Method and apparatus for controlling thickness of protective film on substrate

The controlled deposition of a protective film on recess sidewalls using precursor gases and plasma modification addresses sidewall bowing and maintains opening dimensions in high aspect ratio etching, improving etching quality and memory cell durability in semiconductor manufacturing.

JP7573501B2Active Publication Date: 2024-10-25TOKYO ELECTRON LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021138491
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-28
Filing Date
2021-08-27
Publication Date
2024-10-25
Estimated Expiration
2041-08-27

AI Technical Summary

Technical Problem

Conventional etching processes face challenges in forming high aspect ratio recesses due to sidewall bowing and mask pattern opening blockage, particularly in advanced semiconductor manufacturing, where uniform protective film thickness is difficult to achieve, leading to non-uniform hole sizes and reduced durability of memory cells.

Method used

A method involving controlled deposition of a protective film on the sidewalls of recesses using a combination of precursor gases and plasma modification, including silicon-containing precursors and oxygen-containing radicals, with fluorine-containing gases to inhibit film formation at mask openings, ensuring a controlled thickness distribution that suppresses sidewall bowing and maintains opening dimensions.

Benefits of technology

The method effectively prevents sidewall bowing and maintains opening dimensions by gradually reducing the protective film thickness, enhancing etching quality and memory cell durability by suppressing lateral etching and expanding the recess diameter while controlling film thickness distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573501000002
    Figure 0007573501000002
  • Figure 0007573501000003
    Figure 0007573501000003
  • Figure 0007573501000004
    Figure 0007573501000004
Patent Text Reader

Abstract

To provide a method and device for protecting, by a protection film, a side wall of a concave portion as a part of an etching process to form a concave portion of a high aspect ratio.SOLUTION: The method comprises: an exposure step of exposing a substrate to a precursor to arrange particles of the precursor at least on a side wall of a concave portion of an etching layer in a reaction chamber; a supply step of supplying an inhibition gas and a quality-modification gas into the reaction chamber to generate plasma; and a modification step of modifying, in quality, the precursor particles on the side wall into a protection film while supplying the inhibition gas and quality-modification gas into the reaction chamber.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to etching substrates, and more particularly to a method and apparatus for protecting the sidewalls of high aspect ratio recesses with a protective film as part of an etching process to form the recesses. [Background technology]

[0002] New technologies have improved the way semiconductors are made, resulting in smaller and smaller integrated circuits (ICs, microelectronic circuits, microchips, or simply "chips") and the geometries of the components on an IC. Miniature active and passive semiconductor devices and interconnects are fabricated on a semiconductor substrate (e.g., silicon). In forming such ICs, the substrate is subjected to processes such as doping, ion implantation, etching, thin film deposition of various materials, and photolithographic patterning. The individual microcircuits are finally diced apart and packaged as individual ICs.

[0003] Processes typically used to form ICs on a substrate include atomic layer deposition (ALD), chemical vapor deposition (CVD), atomic layer etching (ALE), etc. In conventional processes, etching conditions may be changed depending on the depth of the pattern to be formed. For example, in conventional processes, chamber pressure, radio frequency (RF) power, and flow ratios of process gases are changed depending on the depth of the pattern to be formed.

[0004] In conventional etching processes, problems include sidewall bowing and other shape deterioration caused by lateral etching (or lateral etching). Conventionally, a protective film is formed on the sidewall of an etched recess using processes such as ALD and CVD. If the protective film is formed to a uniform thickness sufficient to suppress lateral etching, the opening dimensions of the mask pattern will be reduced and the opening will be blocked. Alternatively, if a protective film (with an upper part thicker than a lower part) is formed by subconformal ALD processing in an area of ​​the recess that is easily etched laterally, the opening dimensions of the mask pattern will be reduced and the opening will be blocked.

[0005] Plasma etching is used to form recesses in a substrate. In plasma etching, it is required to suppress the lateral expansion of the recesses. For this reason, a technique is used to form a film on the sidewall surfaces that define the recesses. Such a technique is described, for example, in the following Patent Documents 1 and 2. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] US Patent Application Publication No. 2016 / 0343580 [Patent Document 2] US Patent Application Publication No. 2018 / 0174858 Summary of the Invention [Means for solving the problem]

[0007] According to one embodiment, a method for forming a film on a substrate including an etching layer and a mask formed on the etching layer is provided, the method including: (a) exposing the substrate to a precursor in a reaction chamber to dispose precursor particles on at least a sidewall of a recess in the etching layer, (b) supplying an inhibiting gas and a modifying gas to the reaction chamber to generate a plasma, and (c) modifying the precursor particles on the sidewall into a protective film while supplying the inhibiting gas and the modifying gas to the reaction chamber.

[0008] The above paragraphs are intended to be general and are not intended to limit the scope of the appended claims. The embodiments and advantages described herein will be best understood by reference to the following detailed description when considered in conjunction with the accompanying drawings, in which: [Brief description of the drawings]

[0009] The present disclosure and many of the attendant advantages will be readily appreciated as the same becomes better understood by reference to the following detailed description, when taken in conjunction with the accompanying drawings, in which: [Figure 1] FIG. 13 shows bowing occurring on the sidewall of an etched recess. [Diagram 2] 1 illustrates an example of a substrate processing system according to the present disclosure. [Diagram 3] FIG. 1 illustrates an example of an etching device of a substrate processing system. [Figure 4] FIG. 1 is a block diagram illustrating an example of a processing circuit for performing operations according to the present disclosure on a computer. [Diagram 5] 1 is a flowchart of an example of an etching method. [Figure 6A] FIG. 1 illustrates a recess etched using a sub-conformal ALD protective film according to one embodiment of the present disclosure. [Figure 6B] FIG. 1 illustrates a recess etched using a sub-conformal ALD protective film according to one embodiment of the present disclosure. [Figure 6C]FIG. 1 illustrates a recess etched using a sub-conformal ALD protective film according to one embodiment of the present disclosure. [Figure 7A] 10 is a timing chart of an example of forming a protective film. [Figure 7B] 10 is a timing chart of an example of forming a protective film. [Figure 7C] 10 is a timing chart of an example of forming a protective film. [Figure 8] 11A and 11B are diagrams showing the effect of an embodiment of the present disclosure on the thickness of a protective film at an opening in a mask. [Figure 9A] 13 is a diagram showing another embodiment of the present disclosure in which a protective film is also formed on the bottom surface of the recess in the etching layer. FIG. [Figure 9B] 13 is a diagram showing another embodiment of the present disclosure in which a protective film is also formed on the bottom surface of the recess in the etching layer. FIG. [Figure 9C] 13 is a diagram showing another embodiment of the present disclosure in which a protective film is also formed on the bottom surface of the recess in the etching layer. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The following description, in conjunction with the accompanying drawings, describes various embodiments of the subject matter of the present disclosure, and is not necessarily limited to the described embodiments. In the examples, specific details are described for the purpose of facilitating understanding of the subject matter of the present disclosure. However, it is clear to those skilled in the art that each embodiment can be practiced without such specific details. In some examples, well-known structures and components may be shown in block diagram form to avoid obscuring the concept of the subject matter of the present disclosure.

