Resin molded body with a thickness of 1 mm or less

By laminating and heating a fiber-reinforced resin material with a thermosetting resin and fibers, the method addresses the challenge of producing thin, rigid, and complex-shaped molded products by using a liquid resin as a heat insulator and lubricant, resulting in a composite molded article with a thickness of 1 mm or less.

JP7573577B2Active Publication Date: 2024-10-25INOAC CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022142028
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-07
Publication Date
2024-10-25
Estimated Expiration
2039-09-11

AI Technical Summary

Technical Problem

Existing methods for manufacturing fiber-reinforced resin molded bodies struggle to produce thin products with both rigidity and complex shapes, as the thickness of the layer formed from sheet molding compound is limited to about 70% of its original thickness during compression molding.

Method used

A method involving a fiber-reinforced resin material for a rigid layer and a compound for a shaping layer, both composed of thermosetting resin and fibers, is used. The layers are laminated and heated and compressed together with a liquid resin, which acts as a heat insulator and lubricant, allowing the shaping layer to be thinner and more fluid, enabling complex shapes.

Benefits of technology

The method results in a thin fiber-reinforced resin composite molded article with rigidity and complex shape capabilities by delaying the curing reaction and improving fluidity, achieving a thickness of 1 mm or less for the shaping layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573577000001
    Figure 0007573577000001
  • Figure 0007573577000002
    Figure 0007573577000002
  • Figure 0007573577000003
    Figure 0007573577000003
Patent Text Reader

Abstract

The object is to provide a thin-walled fiber-reinforced resin composite molding that has rigidity and can be formed into complex shapes. [Solution] The product is composed of a rigid layer (11) formed from a fiber-reinforced resin material for the rigid layer, a shape-imparting layer (21) formed on at least one surface of the rigid layer (11) from a compound for the shape-imparting layer composed of a thermosetting resin and fibers shorter than those contained in the fiber-reinforced resin material for the rigid layer, and a resin (31) formed from a liquid resin adhered to the surface of the shape-imparting layer (21), in which the fiber-reinforced resin material for the rigid layer, the compound for the shape-imparting layer, and the liquid resin are heated, compressed, and hardened in a stacked state.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced resin composite molded product and a method for producing the same. [Background technology]

[0002] 2. Description of the Related Art Fiber-reinforced resin molded articles have been used in a wide range of industrial fields, such as sports, leisure, and aviation, due to their high strength and high rigidity. 2. Description of the Related Art As a method for producing fiber-reinforced resin moldings, methods of compression molding prepregs in which reinforcing fibers are impregnated with a thermosetting resin, sheet molding compounds, and the like, are adopted in many fields.

[0003] Prepreg uses long fibers as reinforcing fibers, which allows for the production of high strength and high rigidity molded products, but it is difficult to mold them into complex shapes. In contrast, sheet molding compounds use short fibers as reinforcing fibers, which means that the strength of the molded products is lower than that of prepreg, but they have excellent flowability during molding and are easy to mold into complex shapes such as ribs and bosses.

[0004] Also, in order to incorporate the advantages of both prepregs and sheet molding compounds, while maintaining rigidity, and enabling the creation of complex shapes, it has been proposed to laminate prepregs and sheet molding compounds and perform compression molding (Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-083441 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the case of a composite molded product obtained by laminating prepregs and sheet molding compound and compression molding, the thickness of the layer formed from the sheet molding compound can only be about 70% of the thickness of the sheet molding compound before compression molding, so the overall thickness of the molded product cannot be made thin, and it has not been possible to obtain a thin-walled molded product that is rigid and can be formed into complex shapes.

[0007] The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a fiber-reinforced resin composite molding that has rigidity and can be formed into a complex shape and a thin wall, and a method for producing the same. [Means for solving the problem]

[0008] First aspect of the invention The fiber-reinforced resin composite molding comprises a rigid layer formed from a fiber-reinforced resin material for the rigid layer, a mold layer formed on at least one surface of the rigid layer from a compound for a mold layer comprising a thermosetting resin and fibers shorter than the fibers contained in the fiber-reinforced resin material for the rigid layer, and a resin formed by hardening a liquid resin adhered to the surface of the mold layer, wherein the fiber-reinforced resin material for the rigid layer and the compound for the mold layer are heated, compressed, and hardened together with the liquid resin in a laminated state.

