Energy Storage Devices

A film-like exterior member with a barrier layer and absorbent resin film addresses the challenges of shape diversity, weight reduction, and moisture/gas ingress in power storage devices, ensuring device performance.

JP7574974B2Active Publication Date: 2024-10-29DAI NIPPON PRINTING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024534400
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-12
Filing Date
2023-10-12
Publication Date
2024-10-29
Estimated Expiration
2043-10-12

AI Technical Summary

Technical Problem

Conventional metal exterior members for power storage devices are difficult to shape diversely, limit weight reduction, and expose the power storage device to moisture intrusion, leading to performance deterioration and gas generation.

Method used

A film-like exterior member with a barrier layer and a resin film containing a water and gas absorbent is used to seal the electrode body, preventing moisture ingress and absorbing generated gases.

Benefits of technology

The solution effectively suppresses moisture intrusion and absorbs gases like hydrogen sulfide, maintaining the performance of the power storage device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574974000001
    Figure 0007574974000001
  • Figure 0007574974000002
    Figure 0007574974000002
  • Figure 0007574974000003
    Figure 0007574974000003
Patent Text Reader

Abstract

This power storage device comprises an electrode body, an electrode terminal connected to the electrode body, and an exterior body that seals the electrode body. The exterior body is configured from a film-like exterior member and includes a first sealing portion joined to the exterior member in a state where the exterior member envelops the electrode body. The exterior member includes a barrier layer. The power storage device has a resin film for a power storage device disposed at least partially inwards of the barrier layer. The resin film for a power storage device includes at least one among a water absorbent and a gas absorbent.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electricity storage device. [Background technology]

[0002] Conventionally, various types of electricity storage devices have been developed, and in all electricity storage devices, exterior members are essential components for sealing electrode bodies such as electrodes and electrolytes. Conventionally, metal exterior members have been widely used as exterior members for electricity storage devices.

[0003] Meanwhile, in recent years, various shapes as well as thinner and lighter weight are required for electricity storage devices along with the increasing performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc. However, the metallic exterior members for electricity storage devices that have been widely used in the past have the drawbacks of being difficult to keep up with the diversification of shapes and also having limitations in terms of weight reduction.

[0004] In view of this, a film-like laminate in which a base layer / barrier layer / adhesive layer / thermally adhesive resin layer are laminated in this order has been proposed as an exterior material for an electricity storage device that can be easily processed into a variety of shapes and can be made thin and lightweight (see, for example, Patent Document 1).

[0005] In such exterior materials for electricity storage devices, recesses are generally formed by cold forming, and an electrode body such as an electrode and an electrolyte is placed in the space formed by the recess, and the heat-sealable resin layer is then heat-sealed to obtain an electricity storage device in which the electrode body is housed inside the exterior material for the electricity storage device. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2008-287971 A Summary of the Invention [Problem to be solved by the invention]

[0007] If moisture penetrates into the electrode body, the performance of the electricity storage device will deteriorate, so for example, when the above-mentioned film-like laminate is used as an exterior member, a barrier layer (for example, made of metal foil) is provided. By providing the barrier layer, it is possible to suppress the penetration of moisture from the outside of the barrier layer.

[0008] However, when the electrode body is sealed by heat-sealing the heat-sealable resin layer of the exterior member, the end faces of the heat-sealable resin layer are exposed to the outside, and there is a risk of moisture penetrating from the end faces of the heat-sealable resin layer.

[0009] Furthermore, if the heat-sealable resin layer of the exterior member absorbs water before the electrode body is sealed with the exterior member, there is a risk that the moisture in the heat-sealable resin layer will penetrate into the electrode body after the electrode body is sealed.

[0010] Furthermore, when the power storage device is an all-solid-state battery, if moisture comes into contact with a solid electrolyte contained in an element constituting the all-solid-state battery, gas such as hydrogen sulfide may be generated depending on the type of solid electrolyte.

[0011] An object of the present invention is to provide an electricity storage device that can achieve at least one of the following: suppressing the intrusion of moisture into the inside of an electrode assembly; and absorbing gas generated from the electrode assembly. [Means for solving the problem]

[0012] An electricity storage device according to a first aspect of the present invention comprises an electrode assembly, an electrode terminal connected to the electrode assembly, and an exterior body sealing the electrode assembly. The exterior body is formed of a film-like exterior member, and the exterior body includes a first sealing portion joined in a state in which the exterior member encases the electrode assembly. The exterior member includes a barrier layer. The electricity storage device has a resin film for an electricity storage device arranged at least partially inside the barrier layer. The resin film for an electricity storage device includes at least one of a water absorbing agent and a gas absorbing agent.

[0013] An electricity storage device according to a second aspect of the present invention is the electricity storage device according to the first aspect, wherein the resin film for an electricity storage device is used as a heat-sealable resin layer of the exterior member.

[0014] An electricity storage device according to a third aspect of the present invention is the electricity storage device according to the first or second aspect, wherein the resin film for an electricity storage device is used as an adhesive film for a terminal that joins the exterior member and the electrode terminal.

[0015] An electricity storage device according to a fourth aspect of the present invention is the electricity storage device according to any one of the first to third aspects, further comprising a lid body to which the electrode terminal is attached and which is arranged to the side of the electrode body, and a portion of the lid body is joined to the exterior member.

[0016] An electricity storage device according to a fifth aspect of the present invention is the electricity storage device according to the fourth aspect, wherein a material constituting the lid includes at least one of a resin material and a metal material.

[0017] An electricity storage device according to a sixth aspect of the present invention is the electricity storage device according to the fourth or fifth aspect, wherein the resin film for an electricity storage device is disposed at least partially between the lid body and the electrode body.

[0018] An electricity storage device according to a seventh aspect of the present invention is the electricity storage device according to any one of the fourth to sixth aspects, wherein the resin film for an electricity storage device is disposed at least partially between the lid and the electrode terminal.

[0019] An electricity storage device according to an eighth aspect of the present invention is the electricity storage device according to any one of the fourth to seventh aspects, wherein the resin film for an electricity storage device is disposed at least partially between the lid and the exterior member.

[0020] An electricity storage device according to a ninth aspect of the present invention is the electricity storage device according to any one of the fourth to eighth aspects, wherein the lid has a hole through which the electrode terminal passes, and the resin film for the electricity storage device is disposed in the hole.

[0021] An electricity storage device according to a tenth aspect of the present invention is an electricity storage device according to any one of the fourth to ninth aspects, wherein the lid body includes a first surface facing the electrode body and a second surface opposite to the first surface, and the resin film for electricity storage devices is joined to at least a portion of the second surface of the lid body. Effect of the Invention

[0022] According to the present invention, it is possible to provide an electricity storage device that can achieve at least one of suppressing the intrusion of moisture into the electrode body and absorbing hydrogen sulfide generated from the electrode body. [Brief description of the drawings]

[0023] [Figure 1A] FIG. 1 is a perspective view illustrating a power storage device according to a first embodiment. [Figure 1B] 1B is a cross-sectional view showing an example of a layer structure of the exterior member of FIG. 1A. [Diagram 2] FIG. 2 is a plan view illustrating a schematic diagram of the electricity storage device. [Diagram 3] FIG. 2 is a side view illustrating a schematic diagram of the electricity storage device. [Figure 4] 4 is a side view showing a state in which a sheath member is wrapped around an electrode body during manufacture of the electricity storage device according to the first embodiment. FIG. [Diagram 5] 13 is a view showing a state in which a packaging member is wrapped around an electrode body, as viewed from below, during the manufacture of the electricity storage device according to the first embodiment. FIG. [Figure 6] 6 is a diagram showing a schematic view of a part of a cross section taken along line VI-VI in FIG. 2. [Figure 7A] 11A to 11C are views for explaining a method of forming a second sealing portion. [Figure 7B] 6 is a cross-sectional view showing another example taken along line VI-VI in FIG. 2. [Figure 7C] 6 is a cross-sectional view showing still another example taken along line VI-VI in FIG. 2. [Figure 7D] 6 is a cross-sectional view showing still another example taken along line VI-VI in FIG. 2. [Figure 7E] 6 is a cross-sectional view showing still another example taken along line VI-VI in FIG. 2. [Figure 7F] 1 is a cross-sectional view showing an example of a layer structure of a resin film for an electricity storage device provided in the electricity storage device of the first embodiment. [Figure 7G] FIG. 4 is a cross-sectional view showing another example of the layer structure of the resin film for an electricity storage device provided in the electricity storage device of the first embodiment. [Figure 7H] FIG. 4 is a cross-sectional view showing still another example of the layer structure of the resin film for an electricity storage device provided in the electricity storage device of the first embodiment. [Figure 8] 5 is a flowchart showing a manufacturing procedure of the electricity accumulation device according to the first embodiment. [Figure 9] FIG. 11 is a plan view illustrating a schematic configuration of an electricity accumulation device according to a second embodiment. [Figure 10] FIG. 2 is a side view illustrating a schematic diagram of the electricity storage device. [Figure 11] FIG. 2 is a perspective view showing a typical cover body. [Figure 12] FIG. 13 is a diagram showing a first example in which a lid and an electrode terminal are integrally formed. [Figure 13] FIG. 13 is a diagram showing a second example in which the cover and the electrode terminal are integrally formed. [Figure 14] 10 is a flowchart showing a manufacturing procedure of the electricity accumulation device according to the second embodiment. [Figure 15] 10 is a flowchart showing another manufacturing procedure for the electricity storage device according to the second embodiment. [Figure 16] FIG. 11 is a side view showing a state in which a sheath member is wrapped around an electrode body in a third embodiment. [Figure 17] FIG. 11 is a diagram showing a state in which an exterior member is wrapped around an electrode body and a lid body is attached to the exterior member, as viewed from below, in a third embodiment. [Figure 18]13 is a flowchart showing a manufacturing procedure of the electricity accumulation device according to the third embodiment. [Figure 19] FIG. 13 is a plan view illustrating a power storage device according to a fourth embodiment. [Figure 20] FIG. 13 is a side view diagrammatically illustrating an electricity accumulation device according to a fourth embodiment. [Figure 21] FIG. 11 is a side view showing a state in which an exterior member is wrapped around an electrode body in a modified example. [Figure 22] FIG. 13 is a perspective view illustrating a modified example of an electricity storage device. [Diagram 23] 13 is a perspective view showing a modified example of a cover and an electrode terminal attached to the cover. FIG. [Figure 24] 13A to 13C are diagrams illustrating an insertion step in a manufacturing method for an electricity accumulation device according to a modified example. [Diagram 25] 13 is a perspective view showing a modified example of a cover and an electrode terminal attached to the cover. FIG. [Figure 26] FIG. 24 is a perspective view that illustrates a schematic diagram of an electricity accumulation device to which the lid of FIG. 23 is attached. [Figure 27] FIG. 13 is a front view showing a schematic diagram of a cover according to another modified example. [Figure 28] FIG. 13 is a front view showing a schematic diagram of a cover according to still another modified example. [Figure 29A] 6 is a cross-sectional view showing an example of the arrangement of a resin film for an electricity storage device in an electricity storage device according to a second embodiment. FIG. [Figure 29B] 29B is a cross-sectional view showing another example of the arrangement of the electricity storage device resin film in the electricity storage device of FIG. 29A. [Figure 29C] 29B is a cross-sectional view showing still another example of arrangement of the electricity storage device resin film in the electricity storage device of FIG. 29A. [Diagram 30] FIG. 11 is a plan view illustrating a schematic diagram of an electricity storage device according to another modified example. [Diagram 31] 13 is a side view showing a state in which a sheath member is wrapped around an electrode body during the manufacture of an electricity storage device according to another modified example. FIG. [Diagram 32] FIG. 32 is an enlarged view of a portion X in FIG. [Diagram 33]FIG. 11 is a cross-sectional view of an electricity storage device according to a modified example. [Diagram 34] FIG. 11 is a cross-sectional view of an electricity storage device according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. In addition, the same or corresponding parts in the drawings are given the same reference numerals, and the description thereof will not be repeated. In this embodiment, a numerical range indicated by "~" means "more than or equal to" or "less than or equal to". For example, the notation 2 to 15 mm means 2 mm or more and 15 mm or less. In the numerical ranges described in stages in this embodiment, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, the upper limit and upper limit, the upper limit and lower limit, or the lower limit and lower limit described separately may be combined to form a numerical range.

[0025] [1. First embodiment] <1-1. Configuration of the power storage device> Fig. 1A is a perspective view that typically shows an electricity storage device 10 according to a first embodiment. Fig. 2 is a plan view that typically shows the electricity storage device 10. Fig. 3 is a side view that typically shows the electricity storage device 10. In each of Figs. 2 and 3, the direction of arrows UD indicates the thickness direction of the electricity storage device 10, and the direction of arrows LR indicates the width direction of the electricity storage device 10. Furthermore, the direction of arrows FB indicates the depth direction of the electricity storage device 10. The directions indicated by the arrows UDLRFB are common to the subsequent figures.

[0026] 1A, 1B, 2 and 3, the electricity storage device 10 includes an electrode body 200, an exterior body 100, and a plurality (two) of electrode terminals 300. The electrode body 200 includes electrodes (positive and negative electrodes) and separators constituting an electricity storage member such as a lithium ion battery, a capacitor, or an all-solid-state battery. The shape of the electrode body 200 is a substantially rectangular parallelepiped. Note that the term "substantially rectangular parallelepiped" includes not only a perfect rectangular parallelepiped, but also a solid body that can be regarded as a rectangular parallelepiped by modifying the shape of a portion of the outer surface, for example.

[0027] The electrode terminal 300 is a metal terminal used for inputting and outputting electric power in the electrode body 200. One end of the electrode terminal 300 is electrically connected to an electrode (positive electrode or negative electrode) included in the electrode body 200, and the other end protrudes outward from an edge of the exterior body 100.

[0028] The metal material constituting the electrode terminal 300 is, for example, aluminum, nickel, copper, etc. For example, when the electrode body 200 is a lithium ion battery, the electrode terminal 300 connected to the positive electrode is usually made of aluminum or the like, and the electrode terminal 300 connected to the negative electrode is usually made of copper, nickel, etc.

[0029] The exterior body 100 is composed of a film-like exterior member 101 (FIG. 4, etc.) and seals the electrode body 200. In the electricity storage device 10, the exterior body 100 is formed by wrapping the exterior member 101 around the electrode body 200 and sealing the open portion.

[0030] For example, there is a method of forming a storage portion (recess) for storing the electrode body 200 in the exterior member 101 through cold forming. However, it is not necessarily easy to form a deep storage portion by such a method. If an attempt is made to form a deep storage portion (recess) (for example, a forming depth of 15 mm) through cold forming, there is a high possibility that pinholes or cracks will occur in the exterior member, leading to a decrease in battery performance. On the other hand, since the exterior member 101 is wrapped around the electrode body 200 to seal the electrode body 200, the electrode body 200 can be easily sealed regardless of the thickness of the electrode body 200. Note that in order to reduce the dead space between the electrode body 200 and the exterior member 101 so as to improve the volumetric energy density of the electricity storage device 10, it is preferable that the exterior member 101 is wrapped so as to come into contact with the outer surface of the electrode body 200. Moreover, in an all-solid-state battery, it is necessary to apply a high pressure uniformly from the outer surface of the battery in order to exert battery performance, and therefore it is necessary to eliminate the space between the electrode body 200 and the exterior member 101. Therefore, it is preferable that the exterior member 101 is wrapped around the electrode body 200 so as to be in contact with the outer surface of the electrode body 200.

[0031] 1B is a cross-sectional view showing an example of the layer structure of the exterior member 101. The exterior member 101 is, for example, a laminate 101Z (laminate film) having a base layer 101A, a barrier layer 101B, and a heat-sealable resin layer 101C in this order. Note that the exterior member 101 does not need to include all of these layers, and for example, the base layer 101A may not be included. Note that the exterior member 101 is preferably heat-sealable.

[0032] The base material layer 101A included in the exterior member 101 is a layer for imparting heat resistance to the exterior member 101 and suppressing the occurrence of pinholes that may occur during processing or distribution. The base material layer 101A is configured to include at least one layer of a stretched polyester resin layer and a stretched polyamide resin layer. For example, the base material layer 101A includes at least one layer of a stretched polyester resin layer and a stretched polyamide resin layer, so that the barrier layer 101B can be protected during processing of the exterior member 101 and breakage of the exterior member 101 can be suppressed. In addition, from the viewpoint of increasing the tensile elongation of the exterior member 101, the stretched polyester resin layer is preferably a biaxially stretched polyester resin layer, and the stretched polyamide resin layer is preferably a biaxially stretched polyamide resin layer. Furthermore, in terms of excellent puncture strength or impact strength, the stretched polyester resin layer is more preferably a biaxially stretched polyethylene terephthalate (PET) film, and the stretched polyamide resin layer is more preferably a biaxially stretched nylon (ONy) film. The base layer 101A may be configured to include both a stretched polyester resin layer and a stretched polyamide resin layer. From the viewpoint of film strength, the thickness of the base layer 101A is preferably, for example, 5 to 300 μm, and more preferably 20 to 150 μm.

[0033] Moreover, the barrier layer 101B included in the exterior member 101 is composed of, for example, a metal foil from the viewpoint of processability such as moisture resistance and ductility, and cost. Specifically, aluminum, steel plate, stainless steel, or the like can be used as the metal foil. Moreover, the metal foil preferably contains iron from the viewpoint of packaging suitability and pinhole resistance when packaging the electrode body 200. The iron content in the metal foil is preferably 0.5 to 5.0 mass %, and more preferably 0.7 to 2.0 mass %. By making the iron content 0.5 mass % or more, the exterior member 101 can obtain packaging suitability, excellent pinhole resistance, and ductility. Furthermore, by making the iron content 5.0 mass % or less, the exterior member 101 can obtain excellent flexibility.

[0034] From the viewpoints of barrier properties, pinhole resistance, and packaging suitability, the thickness of the barrier layer 101B is preferably, for example, 15 to 100 μm, and more preferably 30 to 80 μm. When the thickness of the barrier layer 101B is 15 μm or more, the exterior member 101 is less likely to break even when stress is applied during packaging processing. When the thickness of the barrier layer 101B is 100 μm or less, an increase in the mass of the exterior member 101 can be reduced, and a decrease in the weight energy density of the electricity storage device 10 can be suppressed.