[0011] Throughout this specification, "one embodiment" or "embodiment" means that a particular feature, structure, characteristic, operation, or function described with respect to an embodiment is included in at least one embodiment of the presently disclosed subject matter. Thus, the phrases "in one embodiment" or "in an embodiment" used herein do not necessarily refer to the same embodiment. Moreover, the particular features, structures, characteristics, operations, or functions may be combined in any suitable manner in one or more embodiments. Furthermore, embodiments of the presently disclosed subject matter may include modifications and variations of the described embodiments.

[0012] In this specification and the appended claims, the singular forms "a" and "the" include the plural, unless expressly stated otherwise. That is, in this specification, terms such as "a" mean "one or more" unless expressly indicated otherwise. Furthermore, terms such as "left", "right", "top", "bottom", "front", "rear", "side", "height", "length", "width", "upper", "lower", "internal", "external", "inside", "outside", and the like, are used herein merely to indicate reference points and do not necessarily limit embodiments of the subject matter of the present disclosure to a particular orientation or configuration. Furthermore, terms such as "first", "second", "third", and the like, are used herein merely to specify the number of parts, components, reference points, actions, and / or functions, etc., described herein and do not necessarily limit embodiments of the subject matter of the present disclosure to a particular configuration or orientation.

[0013] Throughout this disclosure, "recess" is used as a type of etched feature, and the two terms ("recess" and "etched feature") are interchangeable herein. Furthermore, the term "recess" is not limiting and may refer to holes, slits, grooves, recessed cavities, or other types of patterns where material has been removed in the substrate material being etched.

[0014] The inventors have recognized that performing high aspect ratio (HAR) etching while suppressing the "bowing" phenomenon on the sidewalls of recesses becomes increasingly difficult as the dimensions of the stack increase. For example, in 3D-NAND, alternating layers, often alternating SiO and SiN layers, form the stack. The stack somewhat resembles a skyscraper with many floors, each with many memory cells. Deep etching is required to define the channels between the cells, and ideally the etch is performed so that the hole dimensions are uniform for all layers in the stack. If the etch is not performed properly, the uniformity of a particular hole will be lacking, resulting in a variety of shapes, including bowing, as shown in region 140 of stack 100 in FIG. 1. Bowing is the result of over-etching the sidewalls, especially in the upper portion of etch layer 120. Bowing can also result from ion scattering from the edge of a mask that has been exposed to etching for a long time and has a dropped shoulder. In high aspect ratio etching, ions travel in a very straight line, but some ions bounce off the rounded edge of the mask and are sent to the sidewalls of region 140. Furthermore, as shown in FIG. 1, a mask (amorphous carbon layer) 130 is placed on the etching layer 120 formed on the substrate 110. The rounded angle of the resist mask causes over-etching of the upper part of the sidewalls of the etching layer 120, thus causing bowing of the critical dimension (CD) of the recess, resulting in non-uniformity of the opening dimension along the entire depth of the hole. Such bowing should be avoided to maintain the durability and performance of the memory cell. CD means the diameter of the recess in this specification, but can also include the space CD of the line and space structure (trench) of the recess.

[0015] In conventional devices, a recess is formed in a substrate by repeating a deposition and etching process. In this process, the substrate is first etched. During the etching process, a fluorine-containing gas is typically used. In this application, the fluorine-containing gas is, for example, a C-type fluorine gas such as CF4, C4F6, or C4F8. x F yIt may be a gas, such as NF3 or SF6, but the fluorine-containing gas may also be another gas that contains fluorine.

[0016] After the substrate etching is stopped, a protective film is formed on the sidewall of the recess. The precursor is adsorbed and modified several times to form a protective film of the desired thickness. A precursor with a low adhesion coefficient is used to allow the protective film to penetrate to the depth of the recess. A chemical reactant such as malonyl chloride or ethylenediamine may be used to form the protective film. After the protective film is deposited, etching continues, and the cycle is repeated until the recess is completed. In this application, the precursor may include, for example, aminosilane or other silicon (Si)-containing components. For convenience, Si is exemplified as a precursor component throughout this specification, but it should be understood that precursor components other than or in addition to Si can be used as viable precursor components to be adsorbed to the substrate surface, such as the sidewall. Furthermore, the present teachings are not limited to Si as the only precursor component.

[0017] The present inventors have recognized that conventional substrate processing techniques have some limitations. In conventional substrate etching techniques, film deposition and etching steps are repeated until a recess is completed in the substrate. In addition, in conventional ALD and subconformal ALD processes, if a film deposition step is performed to suppress bowing of the sidewall, the film thickness in the upper region of the recess increases, and the opening dimensions of the mask pattern may be reduced (e.g., the opening may be blocked).

[0018] To address these limitations of the prior art, the present inventors have developed an apparatus and process for controlling (regulating) the deposition amount (thickness distribution of the protective film) in recesses during ALD processing and non-saturated (subconformal) ALD processing. By controlling (regulating) the deposition amount, the thickness of the protective film in the opening of the mask is reduced compared to other parts of the recess of the etch layer. Thus, the opening of the mask is not blocked during or after the deposition of the protective film.

[0019] The present inventors have recognized and developed a process for controlling the amount of deposition within a feature. In one embodiment, the control process is accomplished by a series of steps that begin with adsorbing a first gas (also referred to as a precursor) onto a surface of a substrate. The precursor, which may be a silicon (Si)-containing gas, is supplied to a reaction chamber in which the substrate is disposed. In particular, a precursor component of the first gas, e.g., Si, a component of the silicon-containing gas, adsorbs onto the surface of the substrate. The first gas may be supplied for a first period of time.

