Self-adhesive foam laminate sheet

The self-adhesive foam laminate sheet with a polymer, crosslinking agent, and wax agent composition addresses air release issues under heat and pressure, maintaining strong adhesion and reducing residue.

JP7575194B2Active Publication Date: 2024-10-29ZEON CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020026400
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-19
Publication Date
2024-10-29
Estimated Expiration
2040-02-19

AI Technical Summary

Technical Problem

Conventional self-adhesive foam laminate sheets lack excellent air release properties when exposed to high temperatures and pressures, leading to air pockets and resin residue on adherends.

Method used

A self-adhesive foam laminate sheet comprising a synthetic paper base material and a foam layer formed using a composition containing a polymer, crosslinking agent, and wax agent, with specific monomer units and fatty acid esters to enhance air release properties.

Benefits of technology

The laminate sheet maintains excellent air release properties after heating and pressurizing, reducing resin residue and ensuring strong adhesion to adherends.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575194000002
    Figure 0007575194000002
  • Figure 0007575194000003
    Figure 0007575194000003
  • Figure 0007575194000001
    Figure 0007575194000001
Patent Text Reader

Abstract

To provide a self-adsorption foamed laminate sheet which is excellent in terms of air releasability after heating and pressing.SOLUTION: The self-adsorption foamed laminate sheet comprises a synthetic-paper base and a self-adsorption foamed sheet. The self-adsorption foamed laminate sheet is formed from a composition for the self-adsorption foamed sheet which comprises a polymer, a crosslinking agent, and a wax agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a self-adhesive foam laminate sheet. [Background technology]

[0002] In recent years, a sheet-like member made of a foam material having a large number of fine pores and having self-adhesive properties, that is, a self-adhesive foam sheet (hereinafter sometimes abbreviated as "foam sheet"), has been used as an adhesive sheet to be attached to a smooth adherend such as a window glass. The adhesive mode of the self-adhesive foam sheet is not glue adhesion, but adhesion to the adherend using fine pores. Therefore, the self-adhesive foam sheet is easier to reattach than the conventional adhesive sheet using glue adhesion, and is preferably used for applications such as wallpaper, posters, and stickers. When used for these applications, the self-adhesive foam sheet is used in the form of a self-adhesive foam laminate sheet (hereinafter sometimes abbreviated as "laminate sheet") laminated with a substrate (synthetic paper substrate) made of synthetic paper, for example. By applying decoration such as printing to the surface of the synthetic paper substrate side of this self-adhesive foam laminate sheet, it can be advantageously used for the above-mentioned applications.

[0003] Conventionally, various studies have been conducted to improve the performance of self-adhesive foam laminate sheets.

[0004] For example, in Patent Document 1, a composition used in preparing a foam sheet constituting a laminate sheet (hereinafter referred to as a "self-adhesive foam sheet composition" and sometimes abbreviated as "foam sheet composition") has been improved. According to Patent Document 1, a laminate sheet including a foam sheet formed from a foam sheet composition containing a polymer having predetermined properties and a crosslinking agent can suppress resin residue on glass as an adherend even after weathering. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2018 / 151274 Summary of the Invention [Problem to be solved by the invention]

[0006] Here, the laminate sheet is required to have the property of easily removing air pockets remaining between the sheet and the adherend when the surface on the foamed sheet side is adhered to the adherend (i.e., excellent air release properties). In particular, since the laminate sheet may be exposed to a high-temperature and pressurized environment during transportation, it is required to maintain excellent air release properties even after heating and pressurization (i.e., excellent air release properties after heating and pressurization). However, according to the study by the present inventors, the above-mentioned conventional laminate sheets still have room for improvement in terms of air release properties after heating and pressurization.

[0007] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a self-adhesive foam laminate sheet which is excellent in air release properties after heating and pressurizing. [Means for solving the problem]

[0008] The present inventors have conducted extensive research with the aim of solving the above problems, and have found that by forming a foamed sheet on a synthetic paper substrate using a foamed sheet composition containing a polymer, a crosslinking agent, and a wax agent, the laminated sheet can exhibit excellent air release properties even after heating and pressurization, and have completed the present invention.

[0009] That is, the present invention has an object to advantageously solve the above problems, and the self-adhesive foam laminate sheet of the present invention is a self-adhesive foam laminate sheet comprising a synthetic paper base material and a self-adhesive foam sheet, BubbleThe foam sheet is formed by using a composition for a self-adhesive foam sheet containing a polymer, a crosslinking agent, and a wax agent. In this way, by forming a foam sheet on a substrate made of synthetic paper by using a composition for a foam sheet containing a polymer, a crosslinking agent, and a wax agent, the laminated sheet can exhibit excellent air release properties even after heating and pressing. In the present invention, the term "synthetic paper" refers to a film made from a resin composition containing a thermoplastic resin and a filler.

[0010] Here, in the self-adhesive laminated foam sheet of the present invention, the polymer preferably contains 60% by mass or more and 99% by mass or less of (meth)acrylate monomer units. By forming a foam sheet using a composition for a foam sheet containing a polymer containing (meth)acrylate monomer units in the above-mentioned ratio, it is possible to obtain a laminated sheet that maintains good self-adhesive strength (adhesive strength to an adherend) while suppressing resin residue on the adherend. In the present invention, the phrase "containing a monomer unit" means that "a polymer obtained by using the monomer contains a repeating unit derived from the monomer." In addition, in the present invention, "(meth)acrylate" means acrylate and / or methacrylate.

[0011] In the self-adhesive laminated foam sheet of the present invention, the polymer preferably contains 0.1% by mass or more and 10% by mass or less of unsaturated carboxylic acid monomer units. By forming a foam sheet using a composition for a foam sheet containing a polymer containing unsaturated carboxylic acid monomer units in the above-mentioned ratio, the foam sheet can be given sufficient strength. In addition, a laminated sheet can be obtained in which the resin residue on the adherend is suppressed while maintaining good self-adhesive strength.

[0012] In the self-adhesive laminated foam sheet of the present invention, the polymer preferably does not have an N-methylol group. If a foam sheet is formed using a foam sheet composition containing a polymer that does not have an N-methylol group, the generation of formaldehyde during foaming and curing of the foam sheet composition can be sufficiently suppressed.

[0013] Here, in the self-adhesive foamed laminate sheet of the present invention, the wax agent preferably contains a fatty acid ester having a fatty acid moiety with a carbon number of 16 to 34. If a fatty acid ester having a fatty acid moiety (a structure derived from a fatty acid in a fatty acid ester) with a carbon number within the above-mentioned range is used as the wax agent, the air release property of the laminate sheet after heating and pressing can be further improved.

[0014] Furthermore, in the self-adhesive foamed laminate sheet of the present invention, it is preferable that the fatty acid ester has an alcohol moiety having a carbon number of 30 to 34. If a fatty acid ester having an alcohol moiety (a structure derived from the alcohol in the fatty acid ester) having a carbon number within the above-mentioned range is used as the wax agent, the air release property of the laminate sheet after heating and pressing can be further improved.