[0035] In addition, when the barrier layer 101B is a metal foil, it is preferable to provide a corrosion-resistant film at least on the surface opposite to the base layer 101A to prevent dissolution and corrosion. The barrier layer 101B may have a corrosion-resistant film on both sides. Here, the corrosion-resistant film refers to a thin film that is provided with corrosion resistance (e.g., acid resistance, alkali resistance, etc.) on the barrier layer 101B by performing, for example, hydrothermal conversion treatment such as boehmite treatment, chemical conversion treatment, anodizing treatment, plating treatment such as nickel or chromium, or corrosion prevention treatment by applying a coating agent on the surface of the barrier layer 101B. Specifically, the corrosion-resistant film refers to a film that improves the acid resistance of the barrier layer 101B (acid-resistant film), a film that improves the alkali resistance of the barrier layer 101B (alkali-resistant film), etc. The treatment for forming the corrosion-resistant film may be one type, or two or more types may be combined. In addition, not only one layer but also multiple layers may be formed. Furthermore, among these treatments, hydrothermal conversion treatment and anodizing treatment are treatments in which the metal foil surface is dissolved by a treatment agent to form a metal compound with excellent corrosion resistance. Note that these treatments may be included in the definition of chemical conversion treatment. In addition, when the barrier layer 101B has a corrosion-resistant coating, the corrosion-resistant coating is also included in the barrier layer 101B.

[0036] The corrosion-resistant coating prevents delamination between the barrier layer 101B (e.g., aluminum alloy foil) and the base layer 101A during molding of the exterior member 101, and prevents dissolution and corrosion of the surface of the barrier layer 101B due to hydrogen fluoride produced by a reaction between an electrolyte and moisture, particularly when the barrier layer 101B is an aluminum alloy foil, dissolution and corrosion of aluminum oxide present on the surface of the barrier layer 101B. The corrosion-resistant coating further improves the adhesion (wettability) of the surface of the barrier layer 101B, and exhibits the effect of preventing delamination between the base layer 101A and the barrier layer 101B during heat sealing, and between the base layer 101A and the barrier layer 101B during molding of the exterior member 101.

[0037] The thermally adhesive resin layer 101C included in the exterior member 101 is a layer that imparts heat sealing properties to the exterior member 101. Examples of the thermally adhesive resin layer 101C include a resin film made of a polyolefin resin or an acid-modified polyolefin resin obtained by graft-modifying a polyolefin resin with an acid such as maleic anhydride. From the viewpoints of sealing properties and strength, the thickness of the thermally adhesive resin layer 101C is preferably, for example, 20 to 300 μm, and more preferably 40 to 150 μm.

[0038] If the heat-sealable resin layer 101C is too hard, when the roll material or the exterior member 101 is bagged into the exterior body 100 by the device, it may slip at the contact point with the device and may not be transported properly. In addition, if the exterior member 101 is scratched by the friction, the heat-sealable resin layer 101C may be damaged. Since damage to the heat-sealable resin layer 101C may reduce the heat seal strength, it is preferable that the heat-sealable resin layer has a moderately slippery property. For this reason, when a non-slip or non-slip material is used as the material constituting the heat-sealable resin layer 101C, it is preferable to add a lubricant from the viewpoint of transportability.

[0039] Furthermore, from the viewpoint of contamination resistance and processability, the thermally adhesive resin layer 101C preferably has a tensile modulus of elasticity measured in accordance with the provisions of JIS K7161: 2014 in the range of 500 MPa to 1000 MPa. A more preferred range for the tensile modulus of elasticity of the thermally adhesive resin layer 101C is 500 MPa to 800 MPa, an even more preferred range is 500 MPa to 750 MPa, an even more preferred range is 500 MPa to 700 MPa, and an even more preferred range is 510 MPa to 700 MPa.

[0040] Since the thermally adhesive resin layer 101C has a tensile modulus of 500 MPa or more, contamination of the device during molding and transportation of the exterior body 100 is effectively suppressed. That is, since the thermally adhesive resin layer 101C has a tensile modulus of 500 MPa or more, the lubricant located on the surface of the thermally adhesive resin layer 101C is not easily scraped off by the device, etc., so that the lubricant located on the surface portion of the thermally adhesive resin layer 101C is not easily transferred to the device, etc., and contamination of the device, etc. is effectively suppressed. Furthermore, since the thermally adhesive resin layer 101C has a tensile modulus of 1000 MPa or less, high sealing strength is exerted by heat fusion. That is, since the thermally adhesive resin layer 101C has a tensile modulus of 1000 MPa or less, the thermally adhesive resin layer 101C is not easily brittle, so high sealing strength is exerted by heat fusion. If the tensile modulus of the thermally adhesive resin layer 101C exceeds 1000 MPa, the thermally adhesive resin layer 101C becomes brittle and is easily peeled off from the barrier layer 101B laminated via an adhesive layer, resulting in a decrease in seal strength, or the stretching at the folded portion during molding of the exterior body 100 may cause whitening or cracks in the stretched portion, resulting in a decrease in battery performance. If the tensile modulus of the thermally adhesive resin layer 101C exceeds 1000 MPa, the extrudability decreases, which is a factor in decreasing productivity. Therefore, in the exterior member 101 of the power storage device 10 of this embodiment, by setting the tensile modulus of the thermally adhesive resin layer 101C to a range of 500 to 1000 MPa, the effect of suppressing contamination of the device and the like and the effect of improving the seal strength by heat fusion are suitably exhibited. Note that the tensile modulus of the thermally adhesive resin layer 101C can be adjusted by adjusting the molecular weight, melt mass flow rate (MFR), etc. of the resin constituting the thermally adhesive resin layer 101C.

[0041] Furthermore, when the work of butting together the sealed portions for pillow sealing when making a bag of the exterior body 100, the work of folding, etc., is called processing, the same problems as described above occur during the processing. Since the exterior member 101 is particularly susceptible to damage during processing, solving the above problems is important. By setting the tensile modulus of elasticity of the heat-fusible resin layer 101C in the range of 500 MPa or more and 1000 MPa or less, processing can be performed satisfactorily.

[0042] It is preferable that the exterior member 101 has one or more layers having a buffer function (hereinafter referred to as "buffer layer") on the outer side of the thermally adhesive resin layer 101C (upper side in FIG. 1B), more preferably on the outer side of the barrier layer 101B. The buffer layer may be laminated on the outer side of the base layer 101A, or the base layer 101A may also function as a buffer layer. When the exterior member 101 has multiple buffer layers, the multiple buffer layers may be adjacent to each other, or may be laminated via the base layer 101A, the barrier layer 101B, etc.

[0043] The material constituting the buffer layer can be arbitrarily selected from materials having cushioning properties. The material having cushioning properties is, for example, rubber, nonwoven fabric, or foam sheet. The rubber is, for example, natural rubber, fluororubber, or silicone rubber. The rubber hardness is preferably about 20 to 90. The material constituting the nonwoven fabric is preferably a material having excellent heat resistance. When the buffer layer is made of nonwoven fabric, the lower limit of the thickness of the buffer layer is preferably 100 μm, more preferably 200 μm, and more preferably 1000 μm. When the buffer layer is made of nonwoven fabric, the upper limit of the thickness of the buffer layer is preferably 5000 μm, and more preferably 3000 μm. The thickness of the buffer layer is preferably in the range of 100 μm to 5000 μm, 100 μm to 3000 μm, 200 μm to 5000 μm, 200 μm to 3000 μm, 1000 μm to 5000 μm, or 1000 μm to 3000 μm. Among these, the thickness of the buffer layer is most preferably in the range of 1000 μm to 3000 μm.

[0044] When the buffer layer is made of rubber, the lower limit of the thickness of the buffer layer is preferably 0.5 mm. When the buffer layer is made of rubber, the upper limit of the thickness of the buffer layer is preferably 10 mm, more preferably 5 mm, and more preferably 2 mm. When the buffer layer is made of rubber, the preferred range of the thickness of the buffer layer is 0.5 mm to 10 mm, 0.5 mm to 5 mm, or 0.5 mm to 2 mm.

[0045] When the exterior member 101 has a buffer layer, the buffer layer functions as a cushion, thereby preventing the exterior member 101 from being damaged by impact when the energy storage device 10 is dropped or by handling during the manufacture of the energy storage device 10.

[0046] Since the exterior body 100 of this embodiment can form a deep housing portion, the weight of the electrode body 200 increases, and the attack on the exterior body 100 due to impact or the like becomes large. For this reason, in this embodiment, when the thickness of the exterior member 101 is 195 μm or less and the thickness of the barrier layer 101B is included in the range of 20 to 85 μm, the puncture strength when pierced from the base layer 101A side of the exterior member 101, measured by a method conforming to the provisions of JIS Z1707:1997, is preferably 30 N or more. Examples of preferable ranges of the puncture strength include about 30 to 45 N, about 30 to 40 N, about 35 to 45 N, and about 35 to 40 N. The puncture strength of the exterior member 101 is measured as follows.

[0047] The puncture strength from the base layer 101A side of the exterior member 101 is measured by a method conforming to the provisions of JIS Z1707:1997. Specifically, in a measurement environment of 23±2°C and relative humidity (50±5)%, a test piece is fixed with a 115mm diameter table and a presser plate having a 15mm diameter opening in the center, and a semicircular needle with a diameter of 1.0mm and a tip radius of 0.5mm is pierced at a speed of 50±5mm per minute, and the maximum stress until the needle penetrates is measured. The number of test pieces is five, and the average value is calculated. If the number of test pieces is insufficient to measure five, the number that can be measured is measured, and the average value is calculated. As a measuring device for the puncture strength, Imada's ZP-500N (force gauge) and MX2-500N (measurement stand) can be used.

[0048] In the electricity storage device 10 of this embodiment, as the electrode body 200 becomes heavier, friction between the electricity storage devices 10, friction between the electricity storage device 10 and peripheral members, and friction during transportation of the electricity storage device 10 are likely to occur. For this reason, in this embodiment, in addition to good fixation of the ink (good printing characteristics) on the surface of the base material layer 101A side of the exterior member 101, it is preferable that the fixed ink is not easily lost. From this viewpoint, it is preferable that the contact angle of the surface of the base material layer 101A side of the exterior member 101 of this embodiment is 80° or less. That is, when the base material layer 101A constitutes the outermost surface of the exterior member 101, the contact angle of the surface of the base material layer 101A is 80° or less. Furthermore, when a coating layer is provided on the outside of the base material layer 101A, the contact angle of the surface of the coating layer is 80° or less. In this embodiment, since the contact angle of the surface of the exterior member 101 on the base layer 101A side is 80° or less, ink is not easily repelled on the surface on the base layer 101A side, the printing characteristics are excellent, and the fixed ink is not easily lost. In particular, when ink is printed by pad printing on the exterior member 101 in which a lubricant is present on the surface on the base layer 101A side to enhance formability, the ink may be repelled on the surface on the base layer 101A side, resulting in printing defects. However, even in such a case, the exterior member 101 of the electricity storage device 10 of this embodiment has a contact angle of 80° or less on the surface on the base layer 101A side, so that the ink is not easily repelled, and the exterior member 101 is particularly suitable as an exterior member 101 on which printing or the like is formed on the surface of the base layer 101A by pad printing.

[0049] In this embodiment, from the viewpoint of improving printability and making the fixed ink less likely to disappear, the contact angle of the surface on the substrate layer 101A side is more preferably 79° or less, and even more preferably 72° or less. The contact angle of the surface on the substrate layer 101A side can be determined by measuring the contact angle of the interface between the substrate and the water droplet 5 seconds after the water droplet is applied using LSE-A210 manufactured by NIC Corporation.

[0050] In this embodiment, the contact angle of the surface on the base layer 101A side can be suitably set to 80° or less, for example, by subjecting the surface on the base layer 101A side to a corona treatment. The corona treatment can be performed by irradiating the surface on the base layer 101A side with a corona discharge using a commercially available corona surface treatment device. The corona treatment conditions are, for example, treating the surface on the base layer 101A side with an irradiation output of 1 Kw or more at a speed of 10 MT / min, thereby making it possible to make the contact angle of the surface on the base layer 101A side 80° or less.

[0051] In addition, when printing ink on the surface of the exterior member 101, a corona treatment is performed, and then a step of printing ink on at least a part of the surface of the base material layer 101A is performed. The printing method is not particularly limited, but inkjet printing and pad printing are preferable when printing on the exterior member 101 after molding. Since the contact angle of the surface of the base material layer 101A side of the exterior member 101 of the electricity storage device 10 of this embodiment is set to 80° or less, ink can be suitably printed even by pad printing, in which ink is easily repelled by the base material layer 101A having a lubricant on the surface. Therefore, for example, barcodes, patterns, characters, and the like can be suitably printed on at least a part of the surface of the base material layer 101A.

[0052] FIG. 4 is a side view showing a state in which the exterior member 101 is wound around the electrode body 200 during the manufacturing process of the electricity storage device 10. As shown in FIG. 4, the exterior member 101 is wound around the electrode body 200. In this case, the outermost layer of the electrode body 200 does not necessarily need to be an electrode, and may be, for example, a protective tape or a separator. With the exterior member 101 wound around the electrode body 200, the surfaces (thermally adhesive resin layers) of the exterior member 101 facing each other are heat-sealed to form a first sealing portion 110. The first sealing portion 110 may be formed by joining the innermost layer and the outermost layer of the exterior member 101. In this case, the innermost layer and the outermost layer of the exterior member 101 are preferably heat-sealed resin layers 101C.

[0053] The root portion of the first sealing portion 110 is preferably located on a side 135 of the exterior body 100. In this embodiment, the side 135 is formed at the boundary between the first surface 130 and the second surface 140, which has a smaller area than the first surface 130. That is, in this embodiment, the root portion of the first sealing portion 110 can be said to be formed at the boundary between the first surface 130 and the second surface 140, and can be said to be not present on either the first surface 130 or the second surface 140. The root portion of the first sealing portion 110 may be located at a position other than the side 135. In the power storage device 10, the first sealing portion 110 is folded toward the second surface 140 with the side 135 as the center. In the power storage device 10, the first sealing portion 110 is in contact with the second surface 140 and covers substantially the entire second surface 140. Note that "substantially the entire second surface 140" means a region that occupies 75% or more of the area of ​​the second surface 140.

[0054] That is, in the electricity storage device 10, the first sealing portion 110 is not formed on the first surface 130 having a large area. The first surface 130 is flatter than when a sealing portion such as the first sealing portion 110 is in contact with the first surface 130. Therefore, even if another electricity storage device 10 is placed on the first surface 130, the other electricity storage device 10 does not tilt. As a result, according to the electricity storage device 10, when a plurality of electricity storage devices 10 are stacked, unevenness in the distribution of pressure applied to the lower electricity storage device 10 can be suppressed. In other words, when a module is formed by stacking a plurality of electricity storage devices 10, the first sealing portion 110 is not disposed on the surface (first surface 130) adjacent to the adjacent electricity storage device 10. In addition, such a configuration is preferable from the viewpoint that it is necessary to apply a high pressure uniformly from the outer surface of the battery in an all-solid-state battery to exhibit battery performance.

[0055] Furthermore, in the power storage device 10, a root portion of the first sealing portion 110 is on a side 135 of the exterior body 100. Therefore, according to the power storage device 10, a wider bonding area can be secured in the first sealing portion 110 compared to when the root portion of the first sealing portion 110 is on the second surface 140 (for example, the central portion of the second surface 140 in the direction of the arrow UD). Note that the bonding area of ​​the first sealing portion 110 does not necessarily need to be the entire area of ​​the first sealing portion 110, and may be a part of the first sealing portion 110, such as only the vicinity of the root portion of the first sealing portion 110.

[0056] Furthermore, in the power storage device 10, substantially the entire second surface 140 is covered by the first sealing portion 110. That is, in the power storage device 10, the length of the first sealing portion 110 in the direction of the arrow UD is longer than in the case where the first sealing portion 110 covers only half or less of the area of ​​the second surface 140 (see FIG. 3). Therefore, according to the power storage device 10, a wide bonding area can be secured in the first sealing portion 110. Furthermore, since substantially the entire second surface 140 is covered by the first sealing portion 110, the power storage device 10 is stable even if the power storage device 10 is placed upright so that the second surface 140 is in contact with the mounting surface. That is, the power storage device 10 is unlikely to tilt with respect to the mounting surface. Therefore, such a configuration is effective, for example, when a plurality of power storage devices 10 are arranged side by side to form a module.

[0057] Fig. 5 is a view showing a state in which the exterior member 101 is wound around the electrode body 200 from below during the manufacture of the electricity storage device 10. As shown in Fig. 5, in the electricity storage device 10, the direction along the side 135 is the TD (Transverse Direction) of the exterior member 101, and the direction perpendicular to the side 135 is the MD (Machine Direction) of the exterior member 101. In other words, the direction along the side 135 is the direction (TD) perpendicular to the flow direction (MD) of the exterior member 101.

[0058] In the electricity storage device 10, the first sealing portion 110 is folded along the side 135, and the direction along the side 135 is a direction perpendicular to the flow direction of the exterior member 101. Therefore, according to the electricity storage device 10, even if a crease is formed in the direction perpendicular to the flow direction of the exterior member 101, the exterior member 101 is unlikely to break, and therefore it is possible to reduce the possibility that the first sealing portion 110 will break due to the folding of the first sealing portion 110.

[0059] The machine direction (MD) of the exterior member 101 corresponds to the rolling direction (RD) of the metal foil (aluminum alloy foil, etc.) of the barrier layer included in the exterior member 101. The TD of the exterior member 101 corresponds to the TD of the metal foil. The rolling direction (RD) of the metal foil can be determined by the rolling marks.

[0060] In addition, the sea-island structure can be confirmed by observing multiple cross sections of the heat-fusible resin layer of the exterior member 101 with an electron microscope, and the direction parallel to the cross section in which the average diameter of the islands in the direction perpendicular to the thickness direction of the heat-fusible resin layer (hereinafter also referred to as the "length direction of the heat-fusible resin layer") was maximum can be determined as the MD. When the MD of the exterior member 101 cannot be identified based on the rolling marks of the metal foil, the MD can be identified by this method.

[0061] Specifically, the sea-island structure is confirmed by observing the longitudinal cross section of the heat-sealable resin layer and each cross section (a total of 10 cross sections) at an angle of 10 degrees from the direction parallel to the longitudinal cross section and perpendicular to the longitudinal cross section. Next, for each island on each cross section, the island diameter d is measured by the linear distance connecting both ends in the direction perpendicular to the thickness direction of the heat-sealable resin layer. Next, the average of the diameters d of the top 20 largest islands is calculated for each cross section. The direction parallel to the cross section in which the average island diameter d was the largest is determined to be the MD.

