Method for Extracting Precipitates and / or Inclusions

By electrolyzing metal materials with a flowing electrolytic solution to prevent electrolytic product formation, the method facilitates precise extraction and analysis of precipitates and inclusions in metal materials, overcoming the limitations of existing techniques.

JP7574976B1Active Publication Date: 2024-10-29JFE STEEL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024544876
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-08-31
Filing Date
2024-05-27
Publication Date
2024-10-29
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

Existing methods for extracting precipitates and inclusions in metal materials, such as steel, are hindered by the formation of electrolytic products that interfere with accurate analysis, requiring complex and specific chemical additives for each interfering element.

Method used

The method involves electrolyzing the metal material while flowing an electrolytic solution along its surface to prevent the formation of electrolytic products by keeping interfering elements away from the precipitates, using a flow rate of at least 0.48 mm/s to minimize interference.

Benefits of technology

This approach allows for accurate and easy extraction of precipitates and inclusions in their original state, enabling precise analysis without the need for complex chemical preparations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574976000001
    Figure 0007574976000001
  • Figure 0007574976000002
    Figure 0007574976000002
  • Figure 0007574976000003
    Figure 0007574976000003
Patent Text Reader

Abstract

The metal material is electrolyzed while the electrolytic solution is made to flow. This allows for accurate and simple extraction of precipitates and / or inclusions (precipitates, etc.) in the metal material. It is preferable to perform the electrolysis while making the electrolytic solution flow along at least a part of the electrolytic surface, which is the surface of the metal material that comes into contact with the electrolytic solution. It is preferable that the flow rate of the electrolytic solution flowing along the electrolytic surface is 0.48 mm / s or more. It is preferable that the metal material and the electrolytic solution are contained in an electrolytic cell, and the electrolytic solution is made to flow by injecting and discharging the electrolytic solution into and from the electrolytic cell.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for extracting precipitates and / or inclusions. [Background technology]

[0002] Precipitates and / or inclusions (hereinafter referred to as "precipitates, etc.") present in metal materials such as steel affect the properties of the metal materials depending on their amount and form. Therefore, analysis of precipitates, etc. is important in controlling the properties of metal materials.

[0003] Conventionally, when analyzing precipitates and the like in a metallic material, the metallic material is electrolyzed using an electrolytic solution (Patent Document 1). That is, by dissolving the matrix element of the metallic material (Fe when the metallic material is a steel material), the precipitates and the like are exposed on the electrolytic surface of the metallic material (the surface in contact with the electrolytic solution), and the exposed precipitates and the like are observed or collected. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2017 / 142084 Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors used a steel material containing several mass % of Ni and Mo as the metallic material, electrolyzed this metallic material, and extracted precipitates and the like. As a result, it was found that Fe, Ni and Mo may form some compounds (also called "electrolysis products") on the surface of the deposits to be extracted. In this case, the precipitates and the like are not extracted accurately (in their original state). Since electrolytic products formed on the surface of deposits and the like affect the analysis of the deposits and the like, it is necessary to suppress the formation of electrolytic products.

[0006] Incidentally, in order to address a similar problem, Patent Document 1 discloses a technique for adding an agent to the electrolyte that forms a complex with an element (hereinafter also referred to as an "interfering element") that prevents accurate extraction of precipitates, etc.

[0007] However, when the technique described in Patent Document 1 is adopted, it is necessary to prepare an appropriate agent for each interfering element (e.g., Fe, Ni, and Mo), which is very troublesome. In addition, depending on the interfering element, there are cases where an appropriate agent cannot be prepared. For this reason, a method is desired that can extract precipitates and the like without having to prepare chemicals corresponding to the interfering elements (i.e., simply).