[0015] In the self-adhesive laminated foam sheet of the present invention, the amount of the fatty acid ester is preferably 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the polymer. By using a foamed sheet composition in which the amount of the wax agent per 100 parts by mass of the polymer is within the above-mentioned range, the air release property of the laminated sheet after heating and pressing can be further improved. Effect of the Invention

[0016] According to the present invention, a self-adhesive foam laminate sheet having excellent air release properties after heating and pressurization can be provided. [Brief description of the drawings]

[0017] [Figure 1]1 is a flow chart illustrating an example of a method for producing a self-adhesive foam laminate sheet according to the present invention. [Diagram 2] FIG. 2 is an explanatory diagram showing a schematic configuration of an evaluation device used to evaluate the air release properties of the self-adhesive foam laminated sheets in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail. The self-adhesive foam laminate sheet of the present invention has a foam layer made of a self-adhesive foam sheet obtained by using a composition for a self-adhesive foam sheet, and a synthetic paper substrate as a support layer supporting the foam layer. The foam sheet may be formed directly on the synthetic paper substrate, or may be formed on the synthetic paper substrate via an arbitrary layer.

[0019] (Self-adhesive foam sheet) The foamed sheet that forms the foamed layer in the laminate sheet of the present invention is formed by crosslinking and foaming a predetermined composition for a self-adhesive foamed sheet.

[0020] <Composition for self-adhesive foam sheet> The foam sheet composition comprises a polymer, a crosslinking agent, and a wax agent, and optionally further contains a solvent and other additives. By forming a foamed sheet on a synthetic paper substrate using the foamed sheet composition, a laminated sheet of the present invention having excellent air release properties after heating and pressurization can be obtained.

[0021] <<Polymer>> The polymer used in the foam sheet composition forms a resin matrix in the foam sheet obtained by foaming and crosslinking the foam sheet composition.

[0022] Here, the polymer is not particularly limited, but may contain at least one monomer unit selected from the group consisting of (meth)acrylate monomer units, unsaturated carboxylic acid monomer units, vinyl cyanide monomer units, and alkenyl aromatic monomer units. The polymer may also contain monomer units other than (meth)acrylate monomer units, unsaturated carboxylic acid monomer units, vinyl cyanide monomer units, and alkenyl aromatic monomer units (hereinafter referred to as "other monomer units").

[0023] [(Meth)acrylate monomer unit] The (meth)acrylate monomer unit is a repeating unit derived from a (meth)acrylate monomer. When the polymer contains the (meth)acrylate monomer unit, flexibility is imparted to the resulting foamed sheet, and a laminated sheet having good self-adhesive strength can be obtained.

[0024] The (meth)acrylate monomer is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, n-heptyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and n-dodecyl (meth)acrylate; and (meth)acrylic acid alkoxyalkyl ester monomers such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, and ethoxymethyl (meth)acrylate. The (meth)acrylate monomers may be used alone or in combination of two or more kinds. In the present invention, "(meth)acrylic" means acrylic and / or methacrylic.

[0025] Here, as the (meth)acrylate monomer, from the viewpoint of further increasing the flexibility of the foamed sheet and further ensuring the self-adhesive strength of the laminated sheet, a (meth)acrylic acid alkyl ester monomer is preferred, and a (meth)acrylic acid alkyl ester monomer having an alkyl group (bonded to a non-carbonyl oxygen atom) with 1 to 14 carbon atoms (hereinafter sometimes abbreviated as "C1-14 (meth)acrylic acid alkyl ester monomer") is more preferred.

[0026] Examples of C1-14 (meth)acrylic acid alkyl ester monomers include methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, sec-butyl acrylate, n-heptyl acrylate, n-hexyl acrylate, n-octyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-octyl methacrylate, and n-dodecyl methacrylate. Among these, n-butyl acrylate, ethyl acrylate, and 2-ethylhexyl acrylate are preferred from the viewpoints of self-adhesiveness and cost.

[0027] The proportion of the (meth)acrylate monomer units in the polymer is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 85% by mass or more, and preferably 99% by mass or less, more preferably 95% by mass or less, and even more preferably 92% by mass or less, based on the total repeating units (total monomer units) contained in the polymer being 100% by mass. If the proportion of the (meth)acrylate monomer units in the polymer is 60% by mass or more, the self-adhesive strength of the laminated sheet can be sufficiently ensured. On the other hand, if the proportion of the (meth)acrylate monomer units in the polymer is 99% by mass or less, the self-adhesive strength of the laminated sheet will not be excessively increased. Therefore, the resin residue on the laminated sheet can be suppressed.

[0028] [Unsaturated carboxylic acid monomer unit] The unsaturated carboxylic acid monomer unit is a repeating unit derived from an unsaturated carboxylic acid monomer. Specific examples of the unsaturated carboxylic acid monomer include α,β-ethylenically unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid; α,β-ethylenically unsaturated polycarboxylic acids such as itaconic acid, maleic acid, and fumaric acid; and α,β-ethylenically unsaturated polycarboxylic acid partial esters such as monomethyl itaconate, monobutyl maleate, and monopropyl fumarate. In addition, those having a group that can be derived into a carboxylic acid group by hydrolysis, such as maleic anhydride and itaconic anhydride, can also be used. Among these, itaconic acid, acrylic acid, and methacrylic acid are preferred, and acrylic acid is more preferred, from the viewpoints of reactivity with the crosslinking agent described below, stability of the polymer latex, and cost. The unsaturated carboxylic acid monomers may be used alone or in combination of two or more kinds.

[0029] The proportion of the unsaturated carboxylic acid monomer unit in the polymer is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, more preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 2.5% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer. When the proportion of the unsaturated carboxylic acid monomer unit in the polymer is 0.1% by mass or more, the crosslinking reaction by the crosslinking agent described later can be sufficiently promoted. As a result, the resin residue on the adherend of the laminate sheet can be suppressed while imparting sufficient strength to the obtained foamed sheet. On the other hand, when the proportion of the unsaturated carboxylic acid monomer unit in the polymer is 10% by mass or less, it becomes easy to keep the viscosity of the polymerization system during polymerization within an appropriate range, and the self-adhesive force of the laminate sheet is not impaired due to excessive crosslinking of the polymer.

[0030] [Vinyl cyanide monomer unit] The vinyl cyanide monomer unit is a repeating unit derived from a vinyl cyanide monomer. A specific example of the vinyl cyanide monomer is an α,β-ethylenically unsaturated nitrile monomer. The α,β-ethylenically unsaturated nitrile monomer is not particularly limited as long as it is an α,β-ethylenically unsaturated compound having a nitrile group, and examples thereof include acrylonitrile; α-halogenoacrylonitrile such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkylacrylonitrile such as methacrylonitrile and α-ethylacrylonitrile; and the like. Among these, acrylonitrile is preferred from the viewpoint of improving the cohesive force of the composition for foamed sheet and increasing the breaking strength of the foamed sheet. The vinyl cyanide monomers may be used alone or in combination of two or more.

[0031] The proportion of the vinyl cyanide monomer unit in the polymer is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of all repeating units (all monomer units) contained in the polymer. If the proportion of the vinyl cyanide monomer unit in the polymer is 1% by mass or more, the resulting foamed sheet can be given sufficient strength while suppressing the resin residue on the adherend of the laminated sheet. On the other hand, if the proportion of the vinyl cyanide monomer unit in the polymer is 30% by mass or less, the flexibility of the resulting foamed sheet can be sufficiently ensured, and a laminated sheet having good self-adhesive strength can be obtained.

[0032] [Alkenyl aromatic monomer unit] The alkenyl aromatic monomer unit is a repeating unit derived from an alkenyl aromatic monomer. Specific examples of the alkenyl aromatic monomer include styrene, α-methylstyrene, α-chlorostyrene, vinyltoluene, and divinylbenzene. Among these, styrene is preferred from the viewpoint of polymerizability and cost. The alkenyl aromatic monomers may be used alone or in combination of two or more kinds.

