers) or corrosion, and this may not necessarily be desirable from a hygienic standpoint. The object of the present invention is to provide a cup-shaped container which can be produced inexpensively using paper cup manufacturing equipment, has excellent long-term storage properties for the contents, and can be subjected to aseptic sterilization or retort sterilization, and which can suppress deterioration due to contact with the contents. [Means for solving the problem]

[0009] In order to achieve the above object, the present invention comprises the following aspects.

[0010] 1) A cup-shaped container comprising a body formed into a cylindrical shape by overlapping and joining both end edges of a body blank, and a bottom body having a cross section of a generally inverted U-shape formed by forming a bottom body blank so as to form a bottom and a hanging part extending downward from the outer peripheral edge of the bottom body, the body and bottom body being integrated by joining the outer surface of the hanging part of the bottom body to the inner surface of the lower end of the body, the body blank is formed from a laminate consisting of a metal foil layer and heat-sealable resin layers laminated on both sides of the metal foil layer, and both end edges of the body blank are joined by heat-sealing the heat-sealable resin layers constituting the mutually overlapping surfaces of the metal foil layer, The bottom body blank is formed from a laminate consisting of a metal foil layer and a heat-sealable resin layer laminated on at least one of both sides of the metal foil layer that will be the upper side of the bottom body, and the inner surface of the lower end of the body and the outer surface of the hanging part of the bottom body are joined by heat-sealing the heat-sealable resin layers that make up these surfaces, At least one of the two heat-fusible resin layers of the body blank is composed of two or more layers, and the heat-fusible resin constituting the laminate-side heat-fusible resin layer laminated on the metal foil layer among the two or more layers has a melting point lower than that of the heat-fusible resin constituting the other layers, A cup-shaped container in which, in the overlapping portion of the body, a metal foil layer portion on the inner end face of a body blank located on the inside of the body and an interface portion between the metal foil layer and a heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the heat-sealable resin constituting the laminate side heat-sealable resin layer when the heat-sealable resin layers at both end edges of the body blank are heat-sealed to each other.

[0011] 2) Furthermore, in the overlapping portion of the body, the metal foil layer portion of the outer end face of the body blank located on the outside of the body and the interface portion between the metal foil layer and the heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the heat-sealable resin constituting the laminate-side heat-sealable resin layer when the heat-sealable resin layers at both end edges of the body blank are heat-sealed to each other.

[0012] 3) A cup-shaped container comprising a body formed into a cylindrical shape by overlapping and joining both end edges of a body blank in a palm-to-palm shape, and a bottom body having a cross section of a generally inverted U-shape formed by forming a bottom body blank so as to form a bottom and a hanging part extending downward from the outer peripheral edge of the bottom body, the body and bottom body being integrated by joining the outer surface of the hanging part of the bottom body to the inner surface of the lower end of the body, the body blank is formed from a laminate consisting of a metal foil layer and heat-sealable resin layers laminated on both sides of the metal foil layer, and both end edges of the body blank are joined by heat-sealing the heat-sealable resin layers constituting the mutually overlapping surfaces of the metal foil layer, The bottom body blank is formed from a laminate consisting of a metal foil layer and a heat-sealable resin layer laminated on at least one of both sides of the metal foil layer that will be the upper side of the bottom body, and the inner surface of the lower end of the body and the outer surface of the hanging part of the bottom body are joined by heat-sealing the heat-sealable resin layers that make up these surfaces, the heat-fusible resin layer of the body blank is composed of two or more layers, and the heat-fusible resin constituting the laminate-side heat-fusible resin layer laminated on the metal foil layer among the two or more layers has a melting point lower than that of the heat-fusible resin constituting the other layers; A cup-shaped container in which, at the joint portion of the body, the metal foil layer portions on both end faces of the body blank located on the outside of the body and the interface portions between the metal foil layer and the heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the heat-sealable resin constituting the laminate side heat-sealable resin layer when the heat-sealable resin layers on both end edges of the body blank are heat-sealed to each other.

[0013] 4) The cup-shaped container of 3) above, wherein the joint portion of the body is folded to one side so as to overlap the outer surface of the body and is heat-sealed to said outer surface.

[0014] 5) The cup-shaped container according to any one of 1) to 4) above, wherein the melting point of the heat-fusible resin constituting the laminate side heat-fusible resin layer is 10°C or more lower than the melting point of the heat-fusible resin constituting the other layer.

[0015] 6) The cup-shaped container according to 5) above, wherein the melting point of the heat-fusible resin constituting the laminate side heat-fusible resin layer is 110 to 140°C.

[0016] 7) The cup-shaped container according to any one of 1) to 6) above, wherein the melt mass flow rate (MFR) of the heat-fusible resin constituting the laminate side heat-fusible resin layer is 1 to 5 g / 10 min or more higher than the melt mass flow rate (MFR) of the heat-fusible resin constituting the other layer.

[0017] 8) The cup-shaped container according to 7) above, wherein the melt mass flow rate (MFR) of the heat-fusible resin constituting the laminate side heat-fusible resin layer is 4 to 10 g / 10 min. Effect of the Invention

[0018] According to the cup-shaped container of 1) above, in the overlapping portion of the body, the metal foil layer portion of the inner end face of the body blank located on the inside of the body and the interface portion between the metal foil layer and the heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate-side heat-sealable resin layer in the heat-sealable resin layer consisting of two or more layers of the body blank during heat fusion, and are not exposed to the contents, so that deterioration due to delamination and corrosion of the inner end face is effectively suppressed and it is also preferable from a hygienic standpoint. In addition, for the purpose of specifying this invention, the "melting point" refers to the melting peak temperature (Tmp) measured by differential scanning calorimetry (DSC) in accordance with JIS K7121-1987.

[0019] According to the cup-shaped container of 2) above, in the overlapping portion of the body, the metal foil layer portion of the outer end face of the body blank located on the outside of the body and the interface portion between the metal foil layer and the heat-sealable resin layer are also covered with a protective coating formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate-side heat-sealable resin layer in the heat-sealable resin layer consisting of two or more layers of the body blank during heat fusion, so that deterioration due to delamination and corrosion of the outer end face is effectively suppressed.