[0009] The second aspect of the invention is the same as the first aspect of the invention. In the present invention, the fiber-reinforced resin material for the rigid layer is a prepreg, the compound for the shape-imparting layer is a sheet molding compound, and the liquid resin is a thermosetting resin.

[0010] Third aspect of the inventionis a method for producing a fiber-reinforced resin composite molded body comprising a rigid layer formed from a fiber-reinforced resin material for a rigid layer, a mold layer formed on at least one side of the rigid layer from a compound for a mold layer comprising fibers shorter than the fibers contained in the fiber-reinforced resin material for the rigid layer and a thermosetting resin, and a resin formed by hardening the liquid resin adhering to the surface of the mold layer, characterized in that a liquid resin is applied to the surface of the compound for the mold layer, or a liquid resin is applied to a mold surface of a mold that will press the surface of the compound for the mold layer, and the fiber-reinforced resin material for the rigid layer and the compound for the mold layer are heated and compressed in the mold together with the liquid resin in a stacked state, and hardened.

[0011] The fourth aspect of the invention is the third aspect of the invention. In the present invention, the fiber-reinforced resin material for the rigid layer is a prepreg, the compound for the shape-imparting layer is a sheet molding compound, and the liquid resin is a thermosetting resin. Effect of the Invention

[0012] According to the present invention, the fiber-reinforced resin composite molded body is a product in which the fiber-reinforced resin material for the rigid layer, the compound for the mold layer, and the liquid resin are heated, compressed, and cured together with the liquid resin in a laminated state. Therefore, when the fiber-reinforced resin composite molded body is produced by heating and compressing the compound for the mold layer with a mold, the liquid resin acts as a heat insulating layer between the compound for the mold layer and the mold surface of the mold, and the curing reaction of the compound for the mold layer is delayed. Therefore, the flow amount of the compound for the mold layer increases until the completion of curing, and the mold layer formed from the compound for the mold layer can be made thin. Furthermore, the liquid resin acts as a lubricant between the compound for the mold layer and the mold surface of the mold to improve the fluidity of the compound for the mold layer, which also makes it possible to make the mold layer thinner. As a result, a fiber-reinforced resin composite molded body that has rigidity due to the rigid layer and can be shaped into a complex shape by the mold layer and is further thin can be obtained. [Brief description of the drawings]

[0013] [Figure 1] 1 is a cross-sectional view of one embodiment of a fiber-reinforced resin composite molded product according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of one embodiment of a mold. [Diagram 3] 1 is a table showing the configuration of the applied resin and the thickness after molding in each of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The fiber-reinforced resin composite molded product and the method for producing the same of the present invention will be described below. The fiber-reinforced resin composite molding 10 shown in Figure 1 comprises a rigid layer 11 formed from a rigid fiber-reinforced resin material, a mold layer 21 formed from a mold layer compound, and resin 31 which is hardened liquid resin adhered to the surface of the mold layer compound.

[0015] The rigid layer 11 is made of a fiber-reinforced resin material for a rigid layer that has been heated, compressed and cured. The fiber reinforced resin material for the rigid layer is a fiber sheet impregnated with a thermosetting resin. Examples of the fiber sheet include those made of fibers such as carbon fiber, glass fiber, and aramid fiber. In particular, carbon fiber is preferable from the viewpoints of weight reduction and improved rigidity. The fiber sheet may be woven, knitted, nonwoven, etc. Examples of the woven fabric include plain weave, twill weave, satin weave, and triaxial weave. The fiber sheet may be made of fibers oriented in one direction or multiple directions. The fiber sheet is preferably a woven fiber from the viewpoint of improved rigidity.

[0016] The fibers constituting the fiber sheet are preferably longer than the fibers contained in the compound for the mold-imparting layer described below, and may be, for example, continuous or discontinuous fibers.

