Airless tires

The airless tire's inner rubber layer with a chlorinated surface and solvent-based adhesive improves the adhesion between the tread ring and spokes, enhancing durability by using styrene-butadiene rubber and tackifiers, and polymeric spokes.

JP7574539B2Active Publication Date: 2024-10-29SUMITOMO RUBBER INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020045518
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-16
Publication Date
2024-10-29
Estimated Expiration
2040-03-16

Smart Images

  • Figure 0007574539000002
    Figure 0007574539000002
  • Figure 0007574539000003
    Figure 0007574539000003
  • Figure 0007574539000001
    Figure 0007574539000001
Patent Text Reader

Abstract

To provide an airless tire that can improve the adhesion between the tread ring and the spokes.SOLUTION: An airless tire 1 is equipped with a cylindrical tread ring 2 having a ground contact surface S, a hub 3 arranged inside the tread ring 2 in the radial direction of the tire and fixed to an axle J, and spokes 4 connecting the tread ring 2 and the hub 3. The spokes 4 are made of a polymeric material. The tread ring 2 includes a tread rubber layer 2A forming a ground contact surface S and an inner rubber layer 2B arranged inside the tread rubber layer 2A in the radial direction of the tire. The inner rubber layer 2B has an inner peripheral surface 2a formed from a rubber composition containing styrene-butadiene rubber and a tackifier and chlorinated. The inner peripheral surface 2a of the inner rubber layer 2B is joined to the spokes 4 via an adhesive layer 5 made of an adhesive.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an airless tire. [Background technology]

[0002] Conventionally, there is known an airless tire that includes a cylindrical tread ring having a ground contact surface, a hub that is disposed radially inward of the tread ring and fixed to an axle, and spokes that connect the tread ring and the hub. For example, the following Patent Document 1 proposes a manufacturing method for an airless tire that enhances the bonding strength at the interface between the spokes and the adhesive by preheating the tread ring to which an adhesive layer is applied. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-094825 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, there is a demand for improving the adhesion between the tread ring and the spokes regardless of a specific manufacturing method, and there is a demand for further improvement in the airless tire described in Patent Document 1.

[0005] The present invention has been devised in view of the above circumstances, and has as its main object to provide an airless tire capable of improving adhesion between the tread ring and the spokes. [Means for solving the problem]

[0006] The present invention is an airless tire comprising a cylindrical tread ring having a contact surface, a hub disposed radially inward of the tread ring and fixed to an axle, and spokes connecting the tread ring and the hub, the spokes being formed from a polymeric material, the tread ring including a tread rubber layer constituting the contact surface and an inner rubber layer disposed radially inward of the tread rubber layer, the inner rubber layer being formed from a rubber composition containing styrene butadiene rubber and a tackifier, and having a chlorinated inner circumferential surface, the inner circumferential surface of the inner rubber layer being joined to the spokes via an adhesive layer made of an adhesive.

[0007] In the airless tire of the present invention, it is preferable that the adhesive contains at least one solvent-based adhesive selected from epoxy-based resins, phenol-based resins, olefin-based resins, and vinyl-based resins.

[0008] In the airless tire of the present invention, the spokes are desirably formed from at least one resin material selected from a polyurethane resin, a polyamide resin, and a polyester resin.

[0009] In the airless tire of the present invention, it is preferable that the entire inner circumferential surface of the inner rubber layer is in contact with the adhesive layer.

[0010] In the airless tire of the present invention, the tackifier desirably has a softening point of 60 to 150°C.

[0011] In the airless tire of the present invention, the tackifier desirably has a softening point of 70 to 100°C.

[0012] In the airless tire of the present invention, the tackifier desirably has an acid value of 120 or less.

[0013] In the airless tire of the present invention, the tackifier desirably has an acid value of 45 or less.

[0014] In the airless tire of the present invention, the tackifier is desirably formed from at least one synthetic resin selected from an alkylphenol resin and a petroleum-based hydrocarbon resin. Effect of the Invention

[0015] In the airless tire of the present invention, the spokes are formed from a polymeric material, and the tread ring includes a tread rubber layer that constitutes the contact surface and an inner rubber layer arranged radially inward of the tread rubber layer, the inner rubber layer being formed from a rubber composition containing styrene-butadiene rubber and a tackifier and having a chlorinated inner circumferential surface, and the inner circumferential surface of the inner rubber layer is joined to the spokes via an adhesive layer made of an adhesive.