[0033] The proportion of the alkenyl aromatic monomer unit in the polymer is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 1.5% by mass or more, and preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total repeating units (total monomer units) contained in the polymer being 100% by mass. If the proportion of the alkenyl aromatic monomer unit in the polymer is 0.5% by mass or more, the hydrophobicity of the alkenyl aromatic monomer unit can prevent water from penetrating into the foamed sheet, and the water resistance of the laminated sheet can be improved. On the other hand, if the proportion of the alkenyl aromatic monomer unit in the polymer is 20% by mass or less, the flexibility of the resulting foamed sheet can be sufficiently ensured, and a laminated sheet having good self-adhesive strength can be obtained.

[0034] [Other monomer units] The other monomer units are repeating units derived from other monomers copolymerizable with the above-mentioned monomers. Here, examples of the other monomers include conjugated diene monomers, α,β-ethylenically unsaturated polyvalent carboxylic acid complete ester monomers, carboxylic acid unsaturated alcohol ester monomers, olefin monomers, and other monomers having functional groups. These monomers may be used alone or in combination of two or more. Specific examples of such other monomers are not particularly limited, and may include those described in International Publication No. WO 2018 / 151274.

[0035] In order to sufficiently suppress the generation of formaldehyde during foaming and curing of the foam sheet composition, the polymer preferably does not have an N-methylol group, more specifically, the polymer preferably does not contain a monomer unit having an N-methylol group. Here, examples of the monomer having an N-methylol group include N-methylol acrylamide and N-methylol methacrylamide.

[0036] [Polymer properties] -Glass transition temperature- Here, the glass transition temperature of the polymer is preferably -10°C or lower, more preferably -13°C or lower, even more preferably -17°C or lower, and particularly preferably -20°C or lower. If the glass transition temperature of the polymer is -10°C or lower, the laminate sheet can be well adhered to the adherend while the self-adhesive strength of the laminate sheet is sufficiently ensured, thereby preventing moisture from penetrating between the adherend and the laminate sheet. Therefore, the water resistance of the laminate sheet can be increased. Further, the lower limit of the glass transition temperature of the polymer is not particularly limited, but from the viewpoint of sufficiently suppressing the resin from remaining on the adherend of the laminate sheet, it is preferably −40° C. or higher. The glass transition temperature of the polymer can be measured by the method described in the Examples of this specification.

[0037] -Gel fraction- Here, the gel fraction of the polymer is preferably 95% by mass or less, more preferably 93% by mass or less. If the gel fraction is 95% by mass or less, a foamed sheet and a laminated sheet having appropriate self-adhesive strength and excellent smoothness can be produced. The lower limit of the gel fraction of the polymer is not particularly limited, but can be, for example, 50% by mass or more, and can be 70% by mass or more. The gel fraction of the polymer can be measured by the method described in the Examples of this specification.

[0038] [Method of preparing polymer] The polymerization method for obtaining the polymer is not particularly limited, and may be any of solution polymerization, emulsion polymerization, suspension polymerization, bulk polymerization, etc., or other methods. There is no particular limit to the type or amount of the polymerization initiator, emulsifier, dispersant, etc. used in the polymerization. There is no particular limit to the method of adding the monomer, polymerization initiator, emulsifier, dispersant, etc. during the polymerization. There is also no particular limit to the polymerization temperature, pressure, stirring conditions, etc. Incidentally, the polymer can be used in a solid state. However, when the polymer is used in the form of a latex containing a polymer (polymer latex), such as a latex obtained by emulsion polymerization or a latex obtained by post-emulsification of a polymer, the operation of mixing the polymer with a crosslinking agent, a wax agent, etc. is easy, and it is also convenient for foaming the obtained foam sheet composition. Here, when the polymer is used in the form of a polymer latex for preparing a foam sheet composition as described above, the solids concentration of the polymer latex is, from the viewpoint of maintaining the density of the resulting foam sheet, preferably 40 mass % or more, more preferably 45 mass % or more, even more preferably 50 mass % or more, particularly preferably 52 mass % or more, and is preferably 70 mass % or less, and more preferably 58 mass % or less.

[0039] <<Crosslinking agent>> The crosslinking agent contained in the foamed sheet composition is not particularly limited as long as it can form a crosslinked structure with the above-mentioned polymer (particularly the unsaturated carboxylic acid monomer unit of the above-mentioned polymer). Examples of such crosslinking agents include carbodiimide-based crosslinking agents; epoxy-based crosslinking agents; oxazoline-based crosslinking agents; polyfunctional isocyanate-based crosslinking agents such as tolylene diisocyanate, trimethylolpropane tolylene diisocyanate, and diphenylmethane triisocyanate; metal salt-based crosslinking agents; metal chelate-based crosslinking agents; and peroxide-based crosslinking agents. Among them, epoxy-based crosslinking agents are preferably used, and compounds having two or more epoxy groups in one molecule are more preferably used. As the epoxy-based crosslinking agent, fatty acid polyglycidyl ether, glycerol polyglycidyl ether, and ethylene glycol diglycidyl ether are preferred.

[0040] Here, the epoxy-based crosslinking agent may be synthesized by a known method, or a commercially available product may be used. An example of a commercially available epoxy-based crosslinking agent is "Rikabond (registered trademark)" manufactured by Japan Coating Resin Co., Ltd. The epoxy-based crosslinking agent forms a crosslinked structure within or between the molecules of the polymer by reacting the epoxy group contained therein with a functional group in the polymer (e.g., a carboxylic acid group derived from an unsaturated carboxylic acid monomer unit). By using the epoxy-based crosslinking agent, a foamed sheet having a suitable self-adhesive strength and excellent strength can be formed. Therefore, by using a foamed sheet composition containing an epoxy-based crosslinking agent as a crosslinking agent, the resin residue on the adherend of the laminated sheet can be suppressed.

[0041] In the present invention, it is preferable not to use a crosslinking agent that generates formaldehyde, such as a melamine-formaldehyde resin, a urea-formaldehyde resin, or a phenol-formaldehyde resin.

[0042] Here, the amount of the crosslinking agent in the composition for foamed sheet is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 3 parts by mass or more, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the above-mentioned polymer. By the amount of the crosslinking agent being within the above-mentioned range, a foamed sheet that maintains appropriate strength and elasticity can be obtained. Therefore, when the pressure applied to the foamed sheet is released, the foam cells in the foamed sheet that have been crushed can recover to their original shape. In addition, the self-adhesive force of the laminated sheet can be ensured, and the resin residue on the adherend of the laminated sheet can be sufficiently suppressed.

[0043] <<Wax agent>> The wax agent contained in the foamed sheet composition of the present invention is not particularly limited as long as it contains a fatty acid ester (particularly an ester of a higher fatty acid and a higher alcohol). The content of the fatty acid ester in the wax agent is preferably more than 50% by mass and less than 100% by mass (i.e., the main component) based on 100% by mass of the entire wax agent, preferably 70% by mass or more and less than 100% by mass, more preferably 80% by mass or more and less than 100% by mass, and particularly preferably 90% by mass or more and less than 100% by mass. The wax agent may contain one type of fatty acid ester, or may contain two or more types of fatty acid esters.

[0044] Here, the wax agent functions as a light release agent in the foam sheet formed using the foam sheet composition, and it is presumed that the open cell structure and elasticity of the foam sheet are improved by foaming and curing the foam sheet composition in which the wax agent is blended with the above-mentioned polymer, and the laminate sheet including the foam sheet can have excellent air release properties after heating and pressing.