[0020] According to the cup-shaped container of 3) above, at the joint portion of the body, the metal foil layer portions of both end faces of the body blank located on the outside of the body and the interface portions between the metal foil layer and the heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate-side heat-sealable resin layer in the heat-sealable resin layer consisting of two or more layers of the body blank during heat fusion, so that deterioration due to delamination and corrosion of both end faces is effectively suppressed.

[0021] In the cup-shaped container of 4) above, the joint of the body is folded to one side and heat-sealed to the outer surface of the body, improving the sealing and barrier properties of the joint. Moreover, in this cup-shaped container, the joint does not protrude outward, improving the appearance and making it easier to hold. Furthermore, in this cup-shaped container, a protective coating is formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate-side heat-sealable resin layer in the heat-sealable resin layer constituting the inner surface of the folded joint and the outer surface of the body overlapping it, so that both end surfaces of the body blank are more reliably covered with the protective coating.

[0022] According to the cup-shaped containers of 4) to 7) above, the above effects achieved by the cup-shaped containers of 1) to 4) above are more reliably achieved. [Brief description of the drawings]

[0023] [Figure 1] 1 is a perspective view of a cup-shaped container according to a first embodiment of the present invention. [Diagram 2] This is a vertical cross-sectional view taken along line II-II in FIG. 1, in which the portion surrounded by dashed dotted line A is an enlarged view of the portion surrounded by dashed dotted line a, and the portion surrounded by dashed dotted line B is an enlarged view of the portion surrounded by dashed dotted line b. [Diagram 3] (a) is an enlarged cross-sectional view showing the layer structure of a laminate used as the material for the body blank, and (b) is an enlarged cross-sectional view showing the layer structure of a laminate used as the material for the bottom body blank, showing an embodiment in which each heat-sealable resin layer has a two-layer structure. [Figure 4] (a) is an enlarged cross-sectional view showing the layer structure of a laminate used as the material for the body blank, and (b) is an enlarged cross-sectional view showing the layer structure of a laminate used as the material for the bottom body blank, showing an embodiment in which each heat-sealable resin layer has a three-layer structure. [Diagram 5] FIG. 2 is an enlarged horizontal cross-sectional view showing one embodiment of an overlapping portion of a body of the above-mentioned cup-shaped container. [Figure 6]4 is an enlarged horizontal cross-sectional view showing another embodiment of the overlap portion of the body of the cup-shaped container. FIG. [Figure 7] FIG. 2(a) is a plan view of a fuselage blank, and FIG. 2(b) is a perspective view of a fuselage formed from the fuselage blank. [Figure 8] 1A is a plan view of a bottom body blank, and FIG. 1B is a perspective view of a bottom body formed from the bottom body blank. [Figure 9] 5A to 5C are vertical cross-sectional views showing a part of the manufacturing process of the cup-shaped container. [Figure 10] FIG. 4 is a horizontal cross-sectional view of a cup-shaped container according to a second embodiment of the present invention. [Figure 11] 11 is an enlarged horizontal cross-sectional view showing a portion surrounded by a dashed dotted line c in FIG. 10. [Figure 12] 5A to 5C are horizontal cross-sectional views showing a part of a manufacturing process for the body of the cup-shaped container. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention will be described with reference to FIGS. In the following explanation, "upper and lower" refers to the upper and lower sides of the cup-shaped container, body, and bottom body (e.g., the upper and lower sides in Figures 2 and 9), "inner" refers to the side closer to the center of the cup-shaped container, body, and bottom body (e.g., the bottom in Figures 5 and 6, the right in Figure 9, and the top in Figure 11), and "outer" refers to the side farther from the center of the cup-shaped container, body, and bottom body (e.g., the top in Figures 5 and 6, the left in Figure 9, and the bottom in Figure 11).

[0025] <First embodiment> Figures 1 and 2 show the overall structure of a cup-shaped container (1) according to a first embodiment of the present invention. The container (1) is formed by joining together a body (2) formed from a body blank (20A) and a bottom body (3) formed from a bottom body blank (30A). The body (2) is a tapered cylinder, and is formed by overlapping and joining both end edges of a sector-shaped body blank (20A) as shown in Fig. 7. Therefore, the body (2) has an overlapping portion (21) that extends along its height direction. The body (2) has a folded-back portion (22) folded inward at the edge of the lower opening. The body 2 has an outwardly bent flange 23 at the upper opening edge. The flange 23 is folded downward and formed into a substantially horizontal flat shape. The flange may have a shape other than that shown in the figure, for example, it may be curled downward and formed into a substantially arc-shaped cross section. The bottom body (3) has a generally inverted U-shaped cross section, with a circular, horizontal bottom portion (31) and a hanging portion (32) extending downward from the outer peripheral edge of the bottom portion (31), and is formed by drawing a circular bottom body blank (30A) as shown in Figure 8. The outer surface of the hanging portion (32) of the bottom body (3) is joined to the inner surface of the lower end portion (2a) of the body (2), and the folded portion (22) of the body (2) is joined to the inner surface of the hanging portion (32), thereby integrating the body (2) and the bottom body (3) (see Figures 2 and 9). Although not shown in the figures, the body (2) and the bottom body (3) can be integrated by a connecting structure in which the outer surface of the hanging portion (32) of the bottom body (3) is joined to the inner surface of the lower end (2a) of the body (2) without forming a folded portion (22) at the edge of the lower end opening of the body (2). With this configuration, even if some wrinkles are generated in the hanging portion (32) when the bottom body (3) is molded, the lower end (2a) of the body (2) and the hanging portion (32) of the bottom body (3) can be reliably sealed without mixing in air or the like.