[0016] Such an inner rubber layer contains styrene-butadiene rubber and a tackifier, and the inner circumferential surface is chlorinated, so that it is possible to improve adhesion to polymer materials, and therefore the airless tire of the present invention can improve adhesion between the tread ring and the spokes. [Brief description of the drawings]

[0017] [Figure 1] 1 is a perspective view showing an embodiment of an airless tire of the present invention. FIG. [Diagram 2] FIG. 1 is a schematic diagram showing a cross section of an airless tire. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Fig. 1 is a perspective view showing an airless tire 1 of the present embodiment, and Fig. 2 is a schematic diagram showing a tire meridian cross section of the airless tire 1. As shown in Fig. 1 and Fig. 2, the airless tire 1 of the present embodiment includes a cylindrical tread ring 2 having a contact surface S, a hub 3 disposed on the inner side of the tread ring 2 in the tire radial direction, and spokes 4 connecting the tread ring 2 and the hub 3.

[0019] The airless tire 1 of the present embodiment is suitable for use as a tire for passenger cars. The airless tire 1 is not limited to being used as a tire for passenger cars, and may be used as various tires such as heavy load tires, motorcycle tires, and aircraft tires.

[0020] The hub 3 of this embodiment includes a disk-shaped disk portion 3A fixed to the axle J. The hub 3 preferably further includes a cylindrical spoke attachment portion 3B formed integrally with the disk portion 3A on the opposite side in the tire radial direction. The disk portion 3A has, for example, a hub hole 3a through which the front end portion Ja of the axle J is inserted, and a plurality of bolt insertion holes 3b arranged around the hub hole 3a and through which the bolt portions Jb of the axle J are inserted.

[0021] The spokes 4 of this embodiment are formed from a polymeric material. The spokes 4 preferably integrally include an outer annular portion 4A, an inner annular portion 4B, and a spoke portion 4C. The outer annular portion 4A and the inner annular portion 4B are preferably each formed in a cylindrical shape concentric with the axle J. The spoke portion 4C preferably integrally connects the outer annular portion 4A and the inner annular portion 4B.

[0022] 2, the tread ring 2 of this embodiment includes a tread rubber layer 2A that constitutes the contact surface S, and an inner rubber layer 2B that is disposed radially inward of the tread rubber layer 2A. In such a tread ring 2, the tread rubber layer 2A can be formed from a rubber composition suitable for each well-known performance required for the contact surface S, such as wear resistance.

[0023] The inner rubber layer 2B of the present embodiment is formed from a rubber composition containing a styrene-butadiene rubber and a tackifier. The inner rubber layer 2B can improve the dispersibility of the tackifier by the styrene-butadiene rubber, and is also excellent in processability.

[0024] The inner rubber layer 2B of the tread ring 2 desirably has a surface-treated inner circumferential surface 2a. Examples of the surface treatment of the inner circumferential surface 2a include buffing, cyclization, chlorination, and methylene iodide treatment. The inner rubber layer 2B of this embodiment has a chlorination-treated inner circumferential surface 2a. Such an inner circumferential surface 2a can increase the bonding points of the adhesive.

[0025] The chlorination treatment may be, for example, an organic active halogen compound treatment. The halogen compound used in the organic active halogen compound treatment may be, for example, a halogen compound of isocyanuric acid. In the chlorination treatment of the present embodiment, trichloroisocyanuric acid is used as the halogen compound.

[0026] The inner circumferential surface 2a of the inner rubber layer 2B of this embodiment is joined to the spokes 4 via an adhesive layer 5 made of an adhesive. Such an inner rubber layer 2B contains styrene-butadiene rubber and a tackifier, and the inner circumferential surface is chlorinated, so that the adhesion to polymer materials can be improved. Therefore, the airless tire 1 of this embodiment can improve the adhesion between the tread ring 2 and the spokes 4.