[0045] The wax agent may be a natural wax, a synthetic wax, or a mixture thereof, with the use of a natural wax being preferred. Here, specific examples of natural waxes are not particularly limited as long as they contain naturally derived fatty acid esters, and include, for example, natural waxes derived from plants such as rice bran wax, sugarcane wax, carnauba wax, candelilla wax, jojoba oil, wood wax, and Moringa seed oil; natural waxes derived from animals such as beeswax, sperm oil, and wool fat; and natural waxes derived from minerals such as montan wax, ozokerite, and ceracin. Among these, Moringa seed oil is preferred from the viewpoint of further improving the air release property after heating and pressing the laminated sheet. These natural waxes may be refined from natural materials by known methods, or commercially available products may be used. Examples of commercially available natural waxes include "Refined Moringa Oil" manufactured by Nitto Bussan Shoji Co., Ltd. The wax agents may be used alone or in combination of two or more.

[0046] In addition, the fatty acid portion of the fatty acid ester contained in the wax preferably has 16 or more carbon atoms, more preferably has 18 or more carbon atoms, and preferably has 34 or less carbon atoms, and more preferably has 30 or less carbon atoms. If the carbon number of the fatty acid portion of the fatty acid ester is within the above-mentioned range, the air release property after heating and pressing of the laminated sheet can be further improved. Specific examples of fatty acids having 16 to 34 carbon atoms include saturated fatty acids such as stearic acid (carbon number 18), arachidic acid (carbon number 20), and behenic acid (carbon number 22); and unsaturated fatty acids such as oleic acid (carbon number 18), linoleic acid (carbon number 18), and linolenic acid (carbon number 18). These fatty acids may be used alone or in combination of two or more.

[0047] The alcohol portion of the fatty acid ester contained in the wax preferably has 30 or more carbon atoms, and preferably has 34 or less carbon atoms. If the carbon number of the alcohol portion of the fatty acid ester is within the above-mentioned range, the air release property of the laminated sheet after heating and pressurization can be further improved. Specific examples of alcohols having 30 or more and 34 or less carbon atoms include myricyl alcohol (carbon number 30), melissyl alcohol (carbon number 31), lacceryl alcohol (carbon number 32), cellomelitsyl alcohol (carbon number 33), and tetratriacontanol (carbon number 34). These alcohols may be used alone or in combination of two or more.

[0048] Here, the amount of the wax agent in the foamed sheet composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the polymer. If the amount of the wax agent is 0.5 parts by mass or more per 100 parts by mass of the polymer, the air release property of the laminated sheet after heating and pressing can be further improved. On the other hand, if the amount of the wax agent is 10 parts by mass or less per 100 parts by mass of the polymer, the obtained laminated sheet can be given good self-adhesive strength, and the air release property of the laminated sheet after heating and pressing can be further improved. In addition, the amount of the fatty acid ester having a fatty acid moiety with a carbon number of 16 to 34 in the foam sheet composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less per 100 parts by mass of the above-mentioned polymer. If the amount of the fatty acid ester having a fatty acid moiety with a carbon number of 16 to 34 inclusive is 0.5 parts by mass or more per 100 parts by mass of the polymer, the air release property of the laminate sheet after heating and pressing can be further improved. On the other hand, if the amount of the fatty acid ester having a fatty acid moiety with a carbon number of 16 to 34 inclusive is 10 parts by mass or less per 100 parts by mass of the polymer, the obtained laminate sheet can be given good self-adhesive strength, and the air release property of the laminate sheet after heating and pressing can be further improved.

[0049] <<Solvent>> The solvent that the composition for foam sheets may optionally contain is not particularly limited, but is preferably water. When water is used as the solvent, the water contained in the composition for foam sheets may be, for example, water derived from the polymer latex.

[0050] <<Other additives>> The foam sheet composition may optionally contain various additives to improve the processability in the manufacturing process of the foam sheet and the laminate sheet, and to improve the performance of the resulting foam sheet and the laminate sheet. Examples of such additives include foam stabilizers such as higher fatty acid salts and surfactants, foaming assistants, thickeners, fillers, preservatives, fungicides, gelling agents, flame retardants, antioxidants, antioxidants, pigments, dyes, tackifiers, conductive compounds, water resistance agents, and oil resistance agents. Specific examples of the other additives mentioned above are not particularly limited, and known additives, such as those described in International Publication No. 2016 / 147679, can be used.

[0051] <Properties of foam sheet> The self-adhesive foam sheet which forms the foam layer in the laminate sheet of the present invention is formed by crosslinking and foaming the above-mentioned foam sheet composition. Here, the density of the self-adhesive foam sheet is not particularly limited, but is preferably 0.1 g / cm 3 More than 1.0g / cm 3 It is preferable that the concentration is 0.3 g / cm or less. 3 More than 0.8g / cm 3 More preferably, it is 0.5 g / cm or less. 3 More than 0.7g / cm 3 It is more preferable that the density of the foamed sheet is 0.1 g / cm or less. 3 If the density is more than 1.0 g / cm, the strength of the foam sheet is ensured. 3 If it is equal to or less than this, the air release property of the laminated sheet after heating and pressurization can be further improved, while the resin remaining on the adherend can be sufficiently suppressed. The density of the foamed sheet can be calculated using the method described in the Examples of this specification.

[0052] The thickness of the foamed sheet is preferably 0.03 mm or more, more preferably 0.05 mm or more, even more preferably 0.1 mm or more, and preferably 3 mm or less, more preferably 1 mm or less, even more preferably 0.5 mm or less, and particularly preferably 0.2 mm or less. If the thickness of the foamed sheet is 0.03 mm or more, the mechanical strength of the foamed sheet and the laminated sheet can be sufficiently ensured. On the other hand, if the thickness of the foamed sheet is 3 mm or less, the air release property of the laminated sheet after heating and pressing can be further improved. In addition, a laminated sheet having excellent repeated attachment properties (rework performance) can be obtained.

[0053] (Synthetic paper base material) A synthetic paper substrate is used as the substrate in the laminate sheet of the present invention. The synthetic paper substrate is not particularly limited as long as it is a substrate made of synthetic paper as described above, but it is preferable to use a substrate made by forming a compound (resin composition) containing a thermoplastic resin and a filler, and optionally containing other additives, into a film. A known molding method can be used to form the compound into a film.

[0054] <Thermoplastic resin> Examples of the thermoplastic resin include polyethylene-based resins (low density polyethylene, linear low density polyethylene, medium density polyethylene, high density polyethylene, etc.), polypropylene-based resins, polymethyl-1-pentene, ethylene-cyclic olefin copolymers, and other polyamide resins; polyethylene terephthalate and its copolymers, polyethylene naphthalate, aliphatic polyesters, and other polyester-based resins; polycarbonate, atactic polystyrene, syndiotactic polystyrene, polyphenylene sulfide, and the like. These may be used alone or in combination of two or more. Among these, polyolefin-based resins and polyester-based resins are preferred, and polypropylene-based resins are more preferred. Examples of polypropylene-based resins include propylene homopolymers and copolymers of propylene, which is the main component, with ethylene, 1-butene, 1-hexene, 1-heptene, 4-methyl-1-pentene, and other α-olefins. The stereoregularity is not particularly limited, and isotactic or syndiotactic resins and those showing various degrees of stereoregularity can be used. The copolymer may be a binary, ternary, or quaternary copolymer, and may be a random copolymer or a block copolymer.

[0055] <<Filler>> The filler may be an inorganic filler, an organic filler, or a mixture thereof.

