Polarizing film and its manufacturing method
The polarizing film with a liquid crystal hardened layer and controlled dichroic dye content addresses wrinkles in patterned polarizing films, ensuring high visibility correction transmittance and improved appearance and performance.
Patent Information
- Application Number
- JP2020559954
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-11
- Filing Date
- 2019-12-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-12-04
AI Technical Summary
Patterned polarizing films with narrow regions of high visibility correction transmittance are prone to wrinkles during film formation, leading to poor appearance and polarization performance.
A polarizing film with a liquid crystal hardened layer containing a liquid crystal compound and dichroic dye, featuring distinct regions with varying visibility correction transmittance values, including a second region with a circular, elliptical, or polygonal shape, and a diameter or major axis of 2 cm or less, laminated on a base material layer with an alignment layer, and irradiated with a laser to control dichroic dye content.
The film achieves high visibility correction transmittance with improved appearance and polarization performance, reducing wrinkles and enhancing the film's optical properties.
Smart Images

Figure 0007575275000025 
Figure 0007575275000026 
Figure 0007575275000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film and a method for producing the same. [Background technology]
[0002] Organic EL display devices using organic light-emitting diodes (OLEDs) are not only lighter and thinner than liquid crystal display devices, but also have the advantage of being able to achieve high image quality with a wide viewing angle, fast response speed, and high contrast, and are therefore used in a variety of fields, including smartphones, televisions, and digital cameras. It is known that in organic EL display devices, the anti-reflection performance is improved by using circular polarizers, etc., in order to suppress the deterioration of visibility caused by the reflection of external light.
[0003] As a polarizing film used in such a circular polarizing plate, Patent Documents 1 and 2 describe a patterned polarizing film in which a patterned liquid crystal cured layer is laminated on a substrate. In recent years, the patterned polarizing film is required to have a region with high luminous efficacy corrected transmittance due to the design of smartphones, etc. However, if the region with high luminous efficacy corrected transmittance is wide in the patterned polarizing film, this may cause the polarization performance of the patterned polarizing film to deteriorate. Therefore, there is a demand for a patterned polarizing film with a narrow region with high luminous efficacy corrected transmittance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-206852 A [Patent Document 2] JP 2015-212823 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in a patterned polarizing film having a narrow region of high luminous efficiency corrected transmittance, wrinkles may occur in the film during pattern formation, resulting in a poor appearance of the resulting film.
[0006] An object of the present invention is to provide a polarizing film which has a narrow region of high luminosity-corrected transmittance and excellent appearance, and a method for producing the same. [Means for solving the problem]
[0007] The present invention provides a polarizing film and a method for producing the same, as described below. [1] A polarizing film having a liquid crystal cured layer, The liquid crystal cured layer contains a liquid crystal compound and has at least a first region and a second region having different luminosity-corrected transmittance values, The second region has a luminosity-corrected transmittance higher than that of the first region, and has a shape in a plan view that is circular, elliptical, oval, or polygonal. When the second region is circular, the diameter is 2 cm or less. When the second region is elliptical or oval, the major axis is 2 cm or less. When the second region is polygonal, the diameter of an imaginary circle inscribed in the polygon is 2 cm or less. Polarizing film. [2] Further comprising a substrate layer and an orientation layer laminated on at least one side of the substrate layer, A liquid crystal curing layer is laminated on the alignment layer. The polarizing film according to [1]. [3] The polarizing film according to [2], wherein the alignment layer contains a photoalignable polymer. [4] The polarizing film according to any one of [1] to [3], wherein the liquid crystal compound includes a polymerizable liquid crystal compound. [5] The polarizing film according to any one of [1] to [4], wherein the first region has a higher luminosity-corrected polarization degree value than the second region. [6] The polarizing film according to any one of [1] to [5], wherein the luminous efficacy-corrected polarization degree in the first region is 90% or more. [7] The polarizing film according to any one of [1] to [6], wherein the luminous efficacy-corrected polarization degree in the second region is 10% or less. [8] The polarizing film according to any one of [1] to [7], wherein the liquid crystal cured layer further contains a dichroic dye. [9] The polarizing film according to [8], wherein the first region has a higher content of dichroic dye than the second region.
[10] The polarizing film according to any one of [1] to [9], wherein the luminous efficiency-corrected single transmittance in the first region is 35% or more.
[11] The polarizing film according to any one of [1] to
[10] , wherein the luminous efficiency-corrected single transmittance in the second region is 80% or more.
[12] The polarizing film according to any one of [1] to
[11] , wherein the first region exhibits a Bragg peak in X-ray diffraction measurement.
[13] The polarizing film according to any one of [2] to
[12] , wherein the substrate layer has a quarter-wave plate function.
[14] The polarizing film according to any one of [1] to
[13] , wherein the length of the polarizing film is 10 m or more.
[15] A circularly polarizing plate obtained by laminating the polarizing film according to any one of [1] to
[12] and
[14] and a retardation layer having a function as a quarter-wave plate.
[16] A method for producing a polarizing film, comprising the step of irradiating a laminate film having a base layer and a cured liquid crystal layer containing a dichroic dye with a laser having a wavelength of 300 nm to 800 nm, wherein some regions of the cured liquid crystal layer have a lower content of dichroic dye than other regions.
[17] The method for producing a polarizing film according to
[16] , wherein the laminate film further has an alignment layer, and the alignment layer is laminated on the liquid crystal cured layer.
[18] The method for producing a polarized film described in
[16] or
[17] , wherein the region with reduced dichroic dye content has a circular, elliptical, oval or polygonal shape in a planar view, and when the region is circular, the diameter is 2 cm or less, when the region is elliptical or oval, the major axis is 2 cm or less, and when the region is polygonal, the diameter of an imaginary circle drawn to inscribe the polygon is 2 cm or less.
[19] The method for producing a polarizing film according to any one of
[16] to
[18] , wherein the liquid crystal cured layer contains a polymer of a polymerizable liquid crystal compound.
[20] The method for producing a polarizing film according to any one of
[16] to
[19] , wherein the polarizing film has a length of 10 m or more.
[21] A step (1) of irradiating a laminate film having a liquid crystal cured layer and a base layer with a laser having a wavelength of 300 nm to 800 nm; and a step (2) of laminating the polarizing film obtained in the step (1) on a retardation layer having a quarter-wave plate function. A method for manufacturing a circular polarizing plate.
[22] The method for producing a circularly polarizing plate according to
[21] , wherein the step (1) is carried out after the step (2). Effect of the Invention
[0008] The polarizing film of the present invention has a narrow region in which the luminous efficiency-corrected transmittance is high, and has an excellent appearance. Furthermore, according to the production method of the present invention, the polarizing film of the present invention can be obtained efficiently. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1A is a schematic plan view showing an example of a polarizing film of the present invention, and FIG. 1B is a cross-sectional view taken along the line XX of FIG. [Diagram 2] 2(a) to (c) are schematic cross-sectional views each showing an example of the circularly polarizing plate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The polarizing film of the present invention has a liquid crystal cured layer, the liquid crystal cured layer contains a liquid crystal compound, and has at least a first region and a second region having different luminosity-corrected transmittance values, the second region has a luminosity-corrected transmittance higher than that of the first region, and has a shape in a planar view that is circular, elliptical, oval or polygonal, the diameter of the second region being circular is 2 cm or less, the major axis of the second region being elliptical or oval is 2 cm or less, and the diameter of an imaginary circle inscribed in the polygon being polygonal is 2 cm or less.
[0011] Hereinafter, preferred embodiments of the polarizing film and the manufacturing method thereof of the present invention will be described with reference to the drawings. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.
[0012] <Polarizing film> FIG. 1(a) is a schematic plan view showing an example of the polarizing film of the present invention, and FIG. 1(b) is a cross-sectional view taken along line XX in FIG. 1(a).
[0013] The polarizing film 1 of this embodiment is a film having a function of light absorption anisotropy, and has a liquid crystal cured layer 11 containing a liquid crystal compound. The liquid crystal cured layer 11 has at least two regions distinguished by the value of luminous efficiency corrected transmittance (Ty), and these at least two regions usually have different contents of dichroic dyes.
[0014] The polarizing film 1 has a liquid crystal cured layer 11, and may further have a base layer 13, an alignment layer 12, and other layers.
[0015] 1(b) shows an example in which the alignment layer 12 and the cured liquid crystal layer 11 are provided on one side of the substrate layer 13, but the alignment layer and the cured liquid crystal layer may be provided on both sides of the substrate layer 13. The structures of the cured liquid crystal layers provided on both sides of the substrate layer 13 may be the same or different from each other.
[0016] The polarizing film 1 may be a long polarizing film having a length of 10 m or more. In this case, the polarizing film 1 may be wound into a roll. The polarizing film may be continuously unwound from the roll and may be laminated with a retardation layer, which will be described later, cut into sheets, or the like. The length of the long polarizing film to be wound into a roll is not particularly limited as long as it is 10 m or more, but may be, for example, 10,000 m or less.
[0017] (Liquid crystal hardening layer) The liquid crystal cured layer 11 contains a liquid crystal compound and has a region containing the liquid crystal compound and a dichroic dye. When the polarizing film 1 has polarization characteristics in the plane of the polarizing film 1, it is preferable that the layer has a region in which the dichroic dye and the liquid crystal compound are horizontally aligned with respect to the plane of the polarizing film 1. When the polarizing film 1 has polarization characteristics in the thickness direction of the polarizing film 1, it is preferable that the layer has a region in which the dichroic dye and the liquid crystal compound are horizontally aligned with respect to the plane of the polarizing film 1.
[0018] The liquid crystal cured layer 11 contains a liquid crystal compound, and usually further contains a dichroic dye.
[0019] In the liquid crystal cured layer 11, in the region where the dichroic dye and the liquid crystal compound are horizontally aligned with respect to the polarizing film 1 surface, the dichroic ratio (=A1(λ) / A2(λ)), which is the ratio of the absorbance A1(λ) in the horizontal direction of liquid crystal alignment to the absorbance A2(λ) in the vertical direction in the liquid crystal alignment plane for light with a wavelength of λ nm, is preferably 7 or more, more preferably 20 or more, and even more preferably 30 or more. The higher this value, the more excellent the polarization characteristics in absorption selectivity are. Depending on the type of dichroic dye, when the liquid crystal cured layer 11 is a nematic liquid crystal phase, the above ratio is about 5 to 10. When the liquid crystal cured layer 11 is a nematic liquid crystal phase or a smectic liquid crystal phase described later, it can be confirmed that the liquid crystal compound and the dichroic dye are not phase-separated, for example, by surface observation with various microscopes or scattering degree measurement with a haze meter.
[0020] As shown in FIGS. 1(a) and 1(b), the liquid crystal cured layer 11 has a first region 11a and a second region 11b that are distinguished by luminous-corrected transmittance.
