Transparent erasing composition and its cured product
A transparent eraser composition using a polyvinyl chloride resin, polysiloxane defoaming agent, and polyalkylene glycol derivative defoaming agent addresses the issue of air bubbles, ensuring rapid defoaming and maintaining transparency for efficient eraser production.
Patent Information
- Application Number
- JP2021090625
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-05-28
AI Technical Summary
The inclusion of air bubbles in transparent erasers is undesirable for quality and aesthetics, and existing defoaming methods to remove these bubbles are time-consuming, impacting production efficiency, while adding antifoaming agents can impair transparency.
A transparent eraser composition containing a polyvinyl chloride resin, a polysiloxane defoaming agent, and a defoaming agent with a polyalkylene glycol derivative, optionally with a benzoic acid ester plasticizer, which enhances antifoaming properties and transparency.
The composition achieves rapid defoaming without compromising transparency, improving production efficiency and resulting in transparent erasers with excellent erasability.
Smart Images

Figure 0007575070000001 
Figure 0007575070000002 
Figure 0007575070000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent erasing composition and a cured product thereof. [Background technology]
[0002] In recent years, various improvements have been made to erasers from the viewpoints of design, such as shape and color, as well as practicality. Among them, transparent erasers are in high demand, for example, from the viewpoint of design.
[0003] Regarding transparent erasers, for example, Patent Document 1 below discloses an eraser containing a vinyl chloride resin having an average degree of polymerization of 800 to 1500 and a plasticizer having a refractive index of 1.50 or more and a solubility parameter of 9.4 to 11.0. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2021-30708 Summary of the Invention [Problem to be solved by the invention]
[0005] The inclusion of air bubbles in an eraser is undesirable from the viewpoint of the quality and aesthetics of the eraser, and the inclusion of air bubbles is particularly unacceptable in a transparent eraser. Therefore, a degassing step may be carried out in the manufacture of an eraser composition. In this degassing step, it is necessary to thoroughly remove air bubbles from the eraser composition, but this often requires a lot of time, which is undesirable from the viewpoint of, for example, manufacturing efficiency. If the degassing step can be completed more quickly, the manufacturing efficiency can be improved. In order to complete the defoaming step more quickly, it is conceivable to add an antifoaming agent such as a defoamer or a defoamer, however, the addition of an antifoaming agent may impair the transparency of the eraser.
[0006] Therefore, an object of the present invention is to provide an erasing composition which is capable of providing an erasing agent having excellent defoaming properties and excellent transparency. [Means for solving the problem]
[0007] The present inventors have discovered that the above problems can be solved by using a specific composition.
[0008] That is, the present invention provides a transparent eraser composition comprising a polyvinyl chloride resin, a polysiloxane-based defoaming agent, and a foam breaker containing a polyalkylene glycol derivative. The transparent erasing composition may further contain a benzoate-based plasticizer. The transparent erasing composition may further comprise an organotin stabilizer. The polysiloxane-based defoaming agent may be contained in an amount of 0.001 parts by mass or more and 0.5 parts by mass or less with respect to 100 parts by mass of the polyvinyl chloride resin. The cell opener containing the polyalkylene glycol derivative may be contained in an amount of 0.1 parts by mass or more and 3.0 parts by mass or less based on 100 parts by mass of the polyvinyl chloride resin. The transparent erasing composition may also be a plastisol composition. The present invention further provides a cured product of the transparent erasing composition. The cured product can be used as an eraser. Effect of the Invention
[0009] The transparent erasing composition of the present invention is excellent in antifoaming property and transparency. According to the present invention, it is possible to provide an eraser having excellent transparency while increasing the production efficiency of the erasing composition and the eraser. The effects of the present invention are not limited to those described herein, and may be any of the effects described in this specification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following describes preferred embodiments of the present invention. However, the present invention is not limited to the following preferred embodiments, and can be freely modified within the scope of the present invention. In this specification, percentages are expressed by mass unless otherwise specified.
[0011] The transparent eraser composition of the present invention comprises a polyvinyl chloride resin, a polysiloxane-based defoaming agent, and a defoamer containing a polyalkylene glycol derivative. This composition, particularly the combination of the defoaming agent and the defoamer, improves the defoaming ability of the composition, and improves the transparency of the cured product obtained by curing the composition. The compositions of the present invention are described in more detail below.