[0008] The present invention has been made in consideration of the above points, and has an object to provide a method for accurately and simply extracting precipitates and the like in a metal material. [Means for solving the problem]

[0009] The present inventors have conducted extensive research in order to achieve the above object. the result, a) It is presumed that, when electrolyzing a metal material, elements (interfering elements) constituting the metal material dissolve into the electrolyte and are formed on the surface of the deposit, etc. through some kind of reaction. b) In order to avoid the occurrence of the above reaction, when electrolyzing a metal material, it is necessary to keep the interfering elements dissolved in the electrolyte away from the deposits exposed on the electrolytic surface of the metal material. Thus, the present invention has been completed.

[0010] That is, the present invention provides the following [1] to [5]. [1] A method for extracting precipitates and / or inclusions in a metallic material, comprising electrolyzing the metallic material while flowing an electrolyte. [2] The method for extracting precipitates and / or inclusions described in [1] above, in which the electrolysis is carried out while causing the electrolyte to flow along at least a portion of an electrolysis surface, which is a surface of the metal material that comes into contact with the electrolyte. [3] The method for extracting precipitates and / or inclusions described in [2] above, wherein the flow rate of the electrolyte flowing along the electrolytic surface is 0.48 mm / s or more. [4] The method for extracting precipitates and / or inclusions according to any one of [1] to [3] above, wherein the metal material and the electrolytic solution are contained in an electrolytic cell, and the electrolytic solution is caused to flow by injecting and discharging the electrolytic solution into and from the electrolytic cell. [5] The method for extracting precipitates and / or inclusions according to any one of [1] to [3] above, wherein after the electrolysis, the precipitates and / or inclusions exposed on the surface of the metal material are extracted. Effect of the Invention

[0011] According to the present invention, precipitates and the like in metal materials can be extracted accurately and simply. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing an electrolysis system used for electrolysis of a metal material. [Figure 2A] FIG. 1 is a schematic diagram showing another example of an electrolysis system. [Figure 2B] FIG. 1 is a schematic diagram showing another example of an electrolysis system. [Figure 2C] FIG. 1 is a schematic diagram showing another example of an electrolysis system. [Figure 2D] FIG. 1 is a schematic diagram showing another example of an electrolysis system. [Figure 2E] FIG. 1 is a schematic diagram showing another example of an electrolysis system. [Figure 2F] FIG. 1 is a schematic diagram showing another example of an electrolysis system. [Diagram 3] 1 is an SEM image showing a residue of Example 1. [Figure 4] 1 is an SEM image showing the residue of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] This embodiment will be described below. First, an electrolysis system 1 used for electrolysis of a metal material 13 in this embodiment will be described with reference to FIG.

[0014] Overview of the electrolysis system FIG. 1 is a schematic diagram showing an electrolysis system 1 used for electrolysis of a metal material 13. The electrolysis system 1 generally includes an electrolysis device 10, an electrolyte tank 20, a pump 30, a tube 35, and an electrochemical measurement device 40.

[0015] The electrolysis device 10 includes an electrolytic cell 11 having an opening 11 a , and further includes a cathode 12 and an anode 14 made of a metal material 13 . The inside of the electrolytic cell 11 is filled with an electrolytic solution 5 , and the cathode 12 and the anode 14 (metal material 13 ) are immersed in the electrolytic solution 5 . Although the metal material 13 shown in FIG. 1 is entirely immersed in the electrolytic solution 5, the present invention is not limited to this, and it is sufficient that only a part of the metal material 13 is immersed in the electrolytic solution 5.

[0016] Each component of the electrolysis system 1 will be described in more detail below.

[0017] Metallic materials and anodes There are no particular limitations on the metal material 13 as long as it is a metal material containing precipitates and / or inclusions (precipitates, etc.), but a steel material is preferable. In the steel industry, precise control of the amount and morphology of precipitates in steel materials is used to impart new properties to steel materials or improve existing properties, so it is important to analyze precipitates in steel materials with high accuracy.

[0018] An example of the steel material is a steel material containing a few mass % of Ni and Mo. When this steel material is electrolyzed, nickel (Ni) and molybdenum (Mo) are also dissolved into the electrolytic solution 5 in addition to iron (Fe), which is the matrix metal of the steel material. Such steel materials contain, for example, MnS and Cr compounds as precipitates.