[0021] The polarizing film 1 shown in FIG. 1(a) has two regions each having different luminous efficiency-corrected transmittances, but there may be two or more first regions and two or more second regions.
[0022] The first region 11a of the polarizing film 1 shown in Fig. 1(a) contains a liquid crystal compound and a dichroic dye. The second region 11b contains a liquid crystal compound, but may or may not contain a dichroic dye. When the first region 11a contains a dichroic dye, the content of the dichroic dye is preferably higher than the content of the dichroic dye in the second region 11b.
[0023] The content of the dichroic dye in the liquid crystal cured layer 11 is, for example, the maximum absorption wavelength (λ MAX ) can be determined by measuring the absorbance at
[0024] It is preferable that the first region 11a has a higher luminosity-corrected polarization degree value than the second region 11b.
[0025] The first region 11a is preferably a region having high polarization characteristics, and for example, the luminous efficacy corrected polarization degree (Py) can be 90% or more, preferably 92% or more, more preferably 95% or more, and is usually 100% or less. The first region 11a may have a luminous efficiency corrected transmittance (Ty) of, for example, 35% or more, preferably 40% or more, more preferably 42% or more, and is usually less than 50%.
[0026] The second region 11b is preferably a low polarization region having a luminous-corrected degree of polarization (Py) lower than the luminous-corrected degree of polarization (Py) of the first region 11a.
[0027] The luminous efficiency-corrected polarization degree (Py) in the second region 11b can be, for example, 10% or less, preferably 5% or less, more preferably 1% or less, and may be 0%.
[0028] The second region 11b has a luminosity-corrected transmittance higher than the luminosity-corrected transmittance of the first region 11a. The luminosity-corrected transmittance (Ty) of the second region 11b can be, for example, 80% or more, preferably 85% or more, more preferably 88% or more, and is usually 98% or less.
[0029] The luminosity-corrected transmittance (Ty) and luminosity-corrected polarization degree (Py) in this specification can be calculated based on the polarization degree and single transmittance measured using a spectrophotometer. For example, the transmittance (Ty) in the transmission axis direction (direction perpendicular to the orientation) in the visible light wavelength range of 380 nm to 780 nm is 1 ) and transmittance in the absorption axis direction (same orientation direction) (T 2 ) can be measured by the double beam method using a spectrophotometer equipped with a folder with a polarizer. The degree of polarization and single transmittance in the visible light range can be calculated by using the following formulas (Formula 1) and (Formula 2) to calculate the degree of polarization and single transmittance at each wavelength, and then performing luminosity correction using the 2-degree visual field (C light source) of JIS Z 8701 to calculate the luminosity-corrected degree of polarization (Py) and luminosity-corrected transmittance (Ty).
[0030] Degree of polarization [%] = {(T 1 -T 2 ) / (T 1 +T 2 )}×100 (Equation 1) Transmittance [%]=(T 1 +T 2 ) / 2 (Equation 2)
[0031] The occupied area of the first region 11a and the occupied area of the second region 11b may be appropriately selected depending on the properties required of the polarizing film 1. The ratio of the total occupied area of the first region 11a and the second region 11b to the surface area of the polarizing film 1 is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more.
[0032] The occupied area of the first region 11a is preferably 50% or more, more preferably 70% or more, and even more preferably 80% or more, of the total occupied area of the first region 11a and the second region 11b. For example, as shown in Fig. 1(a), the occupied area of the second region 11b may be smaller than the occupied area of the first region 11a, and the first region 11a may be provided so as to surround the second region 11b. In the polarizing film 1 shown in Fig. 1(a), the first region 11a is provided so as to surround one circular second region 11b, but a plurality of second regions 11b may be provided independently.
[0033] The shape of the first region 11a is not particularly limited, and the first region 11a may have a circular, elliptical, oval, polygonal, linear, band-like, wavy, or other shape in a plan view.
[0034] The second region 11b has a circular, elliptical, oval, or polygonal shape in plan view. When the second region 11b is circular, its diameter is 2 cm or less, preferably 1 cm or less, and more preferably 0.5 cm or less. When the second region 11b is circular, its diameter may be 0.05 cm or more, or may be 0.1 cm or more.
[0035] When the second region 11b is elliptical or oval, its major axis is 2 cm or less, preferably 1 cm or less, and more preferably 0.5 cm or less. When the second region 11b is elliptical or oval, its diameter may be 0.05 cm or more, or may be 0.1 cm or more.
[0036] When the second region 11b is a polygon, the diameter of an imaginary circle drawn to inscribe this polygon is 2 cm or less, preferably 1 cm or less, and more preferably 0.5 cm or less. When the second region 11b is a polygon, the diameter of the imaginary circle may be 0.05 cm or more, or may be 0.1 cm or more.
[0037] The second region 11b having the above-mentioned shape can be suitably used as a region corresponding to the lens position of a camera provided in a smartphone, tablet, etc. In this case, by making the second region 11b a region having a luminous-corrected single transmittance (Ty) of 80% or more and a luminous-corrected polarization degree (Py) of 10% or less, it is possible to reduce coloring of the second region 11b and obtain excellent transparency, thereby improving the performance of the camera.
[0038] A plurality of first regions 11a and a plurality of second regions 11b may be provided alternately.
[0039] When the polarizing film is a long polarizing film, the long polarizing film is usually cut to a predetermined size depending on the application of the polarizing film, and therefore, it is preferable to set the arrangement of the first region 11a and the second region 11b in the long polarizing film so that the first region 11a and the second region 11b are formed at predetermined positions in the polarizing film after cutting. For example, when the polarizing film after cutting is the polarizing film 1 shown in Fig. 1(a), it is preferable to provide a plurality of second regions 11b at predetermined intervals in the length direction and / or width direction of the long polarizing film.
[0040] The thickness of the first region 11a in the liquid crystal cured layer 11 is preferably 0.5 μm or more, more preferably 1 μm or more, and preferably 5 μm or less, and more preferably 3 μm or less. The thickness of the second region 11b in the liquid crystal cured layer 11 is preferably the same as that of the first region 11a, and is preferably 0.5 μm or more, more preferably 1 μm or more, and preferably 5 μm or less, and more preferably 3 μm or less. The thickness of the liquid crystal cured layer 11 can be measured with an interference thickness meter, a laser microscope, a stylus type thickness meter, or the like.
[0041] The thickness of the second region 11b may be smaller than that of the first region 11a, but the difference between the thickness of the first region 11a and the thickness of the second region 11b is preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less. By making the thicknesses of the first region 11a and the second region 11b of the liquid crystal cured layer 11 approximately the same and reducing the step between the first region 11a and the second region 11b, defects such as air bubbles being trapped and wrinkles occurring can be suppressed when a retardation layer or other layers (such as a surface protection layer) described later are laminated on the liquid crystal cured layer 11. In addition, defects such as the formation of rolling marks can also be suppressed when the polarizing film 1 having the liquid crystal cured layer 11 is wound into a roll.
[0042] (liquid crystal compound) A known liquid crystal compound can be used as the liquid crystal compound contained in the liquid crystal cured layer 11. The type of liquid crystal compound is not particularly limited, and a rod-shaped liquid crystal compound, a discotic liquid crystal compound, or a mixture thereof can be used. The liquid crystal compound may be a polymer liquid crystal compound, a polymerizable liquid crystal compound, or a mixture thereof.
[0043] As the liquid crystal compound, it is preferable to use a polymerizable liquid crystal compound. By using a polymerizable liquid crystal compound, the hue of the polarizing film can be arbitrarily controlled, and the polarizing film can be significantly thinned. In addition, since the polarizing film can be produced without performing a stretching process, it is possible to obtain a non-stretchable polarizing film that is not relaxed by stretching due to heat.
[0044] The polymerizable liquid crystal compound refers to a compound having a polymerizable group and liquid crystallinity. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group refers to a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, or an oxetanyl group is preferable, and an acryloyloxy group is more preferable. The liquid crystallinity may be a thermotropic liquid crystal or a lyotropic liquid crystal, but when mixed with a dichroic dye as in the liquid crystal cured layer of this embodiment, it is preferable to use a thermotropic liquid crystal.
[0045] When the polymerizable liquid crystal compound is a thermotropic liquid crystal, it may be a thermotropic liquid crystal compound exhibiting a nematic liquid crystal phase, or a thermotropic liquid crystal compound exhibiting a smectic liquid crystal phase. When the liquid crystal cured layer 11 exhibits a polarizing function as a polymer film obtained by a polymerization reaction, the liquid crystal state exhibited by the polymerizable liquid crystal compound is preferably a smectic phase, and more preferably a high-order smectic phase from the viewpoint of high performance. Among them, a high-order smectic liquid crystal compound forming a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase is more preferable, and a high-order smectic liquid crystal compound forming a smectic B phase, a smectic F phase, or a smectic I phase is even more preferable. When the liquid crystal cured layer 11 formed by the polymerizable liquid crystal compound is in these higher-order smectic phases, a region with higher polarization performance can be formed in the liquid crystal cured layer 11. In addition, such a region with high polarization performance is one in which a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase is obtained in X-ray diffraction measurement. In the polarizing film of the present invention, it is preferable that the first region shows a Bragg peak in X-ray diffraction measurement. The Bragg peak is a peak derived from a periodic structure of molecular orientation, and a film with a periodic interval of 3 to 6 Å can be obtained. In the polarizing film 1 of this embodiment, the liquid crystal cured layer 11 contains a polymer in which the polymerizable liquid crystal compound is polymerized in a smectic phase, so that, for example, the first region 11a can be given a higher polarization characteristic, which is preferable. In addition, the polymerizable liquid crystal compound may be a monomer, but may also be an oligomer or polymer in which a polymerizable group is polymerized.
[0046] Whether or not the polymerizable liquid crystal compound exhibits a nematic liquid crystal phase or a smectic liquid crystal phase can be confirmed, for example, as follows. After a coating film is formed by applying a composition for forming a polarizing film to a substrate, the coating film is heated under conditions in which the polymerizable liquid crystal compound does not polymerize, thereby removing the solvent contained in the coating film. Next, the coating film formed on the substrate is heated to an isotropic phase temperature, and gradually cooled to develop a liquid crystal phase, which is then inspected by texture observation using a polarizing microscope, X-ray diffraction measurement, or differential scanning calorimetry.
[0047] The polymerizable liquid crystal compound is not particularly limited as long as it is a liquid crystal compound having at least one (meth)acryloyl group, and any known polymerizable liquid crystal compound can be used, but a compound showing smectic liquid crystallinity is preferable. For example, such a polymerizable liquid crystal compound includes a compound represented by the following formula (A1) (hereinafter, sometimes referred to as "polymerizable liquid crystal compound (A1)").
