Asphalt composition containing monomeric MDI as a thermosetting reactive compound

Monomeric MDI enhances asphalt compositions by forming a specific colloidal structure, addressing limitations in temperature range and elasticity, resulting in improved stability and reduced deformation.

JP7575381B2Active Publication Date: 2024-10-29BASF SE
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021534361
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-18
Filing Date
2019-12-09
Publication Date
2024-10-29
Estimated Expiration
2039-12-09

AI Technical Summary

Technical Problem

Existing asphalt compositions suffer from a limited useful temperature range, low elasticity, and susceptibility to permanent deformation, particularly in extreme weather conditions.

Method used

Incorporation of monomeric MDI as a thermosetting reactive compound in asphalt compositions, reacting with asphalt components to form a specific colloidal structure, enhancing elasticity and stability across a wider temperature range.

Benefits of technology

The modified asphalt exhibits improved physical properties with an expanded useful temperature range, increased elastic response, better adhesion, and reduced permanent deformation, suitable for various applications including road surfacing and coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575381000001
    Figure 0007575381000001
  • Figure 0007575381000002
    Figure 0007575381000002
  • Figure 0007575381000003
    Figure 0007575381000003
Patent Text Reader

Abstract

An asphalt composition comprising 0.1 to 10.0 mass % of monomeric MDI based on the total mass of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention essentially relates to an asphalt composition containing monomeric MDI as the thermosetting reactive compound. The present invention also relates to a method for producing an asphalt composition. The asphalt compositions of the present invention exhibit an expanded functional temperature range, better storage stability at high temperatures, and improved deformation resistance properties of the asphalt, such as the useful temperature range of the asphalt, increased elasticity, and lower deformation potential. [Background technology]

[0002] Generally, asphalt is a colloidal material that contains various molecular species classified as asphaltenes and maltenes. Being viscoelastic and thermoplastic, asphalt changes properties over a range of temperatures from extremely cold to extremely hot. Asphalt tends to soften in hot weather and crack when very cold. At low temperatures asphalt becomes brittle and prone to cracking, while at high temperatures it softens and loses its physical properties.

[0003] The addition of thermosetting reactive components, either as binders or in more general terms as modifiers, allows the physical properties of the asphalt to remain more consistent over a range of temperatures and / or improves the physical properties over the range of temperatures to which the asphalt is exposed.

[0004] Such asphalts, each modified by an added binder, have been known in the art for many years. However, there remains a need in the asphalt industry for improved asphalts. In part, this is because currently known polymer modified asphalts have several shortcomings, including, for example, susceptibility to permanent deformation (rutting), flexural fatigue, and loss of elasticity during moisture and low temperature use.

[0005] WO 01 / 30911 A1 discloses an asphalt composition comprising about 1-8% by weight of polymeric MDI, based on the total weight of the composition, the polymeric MDI having a functionality of at least 2.5. It also relates to a process for preparing said asphalt composition using a reaction time of less than 2 hours. The formation of the product MDI-asphalt is measured by the increase in viscosity of the product or, more preferably, by dynamic mechanical analysis (DMA).

[0006] WO 01 / 30912 A1 discloses an aqueous asphalt emulsion comprising, in addition to asphalt and water, an emulsifiable polyisocyanate. It also relates to an aggregate composition comprising said emulsion, and a process for preparing said composition.

[0007] WO 01 / 30913 A1 discloses an asphalt composition comprising about 1-5% by weight, based on the total weight of the composition, of a prepolymer based on polymeric MDI, the polymeric MDI having a functionality of at least 2.5. It also relates to a process for preparing said asphalt composition.

[0008] EP 0 537 638 B1 discloses a polymer-modified bitumen composition comprising 0.5 to 10 parts by weight of a functionalized polyoctenamer per 100 parts by weight of bitumen, and optionally a crosslinker, characterized in that the polyoctenamer is predominantly a trans-polyoctenamer and contains carboxyl groups as well as groups derived from the carboxyl groups, for example with maleic acid. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] WO 01 / 30911 [Patent Document 2] WO 01 / 30912 [Patent Document 3] WO 01 / 30913 [Patent Document 4] European Patent No. 0537638 Summary of the Invention [Problem to be solved by the invention]

[0010] As a result, it would be highly desirable to have an asphalt composition and related preparation process that avoids all of the disadvantages associated with the prior art, such as the limited useful temperature range, limited elastic response, and low softening point.