[0062] Fig. 6 is a diagram that diagrammatically shows a part of the cross section taken along line VI-VI in Fig. 2. As shown in Fig. 6, second sealing portion 120 seals exterior body 100 in a state in which electrode terminal 300 is sandwiched between exterior body 100 and electrode terminal 300.

[0063] Fig. 7A is a diagram for explaining a method for forming the second sealed portion 120. As shown in Fig. 7A, the exterior member 101 is folded, and the surfaces (thermally adhesive resin layers) of the exterior member 101 facing each other are heat-sealed to form the second sealed portion 120. Although omitted in Fig. 7A, an electrode terminal 300 is located between the surfaces of the exterior member 101 facing each other. An adhesive film for terminal 30 (see Figs. 7B to 7E), which adheres to both metal and resin, may be disposed between the electrode terminal 300 and the exterior member 101.

[0064] The adhesive film may be, for example, a one-layer or two-layer structure of a resin film made of a polyolefin resin or an acid-modified polyolefin resin obtained by graft-modifying a polyolefin resin with an acid such as maleic anhydride. When the adhesive film is made of two or more layers, it is preferable to arrange a resin film made of a polyolefin resin on the side that is bonded to the exterior member 101. When the adhesive film is made of two or more layers, it is preferable to arrange a resin film made of an acid-modified polyolefin resin obtained by graft-modifying a polyolefin resin with an acid such as maleic anhydride on the side that is bonded to the electrode terminal 300.

[0065] 6 again, the electrode body 200 includes a plurality of electrodes 210 (positive and negative electrodes). A current collector 215 extending from each electrode 210 is connected to an electrode terminal 300. In the electricity storage device 10, a portion of the electrode terminal 300 that is on the outside of the exterior body 100 is located at a position that is approximately half the thickness of the electricity storage device 10 in the thickness direction of the electricity storage device 10. In other words, the length L2 is approximately half the length L1. Note that "approximately half the thickness of the electricity storage device 10" means 35% to 65% of the thickness of the electricity storage device 10.

[0066] Therefore, according to the energy storage device 10, for example, the difference between the longest distance and the shortest distance between each of the multiple electrodes 210 and the electrode terminal 300 can be made smaller compared to when the electrode terminal 300 is located at approximately the same position as the first surface 130 in the thickness direction of the energy storage device 10.

[0067] Since the performance of the electricity storage device 10 deteriorates if moisture penetrates into the electrode body 200, for example, a barrier layer 101B (made of, for example, a metal foil) is provided when the above-mentioned film-like laminate is used as the exterior member 101. By providing the barrier layer 101B, it is possible to suppress the penetration of moisture from the outside of the barrier layer 101B.

[0068] However, when the heat-sealable resin layer 101C of the exterior member 101 is heat-sealed to seal the electrode body 200, the end face of the heat-sealable resin layer 101C is exposed to the outside, and therefore there is a risk of moisture penetrating from the end face of the heat-sealable resin layer 101C.

[0069] In addition, if the heat-sealable resin layer 101C of the exterior member 101 absorbs water before the electrode body 200 is sealed with the exterior member 101, there is a risk that the moisture in the heat-sealable resin layer 101C will penetrate into the electrode body 200 after the electrode body 200 is sealed.

[0070] Furthermore, when the electricity storage device 10 is an all-solid-state battery, if moisture comes into contact with a solid electrolyte contained in an element that constitutes the all-solid-state battery, gas such as hydrogen sulfide may be generated depending on the type of solid electrolyte.

[0071] The electricity storage device 10 of this embodiment includes a resin film 20 for an electricity storage device (hereinafter referred to as "film 20") to achieve at least one of suppressing the intrusion of moisture into the electrode body 200 and absorbing gases such as hydrogen sulfide generated from the electrode body 200. The film 20 contains at least one of a water absorbing agent and a gas absorbing agent. Hereinafter, the case where the film 20 contains at least a water absorbing agent may be referred to as a first embodiment of the film 20. The case where the film 20 contains at least a gas absorbing agent may be referred to as a second embodiment of the film 20.

[0072] In the electricity storage device 10, the location of the film 20 can be arbitrarily selected as long as it is inside the barrier layer 101B of the exterior member 101. In the present embodiment, the inside of the barrier layer 101B is the opposite side of the base layer 101A with respect to the barrier layer 101B in the direction in which the layers 101A to 101C of the exterior member 101 are stacked. By arranging the film 20 of the first aspect inside the barrier layer 101B of the exterior member 101, it is possible to suppress the intrusion of moisture from the end of the heat-sealable resin layer 101C of the exterior member 101 and the intrusion of moisture contained in the heat-sealable resin layer 101C of the exterior member 101 into the electrode body 200. That is, in the electricity storage device 10 including the film 20 of the first aspect, since the film 20 contains a water absorbing agent, the film 20 absorbs and holds moisture that has infiltrated from the heat-sealable resin layer 101C of the exterior member 101, thereby suppressing the moisture from reaching the electrode body 200. Furthermore, by disposing the film 20 of the second embodiment on the inner side of the barrier layer 101B of the exterior member 101, for example, when the electrode body 200 is an all-solid-state battery, it is possible to absorb gases such as hydrogen sulfide generated by contact between a solid electrolyte layer contained in an element constituting the all-solid-state battery and moisture. That is, in the electricity storage device 10 including the film 20 of the second embodiment, the film 20 contains a gas absorbent, so that gases such as hydrogen sulfide generated from the electrode body 200 are absorbed by the film 20. For this reason, it is possible to suppress an excessive increase in the internal pressure of the exterior body 100. A specific example of the arrangement of the film 20 in the electricity storage device 10 will be described below.

[0073] As shown in FIG. 1B, the film 20 can also be used as the heat-sealable resin layer 101C of the exterior member 101. The film 20 may be used as an adhesive layer between the barrier layer 101B and the heat-sealable resin layer 101C. The film 20 can also be used as an adhesive film interposed between the heat-sealable resin layers 101C facing each other at a position where the heat-sealable resin layers 101C of the exterior member 101, such as the first sealing portion 110, are heat-sealed to each other. When the film 20 is used as an adhesive film, the film 20 may have a function of releasing the gas to the outside by peeling off the portion of the heat-sealable resin layer 101C where the film 20 is interposed when the internal pressure of the exterior member 100 increases due to gas generation from the electrode body 200.

[0074] Fig. 7B is another cross-sectional view taken along line VI-VI in Fig. 2. In the example shown in Fig. 7B, the film 20 is disposed between the exterior member 101 and the electrode body 200 so as to cover substantially the entire upper and lower surfaces of the electrode body 200. The film 20 and the inner surface of the exterior member 101 (thermally adhesive resin layer 101C) may or may not be joined together.

[0075] Fig. 7C is a cross-sectional view showing yet another example taken along line VI-VI in Fig. 2. In the example shown in Fig. 7C, the film 20 is disposed between the exterior member 101 and the electrode body 200 so as to cover substantially the entire side surface of the electrode body 200. The film 20 and the inner surface of the exterior member 101 (thermally adhesive resin layer 101C) may or may not be joined together.

[0076] Fig. 7D is a cross-sectional view showing yet another example taken along line VI-VI in Fig. 2. In the example shown in Fig. 7D, the film 20 is disposed between the exterior member 101 and the electrode body 200 so as to cover substantially the entire electrode body 200. The film 20 and the inner surface of the exterior member 101 (thermally adhesive resin layer 101C) may or may not be joined together.

[0077] Fig. 7E is a cross-sectional view showing yet another example taken along line VI-VI in Fig. 2. In the example shown in Fig. 7E, the electricity storage device 10 has a terminal adhesive film 30 that adheres to both metal and resin between the electrode terminal 300 and the exterior member 101. In the example shown in Fig. 7E, the film 20 is used as the terminal adhesive film 30.

[0078] Since the end faces of the adhesive film for a terminal 30 are exposed to the outside, there is a risk of moisture penetrating from the end faces of the adhesive film for a terminal 30. In addition, if the adhesive film for a terminal 30 absorbs water before being interposed between the electrode terminal 300 and the exterior member 101, there is a risk that the moisture in the adhesive film for a terminal 30 will penetrate into the electrode body 200 after the adhesive film for a terminal 30 is interposed between the electrode terminal 300 and the exterior member 101.

[0079] By using the film 20 of the first embodiment as the adhesive film 30 for a terminal, it is possible to effectively prevent moisture from entering from the end of the adhesive film 30 for a terminal, and moisture contained in the adhesive film 30 for a terminal from entering the electrode body 200. That is, in the electricity storage device 10 including the film 20 of the first embodiment, since the film 20 contains a water absorbing agent, the film 20 absorbs and holds the moisture that has entered from the adhesive film 30 for a terminal, thereby preventing moisture from reaching the electrode body 200. In addition, by using the film 20 of the second embodiment as the adhesive film 30 for a terminal, for example, when the electrode body 200 is an all-solid-state battery, gas such as hydrogen sulfide generated by contact between the solid electrolyte layer contained in the element constituting the all-solid-state battery and moisture can be effectively absorbed. That is, in the electricity storage device 10 including the film 20 of the second embodiment, since the film 20 contains a gas absorbent, gas such as hydrogen sulfide generated from the electrode body 200 is absorbed by the film 20. Therefore, gas such as hydrogen sulfide is less likely to be released to the outside.

[0080] <1-2. Specific configuration of resin film for electricity storage device> In the first embodiment of the film 20, the moisture to be absorbed is gaseous and / or liquid moisture. As described later, the gas absorbing film according to the first embodiment of the present embodiment can also absorb sulfur-based gases as necessary. Examples of sulfur-based gases include hydrogen sulfide, dimethyl sulfide, methyl mercaptan, and sulfur oxides represented by SOx. When the moisture to be absorbed is absorbed in, for example, a solid electrolyte type lithium ion battery, it generates various outgases, and the sulfur-based gas is a component of the outgases (for example, generated when the power storage device 10 is an all-solid-state battery using a sulfide-based inorganic solid electrolyte or a lithium secondary battery using lithium sulfur in the positive electrode).

[0081] The film 20 of this embodiment may be composed of a single layer, for example, as shown in Fig. 7F, or may be composed of two or more layers, for example, as shown in Fig. 7G and Fig. 7H. Fig. 7G shows the film 20 composed of a laminate in which the first layer 21 and the second layer 22 are laminated. Fig. 7H shows the film 20 composed of a laminate in which the second layer 22, the first layer 21, and the third layer 23 are laminated in this order.

[0082] In the first embodiment, when the film 20 is composed of two or more layers, at least one of the two or more layers may contain a water absorbing agent. In this embodiment, the layer containing a water absorbing agent may be referred to as a "water absorbing layer". Specific examples of the lamination structure of the film 20 according to the first embodiment include a lamination structure in which the first layer 21 on the exterior member 101 side is a water absorbing layer and the second layer 22 on the electrode body 200 side is a layer that does not contain a water absorbing agent, as shown in FIG. 7G. Also, for example, in FIG. 7H, the lamination structure in which the first layer 21 located in the middle is a water absorbing layer, and the second layer 22 on the electrode body 200 side and the third layer 23 on the exterior member 101 side are layers that do not contain a water absorbing agent; and a lamination structure in which at least one of the first layer 21 and the third layer 23 is a water absorbing layer and the second layer 22 is a layer that does not contain a water absorbing agent.

[0083] In the second aspect, when the film 20 is composed of two or more layers, at least one of the two or more layers may contain a gas absorbent. The gas absorbent is, for example, at least one of a sulfur-based gas absorbent, a carbon dioxide absorbent, and an oxygen absorbent. In this embodiment, the second aspect of the film 20 will be described using a case where the gas absorbent is a sulfur-based gas absorbent as an example. Specific examples of the lamination structure of the film 20 according to the second aspect include, for example, in FIG. 7G, a lamination structure in which the first layer 21 on the exterior member 101 side is a sulfur-based gas absorbing layer and the second layer 22 on the electrode body 200 side is a layer that does not contain a sulfur-based gas absorbent; and a lamination structure in which the first layer 21 on the exterior member 101 side is a layer that does not contain a sulfur-based gas absorbing layer and the second layer 22 on the electrode body 200 side is a layer that contains a sulfur-based gas absorbent. 7H, for example, the first layer 21 located in the middle is a sulfur-based gas absorbing layer, and the second layer 22 on the electrode body 200 side and the third layer 23 on the exterior member 101 side are layers that do not contain a sulfur-based gas absorbent; the first layer 21 and at least one of the third layer 23 are sulfur-based gas absorbing layers, and the second layer 22 is a layer that does not contain a sulfur-based gas absorbent; the first layer 21 located in the middle is a layer that does not contain a sulfur-based gas absorbing layer, and the second layer 22 on the electrode body 200 side and the third layer 23 on the exterior member 101 side are layers that contain a sulfur-based gas absorbent; the first layer 21 and at least one of the third layer 23 are layers that do not contain a sulfur-based gas absorbing layer, and the second layer 22 is a layer that contains a sulfur-based gas absorbent. Since hydrogen sulfide gas is generated from the electrode body 200, it is preferable that the second layer 22 located on the electrode body 200 side is a sulfur-based gas absorbing layer.

[0084] In the first embodiment, it is preferable that one or both sides of the film 20 have heat fusion properties. When the film 20 according to the first embodiment is located in the second sealing portion 120 of the exterior member 101, it is preferable to increase the heat fusion properties of the film 20. Therefore, for example, when the film 20 is composed of three or more layers, it is preferable that the layers located on the surface (the second layer 22 and the third layer 23 in FIG. 7H) contain a heat fusion resin. In addition, from the viewpoint of suppressing the decrease in the heat fusion properties of the layers located on the surface, it is preferable that the layers located on the surface do not contain a water absorbing agent (particularly an inorganic water absorbing agent). In the electricity storage device 10, from the viewpoint of more suitably exhibiting the water absorbing performance of the water absorbing layer of the film 20, it is preferable that the water absorbing layer is provided between the layers located on the surface. This is because if the water absorbing layer is located on the surface, it absorbs moisture in the air before the electricity storage device 10 is manufactured, and the water absorbing performance of the water absorbing layer is likely to decrease. In addition, in the electricity storage device 10, it is also preferable that the third layer 23 located on the exterior member 101 side is the water absorbing layer. This is because the third layer 23 is close to the exterior member 101 and therefore easily absorbs moisture that has infiltrated from the exterior member 101 side. In the electricity storage device 10, it is also preferable that the second layer 22 located on the electrode assembly 200 side is the water absorption layer. This is because the second layer 22 is close to the electrode assembly 200 and therefore easily absorbs moisture contained in the electrode assembly 200.

[0085] In the second embodiment as well, it is preferable that one or both sides of the film 20 have heat fusion properties. When the film 20 according to the second embodiment is located in the second sealing portion 120 of the exterior member 101, it is preferable to enhance the heat fusion properties of the film 20. Therefore, for example, when the film 20 is composed of three or more layers, it is preferable that the layer located on the surface (the second layer 22 and the third layer 23 in FIG. 7H) contains a heat fusion resin. Moreover, from the viewpoint of suppressing a decrease in the heat fusion properties of the layer located on the surface, it is preferable that the layer located on the surface does not contain a sulfur-based gas absorbent.

[0086] The film 20 according to the first embodiment may further contain a sulfur-based gas absorbent, which will be described later, in addition to the water absorbing agent. In this embodiment, the layer containing the sulfur-based gas absorbent may be referred to as a "sulfur-based gas absorbing layer". When the sulfur-based gas absorbent is contained, the sulfur-based gas absorbent may be contained in the water absorbing layer, or may be contained in a layer that does not contain a water absorbing agent. When the film 20 is composed of two or more layers, it is preferable that the sulfur-based gas absorbent is contained in a layer that does not contain a water absorbing agent to constitute the sulfur-based gas absorbing layer. Concerns due to the inclusion of multiple types of particles in a single layer include that the particles are difficult to disperse during the film formation of the film 20, holes are formed in the film, and the strength of the film 20 varies depending on the location. In addition, when the amount of particles contained in a single layer exceeds a certain amount, the elongation and strength of the film decrease, and there is a concern that the film may easily break at the corners of the battery. If the amounts are small, these concerns are unlikely to arise even if the water absorbing agent and the sulfur-based gas absorbent are contained in a single layer. However, in order to maintain the water absorption effect and the sulfur-based gas absorption effect for a long period of time, it is preferable that the water absorption layer and the sulfur-based gas absorbing layer are separate layers.

[0087] When the film 20 according to the first embodiment is composed of two or more layers, a specific example of the laminated structure of the film 20 is, for example, a laminated structure in which the first layer 21 is a water absorption layer and the second layer 22 is a sulfur-based gas absorption layer in FIG. 7G. Also, for example, in FIG. 7H, a laminated structure in which the first layer 21 is a water absorption layer and at least one of the second layer 22 and the third layer 23 is a sulfur-based gas absorption layer; a laminated structure in which at least one of the first layer 21 and the third layer 23 is a water absorption layer and the second layer 22 is a sulfur-based gas absorption layer, and the like are included. Since hydrogen sulfide gas is generated from the electrode body 200, it is preferable that the second layer 22 located on the electrode body 200 side is a sulfur-based gas absorption layer. In addition, as described above, since it is preferable that the water absorption layer is provided between layers located on the surface, among these, a laminated structure in which the first layer 21 located between the second layer 22 and the third layer 23 is a water absorption layer and the second layer 22 located on the electrode body 200 side is a sulfur-based gas absorption layer is the most preferable.

[0088] Moreover, the film 20 according to the second embodiment may further contain a water absorbing agent, which will be described later, in addition to the sulfur-based gas absorbent. As described above, in the present embodiment, the layer containing the water absorbing agent may be referred to as a "water absorbing layer". When the water absorbing agent is contained, the water absorbing agent may be contained in the sulfur-based gas absorbing layer, or may be contained in a layer that does not contain the water absorbing agent. When the film 20 according to the second embodiment is composed of two or more layers, it is preferable that the water absorbing agent is contained in a layer that does not contain the sulfur-based gas absorbent to constitute the water absorbing layer. Concerns due to the inclusion of multiple types of particles in a single layer include that the particles are difficult to disperse during the film formation of the film 20, holes are formed in the film, and the strength of the film 20 varies depending on the location. In addition, when the amount of particles contained in a single layer exceeds a certain amount, the film's elongation and strength decrease, and there is a concern that the film may be easily torn at the corners of the battery. If the amounts are small, these concerns are unlikely to arise even if the water absorbing agent and the sulfur-based gas absorbent are contained in a single layer. However, in order to maintain the water absorption effect and the sulfur-based gas absorption effect for a long period of time, it is preferable that the water absorption layer and the sulfur-based gas absorbing layer are separate layers.