[0017] Examples of the thermosetting resin impregnated into the fiber sheet include epoxy resin, phenol resin, vinyl ester resin, unsaturated polyester resin, and mixed resins thereof. Prepreg is preferable as the fiber reinforced resin material for the rigid layer in which the fiber sheet is impregnated with the thermosetting resin.

[0018] The shape-imparting layer 21 is made of a compound for the shape-imparting layer, which is made of a thermosetting resin and fibers shorter than those contained in the fiber-reinforced resin material for the rigid layer, and is heated, compressed, and hardened. The surface shape of the shape-imparting layer 21 may have an appropriate concave shape, convex shape, or uneven shape depending on the application of the fiber-reinforced resin composite molding 10, etc.

[0019] The length of the fiber contained in the compound for the mold layer is preferably 30 mm or less from the viewpoint of moldability, and is preferably 5 mm or more from the viewpoint of improving rigidity. Examples of the fiber contained in the compound for the mold layer include short fibers such as carbon fiber and glass fiber. In particular, carbon fiber is preferred from the viewpoints of weight reduction and improving rigidity.

[0020] Examples of the thermosetting resin contained in the compound for the mold layer include epoxy resin, phenol resin, vinyl ester resin, unsaturated polyester resin, and mixed resins thereof. The compound for the mold layer is preferably a sheet molding compound (hereinafter referred to as SMC). SMC refers to a sheet-shaped molding material in which a compound containing a thermosetting resin, a filler, a curing agent, etc. is impregnated into a fiber material such as glass fiber or carbon fiber.

[0021] The resin 31 is made of a cured liquid resin. The liquid resin is made of a thermosetting resin. When the fiber-reinforced resin composite molded body 10 is produced, the liquid resin is heated and compressed together with the compound for the mold layer, and is mixed with the curing agent for the thermosetting resin contained in the compound for the mold layer, so that the liquid resin can be cured without the need for a curing agent.

[0022] The thermosetting resin constituting the liquid resin is preferably a radical polymerization type thermosetting resin such as vinyl ester resin, unsaturated polyester resin, or epoxy resin. The thermosetting resin may contain a curing agent, a dispersant, a flame retardant, a UV absorber, or the like, as necessary. The liquid resin may also contain a solvent together with the thermosetting resin, and may be adjusted to a viscosity suitable for application.

[0023] The rigid layer 11, the molding layer 21, and the resin 31 are formed as a single unit by heating and compressing the fiber-reinforced resin material for the rigid layer, the compound for the molding layer, and the liquid resin on their surfaces, which harden in a stacked state when manufactured using the fiber-reinforced resin composite molding 10.

[0024] The following describes a method for producing the fiber reinforced resin composite molded body 10. The method for producing the fiber reinforced resin composite molded body 10 includes a coating step and a heat compression step.

[0025] In the coating step, an uncured liquid resin is applied to one side surface of the compound for the mold layer or to the mold surface of the mold. The mold 60 shown in FIG. 2 is composed of an upper mold 61 and a lower mold 63. When applying the uncured liquid resin to the mold surface of the mold, the liquid resin is applied to the mold surface that will press the compound for the mold layer in the next heating and compression step, for example, the mold surface of the upper mold 61. The liquid resin may be applied to one side surface of the compound for the mold layer by stacking the fiber-reinforced resin material for the rigid layer and the compound for the mold layer on the lower mold 63 of the mold 60, and applying the liquid resin to the surface of the compound for the mold layer. The coating method may be brush coating, roller coating, spray coating, or the like, and any method may be used. The range to which the liquid resin is applied is not limited to the entire surface of the compound for the mold layer, and may be a part of it.