[0011] One of the objectives of the present invention was to provide an asphalt composition that exhibits improved physical properties in that it is more consistent over a range of temperatures and has better storage stability at elevated temperatures. In addition, it exhibits an extended useful temperature interval (UTI) and has improved non-recoverable creep compliance (JCR). nr ), have increased elastic response, have increased load rating, and have reduced potential for permanent asphalt deformation under conditions of increased traffic volume and reduced speed, respectively.

[0012] Additionally, the preparation process of each asphalt composition should have been provided.

[0013] Various physical properties of the asphalt compositions are measured by various tests that are known in the art and are described in detail in the experimental section. [Means for solving the problem]

[0014] Elastic response and non-recoverable creep compliance (J nr) is calculated in a Multiple Stress Creep Recovery (MSCR) test, where the asphalt is subjected to a constant load for a certain time. The total deformation over a specific period is given as a percentage and is a measure of the elasticity of the binder. Additionally, the phase angle can be measured, which illustrates the improved elastic response (reduced phase angle) of the modified binder.

[0015] Accordingly, an asphalt composition was found that contains 0.1 to 10.0 mass % of monomeric MDI, based on the total mass of the composition.

[0016] According to a further aspect of the present invention, there is provided a method for preparing an asphalt composition, the method comprising the steps of: a) heating the raw asphalt to a temperature of 110 to 190 ° C; b) adding under stirring a desired amount of monomeric MDI as a thermosetting reactive compound; c) after step b), stirring the reaction mixture at a temperature in the range of 110-190° C. for at least 2.5 hours; Including, Here, the above reaction is carried out under an oxygen atmosphere, This method achieves the object of the present invention.Furthermore, there is provided a use of the asphalt composition for the preparation of an asphalt mix composition.

[0017] Surprisingly, it has been discovered that asphalt compositions according to the present invention exhibit an expanded useful temperature range, increased elastic response, better adhesion, and increased load rating, as well as a reduced likelihood of permanent asphalt deformation.

[0018] Without being bound by this theory, it is currently believed that a particular morphology of the colloidal structure is necessary to obtain the resulting performance. The thermosetting reactive compounds react with phenolic, carboxylic acid, thiol, anhydride, and / or pyrrolic groups, or any reactive groups from the asphalt components, to bond the asphaltenes together, resulting in larger particles in the resulting asphalt composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Preferred embodiments are set forth in the claims and in the specification, and it is understood that combinations of the preferred embodiments are within the scope of the invention.

[0020] In accordance with the present invention, the asphalt composition comprises monomeric MDI as the thermosetting reactive compound.

[0021] Generally, the asphalt used in the present invention can be any asphalt known in the art, which generally includes any bituminous compound (bitumen). It can be either a bitumen or a material called asphalt.

[0022] For example, distillate, blown, high vacuum, and cutback bitumen, as well as for example asphalt concrete, cast asphalt, asphalt mastic, and natural asphalt. For example, directly distilled asphalt can be used, which has, for example, a penetration of 80 / 100 or 180 / 220. For example, the asphalt can be fly ash-free.

[0023] Preferably, the asphalt has a penetration of 20-30, 30-45, 35-50, 40-60, 50-70, 70-100, 100-150, 160-220, 250-330, or a performance grade of 52-16, 52-22, 52-28, 52-34, 52-40, 58-16, 58-22, 58-28, 58-34, 58-40, 64-16, 64-22, 64-28, 64-34, 64-40, 70-16, 70-22, 70-28, 70-34, 70-40, 76-16, 76-22, 76-28, 76-34, 76-40. More preferably, the asphalt has a penetration of 30 to 45, 35 to 50, 40 to 60, 50 to 70, 70 to 100, 100 to 150, or 160 to 220, or 52-16, 52-22, 52-28, 52-34, 52-40, 58-16, 58-22, 58-28, 58-34, 58-40, 64-16, 64-22, 64-28, 64-34, 70-16, 70-22, 70 Preferably the asphalt has a penetration of 40-60, 50-70, 70-100, 100-150 or a performance grade of 52-16, 52-22, 52-28, 52-34, 52-40, 58-16, 58-22, 58-28, 58-34, 64-16, 64-22, 64-28, 70-16, 70-22, 76-16, 76-22.