[0019] The shape of the metal material 13 is not particularly limited, but from the viewpoint of allowing the electrolyte 5 to flow along the electrolysis surface of the metal material 13 as described below, a shape that does not hinder the flow of the electrolyte 5 (e.g., a cylindrical shape, a rectangular parallelepiped shape, etc.) is preferable.

[0020] The anode 14 is composed of a metal material 13 and a lead wire 25 wound around the metal material 13. An inactive metal such as platinum (Pt) is preferably used as the material for the lead wire 25. By winding the lead wire 25 around the metal material 13, the metal material 13 is made conductive and the metal material 13 is fixed in place.

[0021] The method for fixing the position of the metal material 13 is not limited to this. For example, when electrolyzing a specific surface of the metal material 13 (e.g., a surface to be observed using an SEM after electrolysis), the lead wire 25 may be soldered to a surface other than this specific surface. Moreover, the metal material 13 may be clamped using an alligator clip (not shown) to which the lead wire 25 is connected.

[0022] In the case where the metal material 13 is magnetic, the lead wire 25 may be replaced with a cylindrical member (not shown) made of the same material as the lead wire 25 . The cylindrical member has one end face closed by a bottom plate, and is placed inside electrolytic cell 11 with the bottom plate facing downward. A magnet such as a neodymium magnet is then placed on the upper surface side of the bottom plate (inside the cylindrical member), and metal material 13 is adhered to the lower surface side of the bottom plate (outside the cylindrical member) by the magnetic force of the magnet. In this way, metal material 13 can be fixed in position in a suspended state.

[0023] In addition, in Figure 1, the entire metal material 13 is immersed in the electrolyte 5, so that all areas of the surface of the metal material 13 where the lead wire 25 is not wound (areas not in contact with the wound lead wire 25) can be said to be electrolytic surfaces in contact with the electrolyte 5. Of the surfaces of the metal material 13, those surfaces that do not require electrolysis may be covered with an insulating resin or the like.

[0024] The anode 14 (more specifically, the lead wire 25 constituting the anode 14 ) is connected to an electrochemical measurement device 40 using a conductive wire 15 .

[0025] <cathode> As the cathode 12, various counter electrodes currently in practical use can be appropriately used. Among these, platinum (Pt) is preferable because it has high stability with respect to the electrolyte 5 and is unlikely to contaminate the electrolyte 5. The cathode 12 is connected to an electrochemical measurement device 40 using a lead 16 .

[0026] Electrochemical measurement equipment As the electrochemical measurement device 40, for example, a constant potential electrolysis device may be used when electrolyzing the metal material 13 by controlling the potential of the metal material 13, and a constant current electrolysis device may be used when electrolyzing the metal material 13 by controlling the current of the metal material 13. A potentio-galvanostat having both functions may also be used.

[0027] By driving the electrochemical measurement device 40, the potential or current of the metal material 13 is controlled, and electrolysis is performed on the metal material 13. The electrolysis conditions are not particularly limited, but a potential or current that does not decompose the precipitates and the like to be extracted is preferable.

[0028] Although the electrolysis system 1 shown in Fig. 1 employs a two-electrode method, a three-electrode method using a reference electrode may also be used. The three-electrode method is preferable from the viewpoint of control.

[0029] <Electrolyte tank, tube and pump> In the electrolysis system 1, the electrolyte 5 is contained not only in the electrolytic cell 11 but also in the electrolyte tank 20. One end of a tube 35 is connected to the electrolyte tank 20. The tube 35 is made of a soft material such as silicon. The other end (inlet 19) of the tube 35 is disposed in an opening 11a of the electrolytic cell 11. That is, the electrolyte tank 20 and the electrolytic cell 11 are connected by the tube 35.

[0030] A pump 30 is disposed midway through the tube 35. As the pump 30, a peristaltic pump is preferably used because it does not come into contact with the electrolyte 5 and is less likely to be contaminated. By driving the pump 30, the electrolyte 5 is sucked up from the electrolyte tank 20. The sucked up electrolyte 5 passes through the inside of the tube 35 and is injected into the electrolytic cell 11 from the injection port 19 which is the end of the tube 35.