[0012] (1) Polyvinyl chloride resin The polyvinyl chloride resin is a synthetic resin having a structure represented by CH2-CHCl-. The polyvinyl chloride resin may be a homopolymer of vinyl chloride, or may be, for example, a copolymer of a vinyl chloride monomer and another monomer having an unsaturated bond copolymerizable with the vinyl chloride monomer.
[0013] Specific examples of the other monomer having an unsaturated bond copolymerizable with the vinyl chloride monomer include vinylidene chloride, vinyl acetate, ethylene, propylene, butadiene, styrene, isobutylene, acrylic acid, maleic anhydride, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, acrylonitrile, various vinyl ethers, etc. Furthermore, the other monomer having an unsaturated bond copolymerizable with the vinyl chloride monomer may be one or more selected from this group.
[0014] In addition, the polyvinyl chloride resin may be a polymer blend as long as it does not impair the transparency and erasability of the eraser in the present invention. Examples of the polymer blend include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-alkyl acrylate copolymer, ethylene-propylene copolymer, polypropylene, propylene-α-olefin copolymer, polybutene, polypentene, chloropolyethylene, and chloropolypropylene, and one or more selected from the group consisting of these may be used.
[0015] The suitable average degree of polymerization of the polyvinyl chloride resin is, for example, 500 or more, preferably 700 or more, and more preferably 800 or more. The average degree of polymerization may be, for example, 5000 or less, preferably 3000 or less, and more preferably 2000 or less. The average degree of polymerization within such a range is preferable for imparting suitable hardness and sufficient erasing power to the resulting eraser, and is also preferable for improving the miscibility with the plasticizer and stabilizer described below, thereby enhancing the transparency of the resulting eraser.
[0016] The polyvinyl chloride resin has a K value (degree of polymerization) of, for example, 40 or more, preferably 50 or more, and more preferably 60 or more. The K value is, for example, 90 or less, and preferably 80 or less. The K value may be measured according to JIS K 7367-2.
[0017] In the transparent erasing composition of the present invention, the polyvinyl chloride resin is preferably polyvinyl chloride (a homopolymer of vinyl chloride). The homopolymer is easily mixed with a plasticizer and is suitable for obtaining an eraser with high erasability.
[0018] The polyvinyl chloride resin may be produced by a production method known in the art. The polyvinyl chloride resin may be produced by various polymerization methods such as emulsion polymerization, suspension polymerization, or bulk polymerization. In addition, the polyvinyl chloride resin may be a commercially available product.
[0019] The polyvinyl chloride resin can be classified into paste vinyl chloride resin, suspension vinyl chloride resin, and blend vinyl chloride resin according to the characteristics such as particle shape and particle size. The polyvinyl chloride resin may be any one of paste vinyl chloride resin, suspension vinyl chloride resin, and blend vinyl chloride resin, but is preferably paste vinyl chloride resin. Paste vinyl chloride resin is preferable from the viewpoint of ease of production because it has excellent fluidity and is easy to mold.
[0020] The paste vinyl chloride resin may be a fine powder with a precisely controlled particle size. The paste vinyl chloride resin may be mixed with, for example, a plasticizer to form a paste with good fluidity. The vinyl chloride particles in the paste vinyl chloride resin may be preferably spherical, and in particular may be true spherical with few voids inside and on the surface. The preferred particle size of the primary particles (single particles) in the vinyl chloride resin is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 2.5 μm or less. The preferred particle size of the primary particles (single particles) in the vinyl chloride resin may be, for example, 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.05 μm or more.
[0021] (2) Defoaming agent The defoaming agent contained in the transparent erasing composition of the present invention is a polysiloxane-based defoaming agent. By combining the defoaming agent with the defoamer containing the polyalkylene glycol derivative, the defoaming property and transparency are improved as described above. In addition, the defoaming agent can more quickly remove bubbles before they lose fluidity due to the progress of curing. The defoaming agent has a function of promoting the movement of bubbles to the surface, and may be used to promote the movement. In order to promote the movement, the defoaming agent may have a function of coalescing bubbles present in the system of the composition to make them larger. In terms of transparency, incompatibility with the composition, and insolubility, the defoaming agent is preferably a polysiloxane-based defoaming agent, which is a linear polymer composed of siloxane bonds. Specific examples include polydimethylsiloxane, polymethylphenylsiloxane, polymethylhydrogensiloxane, and the like. In order to obtain appropriate incompatibility and surface tension in the composition, the linear polymer having the polysiloxane bond may have various organic groups introduced into the side chain or terminal, or may be reactive.
