Metal products and their manufacturing methods
By integrating a Si and O-containing adhesion layer and Fe oxide layer between the steel base material and coating film, the adhesion and corrosion resistance of metal products are enhanced, addressing peeling issues in acidic environments.
Patent Information
- Application Number
- JP2021133633
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-08-18
AI Technical Summary
Existing metal products with coating films face issues with poor adhesion, leading to peeling, especially in acidic environments.
Incorporating a metal base material with a steel composition containing Si element, an adhesion layer with Si and O elements, and an oxide layer with Fe element oxide between the base material and the coating film, enhanced by plasma treatment and oxidation processes.
Improves the adhesion of the coating film, enhancing corrosion resistance and durability in acidic conditions.
Smart Images

Figure 0007574764000004 
Figure 0007574764000005 
Figure 0007574764000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal product and a method for producing the same. [Background technology]
[0002] Patent Document 1 discloses a fuel injection valve that injects fuel. The fuel injection valve includes a valve body in which a nozzle hole for injecting fuel is formed, and a valve element that opens and closes the nozzle hole. The valve body is a metal product made of a metal base material or the like. This valve body includes a metal base material, a coating film that covers the surface of the metal base material, and a mixed layer disposed between the metal base material and the coating film. The metal base material is a steel material, and the coating film is an oxide of aluminum. The mixed layer includes an Fe element, which is the same metal element as the main component of the metal base material, an Al element, which is the same metal element as the main component of the coating film, and an O element.
[0003] Patent Document 2 also discloses metal products such as blades and shafts that constitute the rotary compression element of a compressor. The metal product includes a metal substrate, a coating film that covers the surface of the metal substrate, and a compound layer disposed between the metal substrate and the coating film. When the coating layer is made of an oxide, the compound layer is made of an oxide of the same element as the main component of the metal substrate. That is, when the main component of the metal substrate is Fe, the compound layer contains Fe and O. When the coating layer is made of a nitride, the compound layer is made of a nitride of the same metal element as the main component of the metal substrate. That is, when the main component of the metal substrate is Fe, the compound layer contains Fe and N. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-206740 A [Patent Document 2] Japanese Patent Application Laid-Open No. 62-103368 Summary of the Invention [Problem to be solved by the invention]
[0005] In metal products having a coating film, it is desirable for the coating film to have high adhesion, that is, for the coating film to be resistant to peeling.
[0006] An object of the present invention is to provide a metal product and a manufacturing method thereof that can improve the adhesion of a coating film compared to the metal products of the above-mentioned prior art. [Means for solving the problem]
[0007] In order to achieve the above object, according to the invention described in claim 1, Metal products are A metal substrate (20) made of a steel material containing Si as a component and formed into a predetermined shape; A coating film (21) covering a surface of a metal substrate; An adhesion layer (22) disposed between the metal substrate and the coating film, in contact with the metal substrate, containing silicon and oxygen as components, for improving the adhesion of the coating film. and, an oxide layer (23) that is disposed between the metal substrate and the coating film and in contact with the coating film and contains an oxide of Fe; The Si element content of the adhesion layer is greater than the Si element content of the metal substrate and the oxide layer.
[0008] This makes it possible to improve the adhesion of the coating film compared to metal products of the prior art that do not have an adhesion layer containing Si and O elements as components.
[0009] In addition, claims 3 to According to the described invention, The manufacturing method of metal products is as follows: A preparation step (S1) of preparing a metal substrate (20) made of a steel material containing Si as a component and having a predetermined shape; After the preparation step, a coating film forming step (S4) is performed to form a coating film (21) covering the surface of the metal base material; After the preparation step and before the coating film formation step, a reduction treatment is performed by supplying a plasmatized reducing gas to the heated metal base material, and an adhesion layer (22) is formed in contact with the surface of the metal base material, containing Si and O elements as components, and for improving the adhesion of the coating film. and, an oxide layer forming step (S3) of performing an oxidation treatment in which the metal base material is heated in an oxidation gas atmosphere after the adhesion layer forming step and before the coating film forming step, to form an oxide layer (23) containing an oxide of Fe element on the surface of the adhesion layer; include.
[0010] According to this, a metal product is manufactured that has an adhesion layer containing elements Si and O between the metal substrate and the coating film, which adhesion layer improves the adhesion of the coating film compared to metal products of the prior art that do not have this adhesion layer.