[0024] Generally, thermosetting reactive compounds are compounds that can chemically react with the various molecular species classified as asphaltenes and maltenes of the respective asphalt, and help to produce a particular morphology of colloidal structures that cause the physical properties of the asphalt to remain more constant over a wide range of temperatures and / or help to improve the physical properties over the temperature range to which the asphalt is subjected.

[0025] The thermosetting reactive compound according to the present invention is monomeric MDI.

[0026] Generally, monomeric MDI (mMDI) is known in the art and is known as methylene diphenyl diisocyanate. It can occur in various isomeric forms, such as 4,4'-, 2,2'-, and 2,4'-isomers. According to the present invention, any of the known isomers of mMDI or mixtures of various isomers can be used, provided that they are compatible with the asphalt. Preferably, it is pure 4,4'-MDI, a mixture of 2,4'-MDI and 4,4'-MDI, a mixture of 2,4'-MDI and 4,4'-MDI with reduced 2,2'-MDI content, more preferably, it is pure 4,4'-MDI, a mixture of 2,4'-MDI and 4,4'-MDI, and most preferably, it is pure 4,4'-MDI (pure 4,4'-MDI). Preferably, the amount of 4,4'-MDI isomer is in the range of 40 to 99.5%, more preferably in the range of 44% to 99%, and most preferably in the range of 46% to 98.5%.

[0027] The thermosetting reactive compound may also include modified variants containing carbodiimide, uretonimine, isocyanurate, urethane, allophanate, urea, or biuret groups. Preferably, the modified variant according to the present invention is a carbodiimide modified monomeric MDI. More preferably, the carbodiimide modified monomeric MDI is a mixture of 4,4'-MDI and carbodiimide modified monomeric MDI. Preferably, the mass percentage of 4,4'-MDI in the carbodiimide modified monomeric MDI is in the range of 65-85%, and the mass percentage of carbodiimide in the carbodiimide modified monomeric MDI is in the range of 15-35%. More preferably, the mass percentage of 4,4'-MDI in the carbodiimide modified monomeric MDI is in the range of 70-80%, and the mass percentage of carbodiimide in the carbodiimide modified monomeric MDI is in the range of 20-30%. Preferably, the mMDI used in accordance with the present invention has an average isocyanate functionality of at least 2.0, more preferably at least 2.1, and most preferably at least 2.15, for example 2.2, 2.3, or 2.4, all of which are hereinafter referred to as monomeric MDI or mMDI.

[0028] Further, other isocyanates, polymeric isocyanates, and / or prepolymers may be added to adjust the physical properties of each MDI.

[0029] According to the present invention, the amount of monomeric MDI as a thermosetting reactive compound in the asphalt composition is 10.0% by mass or less based on the total mass of the asphalt composition. It is preferably 5.0% by mass or less, more preferably 4.0% by mass or less, and most preferably 3.0% by mass or less based on the total mass of the asphalt composition. According to the present invention, the amount of monomeric MDI as a thermosetting reactive compound in the asphalt composition is at least 0.1% by mass, preferably at least 0.5% by mass, more preferably at least 0.7% by mass, and most preferably at least 0.9% by mass, based on the total mass of the asphalt composition. For example, the amount of monomeric MDI as a thermosetting reactive compound in the asphalt composition can be in the range of 0.5 to 1.8% by mass, 0.8 to 1.7% by mass, 1.0 to 1.9% by mass, 1.1 to 2.0% by mass, 1.8 to 3.2% by mass, 2.1 to 3.7% by mass, or 0.5 to 2.5% by mass.