[0022] The content of the defoaming agent is not particularly limited, but is, for example, 0.001 parts by mass or more, preferably 0.01 parts by mass or more, and more preferably 0.02 parts by mass or more, relative to 100 parts by mass of the vinyl chloride resin. The content of the defoaming agent may be, for example, 0.5 parts by mass or less, preferably 0.2 parts by mass or less, and more preferably 0.1 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. It is preferable that the content is within such a numerical range in order to improve defoaming properties and transparency.
[0023] The defoaming agent may be selected from those having a refractive index at 23° C. in the range of about 1.0 to 2.0. From the viewpoint of transparency, the refractive index of the defoaming agent at 23° C. is preferably 1.2 or more, more preferably 1.3 or more, and more preferably 1.4 or more. The refractive index is preferably 1.8 or less, and more preferably 1.6 or less. Such a refractive index is close to the refractive index of vinyl chloride resin, and is therefore preferable from the viewpoint of improving transparency.
[0024] (3) Foam breaker The defoamer contained in the transparent erasing composition of the present invention is a defoamer containing an alkylene glycol derivative. By combining the defoamer with the polysiloxane-based defoamer, the defoaming property and transparency as described above can be improved. In addition, the defoamer can more quickly remove bubbles before they lose fluidity due to the progress of curing. The defoamer may be used to destabilize bubbles generated on the surface of the composition and eliminate them. Examples of defoamers that can be used in the present invention include activator-based defoamers in which EO (ethylene oxide) or PO (propylene oxide) is added to a hydrocarbon group derived from a higher alcohol, a fatty acid, an alkylphenol, or the like. From the viewpoint of transparency and operability, the defoamer containing an alkylene glycol derivative is particularly suitable. Specific examples include polyoxyalkylene alkyl ethers, polyoxyalkylene alkyl phenyl ethers, polyoxyethylene polyoxypropylene block polymers, polyoxyethylene polyoxypropylene glyceryl ethers, polyoxyalkylene fatty acid monoesters, and polyoxyalkylene fatty acid diesters.
[0025] The preferred cloud point of the cell breaker containing the alkylene glycol derivative is, for example, 0° C. or higher, preferably 5° C. or higher, and more preferably 10° C. or higher. The preferred cloud point of the cell breaker is, for example, 60° C. or lower, preferably 50° C. or lower, and more preferably 30° C. or lower. The cloud point being within such a numerical range is preferable for providing a stronger cell breaking effect around room temperature. By selecting an alkylene glycol derivative-containing cell breaker having such a cloud point, the transparency and operability of the composition of the present invention are improved.
[0026] The content of the defoamer is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1.0 parts by mass or more, relative to 100 parts by mass of the vinyl chloride resin. The content of the defoamer may be, for example, 5.0 parts by mass or less, preferably 3.0 parts by mass or less, and more preferably 2.0 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. It is preferable for the content to be within such a numerical range in order to improve defoaming properties and transparency.
[0027] (4) Plasticizers The transparent eraser composition of the present invention may further contain a plasticizer. The plasticizer is preferably a benzoate ester. The plasticizer improves the processability and product properties of the polyvinyl chloride resin. In addition, the transparent eraser composition can impart appropriate flexibility and friction resistance to the eraser obtained from the transparent eraser composition.
[0028] The plasticizer may be selected from those having a refractive index in the range of about 1.0 to 2.0. From the viewpoint of transparency, the refractive index of the plasticizer is preferably 1.0 or more, more preferably 1.3 or more, and more preferably 1.5 or more. The refractive index is preferably 2.0 or less, more preferably 1.8 or less, and more preferably 1.6 or less. Such a refractive index is close to the refractive index of vinyl chloride resin, and is therefore preferable from the viewpoint of improving transparency. If the refractive index is less than 1.0, the transparency may be impaired due to the difference in refractive index with the vinyl chloride resin.