[0026] As shown in Figures 3(a) and 4(a), the body blank (20A) is formed from a laminate (20) consisting of a metal foil layer (201), an inner heat-sealable resin layer (202) laminated on one of both sides of the metal foil layer (201) that will be on the inside of the body (2), and an outer heat-sealable resin layer (203) laminated on one of both sides of the metal foil layer (201) that will be on the outside of the body (2), and does not have a paper layer. As shown in Fig. 3(b) and Fig. 4(b), the bottom body blank (30A) is also formed of a laminate (30) consisting of a metal foil layer (301), an upper heat-sealable resin layer (302) laminated on one of both sides of the metal foil layer (301) that will be the upper side of the bottom body (3), and a lower heat-sealable resin layer (303) laminated on one of both sides of the metal foil layer (301) that will be the lower side of the bottom body (3), and does not have a paper layer. Note that if the folded portion (22) is not formed at the edge of the lower end opening of the body (2) and a connection structure is formed in which the outer surface of the hanging portion (32) of the bottom body (3) is only joined to the inner surface of the lower end (2a) of the body (2), the lower heat-sealable resin layer (303) of the bottom body blank (30A) can be omitted. The thickness of each laminate (20)(30) is preferably less than 250 μm, and more preferably less than 200 μm. By setting the thickness of each laminate (20)(30) within the above range, as in the case of a paper cup using a laminate with a thickness of about 250 to 400 μm as the blank material, the step of the part of the flange part (23) of the body (2) formed by the overlap part (21) becomes too large, and the lower end part (2a) and the folded part (22) of the body (2) and the hanging part of the bottom body (3) become too large. (32) This reliably avoids problems such as unstable bonding with the

[0027] The metal foil layers (201) (301) function as a barrier layer to protect the contents from gas, water vapor, light, etc. The metal foil constituting the metal foil layer (201) (301) may be aluminum foil, iron foil, stainless steel foil, copper foil, etc., but aluminum foil is preferably used. In the case of aluminum foil, either pure aluminum foil or aluminum alloy foil may be used, and either soft or hard. For example, annealed soft material (O material) of A8000 series (particularly A8079H or A8021H) classified by JIS H4160 is preferably used because it has excellent formability. In addition, when a hard material (H material) is used as the aluminum foil constituting the metal foil layer (201) (particularly the metal foil layer (201) of the body blank (20A)), the strength of the flange portion (23) is increased, deformation of the flange portion (23) due to unexpected impact is suppressed, and the shape retention of the cup-shaped container (1) as a whole is improved. Both sides of the metal foil layers (201) and (301) are subjected to a base treatment such as a chemical conversion treatment, if necessary. Specifically, for example, the surface of the metal foil that has been degreased is 1) Phosphoric acid, Chromic acid, and at least one compound selected from the group consisting of metal salts of fluorides and nonmetal salts of fluorides. 2) phosphoric acid; At least one resin selected from the group consisting of acrylic resins, chitosan derivative resins, and phenolic resins; and at least one compound selected from the group consisting of chromic acid and chromium (III) salts. 3) phosphoric acid, At least one resin selected from the group consisting of acrylic resins, chitosan derivative resins, and phenolic resins; At least one compound selected from the group consisting of chromic acid and chromium (III) salts; and at least one compound selected from the group consisting of metal salts of fluorides and nonmetal salts of fluorides. A coating is formed by applying an aqueous solution of any one of the above 1) to 3) and then drying the applied solution to perform a chemical conversion treatment. The coating formed on the surface of the metal foil layer (201) (301) by the above chemical conversion treatment has a chromium deposition amount (per side) of 0.1 mg / m 2 ~50mg / m 2 It is preferable to use a concentration of 2 mg / m 2 ~20mg / m 2 It is preferable to set the above. The thickness of the metal foil layer (201)(301) is preferably 40 to 200 μm, more preferably 80 to 160 μm. By setting the thickness of the metal foil layer (201)(301) within the above range, sufficient barrier properties and moldability can be obtained.

[0028] The heat-sealable resin layers (202), (203), (302), (303) constitute the inner and outer surfaces of the container (1), and serve to protect the metal foil layers (201), (301) and to impart formability to the laminates (20), (30). They also function as heat-sealing layers when joining both end edges of the body blank (20A) and when joining the lower end (2a) and folded portion (22) of the body (2) to the hanging portion (32) of the bottom body (3). The heat-sealable resin layers (202)(203)(302)(303) are usually made of a general-purpose film having heat-sealability, such as a polypropylene (PP) film or a polyethylene (PE) film, or a composite film made by bonding these together, but a non-oriented polypropylene film (CPP), which has excellent heat resistance and draw formability, is particularly suitable. The heat-sealable resin layers (202)(203)(302)(303) may be formed of a coating layer of maleic acid-modified polyethylene, maleic acid-modified polypropylene, ethylene-vinyl acetate, an epoxy resin, a shellac resin, or the like, instead of the above-mentioned films. The thickness of the heat-sealable resin layers (202), (203), (302), (303) is preferably 5 to 80 μm, and more preferably 10 to 60 μm. By setting the thickness of the heat-sealable resin layers (202), (203), (302), (303) within the above range, sufficient adhesive strength can be obtained at the joint between both end edges of the body blank (20A) and at the joint between the lower end (2a) and the folded-back portion (22) of the body (2) and the hanging portion (32) of the bottom body (3), and the step formed by the overlap portion (21) on the upper surface of the flange portion (23) of the body (2) can be made gentle, resulting in good sealing performance when sealed with a lid.

[0029] The metal foil constituting the metal foil layer (201) (301) and the film constituting the heat-fusible resin layer (202) (203) (302) (303) are laminated, for example, by a dry lamination method via an adhesive layer (not shown). For the adhesive layer, for example, a two-component curing polyester-polyurethane adhesive or a polyether-polyurethane adhesive is used. Due to the presence of the adhesive layer, even if the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) are reduced in thickness due to heat fusion, for example, in the overlapping portion (21) of the body (2), the metal foil layers (201) are prevented from coming into contact with each other, so that the sealing performance is maintained. Furthermore, with the adhesive layer, even if contents that permeate the heat-sealable resin layers (202), (203), (302), (303) are filled, it is possible to prevent the metal foil layers (201), (301) from corroding and causing the contents to leak out.