[0089] When the film 20 according to the second embodiment is composed of two or more layers, a specific example of the laminated structure of the film 20 is, for example, a laminated structure in which the first layer 21 is a sulfur-based gas absorbing layer and the second layer 22 is a water absorbing layer in FIG. 7G. Also, for example, in FIG. 7H, a laminated structure in which the first layer 21 is a sulfur-based gas absorbing layer and at least one of the second layer 22 and the third layer 23 is a water absorbing layer; a laminated structure in which at least one of the first layer 21 and the third layer 23 is a sulfur-based gas absorbing layer and the second layer 22 is a water absorbing layer, and the like are included. In the electricity storage device 10, from the viewpoint of more suitably exerting the water absorbing performance of the water absorbing layer of the film 20, it is preferable that the water absorbing layer is provided between layers located on the surface. This is because if the water absorbing layer is located on the surface, it will absorb moisture in the atmosphere before the electricity storage device 10 is manufactured, and the water absorbing performance of the water absorbing layer is likely to decrease. A laminated structure in which the first layer 21 located between the second layer 22 and the third layer 23 is a water absorption layer described later, and the second layer 22 located on the electrode body 200 side is a sulfur-based gas absorption layer is the most preferable. In the electricity storage device 10, the water absorption layer is preferably the third layer 23 located on the exterior member 101 side. This is because the third layer 23 is close to the exterior member 101 and easily absorbs moisture that has infiltrated from the exterior member 101 side. In the electricity storage device 10, the water absorption layer is preferably the second layer 22 located on the electrode body 200 side. This is because the second layer 22 is close to the electrode body 200 and easily absorbs moisture contained in the electrode body 200.

[0090] In this embodiment, the resin contained in the film 20 is not particularly limited as long as it does not impair the effects of this embodiment. For example, it is preferably a thermoplastic resin, and more preferably a heat-sealable resin. Specific examples of the resin include thermoplastic resins such as polyester, polyolefin, polyamide, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, and phenolic resin, and modified products of these resins. The resin forming the film 20 may be a copolymer of these resins or a modified product of the copolymer. Furthermore, it may be a mixture of these resins. Among these, heat-sealable resins such as polyester and polyolefin are preferred.

[0091] Specific examples of polyesters include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolymerized polyesters. Examples of copolymerized polyesters include copolymerized polyesters in which ethylene terephthalate is the main repeating unit. Specific examples of polyesters include copolymerized polyesters in which ethylene terephthalate is the main repeating unit and is polymerized with ethylene isophthalate (hereinafter, abbreviated as polyethylene (terephthalate / isophthalate)), polyethylene (terephthalate / adipate), polyethylene (terephthalate / sodium sulfoisophthalate), polyethylene (terephthalate / sodium isophthalate), polyethylene (terephthalate / phenyl-dicarboxylate), and polyethylene (terephthalate / decane dicarboxylate). These polyesters may be used alone or in combination of two or more. Among these, polybutylene terephthalate is particularly preferred from the viewpoint of increasing heat resistance and pressure resistance (for example, the decrease in insulation when sealing the electrode body 200 with the exterior member 101 (due to crushing due to heat sealing)).

[0092] Specific examples of polyolefins include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; ethylene-α-olefin copolymers; polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); propylene-α-olefin copolymers; and ethylene-butene-propylene terpolymers. When the polyolefin resin is a copolymer, it may be a block copolymer or a random copolymer. These polyolefin resins may be used alone or in combination of two or more. Among these, polypropylene is particularly preferred because of its excellent thermal fusion properties.

[0093] The resin contained in the film 20 preferably contains a resin containing a polyolefin skeleton as a main component, more preferably contains polyolefin as a main component, and even more preferably contains polypropylene as a main component. Here, the main component means that the content of the resin component contained in the film 20 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, the resin contained in the film 20 containing polypropylene as a main component means that the content of polypropylene of the resin component contained in the film 20 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.

[0094] The resin contained in the film 20 preferably contains polyester as a main component. Here, the main component means that the content of the resin component contained in the film 20 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. For example, the resin contained in the film 20 contains polyester as a main component means that the content of polyester of the resin component contained in the film 20 is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more.

[0095] When producing the film 20 of the present embodiment, a preformed resin film may be used as the film 20. Also, the resin forming the film 20 may be formed into a film by extrusion molding, coating, or the like, to form a resin formed from a resin film.

[0096] In this embodiment, the resin contained in the film 20 may contain an elastomer. The elastomer plays a role of ensuring the durability of the film 20 in a high-temperature environment while increasing its flexibility. Preferred elastomers include at least one thermoplastic elastomer selected from polyesters, polyamides, polyurethanes, polyolefins, polystyrenes, and polyethers, or thermoplastic elastomers that are copolymers of these. The content of the elastomer in the film 20 is not particularly limited as long as it can ensure the durability of the film 20 in a high-temperature environment while increasing its flexibility, and is, for example, about 0.1% by mass or more, preferably about 0.5% by mass or more, more preferably about 1.0% by mass or more, and even more preferably about 3.0% by mass or more. The content is, for example, about 10.0% by mass or less, about 8.0% by mass or less, or about 5.0% by mass or less. Preferred ranges of the content include about 0.1 to 10.0 mass%, about 0.1 to 8.0 mass%, about 0.1 to 5.0 mass%, about 0.5 to 10.0 mass%, about 0.5 to 8.0 mass%, about 0.5 to 5.0 mass%, about 1.0 to 10.0 mass%, about 1.0 to 8.0 mass%, about 1.0 to 5.0 mass%, about 3.0 to 10.0 mass%, about 3.0 to 8.0 mass%, and about 3.0 to 5.0 mass%.

[0097] The content of the resin in the film 20 according to the first embodiment is, for example, 99.9% by mass or more, preferably 99.5% by mass or more, and more preferably 99.0% by mass or more.

[0098] The content of the resin in the film 20 according to the second embodiment is, for example, 50% by mass or more, preferably 55% by mass or more, and more preferably 60% by mass or more.

[0099] The water absorbing agent contained in the film 20 according to the first embodiment is not particularly limited as long as it is dispersed in a resin film and exhibits water absorption. For example, an inorganic water absorbing agent can be suitably used from the viewpoint of stability over time in the power storage device 10. Specific examples of preferred inorganic water absorbing agents include calcium oxide, anhydrous magnesium sulfate, magnesium oxide, calcium chloride, zeolite, aluminum oxide, silica gel, alumina gel, and calcined alum. In general, inorganic chemical water absorbing agents have a higher water absorption effect than inorganic physical water absorbing agents, can reduce the content, and can easily achieve sufficient water absorption and heat fusion in a single layer. Among inorganic chemical water absorbing agents, calcium oxide, anhydrous magnesium sulfate, and magnesium oxide are particularly preferred because they have little re-release of moisture, high stability over time in a low humidity state inside the package, and have an absolute dry effect. The absolute dry effect refers to the effect of absorbing water until the relative humidity becomes close to 0%, and the humidity control effect refers to the effect of absorbing water when the humidity is high and releasing moisture when the humidity is low, thereby keeping the humidity constant. Furthermore, when the material is used in a high-temperature environment, such as for an all-solid-state battery, an inorganic chemical absorbent that re-releases moisture in a high temperature range is preferred.

[0100] In the first embodiment, examples of the resin contained in the water-absorbing layer include the same resins as those exemplified as the resin contained in the film 20.

[0101] In the first embodiment, the content of the resin in the water absorption layer of the film 20 is, for example, 50% by mass or more, preferably 55% by mass or more, and more preferably 60% by mass or more.

[0102] In the first embodiment, the content of the water absorbing agent contained in the film 20 is not particularly limited as long as the effect of the present embodiment is exhibited, and is preferably about 0.5 parts by mass or more, more preferably about 2 parts by mass or more, and even more preferably about 3 parts by mass or more, relative to 100 parts by mass of the resin contained in the film 20, and is also preferably about 50 parts by mass or less, more preferably about 45 parts by mass or less, and even more preferably 40 parts by mass or less. Preferred ranges of the content include about 0.5 to 50 parts by mass, about 0.5 to 45 parts by mass, about 0.5 to 40 parts by mass, about 2 to 50 parts by mass, about 2 to 45 parts by mass, about 2 to 40 parts by mass, about 3 to 50 parts by mass, about 3 to 45 parts by mass, and about 3 to 40 parts by mass. The content of the water absorbing agent contained in the water absorption layer of the film 20 is not particularly limited as long as the effect of this embodiment is exhibited, and is preferably about 0.5 parts by mass or more, more preferably about 2 parts by mass or more, and even more preferably about 3 parts by mass or more relative to 100 parts by mass of the resin contained in the water absorption layer, and is preferably about 50 parts by mass or less, more preferably about 45 parts by mass or less, and even more preferably 40 parts by mass or less. Preferred ranges of the content include about 0.5 to 50 parts by mass, about 0.5 to 45 parts by mass, about 0.5 to 40 parts by mass, about 2 to 50 parts by mass, about 2 to 45 parts by mass, about 2 to 40 parts by mass, about 3 to 50 parts by mass, about 3 to 45 parts by mass, and about 3 to 40 parts by mass.

[0103] In the film 20 according to the first embodiment, the water absorbing agent is preferably contained in the water absorbing layer via a master batch obtained by melt blending the water absorbing agent with a resin. Specifically, the water absorbing agent is melt blended with a resin at a relatively high concentration to prepare a master batch. The obtained master batch is further mixed with a resin and formed into a film to form the water absorbing layer. The content of the water absorbing agent in the master batch is preferably about 20 to 90% by mass, more preferably about 30 to 70% by mass. Within the above range, it is easy to include a necessary and sufficient amount of the water absorbing agent in the water absorbing layer in a dispersed state.

[0104] As described above, the film 20 according to the first embodiment may further contain a sulfur-based gas absorbent in addition to the water absorbing agent. The sulfur-based gas absorbent preferably contains a sulfur-based gas physical absorbent and / or a sulfur-based gas chemical absorbent. By using various sulfur-based gas absorbents in combination, for example, by using a sulfur-based gas physical absorbent and a sulfur-based gas chemical absorbent in combination, it becomes possible to easily absorb various types of sulfur-based gases. The sulfur-based gas absorbent is used, for example, in the form of a powder. The maximum particle size of the sulfur-based gas absorbent is preferably 20 μm or less, and the number average particle size of the powder is preferably 0.1 μm or more and 15 μm or less. If the number average particle size is smaller than the above range, the sulfur-based gas absorbent is likely to aggregate, and if the number average particle size is larger than the above range, the homogeneity of the sulfur-based gas absorbing film may be inferior, and the surface area of ​​the sulfur-based gas absorbent may be reduced, resulting in poor sulfur-based gas absorption.

[0105] (Sulfur gas physical absorbent) The sulfur-based gas physical absorbent is a gas absorbent that has the function of physically absorbing the sulfur-based gas to be absorbed. The sulfur-based gas physical absorbent preferably contains one or more selected from the group consisting of hydrophobic zeolite, bentonite, and sepiolite having a SiO2 / Al2O3 molar ratio of 1 / 1 to 2000 / 1.

[0106] Hydrophobic zeolite is a zeolite with excellent absorption of low polarity molecules such as sulfur-based gases, and has a porous structure. In general, the higher the molar ratio of SiO2 / Al2O3, which is a component of zeolite, the higher the hydrophobicity. And, as the hydrophobicity increases, it becomes easier to absorb low polarity molecules such as sulfur-based gases, and conversely, it becomes difficult to absorb them because the affinity with highly polar molecules such as water decreases. The SiO2 / Al2O3 molar ratio of hydrophobic zeolite is preferably 30 / 1 to 10000 / 1, more preferably 35 / 1 to 9000 / 1, and even more preferably 40 / 1 to 8500 / 1. In addition, hydrophobic zeolite has high heat resistance and can maintain its absorption effect even when exposed to high temperatures of 230°C or more. In the present invention, hydrophobic zeolite with a molar ratio in the above range is preferably used from the balance between sulfur-based gas absorption ability and ease of availability.

[0107] Bentonite is an inorganic substance whose main component is the clay mineral montmorillonite, containing a large amount of layered aluminum phyllosilicate, and containing minerals such as quartz and feldspar as impurities. For example, there are Na-type bentonite that contains a large amount of Na+ ions, Ca-type bentonite that contains a large amount of Ca2+ ions, and activated bentonite that is artificially converted to Na-type by adding a few wt% of sodium carbonate to Ca-type bentonite.

[0108] Sepiolite is a clay mineral whose main component is hydrated magnesium silicate, and its general chemical composition is Mg8Si 12 O 30 It is represented by (OH2)4(OH)4·6-8H2O and has a porous structure. From the viewpoint of availability, the pH (3% suspension) is preferably 8.0-9.0, and more preferably 8.9-9.3.

[0109] (Sulfur gas chemical absorbent) The sulfur-based gas chemical absorbent is a gas absorbent that has the function of chemically absorbing or decomposing the sulfur-based gas of the gas to be absorbed. And, because it is chemically absorbed or decomposed, it is not easily affected by water, etc., and once absorbed, the sulfur-based gas molecules are not easily desorbed, so that it can be efficiently absorbed. In addition, the decomposition product is absorbed by the sulfur-based gas physical absorbent or the sulfur-based gas chemical absorbent. The sulfur-based gas chemical absorbent preferably contains one or more selected from the group consisting of inorganic matter carrying a metal oxide, glass mixed with a metal, and glass mixed with a metal ion. The metal oxide in the inorganic matter carrying a metal oxide preferably contains one or more selected from the group consisting of CuO, ZnO, and AgO. In addition, the inorganic matter to be supported is preferably an inorganic porous body such as zeolite. The metal in the glass containing a metal, or the metal species of the metal ions in the glass containing a metal ion, preferably includes one or more species selected from the group consisting of Ca, Mg, Na, Cu, Zn, Ag, Pt, Au, Fe, Al, and Ni.

[0110] In the first embodiment, the content of the sulfur-based gas absorbent in the film 20 is not particularly limited as long as it absorbs a sulfur-based gas, and is preferably at least about 0.1 part by mass, more preferably at least about 0.2 parts by mass, and even more preferably at least about 0.3 parts by mass, relative to 100 parts by mass of the resin contained in the film 20, and is preferably at most about 30 parts by mass, more preferably at most about 27 parts by mass, and even more preferably at most 25 parts by mass. Preferred ranges of the content include about 0.1 to 30 parts by mass, about 0.1 to 27 parts by mass, about 0.1 to 25 parts by mass, about 0.2 to 30 parts by mass, about 0.2 to 27 parts by mass, about 0.2 to 25 parts by mass, about 0.3 to 30 parts by mass, about 0.3 to 27 parts by mass, and about 0.3 to 25 parts by mass. The content of the sulfur-based gas absorbent contained in the sulfur-based gas absorbing layer of the film 20 is not particularly limited as long as it absorbs sulfur-based gases, and is preferably about 5 parts by mass or more, more preferably about 6 parts by mass or more, and even more preferably about 7 parts by mass or more, relative to 100 parts by mass of the resin contained in the sulfur-based gas absorbing layer. Also, it is preferably about 60 parts by mass or less, more preferably about 55 parts by mass or less, and even more preferably about 50 parts by mass or less, and about 30 parts by mass or less. Preferred ranges of the content include about 5 to 60 parts by mass, about 5 to 55 parts by mass, about 5 to 50 parts by mass, about 5 to 30 parts by mass, about 6 to 60 parts by mass, about 6 to 55 parts by mass, about 6 to 50 parts by mass, about 6 to 30 parts by mass, about 7 to 60 parts by mass, about 7 to 55 parts by mass, about 7 to 50 parts by mass, and about 7 to 30 parts by mass.

[0111] In the first embodiment, the content of the resin contained in the sulfur-based gas absorbing layer is, for example, 50% by mass or more, preferably 55% by mass or more, and more preferably 60% by mass or more.

[0112] In the first embodiment, the sulfur-based gas absorbent contained in the sulfur-based gas absorbing layer is preferably contained via a master batch in which the sulfur-based gas absorbent is melt-blended with a resin. Specifically, it is preferable to melt-blend the sulfur-based gas absorbent with a resin at a relatively high concentration to prepare a master batch, and then dry-blend the master batch with other components to obtain a desired concentration in the sulfur-based gas absorbing layer. The sulfur-based gas absorbent and the resin to be melt-blended may each be one type or two or more types. The content of the sulfur-based gas absorbent in the master batch is preferably about 20 to 90 mass%, more preferably about 30 to 70 mass%. Within the above range, it is easy to contain a necessary and sufficient amount of the sulfur-based gas absorbent in a dispersed state in the sulfur-based gas absorbing layer.

[0113] In the first embodiment, examples of the resin contained in the sulfur-based gas absorbing layer include the same resins as those exemplified as the resin contained in the water absorbing layer.

[0114] As described above, when the film 20 according to the first embodiment contains a sulfur-based gas absorbent, the sulfur-based gas absorbent may be contained in the water-absorbing layer, or may be contained in a layer that does not contain a water-absorbing agent. When the sulfur-based gas absorbent is contained in the water-absorbing layer, the water-absorbing layer also functions as a sulfur-based gas absorbing layer.

[0115] The film 20 according to the first embodiment may contain various plastic compounding agents and additives for the purpose of improving or modifying, for example, processability, heat resistance, weather resistance, mechanical properties, dimensional stability, oxidation resistance, slipperiness, release properties, flame retardancy, mold resistance, electrical properties, strength, etc. The content may be any amount from a trace amount to several tens of percent depending on the purpose. In the above, examples of common additives that may be contained include antiblocking agents, lubricants, crosslinking agents, antioxidants, ultraviolet absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, modifying resins, etc.

[0116] The thickness of the film 20 according to the first embodiment is not particularly limited as long as the effects of the present invention are exhibited, and is preferably about 10 μm or more, more preferably about 15 μm or more, and even more preferably about 20 μm or more, and is preferably about 1000 μm or less, more preferably about 900 μm or less, and even more preferably about 500 μm or less. Preferred ranges of the thickness include about 10 to 1000 μm, about 10 to 900 μm, about 10 to 500 μm, about 15 to 1000 μm, about 15 to 900 μm, about 15 to 500 μm, about 20 to 1000 μm, about 20 to 900 μm, and about 20 to 500 μm.