[0031] <Electrolytic cell> As described above, the electrolytic cell 11 has an opening 11a. If the electrolytic cell 11 is a closed system having no opening 11a, the gas generated by the electrolysis of the metal material 13 may accumulate, causing a positive pressure inside the electrolytic cell 11 and hindering the injection of the electrolyte 5. For this reason, the electrolytic cell 11 is preferably an open system having an opening 11a.

[0032] A tubular outlet 17 is provided on the opposite side of the opening 11a in the electrolytic cell 11 and facing the inlet 19. A cock 18 that can be opened and closed is disposed midway through the outlet 17. When the cock 18 is opened, the electrolyte 5 is discharged from inside the electrolytic cell 11.

[0033] <Electrolyte> The electrolytic solution 5 is not particularly limited, and an electrolytic solution having a conventionally known composition can be appropriately used. However, an electrolytic solution having a composition in which the deposit of the metal material 13 does not dissolve is preferable. Specifically, for example, an AA electrolytic solution (acetylacetone-tetramethylammonium chloride-methanol), an MS electrolytic solution (4% by volume methyl salicylate-1% by mass salicylic acid-methanol), a citric acid electrolytic solution (10% by mass sodium citrate-1% by mass potassium bromide-pure water-citric acid (for pH adjustment)), etc. can be preferably used. For example, when the metal material 13 is a steel material, Fe dissolved in the electrolyte 5 may form iron hydroxide or the like, which may cause clogging of the outlet 17. In such a case, an agent for complexing Fe may be added to the electrolyte 5.

[0034] <electrolytic> In such a configuration, by driving the electrochemical measurement device 40, the electrolytic surface (the surface in contact with the electrolytic solution 5) of the metal material 13 is electrolyzed, and the deposits and the like are exposed. Here, when a steel material containing a few mass % of Ni and Mo is used as the metal material 13, the constituent Fe, Ni and Mo may dissolve into the electrolytic solution 5 as interfering elements and form electrolytic products on the surfaces of exposed deposits, etc.

[0035] Therefore, in this embodiment, during electrolysis of the metal material 13, the cock 18 is opened and the pump 30 is driven. As a result, the electrolytic solution 5 is injected into the electrolytic cell 11 from the inlet 19 and discharged from the outlet 17. That is, the electrolysis of the metal material 13 is carried out while the electrolytic solution 5 is flowing.

[0036] By flowing the electrolyte 5 , even if interfering elements are dissolved into the electrolyte 5 , the dissolved interfering elements move away from deposits and the like exposed on the electrolytic surface of the metal material 13 . In this way, the formation of electrolytic products on the surfaces of deposits and the like can be easily suppressed without using any chemicals corresponding to interfering elements.

[0037] In this embodiment, it is preferable that the electrolytic solution 5 is caused to flow along at least a part of the electrolytic surface of the metal material 13 (for example, the surface to be observed using an SEM after electrolysis). In other words, it is preferable that each of the metal material 13 , the inlet 19 , the outlet 17 , and the like is disposed so that the electrolyte 5 flows along at least a part of the electrolytic surface of the metal material 13 . For example, in the electrolysis system 1 shown in FIG. 1, the electrolytic solution 5 flows at least along the side surface of the metal material 13, which is cylindrical.