[0030] In general, the amount of monomeric MDI as a thermosetting reactive compound may depend on the composition of each asphalt. For hard asphalts with a penetration of less than 85, a smaller amount of monomeric MDI may be required as a thermosetting reactive compound, and for soft asphalts with a penetration of more than 85, a larger amount of each monomeric MDI may be required as a thermosetting reactive compound. Without being bound by this theory, it is currently believed that the amount of each monomeric MDI as a thermosetting reactive compound needs to be readjusted due to the different concentrations of polar components, also called n-heptane insolubles (which include asphaltene), in various asphalts. In soft asphalts corresponding to a penetration of more than 85, asphaltene is diluted and therefore less concentrated, which requires a larger amount of each monomeric MDI as a thermosetting reactive compound and more oxidation (which may be provided by the oxygen atmosphere in the manufacturing process of the asphalt composition) to achieve better performance.

[0031] Generally, for asphalts having a penetration of less than 85 corresponding to a performance grade having a high temperature limit of at least 64, the amount of each monomeric MDI as a thermosetting reactive compound in the asphalt composition can range from 0.1 to 3.0% by weight, preferably the amount of monomeric MDI as a thermosetting reactive compound is not more than 2.5% by weight, most preferably not more than 2.3% by weight, especially not more than 2.0% by weight, and the amount of monomeric MDI as a thermosetting reactive compound is at least 0.1% by weight, preferably at least 0.5% by weight, more preferably at least 0.7% by weight, most preferably at least 1.0% by weight, based on the total weight of the asphalt composition.

[0032] Generally, for asphalts having a penetration greater than 85 corresponding to a performance grade having a high temperature limit of 64 or less, the amount of monomeric MDI as a thermosetting reactive compound in the asphalt composition can range from 2.0% to 10.0% by weight, preferably the amount of monomeric MDI as a thermosetting reactive compound is 5.0% by weight or less, most preferably 4.5% by weight or less, especially 4.0% by weight or less, and the amount of monomeric MDI as a thermosetting reactive compound is at least 2.0% by weight, preferably at least 2.5% by weight, more preferably at least 2.7% by weight, most preferably at least 3.0% by weight, based on the total weight of the asphalt composition.

[0033] Generally, asphalt can be modified to improve performance with respect to various physical properties, for example, increased elastic response can be achieved.

[0034] By using the asphalt composition according to the invention, it is possible to achieve a shift from one grade to another. For example, the modification of asphalt pen 50 / 70 results in polymer modified asphalt 25 / 55-55A using 2% by mass of monomeric MDI as the thermosetting reactive compound, or harder grades such as pen 20 / 30 or 30 / 45, depending on the amount of the respective monomeric MDI as the thermosetting reactive compound. The same applies to converting asphalt with pen 70-100 to pen 50-70 using 2% by mass of monomeric MDI as the thermosetting reactive compound, or to converting to PmB 25 / 55-55A using 3% by mass of monomeric MDI as the thermosetting reactive compound. Also, a shift to higher performance grades is achievable, for example PG64-22 after modification with 2% by weight of the respective monomeric MDI as a thermosetting reactive compound, for example a carbodiimide modified monomeric MDI, for example a mixture of 4,4'-MDI and carbodiimide modified monomeric MDI, gives PG70-22.

[0035] Each of the properties of the bituminous compositions according to the present invention, such as an extended useful temperature range, increased elastic response, better adhesion, and increased load rating, as well as a reduced possibility of permanent bituminous deformation, depend on the concentration of particles having a particular sedimentation coefficient, which is directly related to the particle size of the corresponding composition.

[0036] According to the present invention, the asphalt composition has at least 18% by weight of particles having a sedimentation coefficient in white spirit solvent greater than 5000 Sved based on the total weight of the composition, more preferably 20% by weight of particles having a sedimentation coefficient in white spirit solvent greater than 5000 based on the total weight of the composition, most preferably at least 23% by weight of particles having a sedimentation coefficient in white spirit solvent greater than 5000 Sved based on the total weight of the composition, the particles having a sedimentation coefficient in white spirit solvent greater than 5000 Sved can be 100% by weight or less based on the total weight of the composition, preferably the amount of particles having a sedimentation coefficient in white spirit solvent greater than 5000 Sved is 95% by weight or less based on the total weight of the composition, more preferably 90% by weight or less based on the total weight of the composition, most preferably 80% by weight or less based on the total weight of the composition. For example, particles having a sedimentation coefficient in the range of 15,000 to 170,000 Sved in white spirit solvent may comprise 18% to 75% by weight based on the total weight of the composition, particles having a sedimentation coefficient in the range of 25,000 to 140,000 Sved in white spirit solvent may comprise 23% to 65% by weight based on the total weight of the composition, or particles having a sedimentation coefficient in the range of 22,000 to 95,000 Sved in white spirit solvent may comprise 30% to 52% by weight based on the total weight of the composition.