[0030] The laminate (20) constituting the body blank (20A) and the laminate (30) constituting the bottom blank (30A) are usually the same, but may be made of different materials and / or thicknesses.

[0031] Next, an example of a method for forming the cup-shaped container 1 using the laminates 20 and 30 will be described. First, the laminate (20) is punched into a sector shape of a predetermined size to form a body blank (20A) (see FIG. 7(a)). The laminate (30) is punched out into a circle of a specified size to form a bottom body blank (30A) (see FIG. 8(a)), and this blank (30A) is drawn using a mold (not shown) to form a bottom body (3) having a generally inverted U-shaped cross section and consisting of a bottom portion (31) and a hanging portion (32) (see FIG. 8(b)). The resulting bottom body (3) is free of wrinkles. The corners between the bottom portion (31) and the hanging portion (32) on the outer surface of the bottom body (3) are rounded. The bottom body (3) is set on the top surface of a generally truncated cone mold (not shown) so that the upper surface of the bottom part (31) overlaps, and the body blank (20A) is wrapped around the outer periphery of the mold so that both end edges overlap, and then the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) which form the overlapping surfaces of the overlapping part (21) are heat-sealed to form the tapered cylindrical body (2) (see FIG. 7(b)). The means for heat-sealing the overlapping part (21) may be heat sealing using a hot plate, high-frequency sealing, ultrasonic sealing, or the like. Here, when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) are made of a non-oriented polypropylene film (CPP), the heat sealing is preferably performed under the conditions of a sealing temperature of 160 to 220°C, a load of 80 to 200 kgf, and a sealing time of 1 to 5 seconds. When the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) are made of a polyethylene film (PE), the heat sealing is preferably performed under the conditions of a sealing temperature of 140 to 220°C, a load of 80 to 200 kgf, and a sealing time of 1 to 5 seconds. In other words, in the case of heat sealing, it is preferable to heat both ends of the overlapped body blank (20A) at a temperature 20 to 40°C higher than the melting point of the resin constituting the heat-sealable resin layers (202) and (203) from both sides. Moreover, the high frequency sealing is preferably performed under the conditions of, for example, output: 0.5 to 1.5 kW, sealing time: 3 to 5 seconds, distance from the coil: 0.5 to 15 mm, and load: 100 to 200 kgf. 9, the lower opening edge of the body (2) is folded inward, and the folded portion (22) is pressed against the hanging portion (32) of the bottom body (3) by a disk-shaped rotating die (not shown), and then the inner heat-sealable resin layer (202), the upper heat-sealable resin layer (302), and the lower heat-sealable resin layer (303), which constitute the overlapping surfaces of the lower end (2a) and folded portion (22) of the body (2) and the hanging portion (32) of the bottom body (3), are heat-sealed to join the body (2) and the bottom body (3) together. The heat-sealing of these heat-sealable resin layers (202), (302), and (303) is usually performed by heat sealing using a hot plate or the like, but may also be performed by high-frequency sealing, ultrasonic sealing, or the like. The suitable conditions for heat sealing and high frequency sealing are the same as those for heat fusing the overlapping portion (21) of the body (2). In addition, the upper opening edge of the body (2) is curled outward using a specified curl forming die (not shown) and pressed vertically to form a flat shape, thereby forming a flange portion (23) (see Figure 9). In this way, the cup-shaped container (1) shown in Figures 1 and 2 is obtained.

[0032] In the cup-shaped container (1) of this embodiment, first, the body blank (20A) has the following characteristics: At least one (preferably both) of the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) is made of two or more layers. As shown in FIG. 3(a), when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) each have a two-layer structure, in each layer (202) (203), the heat-sealable resin constituting the laminate side heat-sealable resin layer (202b) (203b) laminated on the metal foil layer (201) has a lower melting point than the heat-sealable resin constituting the seal side heat-sealable resin layer (202a) (203a) constituting the inner or outer surface of the body (2). Furthermore, as shown in FIG. 4(a), when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) each have a three-layer structure, in each layer (202) (203), the heat-sealable resin constituting the laminate-side heat-sealable resin layer (202b) (203b) laminated on the metal foil layer (201) has a lower melting point than the heat-sealable resin constituting the seal-side heat-sealable resin layer (202a) (203a) constituting the inner or outer surface of the body (2) and the heat-sealable resin constituting the intermediate heat-sealable resin layer (202c) (203c) interposed between the laminate-side heat-sealable resin layer (202b) (203b) and the seal-side heat-sealable resin layer (202a) (203a). Similarly, as shown in Figure 3(b), the bottom body blank (30A) can have a two-layer structure with an upper heat-sealable resin layer (302) and a lower heat-sealable resin layer (303), and in each layer (302) (303), the heat-sealable resin constituting the laminate side heat-sealable resin layer (302b) (303b) laminated on the metal foil layer (301) can have a lower melting point than the heat-sealable resin constituting the seal side heat-sealable resin layer (302a) (303a) located on the surface side of the bottom body (3). Alternatively, as shown in FIG. 4(b), the upper heat-sealable resin layer (302) and the lower heat-sealable resin layer (303) can each have a three-layer structure, and in each layer (302) (303), the heat-sealable resin constituting the laminate side heat-sealable resin layer (302b) (303b) laminated on the metal foil layer (301) can have a lower melting point than the heat-sealable resin constituting the seal side heat-sealable resin layer (302a) (303a) located on the surface side of the bottom body (3) and the heat-sealable resin constituting the intermediate heat-sealable resin layer (302c) (303c) interposed between the laminate side heat-sealable resin layer (302b) (303b) and the seal side heat-sealable resin layer (302a) (303a).

