Rubber composition for tires and tires
The tire rubber composition, with styrene-butadiene rubber, butadiene rubber, silica, carbon black, and ethylene copolymer, addresses the need for improved dry and wet handling stability by ensuring uniform hardness and increased interaction, resulting in superior steering stability.
Patent Information
- Application Number
- JP2020139976
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-21
AI Technical Summary
Existing tire rubber compositions do not adequately address the need for improved dry handling stability and wet handling stability, which are crucial for enhanced steering performance on various road conditions.
A rubber composition for tires comprising styrene-butadiene rubber, butadiene rubber, silica, carbon black, a resin component, and an ethylene copolymer, with specific content ratios and properties to enhance compatibility and interaction, resulting in improved hardness uniformity and tackiness.
The composition achieves superior dry handling stability and wet handling stability by ensuring homogeneous rubber phases and increased interaction between components, leading to enhanced steering stability performance.
Smart Images

Figure 0007574570000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for a tire and a tire. [Background technology]
[0002] Conventionally, various methods for improving steering stability on dry road surfaces (dry steering stability) and steering stability on wet road surfaces (wet steering stability) have been studied (for example, see Patent Document 1). However, in recent years, further improvement in these performances has been required. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-186567 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a rubber composition for tires and a tire that can solve the above problems and improve the overall performance of dry steering stability and wet steering stability. [Means for solving the problem]
[0005] The present invention relates to a rubber composition for tires, which comprises a rubber component containing a styrene-butadiene rubber and a butadiene rubber, silica, carbon black, a resin component, and an ethylene copolymer, wherein a content of the resin component >|a content of the silica - a content of the carbon black|, a content of the carbon black > a content of the butadiene rubber, and a content of the butadiene rubber > a content of the ethylene copolymer.
[0006] The butadiene rubber preferably has a cis content of 90% or less.
[0007] The rubber composition preferably contains a styrene-butadiene rubber and / or a butadiene rubber that is soluble in acetone when immersed in acetone for 24 hours.
[0008] It is preferable that the content of the silica is greater than the content of the carbon black.
[0009] The cetyltrimethylammonium bromide specific surface area of the silica is 180m 2 It is preferable that the molecular weight is 1 / g or more.
[0010] The ethylene copolymer is preferably a copolymer having ethylene units, styrene units and butadiene units.
[0011] The resin component preferably contains a phenolic resin.
[0012] The present invention also relates to a tire using the rubber composition. Effect of the Invention
[0013] The present invention provides a rubber composition for tires which contains a rubber component containing styrene-butadiene rubber and butadiene rubber, silica, carbon black, a resin component, and an ethylene copolymer, in which the resin component content > |silica content - carbon black content|, the carbon black content > the butadiene rubber content, and the butadiene rubber content > the ethylene copolymer content, and therefore the overall performance of dry steering stability and wet steering stability is good. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The rubber composition for tires of the present invention contains a rubber component containing styrene-butadiene rubber and butadiene rubber, silica, carbon black, a resin component, and an ethylene copolymer, and the resin component content > |silica content - carbon black content|, the carbon black content > butadiene rubber content, and the butadiene rubber content > ethylene copolymer content.
[0015] The reason why the above-mentioned effects are obtained with the above-mentioned rubber composition is presumed to be as follows. When silica and carbon black are blended, there is a concern that due to differences in dispersibility in the rubber, domains in which only one of them is dispersed may occur, resulting in uneven hardness in the system. In contrast, in the above rubber composition, by making the content of the resin component >|the content of silica - the content of carbon black|, the rubber phase is homogenized (compatibilized) by the resin component, and at the same time, the difference in hardness in the system can be reduced. As a result, a reaction force can be generated in the entire rubber composition, which is believed to improve dry steering stability and wet steering stability. In addition, in the above rubber composition, by making the carbon black content larger than the butadiene rubber content, the amount of carbon black present in the styrene-butadiene rubber phase increases, which makes it easier for an interaction to occur between the styrene part of the styrene-butadiene rubber and the carbon black, and is considered to further improve the dry steering stability performance. In addition, in the above rubber composition, the content of the ethylene copolymer having a low polarity ethylene moiety is made smaller than the content of the butadiene rubber, so that the resin component can be appropriately precipitated on the rubber surface, which is believed to result in the adhesion of the rubber composition being exhibited, leading to good dry steering stability and wet steering stability. It is believed that the combination of these effects significantly improves the overall performance of dry steering stability and wet steering stability.