[0038] The flow rate of the electrolytic solution 5 is determined by, for example, the reaction that produces the electrolytic product (the reaction of the interfering element dissolved in the electrolytic solution 5), and is therefore set appropriately depending on the composition of the metal material, etc. As the reaction time increases, the amount of electrolytic product produced also increases. On the other hand, by increasing the flow speed of the electrolyte 5 flowing along the electrolytic surface of the metal material 13 (for example, the side surface of the cylindrical metal material 13), the time that interfering elements remain on this electrolytic surface is shortened, and the reaction time is reduced. In addition, in the first place, when the flow rate of the electrolyte 5 is high, the effect of keeping interfering elements away from deposits and the like exposed on the electrolytic surface of the metal material 13 is more excellent. Therefore, when the above-mentioned steel material containing Ni and Mo is used as the metal material, the flow speed of the electrolyte 5 flowing along the electrolysis surface is preferably 0.48 mm / s or more, more preferably 0.65 mm / s or more, even more preferably 0.75 mm / s or more, and particularly preferably 1.33 mm / s or more. The upper limit is not particularly limited, and is, for example, 2.00 mm / s. A method for measuring the flow rate of the electrolyte 5 will be described later (see [Examples]).

[0039] The electrolyte 5 discharged from the electrolytic cell 11 through the outlet 17 may be returned to the electrolyte tank 20 and then injected again into the electrolytic cell 11 through the inlet 19. In other words, the electrolyte 5 may be circulated. However, the electrolyte 5 discharged from the outlet 17 contains interfering elements eluted from the metal material 13. For this reason, it is preferable not to circulate the electrolyte 5 from the viewpoint of keeping the interfering elements away from the electrolytic surface of the metal material 13. If the electrolyte 5 is circulated, it is preferable to remove the interfering elements from the electrolyte 5 using an ion exchange resin or the like.

[0040] <extraction> Thereafter, the deposits and the like exposed on the surface of the metal material 13 are extracted by a known method. For example, the metal material 13 after electrolysis is immersed in alcohol such as methanol and ultrasonic vibration is applied to cause exposed deposits and the like to peel off into the alcohol. Next, the alcohol is filtered using a filter (filter paper) to collect the deposits and the like.

[0041] In addition, observing precipitates, etc., exposed on the surface of metal material 13 using a scanning electron microscope (SEM) or the like without peeling them off from metal material 13 and collecting them is also considered to be "extraction."

[0042] The formation of electrolytic products on the surface of the extracted deposits is suppressed, meaning that the deposits can be extracted accurately (in their original state), allowing for highly accurate analysis.

[0043] <Another example of the electrolysis system configuration> 2A to 2F are schematic diagrams illustrating other examples of the electrolysis system 1. 2A to 2F, only electrolytic cell 11, inlet 19, outlet 17, metal material 13, and part of lead wire 25 are shown, and the other components are omitted from the illustration.

[0044] The configuration of the electrolysis system 1 used in this embodiment is not limited to the configuration described based on FIG. 1, as long as the metal material 13 can be electrolyzed while the electrolytic solution 5 is flowing.

[0045] For example, in the electrolysis system 1 described based on FIG. 1, the injection port 19 is disposed in a position facing the exhaust port 17, but this is not limited thereto, and the position of the injection port 19 may be a position that does not face the exhaust port 17, as shown in FIG. 2A.

[0046] In the electrolysis system 1 described based on FIG. 1, the exhaust outlet 17 is provided on the bottom surface of the electrolytic cell 11, but this is not limited thereto. For example, as shown in FIG. 2B, the exhaust outlet 17 may be provided on the side surface of the electrolytic cell 11.

[0047] In addition, in the electrolysis system 1 described based on Figure 1, the injection port 19 is arranged at the opening 11a of the electrolytic cell 11, but this is not limited to this. For example, as shown in Figures 2C and 2D, a hole may be drilled in the side of the electrolytic cell 11 and the injection port 19 may be connected to the hole. Furthermore, for example, as shown in Figs. 2E and 2F, a hole may be formed in the bottom surface of the electrolytic cell 11 and an injection port 19 may be connected to the hole.