[0048] U 1 -V 1 -W 1 -(X 1 -Y 1 -) n -X 2 -W 2 -V 2 -U 2 (A1) [In formula (A1), X 1 and X 2 represent, independently of each other, a divalent aromatic group or a divalent alicyclic hydrocarbon group, in which a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. 1 and X 2 At least one of these is a 1,4-phenylene group which may have a substituent or a cyclohexane-1,4-diyl group which may have a substituent.
[0049] Y 1 is a single bond or a divalent linking group.
[0050] n is 1 to 3. If n is 2 or more, multiple X 1 may be the same or different. X 2 is multiple X 1 When n is 2 or more, a plurality of Y 1 may be the same as or different from each other. From the viewpoint of liquid crystallinity, n is preferably 2 or more.
[0051] U 1 represents a hydrogen atom or a (meth)acryloyloxy group.
[0052] U 2 represents a (meth)acryloyloxy group.
[0053] W 1 and W 2 are each independently a single bond or a divalent linking group.
[0054] V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH 2 - may be replaced by -O-, -CO-, -S- or NH-.
[0055] In the polymerizable liquid crystal compound (A1), X 1 and X 2 are each independently preferably an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group; X 1 and X 2At least one of the groups is a 1,4-phenylene group which may have a substituent, or a cyclohexane-1,4-diyl group which may have a substituent, and is preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent, or the cyclohexane-1,4-diyl group which may have a substituent, include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted.
[0056] The polymerizable liquid crystal compound (A1) is a compound represented by the formula (A1-1): -(X 1 -Y 1 -) n -X 2 - (A1-1) [In the formula, X 1 , Y 1 , X 2 and n have the same meanings as above. It is preferable that the portion represented by the following formula (hereinafter referred to as partial structure (A1-1)) has an asymmetric structure, since this facilitates the development of smectic liquid crystal properties.
[0057] The polymerizable liquid crystal compound (A1) in which the partial structure (A1-1) is an asymmetric structure is, for example, a compound in which n is 1 and one X 1 and X 2 and Y are different from each other. 1 A compound in which two Xs are the same structure. 1 are identical in structure to each other, and one X 2 These two X 1 A polymerizable liquid crystal compound (A1) having a structure different from that of the two X 1 Of the W 1 X binds to 1 But the other X 1 and X 2 The structure is different from that of the other X 1 and X 2Also included are polymerizable liquid crystal compounds (A1) having the same structure as each other. 1 are the same structure as each other, and three X 1 and 1 X 2 The polymerizable liquid crystal compound (A1) includes any one of the following three structures different from all of the other three structures.
[0058] Y 1 -CH 2 CH 2 -, -CH 2 O-, -CH 2 CH 2 O-, -COO-, -OCOO-, single bond, -N=N-, -CR a =CR b -, -C≡C-, -CR a =N- or -CO-NR a - is preferred. a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 -CH 2 CH 2 More preferably, Y is -, -COO-, or a single bond. 1 If present, X 2 Y that binds to 1 -CH 2 CH 2 -or-CH 2 O- is more preferred. 1 and X 2 When all of Y are the same structure, two or more Y 1 It is preferable that there is a plurality of Y 1 When the compound has a structure of asymmetric structure, the compound tends to exhibit smectic liquid crystallinity.
[0059] U 2 is a (meth)acryloyloxy group. 1 is a hydrogen atom or a (meth)acryloyloxy group, and is preferably a (meth)acryloyloxy group. From the viewpoint of improving the adhesion between layers of the polarizing film and heat resistance, U 1and U 2 are preferably both (meth)acryloyloxy groups. The (meth)acryloyloxy group may be in a polymerized state or an unpolymerized state, but is preferably in an unpolymerized state.
[0060] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1 and V 2 is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.
[0061] Examples of the substituent that the alkanediyl group may have include a cyano group and a halogen atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted linear alkanediyl group.
[0062] W 1 and W 2 are each independently preferably a single bond, -O-, -S-, -COO- or -OCOO-, more preferably a single bond or -O-.
[0063] The polymerizable liquid crystal compound is not particularly limited as long as it is a polymerizable liquid crystal compound having at least one (meth)acryloyl group, and known polymerizable liquid crystal compounds can be used, but it is preferable that the polymerizable liquid crystal compound exhibits smectic liquid crystallinity, and the structure that is likely to exhibit smectic liquid crystallinity is preferably an asymmetric molecular structure in the molecular structure, and more preferably, the polymerizable liquid crystal compound has a structure represented by formula (Aa) to (Ai) and exhibits smectic liquid crystallinity. From the viewpoint of easily exhibiting high-order smectic liquid crystallinity, it is more preferable that the polymerizable liquid crystal compound has a structure represented by formula (Aa), formula (Ab) or formula (Ac). In formula (Aa) to formula (Ai), * represents a bond (single bond).
[0064] [ka]
[0065] Specific examples of the polymerizable liquid crystal compound include compounds represented by formulae (A-1) to (A-25). When the polymerizable liquid crystal compound has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.
[0066] [ka]
[0067] [ka]
[0068] [ka]
[0069] [ka]
[0070] [ka]
[0071] Among these, at least one selected from the group consisting of compounds represented by formula (A-2), formula (A-3), formula (A-4), formula (A-5), formula (A-6), formula (A-7), formula (A-8), formula (A-13), formula (A-14), formula (A-15), formula (A-16) and formula (A-17) is preferred. As the polymerizable liquid crystal compound, one type may be used alone, or two or more types may be used in combination.
[0072] The polymerizable liquid crystal compounds can be used in the liquid crystal cured layer 11 either alone or in combination. In addition, when two or more kinds of polymerizable liquid crystal compounds are combined, it is preferable that at least one of them is a polymerizable liquid crystal compound, and it is more preferable that two or more kinds are polymerizable liquid crystal compounds. By combining two or more kinds of polymerizable liquid crystal compounds, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature. When two kinds of polymerizable liquid crystal compounds are combined, the mixing ratio is usually 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50.
[0073] The polymerizable liquid crystal compound can be produced by a known method, for example, as described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) or Japanese Patent No. 4719156.
[0074] The content of the polymerizable liquid crystal compound in the liquid crystal cured layer 11 is usually 50 to 99.5 parts by mass, preferably 60 to 99 parts by mass, more preferably 70 to 98 parts by mass, and further preferably 80 to 97 parts by mass, based on 100 parts by mass of the solid content of the liquid crystal cured layer 11. If the content of the polymerizable liquid crystal compound is within the above range, the alignment tends to be high. Here, the solid content refers to the total amount of components excluding the solvent from the liquid crystal cured layer forming composition described later.
[0075] (dichroic dye) The dichroic dye is a dye that has different absorbance in the long axis direction of the molecule from absorbance in the short axis direction. The dichroic dye is a dye that exhibits dichroism when oriented together with a liquid crystal compound, and the dichroic dye itself may be polymerizable or may have liquid crystal properties. The dichroic dye preferably has a property of absorbing visible light, and has a maximum absorption wavelength (λ ) in the range of 380 to 680 nm. MAX ) is more preferred. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, among which azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, and are preferably bisazo dyes or trisazo dyes. The dichroic dyes may be used alone or in combination of two or more, but in order to obtain absorption over the entire visible light range, it is preferable to combine three or more dichroic dyes, and more preferably to combine three or more azo dyes.
[0076] Examples of the azo dye include a dye represented by the formula (I) T 1 -A 1 (-N=NA 2 ) p -N=NA 3 -T 2 (I) [In formula (I), A 1 , A 2 and A 3 each independently represents a 1,4-phenylene group which may have a substituent, a naphthalene-1,4-diyl group, or a divalent heterocyclic group which may have a substituent; T 1 and T 2 are each independently an electron-withdrawing group or an electron-releasing group, and are positioned at substantially 180° with respect to the azo bond plane. p represents an integer of 0 to 4. When p is 2 or more, each A 2may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO- or -N=CH- bond as long as the compound exhibits absorption in the visible region. (hereinafter, also referred to as "compound (I)").
[0077] A 1 , A 2 and A 3 Examples of the substituent that the 1,4-phenylene group, naphthalene-1,4-diyl group, and divalent heterocyclic group in the formula (I) may optionally have include an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, or a butyl group; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom, such as a chlorine atom or a fluorine atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, and a pyrrolidino group (the substituted amino group means an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is, for example, -NH 2 Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, and a hexyl group. Examples of the alkanediyl group having 2 to 8 carbon atoms include an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, and an octane-1,8-diyl group. In order to include compound (I) in a highly ordered liquid crystal structure such as a smectic liquid crystal, A 1 , A 2 and A 3 are each independently preferably unsubstituted, a 1,4-phenylene group in which hydrogen is substituted with a methyl group or a methoxy group, or a divalent heterocyclic group, and p is preferably 0 or 1. In particular, when p is 1 and A 1 , A 2 and A 3It is more preferable that at least two of the above three structures are 1,4-phenylene groups in terms of both ease of molecular synthesis and high performance.
[0078] Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, and benzoxazole. 2 When is a divalent heterocyclic group, a structure in which the molecular bond angle is substantially 180° is preferred, and specifically, a benzothiazole, benzimidazole, or benzoxazole structure in which two five-membered rings are condensed is more preferred.
[0079] T 1 and T 2 are each independently an electron-withdrawing group or an electron-releasing group, and preferably have different structures; T 1 is an electron withdrawing group and T 2 is an electron releasing group, or T 1 is an electron releasing group and T 2 More preferably, T is an electron withdrawing group. 1 and T 2 are preferably, independently, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, an amino group having one or two alkyl groups having 1 to 6 carbon atoms, an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms, or a trifluoromethyl group, and among these, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms is preferred, since a structure having a smaller excluded volume of the molecule is required for inclusion in a highly ordered liquid crystal structure such as a smectic liquid crystal.
[0080] Examples of the azo dye include the following compounds.
[0081] [ka]
[0082] [ka]
[0083] [In formulas (2-1) to (2-6), B 1 ~B 20 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the definitions of the substituted amino group and the unsubstituted amino group are as described above), a chlorine atom, or a trifluoromethyl group. 2 , B 6 , B 9 , B 14 , B 18 , B 19 is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom.
[0084] n1 to n4 each independently represent an integer of 0 to 3.
[0085] If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.
[0086] The anthraquinone dye is preferably a compound represented by formula (2-7).
[0087] [ka]
[0088] [In formula (2-7), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH 2 , -NHR x , -NR x 2 , -SR x or a halogen atom.
[0089] R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0090] The oxazine dye is preferably a compound represented by formula (2-8).
[0091] [ka]
[0092] [In formula (2-8), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH 2 , -NHR x , -NR x 2 , -SR x or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0093] The acridine dye is preferably a compound represented by formula (2-9).
[0094] [ka]
[0095] [In formula (2-9), R 16 ~R 23 are each independently a hydrogen atom, -R x, -NH 2 , -NHR x , -NR x 2 , -SR x or a halogen atom.
[0096] R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0097] R in formula (2-7), formula (2-8) and formula (2-9) x Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.