[0027] In a more preferred embodiment, the hub 3 is formed from a metal material such as steel, an aluminum alloy, a magnesium alloy, etc. The spoke attachment portion 3B of the hub 3 and the inner annular portion 4B of the spoke 4 are desirably joined via a second adhesive layer 6 made of an adhesive.

[0028] The spokes 4 are formed, for example, from a cast or injection molded article made of a polymer material. Such spokes 4 have good processability and can improve the degree of freedom in shape design.

[0029] The polymeric material constituting the spokes 4 is preferably a resin material or an elastomer material. Examples of the resin material or the elastomer material include polyolefin resin, polyvinyl chloride resin, polystyrene resin, methacrylic resin, polycarbonate resin, polyamide resin, polyimide resin, polyacetal resin, fluororesin, urea resin, phenolic resin, polyester resin, polyurethane resin, epoxy resin, melamine resin, and silicone resin.

[0030] The spokes 4 of the present embodiment are made of at least one resin material selected from polyurethane resin, polyamide resin, and polyester resin. Such spokes 4 have excellent moldability and processability, and can improve the freedom of material design.

[0031] The tread ring 2 may include, for example, a belt layer, a band layer, etc. (not shown). As the belt layer and the band layer, conventionally known ones may be appropriately adopted. It is preferable that a tread groove (not shown) is formed on the contact surface S formed on the tread rubber layer 2A of the tread ring 2.

[0032] In the present embodiment, the entire inner circumferential surface 2a of the inner rubber layer 2B is in contact with the adhesive layer 5. Due to the micro-level roughness of the inner circumferential surface 2a, the inner rubber layer 2B can exert an anchoring effect of the adhesive on the entire inner circumferential surface 2a. Therefore, the inner rubber layer 2B of the present embodiment can further improve adhesion to the spokes 4 made of a polymer material.

[0033] The thickness t1 of the inner rubber layer 2B is preferably 0.5 mm or more. When the thickness t1 of the inner rubber layer 2B is 0.5 mm or more, the effect of the tackifier can be fully exhibited. From this viewpoint, the thickness t1 of the inner rubber layer 2B is more preferably 1 mm or more.

[0034] The thickness t1 of the inner rubber layer 2B is preferably 5 mm or less. By setting the thickness t1 of the inner rubber layer 2B to 5 mm or less, it is possible to maintain good rigidity of the tread ring 2. From this viewpoint, the thickness t1 of the inner rubber layer 2B is more preferably 3 mm or less.

[0035] The rubber composition of the inner rubber layer 2B preferably contains 10 to 100 parts by weight of styrene-butadiene rubber per 100 parts by weight of the rubber component. Such an inner rubber layer 2B is suitable for improving the dispersibility of a tackifier.

[0036] The rubber composition of the inner rubber layer 2B preferably contains 1 to 15 parts by weight of a tackifier per 100 parts by weight of the rubber component. When the amount of the tackifier is 1 part by weight or more, sufficient adhesion can be exhibited and the adhesion to the polymer material can be improved. When the amount of the tackifier is 15 parts by weight or less, good processability can be ensured.

[0037] The tackifier contained in the inner rubber layer 2B is desirably formed from a natural resin or a synthetic resin. Examples of synthetic resins include petroleum-based hydrocarbon resins and alkylphenol-based resins. The tackifier of this embodiment is formed from at least one synthetic resin selected from alkylphenol-based resins and petroleum-based hydrocarbon resins. Such a tackifier has good dispersibility in the rubber composition and can improve the wettability of the adhesive.

[0038] Examples of the alkylphenol resin include alkylphenol acetylene resin and alkylphenol formaldehyde resin. The alkylphenol acetylene resin is a polycondensate of an alkylphenol such as pt-butylphenol and acetylene. The alkylphenol formaldehyde resin is a polycondensate of an alkylphenol such as pt-butylphenol and formaldehyde. The alkylphenol resin is preferably an alkylphenol formaldehyde resin.

[0039] Examples of petroleum-based hydrocarbon resins include aliphatic petroleum resins, aromatic petroleum resins, and aliphatic / aromatic copolymer petroleum resins.