[0048] 1 and 2A to 2F, a method (Method A) in which electrolytic solution 5 is injected into electrolytic cell 11 from inlet 19 while being discharged from outlet 17 has been described. However, the method for flowing the electrolytic solution 5 is not limited to Method A, and for example, a method (Method B) in which the electrolytic solution 5 injected into the electrolytic cell 11 is rotated at high speed using a stirrer or the like without being discharged from the discharge port 17 may also be used. For example, when observing deposits and the like by using an SEM while they are exposed on the surface of the metal material 13, the amount of electrolysis of the metal material 13 is usually small, and therefore the amount of interfering elements dissolved in the electrolytic solution 5 is also small. In this case, even with method B, the above-mentioned effects can be expected. However, when collecting and quantitatively analyzing precipitates and the like exposed on the surface of the metal material 13, the amount of electrolysis of the metal material 13 is relatively large, and therefore, as a method for flowing the electrolyte 5, method A is preferable from the viewpoint of fully obtaining the above-mentioned effects. EXAMPLES

[0049] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the examples described below.

[0050] Example 1 Using the electrolysis system 1 described based on FIG. 1, the metal material 13 was electrolyzed, and then the precipitates and the like were extracted, as described below.

[0051] The cathode 12 was a Pt plate. A cylindrical steel material (diameter: 3.8 mm, length: 33.6 mm) containing 2.1 mass % Ni and 1.1 mass % Mo was used as the metal material 13 constituting the anode 14. The anode 14 was produced by winding a Pt lead wire 25 around the side surface of the cylindrical metal material 13.

[0052] An AA electrolyte solution (acetylacetone-tetramethylammonium chloride-methanol) was used as the electrolyte solution 5. The content of acetylacetone was 10% by volume. The content of tetramethylammonium chloride in 100 mL of the electrolyte solution was 1 g.

[0053] A cylindrical container having an opening 11a on one side was used as the electrolytic cell 11. A hole was drilled in the side of the container opposite to the opening 11a, and a hose with a cock 18 was attached to form an outlet 17. One end of a silicon tube 35 was connected to the electrolyte tank 20, and the other end was used as an inlet 19, which was disposed at the opening 11a of the electrolytic cell 11. More specifically, the inlet 19 was disposed at a position opposite to the outlet 17. A pump 30, which was a peristaltic pump, was disposed midway along the tube 35. A cathode 12 and an anode 14 (metal material 13) were placed inside an electrolytic cell 11, and an electrochemical measurement device 40, which is a potentio-galvanostat, was connected. At this time, the straight line connecting the injection port 19 and the exhaust port 17 was made parallel to the side surface of the cylindrical metal material 13 constituting the anode 14. Furthermore, the upper surface of the cylindrical metal material 13 was placed directly below the injection port 19.

[0054] With the cock 18 of the discharge port 17 open, the pump 30 was operated. As a result, the electrolytic solution 5 was injected into the electrolytic cell 11 from the injection port 19, while being discharged from the discharge port 17. By injecting and discharging the electrolytic solution 5 in this manner, the electrolytic solution 5 was made to flow along the side surface of the cylindrical metal material 13. At this time, the flow rate of the electrolytic solution 5 was set to 0.75 mm / s. The flow rate was determined by the volume (unit: mm 3 / s) was measured and calculated as the area of ​​the bottom of the electrolytic cell 11 (unit: mm 2 ) was calculated.

[0055] Separately, a float was placed in the electrolytic cell 11 to determine the flow velocity of the electrolyte 5 flowing along the side surface of the metal material 13, and the results obtained were the same as those described above.

[0056] In this state, the electrochemical measuring device 40 was driven. In this manner, the electrolytic surface of the metal material 13 was electrolyzed while the electrolytic solution 5 was flowing. The amount of metal material 13 dissolved by electrolysis (amount of electrolysis) was about 0.02 g.

[0057] The electrolyzed metal material 13 was immersed in methanol and subjected to ultrasonic vibration, and then the methanol was filtered using filter paper. The filter paper used was "Nuclepore Membrane" (pore size: 0.2 μm) manufactured by Global Life Science Technologies Japan, Inc. The residue on the filter paper was observed using a scanning electron microscope (SEM).