[0033] The melting point of the heat-sealable resin constituting the laminate side heat-sealable resin layer (202b), (203b), (302b), (303b) is preferably at least 10°C lower, more preferably at least 20°C lower, than the melting point of the heat-sealable resin constituting the seal side heat-sealable resin layer (202a), (203a), (302a), (303a) (and the intermediate heat-sealable resin layer (202c), (203c), (302c), (303c)). Note that the difference in melting points specified here is, in a heat-sealable resin layer consisting of three or more layers, the difference between the melting point of the heat-sealable resin constituting the laminate side heat-sealable resin layer and the lowest melting point of the heat-sealable resin constituting the other two or more heat-sealable resin layers. More specifically, the melting point of the heat-fusible resin constituting the laminate side heat-fusible resin layers (202b), (203b), (302b), (303b) is preferably 110 to 140°C, and more preferably 120 to 135°C. In addition, when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) or the upper heat-sealable resin layer (302) and the lower heat-sealable resin layer (303) of the bottom blank (30A) have a two-layer structure, the melting point of the heat-sealable resin constituting the seal side heat-sealable resin layer (202a) (203a) (302a) (303a) is preferably 150 to 165°C, and more preferably 155 to 160°C. Furthermore, in the case where the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) and the upper heat-sealable resin layer (302) and the lower heat-sealable resin layer (303) of the bottom blank (30A) have a three-layer structure, the melting point of the heat-sealable resin constituting the seal side heat-sealable resin layer (202a), (203a), (302a), (303a) is preferably 110 to 140°C, more preferably 120 to 135°C, and the melting point of the heat-sealable resin layer constituting the intermediate heat-sealable resin layer (202c), (203c), (302c), (303c) is preferably 150 to 165°C, more preferably 155 to 160°C.

[0034] In addition to the above-mentioned melting point difference, the melt mass flow rate (MFR) of the heat-fusible resin constituting the laminate side heat-fusible resin layer (202b), (203b), (302b), (303b) is preferably larger than the melt mass flow rate (MFR) of the heat-fusible resin constituting the seal side heat-fusible resin layer (202a), (203a), (302a), (303a) (and the intermediate heat-fusible resin layer (202c), (203c), (302c), (303c)), more preferably by 1 to 5 g / 10 min or more, and even more preferably by 2 to 4 g / 10 min or more. The difference in melt mass flow rate (MFR) specified here is, in a heat-sealable resin layer consisting of three or more layers, the difference between the MFR of the heat-sealable resin constituting the laminate-side heat-sealable resin layer and the largest MFR among the MFRs of the heat-sealable resins constituting the other two or more heat-sealable resin layers. Here, the melt mass flow rate (MFR) refers to a value determined in accordance with the standard test method for MFR specified in JIS K7210-1-2014. For example, when each heat-sealable resin layer is made of polypropylene, the MFR is a value measured in accordance with the above test method under conditions of a temperature of 230°C and a load of 2.16 kgf. More specifically, the MFR of the heat-fusible resin constituting the laminate side heat-fusible resin layers (202b), (203b), (302b), (303b) is preferably 4 to 10 g / 10 min, and more preferably 5 to 8 g / 10 min. In addition, when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) or the upper heat-sealable resin layer (302) and the lower heat-sealable resin layer (303) of the bottom blank (30A) have a two-layer structure, the MFR of the heat-sealable resin constituting the seal side heat-sealable resin layer (202a), (203a), (302a), (303a) is preferably 4 to 10 g / 10 min, and more preferably 5 to 8 g / 10 min. Furthermore, in the case where the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) of the body blank (20A) and the upper heat-sealable resin layer (302) and the lower heat-sealable resin layer (303) of the bottom blank (30A) have a three-layer structure, the MFR of the heat-sealable resin constituting the seal side heat-sealable resin layer (202a), (203a), (302a), (303a) is preferably 4 to 10 g / 10 min, more preferably 5 to 8 g / 10 min, and the MFR of the heat-sealable resin layer constituting the intermediate heat-sealable resin layer (202c), (203c), (302c), (303c) is preferably 2 to 5 g / 10 min, more preferably 3 to 4 g / 10 min.

[0035] In the cup-shaped container (1) of this embodiment, the overlap portion (21) of the body (2) has the following structural features. That is, as shown in FIG. 5, the metal foil layer (201) portion of the inner end surface (204) of the body blank (20A) located on the inside of the body (2) and the interface portion between the metal foil layer (201) and the heat-sealable resin layers (202) (203) are covered with a protective coating (M1) formed by melting and solidifying the heat-sealable resin constituting the laminate side heat-sealable resin layers (202b) (203b) when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203), which form the overlapping surfaces of both end edges of the body blank (20A), are heat-sealed. In the case of the overlap portion (21) of the body (2) in the embodiment shown in FIG. 6, in addition to covering the inner end surface (204) with the protective coating (M1), the metal foil layer (201) portion of the outer end surface (205) of the body blank (20A) located on the outside of the body (2) and the interface portion between the metal foil layer (201) and the heat-sealable resin layers (202) and (203) are covered with a protective coating (M2) formed by melting and solidifying the heat-sealable resin constituting the laminate-side heat-sealable resin layers (202b) and (203b) when the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203), which constitute the overlapping surfaces of both end edges of the body blank (20A), are heat-sealed.

[0036] In the overlap portion (21) of the body (2) of the cup-shaped container (1), the total thickness (T1) of the inner heat-sealable resin layer (202) and the outer heat-sealable resin layer (203) heat-sealed to each other at both end edges of the body blank (20A) is preferably 8 to 150 μm, more preferably 16 to 80 μm (see FIG. 5). If the total thickness (T1) is less than 8 μm, the sealing property of the overlap portion (21) may be insufficient. On the other hand, if the total thickness (T1) exceeds 150 μm, the barrier property of the overlap portion (21) may be impaired. In the overlapping portion (21) of the body (2), the overlapping width (W1) between the metal foil layers (201) (201) at both ends of the body blank (20A) as viewed in the thickness direction is preferably 2 to 10 mm, more preferably 4 to 8 mm. If the overlapping width (W1) is less than 2 mm, the barrier properties of the overlapping portion (21) may be impaired, and the seal width may be too small, resulting in insufficient sealability. On the other hand, if the overlapping width (W1) exceeds 10 mm, the width of the overlapping portion (21) becomes larger than necessary, leading to increased costs, and furthermore, due to the difference in stress applied to the inner portion (one end edge of the body blank (20A)) and the outer portion (the other end edge of the body blank (20A)) of the overlapping portion (21), there is a risk of wrinkles or other defects in appearance occurring in the inner portion of the overlapping portion (21).