[0029] The plasticizer may be selected from those having a solubility parameter (sp value) in the range of about 9.3 to 12.0. From the viewpoint of compatibility with vinyl chloride resin, the solubility parameter of the plasticizer is preferably 9.4 or more, more preferably 9.5 or more, and more preferably 9.6 or more. The solubility parameter of the plasticizer is preferably 11.0 or less, more preferably 10.5 or less, and more preferably 10.0 or less. When the solubility parameter is within the above range, the compatibility of the plasticizer with vinyl chloride resin is improved, which contributes to improving transparency.
[0030] Examples of plasticizers that can be used in the present invention include epoxy plasticizers, ester plasticizers, polyester plasticizers, etc. In particular, examples of ester plasticizers include 2-ethylhexyl esters, linear alkyl esters, isononyl esters, dipentaerythritol esters, adipic acid esters, phthalic acid esters, benzoic acid esters, tributyl acetyl citrate, alkylsulfonic acid esters, and octyl terephthalate esters. From the viewpoints of transparency and compatibility, the plasticizer is preferably a benzoic acid ester plasticizer.
[0031] The content of the plasticizer is, for example, 60 parts by mass or more, preferably 80 parts by mass or more, more preferably 100 parts by mass or more, relative to 100 parts by mass of the vinyl chloride resin. The content of the plasticizer may be, for example, 360 parts by mass or less, preferably 240 parts by mass or less, more preferably 200 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. A content within such a numerical range is preferable for improving transparency.
[0032] (5) Stabilizers The transparent erasing composition of the present invention may further contain a stabilizer. Examples of stabilizers that can be used in the present invention include organic tin stabilizers, calcium-zinc stabilizers, and barium-zinc stabilizers. The stabilizer is preferably an organic tin stabilizer. The organic tin stabilizer is preferred from the viewpoint of compatibility with the vinyl chloride resin. Examples of the organic tin stabilizer include methyltin mercaptide, butyltin maleate, octyltin mercaptide, and octyltin maleate, and the organic tin stabilizer may contain one or more of these. The organic tin stabilizer provides color prevention, transparency, and stability during processing.
[0033] The content of the stabilizer is, for example, 0.1 parts by mass or more, preferably 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the vinyl chloride resin. The content of the stabilizer may be, for example, 5.0 parts by mass or less, preferably 3.0 parts by mass or less, more preferably 2.0 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. A content within such a numerical range is preferable for improving transparency.
[0034] (6) Other ingredients In the present invention, in addition to the above-mentioned components, various additives can be added so long as they do not impair the transparency and erasability. Examples of the additives include softeners, antioxidants, abrasives, fillers, fragrances, colorants, surfactants, etc. Examples of the softeners include vegetable oils, animal oils, mineral oils, liquid paraffin, polybutene, etc. Examples of the antioxidants include dibutylhydroxytoluene and hindered phenol-based antioxidants. Examples of the colorants that can be used include known pigments such as organic pigments, inorganic pigments, and fluorescent pigments, and known dyes, but are not limited to these examples.
[0035] (7) Method for producing the composition The method for producing the transparent erasing composition of the present invention can be, for example, the method shown below, but is not particularly limited thereto.
[0036] The method for producing the transparent erasing composition of the present invention may include, for example, the following steps. (7)-1 A mixing step of obtaining a mixture by mixing a polyvinyl chloride resin, a polysiloxane-based defoamer, a foam opener containing a polyalkylene glycol derivative, a benzoate-based plasticizer, and an organotin-based stabilizer; and (7)-2 A degassing step of stirring the mixture obtained in the mixing step under reduced pressure to degas the mixture. Each step will be described in detail below.
[0037] (7)-1 Mixing process A polyvinyl chloride resin, a polysiloxane-based defoamer, a defoamer containing a polyalkylene glycol derivative, a benzoate-based plasticizer, and an organotin-based stabilizer are mixed in a mixer or the like to obtain a mixture. The mixing step can be performed by a stirring device known in the art. The liquid temperature in the mixing step may be, for example, 10°C to 50°C, preferably 20°C to 40°C, and more preferably 20°C to 30°C, but is not limited to this range.