[0056] The inorganic filler is not particularly limited as long as it is a filler made of an inorganic compound, and examples thereof include fillers made of at least one of inorganic compounds such as calcium carbonate, calcined clay, silica, diatomaceous earth, talc, mica, synthetic mica, sericite, kaolinite, titanium oxide, barium sulfate, and alumina. The inorganic filler may be used alone or in combination of two or more. Among these, fillers made of calcium carbonate and titanium oxide are preferred.

[0057] As the organic filler, a filler made of a type of resin different from the thermoplastic resin that is the main component described above can be used. For example, when a polyolefin resin is used as the above-mentioned thermoplastic resin, examples of the organic filler include fillers made of at least one of polyethylene terephthalate, polybutylene terephthalate, polycarbonate, nylon 6, nylon 6,6, homopolymers of cyclic olefins, and copolymers of cyclic olefins and ethylene. Furthermore, when a polyester-based resin is used as the thermoplastic resin, examples of the organic filler include fillers made of at least one of polystyrene, polypropylene, polycarbonate, nylon 6, nylon 6,6, polymethyl-1-pentene, homopolymers of cyclic olefins, and copolymers of cyclic olefins and ethylene. The organic filler may be used alone or in combination of two or more. The resin constituting the organic filler preferably has a melting point of 120°C or more and 300°C or less. The resin constituting the organic filler preferably has a glass transition temperature of 120°C or more and 280°C or less.

[0058] The content of the above-mentioned filler in the synthetic paper base material is preferably 8% by mass or more and 65% by mass or less, and more preferably 10% by mass or more and 60% by mass or less. By keeping the filler content within the above range, it is possible to achieve a balance between the whiteness and opacity of the synthetic paper base material.

[0059] <<Other additives>> Examples of other additives include antioxidants, light stabilizers, dispersants, and lubricants. Examples of the antioxidant include sterically hindered phenol-based, phosphorus-based, amine-based, etc. The content of the antioxidant in the synthetic paper base material is, for example, 0.001% by mass or more and 1% by mass or less. Examples of the light stabilizer include sterically hindered amines, benzotriazoles, benzophenones, etc. The content of the light stabilizer in the synthetic paper base material is, for example, 0.001% by mass or more and 1% by mass or less. Examples of dispersants (particularly dispersants for the inorganic fillers described above) include silane coupling agents, higher fatty acids such as oleic acid and stearic acid, metal soaps, polyacrylic acid, polymethacrylic acid, salts thereof, etc. The content of the dispersant in the synthetic paper base material is, for example, 0.01% by mass or more and 4% by mass or less.

[0060] <<Synthetic paper base material properties>> Here, the synthetic paper base material is preferably porous. Specifically, the synthetic paper base material preferably has an overall porosity of 5% or more and 50% or less, and more preferably 15% or more and 45% or less. If the overall porosity is 5% or more, the opacity and flexibility of the synthetic paper base material can be increased, and if it is 50% or less, the mechanical strength of the synthetic paper base material, such as the tensile elastic modulus, can be easily set within an appropriate range. In the present invention, the "total porosity" can be determined by cutting out a cross section of the synthetic paper base material, observing it under an electron microscope, and measuring the area ratio (%) that is occupied by pores to the total area (100%).

[0061] The synthetic paper substrate may have a single layer structure or a multilayer structure. In the case of a single layer structure, the synthetic paper substrate (film) may be unstretched, uniaxially stretched, or biaxially stretched. In the case of a multilayer structure, the synthetic paper substrate may have a two-layer structure or a three or more layer structure. In the case of a two-layer structure, the synthetic paper substrate may have any of the following structures: unstretched / uniaxially stretched, unstretched / biaxially stretched, uniaxially stretched / uniaxially stretched, uniaxially stretched / biaxially stretched, or biaxially stretched / biaxially stretched. In the case of a three or more layer structure, any combination of the above single layer structure and two layer structure may be used.

[0062] The synthetic paper base material preferably has a whiteness of 80% or more, and more preferably 85% or more. By making the whiteness of the synthetic paper base material 80% or more, the content printed and recorded on the synthetic paper base material can be made even easier to distinguish. In the present invention, the "whiteness" can be measured in accordance with the method described in JIS-L1015.

[0063] Here, the synthetic paper base material can be adjusted to an appropriate opacity depending on the application. Specifically, the synthetic paper base material preferably has an opacity of 40% or more and 100% or less, more preferably 70% or more and 100% or less, and even more preferably 80% or more and 100% or less. If the opacity is 40% or more, sufficient hiding power as a printing paper can be obtained. In the present invention, the "opacity" can be measured in accordance with the method described in JIS-P8138.

[0064] The synthetic paper substrate preferably has a thickness of 20 μm or more and 900 μm or less, and more preferably 30 μm or more and 800 μm or less. If the thickness is 20 μm or more, the mechanical strength of the entire laminated sheet including the synthetic paper substrate can be improved, and it becomes possible to form a large-area poster or the like. On the other hand, if the thickness is 900 μm or less, the stiffness of the entire laminated sheet including the synthetic paper substrate can be prevented from becoming too strong, and the weight can be reduced to prevent it from falling off when applied.

[0065] (Method of manufacturing self-adhesive foam laminate sheet) An example of a method for producing the laminate sheet of the present invention will now be described.

[0066] Fig. 1 shows a flow chart for explaining an example of a method S10 for producing a laminated sheet (hereinafter, sometimes abbreviated as "production method S10"). As shown in Fig. 1, the production method S10 includes a composition preparation step S1, a foaming step S2, and a sheet formation step S3, in this order. Each step will be explained below.

[0067] <Composition preparation step S1> The composition preparation step S1 is a step of preparing a composition for a self-adhesive foam sheet.

[0068] Specifically, in the composition preparation step S1, a composition for a foam sheet can be prepared by mixing the essential components of a polymer, a crosslinking agent, and a wax agent, as well as a solvent and other additives that are used as desired, in any manner.

[0069] For example, when a polymer latex is used to prepare a foam sheet composition, the crosslinking agent, the wax agent, and other optional additives may be added to the polymer latex and mixed by a known method. When a solid polymer is used without using a solvent in the preparation of the foamed sheet composition, the solid polymer, the crosslinking agent, the wax agent, and other additives that are optionally used may be mixed by a known method (for example, using a known roll, Henschel mixer, kneader, etc.).

[0070] Here, the viscosity of the foam sheet composition containing a solvent (e.g., in the form of an emulsion or dispersion) is preferably 1,000 mPa·s to 10,000 mPa·s, more preferably 2,000 mPa·s to 10,000 mPa·s, and even more preferably 3,500 mPa·s to 5,500 mPa·s. If the viscosity of the foam sheet composition is 1,000 mPa·s or more, it is possible to prevent dripping, which makes it difficult to control the thickness, when a foam formed from the foam sheet composition is coated on a substrate to form a foam sheet. On the other hand, if the viscosity of the foam sheet composition is 10,000 mPa·s or less, it is also possible to prevent difficulty in controlling the expansion ratio by mechanical foaming when forming a foam sheet. The viscosity of the composition for a foam sheet can be measured by the method described in the Examples of this specification.

[0071] <Foaming process S2> The foaming step S2 is a step of foaming the composition for a foam sheet to obtain a foam of the composition for a foam sheet.

[0072] Specifically, in the foaming step S2, the foamed sheet composition prepared in the composition preparation step S1 is foamed to obtain a foam in an unsolidified (uncrosslinked) state. When the foamed sheet composition is in the form of an emulsion or dispersion, a foamed emulsion or foamed dispersion is obtained.