[0037] In the context of the present invention, white spirit solvent means white spirit high boiling petroleum oil having CAS-Nr.: 64742-82-1, with an aromatic base of 18% and a boiling point of 180-220°C.

[0038] The sedimentation coefficient was detected by ultracentrifugation combined with a light absorption device. The sedimentation and concentration of each component were measured at a wavelength of 350 nm. This method is known in the art and is described in detail in the experimental section.

[0039] The asphalt composition of the present invention can be used as any classical asphalt composition of the prior art. The asphalt composition of the present invention may be particularly useful in the manufacture of: - paints and coatings, especially those for waterproofing; - mastics for filling joints and sealing cracks; - Grout materials and hot injection surface materials for surface finishing of roads, airports, sports fields, etc. - Mixed with stone to provide aggregate (which constitutes approximately 5-20% of the asphalt composition) (e.g. asphalt mix) - Hot coating material for surface treatment as above - Surface coating material for surface treatment as above - Warm Mix Asphalt (WMA) - Hot Mix Asphalt (HMA).

[0040] Furthermore, the present invention relates to a process for the preparation of an asphalt composition according to the invention, which comprises the following steps: a) heating the raw asphalt to a temperature of 110 to 190°C; b) adding under stirring a desired amount of monomeric MDI as a thermosetting reactive compound; c) after step b), stirring the reaction mixture at a temperature in the range of 110-190° C. for at least 2.5 hours; wherein the reaction is carried out under an oxygen atmosphere.

[0041] For example, the process of the present invention can be carried out in step a) and / or step c) at a temperature of 110-190° C. Preferably, the temperature is in the range of 110-180° C., more preferably in the range of 115-170° C., most preferably in the range of 120-155° C., for example the temperature is in the range of 121-152° C.

[0042] Generally, the temperatures of steps a), b) and c) are in the range of 110-190° C. and may be different for each step. Preferably, the temperatures in all three steps are the same and in the range of 110-190° C., more preferably the same and in the range of 110-170° C., and most preferably the same and in the range of 110-160° C.

[0043] According to the present invention, in step b) of the process for preparing the asphalt composition, a desired amount of the respective monomeric MDI as a thermosetting reactive compound is added under stirring, which may range from 0.1 to 10% by weight, based on the total weight of the composition.

[0044] Generally, the amount can also be determined by potentiometric titration, where the amount of reactive groups in the asphalt is determined and related to the equivalent weight of the reactive groups of the respective monomeric MDI as a thermosetting compound. Titration methods are known in the art and are described in detail in the experimental section.

[0045] Generally, asphalts from different suppliers differ in terms of composition, depending on which reservoir the crude oil comes from, as well as the distillation process in the refinery. However, the cumulative total amount of reactive groups can range from 3.1 to 4.5 mg KOH / g.

[0046] For example, asphalts having a penetration of 50-70 or 70-100 will have a stoichiometric amount of mMDI of 0.8-1.2 wt.%. The susceptibility of the asphalt components to oxidation at elevated temperatures during preparation of the asphalt composition will result in an excess of mMDI being used to react with newly formed functional groups.

[0047] According to the invention, step c) of the process is carried out after step b). The reaction mixture is stirred at a temperature in the range of 110-190°C for at least 2.5 hours, preferably the mixing time is at least 3 hours, more preferably the mixing time is at least 3.5 hours, most preferably the mixing time is at least 4 hours. The mixing time can be up to 20 hours, preferably the mixing time is not more than 15 hours, more preferably the mixing time is not more than 12 hours, most preferably the mixing time is not more than 9 hours. For example, after adding 1-1.5% by weight of each mMDI as the thermosetting reactive compound, the mixing time can be in the range of 2.5 hours to 4 hours, for example 3 hours or 3.5 hours. For example, after adding 1.5-5.0% by weight of each mMDI as the thermosetting reactive compound, the mixing time can be in the range of 4 hours to 6 hours, for example 4.5 hours, 5 hours, or 5.5 hours. For example, after adding 5 to 10.0% by mass of each mMDI as a thermosetting reactive compound, the mixing time may be within a range of 6 to 15 hours, for example, 7 hours, 7.5 hours, 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours, 14 hours, or 14.5 hours.