[0040] Aliphatic petroleum resins are resins obtained by cationic polymerization of unsaturated monomers such as isoprene, cyclopentadiene, etc., which are petroleum fractions having 4 to 5 carbon atoms. Aliphatic petroleum resins may be subjected to hydrogenation treatment, for example.

[0041] The aromatic petroleum resin is, for example, a resin obtained by cationic polymerization of monomers such as vinyl toluene and alkyl styrene, which are petroleum fractions having a carbon number of 8 to 10. The aromatic petroleum resin may be, for example, subjected to a hydrogenation treatment.

[0042] The aliphatic / aromatic copolymer petroleum resin is, for example, a resin obtained by copolymerizing a petroleum fraction having 4 to 5 carbon atoms with a petroleum fraction having 8 to 10 carbon atoms. The aliphatic / aromatic copolymer petroleum resin may be, for example, subjected to a hydrogenation treatment.

[0043] The tackifier preferably has a softening point of 60 to 150° C. Such a tackifier can be uniformly dispersed during kneading of the rubber composition. From this viewpoint, the tackifier more preferably has a softening point of 70 to 100° C.

[0044] The tackifier preferably has an acid value of 120 or less. Such a tackifier has good compatibility with the rubber composition. From this viewpoint, the tackifier more preferably has an acid value of 45 or less.

[0045] The thickness t2 of the adhesive layer 5 is not particularly limited, but is preferably 1 μm or more. When the thickness t2 of the adhesive layer 5 is 1 μm or more, the adhesive effect can be fully exerted. From this viewpoint, the thickness t2 of the adhesive layer 5 is more preferably 5 μm or more, and further preferably 7 μm or more.

[0046] The thickness t2 of the adhesive layer 5 is preferably 100 μm or less. By setting the thickness t2 of the adhesive layer 5 to 100 μm or less, the strength of the adhesive itself can be ensured. From this viewpoint, the thickness t2 of the adhesive layer 5 is more preferably 80 μm or less, and further preferably 50 μm or less.

[0047] The adhesive of the adhesive layer 5 is not particularly limited, and examples thereof include solvent-based adhesives containing one or more of epoxy resins, phenolic resins, olefinic resins, polyurethane resins, vinyl resins, synthetic rubbers, etc., as main components. The adhesive of the adhesive layer 5 of this embodiment contains at least one solvent-based adhesive selected from epoxy resins, phenolic resins, olefinic resins, and vinyl resins. Such adhesives are useful for improving the adhesion between the tread ring 2 and the spokes 4.

[0048] The adhesive of the adhesive layer 5 preferably contains at least one solvent-based adhesive selected from epoxy resins and phenol resins. As the solvent-based adhesive, it is more preferable to contain a phenol resin from the viewpoints of workability and applicability.

[0049] The epoxy resin is not particularly limited, but examples thereof include bisphenol type epoxy resins such as bisphenol A type epoxy resins and bisphenol F type epoxy resins, novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins, aliphatic epoxy resins, alicyclic epoxy resins, polyfunctional epoxy resins, biphenyl type epoxy resins, glycidyl ether type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, alcohol type epoxy resins such as hydrogenated bisphenol A type epoxy resins, rubber modified epoxy resins, and urethane modified epoxy resins.

[0050] The epoxy resin may be used alone or in combination of two or more of the above. Among these, the epoxy resin is preferably a bisphenol type epoxy resin such as a bisphenol A type epoxy resin or a bisphenol F type epoxy resin. Such epoxy resins are easily available in grades with different molecular weights, and can be arbitrarily set in adhesiveness and reactivity.

[0051] The phenolic resin is not particularly limited, but examples thereof include condensates of various phenols and formaldehyde, resols obtained by addition reaction of various phenols and formaldehyde with an alkali catalyst, novolacs obtained by condensation reaction of various phenols and formaldehyde with an acid catalyst, etc. Examples of various phenols include phenol, m-cresol, 3,5-xylenol, p-alkylphenol, resorcin, etc.

[0052] The phenolic resin may be used alone or in combination of two or more of the above. Among these, the phenolic resin is preferably a condensate of various phenols and formaldehyde. Such a phenolic resin is excellent in terms of physical properties and workability. Examples of the condensate of various phenols and formaldehyde include alkylphenol resins and xylene formaldehyde resins.