[0011] Note that the reference symbols in parentheses attached to each component indicate an example of the correspondence between the component and specific components described in the embodiments described below. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view of a fuel injection valve according to an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of the valve body in FIG. [Diagram 3] FIG. 3 is an enlarged view of part III in FIG. [Figure 4] 4 is a flowchart showing a method for manufacturing a valve body. [Diagram 5] FIG. 2 is a cross-sectional view of a test specimen of Comparative Example 1. [Figure 6] FIG. 11 is a cross-sectional view of a test specimen of Comparative Example 2. [Figure 7] 1 is a graph showing the relationship between adhesion class and the Si content of the adhesion layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The fuel injection valve 10 of this embodiment shown in Fig. 1 injects fuel used for combustion in an internal combustion engine from a nozzle. The internal combustion engine is a compression autoignition type diesel engine, and is mounted on a vehicle as a driving source. Although not shown, fuel (e.g., diesel) stored in a fuel tank is pumped to a common rail by a high-pressure fuel pump, and then distributed from the common rail to each fuel injection valve 10, and injected from the fuel injection valve 10 into the combustion chamber of the internal combustion engine.
[0014] The fuel injection valve 10 includes a valve body 11 and a valve element 12 .
[0015] 1 and 2, a fuel passage 111 through which fuel distributed from a common rail flows is formed inside the valve body 11. A plurality of nozzle holes 112 for injecting fuel are formed on the tip side of the valve body 11. The plurality of nozzle holes 112 are connected to the fuel passage 111.
[0016] 1, the valve element 12 is housed in a fuel passage 111 of the valve body 11. The valve element 12 opens and closes a plurality of nozzle holes 112.
[0017] When the fuel injection valve 10 is installed in the internal combustion engine, the portion of the valve body 11 on the nozzle hole 112 side is exposed to the space of the combustion chamber of the internal combustion engine. When the temperature of the exhaust gas remaining in the combustion chamber drops after the internal combustion engine is stopped, condensed water formed by condensing water components contained in the exhaust gas may adhere to the valve body 11. Since the exhaust gas contains nitrogen and sulfur, the condensed water adhering to the valve body 11 also contains nitrogen and sulfur. Therefore, the condensed water is an acidic liquid. In this way, the portion of the valve body 11 on the nozzle hole 112 side is exposed to an acidic environment. For this reason, the portion of the valve body 11 on the nozzle hole 112 side is required to have corrosion resistance (i.e., corrosion resistance) against the acidic environment.
[0018] In this embodiment, the internal combustion engine has a function of reducing nitrogen oxides, which are subject to exhaust gas regulations, by recirculating a portion of the exhaust gas of the internal combustion engine to the intake air as recirculation gas. In recent years, there has been a tendency to increase the amount of recirculation gas in response to the strengthening of exhaust gas regulations. Since the recirculation gas contains sulfur and nitrogen, increasing the amount of recirculation gas causes more sulfur and nitrogen to dissolve in the condensed water adhering to the valve body 11. For this reason, the acidity of the condensed water is high, and the valve body 11 is required to have high corrosion resistance.
[0019] Therefore, in this embodiment, the valve body 11 has a structure including a metal base material 20 and a coating film 21, as shown in FIG.
[0020] The metal substrate 20 is made of a steel material containing silicon (Si element) as a component. Here, the steel material contains iron (Fe element) as a main component, and contains five other elements, namely, carbon (C element), silicon (Si element), manganese (Mn element), phosphorus (P element), and sulfur (S element). Carbon steel or alloy steel is used as the steel material. Carbon steel has a content of elements other than the above five elements that is less than a certain value. Alloy steel has a content of elements other than the above five elements that is equal to or greater than a certain value. An example of the alloy steel is chromium molybdenum steel (CrMo steel). The metal substrate 20 has a predetermined shape that is the shape of the valve body 11 shown in FIG. 2.
[0021] The coating film 21 is formed on the surface of the metal substrate 20 and covers the surface of the metal substrate 20. The coating film 21 is formed over the entire valve body 11, covering both the outer and inner surfaces of the valve body 11. The coating film 21 is a film for suppressing corrosion of the metal substrate 20 in an acidic environment. The coating film 21 is made of a material that is less susceptible to corrosion in an acidic environment than the metal substrate 20. Examples of such materials include oxides or nitrides of metal elements such as Al, Ta, Ti, Nb, and Hf.
[0022] Furthermore, the valve body 11 includes an adhesion layer 22 and an oxide layer 23 .