[0048] According to the present invention, the process for preparing the asphalt composition must be carried out under an oxygen atmosphere. Preferably, the oxygen concentration in the oxygen atmosphere is in the range of 1-21% by volume, more preferably, the oxygen concentration in the oxygen atmosphere is in the range of 5-21% by volume, and most preferably, the oxygen concentration in the oxygen atmosphere is in the range of 10-21% by volume, for example, the process of the present invention is carried out under air or in an atmosphere saturated with oxygen.

[0049] According to the present invention, the process for the preparation of the asphalt composition is carried out under stirring to allow vigorous stirring of the respective asphalt and the respective thermosetting compound and to maximize the contact with oxygen. Preferably, the stirring energy is in the range of 1-14 W / l, more preferably the stirring energy is in the range of 2-12 W / l, and most preferably the stirring energy is in the range of 4.0-10.0 W / l.

[0050] In general, the process is not limited to being carried out in one reaction vessel, e.g., a storage vessel (container). Each asphalt can be reacted with mMDI as a thermosetting reactive compound under the conditions described above, e.g., under oxygen at a temperature of 110°C to 190°C, e.g., for 1 hour. The asphalt can then be cooled, transferred to another reaction vessel, and heated so that the total reaction time under oxygen following transfer is at least 2.5 hours. Without being bound by this theory, it is currently believed that steps a) and b) (first step) are to homogenize the mixture and induce reaction between the reactive groups of the asphalt and the reactive groups of the respective mMDI as a thermosetting reactive compound. The thermosetting reactive compound may be introduced to the asphaltene surface. The second or additional heating step, summarized as step c), is to assist the crosslinking reaction by oxidation.

[0051] <Examples of asphalt compositions according to the present invention>

[0052] Z1: 1.0-1.8% by weight of monomeric MDI based on the total weight of the composition, wherein 18% to 65% by weight based on the total weight of the composition are particles having a sedimentation coefficient in the range of 8,000 to 200,000 Svedbergs in white spirit solvent.

[0053] Z2: 1.8-3.2% by weight of 4,4'-MDI based on the total weight of the composition, wherein 22-70% by weight based on the total weight of the composition are particles having a sedimentation coefficient in the range of 20,000-140,000 Svedbergs in white spirit solvent.

[0054] Z3: 1.2-2.2% by weight of carbodiimide modified momeric MDI based on the total weight of the composition, wherein 33-68% by weight based on the total weight of the composition are particles having a sedimentation coefficient in the range of 28,000-1,000,000 Svedbergs in white spirit solvent.

[0055] Z4: 1.2-1.6% by weight mMDI based on the total weight of the composition, wherein 33%-85% by weight based on the total weight of the composition are particles having a sedimentation coefficient in the range of 25,000-150,000 Svedbergs in white spirit solvent.

[0056] Z5: 1.5-2.0% by weight of monomeric MDI, based on the total weight of the composition, wherein 22% to 58% by weight, based on the total weight of the composition, are particles having a sedimentation coefficient in the range of 20,000 to 250,000 Svedbergs in white spirit solvent.

[0057] Z6: 2.3-2.9% by weight of monomeric MDI, based on the total weight of the composition, wherein 27% to 82% by weight, based on the total weight of the composition, are particles having a sedimentation coefficient in the range of 12,000 to 370,000 Svedbergs in white spirit solvent.

[0058] Z7: 3.0-3.6% by weight of monomeric MDI, based on the total weight of the composition, wherein 19% to 62% by weight, based on the total weight of the composition, are particles having a sedimentation coefficient in the range of 15,000 to 135,000 Svedbergs in white spirit solvent.