[0016] The rubber composition contains a rubber component. Here, the rubber component is a component that contributes to crosslinking, and generally has a weight average molecular weight (Mw) of 10,000 or more.
[0017] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.
[0018] In this specification, the weight average molecular weight (Mw) can be determined by converting it into standard polystyrene based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).
[0019] The total styrene content in the rubber component is preferably 15% by mass or more, more preferably 25% by mass or more, and even more preferably 28% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0020] Here, the total amount of styrene in the rubber component is the total content of styrene parts contained in the total amount of rubber component (unit: mass%), and can be calculated by Σ(content of each rubber component × amount of styrene in each rubber component / 100). For example, in a case where 100% by mass of rubber component contains 85% by mass of SBR with styrene content: 40% by mass, 5% by mass of SBR with styrene content: 25% by mass, and 10% by mass of BR with styrene content: 0% by mass, the total amount of styrene in the rubber component is 35.25% by mass (=85×40 / 100+5×25 / 100+10×0 / 100).
[0021] The total vinyl content in the rubber component is preferably 15% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, and is preferably 55% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0022] Here, the total vinyl content in the rubber component is the total content (unit: mass%) of vinyl parts contained in the entire rubber component, and can be calculated by Σ (content of each rubber component × vinyl content in each rubber component / 100). For example, in a case where 100% by mass of the rubber component contains 85% by mass of SBR with a vinyl content of 30% by mass, 5% by mass of SBR with a vinyl content of 20% by mass, and 10% by mass of BR with a vinyl content of 10% by mass, the total vinyl content in the rubber component is 27.5% by mass (=(85×30 / 100+5×20 / 100+10×10 / 100)).
[0023] From the viewpoint of overall performance such as dry steering stability and wet steering stability, it is preferable that the total vinyl amount in the rubber component of the rubber composition is greater than or equal to the total styrene amount in the rubber component.
[0024] The ratio of the total vinyl content in the rubber component to the total styrene content in the rubber component is preferably 1.1 or more, and is preferably 2.5 or less, more preferably 1.8 or less, and further preferably 1.5 or less. Within the above range, the effect tends to be better obtained.
[0025] The styrene amount and vinyl amount in each rubber component can be measured by a nuclear magnetic resonance (NMR) method. In addition, in the examples of this specification, the total styrene amount and the total vinyl amount in the rubber component are calculated according to the above-mentioned formula, but they may also be analyzed from the tire using, for example, a pyrolysis gas chromatograph mass spectrometer (Py-GC / MS) or the like.
[0026] The rubber composition contains styrene-butadiene rubber (SBR) as a rubber component. The SBR is not particularly limited, and for example, emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. Commercially available products include those from Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., etc.
[0027] The styrene content of SBR is preferably 15% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, particularly preferably 35% by mass or more, and is preferably 55% by mass or less, more preferably 45% by mass or less, even more preferably 40% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0028] The vinyl content of the SBR is preferably 15% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, particularly preferably 35% by mass or more, and is preferably 55% by mass or less, more preferably 45% by mass or less, even more preferably 40% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0029] The above-mentioned styrene amount and vinyl amount of SBR mean the styrene amount and vinyl amount of the SBR when there is one type of SBR, and mean the average styrene amount and average vinyl amount when there are multiple types of SBR. The average styrene amount of SBR can be calculated by {Σ(content of each SBR × styrene amount of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a styrene amount of 40% by mass and 5% by mass of SBR with a styrene amount of 25% by mass, the average styrene amount of the SBR is 39.2% by mass (=(85×40+5×25) / (85+5)). Similarly, the average vinyl content of SBR can be calculated by {Σ(content of each SBR × vinyl content of each SBR)} / total content of all SBRs. For example, when 100% by mass of the rubber component contains 85% by mass of SBR with a vinyl content of 30% by mass and 5% by mass of SBR with a vinyl content of 20% by mass, the average vinyl content of the SBR is 29.4% by mass (=(85×30+5×20) / (85+5)).