[0020] After the adsorption of the precursor, a modifying gas (also called a reactant gas) is further introduced. The modifying gas may be supplied to the recess. This modifying gas (e.g., O * A gas containing oxygen (such as oxygen radicals) is supplied to the reaction chamber. A plasma is generated from the modifying gas and the adsorbed precursor is exposed to the plasma to induce a surface reaction and form a protective film on the sidewall of the recess. The oxygen containing gas may be, but is not limited to, O2, CO, CO2, or O3. Additionally, the modifying gas may be, but is not limited to, a nitrogen containing gas such as NH3, N2, or NF3.

[0021] Alternatively, in the case of subconformal ALD, the precursor is adsorbed only on a portion of the substrate surface. Then, a modifying gas is introduced to form a film only on the portion where the precursor is adsorbed. Specifically, for example, the precursor can be supplied for a relatively short time, and the pressure and flow rate can be lower than the standard processing time. The supply of the precursor and the modifying gas constitutes the first cycle of a hybrid gas supply cycle. By supplying the modifying gas, a protective film can be formed on the sidewall of the recess, while the bottom of the recess can be partially etched. A silicon-containing gas is used as the precursor, and O is used as the modifying gas. * When radicals are used, a SiO2 protective film is formed on the sidewalls of the recesses.

[0022] The inventors have recognized that by supplying an inhibitor, such as a fluorine-containing gas, during the modification of the ALD (and subconformal ALD) process, the amount of film deposition in the opening of the mask can be reduced and the blockage of the opening can be suppressed. In particular, fluorine from the fluorine-containing gas adheres to the periphery of the mask opening and prevents adsorption of the precursor in the next iteration of the process. Thus, by gradually reducing the thickness of the protective film along the sidewall of the recess, the amount of film deposition in the opening of the mask can be reduced and the blockage of the opening can be suppressed.

[0023] While the embodiments of the present disclosure provide many benefits, the inventors have recognized several advantages of the embodiments of the present disclosure. One advantage is that it is possible to form a thinner protective film on the mask while forming a protective film with a controlled thickness on the sidewalls. The protective film on the sidewalls may be gradually reduced in thickness as the sidewalls of the recess become deeper. The etching quality is improved because the reduction in the size of the mask opening is suppressed and the thickness distribution of the protective film is controlled. The protective film can be purposefully formed to be relatively thick where lateral etching occurs and relatively thin where lateral etching is not an issue. Furthermore, it is possible to overetch the bottom of the recess while suppressing bowing in the upper portion of the recess.

[0024] 2 illustrates an example of a substrate processing system 200 according to the present disclosure. The substrate processing system 200 includes a transfer apparatus 240 (operating at a reduced pressure relative to the etchers 252, 254, 256, 258) including a transfer robot 242 for transferring substrates W to and from etchers 252, 254, 256, 258. The transfer apparatus 240 has a vacuum transfer chamber coupled to the load lock chambers 232 and 234. The etchers 252, 254, 256, 258 are connected to the transfer apparatus 240 and separated from the load lock chambers 232 and 234.

[0025] The load lock chambers 232 and 234 can compartmentalize the environment between the transfer apparatus 240 and the loader apparatus 220. The loader apparatus 220 has a carrier placement stage on which a carrier is placed. The carrier holds, for example, 25 substrates W, and is disposed in front of the loader apparatus 220 when the carrier is inserted into or removed from the substrate processing system 200. The loader robot 222 transfers substrates between the carrier placement stage and the load lock chambers 232 and 234. The carriers are exchanged at the respective load ports 212 to 218.

[0026] The controller 260 is a microcontroller in this example, although a computer (either a local dedicated computer or a distributed computer) and / or processing circuitry as described in FIG. 4 may be used in place of the controller circuitry configured with computer code to perform the control operations described herein.

[0027] FIG. 3 shows a schematic diagram of an etching apparatus 300 (e.g., a capacitively coupled plasma (CCP) plasma system) coupled to a transfer apparatus via a gate valve. Although a CCP system is shown as an example, any other etching apparatus may be used, such as an inductively coupled plasma (ICP) plasma processing apparatus. The etching apparatus 300 is substantially cylindrical and includes a reaction chamber 310 made of, for example, aluminum. The reaction chamber 310 is connected to a ground potential. A plasma-resistant film is formed on the inner wall surface of the reaction chamber 310, and this film may be a film formed by anodization or a ceramic film such as a film made of yttrium oxide. When RF power is supplied to at least one of the upper electrode 330 and the base 320 (which functions as a lower electrode for generating plasma in the reaction chamber 310) with a substrate W to be processed being placed between them, a plasma 312 is generated between the upper electrode 330 and the base 320. The plasma 312 is formed adjacent to the substrate W, and the substrate W is held on the upper surface of an electrostatic chuck 322 (described in detail below). The base 320 is substantially disc-shaped and electrically conductive.

[0028] The gas source 360 ​​includes multiple gas sources, each controlled through a corresponding set of flow controls, and supplies gases to the reaction chamber 310 through one or more gas lines.

[0029] The etching apparatus 300 further includes a first RF power source 340 that generates RF energy in the range of 27 MHz to 100 MHz, with an exemplary frequency of 60 MHz. The first RF power source 340 is connected to the upper electrode 330 via a matching circuit that matches the output impedance of the first RF power source 340 with the impedance of the upper electrode 330.

[0030] The etching apparatus 300 further includes a second RF power supply 350 that generates RF energy for bias purposes to attract ions to the substrate W. The operating frequency of the second RF power supply 350 is lower than the operating frequency of the first RF power supply 340, typically in the range of 400 kHz to 13.56 MHz. In an alternative embodiment, multiple RF power supplies 340 and 350 may be coupled to the same electrode (base 320).

[0031] The upper electrode 330 has a second power supply which is a variable direct current (DC) power supply 380. The variable DC power supply 380 can also act as a DC bias for the RF energy applied to the upper electrode from the first RF power supply 340. The variability of the variable DC power supply 380 allows for operational control of the ion energy so that the etch rate can be controlled depending on the process being performed.

[0032] The RF energy generated by the second RF power supply 350 may be pulsed. When bias power is supplied to the base / lower electrode, etching is mainly performed. When bias power is not supplied to the base / lower electrode, film deposition is mainly performed. By pulsing the bias, it is possible to separate the etching stage from the film deposition stage. Etching is performed after the protective film is formed to protect the sidewall of the recess from lateral etching. In addition, the balance between etching and film deposition can be controlled by changing the duty ratio of the pulse (bias-on time / (bias-on time+bias-off time)). The longer the bias-off time, the thicker the protective film can be formed, and the higher the protection effect can be obtained. The longer the bias-on time, the higher the etching rate.