[0058] FIG. 3 is an SEM image showing the residue of Example 1. As indicated by the arrows in Figure 3, spherical precipitates were clearly observed in the SEM image. Furthermore, analysis using an energy dispersive X-ray analyzer (EDS) mounted on the SEM revealed that the spherical precipitates were MnS. At this time, no electrolytic products containing Fe, Ni and Mo were observed on the surfaces of the spherical deposits, etc.

[0059] Comparative Example 1 In Comparative Example 1, a metal material 13 was electrolyzed in the same manner as in Invention Example 1, except that a commercially available beaker was used as the electrolytic cell 11 and the electrolytic solution 5 was not caused to flow, and then filtration was performed using filter paper.

[0060] FIG. 4 is an SEM image showing the residue of Comparative Example 1. As indicated by the arrows in FIG. 4, in addition to the spherical precipitates, a coating covering the surface was confirmed in the SEM image. Analysis using an EDS mounted on a SEM revealed that the spherical precipitates were MnS, and that the coating was a compound containing Fe, Ni, and Mo. Since this compound was not identified in an SEM image (not shown) of the surface of the metal material 13 before electrolysis was performed, it can be assumed that it is a compound generated by electrolysis (electrolysis product).

[0061] From the above, it can be said that in Example 1 in which the metal material 13 was electrolyzed while the electrolytic solution 5 was flowing, the formation of electrolytic products on the surfaces of deposits and the like was suppressed.

[0062] <Examples 2 to 5> In Examples 2 to 5, the flow velocity of the electrolytic solution 5 was changed to 1.33 mm / s (Example 2), 0.48 mm / s (Example 3), 0.37 mm / s (Example 4), or 0.12 mm / s (Example 5). Otherwise, the metal material 13 was electrolyzed in the same manner as in Example 1, and then filtration was performed using filter paper. The residue on the filter paper was observed using an SEM. As a result, in the SEM images (not shown) of invention examples 4 and 5, a small amount of electrolytic products was observed on the surface of the precipitates, etc. In contrast, in the SEM images (not shown) of invention examples 2 and 3, similar to invention example 1, no electrolytic products were observed on the surface of the precipitates, etc. [Explanation of symbols]

[0063] 1: Electrolysis system 5: Electrolyte 10: Electrolyzer 11: Electrolytic cell 11a: Opening 12: Cathode 13: Metal material 14:Anode 15: Conductor 16: Conductor 17: Outlet 18: Cook 19: Inlet 20: Electrolyte tank 25: Lead wire 30: Pump 35: Tube 40: Electrochemical measurement device

Claims

1. 1. A method for extracting precipitates and / or inclusions in a metallic material, comprising: The method for extracting precipitates and / or inclusions comprises electrolyzing the metallic material while flowing an electrolyte.

2. 2. The method for extracting precipitates and / or inclusions according to claim 1, wherein the electrolysis is carried out while the electrolytic solution is caused to flow along at least a portion of an electrolytic surface, which is a surface of the metallic material that comes into contact with the electrolytic solution.

3. 3. The method for extracting precipitates and / or inclusions according to claim 2, wherein a flow velocity of the electrolyte flowing along the electrolysis surface is 0.48 mm / s or more.

4. The metal material and the electrolyte are contained in an electrolytic cell; The method for extracting precipitates and / or inclusions according to any one of claims 1 to 3, wherein the electrolytic solution is caused to flow by injecting and discharging the electrolytic solution into and from the electrolytic cell.

5. The method for extracting deposits and / or inclusions according to any one of claims 1 to 3, wherein after the electrolysis, the deposits and / or inclusions exposed on the surface of the metallic material are extracted.

Citation Information

Patent Citations

  • Sample preparation method of scanning electron microscope sample of inclusions in rare earth weathering resistant steel

    CN113447509A

  • Manufacture of transmission type electron microscopic sample

    JP1986079135A

  • JP1989152238U

  • Method for extracting precipitate and / or inclusion, method for quantitative analysis of precipitate and / or inclusion, electrolyte, and method for producing replica sample

    WO2021106705A1

  • Device for electrolytic etching and method for extracting metal compound particles

    WO2017142084A1