[0030] In 100% by mass of the rubber component, the content of SBR is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0031] The rubber composition contains a butadiene rubber (BR) as a rubber component. The BR is not particularly limited, and can be high cis content BR, low cis content BR, BR containing syndiotactic polybutadiene crystals, etc. Commercially available products include those from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc.
[0032] The cis amount (cis content) of BR is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, and is preferably 90% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. Within the above ranges, the effect tends to be better obtained. The cis content of BR can be measured by infrared absorption spectroscopy.
[0033] The above-mentioned cis amount of BR means the cis amount of the BR when there is one type of BR, and means the average cis amount when there are multiple types of BR. The average cis content of BR can be calculated by {Σ(content of each BR × cis content of each BR)} / total content of all BRs. For example, when 100% by mass of the rubber component contains 20% by mass of BR with a cis content of 90% by mass and 10% by mass of BR with a cis content of 40% by mass, the average cis content of BR is 73.3% by mass (=(20×90+10×40) / (20+10)).
[0034] In 100% by mass of the rubber component, the content of BR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. Within the above ranges, the effect tends to be better obtained.
[0035] Examples of rubber components that can be used other than SBR and BR include diene rubbers such as isoprene rubber, acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and styrene-isoprene-butadiene copolymer rubber (SIBR). These may be used alone or in combination of two or more.
[0036] The rubber component may be modified to introduce a functional group that interacts with a filler such as silica. Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.
[0037] Specific examples of compounds (modifiers) having the above-mentioned functional groups include 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, and the like.
[0038] The rubber composition contains silica. Examples of silica include dry silica (anhydrous silicic acid) and wet silica (hydrated silicic acid), but wet silica is preferred because it has a large number of silanol groups. Commercially available products include those from EVONIK, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Co., Ltd., etc. These may be used alone or in combination of two or more.
[0039] The cetyltrimethylammonium bromide (CTAB) specific surface area of the silica is preferably 160 m 2 / g or more, more preferably 180m 2 / g or more, more preferably 190m 2 / g or more, and preferably 250m 2 / g or less, more preferably 230m 2 / g or less, more preferably 210m 2 Within the above range, there is a tendency for the effect to be better obtained. The CTAB specific surface area of silica is measured in accordance with ASTM D3765-92.
[0040] The content of silica is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and even more preferably 50 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0041] The rubber composition contains carbon black. The carbon black is not particularly limited, and examples thereof include N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, and N762. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.
[0042] The cetyltrimethylammonium bromide (CTAB) specific surface area of the carbon black is preferably 110 m 2 / g or more, more preferably 120m 2 / g or more, more preferably 130m 2 / g or more, and preferably 180m 2 / g or less, more preferably 160m 2 / g or less, more preferably 150m 2 Within the above range, there is a tendency for the effect to be better obtained. The CTAB specific surface area of carbon black is a value measured in accordance with JIS K6217-3:2001.
[0043] The amount of carbon black is preferably 20 parts by mass or more, more preferably 35 parts by mass or more, and even more preferably 45 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 65 parts by mass or less, and even more preferably 55 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.
[0044] In the above rubber composition, the carbon black content is greater than the BR content.
[0045] The carbon black content / BR content is preferably 1.5 or more, more preferably 2.0 or more, and even more preferably 2.2 or more, and is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.0 or less. Within the above ranges, the effect tends to be better.