[0033] In one embodiment, the etching apparatus 300 may have a dedicated control circuit (e.g., a processing circuit as shown in FIG. 4) that operates separately from or in cooperation with the control unit 260 (FIG. 2). The control unit 260 executes a control program stored in a memory and controls each component of the etching apparatus 300 based on recipe data stored in a storage device.

[0034] The etching apparatus 300 includes an exhaust system 370 connected to the internal atmosphere of the reaction chamber 310. The exhaust system 370 includes a pressure control unit, such as an automatic pressure control valve, and a vacuum pump (e.g., a turbomolecular pump), to controllably reduce the pressure in the reaction chamber 310 and exhaust gases from the reaction chamber 310.

[0035] FIG. 4 is a block diagram of a processing circuit that performs the operations described herein on a computer. FIG. 4 shows an example of a processing circuit 400 that controls all the control operations, statements, or blocks of the flowchart on a computer and on a cloud. These control operations, statements, or blocks represent portions of code that include one or more executable instructions for performing a particular logical function or step of a module, segment, or process. Those skilled in the art will understand that alternative implementations are included within the scope of the exemplary embodiments of the present disclosure, and that functions may be performed in a different order than that shown or described, such as substantially simultaneously or in reverse order, depending on the functionality involved. The various elements, features, and processes described herein may be used independently of each other or combined in various ways. All possible combinations and subcombinations are included within the scope of the present disclosure.

[0036] In FIG. 4, the processing circuit 400 includes a CPU 401 that performs one or more control processes described above / below. Processing data and instructions can be stored in a memory 402. These processing data and instructions can be stored in a storage medium disk 404, such as a hard disk drive (HDD) or a portable storage medium, or can be stored remotely. Furthermore, the present disclosure as described in the claims is not limited by the form of a computer-readable recording medium on which the instructions of the processes according to the present invention are stored. For example, these instructions can be stored in a CD, DVD, flash memory, RAM, ROM, PROM, EPROM, EEPROM, hard disk, or any other information processing device, such as a server or computer with which the processing circuit 400 communicates. Furthermore, each process can be stored in a storage device on a network, a storage device on a cloud, or other remotely accessible storage device, and can be executed by the processing circuit 400.

[0037] Additionally, the present disclosure as claimed may be provided as a utility application, a background daemon, a component of an operating system, or any combination thereof, and may execute in conjunction with a CPU 401 and an operating system known to those skilled in the art, such as Microsoft Windows, UNIX, Solaris, LINUX, Apple MAC-OS, etc.

[0038] The hardware elements constituting the processing circuit 400 can be realized by various circuit elements. Furthermore, each function of the above-mentioned embodiments can be implemented by a circuit including one or more processing circuits. As shown in Fig. 4, the processing circuit includes a programmed specific processor, for example, processor (CPU) 401. The processing circuit also includes devices such as application specific integrated circuits (ASICs) or conventional circuit components configured to implement the described functions.

[0039] In FIG. 4, the processing circuit 400 includes a CPU 401 that performs the above-mentioned processes. The processing circuit 400 may be a general-purpose computer or a specific dedicated machine. In one embodiment, the processing circuit 400 controls the voltage and the robot arm to replace the ESC in situ without exposing the reaction chamber 310 to the outside atmosphere. When the processor 401 is programmed to replace the ESC in situ, the processing circuit 400 functions as a specific dedicated machine. The processing circuit 400 may be included in the substrate processing system 200 or may be able to communicate locally. In an embodiment, the processing circuit 400 may be remote from the substrate processing system 200 and provide processing instructions to the substrate processing system 200 via a network 428.

[0040] Alternatively or additionally, CPU 401 may be implemented on an FPGA, ASIC, PLD, or may use discrete logic circuitry, as will be appreciated by those skilled in the art. Further, CPU 401 may be implemented as multiple processing units cooperating to perform in parallel the instructions of the processes of the present invention described above.

[0041] The processing circuitry 400 of FIG. 4 also includes a network controller 406 for interfacing with a network 428, such as an Intel Ethernet PRO network interface card from Intel Corporation, USA. As can be appreciated, the network 428 can be a public network, such as the Internet, a private network, such as a LAN or WAN, or any combination thereof, and can include subordinate networks, such as PSTN or ISDN. The network 428 can also be wired, such as an Ethernet network, or wireless, such as a cellular network, including EDGE, 3G, and 4G wireless cellular systems. The wireless network can also be Wi-Fi, Bluetooth, or any other known form of wireless communication.

[0042] The processing circuit 400 further includes a display device controller 408, such as a graphics card or graphics adapter, for interfacing with a display device 410, such as a monitor. A general purpose I / O interface 412 interfaces with a keyboard and / or mouse 414 and a touch panel 416, which may be integral with or separate from the display device 410. The general purpose I / O interface is also connected to various peripheral devices 418, such as printers and scanners.

[0043] The general purpose storage controller 424 is connected to the storage media disk 404 via a communication bus 426, such as ISA, EISA, VESA, PCI, etc., and all components of the processing circuit 400 are connected to each other. The display device 410, keyboard and / or mouse 414, as well as the general features and functions of the display device controller 408, the general purpose storage controller 424, the network controller 406, and the general purpose I / O interface 412 are not described herein for the sake of brevity, as they are well known.

[0044] The exemplary circuit elements described in this disclosure may be substituted with other elements and may have different structures than the examples described herein. Additionally, circuits configured to implement the features described herein may be implemented in multiple circuit units (e.g., chips) or may combine these features as circuits in a single chipset.

[0045] The functions and features described herein may also be performed by various components distributed on the system. For example, one or more processors may perform these functions, in which case the processors are distributed across multiple components communicating over a network. Distributed components may include various human interface and communication devices (e.g., display monitors, smartphones, tablets, personal digital assistants (PDAs), etc.), as well as one or more client and server machines that can share processing. The network may be a private network such as a LAN or WAN, or a public network such as the Internet. Input to the system may be received by direct input by a user, or may be received remotely as a real-time or batch process. Furthermore, some of the implementations may be implemented on modules or hardware that are not identical to those described above. Thus, other implementations are within the scope of the claims.

[0046] Figure 5 is a flow chart of an exemplary etching method according to the present disclosure, which will be described with reference to Figures 6A-6C, which show a recess etched using a sub-conformal ALD protective film.