[0026] The compound for the mold-imparting layer is as explained in the fiber-reinforced resin composite molded body 10. The size of the compound for the mold-imparting layer used here is preferably such that the planar dimensions are 30 to 100% of the product (fiber-reinforced resin composite molded body 10). The liquid resin is as described in the fiber-reinforced resin composite molding 10. The amount of the liquid resin to be applied to the surface of the compound for the mold layer is 20 to 200 g / m2. 2 It is preferable that the above formula be set as follows:

[0027] In the heat compression step, the fiber reinforced resin material for the rigid layer, the compound for the molding layer, and the liquid resin are arranged in a layered state between the mold surface of the upper mold 61 and the mold surface of the lower mold 63 of the metal mold 60, and in this state are heated and compressed by the mold surface of the upper mold 63 and the mold surface of the lower mold 61. A cavity for shaping the fiber reinforced resin composite molded body 10 is formed in the lower mold 63. The planar size of the cavity for shaping is set to be equal to the planar size of the fiber reinforced resin composite molded body 10.

[0028] By heating and compression, the fiber-reinforced resin material for the rigid layer is compressed and the compound for the mold layer is compressed and flows in the mold 60, and the fiber-reinforced resin material for the rigid layer and the compound for the mold layer are shaped into the cavity shape and hardened. At that time, since the liquid resin exists between the compound for the mold layer and the mold surface, the liquid resin acts as a lubricant on the surface of the compound for the mold layer, improving the fluidity of the compound for the mold layer in the mold 60, and the compound for the mold layer is shaped thinly. In addition, the liquid resin acts as a heat insulating layer between the compound for the mold layer and the mold surface, delaying the hardening reaction of the compound for the mold layer due to heat transfer from the mold surface, and increasing the flow amount of the compound for the mold layer until hardening is completed, which also causes the compound for the mold layer to be shaped thinly.

[0029] During heating and compression, the liquid resin on the surface of the compound for the mold layer is pressed by the mold surface, and is mixed with the thermosetting resin on the surface of the compound for the mold layer and in the vicinity thereof and hardens. At that time, even if the liquid resin does not contain a hardener, it can harden by mixing with the hardener contained in the compound for the mold layer.

[0030] Heating during the heat compression step is performed by a heating means such as an electric heater provided in the mold, or by a method in which the mold is heated in advance in a heating furnace, etc. The heating temperature is set to a temperature at which the thermosetting resin and liquid resin contained in the fiber reinforced resin material for the rigid layer and the compound for the shape-imparting layer are cured.

[0031] The heating and compression process integrates the rigid layer formed by compressing and hardening the fiber-reinforced resin material for the rigid layer, the shaping layer formed by compressing and hardening the compound for the shaping layer in a thin shaped state, and the resin formed by hardening the liquid resin on its surface, resulting in a thin fiber-reinforced resin composite molding 10 consisting of the rigid layer 11, the shaping layer 21, and the resin 31 on its surface as shown in Figure 1. EXAMPLES

[0032] A carbon fiber fabric (Teijin Limited, product name: W-3161L, thickness 0.22 mm) cut to a size of 400 x 400 mm was immersed in a phenolic resin solution (Sumitomo Bakelite Co., Ltd., product name: PR-55791B, resin concentration 60 wt% ethanol solution), removed, and then naturally dried at a room temperature of 25°C for 2 hours, and then dried in an atmosphere of 60°C for 1 hour to form a fiber-reinforced resin material (prepreg) for the rigid layer.

[0033] A sheet of fiber-reinforced resin material (prepreg) for the rigid layer was placed on the molding surface of the lower part of the mold, and a compound for the mold layer (SMC, manufactured by Mitsubishi Chemical Corporation, product name: STR120N131, thickness 2 mm, fiber content 53%) cut to a size of 300 x 300 mm was laminated on top of it. The surface of the compound for the mold layer was coated with the liquid uncured coating resin (thermosetting resin) shown in each example in Figure 3 using a brush, and then the mold was closed and the mold was heated at 150 °C for 20 minutes at a pressure of 200 kgf / cm. 2 The fiber-reinforced resin material for the rigid layer (prepreg), the compound for the mold layer, and the applied resin were heated and compressed at 400° C. to harden the fiber-reinforced resin material for the rigid layer (prepreg), the compound for the mold layer, and the applied resin in a laminated compressed state. This produced a fiber-reinforced resin composite molded product consisting of a laminated integral product of the rigid layer formed from the fiber-reinforced resin material for the rigid layer (prepreg), the mold layer formed from the compound for the mold layer, and the resin formed from the applied resin. The mold was made of a lower mold and an upper mold, and had a molding surface of 460 mm wide x 460 mm long.