[0046] In these relationships, the carbon black content is the content (unit: parts by mass) relative to 100 parts by mass of the rubber component, and the BR content is the content (unit: % by mass) in 100% by mass of the rubber component.
[0047] From the viewpoint of overall performance such as dry steering stability and wet steering stability, it is preferable that the silica content in the rubber composition is greater than the carbon black content.
[0048] The silica content / carbon black content is preferably 1.1 or more, and is preferably 2.5 or less, more preferably 1.8 or less, and even more preferably 1.5 or less. Within the above range, the effect tends to be better.
[0049] In these relationships, the carbon black content and the silica content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0050] The rubber composition preferably contains a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl, mercapto-based compounds such as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane; vinyl-based compounds such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based compounds such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based compounds such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based compounds such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based compounds such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. As commercially available products, for example, products from Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azumax Co., Ltd., Toray Dow Corning Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, sulfide-based products are preferred.
[0051] The content of silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, even more preferably 8 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, even more preferably 10 parts by mass or less, based on 100 parts by mass of silica.When it is within the above range, the effect tends to be better obtained.
[0052] The rubber composition contains a resin component. Examples of the resin component include aromatic resins, terpene resins, etc. These may be used alone or in combination of two or more. Among these, aromatic resins are preferred.
[0053] An aromatic resin is a polymer containing an aromatic monomer as a constituent monomer, and examples of such a resin include a homopolymer obtained by polymerizing one type of aromatic monomer alone, a copolymer obtained by copolymerizing two or more types of aromatic monomers, and a copolymer of an aromatic monomer and another monomer that can be copolymerized with the aromatic monomer.
[0054] Examples of aromatic monomers include styrene monomers such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-methoxystyrene, p-tert-butylstyrene, p-phenylstyrene, o-chlorostyrene, m-chlorostyrene, and p-chlorostyrene; phenol monomers such as phenol, alkylphenol, and alkoxyphenol; naphthol monomers such as naphthol, alkylnaphthol, and alkoxynaphthol; coumarone, indene, etc. These may be used alone or in combination of two or more.
[0055] As the aromatic resin, a polymer containing a phenolic monomer as a constituent monomer (phenolic resin) or a polymer containing coumarone and indene as constituent monomers (coumarone-indene resin) is preferred, and a phenolic resin is more preferred, because these tend to produce better effects.
[0056] Examples of phenolic resins include phenol-aldehyde condensation resins obtained by reacting a phenolic monomer with an aldehyde such as formaldehyde, acetaldehyde, or furfural using an acid or alkali catalyst, phenol-alkyne condensation resins obtained by reacting a phenolic monomer with an alkyne such as acetylene, and modified phenolic resins obtained by modifying these resins with a compound such as cashew oil. Among these, phenol-alkyne condensation resins are preferred, and alkylphenol-acetylene condensation resins are more preferred.
[0057] Examples of commercially available resins that can be used include products from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nippon Paint Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Nippon Oil & Energy Corporation, Arakawa Chemical Industries, Ltd., and Taoka Chemical Co., Ltd.
[0058] The amount of the resin component (when a plurality of resins are used in combination, the total amount) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less. Within the above range, the effect tends to be better obtained.
[0059] In the above rubber composition, the relationship is: resin component content>|silica content−carbon black content|.
[0060] The resin component content / |silica content-carbon black content| is preferably 1.2 or more, more preferably 2.0 or more, even more preferably 3.0 or more, particularly preferably 3.5 or more, and is preferably 5.0 or less, more preferably 4.5 or less, even more preferably 4.0 or less. Within the above range, the effect tends to be better.
[0061] In these relationships, the resin component content, silica content, and carbon black content are amounts per 100 parts by mass of the rubber component (unit: parts by mass).