[0047] The etching method begins at step 510 with providing a substrate having an etch layer 610 and a mask layer 620 disposed on the etch layer 610. The substrate having the etch layer 610 and the mask layer 620 may be the substrate W described with respect to Figures 2 and 3. For example, the processing circuitry 400 may control the transport device 240 to transport the substrate W to the etching system.

[0048] In step 520, the processing circuitry 400 controls the etching system to partially etch the etching layer to form a recess in the etching layer 610 through the opening 630. The etching in this step may use a plasma or other etching gases as described above with respect to the plasma 312. Any known etching method may be used in step 520. A plasma is generated from the etching gas and ions are extracted from the plasma by providing an electrical bias to the substrate.

[0049] In step 530, the processing circuit 400 controls the etching device 300 to form a protective film 640 on the sidewall of the recess in the etching layer 610. To form the protective film 640, first, precursor particles are adsorbed on the sidewall surface of the recess in the etching layer 610. The precursor adsorption may be performed with or without generating a plasma of the precursor gas. The precursor particles are then exposed to a modifying gas to form the protective film 640.

[0050] The protective film 640 may be formed by a conventional ALD-type process or a sub-conformal ALD process, which is described below with respect to Figures 9A-9C.

[0051] Two aspects of subconformal ALD processing are presented below.

[0052] (1) The precursor may be adsorbed over the entire surface of the substrate. The surface of the substrate includes the surface of the recess (the sidewall and bottom of the etched recess). After the precursor is adsorbed, the modifying gas is controlled to be supplied for a relatively short period of time. By controlling the supply of the modifying gas in this manner, for example, O generated from the modifying gas can be prevented from being generated. * Radicals are less likely to reach the lower part or bottom of the recess, and as a result, O * The number of radicals decreases.

[0053] (2) The precursor is adsorbed only on a portion of the surface of the substrate, and then a modifying gas is introduced to form a film only on the portion of the surface where the precursor is adsorbed. For example, the precursor may be supplied for a relatively short period of time, and the pressure and precursor flow rate may be reduced.

[0054] In forming the protective film 640, precursors are supplied to the reaction chamber and the precursors are adsorbed on the sidewalls of the recesses. After the precursors are adsorbed on the recesses, a modifying gas (such as O2 gas) and an inhibiting gas are supplied to the reaction chamber. The precursor particles disposed on the substrate combine with the modifying gas supplied to the reaction chamber. In one exemplary implementation, silicon-containing precursor particles from a silicon-containing precursor gas are disposed on the sidewalls, and then O2 gas from the modifying gas is supplied to the reaction chamber. * By combining with the radicals and oxidizing the silicon-containing precursor particles on the sidewalls, SiO x A protective layer is formed. This process may be repeated until the thickness of the protective layer is controlled.

[0055] In some embodiments, the inhibitor gas and the modifying gas are provided during the modification stage of step 530, but not during the adsorption stage of step 530. In other embodiments, the inhibitor gas and the modifying gas are provided continuously throughout step 530. When the inhibitor gas is a fluorine-containing gas, fluorine species from the fluorine-containing gas will adhere to the periphery of the mask opening and prevent adsorption of the precursor in the next iteration of the process. Thus, by gradually reducing the thickness of the protective film along the sidewall of the recess, the amount of film deposited at the mask opening can be reduced, and the opening can be prevented from being blocked.

[0056] In some embodiments, an electrical bias may be applied to the substrate during step 530. The electrical bias may be less than the electrical bias during the etching steps 520 and 540. Further details regarding the adsorption, modification, and purging steps of step 530, and the formation of the protective film 640, are described below with respect to Figures 7A-7C.

[0057] In step 530, a plasma is generated from the modifying gas using the method having the above-mentioned steps (1) or (2), and the adsorbed precursor is exposed to the plasma to cause a surface reaction, forming a protective film 640 with a thickness that gradually decreases downward on the sidewalls of the recesses in the etching layer 610. By supplying a fluorine-based inhibitor gas and a modifying gas during the adsorption and / or modification steps, adsorption of the precursor in the mask openings is prevented.

[0058] The sequence (cycle) of forming the protective film 640 in step 530 is repeated until a predetermined, controllable film thickness is obtained. Thus, the opening dimensions of the recess are maintained because there is a protective film on the sidewalls that protects the sidewalls from bowing, which is a problem associated with conventional etching processes.

[0059] After forming protective layer 640, the process proceeds to step 540 where the substrate is further etched as in step 520.

[0060] In step 550, the process circuitry 400 determines whether an additional protective film 640 needs to be formed to further protect the sidewalls before performing the subsequent etching step. The process circuitry 400 determines whether the additional protective film 640 is needed based on an analysis (e.g., transmission or scanning electron microscopy, TEM or SEM) of several prototype substrates that have been processed according to the method. Once the number of cycles that results in a given film thickness is identified, the process is recorded in a process recipe. The process recipe is used to program the process circuitry 400 to control the deposition / etch steps for processing substrates in subsequent process batches.

[0061] If there is an insufficient amount of protective film 640 remaining on the sidewalls to protect them during the subsequent etching step (YES at step 550), the process returns to step 530 to form additional protective film on the sidewalls. On the other hand, if at step 550 it is determined that there is enough protective film to protect the sidewalls during further etching to the final depth (NO at step 550), the process proceeds to step 560 to continue etching until the final depth is reached.

[0062] The determination in step 550 may be made by processing circuitry 400 in accordance with a process in which processing circuitry 400 determines whether additional repeated etching processes are necessary based on whether a predetermined etching time has elapsed. To that end, processing circuitry 400 may record the cumulative etching time over which the etching processes are repeated in step 540 and compare the cumulative etching time to the predetermined etching time. Thus, processing circuitry 400 recording the cumulative etching time can determine whether additional etching processes can be performed without further replenishing the protective film on the sidewalls of the recesses.

[0063] The process is completed by further etching the substrate etch layer 610 to a final depth in step 560. Thus, steps 530, 540, and 550 may be repeated a predetermined number of times, and the determination in step 550 may be based on the number of iterations performed under the same process conditions as in the manufacture of the prototype substrate.

[0064] In one exemplary implementation, the processing circuitry 400 controls at least steps 520 through 560 to be performed in the reaction chamber 310. In another implementation, the processing circuitry 400 controls to form the protective film 640 in one reaction chamber and to perform the etching in another reaction chamber.

[0065] In yet another implementation, the processing circuitry controls an initial etch in a first reaction chamber and a further repeated etch in a second reaction chamber, and the formation of the protective film may be performed in the first reaction chamber, the second reaction chamber, or a third reaction chamber.