[0038] (7)-2 Defoaming process The mixture obtained in the mixing step may be subjected to a defoaming step under atmospheric pressure, or may be stirred under reduced pressure to promote defoaming. In this specification, "under reduced pressure" may mean, for example, an absolute pressure of 10 kPa or less, preferably 5 kPa, and more preferably 2.5 kPa or less. The defoaming step may be performed under absolute vacuum (0 kPa). The liquid temperature in the defoaming step may be, for example, 10°C to 50°C, preferably 20°C to 40°C, and more preferably 20°C to 30°C, but is not limited to this range.
[0039] (8) Properties and Use of Transparent Eraser Composition The transparent eraser composition of the present invention may be in a sol state, and is preferably a plastisol composition. A plastisol composition is preferred from the viewpoint of ease of production of the eraser, since it is easy to pour into a mold having a desired shape. The viscosity of the plastisol composition at 23±2° C. may be, for example, 50 mPa·s to 10,000 mPa·s, and preferably 500 mPa·s to 5,000 mPa·s. The transparent erasing composition of the present invention can be used as an eraser by curing it. As described later, the eraser may be used to erase handwriting of a pencil, a mechanical pencil, a friction ballpoint pen (e.g., a ballpoint pen using a reversible thermochromic ink), etc.
[0040] The erasability of the eraser can be evaluated by the erasing rate. The erasing rate E (%) is calculated from the density M of the erased part and the density C of the colored part by the following formula 1. The values of M and C may be measured according to JIS S 6050.
[0041]
number
[0042] The erasability of the transparent eraser obtained from the transparent erasing composition of the present invention may be, for example, 60% to 100%, preferably 70% to 100%, and more preferably 80% to 100%.
[0043] (9) Method for curing transparent eraser composition The cured product of the transparent erasing composition of the present invention can be obtained by heating and melting the composition and molding it. Examples of the molding method include injection molding, extrusion molding, and press molding using a hot plate. In the cured product of the transparent erasing composition of the present invention, the composition (particularly, the composition in a sol state, more particularly, the plastisol composition) may be poured into a predetermined mold, and heated in the mold to be cured. In the present invention, the following method may be used as an example, but is not limited thereto.
[0044] The temperature applied for the curing is, for example, 100° C. or more, preferably 120° C. or more, more preferably 130° C. or more. The temperature is, for example, 200° C. or less, preferably 180° C. or less, more preferably 150° C. or less. The time for which the temperature is maintained is, for example, 3 minutes or more, preferably 5 minutes or more, more preferably 10 minutes or more, and is, for example, 30 minutes or less, preferably 20 minutes or less, more preferably 15 minutes or less. The composition of the present invention is used to be cured by subjecting it to a heating step at such a temperature and / or for such a time. In addition, the cured product of the transparent erasing composition of the present invention may be subjected to a cutting process after curing. In the cutting process, the cured product may be cut into a desired shape. The shape may be appropriately selected by a person skilled in the art. As a cutting means, a device known in the art may be used, for example, a lever-type cutting cutter, a disk cutter, or an electric saw may be adopted, but is not limited thereto.
[0045] (10) Use of the cured product The cured product obtained by the above-mentioned curing method can be used as an eraser. For example, handwriting made with a pencil or ballpoint pen can be erased by rubbing the eraser with the above-mentioned eraser.
[0046] (11) Physical properties of the cured product The cured product obtained by curing the transparent erasing composition of the present invention exhibits excellent transparency, which can be evaluated by the following physical properties.
[0047] (11)-1 Haze value The haze value is used as an index representing the transparency of materials such as plastics and glass. The haze value is calculated from the values of "total light transmittance (Tt)" and "parallel light transmittance (Pt)" measured using known measuring equipment using the following formula 2.
[0048]
number
[0049] The transparent erasing composition of the present invention was deposited to a thickness of 1.5 mm and cured by heating at 180° C. for 90 seconds to obtain a cured product. The haze value of the obtained cured product is preferably 25 or less, more preferably 20 or less. A composition that gives a cured product having such a haze value is suitable for producing a transparent eraser.