[0098] As the cyanine dye, the compounds represented by formula (2-10) and formula (2-11) are preferred.
[0099] [ka]
[0100] [In formula (2-10), D 1 and D. 2 each independently represents a group represented by any one of formulas (2-10a) to (2-10d). n5 represents an integer of 1 to 3.
[0101] [ka]
[0102] [ka]
[0103] [In formula (2-11), D 3 and D. 4each independently represents a group represented by any one of formulas (2-11a) to (2-11h). n6 represents an integer of 1 to 3.
[0104] [ka]
[0105] In order to obtain good light absorption properties, the content of the dichroic dye (the ratio of the total amount when multiple types are included) is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, and even more preferably 3 to 15 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound in a region having a polarizing property such as the first region 11a of the liquid crystal cured layer 11. If the content of the dichroic dye is lower than this range, the light absorption becomes insufficient and sufficient polarizing performance cannot be obtained, and if it is higher than this range, the alignment of the liquid crystal molecules may be hindered. The second region 11b of the liquid crystal cured layer 11 usually has a lower content of the dichroic dye than the first region 11a of the liquid crystal cured layer 11.
[0106] (base material layer) The polarizing film 1 may have a base layer 13. The base layer 13 can be used to support the alignment layer 12 and the cured liquid crystal layer 21 described later when producing the polarizing film 1, for example, as described later, and can also be used to support the cured liquid crystal layer 11 of the polarizing film 1.
[0107] The substrate layer 13 may be a glass substrate or a resin substrate, but is preferably a resin substrate. In order to continuously produce the polarizing film 1, it is more preferable that the substrate layer 13 is a long resin substrate that is wound in a roll and then unwound. The resin substrate is preferably a substrate having translucency that allows visible light to pass through. Here, translucency refers to a luminosity-corrected single transmittance of 80% or more for light in the wavelength range of 380 to 780 nm.
[0108] The thickness of the substrate layer 13 is preferably thin, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the substrate layer 13 is usually 5 μm to 300 μm, and preferably 20 μm to 200 μm. The substrate layer 13 may be provided in a peelable manner, and may be peelable from the polarizing film 1 after the liquid crystal cured layer 11 of the polarizing film 1 is bonded to a member constituting a display device or a retardation layer described later.
[0109] Examples of resins constituting the resin substrate include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene-based polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide and polyphenylene oxide; and the like.
[0110] Examples of commercially available cellulose ester resin substrates include "FUJITAC FILM" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto, Inc.).
[0111] Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona, Germany), "Arton" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by Zeon Corporation), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Such cyclic olefin resins can be formed into a film by known means such as a solvent casting method or a melt extrusion method to form a resin substrate. A resin substrate made of a commercially available cyclic olefin resin can also be used. Examples of commercially available resin substrates made of a cyclic olefin resin include "S-Cina" (registered trademark), "SCA40" (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), "ZEONOR Film" (registered trademark) (manufactured by Optes Co., Ltd.), and "Arton Film" (registered trademark) (manufactured by JSR Corporation).
[0112] The base layer 13 may have a single-layer structure or a multi-layer structure of two or more layers. When the base layer 13 has a multi-layer structure, the layers may be made of the same material or different materials.
[0113] The base layer 13 may have a quarter-wave plate function. By the base layer 13 having the quarter-wave plate function, a polarizing film having the function of a circular polarizing plate can be obtained by combining the base layer 13 with the liquid crystal cured layer 11. This makes it possible to obtain a circular polarizing plate without laminating a retardation layer having a quarter-wave plate function to the polarizing film 1 separately from the base layer 13. When the base layer 13 has a multi-layer structure, a circular polarizing plate can be obtained by using a member in which a layer having a half-wave plate function and a layer having a quarter-wave plate function are laminated, and laminating the liquid crystal cured layer 11 on the layer having the half-wave plate function. Alternatively, when the base layer 13 has a multi-layer structure, a circular polarizing plate can also be obtained by using a member in which a layer having a quarter-wave plate function with reverse wavelength dispersion and a layer having a positive C plate function are laminated.
[0114] (Alignment layer) The polarizing film 1 may have an alignment layer 12 on a substrate layer 13, and the alignment layer 12 is disposed between the substrate layer 13 and the liquid crystal cured layer 11. The alignment layer 12 can have an alignment regulating force that causes the liquid crystal compound in the liquid crystal cured layer 11 laminated thereon to be aligned in a desired direction.
[0115] The alignment layer 12 facilitates the alignment of the liquid crystal compound. The state of liquid crystal alignment, such as horizontal alignment, vertical alignment, hybrid alignment, and tilt alignment, varies depending on the properties of the alignment layer 12 and the liquid crystal compound, and the combination can be selected arbitrarily. For example, if the alignment layer 12 is a material that exhibits horizontal alignment as an alignment control force, the liquid crystal compound can form a horizontal alignment or a hybrid alignment. If the alignment layer 12 is a material that exhibits vertical alignment, the liquid crystal compound can form a vertical alignment or a tilt alignment. The expressions horizontal, vertical, and the like refer to the direction of the long axis of the aligned liquid crystal compound when the polarizing film 1 plane is used as a reference. For example, vertical alignment means that the long axis of the aligned polymerizable liquid crystal is in a direction perpendicular to the polarizing film 1 plane. The vertical here means 90°±20° to the polarizing film 1 plane. Since the polarizing film 1 preferably has the polarization characteristics of the polarizing film 1 plane, the alignment layer 12 is preferably formed using a material that exhibits horizontal alignment.
[0116] The alignment regulating force of the alignment layer 12 can be arbitrarily adjusted by the surface state or rubbing conditions when the alignment layer 12 is made of an alignment polymer, and can be arbitrarily adjusted by the polarized light irradiation conditions, etc. In addition, the liquid crystal alignment can be controlled by selecting the physical properties, such as the surface tension and liquid crystallinity, of the polymerizable liquid crystal compound.
[0117] The thickness of the alignment layer 12 is usually 10 nm to 5000 nm, preferably 10 nm to 1000 nm, and more preferably 30 nm to 300 nm. The alignment layer 12 formed between the substrate layer 13 and the cured liquid crystal layer 11 is preferably insoluble in a solvent used when forming the cured liquid crystal layer 11 on the alignment layer 12, and has heat resistance in a heat treatment for removing the solvent and for aligning the liquid crystal.
[0118] Examples of the alignment layer 12 include an alignment film made of an oriented polymer, a photo-alignment film, a groove alignment film, etc. When the base layer 13 is unwound from a roll of a long resin base material, the alignment layer 12 is preferably a photo-alignment film because the alignment direction can be easily controlled.
[0119] Examples of the oriented polymer include polyamide and gelatin having an amide bond in the molecule, polyimide having an imide bond in the molecule, and their hydrolyzates such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid ester. Among these, polyvinyl alcohol is preferred. These oriented polymers may be used alone or in combination of two or more.
[0120] The composition for forming the alignment layer in the alignment layer forming step includes the below-described alignment polymer composition, the composition for forming a photoalignment film, etc. The alignment layer forming step includes the following steps.
[0121] An alignment layer made of an alignment polymer can be obtained, for example, by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an "alignment polymer composition") to a substrate layer and removing the solvent, or by applying an alignment polymer composition to a substrate layer, removing the solvent, and rubbing the substrate (rubbing method).
[0122] Examples of the solvent used in the oriented polymer composition include water; alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, or propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, or ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, or methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, or heptane; aromatic hydrocarbon solvents such as toluene or xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran or dimethoxyethane; and chlorine-substituted hydrocarbon solvents such as chloroform or chlorobenzene. These solvents may be used alone or in combination of two or more.
[0123] The content of the orienting polymer in the orienting polymer composition may be within a range in which the orienting polymer can be completely dissolved in the solvent, and is preferably 0.1 to 20 mass % in terms of solid content relative to the solution, and more preferably 0.1 to 10 mass %.
[0124] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark) (manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark) (manufactured by JSR Corporation).
[0125] Examples of a method for applying the oriented polymer composition to the substrate layer include known methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography. When the polarizing film 1 is produced by a roll-to-roll continuous production method, the application method can usually be a printing method such as gravure coating, die coating, or flexography.
[0126] The solvent contained in the oriented polymer composition is removed to form a dry coating of the oriented polymer. Methods for removing the solvent include natural drying, ventilation drying, heat drying, and reduced pressure drying. The dried coating is then brought into contact with a rotating rubbing roll wrapped with a rubbing cloth to form the orientation layer 12.
[0127] The photo-alignment film can be obtained by irradiating a coating layer for an alignment layer formed by coating a substrate layer with a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter, sometimes referred to as a "photo-alignment film-forming composition") with polarized light (preferably polarized UV). The photo-alignment film is more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the polarized light to be irradiated.
[0128] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it is a group that generates a photoreaction that is the origin of liquid crystal alignment ability, such as molecular alignment induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, which occurs by irradiation with light. Among the photoreactive groups, those that cause a dimerization reaction or a photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group that can generate the above-mentioned reaction, those having an unsaturated bond, particularly a double bond, are preferred, and groups having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) are more preferred.
[0129] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. From the viewpoint of easy control of reactivity and expression of alignment control force during photoalignment, chalcone groups and cinnamoyl groups are preferred. Examples of photoreactive groups having a C=N bond include groups having a structure such as aromatic Schiff bases or aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having azoxybenzene as a basic structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have a substituent such as an alkyl group, an alkoxy group, an aryl group, an allyloxy group, a cyano group, an alkoxycarbonyl group, a hydroxyl group, a sulfonic acid group, or a halogenated alkyl group.
[0130] The solvent for the composition for forming a photo-alignment film is preferably one that dissolves the polymer and monomer having a photoreactive group, and examples of the solvent include the solvents exemplified above as the solvent for the alignment polymer composition.
[0131] The content of the polymer or monomer having a photoreactive group in the composition for forming a photoalignment film can be appropriately adjusted depending on the type of the polymer or monomer having a photoreactive group and the thickness of the photoalignment film to be produced, but is preferably 0.2 mass% or more, and particularly preferably in the range of 0.3 to 10 mass%. Polymer materials such as polyvinyl alcohol and polyimide and photosensitizers may be included within a range that does not significantly impair the properties of the photoalignment film.
[0132] The method for coating the composition for forming a photo-alignment film on the substrate layer can be the same as the method for coating the above-mentioned oriented polymer composition on the substrate layer 13. The method for removing the solvent from the coated composition for forming a photo-alignment film can be the same as the method for removing the solvent from the oriented polymer composition.
[0133] Polarized light irradiation may be performed directly from the dried film, or from the substrate layer side so that the polarized light transmitted through the substrate layer is irradiated onto the dried film. It is particularly preferable that the polarized light used for polarized light irradiation is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, or metal halide lamps are more preferable. These lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. Polarized light can be irradiated by irradiating light from a light source through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as Glan-Thompson or Glan-Taylor, or a wire grid type polarizer can be used.