[0037] The cup-shaped container (1) of this embodiment provides the following advantages. a) The body blank (20A) and the bottom blank (30A) are each formed from a laminate (20) (30) consisting of a metal foil layer (201) (301) and heat-sealable resin layers (202) (203) (302) (303) laminated on both sides thereof, and therefore can be produced inexpensively using paper cup production equipment. b) The laminates (20) (30) from which the blanks (20A) (30A) are made have metal foil layers (201) (301), so that the contents can be stored for a long time. c) Since the thickness of the body blank (20A) is smaller than that of a paper cup, the step on the upper surface of the flange portion (23) of the body (2) formed by the overlap portion (21) can be made smaller, and therefore poor sealing is less likely to occur when sealing the lid to the upper surface of the flange portion (23) of the container (1). Also, when performing aseptic (sterile) filling, sterilizing liquid is less likely to remain in the step on the upper surface of the flange portion (23). d) Since the bottom body (3) is formed by drawing the bottom body blank (30A), wrinkles do not occur in the bottom body (3). Therefore, there is no risk of poor bonding between the hanging portion (32) of the bottom body (3) and the lower end portion (2a) and the folded portion (22) of the body (2) or of reduced barrier properties, as occurs with conventional paper cups. e) Since the thickness of the body blank (20A) and the bottom blank (30A) is smaller than that of a paper cup, the lower end (2a) and the folded portion (22) of the body (2) can be stably joined to the hanging portion (32) of the bottom body (3). f) Compared to a paper cup, the radius of curvature (R) of the corner portion between the bottom portion (31) and the hanging portion (32) on the outer surface of the base body (3) can be made smaller, so that when performing aseptic filling, sterilizing liquid is less likely to remain at the boundary between the upper surface of the bottom body (3) and the inner surface of the body (2) of the cup-shaped container (1). g) Since the laminates 20, 30 from which the blanks 20A, 30A are made do not have a paper layer, retort sterilization can be carried out without any problems. h) In the overlap portion (21) of the body (2), the metal foil layer (201) portion of the inner end surface (204) of the body blank (20A) located on the inside of the body (2) and the interface portion between the metal foil layer (201) and the heat-sealable resin layers (202), (203) are covered with a protective coating (M1) formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate-side heat-sealable resin layers (202b), (203b) of the heat-sealable resin layers (202), (203) of the multilayer structure of the body blank (20A) during heat fusion, and are not exposed to the contents, so that deterioration due to delamination and corrosion of the inner end surface (204) is effectively suppressed, and this is also preferable from a hygienic standpoint. In particular, since the protective coating (M1) is made of a modified polyolefin that has excellent adhesive strength with the metal foil layer (202), it is believed that the above-mentioned effects will last for a long period of time. i) In the overlap portion (21) of the body (2), the metal foil layer (201) portion of the outer end surface (205) of the body blank (20A) located on the outside of the body (2) and the interface portion between the metal foil layer (201) and the heat-sealable resin layers (202), (203) are covered with a protective coating (M2) formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate-side heat-sealable resin layers (202b), (203b) of the heat-sealable resin layers (202), (203) of the multilayer structure of the body blank (20A) during heat fusion, so that deterioration of the outer end surface (205) due to delamination and corrosion is effectively suppressed for a long period of time.

[0038] Although not shown in the figure, the metal foil layer (301) and the interface between the metal foil layer (301) and the heat-sealable resin layer (302) (303) on the end surface of the bottom body blank (30A), i.e., the lower end surface of the hanging portion (32) of the bottom body (3), may be covered with a protective coating formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate side heat-sealable resin layer (302b) (303b) (202b) when the heat-sealable resin layers (302) (303) (202) constituting the overlapping surfaces of the hanging portion (32) of the bottom body (3) and the lower end portion (2a) and the folded-back portion (22) of the body (2) are heat-sealed to each other. This effectively suppresses deterioration due to delamination and corrosion on the lower end surface of the hanging portion (32) of the bottom body (3). In addition, in the upper and lower end edge surfaces of the body blank (20A), i.e., the tip surface of the flange portion (23) of the body (2) and the tip surface of the folded portion (22) of the body (2) (if the body (2) does not have the folded portion (22), the lower end surface of the body (2)), the same as described above, for example, when a lid material is heat-sealed to the flange portion (23) of the body (2) or when the lower end portion (2a) and the folded portion (22) of the body (2) hang down relative to the bottom body (3). When the end portion (32) is heat-sealed to the end portion (33), the end portion (32) may be covered with a protective coating formed by melting and solidifying the low-melting point heat-sealable resin constituting the laminate-side heat-sealable resin layers (202b), (203b), (302b), and (303b) of the multilayered heat-sealable resin layers (202), (203), (302), and (303), thereby effectively suppressing deterioration due to delamination and corrosion of each of the end faces.