[0050] The present invention will be described in more detail below based on experimental examples. Note that the experimental examples described below are representative examples of the present invention, and the scope of the present invention is not limited to these.
[0051] 1. Preparation of Transparent Eraser Composition
[0052] (Experimental Example 1) (1)Mixing process 100 parts by mass of R-860 (manufactured by Tosoh Corporation, average degree of polymerization 1600) as a vinyl chloride resin, 120 parts by mass of PN-6122 (manufactured by ADEKA Corporation) as a plasticizer, and 1 part by mass of STX-80 (manufactured by Daikyo Kasei Co., Ltd.) as a stabilizer were stirred in a blender to obtain Mixture 1, which is a plastisol composition.
[0053] (2)Defoaming process The mixture 1 obtained in the above (1) was degassed under reduced pressure (0.1 kPa) using a desiccator to obtain the desired transparent eraser composition 1.
[0054] (Experimental Example 2) Mixture 2 and the target transparent eraser composition 2 were obtained in the same manner as in Experimental Example 1, except that 0.02 parts by mass of BYK-3105 (manufactured by BYK) was added as a defoaming agent.
[0055] (Experimental Example 3) A mixture 3 and the target transparent eraser composition 3 were obtained in the same manner as in Experimental Example 1, except that 1 part by mass of Disfoam CD-432 (manufactured by NOF Corp.) was added as a defoamer.
[0056] (Experimental Example 4) The mixture 4 and the target transparent eraser composition 4 were obtained in the same manner as in the above-mentioned Experimental Example 1, except that 0.02 parts by mass of BYK-3105 (manufactured by BYK) was added as a defoaming agent, and 1 part by mass of Disfoam CD-432 (manufactured by NOF Corp.) was added as a defoaming agent.
[0057] (Experimental Example 5) Mixture 5 and the target transparent eraser composition 5 were obtained in the same manner as in Experimental Example 2, except that 1 part by mass of Disparlon P-450 (manufactured by Kusumoto Chemicals Co., Ltd.) was added as a defoamer.
[0058] (Experimental Example 6) A mixture 6 and the target transparent eraser composition 6 were obtained in the same manner as in Experimental Example 2, except that 1 part by mass of Surfynol DF-58 (manufactured by Nissin Chemical Industry Co., Ltd.) was added as a defoamer.
[0059] 2. Preparation of the cured transparent erasing composition
[0060] The transparent erasing compositions 1 to 4 obtained in the above Experimental Examples 1 to 6 were placed in a mold and cured (gelled) by heating at 180°C for 90 seconds. After the mold was cooled, the cured products were removed from the mold to obtain cured product samples 1 to 6. The cured product samples 1 to 6 were poured into the mold to a thickness of 1.5 mm and cured.
[0061] The transparent erasing compositions 1 to 6 and the cured product samples 1 to 6 obtained in Experimental Examples 1 to 6 were each evaluated as follows.
[0062] 1. Antifoaming evaluation
[0063] 1-1 Evaluation of time required When 80 g of each of the mixtures 1 to 6 was degassed, the time until foam generation ceased and the liquid level returned to the original height was measured.
[0064] 1-2 Evaluation by number of bubbles For each of the cured product samples 1 to 6, the number of bubbles remaining in the sample was counted.
[0065] 2. Transparency assessment
[0066] 2-1 Evaluation by haze value The haze value was measured for the 1.5 mm-thick cured product samples 1 to 6. The measurement conditions were as follows.
[0067] The transparency of the cured product samples 1 to 6 was evaluated according to the haze value measured by the above method, using the following three-level evaluation system. A: Haze value is 25 or less B: Haze value is over 25 and 50 or less C: Haze value is over 50
[0068] The composition of each experimental example and the results of each evaluation are shown in Table 1.
[0069] [Table 1]
[0070] From the results of Experimental Examples 1 to 6, it was found that the transparent eraser composition containing a polyvinyl chloride resin, a polysiloxane-based defoaming agent, and a defoamer containing a polyalkylene glycol derivative has excellent defoaming properties and exhibits transparency.