[0059] Z8: 1.6 to 3.5 mass% of carbodiimide-modified monomeric MDI based on the total mass of the composition (4,4'-MDI in this carbodiimide-modified monomeric MDI is 70 to 80% of the carbodiimide-modified monomeric MDI, carbodiimide in the carbodiimide-modified monomeric MDI is 20 to 30% of the carbodiimide-modified monomeric MDI, and 21 mass% to 50 mass% based on the total mass are particles having a sedimentation coefficient in the range of 17,000 to 500,000 Svedberg in white spirit solvent). EXAMPLES

[0060] <Examples and Comparative Examples> [General procedure for the preparation of asphalt compositions]

[0061] According to Table 1, 2.5 kg of each grade of asphalt was heated to 140°C under oxygen atmosphere and stirred at 400 rpm in an oil bath (set to a temperature of up to 150°C). When the internal temperature reached 100°C, 50 g of the respective thermosetting reactive compound according to Table 1 was added to the molten asphalt. The stirring energy varied from 5.6 to 12 W / l. The reactants were further treated at 140°C for 420 min and then cooled at room temperature. The samples were canned and stored at room temperature for further testing.

[0062] For Comparative Examples 1 (#1), 4 (#4), and 6 (#6), 2.5 kg of each grade of asphalt was heated to 140°C under oxygen atmosphere according to Table 1, stirred at 400 rpm in an oil bath (set at a temperature of ~150°C) for ~420 min, and then cooled at room temperature. The samples were canned and stored at room temperature for further testing.

[0063] For Example 5 (#5), 3000 g of asphalt 64-22 was heated in a closed container at 150° C. in an oven for 2 hours. When the cover was removed, the preheated sample had a temperature of 150° C. It was then tied up in a heating mantle under oxygen atmosphere. At 20% mixer speed, the asphalt was further heated with an electric heating mantle using a temperature controller placed in the asphalt to maintain the temperature at 150° C.±2° C. Once the internal temperature reached 150° C., 60 g of mMDI (CDI13) with functionality of 2.2 was added to the molten asphalt. The reaction was further processed at 150° C. for 150 minutes.

[0064] For Comparative Example 2 (#2), 2.5 kg of Asphalt 50-70 was heated to 140°C under oxygen atmosphere and stirred at 400 rpm in an oil bath (temperature set at 150°C). When the internal temperature reached 100°C, 50 g of AS20 (2.0 wt%) was added to the molten asphalt. The reaction was further stirred at 140°C for 420 minutes and then cooled at room temperature. The sample was then used to determine the particle percentage of the asphalt composition using an analytical ultracentrifuge. See the results in Table 2.

[0065] For Example 3 (#3), 2.5 kg of Asphalt 50-70 was heated to 140° C. under oxygen atmosphere and stirred at 400 rpm in an oil bath (temperature set at 150° C.). When the internal temperature reached 100° C., 50 g of mMDI CDI13 (2.0 wt %) was added to the molten asphalt. The reaction was further stirred at 140° C. for 420 minutes and then cooled at room temperature. The sample was then used to determine the particle percentage of the asphalt composition using an analytical ultracentrifuge. See results in Table 2.

[0066] For Example 7 (#7), 2.5 kg of asphalt 70-100 was heated to 140°C under oxygen atmosphere and stirred at 400 rpm in an oil bath (temperature set at 150°C). When the internal temperature reached 100°C, 50 g of mMDI CDI13 (2.0 wt%) was added to the molten asphalt. The reaction was further treated at 140°C for 420 minutes and then cooled at room temperature. The sample was then used to determine the particle percentage of the asphalt composition using an analytical ultracentrifuge. See the results in Table 2.

[0067] <Thermosetting reactive compounds used in the examples> A mMDI, designated CDI13, with a functionality of 2.2, an NCO content of 29.5% and a viscosity of 40 mPa·s at 25 °C, and a pMDI, designated As20, with a functionality of 2.7, an NCO content of 31.5% and a viscosity of 210 mPa·s at 25 °C, were used. mMDI and pMDI with the respective functionality are commercially available, for example, from the following companies: Covestro, BASF SE, Huntsmann, etc.

[0068] <Method for detecting physical properties of asphalt or asphalt composition or asphalt mixture> The values ​​of the examples (Working Examples and Comparative Examples) are determined in accordance with the respective DIN standards.