[0062] In the rubber composition, the resin component content / silica content is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more, and is preferably 1.2 or less, more preferably 0.8 or less, and even more preferably 0.6 or less. Within the above ranges, the effect tends to be better obtained. In this relationship, the resin component content and the silica content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0063] In the rubber composition, the resin component content / carbon black content is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more, and is preferably 1.2 or less, more preferably 0.8 or less, and even more preferably 0.6 or less. Within the above ranges, the effect tends to be better obtained. In this relationship, the resin component content and the carbon black content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.
[0064] The rubber composition contains an ethylene copolymer. The ethylene copolymer is a copolymer containing a structural unit (ethylene unit) derived from ethylene, and examples thereof include a copolymer of ethylene and an aromatic monomer (e.g., styrene), and a copolymer of ethylene, an aromatic monomer, and a conjugated diene monomer (e.g., 1,3-butadiene). Specific examples include an ethylene-styrene copolymer, an ethylene-styrene-butadiene copolymer, and the like, and as a commercially available product, a product from Struktol, etc. can be used. These may be used alone or in combination of two or more types. The ethylene copolymer is not included in the resin component.
[0065] In the ethylene copolymer, the ethylene unit may be formed by hydrogenating a structural unit derived from 1,3-butadiene (butadiene unit). That is, the ethylene copolymer may be a hydrogenated product of a (co)polymer having a butadiene unit.
[0066] As the ethylene copolymer, a copolymer having a structural unit derived from styrene (styrene unit) and a structural unit derived from 1,3-butadiene (butadiene unit) in addition to ethylene units is preferred, an ethylene-styrene-butadiene copolymer or a hydrogenated styrene-butadiene copolymer is more preferred, and a hydrogenated styrene-butadiene copolymer is even more preferred, because there is a tendency that the effect is more favorably obtained.
[0067] When the ethylene copolymer is a hydrogenated styrene-butadiene copolymer, the hydrogenation rate is preferably 30 mol% or more, more preferably 40 mol% or more, and even more preferably 50 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less, based on 100 mol% of the total butadiene units before hydrogenation. When it is within the above range, the effect tends to be better obtained. The hydrogenation rate is 1 It can be calculated from the spectral reduction rate of the unsaturated bond part of the spectrum obtained by measuring H-NMR.
[0068] The content of the ethylene copolymer is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, relative to 100 parts by mass of the rubber component, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. Within the above ranges, the effect tends to be better obtained.
[0069] In the above rubber composition, the content of BR is greater than the content of ethylene copolymer.
[0070] The BR content / ethylene copolymer is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, and is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. Within the above ranges, the effect tends to be better obtained.
[0071] In these relationships, the BR content is the content (unit: mass %) in 100% by mass of the rubber component, and the ethylene copolymer content is the content (unit: mass parts) relative to 100 parts by mass of the rubber component.
[0072] The rubber composition preferably contains SBR and / or BR that is soluble in acetone when immersed in acetone for 24 hours. In this specification, SBR and BR that are soluble in acetone when immersed in acetone for 24 hours refer to SBR and BR that are at least partially eluted into acetone when the above rubber composition after vulcanization is subjected to acetone extraction for 24 hours according to a method in accordance with JIS K 6229: 2015. Such SBR and BR are not included in the rubber component and resin component.
[0073] As the SBR or BR that is soluble in acetone when immersed in acetone for 24 hours, SBR or BR that is liquid at room temperature (25°C) (hereinafter also referred to as liquid SBR or liquid BR) can be used, and commercially available products such as those from Cray Valley and Kuraray Co., Ltd. can be used.
[0074] The weight average molecular weight (Mw) of SBR or BR (liquid SBR or liquid BR) that is soluble in acetone when immersed in acetone for 24 hours is preferably 9000 or less, more preferably 6000 or less, and even more preferably 4500 or less, and is preferably 100 or more, more preferably 1000 or more, and even more preferably 2000 or more. Within the above ranges, the effect tends to be better obtained.