[0066] In an exemplary implementation of the present disclosure, after performing the process shown in Figure 5, the critical dimension (CD) of the vertical center region of the sidewall after the protective film is formed is smaller than the CD of the upper part of the sidewall. Furthermore, the thickness of the protective film formed on the upper part of the recess is smaller than the maximum thickness of the protective film formed on the sidewall of the recess of the etching layer.

[0067] In another exemplary implementation of the present disclosure, after performing the process shown in FIG. 5, a different type of inhibiting gas may be used to reduce the amount of CD deposition on the lower or central portions of the sidewalls of the feature. x F y The gas species may be varied to reduce deposition on the lower portion of the sidewalls or in the center of the etched recess.

[0068] Figures 6A to 6C show a substrate that has been subjected to the process shown in Figure 5. In particular, Figure 6A shows a recess in an etching layer 610, which has been partially etched through an opening 630 in a masking layer 620.

[0069] 6B shows the formation of a protective film 640 on the sidewall of the recess in the etching layer 610. The protective film 640 is formed by (1) adsorbing precursor particles on the sidewall surface of the recess in the etching layer 610, (2) purging the gas in the reaction chamber, (3) converting the precursor into a protective film by supplying a modifying gas and an inhibiting gas, and (4) purging the gas in the reaction chamber again. The adsorption of the precursor particles may be performed with or without generating a plasma of the precursor gas. The purging step of the gas in the reaction chamber may be optional.

[0070] Figure 6C shows a recess in the etch layer 610 by further partial etching through the opening 630 in the mask layer 620. Due to the presence of the protective film 640, the recess in Figure 6C has been etched less laterally and does not exhibit a bowing shape.

[0071] As described with respect to FIG. 5, the formation of the protective film 640 and further etching of the substrate may be repeated until a final depth for the recess in the etching layer 610 is obtained.

[0072] The material of the etching layer 610 is not limited. For example, the etching layer 610 can be a silicon-containing film, SiO x Examples of silicon-containing dielectric films include SiO x and SiN alternately laminated (ONON laminate), and SiO x and polysilicon alternately laminated (OPOP laminate). The etching layer 610 may further include an organic film. The aspect ratio of the recess may be 10 to 20 or more, or 30 or more.

[0073] The following table shows examples of combinations of materials for the etching layer, mask, and etching gas. [Table 1]

[0074] However, the materials of the etching layer, mask, and main etching gas are not limited.

[0075] In another exemplary implementation of the present disclosure, during the formation of the protective film 640, the etching layer 610, such as an organic film, may be etched by plasma generated from an oxygen-containing gas.

[0076] 7A to 7C show a timing chart of an example of the formation of a protective film.

[0077] FIG. 7A is a first timing diagram of supplying precursor to the substrate before supplying RF power, fluorine-containing gas, and oxygen-containing gas. In particular, the precursor is adsorbed on the substrate surface during the adsorption period A. When the adsorption period is completed, the supply of the precursor is terminated, and the fluorine-containing gas and oxygen-containing gas are supplied during the modification period M. In particular, during the modification period M (step 530), a protective film is formed by the surface reaction of the precursor layer with the plasma of the modification gas, and an inhibitor is formed at the top edge of the pattern (near the mask opening) by a gaseous inhibitor such as the fluorine-containing plasma of the fluorine-containing gas. Therefore, in the subsequent cycle, the precursor is less likely to be adsorbed at the top edge of the pattern (near the mask opening), and as a result, the formation of the protective film at the top edge of the pattern is reduced.

[0078] The RF supply is synchronized with the supply of the oxygen-containing gas and the fluorine-containing gas. After the completion of the reforming period, a new adsorption period A may be started. The adsorption and reforming periods may be alternated multiple times.

[0079] Purging of the interior of the chamber may be performed between adsorption and reforming and / or after reforming.

[0080] In some embodiments, RF may be provided during both the adsorption and reforming periods depending on the type of precursor used during the adsorption step.

[0081] 7B shows a second timing diagram for continuously supplying fluorine-containing gas and oxygen-containing gas during both the adsorption period and the modification period. In particular, fluorine-containing gas and oxygen-containing gas are supplied from the beginning of the adsorption period to adsorb the precursor on the surface of the substrate. The fluorine-containing gas and oxygen-containing gas are continuously supplied during the adsorption period and then continuously supplied during the modification period during which RF is supplied. The adsorption period and the modification period may be alternated multiple times, with the fluorine-containing gas and oxygen-containing gas being continuously supplied during the adsorption period and the modification period.

[0082] In another exemplary implementation, a fluorine-containing gas or an oxygen-containing gas may be intermittently supplied while RF is being supplied.

[0083] Purging of the interior of the chamber may be performed between adsorption and reforming and / or after reforming.

[0084] 7C shows a third timing diagram of an example of a process in which purging is performed between the adsorption period and the reforming period, and after the reforming period. In this example process, the reaction chamber can be held at a chamber pressure of 10 mTorr during the formation of the protective film. This chamber pressure is an example, and the chamber pressure can be held at other static or dynamic pressures.

[0085] As shown in Figure 7C, the precursor is delivered at the beginning of the adsorption period. In this exemplary process, the precursor may be aminosilane and is delivered at 20 sccm with a 2 second adsorption period. However, the precursor may be other material combinations and delivered at different flow rates. Additionally, the length of the adsorption period may vary.

[0086] At the beginning of the adsorption period, a fluorine-containing gas and an oxygen-containing gas are also supplied. The fluorine-containing gas and the oxygen-containing gas are supplied continuously. In this exemplary process, the fluorine-containing gas (e.g., CF4) is supplied continuously at 100 sccm, and the oxygen-containing gas (O2 gas) is supplied continuously at 300 sccm. However, other forms of fluorine-containing gas and oxygen-containing gas may be supplied at different flow rates.

[0087] After the adsorption period is completed, a first purge period is performed to purge the fluorine-containing gas and oxygen-containing gas from the reaction chamber. In this exemplary process, the first purge period has a length of 1.5 seconds. However, the length of the first purge period may vary. The supply of the fluorine-containing gas and oxygen-containing gas may be continued throughout the first purge period. Alternatively, the supply of the fluorine-containing gas and oxygen-containing gas may be paused at the beginning of the first purge period and resumed at the end of the first purge period.