[0023] The adhesion layer 22 is a layer for improving the adhesion of the coating film 21. The adhesion layer 22 is disposed between the coating film 21 of the metal base material 20 and in contact with the metal base material 20. The adhesion layer 22 contains Si and O elements as components. The adhesion layer 22 contains Fe element which is the main component of the metal base material 20. The adhesion layer 22 may contain the same metal element as the component of the metal base material 20 as a component, in addition to Fe element.
[0024] The oxide layer 23, together with the adhesion layer 22, is a layer for improving the adhesion of the coating film 21. The oxide layer 23 is disposed between the coating film 21 of the metal base material 20 and in contact with the coating film 21. That is, the oxide layer 23 is disposed between the adhesion layer 22 and the coating film 21. The oxide layer 23 contains an oxide of Fe, which is the same element as the main component of the metal base material 20.
[0025] The valve body 11 may not have the oxide layer 23. In this case, the adhesion layer 22 is disposed between the metal base material 20 and the coating film 21, and in contact with both the metal base material 20 and the coating film 21.
[0026] Next, a description will be given of a method for manufacturing the valve body 11. As shown in Fig. 4, the method for manufacturing the valve body 11 includes a preparation step S1, a coating film forming step S4, an adhesion layer forming step S2, and an oxide layer forming step S3.
[0027] In the preparation step S1, a metal base 20 made of a steel material containing Si element as a component and shaped into a predetermined shape is prepared.
[0028] The coating film forming step S4 is performed after the preparation step S1. In the coating film forming step S4, a coating film 21 is formed to cover the surface of the metal base material 20. The coating film 21 is formed by atomic layer deposition (i.e., ALD: Atomic layer Deposition). The atomic layer deposition is a type of chemical vapor deposition method in which a source gas containing components of a desired thin film is supplied onto the surface of a heated material in an apparatus for forming the coating film 21, and a film is deposited by a chemical reaction on the surface or in the gas phase of the material. In the atomic layer deposition, atomic layers are formed discontinuously one by one.
[0029] The adhesion layer forming step S2 is performed after the preparation step S1 and before the coating film forming step S4. In the adhesion layer forming step S2, a reduction process is performed in which a plasmatized reducing gas is supplied to the heated metal substrate 20 in an apparatus for forming the coating film 21. As the reducing gas, a gas containing hydrogen atoms in its molecular structure, such as hydrogen (H2), ammonia (NH3), silane (SiH4), hydrazine (N2H4), etc., is used. In a state in which the reducing gas flows between two electrodes, a high-frequency high voltage is applied to the two electrodes to generate a discharge between the two electrodes, and the reducing gas is plasmatized. The reduction gas is plasmatized when the molecules of the reducing gas are ionized and separated into positive ions and electrons. The reduction gas is activated by being plasmatized, compared to when it is not plasmatized. For this reason, the reduction process time may be shorter than the processing time of the reduction process described in Patent Document 1. The reducing gas plasma impinges on the surface of the metal base 20, thereby forming an adhesion layer 22 in contact with the surface of the metal base 20 and containing Si elements and O elements as components.
[0030] The oxide layer forming step S3 is performed after the adhesion layer forming step S2 and before the coating film forming step S4. In the oxide layer forming step S3, an oxidation treatment is performed in which the metal substrate 20 is heated in an oxidation gas atmosphere in an apparatus for forming the coating film 21. As the oxidation gas, a gas containing oxygen atoms in its molecular structure, such as oxygen (O2) or water (H2O), is used. The oxidation gas may or may not be plasmatized. As a result, an oxide layer 23 containing an oxide of Fe element is formed on the surface of the adhesion layer 22.
[0031] After the oxide layer forming step S3, a coating film forming step S4 is performed, whereby a coating film 21 is formed on the surface of the oxide layer 23. If the valve body 11 does not have the oxide layer 23, the oxide layer forming step S3 is not performed. After the adhesion layer forming step S2, a coating film 21 is formed on the surface of the adhesion layer 22 by performing the coating film forming step S4.
[0032] As described above, according to the present embodiment, the valve body 11 includes the metal base material 20 and the coating film 21. As a result, the metal base material 20 is covered with the coating film 21, and thus corrosion of the metal base material 20 is suppressed.