[0075] The content of SBR or BR soluble in acetone when immersed in acetone for 24 hours (liquid SBR or liquid BR) is preferably 5 parts by mass or more, more preferably 8 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of the rubber component, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 15 parts by mass or less. Within the above ranges, the effect tends to be better obtained.
[0076] The rubber composition preferably contains a borate compound as a processing aid. Examples of borate compounds include alkali metal salts such as sodium borate and potassium borate, alkaline earth metal salts such as magnesium borate, and hydrates thereof. These may be used alone or in combination of two or more. Among these, alkali metal salts and hydrates thereof are preferred, sodium borate and hydrates thereof are more preferred, and sodium tetraborate decahydrate (borax) is even more preferred.
[0077] As commercially available borate compounds, products from Kishida Chemical Co., Ltd., Kenei Pharmaceutical Co., Ltd., etc. can be used.
[0078] The content of the borate compound is preferably 0.8 parts by mass or more, more preferably 1.2 parts by mass or more, even more preferably 1.5 parts by mass or more, and is preferably 4.5 parts by mass or less, more preferably 3.5 parts by mass or less, even more preferably 2.5 parts by mass or less. When the content is within the above range, the effect tends to be better.
[0079] The rubber composition may contain oil. Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., JXTG Nippon Oil & Energy Corporation, Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and the like. These may be used alone or in combination of two or more.
[0080] The content of the oil is preferably 15 parts by mass or more, more preferably 25 parts by mass or more, and even more preferably 30 parts by mass or more, and is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0081] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more.
[0082] The content of the antioxidant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.
[0083] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0084] The amount of the wax is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0085] The rubber composition may contain stearic acid. As the stearic acid, a conventionally known one can be used, and as a commercially available product, a product from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Corp., Chiba Fatty Acid Corp., etc. can be used. These may be used alone or in combination of two or more kinds.
[0086] The content of stearic acid is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.
[0087] The rubber composition may contain zinc oxide. As the zinc oxide, a conventionally known one can be used, and as a commercially available product, it is possible to use products from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0088] The amount of zinc oxide is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.
[0089] The rubber composition may contain sulfur. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are commonly used in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0090] The amount of sulfur is preferably 0.8 parts by mass or more, more preferably 1.2 parts by mass or more, and even more preferably 1.5 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.
[0091] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, and dibenzothiazolyl disulfide (MBTS); thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD) and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazolyl sulfenamide (TBBS), N-oxyethylene-2-benzothiazole sulfenamide, and N,N'-diisopropyl-2-benzothiazole sulfenamide; and guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine, and orthotolylbiguanidine. Commercially available products include products from Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.
[0092] The content of the vulcanization accelerator is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 4 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and even more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.
[0093] In addition to the above components, the rubber composition may further contain additives commonly used in the tire industry, such as organic peroxides, etc. The content of the additive is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.
[0094] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.
[0095] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.
[0096] The rubber composition can be used (as a rubber composition for tires) for tire components such as treads (cap treads), sidewalls, base treads, under treads, shoulders, clinches, bead apexes, breaker cushion rubbers, carcass cord covering rubbers, insulations, chafers, inner liners, and side reinforcing layers of run-flat tires. Among these, the rubber composition is particularly suitable for treads.
[0097] The tire of the present invention is produced by a conventional method using the above rubber composition. That is, the rubber composition is extruded in an unvulcanized state to match the shape of the tread, etc., and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is then heated and pressurized in a vulcanizer to obtain a tire.
[0098] The above tires (pneumatic tires, etc.) can be used for passenger car tires; truck and bus tires; motorcycle tires; high-performance tires; winter tires such as studless tires; run-flat tires with side reinforcing layers; tires with sound-absorbing material having a sound-absorbing material such as sponge in the tire cavity; tires with sealing material having a sealant inside or in the tire cavity that can seal in the event of a puncture; tires with electronic components having electronic components such as sensors and wireless tags inside or in the tire cavity, etc., and are suitable for passenger car tires.