[0073] Mechanical foaming is usually used as the foaming method. The foaming ratio may be adjusted as appropriate, but is usually 1.2 to 5 times, preferably 1.5 to 4 times. The mechanical foaming method is not particularly limited, but can be carried out by mixing a certain amount of air into the emulsion or dispersion of the foamed sheet composition and stirring it continuously or batchwise with an oak mixer, whipper, or the like. The foamed emulsion or foamed dispersion thus obtained is creamy. By forming pores by the mechanical foaming, a foamed sheet having excellent air escape properties can be obtained through a sheet forming step S3 described later. When the foaming ratio is 1.2 times or more, the air escape properties can be prevented from decreasing, and when the foamed sheet is 5 times or less, the strength can be prevented from decreasing.

[0074] <<Sheeting process S3>> The sheet forming step S3 is a step of forming the foam into a sheet shape and then subjecting the foam to a crosslinking reaction to produce a foam sheet.

[0075] In the sheeting step S3, the method for forming the foam produced in the foaming step S2 into a sheet is not particularly limited. A suitable method is, for example, a method in which the foam is coated on a desired synthetic paper base material and then formed into a sheet. In this way, by coating the foam on the desired synthetic paper base material and allowing the crosslinking reaction to proceed, a laminated sheet in which a foam sheet is provided directly on the synthetic paper base material can be obtained.

[0076] The foam coating can also be performed on a release sheet (such as a release-capable processing paper) instead of the synthetic paper substrate. If the foam is coated on the release sheet and a crosslinking reaction is allowed to proceed, a laminate in which the foam sheet is provided directly on the release sheet can be obtained. Then, by peeling the release sheet from the foam sheet of this laminate, the foam sheet can be obtained alone (as an independent film).

[0077] As a method for coating the foam onto a synthetic paper substrate or a release sheet (hereinafter, these may be collectively referred to as "substrate, etc."), a commonly known coating device such as an applicator, bar coater, roll coater, reverse roll coater, screen coater, doctor knife coater, or comma knife coater can be used.

[0078] A method for crosslinking a foam coated in a sheet form on a synthetic paper substrate or the like is preferably a method for heating and drying the foam. The heating and drying method is not particularly limited as long as it is a method capable of drying and crosslinking a foam coated on a synthetic paper substrate or the like, and a known drying oven (for example, a hot air circulation type oven, a hot oil circulation hot air chamber, a far infrared heater chamber) can be used. The drying temperature can be, for example, 60°C or higher and 180°C or lower. In addition, it is preferable to perform multi-stage drying such that drying is performed from the inside at a low temperature in the early stage of drying and is sufficiently dried at a higher temperature in the later stage of drying, rather than performing drying at a constant temperature.

[0079] The properties (density, thickness, hardness, etc.) of the foamed sheet can be adjusted, for example, by changing the mixing ratio of air bubbles, the composition of the foamed sheet composition, the solids concentration, the drying and crosslinking conditions, etc.

[0080] The laminated sheet obtained through the above-mentioned steps S1 to S3 can be processed into an easy-to-use size by, for example, applying a separator film to the self-adhesive surface (i.e., the surface on the foamed sheet side), winding it up with a winder, and cutting it with a press cutter, slitter, or the like, without any particular limitation.

[0081] (Applications of laminated sheets) The synthetic paper base surface of the laminate sheet of the present invention can be printed using, for example, offset printing, seal printing, flexographic printing, silk screen printing, gravure printing, laser printers, thermal transfer printers, inkjet printers, and the like. Laminated sheets printed on the synthetic paper base surface can be advantageously used for outdoor purposes such as sales promotion cards, so-called POP cards (posters, stickers, displays, etc.), gardening POP (insertion labels, etc.), road signs (for funerals, home exhibitions, etc.), and signboards (for no entry, forest road work, etc.). EXAMPLES

[0082] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" expressing amounts are based on mass unless otherwise specified. In a polymer produced by polymerizing a plurality of types of monomers, the ratio of a monomer unit formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of the certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, the glass transition temperature and gel fraction of the polymer, the viscosity of the foam sheet composition, the density of the foam sheet, and the air release property (initial and after heating and pressing) and formaldehyde emission amount of the laminate sheet were evaluated by the following methods.