[0033] Furthermore, an adhesion layer 22 and an oxide layer 23 are disposed between the metal substrate 20 and the coating film 21. Alternatively, of the adhesion layer 22 and the oxide layer 23, only the adhesion layer 22 is disposed between the metal substrate 20 and the coating film 21. This makes it possible to improve the adhesion of the coating film 21 compared to a valve body of the prior art that does not include the adhesion layer 22.
[0034] In this embodiment, the Si element content of the adhesion layer 22 is preferably larger than the Si element content of the metal base 20. This is because the adhesion of the coating film is improved compared to when the Si element content of the adhesion layer is smaller than the Si element content of the metal base.
[0035] (Other embodiments) (1) In the above embodiment, the coating film 21 is formed on both the outer surface and the inner surface of the valve body 11 over the entirety of the valve body 11. However, the coating film 21 does not have to be formed over the entirety of the valve body 11. It is sufficient that the coating film 21 is formed at least in a portion that requires corrosion resistance in an acidic environment.
[0036] (2) In each of the above-described embodiments, the fuel injection valve 10 having the valve body 11 to which the present invention is applied is mounted on an internal combustion engine having a function of recirculating a portion of exhaust gas to the intake air. However, the fuel injection valve 10 may be mounted on an internal combustion engine that does not have the recirculation function.
[0037] (3) In each of the above-described embodiments, the metal product to which the present invention is applied is the valve body 11 of the fuel injection valve 10. The metal substrate 20 has the shape of the valve body 11. However, the metal product to which the present invention is applied may be a metal product other than the valve body 11. The metal substrate 20 has a predetermined shape. In this case, it is preferable that the metal product is used in an acidic environment.
[0038] (4) The present invention is not limited to the above-described embodiments, and can be modified as appropriate within the scope of the claims, including various modified examples and modifications within the scope of equivalents. Furthermore, it goes without saying that in each of the above-described embodiments, the elements constituting the embodiments are not necessarily essential, except in cases where they are particularly clearly stated as essential or where they are clearly considered essential in principle. EXAMPLES
[0039] Example 1 In Example 1, an adhesion layer 22, an oxide layer 23, and a coating film 21 were formed in this order on the surface of a plate-shaped metal substrate 20 by the same method as the manufacturing method of the valve body 11 of the above-mentioned embodiment. Specifically, in a preparation step S1, a plate-shaped CrMo steel was prepared as the metal substrate 20. The prepared metal substrate 20 was subjected to the following treatments 1 to 4. Then, an evaluation test of adhesion of the coating film 21 was performed.
[0040] <Process 1> The metal substrate 20 was placed in an apparatus for forming the coating film 21, and the metal substrate 20 was heated in a vacuum created by a vacuum pump. The heating temperature was 300° C., which is the same temperature as that used for forming the coating film 21. At this time, oxygen remained in the apparatus, and thus an oxide layer containing an oxide of Fe element was formed on the surface of the metal substrate 20.
[0041] <Process 2> Next, a reduction treatment was performed in the adhesion layer forming step S2 to form the adhesion layer 22. In this reduction treatment, plasmatized ammonia gas was used. The reduction treatment time was 10 minutes. The heating temperature was 300°C, which is the same as the film formation temperature when forming the coating film 21.
[0042] <Process 3> Next, an oxidation treatment was performed in the oxide layer forming step S3 to form an oxide layer 23. In this oxidation treatment, oxygen gas in plasma form was used. The oxidation treatment time was 2 minutes. The heating temperature was 300° C., which is the same as the film formation temperature when forming the coating film 21.
[0043] <Process 4> Next, in the coating film formation step S4, the coating film 21 was formed by ALD. The formed coating film 21 was an oxide of Al element (i.e., alumina). The temperature of the metal base material 20 when the coating film 21 was formed was 300° C. The formed coating film 21 had a thickness of 40 nm.
[0044] <Adhesion evaluation test> The evaluation test was carried out using a Rockwell hardness test. That is, a Rockwell hardness test was carried out on the coating film 21, peeling near the edge of the indentation was analyzed, and the film was classified into one of six adhesion classes (HF1 to HF6) based on the German standard VDI3198. At this time, if there is little peeling or cracking around the indentation, the adhesion is judged to be good, and if there is large peeling or intersection of cracks, the adhesion is judged to be poor (see the literature below). C.-C. Chen and F. Chau-Nan Hong: Appl. Surf. Sci. 243(2005)296- 303.