[0099] The size of the tire is not particularly limited, and can be appropriately selected, for example, from a tire width in the range of 100 to 400 mm, an aspect ratio in the range of 25 to 85%, and a rim diameter in the range of 10 to 25 inches. Specific examples include 105 / 50R16, 115 / 50R17, 125 / 55R20, 135 / 45R21, 145 / 45R21, 155 / 45R18, 165 / 45R22, 175 / 45R23, 185 / 60R20, 195 / 55R14, 205 / 40R16, 215 / 40R16, 225 / 40R17, 235 / 40R17, 245 / 40R16, 255 / 40R17, 265 / 40R17, 275 / 35R18, 285 / 30R19, and 295 / 45R20. EXAMPLES
[0100] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0101] The various chemicals used in the examples and comparative examples will be described below.
[0102] (Rubber component) SBR1: Modified SBR synthesized in Production Example 1 below (styrene content: 25% by mass, vinyl content: 55% by mass, Mw: 450,000) SBR2: Modified SBR synthesized in Production Example 2 below (styrene content: 40% by mass, vinyl content: 30% by mass, Mw: 950,000) SBR3: Buna VSL5025-2 HM manufactured by LANXESS (styrene content: 25% by mass, vinyl content: 50% by mass, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) SBR4: Buna VSL 2438-2 HM manufactured by LANXESS (styrene content: 38% by mass, vinyl content: 24% by mass, contains 37.5 parts by mass of oil per 100 parts by mass of rubber solids) BR1: BR150B manufactured by Ube Industries, Ltd. (cis content: 97% by mass, vinyl content: 1% by mass) BR2: N103 manufactured by Asahi Kasei Chemicals Corporation (cis content: 38% by mass, vinyl content: 12% by mass)
[0103] (Chemicals other than rubber components) Carbon black: N134 (CTAB: 135m 2 / g) Silica 1: Ultrasil VN3 (CTAB: 165 m) manufactured by Evonik Degussa 2 / g) Silica 2: Rhodia Zeosil Premium 200MP (CTAB:203m 2 / g) Silane coupling agent: Si266 (bis(3-triethoxysilylpropyl) disulfide) manufactured by Evonik Degussa Liquid SBR: Ricon 100 (liquid SBR, Mw: 4500) manufactured by Cray Valley Resin 1: Nitto Chemical Co., Ltd. Knit Resin Kumarone V-120 (kumarone indene resin) Resin 2: Cholesin (pt-butylphenol-acetylene condensation resin) manufactured by BASF Oil: A / O Mix manufactured by Sankyo Yuka Kogyo Co., Ltd. Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Antioxidant 1: Nocrac 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Antioxidant 2: Nocrac RD (poly(2,2,4-trimethyl-1,2-dihydroquinoline)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Ethylene copolymer 1: Struktol 40MS (ethylene-styrene copolymer) manufactured by Struktol Ethylene copolymer 2: Hydrogenated product of Ricon 100 manufactured by Cray Valley (hydrogenated product of styrene-butadiene copolymer, hydrogenation rate: 50 mol%) Borate compound: Sodium tetraborate decahydrate manufactured by Kishida Chemical Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noccela CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Noccelaer D (diphenyl guanidine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0104] (Production Example 1) Cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. After adjusting the temperature of the reactor contents to 20°C, n-butyllithium was added to initiate polymerization. Polymerization was performed under adiabatic conditions, with the maximum temperature reaching 85°C. When the polymerization conversion reached 99%, 1,3-butadiene was added, and polymerization was continued for another 5 minutes, after which 3-diethylaminopropyltrimethoxysilane was added as a modifier to carry out the reaction. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and the mixture was dried with a heated roll adjusted to 110°C to obtain SBR1.