[0039] <Second embodiment> Figures 10 to 12 show a cup-shaped container according to a second embodiment of the present invention. The cup-shaped container of this embodiment is substantially the same as the cup-shaped container of the first embodiment shown in Figures 1 to 9, except for the following points. That is, as shown in Figures 10 and 11, in the cup-shaped container 1X of this embodiment, the body 2 is formed into a cylindrical shape by overlapping and joining both end edges of a body blank 20A in a palm-to-palm shape (see Figure 12(a)). More specifically, both end edges of the body blank 20A overlapped in a palm-to-palm shape are joined by thermally fusing their inner heat-fusible resin layers 202 together. Also, the joint portion (21X) of the body (2) is bent to one side so as to overlap with the outer surface of the body (2) and is heat-sealed to the outer surface (see FIG. 12(b)). The width (overlap) of the joint portion (21X) of the body (2) is preferably 5 to 20 mm, and more preferably 10 to 18 mm. If the width is less than 5 mm, sealing the joint portion (21X) may be difficult. On the other hand, if the width exceeds 20 mm, the width of the joint portion (21X) becomes larger than necessary, leading to increased costs. Furthermore, when the joint portion (21X) is folded to one side so as to overlap with the outer surface of the body (2) and joined to the outer surface, wrinkles or other defects in appearance may occur in the joint portion (21X). According to the above-mentioned cup-shaped container (1X), the two end faces of the body blank (20A) at the joint (21X) of the body (2) do not come into contact with the contents contained in the container (1X), thereby suppressing the occurrence of delamination, corrosion, etc. Furthermore, according to the container (1X), the surfaces that come into contact with the contents can be made of one type of resin, which makes sterilization easy and is advantageous in terms of hygiene. In addition, according to the above cup-shaped container (1X), the joint portion (21X) of the body (2) is bent to one side and heat-sealed to the outer surface of the body (2), improving the sealing and barrier properties of the same part. Moreover, according to the cup-shaped container (1X), the joint portion (21X) does not protrude outward, improving the appearance and making it easier to hold.

[0040] As shown in detail in FIG. 11, when the metal foil layer (201) of both end faces (206) of the body blank (20A) located on the outside of the body (2) and the interface between the metal foil layer (201) and the heat-sealable resin layers (202) and (203) of the multi-layered inner heat-sealable resin layers (202) at both end edges of the body blank (20A) are heat-sealed to each other, and further, when the joint portion (21X) of the body (2) is moved to one side so as to overlap the outer surface of the body (2), When the blank (20A) is folded and heat-sealed to its outer surface, i.e., when the inner surface of the folded joint (21X) and the overlapping outer surface of the body (2) are heat-sealed to each other, the laminate side heat-sealable resin layers (202b) and (203b) of the layers (202) and (203) are covered with a protective coating (M3) formed by melting and solidifying the low-melting-point heat-sealable resin constituting the laminate side heat-sealable resin layers (202b) and (203b) of the layers (202) and (203). This protective coating (M3) effectively prevents the deterioration of both end surfaces (206) of the body blank (20A) due to delamination and corrosion for a long period of time.

[0041] In manufacturing the above-mentioned cup-shaped container (1X), the step of forming the body (2) is carried out, for example, as follows. That is, both end edge portions of the body blank (20A) are overlapped in a palm-to-palm manner, and the inner heat-sealable resin layers (202) constituting the overlapping surfaces are joined together by a first heat fusion to form a cylindrical body (2) having a palm-to-palm portion (21X). The first heat fusion is usually performed by heat sealing using a hot plate or the like, but may also be performed by high-frequency sealing, ultrasonic sealing, or the like. Next, the joint portion (21X) is folded to one side and placed on the outer surface of the body (2), and in this state, a second heat fusion is performed by high frequency sealing. As a result, the inner heat fusion resin layers (202) constituting the overlapping surfaces of both end edges of the body blank (20A) are further heat fused to each other, and at the same time, the inner surface of the folded joint portion (21X) and the outer heat fusion resin layers (203) constituting the overlapping outer surface of the body (2) are heat fused to each other, and the joint portion (21X) is joined to the outer surface of the body (2). By the above-described two-stage heat sealing, both end edges of the body blank (20A) are more reliably joined together, the heat sealing makes it easier for the protective coating (M3) to be formed at the joint, and furthermore, deformation and the like due to the heat sealing are suppressed. EXAMPLES

[0042] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.

[0043] <Example 1> A two-component curing urethane adhesive was applied at approximately 3 g / m2 to both sides of a 100 μm thick aluminum foil (A8021H-O) that had been chemically treated. 2 The adhesive was applied to a 40 μm thick non-oriented polypropylene film (CPP) and dry laminated. A laminate was obtained by carrying out a predetermined aging treatment to harden the adhesive. Here, a co-extruded film consisting of a 12 μm thick ethylene-propylene random copolymer layer (melting point = 130 ° C) and a 28 μm thick homopolypropylene (rPP) layer (melting point = 160 ° C) was used as the non-oriented polypropylene film, and the surface of the ethylene-propylene random copolymer layer of the film was bonded to the aluminum foil. Next, the obtained laminate was punched into a predetermined shape to form a body blank and a bottom blank (see Figs. 7 and 8). Then, using the body blank and the bottom blank, a cup-shaped container shown in FIGS. 1 and 2 was produced by the same process as in the above-described embodiment, and this was designated as Example 1. The resulting cup-shaped container is made of aluminum foil with a thickness of 100 μm, and therefore has excellent barrier properties with almost no permeation of oxygen or water vapor. The dimensions of the cup-shaped container were as follows: -Inner diameter of the opening at the top of the cup-shaped container: 65mm -Inner diameter of the bottom of the cup-shaped container: 50mm Flange width: 4mm Height of cup: 95mm Height of the cup-shaped container's legs (folded part (22)): 6 mm -Width of fuselage overlap (overlap): 8mm In addition, when the overlapping portion of the body of the cup-shaped container was cut transversely and the cut surface was observed under a microscope, it was confirmed that the inner end surface of the body blank was covered with a protective coating of ethylene-propylene random copolymer formed during heat sealing, and that the outer end surface of the body blank was covered with a protective coating of ethylene-propylene random copolymer formed during heat sealing.