[0134] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.
[0135] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When liquid crystal molecules are placed on a film that has multiple equally spaced linear grooves, the liquid crystal molecules are oriented in the direction along the grooves.
[0136] Methods for obtaining a groove alignment film include a method of forming a concave-convex pattern by exposing a photosensitive polyimide film surface through an exposure mask having slits in a pattern shape, followed by development and rinsing, a method of forming a layer of UV-curable resin before curing on a plate-shaped master having grooves on the surface, transferring the resin layer to a substrate and curing it, a method of pressing a roll-shaped master having a plurality of grooves against a film of UV-curable resin before curing formed on a substrate to form concave-convex patterns, and then curing the film, etc. Specific examples of the method include the methods described in JP-A-6-34976 and JP-A-2011-242743.
[0137] In order to obtain an alignment with little alignment disturbance, the width of the convex portions of the groove alignment film is preferably 0.05 μm to 5 μm, the width of the concave portions is preferably 0.1 μm to 5 μm, and the depth of the unevenness is preferably 2 μm or less, more preferably 0.01 μm to 1 μm or less.
[0138] (Other layers) The polarizing film 1 may have layers other than the substrate layer 13 and the alignment layer 12. For example, a protective film for protecting the surface of the liquid crystal cured layer 11 may be provided on the surface of the liquid crystal cured layer 11 opposite to the substrate layer 13. When the substrate layer 13 is peeled off for use, a protective film may be provided on the surface of the liquid crystal cured layer 11 from which the substrate layer 13 has been peeled off. The protective film may have a single layer structure or a multilayer structure. When the protective film has a multilayer structure, the layers may be formed of the same material or different materials.
[0139] The polarizing film of the present invention can be produced by preparing a liquid crystal cured layer and further providing a second region. The method of preparing the liquid crystal cured layer and the method of providing the second region are not particularly limited, but it is preferable to produce the polarizing film by the method described later in the production method.
[0140] <Circular polarizing plate> 2(a) to 2(c) are schematic cross-sectional views showing an example of the circular polarizer of the present invention. The polarizing film 1 shown in FIG. 1(b) can be made into the circular polarizers 5a and 5b shown in FIG. 2(a) and 2(b) by laminating a retardation layer 15 having a ¼ wavelength plate function. The retardation layer 15 may be laminated on the liquid crystal cured layer 11 side of the polarizing film 1 (FIG. 2(a)), or on the substrate layer 13 side (FIG. 2(b)). The substrate layer 13 may be peeled off from the circular polarizer 5a shown in FIG. 2(a) to be used as the circular polarizer 5c (FIG. 2(c)). In this case, the alignment layer 12 may be peeled off together with the substrate layer 13.
[0141] The circular polarizing plate may be a laminate of the polarizing film 1 and a retardation layer having a multi-layer structure. In this case, a multilayer retardation layer can be used in which a layer having a 1 / 2 wavelength plate function and a layer having a 1 / 4 wavelength plate function are laminated, and a circular polarizing plate can be obtained by laminating the layer having the 1 / 2 wavelength plate function of the multilayer retardation layer with the polarizing film 1. Alternatively, a circular polarizing plate can also be obtained by using a multilayer retardation layer in which a layer having a 1 / 4 wavelength plate function with reverse wavelength dispersion and a layer having a positive C plate function are laminated.
[0142] A material having a function as a retardation layer may be used as the base layer 13 of the polarizing film 1, and a retardation layer may be further laminated thereon to form a circular polarizing plate. In this case, the functions of the base layer 13 and the retardation layer as a retardation layer may be selected according to the lamination positions of the base layer 13 and the retardation layer in the circular polarizing plate.
[0143] The polarizing film and the retardation layer can be laminated via an adhesive layer using a known pressure-sensitive adhesive or adhesive.
[0144] <Method of manufacturing polarizing film>
[0145] The method for producing a polarizing film of the present invention includes a step of irradiating a laminated film having a cured liquid crystal layer and a base material layer with a laser having a wavelength of 300 nm to 800 nm, and is a method for producing a polarizing film in which a part of the cured liquid crystal layer has a lower content of dichroic dye than other parts of the cured liquid crystal layer.
[0146] The laminated film having a cured liquid crystal layer and a substrate is not particularly limited as long as it has a cured liquid crystal layer on at least one side of the substrate layer. The substrate may be a protective film, which will be described later. In the laminated film, the protective film may be laminated not only as the substrate but also on the opposite side of the liquid crystal cured layer to the substrate.
[0147] When the laminated film further has an orientation layer, it is preferable that the orientation layer and the liquid crystal cured layer are laminated in this order on the base layer. The laminated film further having an orientation layer can be produced through a step of forming an orientation layer by applying an orientation layer-forming composition to one side of the base layer, and a step of forming a liquid crystal cured layer by applying a liquid crystal cured layer-forming composition to the side on which the orientation layer is formed.
[0148] In the alignment layer forming step, the substrate layer 13 may be subjected to a surface treatment before applying the alignment layer forming composition. Examples of the surface treatment method include corona treatment, plasma treatment, laser treatment, ozone treatment, saponification treatment, flame treatment, application of a coupling agent, and primer treatment. As the alignment layer forming composition, the above-mentioned alignable polymer composition, photoalignment film forming composition, and composition containing a resin material for forming a groove alignment film can be used. The method of forming an alignment layer using each composition is also as described above. For example, when the composition for forming an alignment layer contains a photoalignable polymer, the alignment layer formation process can form an alignment layer having an alignment control force in a predetermined direction by irradiating a coating layer for an alignment layer formed by applying the composition for forming an alignment layer with polarized light.
[0149] The liquid crystal cured layer forming composition is a composition containing a liquid crystal compound and a dichroic dye, and preferably contains a solvent and a polymerization initiator, and may contain a sensitizer, a polymerization inhibitor, a leveling agent, a reactive additive, etc. As the liquid crystal compound and the dichroic dye, those described above can be used. As the solvent, polymerization initiator, sensitizer, polymerization inhibitor, leveling agent, and reactive additive, those described below can be used.
[0150] Examples of the method for coating the liquid crystal cured layer-forming composition include extrusion coating, direct gravure coating, reverse gravure coating, CAP coating, slit coating, microgravure, die coating, and inkjet coating. Also included are methods of coating using a coater such as a dip coater, bar coater, or spin coater. Among these, when continuously coating in a roll to roll format, the microgravure, inkjet, slit coating, and die coating methods are preferred, and when coating a sheet-like substrate such as glass, the highly uniform spin coating method is preferred. When coating in a roll to roll format, the substrate layer is coated with a composition for forming an alignment film to form an alignment layer, and the liquid crystal cured layer-forming composition can be continuously coated on the resulting alignment layer.
[0151] When forming a liquid crystal cured layer by coating the liquid crystal cured layer forming composition, the solvent is removed from the coated liquid crystal cured layer forming composition to form a liquid crystal cured layer coating layer. The method for removing the solvent can be the same as the method for removing the solvent from the orientable polymer composition, and examples of the method include natural drying, ventilation drying, heat drying, reduced pressure drying, and combinations of these. Of these, natural drying or heat drying is preferred. The drying temperature is preferably in the range of 0 to 200°C, more preferably in the range of 20 to 150°C, and even more preferably in the range of 50 to 130°C. The drying time is preferably 10 seconds to 10 minutes, more preferably 30 seconds to 5 minutes.
[0152] When the liquid crystal compound contained in the liquid crystal cured layer forming composition is a polymerizable liquid crystal compound, it is preferable to irradiate the liquid crystal cured layer coating layer formed in the liquid crystal cured layer forming step with active energy rays to photopolymerize the polymerizable liquid crystal compound and form a liquid crystal cured layer as a polymer layer of the polymerizable liquid crystal compound. The active energy to be irradiated is appropriately selected according to the type of polymerizable liquid crystal compound contained in the liquid crystal cured layer coating layer (particularly, the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator when a photopolymerization initiator is contained, and the amount thereof. Specifically, one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be mentioned. Among them, ultraviolet light is preferred in terms of ease of controlling the progress of the polymerization reaction and the fact that photopolymerization devices widely used in this field can be used, and it is preferable to select the type of polymerizable liquid crystal compound so that it can be photopolymerized by ultraviolet light.
[0153] Examples of light sources for active energy rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.
[0154] The irradiation intensity of active energy rays is usually 10 mW / cm 2 ~3000mW / cm 2 The irradiation intensity of the active energy rays is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a radical polymerization initiator. The time for irradiating the active energy rays is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. When irradiating once or multiple times with such an irradiation intensity of the active energy rays, the integrated light amount is 10 mJ / cm 2 ~3000mJ / cm 2 , preferably 50 mJ / cm 2 ~2,000mJ / cm 2, more preferably 100 mJ / cm 2 ~1000mJ / cm 2 If the accumulated light amount is less than this range, the polymerizable liquid crystal compound may not be cured sufficiently, and good transferability may not be obtained. Conversely, if the accumulated light amount is more than this range, the liquid crystal cured layer may be colored.
[0155] (solvent) The liquid crystal cured layer forming composition may contain a solvent. In general, polymerizable liquid crystal compounds have high viscosity, so when a polymerizable liquid crystal compound is used as the liquid crystal compound, the liquid crystal cured layer forming composition containing a solvent is used to facilitate coating, and as a result, the liquid crystal cured layer is easily formed. As the solvent, one that can completely dissolve the polymerizable liquid crystal compound and the dichroic dye is preferable. The solvent is preferably inactive to the polymerization reaction of the polymerizable liquid crystal compound.
[0156] Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These solvents may be used alone or in combination of two or more.
[0157] The content of the solvent contained in the composition for forming a liquid crystal cured layer is preferably 50 to 98% by mass based on the total amount of the composition for forming a liquid crystal cured layer. In other words, the content of the solid content in the composition for forming a liquid crystal cured layer is preferably 2 to 50% by mass. When the content of the solid content is 50% by mass or less, the viscosity of the composition for forming a liquid crystal cured layer is low, so that the thickness of the liquid crystal cured layer 21 becomes approximately uniform, and unevenness tends to be less likely to occur in the liquid crystal cured layer 21. The content of the solid content can be determined in consideration of the thickness of the liquid crystal cured layer 21 to be manufactured.
[0158] (Polymerization initiator) The liquid crystal cured layer forming composition may contain a polymerization initiator. The polymerization initiator can be used when a polymerizable liquid crystal compound is used as the liquid crystal compound, and is a compound that can initiate a polymerization reaction of the polymerizable liquid crystal compound, etc. As the polymerization initiator, a photopolymerization initiator that generates active radicals by the action of light is preferable from the viewpoint of not depending on the phase state of the thermotropic liquid crystal.
[0159] Examples of the polymerization initiator include a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, or a sulfonium salt.