[0117] In the first embodiment, when the film 20 is composed of two or more layers, the thickness of each layer may be as described above for the film 20. For example, the thickness of the water-absorbing layer is preferably about 5 μm or more, more preferably about 6 μm or more, and even more preferably about 7 μm or more, and is preferably about 500 μm or less, more preferably about 400 μm or less, and even more preferably about 300 μm or less, and preferred ranges for the thickness include about 5 to 500 μm, about 5 to 400 μm, about 5 to 300 μm, about 6 to 500 μm, about 6 to 400 μm, about 6 to 300 μm, about 7 to 500 μm, about 7 to 400 μm, and about 7 to 300 μm. The thickness of the sulfur-based gas absorbing layer is preferably about 5 μm or more, more preferably about 7 μm or more, and even more preferably about 10 μm or more, and is preferably about 500 μm or less, more preferably about 400 μm or less, and even more preferably about 300 μm or less. Preferred ranges of the thickness include about 5 to 500 μm, about 5 to 400 μm, about 5 to 300 μm, about 7 to 500 μm, about 7 to 400 μm, about 7 to 300 μm, about 10 to 500 μm, about 10 to 400 μm, and about 10 to 300 μm.

[0118] In the second embodiment, the sulfur-based gas absorbent preferably contains a sulfur-based gas physical absorbent and / or a sulfur-based gas chemical absorbent. By using various sulfur-based gas absorbents in combination, for example, by using a sulfur-based gas physical absorbent and a sulfur-based gas chemical absorbent in combination, it becomes possible to easily absorb various types of sulfur-based gases. The sulfur-based gas absorbent is used, for example, in the form of a powder. The maximum particle size of the sulfur-based gas absorbent is preferably 20 μm or less, and the number average particle size of the powder is preferably 0.1 μm or more, 1.0 μm or more, and is preferably 15 μm or less, 10 μm or less, or 8 μm or less, and preferred ranges include about 0.1 to 15 μm, about 0.1 to 10 μm, about 0.1 to 8 μm, about 1 to 15 μm, about 1 to 10 μm, and about 1 to 8 μm. If the number average particle size is smaller than the above range, the sulfur-based gas absorbent will be prone to aggregation, and if the number average particle size is larger than the above range, the homogeneity of the sulfur-based gas absorbing film may be poor, and the surface area of ​​the sulfur-based gas absorbent may be reduced, resulting in poor sulfur-based gas absorption.

[0119] (Sulfur gas physical absorbent) The sulfur-based gas physical absorbent is a gas absorbent that has the function of physically absorbing the sulfur-based gas to be absorbed. The sulfur-based gas physical absorbent preferably contains one or more selected from the group consisting of hydrophobic zeolite, bentonite, and sepiolite having a SiO2 / Al2O3 molar ratio of 1 / 1 to 2000 / 1.

[0120] Specific examples of the hydrophobic zeolite, bentonite, and sepiolite are the same as those described in the first embodiment, and description thereof will be omitted.

[0121] (Sulfur gas chemical absorbent) The sulfur-based gas chemical absorbent is as described in the first embodiment, and the description thereof will be omitted.

[0122] Examples of the resin contained in the sulfur-based gas absorbing layer include the same resins as those exemplified as the resin contained in the film 20 .

[0123] In the second embodiment, the content of the sulfur-based gas absorbent in the film 20 is not particularly limited as long as it absorbs a sulfur-based gas, and is preferably at least about 0.1 part by mass, more preferably at least about 0.2 parts by mass, and even more preferably at least about 0.3 parts by mass, relative to 100 parts by mass of the resin contained in the film 20, and is preferably at most about 30 parts by mass, more preferably at most about 29 parts by mass, and even more preferably at most 28 parts by mass. Preferred ranges of the content include about 0.1 to 30 parts by mass, about 0.1 to 29 parts by mass, about 0.1 to 28 parts by mass, about 0.2 to 30 parts by mass, about 0.2 to 29 parts by mass, about 0.2 to 28 parts by mass, about 0.3 to 30 parts by mass, about 0.3 to 29 parts by mass, and about 0.3 to 28 parts by mass. The content of the sulfur-based gas absorbent contained in the sulfur-based gas absorbing layer of the film 20 is not particularly limited as long as it absorbs sulfur-based gases, and is preferably about 5 parts by mass or more, more preferably about 6 parts by mass or more, and even more preferably about 7 parts by mass or more, relative to 100 parts by mass of the resin contained in the sulfur-based gas absorbing layer. Also, it is preferably about 60 parts by mass or less, more preferably about 55 parts by mass or less, even more preferably about 50 parts by mass or less, and even more preferably about 30 parts by mass or less. Preferred ranges of the content include about 5 to 60 parts by mass, about 5 to 55 parts by mass, about 5 to 50 parts by mass, about 5 to 30 parts by mass, about 6 to 60 parts by mass, about 6 to 55 parts by mass, about 6 to 50 parts by mass, about 6 to 30 parts by mass, about 7 to 60 parts by mass, about 7 to 55 parts by mass, about 7 to 50 parts by mass, and about 7 to 30 parts by mass.

[0124] In the second embodiment, the content of the resin contained in the sulfur-based gas absorbing layer is, for example, 40 mass % or more, preferably 45 mass % or more, and further preferably 50 mass % or more.

[0125] In the second embodiment, the sulfur-based gas absorbent contained in the sulfur-based gas absorbing layer is preferably contained via a master batch in which the sulfur-based gas absorbent is melt-blended with a resin. Specifically, it is preferable to melt-blend the sulfur-based gas absorbent with a resin at a relatively high concentration to prepare a master batch, and then dry-blend the master batch with other components to obtain a desired concentration in the sulfur-based gas absorbing layer. The sulfur-based gas absorbent and the resin to be melt-blended may each be one type or two or more types. The content of the sulfur-based gas absorbent in the master batch is preferably about 20 to 90 mass%, more preferably about 30 to 70 mass%. Within the above range, it is easy to contain a necessary and sufficient amount of the sulfur-based gas absorbent in a dispersed state in the sulfur-based gas absorbing layer.

[0126] As described above, in the second embodiment, the film 20 may further include a water absorbing agent in addition to the sulfur-based gas absorbent. The water absorbing agent contained in the film 20 is not particularly limited as long as it is dispersed in the resin film and exhibits water absorption. For example, from the viewpoint of stability over time in the power storage device 10, an inorganic water absorbing agent can be suitably used. Specific examples of preferred inorganic water absorbing agents include calcium oxide, anhydrous magnesium sulfate, magnesium oxide, calcium chloride, zeolite, aluminum oxide, silica gel, alumina gel, and burnt alum. In general, among inorganic water absorbing agents, inorganic chemical water absorbing agents have a higher water absorption effect than inorganic physical water absorbing agents, can reduce the content, and are easy to achieve sufficient water absorption and heat fusion in a single layer. Among inorganic chemical water absorbing agents, calcium oxide, anhydrous magnesium sulfate, and magnesium oxide are particularly preferred because they release less moisture again, have high stability over time in a low humidity state in the package, and have an absolute dry effect. The bone-drying effect refers to the effect of absorbing water until the relative humidity is close to 0%, and the humidity control effect refers to the effect of absorbing water when the humidity is high and releasing moisture when the humidity is low, thereby keeping the humidity constant. In addition, when used in a high-temperature environment, such as for an all-solid-state battery, an inorganic chemical absorbent with a high temperature range for re-releasing moisture is preferred.

[0127] In the second embodiment, the content of the water absorbing agent contained in the film 20 is not particularly limited as long as the effect of the present embodiment is exhibited, and is preferably about 0.5 parts by mass or more, more preferably about 2 parts by mass or more, and even more preferably about 3 parts by mass or more, relative to 100 parts by mass of the resin contained in the film 20, and is also preferably about 50 parts by mass or less, more preferably about 45 parts by mass or less, and even more preferably 40 parts by mass or less. Preferred ranges of the content include about 0.5 to 50 parts by mass, about 0.5 to 45 parts by mass, about 0.5 to 40 parts by mass, about 2 to 50 parts by mass, about 2 to 45 parts by mass, about 2 to 40 parts by mass, about 3 to 50 parts by mass, about 3 to 45 parts by mass, and about 3 to 40 parts by mass. The content of the water absorbing agent contained in the water absorption layer of the film 20 is not particularly limited as long as the effect of this embodiment is exhibited, and is preferably about 0.5 parts by mass or more, more preferably about 2 parts by mass or more, and even more preferably about 3 parts by mass or more relative to 100 parts by mass of the resin contained in the water absorption layer, and is preferably about 50 parts by mass or less, more preferably about 45 parts by mass or less, and even more preferably 40 parts by mass or less. Preferred ranges of the content include about 0.5 to 50 parts by mass, about 0.5 to 45 parts by mass, about 0.5 to 40 parts by mass, about 2 to 50 parts by mass, about 2 to 45 parts by mass, about 2 to 40 parts by mass, about 3 to 50 parts by mass, about 3 to 45 parts by mass, and about 3 to 40 parts by mass.

[0128] In the film 20 according to the second embodiment, the water absorbing agent is preferably contained in the water absorbing layer via a master batch obtained by melt blending the water absorbing agent with a resin. Specifically, the water absorbing agent is melt blended with a resin at a relatively high concentration to prepare a master batch. The obtained master batch is further mixed with a resin and formed into a film to form the water absorbing layer. The content of the water absorbing agent in the master batch is preferably about 20 to 90% by mass, more preferably about 30 to 70% by mass. Within the above range, it is easy to include a necessary and sufficient amount of the water absorbing agent in the water absorbing layer in a dispersed state.

[0129] In the second embodiment, examples of the resin contained in the water-absorbing layer include the same resins as those exemplified as the resin contained in the film 20.

[0130] In the second embodiment, the content of the resin in the water absorption layer of the film 20 is, for example, 50% by mass or more, preferably 55% by mass or more, and more preferably 60% by mass or more.

[0131] As described above, when the film 20 according to the second embodiment contains a water absorbing agent, the water absorbing agent may be contained in the sulfur-based gas absorbing layer, or may be contained in a layer that does not contain the sulfur-based gas absorbent. When the water absorbing agent is contained in the sulfur-based gas absorbing layer, the sulfur-based gas absorbing layer also functions as a water absorbing layer.

[0132] In the second embodiment, the film 20 may contain various plastic compounding agents and additives for the purpose of improving or modifying, for example, processability, heat resistance, weather resistance, mechanical properties, dimensional stability, oxidation resistance, slipperiness, release properties, flame retardancy, mold resistance, electrical properties, strength, etc. The content may be any amount ranging from a trace amount to several tens of percent depending on the purpose. In the above, examples of typical additives that may be contained include antiblocking agents, lubricants, crosslinking agents, antioxidants, ultraviolet absorbers, light stabilizers, fillers, reinforcing agents, antistatic agents, pigments, modifying resins, etc.

[0133] In the second embodiment, the thickness of the film 20 is not particularly limited as long as the effects of the present invention are exhibited, and is preferably about 25 μm or more, more preferably about 30 μm or more, and even more preferably about 40 μm or more, and is preferably about 250 μm or less, more preferably about 240 μm or less, and even more preferably about 230 μm or less. Preferred ranges of the thickness include about 25 to 250 μm, about 25 to 240 μm, about 25 to 230 μm, about 30 to 250 μm, about 30 to 240 μm, about 30 to 230 μm, about 40 to 250 μm, about 40 to 240 μm, and about 40 to 230 μm.

[0134] In the second embodiment, when the film 20 is composed of two or more layers, the thickness of each layer may be as described above for the film 20. For example, the thickness of the sulfur-based gas absorbing layer is preferably about 10 μm or more, more preferably about 15 μm or more, and even more preferably about 20 μm or more, and is, for example, about 100 μm or less, preferably about 95 μm or less, more preferably about 90 μm or less, and even more preferably about 85 μm or less, and preferred ranges of the thickness include about 10 to 100 μm, about 10 to 95 μm, about 10 to 90 μm, about 10 to 85 μm, about 15 to 100 μm, about 15 to 95 μm, about 15 to 90 μm, about 15 to 85 μm, about 20 to 100 μm, about 20 to 95 μm, about 20 to 90 μm, and about 20 to 85 μm. The thickness of the water absorption layer is preferably about 5 μm or more, more preferably about 6 μm or more, and even more preferably about 7 μm or more, and is preferably about 60 μm or less, more preferably about 55 μm or less, and even more preferably about 50 μm or less. Preferred ranges for the thickness include about 5 to 60 μm, about 5 to 55 μm, about 5 to 50 μm, about 6 to 60 μm, about 6 to 55 μm, about 6 to 50 μm, about 7 to 60 μm, about 7 to 55 μm, and about 7 to 50 μm.

[0135] (Method of manufacturing film 20) In this embodiment, the method for producing the film 20 is not particularly limited as long as the film 20 can be obtained, and known or commonly used film-forming methods and lamination methods can be applied. The film 20 can be produced by known film-forming methods and / or lamination methods, such as an extrusion method or a co-extrusion method, a cast molding method, a T-die method, a cutting method, or an inflation method. When the film 20 is composed of two or more layers, for example, the films constituting each layer that have been produced in advance may be laminated via an adhesive layer, a molten resin composition may be laminated on a layer that has been produced in advance by extrusion or co-extrusion, a plurality of layers may be simultaneously produced and laminated by melt pressure bonding, or one or more resins may be applied and dried to coat another layer.

[0136] In the first embodiment, the layers constituting the film 20, such as the water-absorbing layer (sulfur-based gas absorbing layer), may be laminated by extrusion or co-extrusion using an extrusion coating method, or may be laminated via an adhesive layer after film formation using an inflation method or cast method. Even in the case of the extrusion coating method, they may be laminated via an adhesive layer as necessary. Alternatively, a film for the water-absorbing layer (or sulfur-based gas absorbing layer) previously formed may be laminated and bonded via an adhesive layer laminated by an extrusion coating method, a dry lamination method, a non-solvent lamination method, or the like. Then, an aging treatment may be performed as necessary.

[0137] In the first embodiment, for example, when laminating a water-absorbing layer or the like by extrusion coating, first, the resin composition forming the layer such as the water-absorbing layer is heated and melted, and then expanded and stretched in the required width direction by a T-die to be extruded or co-extruded in a curtain shape, and the molten resin is allowed to flow down onto the surface to be laminated, and sandwiched between a rubber roll and a cooled metal roll, thereby forming the layer such as the water-absorbing layer, laminating it on the surface to be laminated, and adhering it to the surface to be laminated can be performed simultaneously. When laminating by extrusion coating, the melt flow rate (MFR) of the resin component contained in each layer is preferably 0.2 to 50 g / 10 min, more preferably 0.5 to 30 g / 10 min. If the MFR is smaller or larger than the above range, the processability is likely to be inferior. In this specification, the MFR is a value measured by a method based on JIS K7210.

[0138] In the first embodiment, the melt flow rate (MFR) of the resin component contained in each layer when the inflation method is used is preferably 0.2 to 10 g / 10 min, more preferably 0.2 to 9.5 g / 10 min. If the MFR is smaller or larger than the above range, the processability is likely to be poor.

[0139] In the second embodiment, the layers constituting the film 20, such as the sulfur-based gas absorbing layer (water absorbing layer), may be laminated by extrusion or co-extrusion using an extrusion coating method, or may be laminated via an adhesive layer after film formation using an inflation method or cast method. Even in the case of the extrusion coating method, they may be laminated via an adhesive layer as necessary. Alternatively, a film for a sulfur-based gas absorbing layer (or water absorbing layer) that has been previously formed may be laminated and bonded via an adhesive layer laminated by an extrusion coating method, a dry lamination method, a non-solvent lamination method, or the like. Then, an aging treatment may be performed as necessary.

[0140] In the second embodiment, for example, when laminating a sulfur-based gas absorbing layer or the like by extrusion coating, first, the resin composition forming the layer such as the sulfur-based gas absorbing layer is heated and melted, and then expanded and stretched in the required width direction by a T-die to be extruded or co-extruded in a curtain shape, and the molten resin is allowed to flow down onto the surface to be laminated, and sandwiched between a rubber roll and a cooled metal roll, so that the formation of the layer such as the sulfur-based gas absorbing layer and the lamination and adhesion to the surface to be laminated can be performed simultaneously. When laminating by extrusion coating, the melt flow rate (MFR) of the resin component contained in each layer is preferably 0.2 to 50 g / 10 min, more preferably 0.5 to 30 g / 10 min. If the MFR is smaller or larger than the above range, the processability is likely to be inferior. In this specification, the MFR is a value measured by a method based on JIS K7210.

[0141] In the second embodiment, the melt flow rate (MFR) of the resin component contained in each layer when the inflation method is used is preferably 0.2 to 10 g / 10 min, more preferably 0.2 to 9.5 g / 10 min. If the MFR is smaller or larger than the above range, the processability is likely to be poor.

[0142] In this embodiment, in order to improve the adhesion between the layers constituting the film 20, a desired surface treatment may be applied in advance to the surface of each layer as necessary. For example, a corona-treated layer, an ozone-treated layer, a plasma-treated layer, an oxidation-treated layer, or the like may be formed by optionally performing a pretreatment such as a corona discharge treatment, an ozone treatment, a low-temperature plasma treatment using oxygen gas or nitrogen gas, a glow discharge treatment, or an oxidation treatment using chemicals. Alternatively, various coating layers such as a primer coating layer, an undercoat coating layer, an anchor coating layer, an adhesive layer, and a vapor deposition anchor coating layer may be optionally formed on the surface to form a surface treatment layer. For the various coating layers, for example, a resin composition containing a polyester resin, a polyamide resin, a polyurethane resin, an epoxy resin, a phenol resin, a (meth)acrylic resin, a polyvinyl acetate resin, a polyolefin resin such as polyethylene or polypropylene, or a copolymer or modified resin thereof, or a cellulose resin as the main component of the vehicle may be used.

[0143] In this embodiment, each layer constituting the film 20 can be further uniaxially or biaxially stretched by a conventionally known method using a tenter system, a tubular system, or the like, as necessary.

[0144] <1-3. Manufacturing method of energy storage device> Fig. 8 is a flowchart showing a manufacturing procedure of the power storage device 10. The steps shown in Fig. 8 are performed by a manufacturing apparatus for the power storage device 10, for example.

[0145] The manufacturing equipment wraps the exterior member 101 around the electrode body 200 (step S100). The manufacturing equipment forms the first sealed portion 110 by heat-sealing the mutually facing surfaces (thermally adhesive resin layers) of the exterior member 101 (step S110). This completes the unfinished product shown in Figs. 4 and 5.