[0083] <Glass transition temperature of polymer> The glass transition temperature (Tg) of the polymer used as the material of the self-adhesive foam laminate sheet was measured by the following method. A polymer latex containing a polymer was applied to a polyethylene terephthalate film having a thickness of 50 μm with a 250 μm applicator, and dried at room temperature for 24 hours to obtain a film formed on the polyethylene terephthalate film. The glass transition temperature (°C) of the film formed on the polyethylene terephthalate film (other than the polyethylene terephthalate film) was measured as a sample according to JIS K 7121 using a differential scanning calorimeter (DSC7000X manufactured by Hitachi High-Tech Science Corporation) under the conditions of a measurement temperature of -50°C or more and 160°C or less, and a heating rate of 10°C / min. <Gel fraction of polymer> The gel fraction of the polymer used in the laminate sheet was measured by the following method. The polymer was applied to a 50 μm thick polyethylene terephthalate (PET) film with a 250 μm applicator and dried at room temperature for 24 hours to obtain a resin film. A predetermined amount (X) (about 500 mg) of this film was precisely weighed as a sample, and this was immersed in 100 ml of ethyl acetate at room temperature for 3 days, after which the insoluble matter was filtered through a 200 mesh wire net, air-dried at room temperature for 15 hours, then dried at 100 ° C for 2 hours, cooled at room temperature, and the weight (Y) of the sample was measured. The gel fraction was calculated by substituting X and Y into the following formula. Gel fraction (%) = (Y) / (X) x 100 <Viscosity of the composition for foam sheet> The viscosity of the composition for foamed sheet was measured at 23° C. using a Brookfield viscometer (manufactured by Rion Co., Ltd., "VISCOTESTER VT-06"). <Density of foam sheet> After preparing the laminated sheet, a test piece was prepared by cutting it to a size of 20 cm x 20 cm. The mass of the cut-out test piece: Xg was precisely weighed, and the mass of the substrate cut to 20 cm x 20 cm: Yg was precisely weighed. Thereafter, the thicknesses of the prepared laminated sheet and substrate were measured with a thickness gauge, and the thickness of the substrate was subtracted from the thickness of the laminated sheet to obtain the thickness of the foamed sheet: Tcm. At this time, the thickness value was calculated from the average value when six points were measured. The density of the foamed sheet was calculated by substituting the measured values ​​of X, Y, and T into the following formula. Density (g / cm 3 )=(XY) / (T×20×20) <Air release> <<Evaluation equipment>> The air release property was evaluated using an evaluation device 100 shown in Fig. 2. The evaluation device 100 shown in Fig. 2 is a device for evaluating the air release property of a laminated sheet 50 formed by laminating a foamed sheet 51 and a base material 52, and includes a sample fixing plate 10 having a through hole 11, and a gas pressure-feeding mechanism 40 that pressure-feeds air as a gas at a constant pressure from the other surface side (upper side in Fig. 2) of the sample fixing plate 10 to one surface side (lower side in Fig. 2) through the through hole 11. Here, the gas pressure-feeding mechanism 40 has a syringe 20 whose tip is connected to the through-hole 11 of the sample fixing plate 10 on the other surface side of the sample fixing plate 10, and a weight 30. The syringe 20 is connected to the sample fixing plate 10 with its tip facing vertically downward (downward in FIG. 2), and is equipped with a needle 21 inserted and fixed in the through-hole 11 of the sample fixing plate 10, a cylindrical outer tube 22 whose tip (the lower end in FIG. 2) is connected to the through-hole 11 via the needle 21, and a piston 23 inserted into the outer tube 22 from the rear end side of the outer tube 22. Weight 30 is attached onto a flange provided at the rear end of piston 23 (the upper end in FIG. 2). In addition, in the gas pressure-transfer mechanism 40 having the above-mentioned configuration, the piston 23 is pushed into the outer tube 22 by the weight of the piston 23 and the weight 30, and the air inside the outer tube 22 is pressure-transferred at a constant pressure to one surface side (foam sheet 51) of the sample fixing plate 10 through the needle 21 and the through hole 11. In the evaluation device 100 having the above-mentioned configuration, for example, after attaching the laminated sheet 50 to one surface (the side opposite to the needle 21 side) of the sample fixing plate 10 to which the needle 21 is fixed so as to cover the through-hole 11 (step (A)), the outer cylinder 22 in which the piston 23 to which the weight 30 is attached is inserted to a position where the distance from the tip is L is connected to the needle 21, and the time required for the piston 23 to move the distance L under the weight of the piston 23 and the weight 30 is measured (step (B)), thereby making it possible to evaluate the air release property of the laminated sheet 50. That is, since the air in the outer cylinder 22 is pushed out of the through-hole 11 with a constant pressure due to the weight of the piston 23 and the weight 30, if the distance L is constant and the amount of air pushed out from the outer cylinder 22 is constant, the laminated sheet 50 with lower air release property takes longer to move the distance L, and the laminated sheet 50 with higher air release property takes shorter to move the distance L. Therefore, the air release property of the laminated sheet 50 can be quantitatively evaluated based on the time required for the piston 23 to move the distance L. In addition, since the evaluation can be performed under conditions where the amount and pressure of the compressed air are constant, the air release property can be evaluated with high repeatability. Furthermore, since the evaluation can be performed in a state where the laminated sheet 50 is attached to the sample fixing plate 10, the air release property of the laminated sheet 50 in a state where it is attached to an adherend can be accurately evaluated. The sample fixing plate 10 was a 1 mm thick transparent polycarbonate plate (50 mm x 50 mm), the syringe 20 was a 2 mL glass syringe with a metal syringe needle with a diameter of 2 mm, and the weight 30 was a 30 g weight attached to the piston 23 with double-sided tape. <<Evaluation of air release (initial stage)>> After the laminate sheet was produced, it was cut to a size of 40 mm x 40 mm to be used as a sample to be evaluated. Then, the foamed sheet side of the prepared sample was attached to one surface (the side opposite to the needle 21 side) of the sample fixing plate 10 to which the needle 21 was fixed so as to cover the through hole 11 and prevent air from entering (step (A)), and then the outer cylinder 22, in which the piston 23 to which the weight 30 was attached was inserted to a position where the scale was 2 mL, was connected to the needle 21. Thereafter, the weight 30 and the piston 23 were released, and the time required for the piston 23 and the weight 30 to fall completely under their own weight (i.e., until 2 mL of air was pumped out) was measured (step (B)). This measurement operation was repeated three times, and the average value of the measured times was calculated and evaluated according to the following criteria. The smaller this average value, the better the air release property (initial stage) of the laminated sheet. A: The average measured time is 10 seconds or less B: The average measured time is more than 10 seconds and less than 20 seconds C: The average measured time is more than 20 seconds and less than 30 seconds D: The average measured time is more than 30 seconds. <<Evaluation of air release (after heating and pressurization)>> The laminated sheet was cut to a size of 80 mm x 120 mm, and then subjected to a 110 g / cm 2 A pressure of 10 ... <Formaldehyde emission amount> A self-adhesive foam sheet was prepared, and a separator film was attached to the surface of the foam layer (adsorption layer), and then a test piece was cut to a size of 200 mm x 200 mm. The test piece was placed in a 5 L Tedlar bag and sealed. 2 L of air was sealed in the bag, and the bag was left in a thermostatic chamber set at 23°C and 50% RH for 6 hours, after which the formaldehyde concentration in the bag was measured using a detector tube (Gastec Corporation, No. 91L). A formaldehyde concentration of 0.1 ppm or less was rated as "A," and a concentration of more than 0.1 ppm was rated as "B."

[0084] Example 1 <Preparation of Polymer> A monomer mixture consisting of 64 parts of ethyl acrylate, 12 parts of 2-ethylhexyl acrylate, 12 parts of n-butyl acrylate, 9 parts of acrylonitrile, 2 parts of styrene and 1 part of acrylic acid, and 0.4 parts of sodium polyoxyethylene alkyl sulfate (Kao Corporation: Latemul E-118B) were mixed and stirred with 27.0 parts of deionized water to obtain a monomer emulsion. Next, a glass reaction vessel equipped with a reflux condenser, a dropping funnel, a thermometer, a nitrogen inlet, and a stirrer was prepared separately from the above, and 43.0 parts of deionized water and 0.2 parts of sodium polyoxyethylene alkyl sulfate were placed in this glass reaction vessel, and the temperature was raised to 80°C while stirring. Then, while maintaining the temperature at 80°C, 0.3 parts of ammonium persulfate dissolved in 5.7 parts of deionized water was added, and then the monomer emulsion obtained above was gradually added over 4 hours. After the addition was completed, stirring was continued for another 4 hours, and then the reaction was terminated by cooling to obtain a reaction mixture. The polymerization conversion rate at this time was almost 100% (98% or more), and the obtained reaction mixture was adjusted to pH 5.0 with 5% ammonia water, and 2.5 parts of polyoxyethylene lauryl ether (Kao Corporation: Emulgen 120) was added, followed by concentration to obtain a polymer latex with a solid concentration of 55%. Then, the glass transition temperature and gel fraction of the polymer contained in the obtained polymer latex were measured. The results are shown in Table 1. <Preparation of foam sheet composition> In a mixing vessel, 100 parts of the polymer latex (i.e., 55 parts of the polymer contained in the polymer latex), 3 parts (5.5 parts per 100 parts of the polymer) of an epoxy-based crosslinking agent (Rikabond EX-8, fatty acid polyglycidyl ether, manufactured by Japan Coating Resins Co., Ltd.), 2 parts (3.6 parts per 100 parts of the polymer) of a wax agent (containing a fatty acid ester having a fatty acid moiety having a carbon number of 16 to 34) and 4 parts of a foam stabilizer [ammonium stearate (Nopco DC-100A, manufactured by San Nopco Co., Ltd.)] were added in this order. Finally, a thickener [sodium polyacrylate (Aron A-20L, manufactured by Toagosei Co., Ltd.)] was added to adjust the viscosity to 4250 mPa s, thereby obtaining a foam sheet composition. <Preparation of synthetic paper substrate> Propylene homopolymer (Novatec PP:MA4, Japan Polychem Corporation) 74%, high density polyethylene (Novatec HD:HJ360, Japan Polychem Corporation) 10%, and calcium carbonate (Softon 1800, Bihoku Funka Kogyo Co., Ltd.) 16% were melt-kneaded at 250°C, fed into a die set at 250°C, extruded into a sheet, and cooled with a cooling roll to obtain an unstretched sheet. The unstretched sheet obtained was heated to 135°C and stretched 4 times in the machine direction to obtain the base layer (b). Next, 52% propylene homopolymer (Novatec PP: EA8, manufactured by Japan Polychem Corporation), 3% high density polyethylene (Novatec HD: HJ360, manufactured by Japan Polychem Corporation), and 45% calcium carbonate (Softon 1800, manufactured by Bihoku Funka Kogyo Co., Ltd.) were melt-kneaded at 250°C in separate extruders, and then fed into a die set at 250°C and extruded into a sheet. The sheet was laminated on both sides of the above-mentioned base layer (b) as the surface layer (a) and back layer (c), and cooled to 60°C to obtain a three-layer laminate film (a / b / c). The resulting three-layer laminate film was heated again to 180°C and stretched 9 times in the transverse direction using a tenter, then annealed at 160°C, cooled to 60°C, and the edges were slit to obtain a synthetic paper substrate made of a multilayered resin stretched film. <Preparation of laminated sheet> The composition for a foamed sheet obtained as described above was stirred with a whisk until the foaming ratio reached 1.6 times, and the stirring speed was further reduced and stirring was continued for 5 minutes. The foamed foam sheet composition (foam) was coated on the above-mentioned synthetic paper substrate using a 0.3 mm applicator. This was placed in a drying oven and held at 80°C for 1.33 minutes, 120°C for 1.33 minutes, and 140°C for 1.33 minutes to perform drying and crosslinking, thereby obtaining a laminated sheet having a foamed sheet on a synthetic paper substrate. The thickness of the foamed sheet after drying was 0.133 mm. Various evaluations were performed using the obtained laminated sheet. The results are shown in Table 1.