[0088] After completion of the first purge period, a reforming period is performed during which RF power is supplied. The fluorine-containing gas and the oxygen-containing gas are supplied continuously throughout the reforming period. In this exemplary process, the reforming period is 1 second in length. However, the length of the reforming period may vary. In this exemplary process, RF power may be supplied as a 60 MHz continuous wave or a 20 kHz pulsed wave. However, other RF power values, waveform styles, and frequencies may be used.

[0089] After the reforming period is completed, a second purge period is performed to purge the fluorine-containing gas and oxygen-containing gas in the reaction chamber. In this exemplary process, the second purge period has a length of 1 second. However, the length of the second purge period may vary. The supply of the fluorine-containing gas and oxygen-containing gas may be continued throughout the second purge period. Alternatively, the supply of the fluorine-containing gas and oxygen-containing gas may be paused at the beginning of the second purge period and resumed at the end of the second purge period.

[0090] After the second purge period is completed, the cycle may be restarted with the next adsorption period. The cycle of this exemplary process may be performed until the thickness of the protective film is controlled. As an example, the cycle of adsorption / first purge / modification / second purge may be performed 50 times to control the thickness of the protective film.

[0091] FIG. 8 illustrates the effect of embodiments of the present disclosure on sidewall CD at mask openings. In particular, FIG. 8 illustrates the feature depth Z (in μm, measured from the mask surface to the bottom of the feature, with the mask opening being zero) versus the feature CD (in nm). FIG. 8 further illustrates data for an etched substrate ("initial"), a reference substrate using a conventional sub-conformal ALD process ("reference"), and a substrate using a sub-conformal ALD process according to the present disclosure in which CF4 is continuously supplied throughout the formation of the protective film ("w / CF4").

[0092] As shown in FIG. 8, the sidewall CD changes at a different rate closer to the mask opening (closer to zero depth) when a subconformal ALD process is applied.

[0093] The initial substrate is a substrate in a state after etching with a fluorocarbon gas or the like and before subconformal ALD film formation is performed.

[0094] For the reference substrate, the CD decreases from the middle to the upper part of the sidewall (-0.5 μm to 0 μm) as it approaches the mask opening, due to the increase in the protective film thickness as a result of the conventional subconformal ALD process.

[0095] In contrast, when CF4 is supplied during subconformal ALD processing in accordance with the present disclosure, the CD of the recess continues to increase (w / CF4) from the middle to the upper portion of the sidewall (−0.5 μm to 0 μm) as it approaches the mask opening.

[0096] Therefore, as shown in FIG. 8, a subconformal ALD process can be applied and the thickness of the protective film formed on the mask can be controlled to be reduced by continuously supplying CF4 throughout the subconformal ALD process. By adding CF4 in the ALD (subconformal ALD) process, the amount of film formed in the opening of the mask can be reduced. Thus, the blockage of the opening can be suppressed compared to a standard subconformal ALD process where no fluorine-containing gas (e.g., CF4) is supplied during the process.

[0097] In particular, the film is formed thickly in areas where lateral etching is likely to occur (e.g. directly under the mask) and thinly on the mask, which prevents the mask opening from shrinking and controls the film thickness distribution, improving the shape of the recess.

[0098] Furthermore, the present disclosure provides an etching technique for forming a film that is thick in areas where lateral etching is likely to occur and thin in other areas, such as the mask and / or the bottom of the recess. Also, the subconformal ALD process according to the present disclosure can enlarge the bottom of the recess by over-etching while suppressing bowing of the recess due to lateral etching.

[0099] Figures 9A to 9C show another embodiment of the present disclosure in which a protective film is also formed on the bottom surface of the recess in the etching layer. A modification of the process shown in Figure 5 can be used to form the recess shown in Figures 9A to 9C.

[0100] Specifically, in step 510, a substrate is provided having an etch layer 910 and a mask 920 disposed on the etch layer 910. In step 520, the processing circuitry 400 controls the etching device 300 to partially etch the etch layer 910 through the mask openings 930.

[0101] In step 530, the processing circuit 400 controls the etching device 300 to form a protective film 940 on the substrate. In this case, the processing circuit 400 controls the etching device 300 to form the protective film 940 on the bottom surface of the recess as well as on the sidewall of the etching layer 910. In step 540, the bottom surface of the protective film is etched, and the substrate is further etched similarly to step 520 to further etch the etching layer 910 to increase the depth of the etching layer. In step 550, the processing circuit 400 determines whether an additional protective film 940 needs to be formed to adequately protect the sidewall of the recess. As the inventors have recognized, the presence of the protective layer has the effect of preventing the sidewall of the recess of the silicon-containing layer from being removed by ion bombardment with relatively low energy. On the other hand, ions hitting the bottom surface of the recess have high energy and therefore can remove (etch) the bottom surface of the recess even if a protective layer is formed on the bottom surface of the recess. Thus, the protective layer is chemically strong enough not to be removed by low energy ions that graze the sidewalls, and preferentially protects the sidewalls against undesired etching of the sidewalls, while high energy ions that directly impinge on the bottom of the recess have sufficient energy to etch the protective layer at the bottom of the recess, thus making it possible to etch high aspect ratio recesses with reduced bowing of the sidewalls.

[0102] If more protective coating 640 is needed (YES at step 550), the process returns to step 530. If more protective coating 640 is not needed (NO at step 550), the process proceeds to step 560. At step 560, the substrate is further etched through etching layer 910 to a final depth and the process is complete.

[0103] As described above with respect to FIG. 5 and FIG. 6A-6C, the protective film 940 is formed by (1) adsorbing a precursor on the sidewall and bottom surfaces of the recess of the etching layer 910, (2) purging the gas in the reaction chamber, (3) converting the precursor into a protective film, and (4) purging the gas in the reaction chamber again. The adsorption of the precursor may be performed with or without generating a plasma of the precursor gas. The purging step of the gas in the reaction chamber may be optional. Furthermore, the supply of the inhibitor gas and the modifying gas may be continuously performed during the purge or may be stopped before the purge and resumed after the purge. In another example, after the adsorption of the precursor, in either the subconformal ALD or ALD, a plasma may be generated from a modifying gas (e.g., an oxygen-containing gas) to perform the modification. Then, the inhibitor gas may be supplied to form a plasma and the substrate may be exposed to the plasma.

[0104] In an exemplary embodiment for forming the protective film 940 of FIGS. 9A-9C, the precursor delivery time and / or modification time are longer than the precursor delivery time and / or modification time in the subconformal ALD process described for forming the protective film 640 of FIGS. 6A-6C.