[0146] The manufacturing equipment folds the first sealing portion 110 so that the first sealing portion 110 contacts the second surface 140 (step S120). The manufacturing equipment folds the exterior member 101 in a state in which the electrode body 200 is stored, and forms the second sealing portion 120 by heat-sealing the mutually facing surfaces (thermally adhesive resin layers) of the exterior member 101 (step S130). This completes the electricity storage device 10.

[0147] <1-4.Features> In the electricity storage device 10 including the film 20 of the first embodiment, since the film 20 contains a water absorbing agent, the film 20 absorbs and retains moisture that has infiltrated from the heat-sealable resin layer 101C of the exterior member 101, thereby preventing the moisture from reaching the electrode assembly 200. In the electricity storage device 10 including the film 20 of the second embodiment, since the film 20 contains a sulfur-based gas absorbent, hydrogen sulfide generated from the electrode assembly 200 is absorbed by the film 20. As a result, the internal pressure of the exterior assembly 100 can be prevented from increasing excessively.

[0148] In the energy storage device 10 according to the first embodiment, the first sealing portion 110 is folded toward the second surface 140, which has a smaller area. That is, the first sealing portion 110 does not exist on the first surface 130, which has a larger area. Therefore, even if another energy storage device 10 is placed on the first surface 130, the other energy storage device 10 does not tilt. As a result, according to the energy storage device 10, when a plurality of energy storage devices 10 are stacked, unevenness in the distribution of pressure applied to the lower energy storage device 10 can be suppressed. In addition, when used in an all-solid-state battery, it is necessary to apply a high pressure uniformly from the outer surface of the battery to exhibit the battery performance, so that the packaging form of the present invention is preferable. In addition, in the energy storage device 10, the root portion of the first sealing portion 110 is on the side 135 of the exterior body 100. Therefore, according to the energy storage device 10, when the first sealing portion 110 is fitted onto the second surface 140, a wider bonding width can be ensured in the first sealing portion 110 compared to when the base portion of the first sealing portion 110 is located on the second surface 140.

[0149] [2. Second embodiment] In the electricity storage device 10 according to the first embodiment, the second sealed portion 120 is formed by folding the exterior member 101 and heat-sealing the mutually facing surfaces of the exterior member 101. However, the shape and the method of forming the second sealed portion 120 are not limited thereto. Note that, in the following, the portions different from the first embodiment will be mainly described, and the portions in common with the first embodiment will not be described.

[0150] <2-1. Configuration of the power storage device> Fig. 9 is a plan view diagrammatically illustrating an electricity storage device 10X according to the second embodiment, Fig. 10 is a side view diagrammatically illustrating an electricity storage device 10X, and Fig. 11 is a perspective view diagrammatically illustrating a lid body 400.

[0151] 9, 10, and 11, the exterior body 100X is formed by fitting a lid body 400 into each of the openings at both ends of an exterior member 101 wrapped around an electrode assembly 200. With the lid body 400 fitted in, the exterior member 101 and the lid body 400 are heat-sealed to form a second sealed portion 120X.

[0152] The lid 400 is a bottomed tray-like member having a rectangular shape in a plan view, and is formed by, for example, cold forming the exterior member 101. The lid 400 does not necessarily have to be made of the exterior member 101, and may be a metal molded product or a resin molded product. That is, the material constituting the lid 400 may include at least one of a resin material and a metal material. For example, the lid 400 may have a main body portion containing a metal material and a covering body containing a resin material that covers a part of the main body portion. The covering body may be a frame-shaped object of a resin molded product, or may be an adhesive film that is suitably bonded to both a metal material and a resin material. It is preferable that the main body portion is bonded to the exterior member 101 via the covering body. In the power storage device 10X, the lid 400 is arranged so that the bottom side of the lid 400 is located inside the exterior member 100X. In the power storage device 10X, the bottom side of the lid 400 does not necessarily have to be located inside the exterior member 100X. In the electricity storage device 10X, the bottom side of the lid body 400 may be located outside the exterior body 100X. When the lid body 400 is a metal molded product or a resin molded product, it is preferable that the material constituting the lid body 400 has a certain degree of thickness so that the exterior body 100X is prevented from deforming even when the electricity storage device 10X is arranged in a stacked manner. The minimum value of the thickness of the material constituting the lid body 400 is, for example, 1.0 mm, more preferably 3 mm, and further preferably 4 mm. The maximum value of the thickness of the material constituting the lid body 400 is, for example, 10 mm, more preferably 8.0 mm, and further preferably 7.0 mm. The maximum value of the thickness of the material constituting the lid body 400 may be 10 mm or more. The preferred ranges of thickness of the material constituting the lid body 400 are 1.0 mm to 10 mm, 1.0 mm to 8.0 mm, 1.0 mm to 7.0 mm, 3.0 mm to 10 mm, 3.0 mm to 8.0 mm, 3.0 mm to 7.0 mm, 4.0 mm to 10 mm, 4.0 mm to 8.0 mm, and 4.0 mm to 7.0 mm. In the present disclosure, when the lid body 400 is expressed as a metal molded product or a resin molded product, a film is not included as a material constituting the lid body 400. The film is, for example, a film defined by the JIS (Japanese Industrial Standards) [Packaging Terminology] standard.The film specified by the JIS [Packaging Terminology] standard is a plastic membrane having a thickness of less than 250 μm. The thickness of the material constituting the lid body 400 may vary depending on the part of the lid body 400. When the thickness of the material constituting the lid body 400 varies depending on the part of the lid body 400, the thickness of the material constituting the lid body 400 is the thickness of the thickest part.

[0153] In addition, when the electrode body 200 is stored, the electrode terminal 300 passes between the lid body 400 and the exterior member 101 and protrudes to the outside of the exterior body 100X. That is, the lid body 400 and the exterior member 101 are heat sealed with the electrode terminal 300 sandwiched between them. In the power storage device 10X, the position where the electrode terminal 300 protrudes to the outside does not necessarily have to be between the lid body 400 and the exterior member 101. For example, the electrode terminal 300 may protrude to the outside from a hole formed on any one of the six surfaces of the exterior body 100X. In this case, a small gap between the exterior body 100X and the electrode terminal 300 is filled with, for example, resin.

[0154] Furthermore, in the power storage device 10X, the lid body 400 and the electrode terminal 300 are provided as separate bodies. However, the lid body 400 and the electrode terminal 300 do not necessarily have to be provided as separate bodies. For example, the lid body 400 and the electrode terminal 300 may be formed integrally.

[0155] FIG. 12 is a diagram showing a first example in which the lid 400 and the electrode terminal 300 are integrally formed. As shown in FIG. 12, in the first example, the electrode terminal 300 is heat-sealed in advance to the side of the lid 400. For example, when the lid 400 is made of the exterior member 101, an adhesive film that adheres to both the metal and the resin described in the first embodiment may be disposed between the lid 400 and the electrode terminal 300. When the adhesive film is made of two or more layers, it is preferable to dispose a resin film made of a polyolefin resin on the side that is joined to the lid 400. When the adhesive film is made of two or more layers, it is preferable to dispose a resin film made of an acid-modified polyolefin resin obtained by graft-modifying a polyolefin resin with an acid such as maleic anhydride on the side that is joined to the electrode terminal 300.

[0156] Fig. 13 is a diagram showing a second example in which the lid 400 and the electrode terminal 300 are integrally formed. As shown in Fig. 13, in the second example, the electrode terminal 300 passes through a hole formed in the bottom surface portion of the lid 400. A small gap in the hole in the bottom surface of the lid 400 is filled with, for example, resin.

[0157] Furthermore, in the power storage device 10X, a gas valve may be attached to a hole formed in the second sealing portion 120X or any one of the six faces of the exterior body 100X. The gas valve is configured, for example, as a check valve or a breaker valve, and is configured to reduce the pressure inside the exterior body 100X when the pressure increases due to gas generated inside the power storage device 10X.

[0158] <2-2. Manufacturing method of electricity storage device> Fig. 14 is a flowchart showing a manufacturing procedure for the power storage device 10X. The steps shown in Fig. 14 are performed, for example, by a manufacturing apparatus for the power storage device 10X.

[0159] The manufacturing equipment wraps the exterior member 101 around the electrode body 200 (step S200). The manufacturing equipment forms the first sealed portion 110 by heat-sealing the mutually facing surfaces (thermally adhesive resin layers) of the exterior member 101 (step S210). This completes the unfinished product shown in Figs. 4 and 5.

[0160] The manufacturing equipment bends the first sealing portion 110 so that the first sealing portion 110 contacts the second surface 140 (step S220). The manufacturing equipment houses the electrode body 200 in the unfinished product produced in step S220 and attaches the lid body 400 to each of the openings at both ends (step S230). The manufacturing equipment forms the second sealing portion 120X by heat-sealing the exterior member 101 and the lid body 400 (step S240). This completes the electricity storage device 10X.

[0161] <2-3.Features> In the power storage device 10X according to the second embodiment, the first sealing portion 110 is also bent toward the second surface 140 having a smaller area. Therefore, according to the power storage device 10X, when a plurality of power storage devices 10X are stacked, unevenness in the distribution of pressure applied to the lower power storage device 10X can be suppressed.

[0162] <2-4.Other features> In the power storage device 10X according to the second embodiment, the first sealing portion 110 does not necessarily have to be bent towards the second surface 140 having a smaller area. For example, the first sealing portion 110 may be bent towards the first surface 130 having a larger area. Furthermore, the root portion of the first sealing portion 110 does not necessarily have to be on the side 135 of the exterior body 100X. The root portion of the first sealing portion 110 may be located on a surface of the exterior body 100X other than the lid body 400, for example. Even in this case, the power storage device 10X according to the second embodiment includes, for example, the following features.

[0163] The energy storage device 10X comprises an electrode body (electrode body 200) and an exterior body (exterior body 100X) that seals the electrode body (electrode body 200). The exterior body (exterior body 100X) is wrapped around the electrode body (electrode body 200) and comprises an exterior member (exterior member 101) having openings formed at both ends, and a lid body (lid body 400) that seals the openings.

[0164] In the electricity storage device 10X, the second sealed portion 120X is not formed by heat sealing mutually facing surfaces of the exterior member 101 as in the first embodiment (see FIG. 7). In the electricity storage device 10X, the opening of the exterior member 101 wrapped around the electrode body 200 is sealed by the lid body 400. That is, the second sealed portion 120X is formed in the portion where the lid body 400 and the exterior member 101 overlap (see FIGS. 9 and 10). With this configuration, the area of ​​the second sealed portion 120X can be easily narrowed by adjusting the depth L3 (FIG. 11) of the lid body 400.

[0165] Furthermore, in the electricity storage device 10X, at a position of the exterior member 101 that covers the corner C1 (FIGS. 9 and 10) of the electrode body 200, no excessive load is generated due to the corner C1 piercing the exterior member 101. This is because, as described above, in the electricity storage device 10X, the second sealed portion 120X is not formed by heat sealing mutually facing surfaces of the exterior member 101 as in the first embodiment.

[0166] Furthermore, the manufacturing procedure of the power storage device 10X is not limited to the procedure shown in the flowchart of Fig. 14. For example, the power storage device 10X may be manufactured according to the procedure shown in the flowchart of Fig. 15.

[0167] FIG. 15 is a flowchart showing another manufacturing procedure of the power storage device 10X according to the second embodiment. The steps shown in FIG. 15 are performed, for example, by a manufacturing apparatus for the power storage device 10X. The manufacturing apparatus attaches a member (for example, a member shown in FIGS. 12 and 13) in which the electrode terminal 300 and the lid body 400 are integrated to the electrode body 200 (step S250). For example, the electrode terminal 300 is welded to the electrode body 200. Thereafter, the manufacturing apparatus wraps the exterior member 101 around the electrode body 200 (step S260). The manufacturing apparatus forms the first sealed portion 110 by heat-sealing the mutually facing surfaces (thermally adhesive resin layers) of the exterior member 101, and forms the second sealed portion 120X by heat-sealing the exterior member 101 and the lid body 400 together (step S270). This completes the power storage device 10X. The power storage device 10X may be manufactured by such a procedure.

[0168] [3. Third embodiment] In a battery manufacturing process, a temporarily sealed electricity storage device is generally subjected to a process of aging in a predetermined temperature environment for a predetermined time for the purpose of permeating an electrolyte into the electrode body (hereinafter referred to as an aging process). In the aging process, gas is generated from the electrode body 200, and it is necessary to discharge the gas to the outside of the battery. In the electricity storage device 10X according to the second embodiment, no mechanism is provided for releasing the gas generated in the aging process in the final stage of manufacturing the electricity storage device 10X. In the electricity storage device 10Y according to the third embodiment, a mechanism is provided for releasing the gas generated from the electrode body 200 in the final stage of manufacturing the electricity storage device 10Y. In the following, differences from the second embodiment will be mainly described, and descriptions of parts common to the second embodiment will be omitted.

[0169] <3-1. Configuration of the power storage device> Fig. 16 is a side view showing a state in which the exterior member 101Y is wrapped around the electrode body 200 during the manufacture of the electricity storage device 10Y. Fig. 17 is a bottom view showing a state in which the exterior member 101Y is wrapped around the electrode body 200 and a lid body 400 is attached to the exterior member 101Y during the manufacture of the electricity storage device 10Y.

[0170] As shown in Fig. 16 and Fig. 17, the piece 150 is formed in a state where the exterior member 101Y is wound around the electrode body 200. The piece 150 is formed by joining mutually facing surfaces of the exterior member 101Y in a state where the exterior member 101Y is wound around the electrode body 200. More specifically, the piece 150 is formed by joining (heat sealing) the peripheries of the mutually facing surfaces in a state where the exterior member 101Y is wound around the electrode body 200. That is, in the piece 150, a first sealed portion 154 is formed on the periphery.

[0171] Further, in the piece 150, a space 152 is formed where the opposing surfaces of the exterior member 101Y are not joined to each other. In the vicinity of the side 135, a joining region 151 where the opposing surfaces of the exterior member 101Y are joined to each other and an unjoined region 153 where the opposing surfaces of the exterior member 101Y are not joined to each other are arranged alternately. That is, in the piece 150, a pattern of the joining region 151 is formed along the side 135.

[0172] The gas generated from the electrode body 200 is discharged to the outside of the exterior body 100Y by releasing the sealed state of the exterior body 100Y, for example by cutting off a part of the piece 150. Note that the gas discharged to the outside of the exterior body 100Y here is not necessarily limited to the gas generated from the electrode body 200, and may be a gas other than the gas generated from the electrode body 200, such as air, water vapor, or hydrogen sulfide.

[0173] Thereafter, the portion including the vicinity of the side 135 is heat-sealed in a strip shape, thereby sealing the exterior body 100Y again. This completes the electricity storage device 10Y. In the completed electricity storage device 10Y, in the vicinity of the side 135, regions where the bonding strength between the mutually facing surfaces of the exterior member 101Y is strong and regions where the bonding strength between the surfaces is weak are alternately arranged along the side 135. In other words, in the heat-sealed portion in the vicinity of the side 135, thin portions and thick portions are alternately arranged along the side 135. This is because, by heat-sealing the vicinity of the side 135 again, the unbonded region 153 is single-sealed, but the bonded region 151 is double-sealed.

[0174] <3-2. Manufacturing method of electricity storage device> Fig. 18 is a flowchart showing a manufacturing procedure for the power storage device 10Y. The steps shown in Fig. 18 are performed by, for example, a manufacturing apparatus for the power storage device 10Y.

[0175] The manufacturing equipment wraps the exterior member 101Y around the electrode body 200 (step S300). The manufacturing equipment forms the first sealed portion 154 by heat-sealing the peripheral edges of the mutually facing surfaces (thermally adhesive resin layers) of the exterior member 101Y (step S310). The manufacturing equipment forms a pattern of the bonding region 151 by heat-sealing the mutually facing surfaces of the exterior member 101Y in the vicinity of the side 135 (step S320).

[0176] The manufacturing equipment attaches the lid body 400 to each of the openings at both ends with the electrode body 200 housed in the unfinished product produced in step S320 (step S330). The manufacturing equipment forms the second sealed portion 120X by heat-sealing the exterior member 101Y and the lid body 400 (step S340). Then, an aging process is performed.

[0177] The manufacturing equipment removes gas generated in the aging process by, for example, cutting off piece 150 (step S350). The manufacturing equipment reseals exterior body 100Y by heat-sealing a portion of piece 150 including bonding region 151 into a strip shape and removing the edge portion (step S360). Thereafter, piece 150 is folded toward second surface 140 to complete electricity storage device 10Y.

[0178] <3-3.Features> In the electricity storage device 10Y according to the third embodiment, the piece 150 including the first sealing portion 154 is also folded toward the second surface 140 having a smaller area. Therefore, according to the electricity storage device 10Y, when a plurality of electricity storage devices 10Y are stacked, unevenness in the distribution of pressure applied to the lower electricity storage device 10Y can be suppressed. When used in an all-solid-state battery, it is necessary to apply high pressure uniformly from the outer surface of the battery to exhibit battery performance, and therefore the packaging form of the present invention is preferable.

[0179] [4. Fourth embodiment] In the power storage device 10X according to the second embodiment, the position from which the electrode terminal 300 protrudes to the outside is between the lid body 400 and the exterior member 101. However, the position from which the electrode terminal 300 protrudes to the outside is not limited thereto. Note that, in the following, the description will be centered on the parts different from the second embodiment, and the description of the parts in common with the second embodiment will be omitted.

[0180] <4-1. Configuration of the power storage device> FIG. 19 is a plan view that typically shows an electricity storage device 10XA according to a fourth embodiment. FIG. 20 is a side view that typically shows an electricity storage device 10XA. The exterior body 100X of the electricity storage device 10XA includes a pair of long sides 100XA and a pair of short sides 100XB in a plan view. The exterior body 100X is configured by fitting a lid body 400 into each of the openings along the long sides 100XA of an exterior member 101 that is wrapped around an electrode body 200. With the lid body 400 fitted in, the exterior member 101 and the lid body 400 are heat-sealed to form a second sealed portion 120X. A through hole (not shown) is formed in the lid body 400. Two electrode terminals 300 protrude from the through holes of the lid body 400 to the outside of the exterior body 100X. The two electrode terminals 300 are shaped to fit along the long side 100XA of the exterior body 100X. Small gaps between the through holes and the electrode terminals 300 are filled with, for example, resin. In the fourth embodiment, the first sealing portion 110 is formed on one of the pair of short sides 100XB.