[0071] In Experimental Examples 2 and 3, a defoaming agent having a polysiloxane structure and a foam breaker containing a polyalkylene glycol derivative were added to the composition of Experimental Example 1. Here, in Experimental Example 2, the defoaming time was shortened by 1 minute 58 seconds compared to Experimental Example 1, and all the bubbles in the cured product sample 2 were eliminated. In Experimental Example 3, the defoaming time was shortened by 48 seconds compared to Experimental Example 1, but 6 bubbles remained in the cured product sample 3.
[0072] On the other hand, Experimental Example 4 is an experimental example in which both the defoaming agent having a polysiloxane structure and the foam breaker containing a polyalkylene glycol derivative, which were added in Experimental Examples 2 and 3, were added. In the evaluation of Experimental Example 4, the time required for defoaming was significantly reduced to 3 minutes and 28 seconds compared to Experimental Example 1, and all the bubbles in the cured product sample 4 were eliminated. From this, it can be seen that by comparing Experimental Examples 2 and 3 with Experimental Example 4, an extremely excellent defoaming effect can be obtained by using a defoaming agent having a polysiloxane structure and a foam breaker containing a polyalkylene glycol derivative in combination. In addition, the transparency was evaluated as A based on the haze value.
[0073] From the above, the transparent eraser composition containing polyvinyl chloride resin, a defoaming agent having a polysiloxane structure, and a defoaming agent containing a polyalkylene glycol derivative has excellent transparency and can improve production efficiency due to its excellent defoaming properties.
[0074] Moreover, Experimental Examples 5 and 6 are experimental examples in which a defoamer and a foam opener having a polysiloxane structure were used in combination with Experimental Example 1. However, the foam opener used in Experimental Example 5 is a foam opener whose main component is a special vinyl polymer, while the foam opener used in Experimental Example 6 is a nonionic surfactant with an acetylene group in the center and a symmetrical structure.
[0075] In the evaluation of Experimental Example 5, the time required for defoaming was significantly reduced to 3 minutes and 33 seconds compared to Experimental Example 1, and all bubbles in the cured product sample 5 were eliminated. However, the evaluation based on the haze value was lowered, and transparency was impaired. In addition, in Experimental Example 6, the time required for defoaming was 12 seconds longer than in Experimental Example 1, and two bubbles remained in the cured product sample 6. In addition, although transparency was maintained, the evaluation based on the haze value was lowered compared to Experimental Example 1.
[0076] It is also evident from the results of Experimental Examples 4, 5 and 6 that the types of defoaming agent and cell breaker that can be used in combination are important. In other words, it is also evident that the combination of a polysiloxane-based defoaming agent and a cell breaker containing a polyalkylene glycol derivative is important for achieving excellent transparency.
[0077] 3. Manufacturing of transparent erasers The composition of Experimental Example 4 was cured to prepare a transparent eraser having a thickness of 10 mm. The transparent eraser was visually evaluated and found to be transparent. In other words, it was confirmed that a transparent eraser can be produced by the transparent eraser composition of the present invention.
Claims
1. Polyvinyl chloride resin; A polysiloxane-based defoaming agent; A foam breaker comprising a polyalkylene glycol derivative; A transparent erasing composition comprising:
2. 2. The transparent erasing composition according to claim 1, further comprising a benzoate-based plasticizer.
3. 3. The transparent erasing composition according to claim 1, further comprising an organotin stabilizer.
4. 4. The transparent erasing composition according to claim 1, wherein the polysiloxane defoaming agent is contained in an amount of 0.001 parts by mass or more and 0.5 parts by mass or less based on 100 parts by mass of the polyvinyl chloride resin.
5. 5. The transparent eraser composition according to claim 1, wherein the amount of the defoamer containing the polyalkylene glycol derivative is 0.1 parts by mass or more and 3.0 parts by mass or less based on 100 parts by mass of the polyvinyl chloride resin.
6. 6. The transparent erasing composition according to claim 1, which is a plastisol composition.
7. A cured product of the transparent erasing composition according to any one of claims 1 to 6.
8. The cured product according to claim 7 , which is used as an eraser.
Citation Information
Patent Citations
Perspective eraser and preparation method thereof
CN114262489A
Plastic eraser composition
JP1981090864A
Eraser made of vinyl chloride group resin
JP1987042898A
Eraser
JP2013233725A
Character eraser
JP2014008773A