[0105] Although embodiments of the subject matter of the present disclosure have been described, those skilled in the art will understand that the above is merely illustrative, not limiting, and is presented by way of example only. Thus, although certain configurations have been described herein, other configurations can be employed. Numerous modifications and other embodiments (e.g., combinations, rearrangements, etc.) are possible from the present disclosure and are within the scope of one skilled in the art and are intended to be encompassed within the scope of the subject matter of the present disclosure and any equivalents thereof. Further embodiments can be obtained by combining, rearranging, or omitting features of the embodiments of the present disclosure within the scope of the present invention. Furthermore, certain features may be used alone and other features may not be used correspondingly. Accordingly, the applicant intends to embrace all such alternatives, modifications, equivalents, and variations that are within the spirit and scope of the subject matter of the present disclosure. [Explanation of symbols]

[0106] W...substrate, 100...layer stack, 110...substrate, 120...etching layer, 130...mask, 140...region, 200...substrate processing system, 212, 214, 216, 218...load port, 220...loader device, 222...loader robot, 232, 234...load lock chamber, 240...transfer device, 242...transfer robot, 252, 254, 256, 258, 300...etcher, 260...controller, 310...reaction chamber, 312...plasma, 320...base, 322...electrostatic chuck, 330...upper electrode, 340...first RF power source, 350...second RF power source, 360...gas source , 370...exhaust device, 380...variable DC power supply, 400...processing circuit, 401...CPU, 402...memory, 404...storage medium disk, 406...network control unit, 408...display device control unit, 410...display device, 412...general-purpose I / O interface, 414...keyboard / mouse, 416...touch panel, 418...peripheral devices, 424...general-purpose storage device control unit, 426...communication bus, 428...network, 610...etching layer, 620...mask layer, 630...opening, 640...protective film, 910...etching layer, 920...mask, 930...mask opening, 940...protective film.

Claims

1. 1. A method of forming a film on a substrate comprising an etching layer and a mask formed on the etching layer, comprising: (a) exposing the substrate to a precursor in a reaction chamber to deposit precursor particles on at least sidewalls of recesses in the etch layer; (b) a supply step of supplying an inhibitor gas, which is a gas that inhibits adsorption of the precursor, and a modifying gas into the reaction chamber to generate plasma; (c) a modifying step of modifying the precursor particles on the sidewall into a protective film while supplying the inhibiting gas and the modifying gas to the reaction chamber; Including, The method, wherein the precursor is a Si-containing gas.

2. The method of claim 1 , further comprising, after the (c) modifying step, (d) etching the substrate using the plasma.

3. The method of claim 1 , wherein the (b) supplying step is carried out continuously throughout the (a) exposing step and the (c) modifying step.

4. The method of claim 1 , wherein the (a) exposing step is repeated after completion of the (c) modifying step.

5. The (a) exposure step is carried out so as to additionally dispose precursor particles on a bottom surface of the recess of the etching layer; The method according to claim 1 , wherein the (c) modifying step includes modifying the precursor particles on the bottom surface of the recess into the protective film.

6. The inhibitor gas is C x F y The method of claim 1 , wherein the gas is a gas.

7. The thickness of the protective film formed on the upper portion of the recess is C x F y The method of claim 6 , wherein the thickness of the protective film formed on the upper portion of the recess is smaller than the thickness of the protective film formed on the upper portion of the recess under a condition in which no gas is supplied.

8. 2. The method of claim 1, wherein a critical dimension (CD) of a vertical center region of the sidewall after forming the protective film is smaller than a CD of an upper portion of the sidewall.

9. The method of claim 1 , wherein a thickness of the protective film formed on an upper portion of the recess is smaller than a thickness of the protective film formed on a remaining portion of the sidewall.

10. The method of claim 1 , wherein the reformulated gas and the inhibiting gas are supplied sequentially.

11. The method of claim 1 , further comprising: (e) a purging step of purging the interior of the reaction chamber.

12. The method of claim 11 , wherein the (e) purging step is performed after the (a) exposing step and then again after the (c) modifying step.

13. The method of claim 2 , wherein the etching step (d) comprises applying a bias power to an electrode in the reaction chamber.

14. The method of claim 1 , wherein the (c) reforming step includes supplying radio frequency (RF) to an electrode in the reaction chamber during the (c) reforming step.

15. 1. A method of forming a film on a substrate comprising an etching layer and a mask formed on the etching layer, comprising: During the first period, (a) exposing the substrate to a precursor in a reaction chamber to deposit precursor particles on at least sidewalls of recesses in the etch layer; During the second period, (b) a supply step of supplying an inhibitor gas, which is a gas that inhibits adsorption of the precursor, and a modifying gas into the reaction chamber to generate plasma; (c) a modifying step of modifying the precursor particles on the sidewall into a protective film while supplying the inhibiting gas and the modifying gas to the reaction chamber; Including, The method, wherein the precursor is a Si-containing gas.

16. 16. The method of claim 15, wherein at least a portion of said (b) providing step and said (c) reforming step are performed simultaneously during said second period of time.

17. 16. The method of claim 15, further comprising providing radio frequency (RF) power during (c) the modifying step.

18. An apparatus for forming a film on a substrate including an etching layer and a mask formed on the etching layer, comprising: A processing circuit is provided, the processing circuit comprising: controlling a supply of precursor to a reaction chamber, thereby exposing the substrate to deposit precursor particles on at least sidewalls of recesses in the etching layer; controlling a gas source to supply an inhibitor gas, which is a gas that inhibits adsorption of the precursor, and a modifying gas to the reaction chamber to generate plasma; configured to control a radio frequency (RF) source to supply RF on the sidewall of the recess to modify the precursor particles on the sidewall into a protective film while supplying the inhibiting gas and the modifying gas to the reaction chamber; The apparatus, wherein the precursor is a Si-containing gas.

19. 20. The apparatus of claim 18, wherein the inhibiting gas and the modifying gas are supplied continuously throughout the supply of the precursor and throughout the modification of the precursor particles into the protective film.

20. 20. The apparatus of claim 18, wherein the processing circuitry is further configured to control gas exhaust to purge the inhibiting gas and the modified gas from the reaction chamber.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor device, method of processing substrate, and substrate processing apparatus

    JP2011129879A

  • Method for processing workpiece

    JP2018037453A

  • Plasma processing method and plasma processing device

    JP2020025078A

  • Substrate processing method and substrate processing apparatus

    JP2021077843A

  • Technique to deposit sidewall passivation for high aspect ratio cylinder etch

    US20160343580A1