[0181] In the thickness direction (arrow UD direction) of the power storage device 10XA, the position from which the electrode terminal 300 of the lid body 400 protrudes can be selected arbitrarily. In the fourth embodiment, as shown in Fig. 20, the electrode terminal 300 protrudes from approximately the center of the lid body 400 to the outside of the exterior body 100X in the thickness direction of the power storage device 10XA. The length of the electrode terminal 300 in the depth direction (arrow FB direction) of the power storage device 10XA can be selected arbitrarily. In the fourth embodiment, the length of the electrode terminal 300 in the depth direction (arrow FB direction) of the power storage device 10XA is substantially the same as the length of the electrode body 200.

[0182] <4-2.Features> In the power storage device 10XA according to the fourth embodiment, the electrode terminals 300 are arranged along the long side 100XA that is longer in the depth direction, so that larger electrode terminals 300 can be used, and therefore a high-output power storage device 10XA can be provided.

[0183] [5. Modifications] The above-mentioned embodiments are examples of forms that the power storage device according to the present invention can take, and are not intended to limit the forms. The power storage device according to the present invention can take forms different from those exemplified in the above-mentioned embodiments. One example is a form in which a part of the configuration of each of the above-mentioned embodiments is replaced, changed, or omitted, or a form in which a new configuration is added to each of the above-mentioned embodiments. Some examples of modified examples of each of the above-mentioned embodiments are shown below. The above-mentioned embodiments can also be combined within a range that does not cause technical contradiction.

[0184] <5-1> In the first to fourth embodiments, one exterior member is wound around the electrode body 200. However, it is not necessary to wind one exterior member around the electrode body 200. For example, two or more exterior members may be wound around the electrode body 200.

[0185] FIG. 21 is a side view showing a state in which the exterior members 101Z1 and 101Z2 are wound around the electrode body 200 during the manufacturing process of the electric storage device in the modified example. As shown in FIG. 21, the electrode body 200 is covered with the exterior members 101Z1 and 101Z2. The first sealing portion 110Z is formed by joining the opposing surfaces of the exterior members 101Z1 and 101Z2. In this example, each first sealing portion 110Z is folded toward the second surface 140Z side, not toward the first surface 130Z side. Even with this configuration, it is possible to achieve the effect of suppressing unevenness in the distribution of pressure applied to the lower electric storage device when multiple electric storage devices are stacked. When used in an all-solid-state battery, it is necessary to apply a high pressure uniformly from the outer surface of the battery to exhibit battery performance, so the packaging form of the present invention is preferable. In this example, each first sealing portion 110Z does not necessarily need to be folded. In this modification, each sealing portion 110Z may be sealed in a state in which it sandwiches a part of the electrode terminal 300. Furthermore, in this modification, each first sealing portion 110Z does not need to be formed on the side 135Z, and may protrude outward from approximately the center of the second surface 140Z in the thickness direction of the power storage device.

[0186] <5-2> In the first to fourth embodiments, the electrode body 200 is a so-called stack type configured by stacking a plurality of electrodes 210, but the form of the electrode body 200 is not limited to this. The electrode body 200 may be, for example, a so-called wound type configured by winding a positive electrode and a negative electrode via a separator. The electrode body 200 may also be configured by stacking a plurality of so-called wound type electrode bodies.

[0187] <5-3> In the first to fourth embodiments, the second surface 140 is a plane extending downward from the first surface 130 at a substantially right angle. However, the form of the second surface 140 is not limited to this. For example, consider a case where the electrode body 200 is a wound electrode body having a plane surface and a curved surface formed on the outer periphery. Here, it is assumed that the area of ​​the plane surface is larger than the area of ​​the curved surface, the first surface 130 covers the plane surface of the electrode body, and the second surface 140 covers the curved surface of the electrode body. In this case, the second surface 140 may be configured as a curved surface. In this case, the boundary portion where the second surface 140 extends downward from the first surface 130 is the side 135.

[0188] <5-4> Furthermore, in the third embodiment, the bonding regions 151 are formed in four locations. However, the number of locations where the bonding regions 151 are formed is not limited to this. For example, the bonding regions 151 may be formed in two locations near both ends along the side 135, in one location near the center of the side 135, or in five or more locations.

[0189] <5-5> In the second embodiment, the electrode terminal 300 is disposed in the second sealing portion 120X, but the position where the electrode terminal 300 is disposed in the exterior body 100X is not limited thereto. For example, as shown in FIG. 22, in the second embodiment, the electrode terminal 300 can also be disposed in the first sealing portion 110. In other words, the first sealing portion 110 is sealed in a state where the electrode terminal 300 is sandwiched between them. In this modification, at least one of the two electrode terminals 300 may be folded toward the second surface 140 side, may be folded toward the opposite side to the second surface 140, or may not be folded so as to protrude outward from the side 135. In this modification, the electrode terminal 300 and the first sealing portion 110 can be easily sealed, so that the sealing property of the exterior body 100X is improved. In addition, the electrode body 200 can be easily accommodated in the exterior body 100X. In this modification, for example, the lid body 400 is fitted into each of the openings at both ends of the exterior member 101X as in the second embodiment. With the lid body 400 fitted, the exterior member 101X and the lid body 400 are heat sealed together to form the second sealed portion 120. In the first embodiment, the electrode terminal 300 may also be disposed in the first sealed portion 110.

[0190] <5-6> In the second embodiment, the configuration of the lid 400 can be changed arbitrarily. FIG. 23 is a perspective view showing a lid 500 of a modified example of the lid 400. The lid 500 is, for example, plate-shaped and includes a first surface 500A facing the electrode body 200 (see FIG. 9) and a second surface 500B opposite to the first surface 500A. A hole 500C penetrating the first surface 500A and the second surface 500B is formed in the center of the lid 500. The material constituting the lid 500 includes, for example, a resin material. The lid 500 may be configured including a metal material. That is, the material constituting the lid 500 may include at least one of a resin material and a metal material. For example, the lid 500 may have a main body portion including a metal material and a covering body including a resin material that covers a part of the main body portion. The covering body may be a frame-shaped object of a resin molded product, or an adhesive film that is suitably bonded to both a metal material and a resin material. The main body is preferably joined to the exterior member 101 via a cover. In this modification, a terminal adhesive film 530 that adheres to both the electrode terminal 300 and the lid body 500 is preferably attached to a predetermined range including a portion of the electrode terminal 300 that is joined to the lid body 500. The specifications of the terminal adhesive film 530 are the same as those of the terminal adhesive film 30 described in the first embodiment. In this modification, the manufacturing method of the electricity storage device 10X may include a step of electrically connecting the electrode body 200 and the electrode terminal 300, a step of manufacturing the lid body 500, and a step of inserting the electrode terminal 300 connected to the electrode body 200 into the hole 500C of the lid body 500 (see FIG. 24, hereinafter referred to as the "insertion step").

[0191] When the lid body 500 is plate-shaped, it is preferable that the lid body 500 has a certain degree of thickness so that deformation of the exterior body 100X is suppressed even when the power storage device 10X is arranged in a stacked manner. From another viewpoint, when the lid body 500 is plate-shaped, it is preferable that the side surface of the lid body 500 has a certain degree of thickness so that the side surface of the lid body 500 and the exterior member 101X can be suitably heat-sealed when forming the second sealing portion 120X. The minimum value of the thickness of the lid body 500 is, for example, 1.0 mm, more preferably 3 mm, and further preferably 4 mm. The maximum value of the thickness of the lid body 500 is, for example, 10 mm, more preferably 8.0 mm, and further preferably 7.0 mm. The maximum value of the thickness of the lid body 500 may be 10 mm or more. The preferred ranges of the thickness of the material constituting the lid body 500 are 1.0 mm to 10 mm, 1.0 mm to 8.0 mm, 1.0 mm to 7.0 mm, 3.0 mm to 10 mm, 3.0 mm to 8.0 mm, 3.0 mm to 7.0 mm, 4.0 mm to 10 mm, 4.0 mm to 8.0 mm, and 4.0 mm to 7.0 mm. In the present disclosure, when the lid body 500 is expressed as a plate-like body, the film defined by the [Packaging Terminology] standard of the JIS (Japanese Industrial Standards) is not included as the material constituting the lid body 500. The thickness of the lid body 500 may vary depending on the part of the lid body 500. When the thickness of the lid body 500 varies depending on the part, the thickness of the lid body 500 is the thickness of the thickest part.

[0192] The lid 500 may be constructed of a member divided into a first portion 510 and a second portion 520, and may be manufactured by joining the first portion 510 and the second portion 520 so as to sandwich the electrode terminal 300 and the terminal adhesive film 530. In these modified examples, if a gap occurs between the terminal adhesive film 530 and the hole 530C, the gap is preferably filled with a resin material such as hot melt or by resin welding.

[0193] When the lid body 500 is composed of a member divided into the first portion 510 and the second portion 520, the relationship between the width LA of the electrode terminal 300 and the width LB of the lid body 500 can be selected arbitrarily. From the viewpoint of more firmly bonding the electrode terminal 300 and the lid body 500, it is preferable that the ratio RA of the width LA to the width LB is 50% or more. In the example shown in FIG. 25, the width LA and the width LB are substantially equal, in other words, the ratio RA is 100%. When the ratio RA is 50% or more, the area of ​​the electrode terminal 300 that is bonded to the lid body 500 is large, so that the electrode terminal 300 and the lid body 500 can be more firmly bonded by heating the electrode terminal 300. In this modification, it is preferable that the width LC of the terminal adhesive film 530 is substantially equal to the width LA of the electrode terminal 300.

[0194] The lid body 500 may be manufactured by insert molding the lid body 500 onto the electrode terminal 300 to which the terminal adhesive film 530 is attached. In this case, the manufacturing method of the electricity storage device 10X includes a step of electrically connecting the electrode body 200 and the electrode terminal 300, and a step of insert molding the lid body 500 onto the electrode terminal 300 in a state connected to the electrode body 200 (hereinafter referred to as an "insert molding step"). After the insert molding step, the exterior member 101 is wrapped around the electrode body 200 and the lid body 500. Note that, in the insert molding step, it is preferable to place a heat insulating material for protecting the electrode body 200 between the electrode body 200 and the portion where the lid body 500 is formed. It is preferable to remove the heat insulating material after the insert molding step.

[0195] In these modified examples, as shown in FIG. 26, the exterior body 100X may be formed by joining the exterior member 101 and the second surface 500B of the lid body 500 with the lid body 500 fitted therein, to form the second sealing portion 120X. The joining means between the exterior member 101 and the second surface 500B of the lid body 500 is, for example, heat sealing. In this modified example, the exterior member 101 is joined to a wider area of ​​the lid body 500, so that the sealing property of the exterior body 100X is improved. Note that the lid body may be formed by folding the terminal adhesive film 530, and the second sealing portion 120X may be formed by joining any part of the terminal adhesive film 530 to the exterior member 101X. In these modified examples, it is preferable that a barrier layer is laminated on at least a part of the surface of the lid body 500. Alternatively, when the lid body 500 has a plurality of layers, a barrier layer may be formed on any layer. The material constituting the barrier layer is, for example, aluminum, steel plate, or stainless steel.

[0196] FIG. 27 is a front view of a lid body 600 of another modified example of the lid body 400 in the second embodiment. The lid body 600 includes a metal part 610 that is a part where metal is exposed on the surface, and the metal part 610 and the electrode 210 of the electrode body 200 are welded. The lid body 600 may be entirely composed of the metal part 610, or the metal part 610 may be partially formed. When the metal part 610 is partially formed, the lid body 600 is composed of a material having a multilayer structure including a metal layer. When the lid body 600 is composed of a material having a multilayer structure with a metal layer as an intermediate layer, the metal part 610 is a part where layers other than the metal layer are partially removed so that the metal layer is exposed. In the example shown in FIG. 27, the metal part 610 of the lid body 600 functions as an electrode terminal, so that a space between the lid body 600 and the electrode 210 is not required. Therefore, the electricity storage device 10X (see FIG. 9) can be configured to be small.

[0197] Fig. 28 is a front view of a lid body 700 which is another modified example of the lid body 400 in the second embodiment. The lid body 700 includes a metal portion 710 made of a metal material, and a non-metal portion 720 connected to the metal portion 710 and made of a resin material. The metal portion 710 is welded to the electrode 210 of the electrode body 200. In the example shown in Fig. 28, the metal portion 710 of the lid body 700 functions as an electrode terminal, and therefore no space is required between the lid body 700 and the electrode 210. This allows the power storage device 10X (see Fig. 9) to be configured in a small size.

[0198] <5-7> The electricity storage device 10X of the second embodiment or the modified example of the second embodiment may include the film 20 shown in the first embodiment. In the electricity storage device 10X, the location where the film 20 is arranged can be selected arbitrarily as long as it is inside the barrier layer 101B (see FIG. 2) of the exterior member 101. By arranging the film 20 of the first aspect inside the barrier layer 101B of the exterior member 101, it is possible to suppress the intrusion of moisture from the end of the heat-sealable resin layer 101C of the exterior member 101 and the intrusion of moisture contained in the heat-sealable resin layer 101C of the exterior member 101 into the electrode body 200. That is, in the electricity storage device 10X including the film 20 of the first aspect, since the film 20 contains a water absorbing agent, the film 20 absorbs and holds the moisture that has infiltrated from the heat-sealable resin layer 101C of the exterior member 101, and thus it is possible to suppress the moisture from reaching the electrode body 200. Furthermore, by disposing the film 20 of the second embodiment on the inner side of the barrier layer 101B of the exterior member 101, for example, when the electrode body 200 is an all-solid-state battery, it is possible to absorb gases such as hydrogen sulfide generated by contact between a solid electrolyte layer included in an element constituting the all-solid-state battery and moisture. That is, in the electricity storage device 10X including the film 20 of the second embodiment, the film 20 contains a gas absorbent, and therefore gases such as hydrogen sulfide generated from the electrode body 200 are absorbed by the film 20.

[0199] 29A is a cross-sectional view showing a modified example of the electricity storage device 10X of the second embodiment. In the example shown in FIG. 29A, the film 20 is disposed between the exterior member 101 and the electrode body 200 so as to cover substantially the entire upper and lower surfaces of the electrode body 200. The film 20 and the inner surface of the exterior member 101 (thermally adhesive resin layer 101C) may or may not be bonded to each other. At least a portion of the film 20 may be disposed between the exterior member 101 and the lid body 500.

[0200] FIG. 29B is a cross-sectional view showing another modified example of the electricity storage device 10X of the second embodiment. In the example shown in FIG. 29B, the film 20 is disposed between the lid body 500 and the electrode body 200 so as to cover substantially the entire side surface of the electrode body 200. The film 20 and the first surface 500A of the lid body 500 may be bonded or not bonded. The film 20 and the first surface 500A of the lid body 500 may be in contact or may be spaced apart. The film 20 may be disposed between the exterior member 101 and the electrode body 200 so as to cover substantially the entire electrode body 200. The film 20 and the inner surface (thermally adhesive resin layer 101C) of the exterior member 101 may be bonded or not bonded.

[0201] FIG. 29C is a cross-sectional view showing another modified example of the electricity storage device 10X of the second embodiment. In the example shown in FIG. 29C, the electricity storage device 10X has a terminal adhesive film 530 that adheres to both metal and resin between the electrode terminal 300 and the lid body 500. In the example shown in FIG. 29C, the film 20 is used as the terminal adhesive film 530. The film 20 is preferably disposed at least in the hole 500C of the lid body 500. The film 20 may be exposed from the hole 500C of the lid body 500. The electricity storage device 10X including the lid body 500 may have a risk of moisture intrusion from the hole 500C of the lid body 500. In the electricity storage device 10X including the film 20 of the first aspect, since the film 20 contains a water absorbing agent, the film 20 absorbs and holds the moisture that has infiltrated from the hole 500C of the lid body 500, and thus the moisture can be prevented from reaching the electrode body 200. In the electricity storage device 10X including the film 20 of the second embodiment, the film 20 contains a gas absorbent, and therefore gases such as hydrogen sulfide generated from the electrode body 200 are absorbed by the film 20. For this reason, gases such as hydrogen sulfide are less likely to be released to the outside through the holes 500C of the lid body 500.

[0202] 23, when the lid body 500 is composed of a member divided into at least a first portion 510 and a second portion 520, the film 20 may be disposed at least partially between the first portion 510 and the second portion 520. Also, for example, when the lid body 500 is composed of one part and the electrode terminal 300 is disposed between the top surface of the lid body 500 and the exterior member 101, the film 20 as the terminal adhesive film 530 may be disposed between the top surface of the lid body 500 and the exterior member 101.

[0203] <5-8> In the first embodiment, the second sealed portion 120 is formed by folding the exterior member 101 and heat-sealing the thermally adhesive resin layers of the exterior member 101. However, the method of forming the second sealed portion 120 is not limited to this. FIG. 30 is a plan view that shows a schematic diagram of an electricity storage device 10 having a second sealed portion 120Y of a modified example. The exterior member 101 has a protruding portion 101XA that extends outward from the exterior body 100, and the thermally adhesive resin layers of the protruding portion 101XA are heat-sealed to each other to form the second sealed portion 120Y. In the portion of the protruding portion 101XA where the electrode terminal 300 is disposed, the thermally adhesive resin layer of the protruding portion 101XA and the electrode terminal 300 are heat-sealed. According to this modified example, the second sealed portion 120Y can be heat-sealed more firmly, so that the hermeticity of the exterior body 100 is improved. In this modification, the protruding portion 101XA may be cut as necessary except for the portion heat-sealed to the electrode terminal 300. This modification can also be applied to the modification shown in FIG.

[0204] <5-9> In the first embodiment, the method of forming the first sealing portion 110 can be selected arbitrarily. As shown in FIG. 31, for example, the manufacturing apparatus may form the first sealing portion 110 by pressing the seal bar 800 to a position away from the base 135X of the portion 110Y of the exterior body 100 where the first sealing portion 110 is to be formed (see FIG. 8) in step S110. According to this manufacturing method, as shown in FIG. 32, the first sealing portion 110 is formed with a recess 110X that is a trace of the seal bar 800 being pressed. In the portion of the exterior body 100 where the recess 110X is formed, the surfaces (thermally adhesive resin layers) of the exterior member 101 facing each other are directly joined to each other. Between the recess 110X and the base 135X of the exterior body 100, a poly pool 900 in which a part of the resin constituting the exterior member 101 has melted out is formed between the surfaces of the exterior member 101 facing each other. In the portion between the recess 110X and the base 135X of the exterior body 100, the surfaces (thermally adhesive resin layers) of the exterior member 101 facing each other are joined via the poly pool 900. That is, in this modified example, the first sealing portion 110 includes a portion where the surfaces of the exterior member 101 facing each other are directly joined, and a portion where the surfaces of the exterior member 101 facing each other are joined via the poly pool 900. The poly pool 900 prevents water vapor and the like from entering the interior of the exterior body 100 from the outside, thereby improving the barrier property of the exterior body 100. When the seal bar 800 is pressed against the portion 110Y, it is necessary that the surfaces of the exterior member 101 facing each other in the portion where the poly pool 900 is formed, in other words, in the portion between the recess 110X and the base 135X, are in contact with each other.