[0045] Comparative Example 1 In Comparative Example 1, as shown in FIG. 5, an oxide layer 31 containing an oxide of Fe element and a coating film 21 were formed in this order on the surface of a metal substrate 20 by a method based on the manufacturing method described in Patent Document 1. In Comparative Example 1, the adhesion layer 22 of the present invention was not formed between the metal substrate 20 and the oxide layer 31. Specifically, in Comparative Example 1, similar to Example 1, a plate-shaped CrMo steel was prepared as the metal substrate 20, and the prepared metal substrate 20 was subjected to treatment 1. Thereafter, unlike Example 1, a reduction treatment was performed on the heated metal substrate 20 using ammonia gas that was not plasmatized. The reduction treatment time was 30 minutes. Thereafter, similar to Example 1, treatment 3 and treatment 4 were performed in order to form an oxide layer 31 and a coating film 21. The treatment 3 time was 10 minutes. Then, similar to Example 1, an evaluation test of adhesion was performed on the coating film 21.
[0046] Comparative Example 2 In Comparative Example 2, as shown in FIG. 6, an oxide layer 32 containing an oxide of Fe element and a coating film 21 were formed in this order on the surface of a metal substrate 20 to obtain the same structure as that described in Patent Document 2. In Comparative Example 2, the adhesion layer 22 of the present invention was not formed between the metal substrate 20 and the oxide layer 32. Specifically, in Comparative Example 2, similar to Example 1, a plate-shaped CrMo steel was prepared as the metal substrate 20, and the prepared metal substrate 20 was subjected to treatment 1 to form an oxide layer 32. Thereafter, treatments 2 and 3 of Example 1 were not performed, and treatment 4 of Example 1 was performed to form a coating film 21. Then, similar to Example 1, an evaluation test of adhesion was performed on the coating film 21.
[0047] (Results of Adhesion Evaluation Test for Example 1, Comparative Example 1, and Comparative Example 2) The adhesion class of Comparative Example 1 was HF5, the adhesion class of Comparative Example 2 was HF6, and the adhesion class of Example 1 was HF1. The smaller the adhesion class value, the better the adhesion. From these results, it was confirmed that the adhesion of Example 1 was higher than that of Comparative Examples 1 and 2, and that according to the present invention, it is possible to improve the adhesion of the coating film 21 compared to the conventional technology.
[0048] Example 2 In Example 2, similarly to Example 1, treatments 1 to 4 were performed on a plate-shaped CrMo steel as a metal substrate 20 to form coating films 21 of specimens A1 to A3, B1, C1, and C2. The times of treatments 2 and 3 were different in the formation of each specimen. Then, similarly to Example 1, an evaluation test of the adhesion of the coating film 21 of each specimen was performed. In addition, a quantitative analysis was performed on the adhesion layer 22 of each specimen. The quantitative analysis was performed by TEM-EDX (i.e., energy dispersive X-ray analysis). The apparatus and measurement conditions used are as follows: Equipment manufacturer: Hitachi High-Technologies Device name: HD-2700 Acceleration voltage: 200kV Magnification: 500,000x
[0049] In addition, the adhesion evaluation test of the coating film was also carried out for the specimens A4, B2, and C3 as comparative examples. The results of the adhesion evaluation test and the Si content of the adhesion layer 22 for each specimen are shown in FIG.
[0050] In the specimens A1 to A4 in FIG. 7, the oxidation treatment time in the treatment 3 was 10 minutes, and the thickness of the oxide layer was 30 nm. The reduction treatment time in the treatment 2 for the specimens A1 to A3 was 5 minutes for the specimen A1, 10 minutes for the specimen A2, and 60 minutes for the specimen A3. As can be seen by comparing the specimens A1 to A3 in FIG. 7, the shorter the reduction treatment time, the higher the Si content of the adhesion layer. The specimen A4 did not undergo treatment 2, and the adhesion layer 22 was not formed. For this reason, the specimen A4 is plotted at the position of 0 Si content in FIG. 7.
[0051] Tables 1 to 3 show the results of qualitative analysis of the metal substrate 20, the adhesion layer 22, and the oxide layer 23 of the specimen A1. The values in the tables show at% (i.e., atomic percentages), which indicate the proportion of the number of atoms of each element relative to the total atomic amount (100 atomic %) of the multiple elements listed in the tables.
[0052] [Table 1]
[0053] As shown in Table 1, the metal base 20 contains the element Si as a component. The metal base 20 used was made of CrMo steel, but the amount of Mo element was so small that it was not detected by TEM-EDX.