[0085] Example 2 A foam sheet composition and a laminate sheet were prepared or produced in the same manner as in Example 1, except that the polymer prepared as follows was used. Evaluations were then performed in the same manner as in Example 1. The results are shown in Table 1. <Preparation of Polymer> A monomer mixture consisting of 56 parts of ethyl acrylate, 15 parts of 2-ethylhexyl acrylate, 18 parts of n-butyl acrylate, 8 parts of acrylonitrile, 2 parts of styrene, and 1 part of acrylic acid, and 0.4 parts of sodium polyoxyethylene alkyl sulfate (Latemul E-118B, manufactured by Kao Corporation) were mixed and stirred into 27.0 parts of deionized water to obtain a monomer emulsion. A polymer latex was obtained in the same manner as in Example 1 except for the above.

[0086] Comparative Example 1 <Preparation of Polymer> A monomer mixture consisting of 46.9 parts of ethyl acrylate, 45.8 parts of n-butyl acrylate, 5.9 parts of acrylonitrile, and 1.4 parts of N-methylol acrylamide, and 0.4 parts of sodium polyoxyethylene alkyl sulfate (Latemul E-118B, manufactured by Kao Corporation) were mixed and stirred into 27.0 parts of deionized water to obtain a monomer emulsion. A polymer latex was obtained in the same manner as in Example 1 except for the above. Evaluation was then performed in the same manner as in Example 1. The results are shown in Table 1. <Preparation of foam sheet composition> The polymer latex obtained as described above was used, and the amount of the crosslinking agent added was changed from 3 parts to 3.6 parts (i.e., 6.5 parts of crosslinking agent per 100 parts of polymer). No wax agent was added. A foam sheet composition was prepared in the same manner as in Example 1 except for the above. <Preparation of laminated sheet> The foaming ratio was changed from 1.6 to 2, and the foamed sheet composition obtained as described above was used. Except for this, a laminate sheet was produced in the same manner as in Example 1. Evaluation was then performed in the same manner as in Example 1. The results are shown in Table 1.

[0087] Comparative Example 2 <Preparation of Polymer> A monomer mixture consisting of 70 parts of n-butyl acrylate, 14 parts of methyl methacrylate, 14 parts of styrene, and 2 parts of itaconic acid, and 0.4 parts of sodium polyoxyethylene alkyl sulfate (Latemul E-118B, manufactured by Kao Corporation) were mixed and stirred into 27.0 parts of deionized water to obtain a monomer emulsion. A polymer latex was obtained in the same manner as in Example 1 except for the above. Evaluation was then performed in the same manner as in Example 1. The results are shown in Table 1. <Preparation of foam sheet composition> The polymer latex obtained as described above was used, and the amount of the crosslinking agent added was changed from 3 parts to 3.6 parts (i.e., 6.5 parts of crosslinking agent per 100 parts of polymer). No wax agent was added. A foam sheet composition was prepared in the same manner as in Example 1 except for the above. <Preparation of laminated sheet> Except for using the foamed sheet composition obtained as described above, a laminate sheet was produced in the same manner as in Example 1. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.

[0088] In addition, in Table 1 shown below, "EA" represents an ethyl acrylate unit; "MMA" indicates a methyl methacrylate unit, "2EHA" indicates a 2-ethylhexyl acrylate unit, "BA" indicates an n-butyl acrylate unit; "AA" represents an acrylic acid unit; "IA" represents an itaconic acid unit; "AN" indicates an acrylonitrile unit, "ST" indicates a styrene unit, "NMA" indicates an N-methylolacrylamide unit; "Tg" refers to the glass transition temperature.

[0089] [Table 1]

[0090] From Table 1, it is seen that in Examples 1 and 2, which used a foam sheet composition containing a polymer, a crosslinking agent, and a wax agent, a laminate sheet having excellent air release properties after heating and pressing could be formed. On the other hand, in Comparative Examples 1 and 2, in which a foamable sheet composition not containing a wax agent was used, it was found that a laminate sheet having excellent air release properties after heating and pressurization could not be formed. [Industrial Applicability]

[0091] According to the present invention, a self-adhesive foam laminate sheet having excellent air release properties after heating and pressurization can be provided. [Explanation of symbols]

[0092] S1 Composition preparation process S2 Foaming process S3 Sheeting process S10 Method for manufacturing laminated sheets 10 Sample fixing plate 11 Through hole 20 Syringe 21 needles 22 Outer cylinder 23 Piston 30 weights 40 Gas pumping mechanism 50 Laminated Sheet 51 Foam Sheet 52 Base material 100 Evaluation device

Claims

1. A self-adhesive foam laminate sheet comprising a synthetic paper substrate and a self-adhesive foam sheet, the self-adhesive foam sheet is formed using a composition for a self-adhesive foam sheet, the composition comprising a polymer, a crosslinking agent, and a wax agent; The proportion of alkenyl aromatic monomer units in the polymer is 0.5% by mass or more and 20% by mass or less, with the total amount of all repeating units contained in the polymer being 100% by mass, and The content of (meth)acrylate monomer units in the polymer is 60% by mass or more and 99% by mass or less, with the total amount of repeating units contained in the polymer being 100% by mass. Self-adhesive foam laminate sheet.

2. The self-adhesive foam laminate sheet according to claim 1 , wherein the polymer contains 0.1% by mass or more and 10% by mass or less of an unsaturated carboxylic acid monomer unit.

3. 3. The self-adhesive foam laminate sheet according to claim 1, wherein the polymer has no N-methylol groups.

4. The self-adhesive foam laminate sheet according to any one of claims 1 to 3, wherein the wax agent contains a fatty acid ester having a fatty acid moiety having 16 to 34 carbon atoms.

5. The self-adhesive foam laminate sheet according to claim 4, wherein the fatty acid ester has an alcohol moiety having 30 to 34 carbon atoms.

6. The self-adhesive foam laminate sheet according to claim 4 or 5, wherein the amount of the fatty acid ester contained in the composition for the self-adhesive foam sheet is 0.5 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the polymer.

Citation Information

Patent Citations

  • Molding laminate and preparation thereof

    JP1990022046A

  • Composition for acrylic foam

    JP1993311024A

  • Vinyl polymer emulsion composition for foam

    JP1994016954A

  • New high-quality wallpaper and method for producing the same

    JP2001248079A

  • Resin composition, self-adsorption foamed sheet and protective material

    JP2006176693A