[0044] <Example 2> Using the same body blank and bottom blank as in Example 1, a cup-shaped container as shown in FIGS. 12 and 13 was produced by the same process as in the second embodiment described above. This was used as Example 2. The dimensions of the cup-shaped container of Example 2 were the same as those of Example 1, except that the width (overlapping area) of the joint portion of the body was 15 mm. When the joint of the body of the cup-shaped container was cut transversely and the cut surface was observed under a microscope, it was confirmed that both end surfaces of the body blank were covered with a protective coating of ethylene-propylene random copolymer formed during heat fusion. [Industrial Applicability]

[0045] The present invention can be suitably used as a cup-shaped container for holding, for example, liquid food or beverage. [Explanation of symbols]

[0046] (1)(1X): Cup-shaped container (2): Torso (2a): Lower end of the fuselage (21): Overlap section (21X): Gassho part (23): Flange (20A): Body blank (20): Laminate (201): Metal foil layer (202): Inner heat-sealable resin layer (202a): Heat-sealing resin layer on the sealing side (202b): Laminate side heat-sealable resin layer (203):Outer heat-fusible resin layer (203a): Heat-sealing resin layer on the sealing side (203b): Laminate side heat-sealable resin layer (204): Inner end face (of the body blank) (205): Outer end face (of the fuselage blank) (206): Both end faces (of the fuselage blank) (3): Bottom body (31):Bottom (32): Drooping part (30A): Bottom blank (30): Laminate (301):Metal foil layer (302): Upper heat-sealable resin layer (303): Lower heat-fusible resin layer (M1):Protective coating (M2):Protective coating (M3):Protective coating

Claims

1. A cup-shaped container comprising a body formed into a cylindrical shape by overlapping and joining both end edges of a body blank, and a bottom body having a generally inverted U-shaped cross section formed by forming a bottom body blank so as to form a bottom and a hanging part extending downward from the outer peripheral edge of the bottom body, the body and the bottom body being integrated by joining the outer surface of the hanging part of the bottom body to the inner surface of the lower end of the body, the body blank is formed from a laminate consisting of a metal foil layer and heat-sealable resin layers laminated on both sides of the metal foil layer, and both end edges of the body blank are joined by heat-sealing the heat-sealable resin layers constituting the mutually overlapping surfaces of the metal foil layer, The bottom body blank is formed from a laminate consisting of a metal foil layer and a heat-sealable resin layer laminated on at least one of both sides of the metal foil layer that will be the upper side of the bottom body, and the inner surface of the lower end of the body and the outer surface of the hanging part of the bottom body are joined by heat-sealing the heat-sealable resin layers that make up these surfaces, At least one of the two heat-fusible resin layers of the body blank is composed of two or more layers, and the melting point of the heat-fusible resin constituting the laminate-side heat-fusible resin layer laminated on the metal foil layer among the two or more layers is 10°C or more lower than the melting point of the heat-fusible resin constituting the other layer and is 110 to 140°C; A cup-shaped container in which, in the overlapping portion of the body, a metal foil layer portion on the inner end face of a body blank located on the inside of the body and an interface portion between the metal foil layer and a heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the heat-sealable resin constituting the laminate side heat-sealable resin layer when the heat-sealable resin layers at both end edges of the body blank are heat-sealed to each other.

2. The cup-shaped container of claim 1, further comprising: a metal foil layer portion on the outer end face of the body blank located on the outside of the body, and an interface portion between the metal foil layer and the heat-sealable resin layer, the metal foil layer being covered with a protective coating formed by melting and solidifying the heat-sealable resin constituting the laminate side heat-sealable resin layer when the heat-sealable resin layers at both end edges of the body blank are heat-sealed to each other.

3. A cup-shaped container comprising a body formed into a cylindrical shape by overlapping and joining both end edges of a body blank in a palm-to-palm shape, and a bottom body having a generally inverted U-shaped cross section formed by forming a bottom body blank so as to form a bottom and a hanging part extending downward from the outer peripheral edge of the bottom body, the body and bottom body being integrated by joining the outer surface of the hanging part of the bottom body to the inner surface of the lower end of the body, the body blank is formed from a laminate consisting of a metal foil layer and heat-sealable resin layers laminated on both sides of the metal foil layer, and both end edges of the body blank are joined by heat-sealing the heat-sealable resin layers constituting the mutually overlapping surfaces of the metal foil layer, The bottom body blank is formed from a laminate consisting of a metal foil layer and a heat-sealable resin layer laminated on at least one of both sides of the metal foil layer that will be the upper side of the bottom body, and the inner surface of the lower end of the body and the outer surface of the hanging part of the bottom body are joined by heat-sealing the heat-sealable resin layers that make up these surfaces, the heat-fusible resin layer of the body blank is composed of two or more layers, and the melting point of the heat-fusible resin constituting the laminate side heat-fusible resin layer laminated on the metal foil layer among the two or more layers is lower by 10°C or more than the melting points of the heat-fusible resins constituting the other layers and is 110 to 140°C; A cup-shaped container in which, at the joint portion of the body, the metal foil layer portions on both end faces of the body blank located on the outside of the body and the interface portions between the metal foil layer and the heat-sealable resin layer are covered with a protective coating formed by melting and solidifying the heat-sealable resin constituting the laminate side heat-sealable resin layer when the heat-sealable resin layers on both end edges of the body blank are heat-sealed to each other.

4. 4. The cup-shaped container according to claim 3, wherein the joint portion of the body is folded to one side so as to overlap the outer surface of the body and is heat-sealed to said outer surface.

5. The cup-shaped container according to any one of claims 1 to 4, wherein the melt mass flow rate (MFR) of the heat-fusible resin constituting the laminate-side heat-fusible resin layer is 1 to 5 g / 10 min or more higher than the melt mass flow rate (MFR) of the heat-fusible resin constituting the other layer.

6. 6. The cup-shaped container according to claim 5, wherein the melt mass flow rate (MFR) of the heat-fusible resin constituting the laminate side heat-fusible resin layer is 4 to 10 g / 10 min.

Citation Information

Patent Citations

  • JP1977008579U

  • Method of sealing up cylindrical container

    JP1979040774A

  • Vessel with sealing cover

    JP1983030955A

  • Manufacture of paper can drum

    JP1985046233A

  • Paper cup

    JP2006256643A