[0160] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0161] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0162] Examples of the alkylphenone compound include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0163] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0164] Examples of triazine compounds include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl] 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine.
[0165] As the polymerization initiator, a commercially available product can also be used. Examples of commercially available polymerization initiators include Irgacure (registered trademark) 907, 184, 651, 819, 250, 369, 379, 127, 754, OXE01, OXE02, or OXE03 (manufactured by Chiba Specialty Chemicals Co., Ltd.); Seikuol (registered trademark) BZ, Z, or BEE (manufactured by Seiko Chemical Co., Ltd.); Kayacure (registered trademark) BP100 or UVI-6992 (manufactured by Dow Chemical Co., Ltd.); Adeka Optomer SP-152, N-1717, N-1919, SP-170, Adeka Arcles NCI-831, Adeka Arcles NCI-930 (manufactured by ADEKA Corporation); TAZ-A or TAZ-PP (manufactured by Nippon SiberHegner Co., Ltd.); and TAZ-104 (manufactured by Sanwa Chemical Co., Ltd.). The polymerization initiator in the liquid crystal cured layer forming composition may be one type, or two or more types of polymerization initiators may be mixed and used in accordance with the light source.
[0166] The content of the polymerization initiator in the liquid crystal cured layer forming composition can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, but is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is within the above range, polymerization can be performed without disturbing the alignment of the polymerizable liquid crystal compound.
[0167] (sensitizer) The liquid crystal cured layer forming composition may contain a sensitizer. The sensitizer can be suitably used when a polymerizable liquid crystal compound is used as the liquid crystal compound. When a polymerizable liquid crystal compound having a photopolymerizable group is used, the sensitizer is preferably a photosensitizer. Examples of the sensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and an alkoxy group-containing anthracene (dibutoxyanthracene, etc.); phenothiazine or rubrene, etc.
[0168] When the liquid crystal cured layer forming composition contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the liquid crystal cured layer forming composition can be further promoted. The amount of the sensitizer used is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound.
[0169] (Polymerization inhibitor) The liquid crystal cured layer forming composition may contain a polymerization inhibitor from the viewpoint of stably proceeding with the polymerization reaction. The polymerization inhibitor can be suitably used when a polymerizable liquid crystal compound is used as the liquid crystal compound, and the polymerization inhibitor can control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.
[0170] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenol compounds; β-naphthylamine compounds, and β-naphthol compounds.
[0171] When the liquid crystal cured layer forming composition contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and further preferably 0.5 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization inhibitor is within the above range, polymerization can be performed without disturbing the alignment of the polymerizable liquid crystal compound.
[0172] (Leveling agent) The liquid crystal cured layer forming composition may contain a leveling agent. The leveling agent is an additive having a function of adjusting the fluidity of the composition and making the film obtained by applying the composition flatter, and examples of the leveling agent include organic modified silicone oil-based, polyacrylate-based, and perfluoroalkyl-based leveling agents. Specifically, DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, FZ2123 (all manufactured by Dow Corning Toray Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, TSF4460 (all manufactured by Momentive Performance Materials Co., Ltd.) Japan LLC), Fluorinert (registered trademark) FC-72, FC-40, FC-43, FC-3283 (all manufactured by Sumitomo 3M Limited), Megafac (registered trademark) R-08, R-30, R-90, F-410, F-411, F-443, F-445, F-470, F-477, F-479, F-482, F-483 (all manufactured by DIC Corporation), F-top (trade name) EF301, EF303, EF351, EF352 (all manufactured by Mitsubishi Materials Electronics Co., Ltd.), Surflon (registered trademark) S-381, S-382, S-383, S-393, SC-101, SC-105, KH-40, SA-100 (all manufactured by AGC Seimi Chemical Co., Ltd.), trade names E1830, E5844 (manufactured by Daikin Fine Chemical Research Institute Co., Ltd.), BM-1000, BM-1100, BYK-352, BYK-353 or BYK-361N (all trade names: manufactured by BM Chemie Co., Ltd.), etc. Among them, polyacrylate-based leveling agents or perfluoroalkyl-based leveling agents are preferred.
[0173] When the composition for forming a liquid crystal cured layer contains a leveling agent, the amount is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the liquid crystal compound. When the amount of the leveling agent is within the above range, the liquid crystal compound is easily aligned horizontally, and the obtained liquid crystal cured layer tends to be smoother. When the amount of the leveling agent relative to the liquid crystal compound exceeds the above range, the obtained liquid crystal cured layer tends to be easily uneven. The composition for forming a liquid crystal cured layer may contain two or more types of leveling agents.
[0174] (Reactive Additives) The liquid crystal cured layer forming composition may contain a reactive additive. The reactive additive preferably has a carbon-carbon unsaturated bond and an active hydrogen reactive group in its molecule. The "active hydrogen reactive group" referred to here is a carboxyl group (-COOH), a hydroxyl group (-OH), an amino group (-NH 2 Representative examples of the reactive additive include a glycidyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, an isocyanate group, a thioisocyanate group, a maleic anhydride group, etc. The number of carbon-carbon unsaturated bonds or active hydrogen reactive groups contained in the reactive additive is usually 1 to 20, and preferably 1 to 10, respectively.
[0175] In the reactive additive, it is preferable that at least two active hydrogen reactive groups are present, and in this case, the multiple active hydrogen reactive groups present may be the same or different.
[0176] The carbon-carbon unsaturated bond of the reactive additive may be a carbon-carbon double bond, a carbon-carbon triple bond, or a combination thereof, but is preferably a carbon-carbon double bond. Among them, the reactive additive preferably contains a carbon-carbon unsaturated bond as a vinyl group and / or a (meth)acrylic group. Furthermore, the reactive additive is preferably one in which the active hydrogen reactive group is at least one selected from the group consisting of an epoxy group, a glycidyl group, and an isocyanate group, and more preferably a reactive additive having an acrylic group and an isocyanate group.
[0177] Specific examples of reactive additives include compounds having a (meth)acrylic group and an epoxy group, such as methacryloxyglycidyl ether and acryloxyglycidyl ether; compounds having a (meth)acrylic group and an oxetane group, such as oxetane acrylate and oxetane methacrylate; compounds having a (meth)acrylic group and a lactone group, such as lactone acrylate and lactone methacrylate; compounds having a vinyl group and an oxazoline group, such as vinyl oxazoline and isopropenyl oxazoline; oligomers of compounds having a (meth)acrylic group and an isocyanate group, such as isocyanatomethyl acrylate, isocyanatomethyl methacrylate, 2-isocyanatoethyl acrylate, or 2-isocyanatoethyl methacrylate. In addition, compounds having a vinyl group or a vinylene group and an acid anhydride, such as methacrylic anhydride, acrylic anhydride, maleic anhydride, or vinyl maleic anhydride, can be mentioned. Among these, methacryloxyglycidyl ether, acryloxyglycidyl ether, isocyanatomethyl acrylate, isocyanatomethyl methacrylate, vinyloxazoline, 2-isocyanatoethyl acrylate, 2-isocyanatoethyl methacrylate, or oligomers thereof are preferred, and isocyanatomethyl acrylate, 2-isocyanatoethyl acrylate, or oligomers thereof are particularly preferred.
[0178] Specifically, a compound represented by the following formula (Y) is preferred.
[0179] [ka]
[0180] [In formula (Y), n represents an integer of 1 to 10, and R 1’ represents a divalent aliphatic or alicyclic hydrocarbon group having 2 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 5 to 20 carbon atoms. Two R in each repeat unit 2’ is -NH- on one side and >NC(=O)-R on the other side. 3’ R 3’ represents a hydroxyl group or a group having a carbon-carbon unsaturated bond.
[0181] R in formula (Y) 3’ At least one R 3’ is a group having a carbon-carbon unsaturated bond.
[0182] Among the reactive additives represented by the formula (Y), a compound represented by the formula (YY) (hereinafter, sometimes referred to as compound (YY)) is particularly preferred (n has the same meaning as above).
[0183] [ka]
[0184] Compound (YY) may be a commercially available product, either as is or after purification as necessary. Examples of commercially available products include Laromer (registered trademark) LR-9000 (manufactured by BASF).
[0185] When the liquid crystal cured layer forming composition contains a reactive additive, the content of the reactive additive is usually 0.01 to 10 parts by mass, and preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the liquid crystal compound.
[0186] The laminate film in the present invention may have, for example, a protective film laminated on the liquid crystal cured layer obtained by the above-mentioned method.
[0187] (Protective film) The protective film can be a film made of a light-transmitting (preferably optically transparent) thermoplastic resin, for example, a polyolefin resin such as a chain polyolefin resin (polypropylene resin, etc.) or a cyclic polyolefin resin (norbornene resin, etc.); a cellulose resin such as triacetyl cellulose or diacetyl cellulose; a polyester resin such as polyethylene terephthalate or polybutylene terephthalate; a polycarbonate resin; a (meth)acrylic resin such as a methyl methacrylate resin; a polystyrene resin; a polyvinyl chloride resin; an acrylonitrile-butadiene-styrene resin; an acrylonitrile-styrene resin; a polyvinyl acetate resin; a polyvinylidene chloride resin; a polyamide resin; a polyacetal resin; a modified polyphenylene ether resin; a polysulfone resin; a polyethersulfone resin; a polyarylate resin; a polyamideimide resin; a polyimide resin, etc.
[0188] Examples of linear polyolefin resins include linear olefin homopolymers such as polyethylene resins (polyethylene resins which are homopolymers of ethylene, and copolymers mainly composed of ethylene) and polypropylene resins (polypropylene resins which are homopolymers of propylene, and copolymers mainly composed of propylene), as well as copolymers composed of two or more types of linear olefins.
[0189] Cyclic polyolefin resin is a general term for resins polymerized with cyclic olefin as a polymerization unit, and examples thereof include resins described in JP-A-1-240517, JP-A-3-14882, JP-A-3-122137, etc. Specific examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (typically random copolymers) of cyclic olefins and chain olefins such as ethylene and propylene, and graft polymers modified with unsaturated carboxylic acids or derivatives thereof, as well as hydrogenated products thereof. Among these, norbornene resins using norbornene monomers such as norbornene or polycyclic norbornene monomers as cyclic olefins are preferably used.
[0190] The polyester resin is a resin having an ester bond, excluding the cellulose ester resin described below, and is generally made of a polycondensate of a polyvalent carboxylic acid or its derivative and a polyhydric alcohol. As the polyvalent carboxylic acid or its derivative, a divalent dicarboxylic acid or its derivative can be used, for example, terephthalic acid, isophthalic acid, dimethyl terephthalate, and dimethyl naphthalenedicarboxylate. As the polyhydric alcohol, a divalent diol can be used, for example, ethylene glycol, propanediol, butanediol, neopentyl glycol, and cyclohexanedimethanol. A representative example of the polyester resin is polyethylene terephthalate, which is a polycondensate of terephthalic acid and ethylene glycol.