[0054] [Table 2]
[0055] As shown in Table 2, the adhesion layer 22 contained elements Si, O, and Fe as components. The content of Si in the adhesion layer 22 was greater than the content of Si in the metal base 20.
[0056] [Table 3]
[0057] As shown in Table 3, the oxide layer 23 contained, as its components, the O element and the Fe element, which is the same as the main component of the metal base material 20. The oxide layer 23 contained, as its other components, the Si element and the Mn element, which are the same as the components of the metal base material 20, and the Al element, which is the same as the components of the coating film 21.
[0058] The adhesion layer 22 and the oxide layer 23 have different Fe element contents, which makes it possible to distinguish between them in the TEM image.
[0059] In both specimens B1 and B2 in FIG. 7, the oxidation treatment time in treatment 3 was 2 minutes, and the thickness of the oxide layer was 12 nm. The reduction treatment time in treatment 2 for specimen B1 was 10 minutes. The adhesion layer 22 of specimen B1 contained Si elements. Specimen B2 was not subjected to treatment 2, and no adhesion layer 22 was formed. For this reason, specimen B2 is plotted at the position of 0 Si content in FIG. 7.
[0060] None of specimens C1 to C3 in FIG. 7 were subjected to treatment 3, and no oxide layer 23 was formed (i.e., no oxide layer). The reduction treatment time in treatment 2 was 10 minutes for specimen C1 and 60 minutes for specimen C2. The adhesion layers 22 of specimens C1 and C2 contained Si elements. As can be seen by comparing specimens C1 and C2 in FIG. 7, the shorter the reduction treatment time, the higher the Si content in the adhesion layer.
[0061] 7, the adhesion class values of specimens A1 to A3, B1, C1, and C2 were all smaller than those of specimens A4, B2, and C3. This confirmed that the formation of adhesion layer 22 containing Si element as a component improves adhesion compared to the case where adhesion layer 22 is not formed.
[0062] 7, when comparing specimens A1 to A4 with each other, specimens B1 and B2 with each other, or specimens C1 to C3 with each other, there was a tendency that the adhesion class value decreased and adhesion improved as the Si element content of adhesion layer 22 increased. From this, it can be seen that when the Si element content of adhesion layer 22 is greater than the Si element content of metal base material 20, the adhesion of coating film 21 is improved compared to when the Si element content of adhesion layer is smaller than the Si element content of metal base material 20. [Explanation of symbols]
[0063] 11 Valve body 20 Metal base material 21 Coating film 22 Adhesion layer 23 Oxide layer
Claims
1. A metal product, A metal substrate (20) made of a steel material containing Si as a component and having a predetermined shape; A coating film (21) covering the surface of the metal substrate; an adhesion layer (22) disposed between the metal substrate and the coating film in contact with the metal substrate, containing Si and O as components, and for improving adhesion of the coating film; and an oxide layer (23) disposed between the metal substrate and the coating film and in contact with the coating film, the oxide layer containing an oxide of Fe element; The content of Si element in the adhesion layer is higher than the content of Si element in the metal substrate and the oxide layer. metal products.
2. 2. The metal product according to claim 1, wherein the metal product is a valve body (11) of a fuel injection valve (10) that injects fuel used for combustion in an internal combustion engine, the valve body having a nozzle hole (112) for injecting fuel formed therein.
3. A method for manufacturing a metal product, comprising the steps of: A preparation step (S1) of preparing a metal substrate (20) made of a steel material containing Si as a component and having a predetermined shape; After the preparation step, a coating film forming step (S4) is performed to form a coating film (21) covering the surface of the metal base material; an adhesion layer forming step (S2) for forming an adhesion layer (22) for improving adhesion of the coating film, the adhesion layer (22) being in contact with the surface of the metal base and containing Si and O elements as components, the adhesion layer (22) being formed after the preparation step and before the coating film forming step; and an oxide layer forming step (S3) of performing an oxidation treatment of heating the metal base material in an oxidizing gas atmosphere after the adhesion layer forming step and before the coating film forming step, thereby forming an oxide layer (23) containing an oxide of Fe element on a surface of the adhesion layer.
Citation Information
Patent Citations
Ceramic coating metal
JP1987103368A
Metal coating method using low temperature plasma and electrodeposition
JP1995504943A
Surface coated member and manufacturing method thereof
JP2019206740A
Surface coated member and manufacturing method thereof
JP2019206741A