[0205] The distance X between the root 135X and the edge 810 of the seal bar 800 in the LR direction, in other words, the distance between the root 135X and the recess 110X in the LR direction, can be arbitrarily selected. From the viewpoint of forming the poly pool 900 in a wider range, the distance X is, for example, preferably 1 mm or more, more preferably 1.5 mm or more, and even more preferably 1.7 mm or more. From the viewpoint of forming the first sealing portion 110 compactly, the distance X is, for example, preferably 10 mm or less, more preferably 5 mm or less, and even more preferably 3 mm or less. The preferred range of the distance X is, for example, about 1 mm or more and 10 mm or less, about 1 mm or more and 5 mm or less, about 1 mm or more and 3 mm or less, about 1.5 mm or more and 10 mm or less, about 1.5 mm or more and 5 mm or less, about 1.5 mm or more and 3 mm or less, about 1.7 mm or more and 10 mm or less, about 1.7 mm or more and 5 mm or less, and about 1.7 mm or more and 3 mm or less. The distance X is most preferably, for example, 2 mm. The distance X may be substantially 0. When the distance X is substantially 0, the seal bar 800 is pressed against the exterior body 100 so that the base 135X and the edge 810 of the seal bar 800 substantially coincide with each other. Note that substantially coinciding includes a case where the base 135X and the edge 810 of the seal bar 800 completely coincide with each other, and a case where the positions of the base 135X and the edge 810 of the seal bar 800 are slightly shifted due to an error during manufacturing or the like. Therefore, the distance X being substantially 0 also includes a case where the distance X is less than 1 mm, for example. These modified examples can be similarly applied to the second to fourth embodiments. Note that depending on the shape of the portion of the recess 110X corresponding to the edge 810 of the seal bar 800, the distance between the base 135X and the recess 110X may not be constant. In such a case, the distance X may be the distance between the center of the recess 110X and the center of the base 135X in the FB direction. In another example, the distance X may be calculated based on the average value of a plurality of values ​​including the maximum and minimum values ​​of the distance between the base 135X and the recess 110X. Similarly, depending on the shape of the base 135X, the distance between the base 135X and the recess 110X may not be constant. In such a case, the distance X may be the distance between the center of the base 135X and the center of the recess 110X in the FB direction.In another example, the distance X may be calculated based on the average value of a plurality of values ​​including the maximum and minimum values ​​of the distance between the recess 110X and the base 135X.

[0206] In the second embodiment, as shown in FIG. 33, the exterior body 100X may include a barrier film 91 that suppresses permeation of the electrolyte. The barrier film 91 is preferably disposed at least between the inner surface of the exterior member 101X and the electrode body 200. The barrier film 91 is preferably bonded to the inner surface of the exterior member 101X. The barrier film 91 is preferably made of a material that allows permeation of gas generated in the exterior body 100X. The material constituting the barrier film 91 is, for example, a resin film or a porous film. Since the exterior body 100X has the barrier film 91, deterioration of the exterior member 101X due to the electrolyte can be suppressed.

[0207] In the first embodiment, as shown in FIG. 34, the exterior body 100 may include a buffer film 92 for increasing the strength of the exterior member 101. The buffer film 92 is preferably disposed on at least a corner 100Z of the exterior body 100 among the inner surface of the exterior member 101. Since the exterior body 100 includes the buffer film 92, it is possible to suppress the occurrence of pinholes in the exterior body 100. The material constituting the buffer film 92 is, for example, a polyester-based material, a polyolefin-based material, or a fluorine-based material. In this modification, as shown in FIG. 34, the second sealing portion 120 may be formed by joining the inner surface of the exterior member 101 and the electrode terminal 300. It is preferable that the space 93 between the second sealing portion 120 and the electrode body 200 is filled with an electrolyte.

[0208] In the first embodiment, it has been explained that an adhesive film for a terminal 30 that adheres to both metal and resin may be disposed between the electrode terminal 300 and the exterior member 101, but in other embodiments, an adhesive film for a terminal 30 may be disposed in a similar manner.

[0209] In the second embodiment, it has been explained that an adhesive film for terminals 30 that adheres to both metal and resin, similar to that in the first embodiment, may be disposed between the lid body 400 and the electrode terminal 300, but an adhesive film may also be disposed in a similar manner in other embodiments.

[0210] 6. Working Examples The inventors of the present application manufactured electricity storage devices of Examples 1 and 2 and Comparative Example 1, and conducted tests to confirm whether moisture penetrates into the electrode body. In the following, for the sake of convenience, among the elements constituting the electricity storage devices of Examples 1 and 2 and Comparative Example 1, the same elements as those in the embodiment may be described by using the same reference numerals as those in the embodiment.

[0211] The power storage devices of Examples 1 and 2 and Comparative Example 1 have a configuration similar to that of the power storage device 10X of the second embodiment. The power storage devices of Examples 1 and 2 and Comparative Example 1 include two lid bodies 500 (see FIG. 23). However, in the power storage devices of Examples 1 and 2 and Comparative Example 1, the two lid bodies 500 are not divided into a first portion 510 and a second portion 520. The size of the two lid bodies 500 is 100 mm in width, 30 mm in height, and 5 mm in thickness. The power storage devices of Examples 1 and 2 and Comparative Example 1 have an aluminum block instead of the electrode body 200. The size of the aluminum block is 100 mm in width, 30 mm in height, and 150 mm in thickness.

[0212] The inventor of the present application bonded the film 20 of the first embodiment to the first surface 500A of the two lid bodies 500. The size of one sheet of film 20 is 100 mm in width and 30 mm in height. The film 20 was used after being left to stand in a vacuum oven (-50 MPa) for 24 hours and dried before the test (before sealing). In the electricity storage device of Example 1, three sheets of film 20 are bonded to each of the first surfaces 500A of the two lid bodies 500 in a stacked manner. In the electricity storage device of Example 2, six sheets of film 20 are bonded to each of the first surfaces 500A of the two lid bodies 500 in a stacked manner. In the electricity storage devices of Examples 1 and 2, the film 20 covers almost the entire first surface 500A of the lid body 500. In the electricity storage device of Comparative Example 1, the film 20 is not bonded to the lid body 500.

[0213] The inventors of the present application wrapped the exterior member 101 around the aluminum block and the two lid bodies 500 to which the film 20 was joined, to form the first sealed portion 110. The exterior member 101 has a rectangular shape of 300 mm x 160 mm. The heat sealing conditions for forming the first sealed portion 110 are a temperature of 190°C, a pressure of 1 MPa, and a time of 3 seconds.

[0214] Next, the inventors of the present application formed the second sealed portion 120 by heat-sealing the side surfaces (total of eight sides) of the two lid bodies 500 to the exterior member 101. The heat-sealing conditions for forming the second sealed portion 120 were a temperature of 180° C., a pressure of 0.2 MPa, and a time of 5 seconds.

[0215] Next, the inventors of the present application cut the electricity storage devices of Examples 1 and 2 and Comparative Example 1 in half at a position 80 mm from the end of the lid body 500 to form an opening, and removed the aluminum block from the opening. Then, 20 g of salt-free electrolyte (EC:DMC:DEC=1:1:1) was poured from the opening, and the heat-sealable resin layers 101C present in the opening were strongly heat-sealed twice with a 7 mm wide seal bar to close the layers. The second strong heat-seal was strongly heat-sealed so as to overlap the first strong heat-sealed portion by 4 mm. Therefore, the seal width of the opening is 10 mm. The heat-sealing conditions for strongly heat-sealing the heat-sealable resin layers 101C present in the opening are a temperature of 220° C., a pressure of 0.45 MPa, and a time of 3 seconds.

[0216] The electricity storage devices of Examples 1 and 2 and Comparative Example 1 were left in a thermostatic chamber at a temperature of 65° C. and a humidity of 90% for one week, and then an arbitrary portion of the exterior member 101 was opened, and the moisture content of the salt-free electrolyte was measured by the Karl Fischer method. The Karl Fischer moisture meter used in this test was a Karl Fischer moisture meter MKC-610 manufactured by Kyoto Electronics Manufacturing Co., Ltd. The anolyte used was Chem-Aqua anolyte AGE, and the catholyte used was Chem-Aqua catholyte CGE. For the electricity storage devices of Examples 1 and 2 and Comparative Example 1, the moisture content of the salt-free electrolyte after the test was measured three times using 1 g of the sample, and the average value of the three measurements was used as the measurement result. Note that 1 g of the sample includes an error of about 0.95 g to 1.05 g.

[0217] In the electricity storage device of Example 1, the moisture content of the salt-free electrolyte after the test, which is obtained by subtracting the moisture content of the salt-free electrolyte before the test, was 3 mg. In the electricity storage device of Example 2, the moisture content of the salt-free electrolyte after the test, which is obtained by subtracting the moisture content of the salt-free electrolyte before the test, was 1.5 mg. In the electricity storage device of Comparative Example 1, the moisture content of the salt-free electrolyte after the test, which is obtained by subtracting the moisture content of the salt-free electrolyte before the test, was 25 mg.

[0218] It was confirmed that the moisture content of the electrolyte solution in the electricity storage devices of Examples 1 and 2 increased only slightly compared to the moisture content of the electrolyte solution before the test. From this result, it is considered that the electricity storage device including the film 20 of the first aspect can suppress the intrusion of moisture from the end of the heat-sealable resin layer 101C of the exterior member 101 and the intrusion of moisture contained in the heat-sealable resin layer 101C of the exterior member 101 into the electrode body 200.

[0219] [7. Additional Notes] A first aspect of the film 20 of each of the above embodiments includes the following features.

[0220] Item 1A. A resin film for an electricity storage device that is disposed on the inner side of a barrier layer of an exterior member of an electricity storage device, the resin film for an electricity storage device containing a water absorbing agent. Item 2A. The resin film for a storage battery device according to Item 1A, wherein the water absorbing agent is an inorganic water absorbing agent. Item 3A. The resin film for a storage battery device according to Item 1A or 2A, wherein the water absorbing agent is at least one selected from the group consisting of calcium oxide, anhydrous magnesium sulfate, magnesium oxide, calcium chloride, zeolite, aluminum oxide, silica gel, alumina gel, and calcined alum. Item 4A: The resin film for an electricity storage device according to any one of Items 1A to 3A, wherein the content of the water absorbing agent is 0.1 parts by mass or more per 100 parts by mass of resin contained in the resin film for an electricity storage device. Item 5A: The resin film for an electricity storage device according to any one of Items 1A to 4A, which is constituted of two or more layers. Item 6A. The resin film for a storage battery device according to Item 5A, wherein at least one of the two or more layers contains the water absorbing agent and at least one of the layers contains a sulfur-based gas absorbing agent. Item 7A: The resin film for an electricity storage device according to any one of Items 1A to 6A, wherein the layer containing the water absorbing agent of the resin film for an electricity storage device contains 0.5 mass parts of the absorbent or more per 100 mass parts of resin. Item 8A: The resin film for an electricity storage device according to any one of items 1A to 7A, which contains a heat-fusible resin. Item 9A. The resin film for a storage battery device according to Item 8A, wherein the heat-fusible resin includes at least one selected from the group consisting of polyesters and polyolefins.

[0221] A second aspect of the film 20 of each of the above embodiments includes the following. Item 1B. A resin film for an electricity storage device, the resin film for an electricity storage device being disposed on the inner side of a barrier layer of an exterior member of the electricity storage device, the resin film for an electricity storage device containing a sulfur-based gas absorbent. Item 2B. The resin film for an electricity storage device according to item 1B, wherein the content of the sulfur-based gas absorbent is 0.1 parts by mass or more per 100 parts by mass of resin contained in the resin film for an electricity storage device. Item 3B. The resin film for a storage battery device according to Item 1B or 2B, wherein the sulfur-based gas absorbent has a maximum particle size of 20 μm or less and a number average particle size of 0.1 μm or more and 15 μm or less. Item 4B: The resin film for a storage battery device according to any one of Items 1B to 3B, wherein the sulfur-based gas absorbent includes at least one selected from the group consisting of a sulfur-based gas chemical absorbent and a sulfur-based gas physical absorbent. Item 5B: The resin film for a storage battery device according to Item 4B, wherein the sulfur-based gas physical absorbent includes at least one selected from the group consisting of hydrophobic zeolite having a SiO2 / Al2O3 molar ratio of 1 / 1 to 2000 / 1, bentonite, and sepiolite. Item 6B: The resin film for a storage battery device according to Item 4B or 5B, wherein the sulfur-based gas chemical absorbent is a metal oxide or an inorganic material carrying or containing a metal or metal ion. Item 7B: The resin film for a storage battery device according to Item 6B, wherein the metal oxide includes at least one selected from the group consisting of CuO, ZnO, and AgO. Item 8B: The resin film for a storage battery device according to Item 6B or 7B, wherein the metal species in the inorganic material carrying or containing a metal or metal ion is at least one selected from the group consisting of Ca, Mg, Na, Cu, Zn, Ag, Pt, Au, Fe, Al, and Ni. Item 9B: The resin film for an electrical storage device according to any one of Items 1B to 8B, wherein the layer containing the sulfur-based gas absorbent of the resin film for an electrical storage device contains 5 mass parts of the sulfur-based gas absorbent or more per 100 mass parts of resin. Item 10B: The resin film for an electricity storage device according to any one of items 1B to 9B, which contains a heat-fusible resin. Item 11B: The resin film for an electricity storage device according to Item 10B, wherein the heat-fusible resin includes at least one selected from the group consisting of polyesters and polyolefins. [Explanation of symbols]

[0222] 10, 10X, 10XA, 10Y, 10Z Energy storage device 20 Resin films for energy storage devices 30 Adhesive film for terminals 100, 100X, 100Y Exterior body 101, 101Y, 101Z1, 101Z2 Exterior materials 101A Base material layer 101B Barrier layer 101C Heat-fusible resin layer 101Z Laminate 101X Overhang 110,110Z,154 1st sealing part 110X Recess 120,120X,120Y 2nd sealing part 130,130Z Page 1 135,135Z Side 1 35X Base 140,140Z 2nd side 150 One side 151 Joint area 152 Space 153 Unjoined area 200 Electrode body 210 electrode 215 Current collector 300 electrode terminal 500A Page 1 500B 2nd side 400,500,700 Lid 610,710 Metal parts 800 Seal Bar C1 corner.

Claims

1. An electrode body; an electrode terminal connected to the electrode body; An electric storage device comprising: an exterior body that seals the electrode body, The exterior body is formed of a film-like exterior member, The exterior body is a first sealing portion in which the exterior member is joined while encasing the electrode body; a cover body to which the electrode terminal is attached and which is disposed on a side of the electrode body; A portion of the lid body is joined to the exterior member, The exterior member includes a barrier layer, the electricity storage device has a resin film for an electricity storage device disposed at least partially on the inner side of the barrier layer, The resin film for an electrical storage device contains at least one of a water absorbing agent and a gas absorbing agent, is disposed at least in a portion between the lid body and the exterior member, and is used as a heat-sealable resin layer of the exterior member. Energy storage device.

2. An electrode body, an electrode terminal connected to the electrode body; An electric storage device comprising: an exterior body that seals the electrode body, The exterior body is formed of a film-like exterior member, The exterior body is a first sealing portion in which the exterior member is joined while encasing the electrode body; a cover body to which the electrode terminal is attached and which is disposed on a side of the electrode body; A portion of the lid body is joined to the exterior member, The exterior member includes a barrier layer, the electricity storage device has a resin film for an electricity storage device disposed at least partially on the inner side of the barrier layer, The resin film for an electrical storage device contains at least one of a water absorbing agent and a gas absorbing agent, is disposed at least partially between the lid body and the exterior member, and is used as an adhesive film for a terminal that bonds the exterior member and the electrode terminal. Energy storage device.

3. An electrode body, an electrode terminal connected to the electrode body; An electric storage device comprising: an exterior body that seals the electrode body, The exterior body is formed of a film-like exterior member, The exterior body is a first sealing portion in which the exterior member is joined while encasing the electrode body; a cover body to which the electrode terminal is attached and which is disposed on a side of the electrode body; the lid has a hole through which the electrode terminal passes, A portion of the lid body is joined to the exterior member, The exterior member includes a barrier layer, the electricity storage device has a resin film for an electricity storage device disposed at least partially on the inner side of the barrier layer, The resin film for an electricity storage device contains at least one of a water absorbing agent and a gas absorbing agent, and is disposed at least partially between the lid body and the exterior member, and is disposed in the hole. Energy storage device.

4. An electrode body, an electrode terminal connected to the electrode body; An electric storage device comprising: an exterior body that seals the electrode body, The exterior body is formed of a film-like exterior member, The exterior body is a first sealing portion in which the exterior member is joined while encasing the electrode body; a cover body to which the electrode terminal is attached and which is disposed on a side of the electrode body; The cover body includes a first surface facing the electrode body and a second surface opposite to the first surface, A portion of the lid body is joined to the exterior member, The exterior member includes a barrier layer, the electricity storage device has a resin film for an electricity storage device disposed at least partially on the inner side of the barrier layer, The resin film for an electrical storage device contains at least one of a water absorbing agent and a gas absorbing agent, is disposed at least in a portion between the lid body and the exterior member, and is joined to at least a portion of the second surface of the lid body. Energy storage device.

5. The material constituting the lid body includes at least one of a resin material and a metal material. The electricity storage device according to any one of claims 1 to 4.

6. The resin film for an electricity storage device is disposed at least partially between the lid body and the electrode body. The electricity storage device according to any one of claims 1 to 4.

7. The resin film for an electricity storage device is disposed at least partially between the lid and the electrode terminal. The electricity storage device according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • battery

    JP2001068074A

  • Laminate battery and vehicle mounted with the same

    JP2004039358A

  • Layered package material, outer package material for battery, and the battery

    JP2008287971A

  • Laminate sheet for sulfide-based all-solid-state battery and laminate pack using the same

    JP2020187855A

  • Packaging material and packaging body for all-solid lithium ion battery