[0191] The (meth)acrylic resin is a resin whose main constituent monomer is a compound having a (meth)acryloyl group. Specific examples of the (meth)acrylic resin include poly(meth)acrylic acid ester such as polymethyl methacrylate; methyl methacrylate-(meth)acrylic acid copolymer; methyl methacrylate-(meth)acrylic acid ester copolymer; methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymer; methyl (meth)acrylate-styrene copolymer (MS resin, etc.); copolymers of methyl methacrylate and a compound having an alicyclic hydrocarbon group (e.g., methyl methacrylate-cyclohexyl methacrylate copolymer, methyl methacrylate-norbornyl (meth)acrylate copolymer, etc.). Preferably, poly(meth)acrylic acid C such as polymethyl (meth)acrylate is used. 1-6 A polymer containing an alkyl ester as a main component is used, and more preferably, a methyl methacrylate-based resin containing methyl methacrylate as a main component (50 to 100% by weight, preferably 70 to 100% by weight) is used.
[0192] The cellulose ester resin is an ester of cellulose and a fatty acid. Specific examples of the cellulose ester resin include cellulose triacetate, cellulose diacetate, cellulose tripropionate, and cellulose dipropionate. In addition, copolymers thereof and those in which a part of the hydroxyl group is modified with another substituent are also included. Among these, cellulose triacetate (triacetyl cellulose) is particularly preferred.
[0193] Polycarbonate resins are engineering plastics made of polymers in which monomer units are bonded via carbonate groups.
[0194] The thickness of the protective film is usually 1 to 100 μm, but is preferably 5 to 60 μm, and more preferably 5 to 50 μm, from the viewpoints of strength, handling, etc. If the thickness is within this range, the cured liquid crystal layer is mechanically protected, and the cured liquid crystal layer does not shrink even when exposed to a humid and hot environment, and stable optical properties can be maintained.
[0195] The protective film can be attached to the liquid crystal cured layer via, for example, an adhesive layer. As the adhesive for forming the adhesive layer, a water-based adhesive, an active energy ray curable adhesive, or a heat-curable adhesive can be used, and a water-based adhesive or an active energy ray curable adhesive is preferable.
[0196] Examples of the aqueous adhesive include an adhesive made of an aqueous polyvinyl alcohol resin solution, an aqueous two-liquid urethane emulsion adhesive, and the like. Among them, an aqueous adhesive made of an aqueous polyvinyl alcohol resin solution is preferably used. Examples of the polyvinyl alcohol resin include a vinyl alcohol homopolymer obtained by saponifying polyvinyl acetate, which is a homopolymer of vinyl acetate, a polyvinyl alcohol copolymer obtained by saponifying a copolymer of vinyl acetate and another monomer copolymerizable therewith, and a modified polyvinyl alcohol polymer in which the hydroxyl groups of these are partially modified. The aqueous adhesive may contain a crosslinking agent such as an aldehyde compound (such as glyoxal), an epoxy compound, a melamine compound, a methylol compound, an isocyanate compound, an amine compound, or a polyvalent metal salt.
[0197] When using a water-based adhesive, it is preferable to carry out a drying process to remove water contained in the water-based adhesive after laminating the liquid crystal cured layer and the protective film. After the drying process, a curing process may be carried out at a temperature of, for example, 20 to 45°C.
[0198] The active energy ray-curable adhesive is an adhesive containing a curable compound that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, and is preferably an ultraviolet ray-curable adhesive.
[0199] The curable compound may be a cationic polymerizable curable compound or a radical polymerizable curable compound. Examples of the cationic polymerizable curable compound include an epoxy compound (a compound having one or more epoxy groups in the molecule), an oxetane compound (a compound having one or more oxetane rings in the molecule), or a combination thereof. Examples of the radical polymerizable curable compound include a (meth)acrylic compound (a compound having one or more (meth)acryloyloxy groups in the molecule), other vinyl compounds having a radical polymerizable double bond, or a combination thereof. A cationic polymerizable curable compound and a radical polymerizable curable compound may be used in combination. An active energy ray curable adhesive usually further includes a cationic polymerization initiator and / or a radical polymerization initiator for initiating the curing reaction of the curable compound.
[0200] When laminating the liquid crystal cured layer and the protective film, at least one of the laminating surfaces may be subjected to a surface activation treatment in order to enhance adhesion. Examples of the surface activation treatment include dry treatments such as corona treatment, plasma treatment, discharge treatment (glow discharge treatment, etc.), flame treatment, ozone treatment, UV ozone treatment, and ionizing active ray treatment (ultraviolet ray treatment, electron beam treatment, etc.); and wet treatments such as ultrasonic treatment using a solvent such as water or acetone, saponification treatment, and anchor coat treatment. These surface activation treatments may be performed alone or in combination of two or more.
[0201] When protective films are attached to both sides of the cured liquid crystal layer, the adhesive for attaching these protective films may be the same type of adhesive or different types of adhesive.
[0202] (Laser irradiation process) In the present invention, the step of irradiating the laminated film with a laser having a wavelength of 300 nm to 800 nm can be carried out, for example, in the following embodiment.
[0203] The laser is not particularly limited, and a solid-state laser such as a YAG laser, a YLF laser, a YVO4 laser, or a titanium sapphire laser can be used.
[0204] In the above process, the wavelength of the laser can be appropriately selected depending on the composition and thickness of the liquid crystal cured layer or the substrate to be irradiated, but is preferably 350 nm or more, more preferably 400 nm or more. The upper limit of the laser wavelength is preferably 750 nm, more preferably 700 nm.
[0205] When the laminated film is irradiated with a laser, it is preferable to irradiate the liquid crystal cured layer with the laser. When the protective film is irradiated with a laser, the protective film preferably has a transmittance of 20% or more, more preferably 50% or more, at the laser wavelength on the side irradiated with the laser.
[0206] In the above process, the conditions for irradiating the laser light can be appropriately selected depending on the composition and thickness of the irradiated liquid crystal cured layer or substrate, the laser device, etc., but for example, when using a solid laser, the laser power is preferably 0.3 W or more, more preferably 0.5 W or more, and preferably 10 W or less, more preferably 5 W or less. The switching frequency is preferably 1000 Hz or more, more preferably 15000 Hz or more, preferably 1000000 Hz or less, more preferably 300000 Hz or less. The scanning speed is preferably 100 mm / sec or more, more preferably 200 mm / sec or more, preferably 10000 mm / sec or less, and preferably 5000 mm / sec or less. By irradiating under such conditions, it is possible to efficiently form a region in which the dichroic dye is reduced while suppressing thermal damage to the substrate.
[0207] The polarizing film can be continuously produced by a roll to roll method. For example, a laminate having a substrate and a liquid crystal cured layer is wound in advance into a roll, and the laminate is transported while unwinding, and a step of laminating a protective film and a step of irradiating a laser can be continuously performed. In the step of laminating a protective film, the protective film wound in a roll is transported while unwinding, and the protective film is laminated on the laminate and bonded to obtain a laminated film. In the laser irradiation step, the laminated film can be irradiated with a laser while being continuously transported. After the laser irradiation step, the obtained polarizing film can be further wound into a roll to form a rolled body. When the polarizing film is continuously produced, a polarizing film having a length of, for example, 10 m or more can be produced.
[0208] In the method for producing a polarizing film of the present invention, a polarizing film can be continuously produced by further including an alignment layer forming step and a liquid crystal cured layer forming step. When the alignment layer forming step is further included, the substrate layer wound in a roll shape is conveyed while being unwound, and the alignment layer is formed by continuously applying the alignment layer forming composition to this substrate layer using a coating device. When the liquid crystal cured layer forming step is continuously performed, the liquid crystal cured layer is formed by applying the liquid crystal cured layer forming composition to the surface of the substrate layer with the alignment layer on which the alignment layer is formed while the substrate layer with the alignment layer is continuously conveyed.
[0209] <Method of manufacturing circularly polarizing plate> The circular polarizing plate of the present invention can be manufactured by laminating the polarizing film of the present invention and the retardation layer. As described above, when the polarizing film is a continuously manufactured long polarizing film having a length of 10 m or more, it is preferable to use a long retardation layer having a length of 10 m or more as the retardation layer, and laminate the long polarizing film and the long retardation layer while continuously transporting both to form a long laminate. At this time, it is preferable to coat at least one of the long polarizing film and the long retardation layer with a pressure sensitive adhesive or adhesive to laminate both.
[0210] The method for producing a circularly polarizing plate of the present invention may include a step of cutting a long laminate obtained by laminating a long polarizing film and a long retardation layer into sheets of a predetermined size so that the polarizing film can be attached to a display device or the like of a predetermined size. In the cutting step, it is preferable to cut the long laminate in at least one of the length direction and width direction of the long laminate. In this case, it is preferable to determine the cutting position in the long laminate so that the second region of the liquid crystal cured layer is located at a predetermined position in the cut sheet. EXAMPLES
[0211] The present invention will be described in more detail with reference to examples, although the present invention is not limited to these examples.
[0212] (Visibility correction transmittance (Ty), visibility correction polarization degree (Py)) For each sample, the luminous efficiency corrected degree of polarization (Ty) and the luminous efficiency corrected degree of polarization (Py) were calculated by the following procedure.
[0213] Procedure: Measure the transmittance (T 1 ) and transmittance along the absorption axis (T 2 ) was measured by the double beam method using a spectrophotometer (Shimadzu Corporation UV-3150) equipped with a folder with a polarizer. The reference side of the folder was equipped with a mesh that cuts the amount of light by 50%. Using the following (Equation 1) and (Equation 2), the transmittance and degree of polarization at each wavelength were calculated, and luminosity correction was further performed using the 2-degree visual field (C light source) of JIS Z 8701 to calculate the luminosity-corrected transmittance (Ty) and luminosity-corrected degree of polarization (Py).
[0214] Transmittance [%]=(T 1 +T 2 ) / 2 (formula 1) Degree of polarization [%] = {(T 1 -T 2 ) / (T 1 +T 2 )}×100 (Equation 2)
[0215] Example 1 (Production of composition for forming alignment layer) Two parts of polymer (1) having a number average molecular weight of 28,000 and represented by the following chemical formula was mixed with 98 parts of o-xylene, and the resulting mixture was stirred at 80° C. for one hour to obtain a composition for forming an alignment layer.
[0216] Polymer (1) TIFF0007575275000018.tif33120
[0217] (In the formula, Me represents a methyl group.)