[0053] Examples of olefin-based resins include those based on modified polyolefins, such as modified polyethylene and modified polypropylene, which are polyolefins that have been given adhesive properties by introducing functional groups into them.

[0054] Although a particularly preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the above-described embodiment and can be modified in various ways. EXAMPLES

[0055] A prototype rubber having a rubber composition corresponding to the inner rubber layer was produced according to the formulation shown in Table 1. The prototype rubber, which was surface-treated by chlorination as necessary, was placed in a mold, and then an elastomer precursor corresponding to the polymer material of the spokes was poured into the mold, adjusted to a thickness of 2 mm, to form a vulcanized rubber-elastomer composite. The poured vulcanized rubber-elastomer composite was then cured in a hot air circulating drying oven at 110°C for 90 minutes.

[0056] A rectangular test piece 25 mm wide and 100 mm long was cut from the cured vulcanized rubber-elastomer composite and subjected to a T-peel test in accordance with JIS K 6854. The method for forming the prototype rubber, the chlorination treatment carried out as necessary, the type of adhesive and its application method shown in Table 1, the elastomer shown in Table 1, and the T-peel test method are as follows.

[0057] <Prototype rubber> The rubber composition shown in Table 1 was press-vulcanized for 15 minutes at a temperature of 170°C and a pressure of 50 kg / cm2 to form a 4 mm x 120 mm x 150 mm sheet of vulcanized rubber. This vulcanized rubber was degreased with isopropanol (IPA) to form a prototype rubber.

[0058] <Chlorination treatment> Chemlock 7701 manufactured by Lord Japan Inc. was applied to the surface of the prototype rubber, and after the solvent had evaporated, the same procedure was repeated a total of two times.

[0059] <Adhesive> A: Phenolic resin: Chemlock 218E manufactured by Lord Japan Inc. B: Epoxy resin: Chemlok 210 manufactured by Lord Japan Inc. C: Olefin resin: Chemlock 6108 manufactured by Lord Japan Inc.

[0060] <Adhesive application method> The adhesive was diluted with isopropanol (IPA) so that the ratio of adhesive to IPA was 1:2, and it was applied to the surface of the prototype rubber with a brush. After the applied solvent evaporated and dispersed, the same operation was repeated a total of 3 times.

[0061] <Elastomer> a: Urethane resin b: Polyester resin c: Polyamide resin

[0062] <T-peel test> The non-adhered end of the test piece was fixed with the gripper of a tensile testing machine, and the gripper was separated at a speed of 50 mm per minute. The peel force until the adhesive surface peeled was measured as the adhesive strength. If the test piece broke before the adhesive surface peeled, the test was terminated at that point. The results were shown as numerical values for the adhesive strength, and when the test piece broke, it was recorded as "broken".

[0063] In addition, a non-pneumatic tire (a tire corresponding to a tire size of 145 / 70R12) having the basic structure shown in FIGS. 1 and 2 using the prototype rubber for the inner rubber layer was prototyped. Using the prototyped non-pneumatic tire, a durability test was conducted. The durability test method is as follows.

[0064] <Durability> The prototyped non-pneumatic tire was mounted on a drum testing machine, a vertical load of 3 kN was applied, and it was continuously run at a speed of 60 km / h. The distance until the joint part between the tread ring and the spoke peeled was measured. The results were shown as an index with Comparative Example 1 as 100. The larger the numerical value, the longer the distance until peeling, indicating excellent durability.

[0065] The test results are shown in Table 1.