[0034] Furthermore, the fiber-reinforced resin composite molded bodies of Comparative Examples 1 to 3 were produced by performing heat compression molding on the compound for the mold-imparting layer without applying a thermosetting resin to the surface thereof. The thickness after molding was measured for the fiber-reinforced resin composite molded body of each Example and Comparative Example. The results are shown in Figure 3. The charge rate [%] in Figure 3 is the ratio of the thickness of the molded layer to the original thickness (2 mm) of the compound for the molded layer. In calculating the charge rate, the thickness of the molded layer was calculated by subtracting the thickness (0.22 mm) of the fiber-reinforced resin material for the rigid layer (prepreg) from the thickness after molding (thickness of the fiber-reinforced resin composite molded body), assuming that the thickness (0.22 mm) of the fiber-reinforced resin material for the rigid layer (prepreg) does not change due to heating and compression.

[0035] In Example 1, a vinyl ester resin (manufactured by Showa Denko K.K., product name: Lipoxy R-806) was applied as a coating resin (thermosetting resin) to the surface of the compound for the mold layer at a rate of 50 g / m. 2 This is an example of application. In Example 1, the thickness of the fiber reinforced resin composite molding after molding was 0.95 mm, and the charge rate was 37%. The thickness of the molding layer formed from the compound for molding layer (thickness 2 mm) was the thickness of the fiber reinforced resin composite molding (0.95 mm) - the thickness of the fiber reinforced resin material for rigid layer (0.22 mm) = 0.73 mm, and the molding layer was formed thin.

[0036] In Example 2, the same vinyl ester resin (manufactured by Showa Denko K.K., product name: Lipoxy R-806) as in Example 1 was applied as a coating resin (thermosetting resin) to the surface of the compound for the mold layer at a rate of 75 g / m 2 In Example 2, the thickness of the fiber-reinforced resin composite molding after molding was 0.93 mm, and the charge rate was 36%. The thickness of the molding layer formed from the compound for molding layer (thickness 2 mm) was the thickness of the fiber-reinforced resin composite molding (0.93 mm) - the thickness of the fiber-reinforced resin material for rigid layer (0.22 mm) = 0.71 mm, and the amount of coating resin was increased compared to Example 1, so that the molding layer was formed thinner than Example 1.

[0037] In Example 3, the same vinyl ester resin (manufactured by Showa Denko K.K., product name: Lipoxy R-806) as in Examples 1 and 2 was applied as a coating resin (thermosetting resin) to the surface of the compound for the mold layer at a rate of 100 g / m 2In Example 3, the thickness of the fiber-reinforced resin composite molding after molding was 0.91 mm, and the charge rate was 35%. The thickness of the molding layer formed from the compound for molding layer (thickness 2 mm) was the thickness of the fiber-reinforced resin composite molding (0.91 mm) - the thickness of the fiber-reinforced resin material for rigid layer (0.22 mm) = 0.69 mm, and the amount of the applied resin was increased compared to Examples 1 and 2, so that the molding layer was formed even thinner than Examples 1 and 2.

[0038] In Example 4, an unsaturated polyester resin (manufactured by Showa Denko K.K., product name: RIGOLAC T-543TPA) was applied as a coating resin (thermosetting resin) to the surface of the compound for the mold layer at a rate of 50 g / m 2 In Example 4, the thickness of the fiber-reinforced resin composite molding after molding was 1.00 mm, and the charge rate was 39%. The thickness of the molding layer formed from the compound for molding layer (thickness 2 mm) was the thickness of the fiber-reinforced resin composite molding (1.00 mm) - the thickness of the fiber-reinforced resin material for rigid layer (0.22 mm) = 0.78 mm, and it was formed thin.