[0218] (Production of composition for forming liquid crystal cured layer) The following components were mixed and stirred for 1 hour at 80° C. to obtain a composition for forming a liquid crystal cured layer. The azo-based dye described in the examples of JP-A-2013-101328 was used as the dichroic dye. 75 parts of a polymerizable liquid crystal compound represented by formula (1-6) TIFF0007575275000019.tif19160
[0219] 25 parts of a polymerizable liquid crystal compound represented by formula (1-7) TIFF0007575275000020.tif18140
[0220] 2.8 parts of the dichroic dye (1) shown below TIFF0007575275000021.tif16130
[0221] 2.8 parts of the dichroic dye (2) shown below TIFF0007575275000022.tif17134
[0222] 2.8 parts of the dichroic dye (3) shown below TIFF0007575275000023.tif21144
[0223] Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent: Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) 1.2 parts Solvent: Cyclopentanone 250 parts
[0224] (Manufacture of Laminated Film 1) A triacetyl cellulose film (KC4UY-TAC, manufactured by Konica Minolta, 40 μm thick) serving as a base layer was cut into a size of 50×50 mm, and its surface was subjected to a corona treatment (AGF-B10, manufactured by Kasuga Electric Co., Ltd.). The above-mentioned base layer had a luminous efficiency-corrected transmittance (Ty) of 2% at 355 nm and a luminous efficiency-corrected transmittance (Ty) of 92% at 532 nm.
[0225] The above composition for forming an alignment layer was applied to the corona-treated film surface using a bar coater, and then dried for 1 minute in a drying oven set at 120°C to obtain a coating layer for an alignment layer. Polarized UV was irradiated onto the coating layer for an alignment layer at 50 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.). 2 An alignment layer was formed by irradiating the substrate with an integrated light amount (based on 313 nm).
[0226] A liquid crystal cured layer-forming composition was applied onto the obtained alignment layer using a bar coater, and then dried in a drying oven set at 110° C. for 1 minute.
[0227] Then, a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate the specimen with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, cumulative light intensity at wavelength 365 nm: 1000 mJ / cm 2 ) to form a liquid crystal cured layer 1 in which the liquid crystal compound and the dichroic dye were aligned, thereby obtaining a laminated film 1 having the base layer, the alignment layer, and the liquid crystal cured layer in this order.
[0228] The cured liquid crystal layer 1 in the laminate film 1 had a luminous efficiency-corrected transmittance of 42% and a luminous efficiency-corrected polarization degree of 98%.
[0229] (Creating polarizing film) A polarizing film was obtained by irradiating the laminated film 1 from the liquid crystal cured layer side with a 355 nm laser using a laser marker manufactured by Keyence Corporation at an output of 3.2 W, a switching frequency of 100,000 Hz, and a scan speed of 1,000 mm / sec. In the obtained polarizing film, the area formed by laser irradiation was circular (diameter 10 mm) and had a visibility-corrected transmittance of 86%. Furthermore, the appearance and hue of the area formed by laser irradiation were visually observed. The results are shown in Table 1.
[0230] Example 2 A polarizing film was prepared and observed in the same manner as in Example 1, except that the laser wavelength was changed to 532 nm. The results are shown in Table 1. Example 3 A polarizing film was prepared and observed in the same manner as in Example 2, except that the laser irradiation diameter was set to 1 mm. The results are shown in Table 1. Example 4 A polarizing film was prepared and observed in the same manner as in Example 2, except that the laser irradiation diameter was set to 3 mm. The results are shown in Table 1. [ Reference example 1 〕 A polarizing film was prepared and observed in the same manner as in Example 2, except that the laser irradiation diameter was set to 20 mm. The results are shown in Table 1. Example 6 A polarizing film was prepared and observed in the same manner as in Example 1, except that the laser was irradiated from the side of the base layer (triacetyl cellulose film). The results are shown in Table 1. Example 7 A polarizing film was prepared and observed in the same manner as in Example 4, except that the laser was irradiated from the side of the base layer (triacetyl cellulose film). The results are shown in Table 1. Comparative Example 1 A polarizing film was prepared and observed in the same manner as in Example 2, except that the following laminate film 2 was used. The results are shown in Table 1. (Manufacture of Laminated Film 2) A 30 μm thick polyvinyl alcohol film (average degree of polymerization: about 2400, saponification degree: 99.9 mol% or more) was uniaxially stretched about 5 times by dry stretching, and then, while maintaining the tension, was immersed in pure water at 40° C. for 40 seconds. After that, it was immersed in a dyeing solution with a mass ratio of iodine / potassium iodide / water of 0.044 / 5.7 / 100 at 28° C. for 30 seconds to perform a dyeing process. Next, the film was immersed in an aqueous boric acid solution with a mass ratio of potassium iodide / boric acid / water of 11.0 / 6.2 / 100 at 70° C. for 120 seconds. After washing with pure water at 8° C. for 15 seconds, the film was dried at 60° C. for 50 seconds and then at 75° C. for 20 seconds while being held under a tension of 300 N, to obtain a 12 μm-thick liquid crystal cured layer in which iodine was adsorbed and aligned on the polyvinyl alcohol film. A water-based adhesive was poured between the obtained liquid crystal cured layer and a triacetyl cellulose film (KC4UY-TAC manufactured by Konica Minolta, Inc., thickness 40 μm), and the layers were laminated together using a nip roll. The resulting laminate was dried at 60°C for 2 minutes while maintaining the tension at 430 N / m to obtain a laminate film 2 having a cycloolefin film as a protective film on one side. The aqueous adhesive was prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (Kuraray Poval KL318; manufactured by Kuraray Co., Ltd.) and 1.5 parts of water-soluble polyamide epoxy resin (Sumirez Resin 650; manufactured by Sumika Chemtex Co., Ltd., aqueous solution with a solid content of 30%) to 100 parts of water. Comparative Example 2 A polarizing film was prepared and observed in the same manner as in Example 1, except that the laser wavelength was changed to 1064 nm. The results are shown in Table 1. Comparative Example 3 A polarizing film was prepared and observed in the same manner as in Example 2, except that the laser irradiation diameter was changed to 30 mm. The results are shown in Table 1.
[0231] [Table 1]
[0232] In each of the polarizing films of Examples 1 to 7, the region irradiated with the laser had a transparent hue. In other words, each of the polarizing films of Examples 1 to 7 had a region with higher transparency (i.e., a region with a higher luminosity-corrected transmittance) than the region not irradiated with the laser. Therefore, it was found that in each of the polarizing films of Examples 1 to 7, the region not irradiated with the laser corresponds to the first region, and the region irradiated with the laser corresponds to the second region. On the other hand, no area having a transparent hue was observed in Comparative Example 2. Therefore, it was found that the polarizing film of the present invention cannot be obtained by the production method of Comparative Example 2. [Explanation of symbols]
[0233] 1 polarizing film, 11 liquid crystal cured layer, 11a first region, 11b second region, 12 alignment layer, 13 substrate layer, 15 retardation layer,
Claims
1. A polarizing film having a liquid crystal cured layer, The liquid crystal cured layer is formed by curing a compound containing a liquid crystal compound, and has at least a first region and a second region having different luminosity-corrected transmittance values, The difference between the thickness of the first region and the thickness of the second region is 0.5 μm or less; The liquid crystal compound includes a polymerizable liquid crystal compound, The second region has a luminosity-corrected transmittance higher than that of the first region, and has a shape in a plan view that is circular, elliptical, oval, or polygonal. When the second region is circular, the diameter is 1 cm or less. When the second region is elliptical or oval, the major axis is 1 cm or less. When the second region is polygonal, the diameter of an imaginary circle inscribed in the polygon is 1 cm or less. Polarizing film.
2. 2. The polarizing film according to claim 1, wherein the first region has a higher luminosity-corrected polarization degree than the second region.
3. 3. The polarizing film according to claim 1, wherein the luminosity-corrected polarization degree in the first region is 90% or more.
4. 4. The polarizing film according to claim 1, wherein the luminosity-corrected polarization degree in the second region is 10% or less.
5. 5. The polarizing film according to claim 1, wherein the liquid crystal cured layer further contains a dichroic dye.
6. 8. The polarizing film according to claim 7, wherein the first region has a higher content of the dichroic dye than the second region.
7. The polarizing film according to any one of claims 1 to 6, wherein the luminosity-corrected single transmittance in the first region is 35% or more.
8. The polarizing film according to any one of claims 1 to 7, wherein the luminosity-corrected single transmittance in the second region is 80% or more.
9. The polarizing film according to any one of claims 1 to 8, wherein the first region exhibits a Bragg peak in X-ray diffraction measurement.
10. The polarizing film according to any one of claims 1 to 9, wherein the length of the polarizing film is 10 m or more.
11. Further, the substrate has a substrate layer and an orientation layer laminated on at least one side of the substrate layer, A liquid crystal curing layer is laminated on the alignment layer. The polarizing film according to any one of claims 1 to 10.
12. The polarizing film of claim 11 , wherein the alignment layer comprises a photoalignable polymer.
13. The polarizing film according to claim 11 or 12, wherein the substrate layer has a function of a quarter-wave plate.
14. 13. A circularly polarizing plate comprising the polarizing film according to claim 1 and a retardation layer having a quarter-wave plate function laminated thereon.
15. The method includes a step of irradiating a laminated film having a liquid crystal cured layer containing a dichroic dye and a substrate layer with a laser having a wavelength of 300 nm to 800 nm. The method for producing a polarizing film according to any one of claims 1 to 13, wherein a part of the liquid crystal cured layer has a lower content of the dichroic dye than the other part.
16. The laminated film further has an orientation layer, The alignment layer is laminated to the liquid crystal curing layer. The method for producing the polarizing film according to claim 15 .
17. 17. The method for producing a polarized film according to claim 15 or 16, wherein the region with a reduced dichroic dye content has a circular, elliptical, oval, or polygonal shape in a planar view, and when the region is circular, the diameter is 1 cm or less, when the region is elliptical or oval, the major axis is 1 cm or less, and when the region is polygonal, the diameter of an imaginary circle inscribed in the polygon is 1 cm or less.
18. The method for producing a polarizing film according to any one of claims 15 to 17, wherein the liquid crystal cured layer contains a polymer of a polymerizable liquid crystal compound.
19. The method for producing a polarizing film according to any one of claims 15 to 18, wherein the polarizing film has a length of 10 m or more.
20. A step (1) of irradiating a laminated film having a liquid crystal cured layer having a dichroic dye and a substrate with a laser having a wavelength of 300 nm to 800 nm; and a step (2) of laminating the polarizing film obtained by the step (1) and a retardation layer having a quarter-wave plate function, The method for producing a circularly polarizing plate, wherein the polarizing film is the polarizing film according to any one of claims 1 to 13.
21. The method for producing a circularly polarizing plate according to claim 20, wherein the step (1) is carried out after the step (2).
Citation Information
Patent Citations
Polarizer and image display device
JP2014164084A
Method for manufacturing patterned polarization film
JP2015206852A
Patterned polarizing film
JP2015212823A
Polarizing plate having a locally depolarized region and method for manufacturing the same
JP2016531317A
Polarizing member including a local decoloring region, polarizing member roll, and method for manufacturing a sheet-type polarizing member
JP2017500606A