Table 1

[0066] As a result of the test, the prototype rubber of the test piece of each example broke before the adhesive surface peeled off, and it was confirmed that the adhesiveness between the rubber composition corresponding to the inner rubber layer of the tread ring and the elastomer corresponding to the polymer material of the spokes was improved. It was also confirmed that the airless tires of the example had significantly improved durability compared to the comparative example. [Explanation of symbols]

[0067] 1. Airless tires 2 Tread Ring 2A Tread rubber layer 2B inner rubber layer 3. Hub 4 spokes 5 Adhesive layer

Claims

1. An airless tire, The tire has a cylindrical tread ring having a ground contact surface, a hub disposed radially inward of the tread ring and fixed to an axle, and spokes connecting the tread ring and the hub, the spokes are formed from at least one resin material selected from a polyurethane resin, a polyamide resin, and a polyester resin; The tread ring includes a tread rubber layer that constitutes the ground contact surface, and an inner rubber layer that is disposed radially inward of the tread rubber layer, the inner rubber layer is formed from a rubber composition containing a styrene-butadiene rubber and a tackifier, and has a chlorinated inner peripheral surface; the inner circumferential surface of the inner rubber layer is joined to the spokes via an adhesive layer made of an adhesive, The tackifier has a softening point of 70 to 100° C. The adhesive includes at least one solvent-based adhesive selected from an epoxy resin, a phenolic resin, an olefin resin, and a vinyl resin. Airless tires.

2. An airless tire, The tire has a cylindrical tread ring having a ground contact surface, a hub disposed radially inward of the tread ring and fixed to an axle, and spokes connecting the tread ring and the hub, the spokes are formed from at least one resin material selected from a polyurethane resin, a polyamide resin, and a polyester resin; The tread ring includes a tread rubber layer that constitutes the ground contact surface, and an inner rubber layer that is disposed radially inward of the tread rubber layer, the inner rubber layer is formed from a rubber composition containing a styrene-butadiene rubber and a tackifier, and has a chlorinated inner peripheral surface; the inner circumferential surface of the inner rubber layer is joined to the spokes via an adhesive layer made of an adhesive, The tackifier has an acid value of 120 or less, The adhesive includes at least one solvent-based adhesive selected from an epoxy resin, a phenolic resin, an olefin resin, and a vinyl resin. Airless tires.

3. An airless tire, The tire has a cylindrical tread ring having a ground contact surface, a hub disposed radially inward of the tread ring and fixed to an axle, and spokes connecting the tread ring and the hub, the spokes are formed from at least one resin material selected from a polyurethane resin, a polyamide resin, and a polyester resin; The tread ring includes a tread rubber layer that constitutes the ground contact surface, and an inner rubber layer that is disposed radially inward of the tread rubber layer, the inner rubber layer is formed from a rubber composition containing a styrene-butadiene rubber and a tackifier, and has a chlorinated inner peripheral surface; the inner circumferential surface of the inner rubber layer is joined to the spokes via an adhesive layer made of an adhesive, The tackifier has an acid value of 45 or less, The adhesive includes at least one solvent-based adhesive selected from an epoxy resin, a phenolic resin, an olefin resin, and a vinyl resin. Airless tires.

4. An airless tire, The tire has a cylindrical tread ring having a ground contact surface, a hub disposed radially inward of the tread ring and fixed to an axle, and spokes connecting the tread ring and the hub, the spokes are formed from at least one resin material selected from a polyurethane resin, a polyamide resin, and a polyester resin; The tread ring includes a tread rubber layer that constitutes the ground contact surface, and an inner rubber layer that is disposed radially inward of the tread rubber layer, the inner rubber layer is formed from a rubber composition containing a styrene-butadiene rubber and a tackifier, and has a chlorinated inner peripheral surface; the inner circumferential surface of the inner rubber layer is joined to the spokes via an adhesive layer made of an adhesive, The tackifier is formed from at least one synthetic resin selected from an alkylphenol resin and a petroleum hydrocarbon resin, The adhesive includes at least one solvent-based adhesive selected from an epoxy resin, a phenolic resin, an olefin resin, and a vinyl resin. Airless tires.

5. The airless tire according to any one of claims 2 to 4, wherein the tackifier has a softening point of 60 to 150°C.

6. The airless tire according to claim 1 , wherein the entire inner circumferential surface of the inner rubber layer is in contact with the adhesive layer.

Citation Information

Patent Citations

  • Tansenihokyogomufukugotai

    JP1976102081A

  • Method for adhesion between vulcanized rubber and hard member

    JP2002069389A

  • rubber mixture

    JP2013536268A

  • Tire

    JP2016222051A

  • Method for manufacturing airless tire

    JP2018094825A