[0039] In this way, in Examples 1 to 4, by applying a liquid thermosetting resin to the surface of the compound for the mold layer laminated to the fiber-reinforced resin material (prepreg) for the rigid layer and then performing heated compression molding, the thickness of the mold layer formed from the compound for the mold layer could be formed to a thin thickness of 0.69 to 0.78 mm, and a thin fiber-reinforced resin composite molding with a thickness of 1 mm or less could be obtained.

[0040] Comparative Example 1 is an example in which no liquid thermosetting resin was applied to the surface of the compound for the mold layer, and the heating and compression conditions were the same as those of Examples 1 to 4. In Comparative Example 1, the thickness of the fiber-reinforced resin composite molding after molding was 1.12 mm, and the charge rate was 45%. The thickness of the mold layer formed from the compound for the mold layer (thickness 2 mm) was the thickness of the fiber-reinforced resin composite molding (1.12 mm) - the thickness of the fiber-reinforced resin material for the rigid layer (0.22 mm) = 0.90 mm, and the mold layer was formed thicker than Examples 1 to 4 by not applying a liquid thermosetting resin to the surface of the compound for the mold layer.

[0041] Comparative Example 2 is an example in which the area of ​​the compound for the mold layer in Comparative Example 1 was increased by 10%, and liquid thermosetting resin was not applied. In Comparative Example 2, the thickness of the fiber reinforced resin composite molding after molding was 1.30 mm, and the charge rate was 54%. The thickness of the mold layer formed from the compound for the mold layer (thickness 2 mm) was the thickness of the fiber reinforced resin composite molding (1.30 mm) - the thickness of the fiber reinforced resin material for the rigid layer (0.22 mm) = 1.08 mm, and by increasing the amount of the compound for the mold layer, the mold layer was formed thicker than in Comparative Example 1.

[0042] Comparative Example 3 is an example in which the area of ​​the compound for the mold layer in Comparative Example 1 was increased by 20%, and liquid thermosetting resin was not applied. In Comparative Example 3, the thickness of the fiber reinforced resin composite molding after molding was 1.60 mm, and the charge rate was 69%. The thickness of the mold layer formed from the compound for the mold layer (thickness 2 mm) was the thickness of the fiber reinforced resin composite molding (1.60 mm) - the thickness of the fiber reinforced resin material for the rigid layer (0.22 mm) = 1.38 mm, and by increasing the amount of the compound for the mold layer, the mold layer was formed thicker than in Comparative Examples 1 and 2.

[0043] Thus, according to the present invention, it is possible to obtain a fiber-reinforced resin composite molding that has both the rigidity provided by the rigid layer and the ability to be shaped into a complex shape due to its thin wall provided by the shape-imparting layer. [Explanation of symbols]

[0044] 10 Fiber-reinforced resin composite molding 11 Rigid layer 21 Molding layer 31 Resin 60 Mold 61 Upper mold 63 Lower mold

Claims

1. A cured resin layer; A shape-imparting layer containing only a thermosetting resin and short fibers having a fiber length of 30 mm or less; a rigid layer including only fiber sheets having a fiber length longer than the short fibers, The cured resin layer, the shape-imparting layer, and the rigid layer are laminated in this order. A resin molded body with a thickness of 1 mm or less.

2. A cured resin layer; A shape-imparting layer made of a sheet molding compound containing a thermosetting resin and short fibers having a fiber length of 30 mm or less; and a rigid layer made of a prepreg including a fiber sheet having a fiber length longer than the short fibers, The cured resin layer, the shape-imparting layer, and the rigid layer are laminated in this order. A resin molded body with a thickness of 1 mm or less.

Citation Information

Patent Citations

  • FRP moulding material

    JP1977006768A

  • Fiber reinforced resin molding sheet and method for molding fiber reinforced resin

    JP1990273223A

  • Gelcoat sheet for molding and preparation thereof and preparation of molding with gelcoat layer using said gelcoat sheet for molding

    JP1993318468A

  • Phenol frp molding and its production

    JP1995097459A

  • Production of fiber reinforced plastic molded object

    JP1996118379A