[0105] (Production Example 2) Cyclohexane, tetrahydrofuran, styrene, and 1,3-butadiene were charged into a nitrogen-substituted autoclave reactor. After adjusting the temperature of the reactor contents to 20°C, n-butyllithium was added to initiate polymerization. Polymerization was performed under adiabatic conditions, with the maximum temperature reaching 85°C. When the polymerization conversion reached 99%, 1,3-butadiene was added, and polymerization was continued for another 5 minutes, after which N,N-bis(trimethylsilyl)-3-aminopropyltriethoxysilane was added as a modifier to carry out the reaction. After the polymerization reaction was completed, 2,6-di-tert-butyl-p-cresol was added. Next, the solvent was removed by steam stripping, and the mixture was dried with a heated roll adjusted to 110°C to obtain SBR2.
[0106] Examples and Comparative Examples According to the composition shown in Table 1, materials other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the obtained kneaded product, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain an unvulcanized rubber composition. The obtained unvulcanized rubber composition was molded into a tread shape, and laminated together with other tire components to form an unvulcanized tire, which was press-vulcanized for 12 minutes at 150°C to produce a test tire (size: 175 / 60R18). The obtained test tire was used to perform the following evaluations, and the results are shown in Table 1. In Table 1, the rubber content in oil-extended rubber is listed in the rubber column, and the oil content in oil-extended rubber is added to the oil column.
[0107] (Dry steering stability) The lap time was measured when a vehicle fitted with the above test tires on all wheels ran 10 laps around a test course on a dry road surface. A reference tire with a longer lap time than any of the examples and comparative examples was also used to run under similar conditions. The difference in lap time between each example and comparative example and the reference tire was expressed as an index, with Comparative Example 3 being set at 100. The larger the index, the larger the difference from the lap time of the reference tire (reduction in lap time) and the better the dry steering stability (steering stability on a dry road surface).
[0108] (Wet driving stability) The lap time was measured when a vehicle fitted with the above test tires on all wheels ran 10 laps around a test course on a wet road surface. A reference tire with a longer lap time than any of the examples and comparative examples was also used to run under similar conditions. The difference in lap time between each example and comparative example and the reference tire was expressed as an index, with Comparative Example 4 being set at 100. The larger the index, the larger the difference from the lap time of the reference tire (reduction in lap time) and the more excellent the wet steering stability (steering stability on a wet road surface).
[0109] [Table 1]
[0110] As can be seen from Table 1, the Examples were superior to the Comparative Examples in the overall performance (total of each index) of the targeted dry steering stability and wet steering stability.
Claims
1. The rubber component includes a styrene-butadiene rubber and a butadiene rubber, silica, carbon black, a resin component A, and an ethylene copolymer that is a compound different from the resin component A, the content of the resin component A>|the content of the silica−the content of the carbon black|, the content of the carbon black is greater than the content of the butadiene rubber, The rubber composition for tires, wherein the content of the butadiene rubber is greater than the content of the ethylene copolymer.
2. 2. The rubber composition for tires according to claim 1, wherein the cis content of the butadiene rubber is 90% or less.
3. 3. The rubber composition for tires according to claim 1 or 2, which contains a styrene-butadiene rubber and / or a butadiene rubber which is soluble in acetone when immersed in acetone for 24 hours.
4. The rubber composition for tires according to any one of claims 1 to 3, wherein the content of said silica is greater than the content of said carbon black.
5. The cetyltrimethylammonium bromide specific surface area of the silica is 180 m 2 The rubber composition for tires according to any one of claims 1 to 4, wherein the viscosity is 1 / g or more.
6. The rubber composition for tires according to any one of claims 1 to 5, wherein the ethylene copolymer is a copolymer having ethylene units, styrene units and butadiene units.
7. The rubber composition for tires according to any one of claims 1 to 6, wherein the resin component contains a phenol-based resin.
8. A tire using the rubber composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Rubber composition for tread of tire
JP2007186567A
Rubber composition for tire tread
JP2014189698A
Rubber composition and pneumatic tire
JP2018016768A
Rubber composition and tire
JP2018035235A
Pneumatic tire
JP2019014796A