[0069] <Detailed description of the methods used>

[0070] [Asphalt testing]

[0071] [Softening point DIN EN 1427] Two horizontal disks of bitumen cast into shouldered brass rings are heated at a controlled rate in a liquid bath while each supports a steel ball. The softening point is reported as the average temperature at which the two disks soften sufficiently to allow each bitumen-encased ball to fall a distance of (25 ± 0.4) [mm].

[0072] [Rolling thin film oven test DIN EN 12607-1] The bitumen is heated in the bottles in an oven at 163°C for 85 minutes. The bottles are rotated at 15 rpm and heated air is blown into each bottle at the point of minimum movement at 4000 mL / min. The effects of heat and air are determined from the change in physical test values ​​measured before and after oven treatment.

[0073] [Dynamic Shear Rheometer (DSR) DIN EN 14770-ASTM D7175] The dynamic shear rheometer test system consists of parallel plates, a means for controlling the temperature of the test specimen, a loading device, and a control and data acquisition system.

[0074] [Multiple stress creep recovery test DIN EN 16659-ASTM D7405] This test method was used to determine the presence of elastic response in asphalt binders under shear creep and recovery at two stress levels (0.1 and 3.2 kPa) and a specific temperature (50°C). The test uses a DSR with a load of 25 mm for 1 s at a constant stress, followed by recovery for 9 s. Ten creep and recovery cycles at a creep stress of 0.100 kPa, followed by 10 cycles at a creep stress of 3.200 kPa.

[0075] Potentiometric titration method for determining reactive groups in asphalt

[0076] [Acid value] Approximately 0.5-1 g of sample was dissolved in 50 ml of toluene and titrated potentiometrically with a 0.1 mol / l tetrabutylammonium hydroxide solution. A few drops of water can be added to the titration solution to ensure sufficient conductivity. Blank values ​​were determined in the same way.

[0077] [Base number] Approximately 0.5-1 g of sample was dissolved in 50 ml of toluene and titrated potentiometrically with a 0.1 mol / l trifluoromethanesulfonic acid solution. A few drops of water can be added to the titration solution to ensure sufficient conductivity. Blank values ​​were determined in the same way.

[0078] [Measurement of the particle fraction of asphalt compositions using an analytical ultracentrifuge (AUC)] To determine the particle fraction of the asphalt composition, a fractionation test using analytical ultracentrifugation was performed. Settling velocity tests were performed using a Beckman Optima XL-I (Beckman Instruments, Palo Alto, USA). An integrated scanning UV / VIS absorbance optical system was used. A wavelength of 350 nm was selected. Samples were measured at a concentration of about 0.2 g / L after dilution with white spirit solvent (CAS-Nr.: 64742-82-1). To detect the soluble and insoluble fractions, the centrifugation speed was varied between 1000 rpm and 55,000 rpm. The distribution of sedimentation coefficients, defined as the weight fraction with a sedimentation coefficient between s and s+ds, and the concentration of one sedimentation fraction, were determined using standard analytical software (SEDFIT). The change in the concentration profile over time in the entire radial direction was recorded and converted to a distribution of sedimentation coefficients g. The sedimentation coefficient is in Sved (1 Sved = 10-13 sec). The particulate fraction of the asphalt composition was determined by quantifying the optical absorption of the fast and slow settling fractions at the wavelengths used.

[0079] [Table 1]

[0080] [Table 2]

[0081] [Table 3]

Claims

1. 1. An asphalt composition comprising 0.1 to 10.0 wt. % monomeric MDI based on the total weight of the composition, Monomeric MDI is carbodiimide-modified, The weight percentage of 4,4'-MDI in the carbodiimide-modified monomeric MDI is in the range of 65-85% and the weight percentage of carbodiimide in the carbodiimide-modified monomeric MDI is in the range of 15-35%; and An asphalt composition, wherein the carbodiimide-modified monomeric MDI has a functionality in the range of 2.1 to 2.5 (excluding asphalt compositions that contain a polyurethane polymer and / or a polymer having hydroxyl groups capable of forming a polyurethane polymer with the monomeric MDI).

2. 10. The asphalt composition of claim 1, wherein at least 18% by weight, based on the total weight of the composition, are particles having a sedimentation coefficient in white spirit solvent of greater than 5000 Sved.

3. 3. The bituminous composition of claim 1 or 2, wherein greater than 20% by weight, based on the total weight of the composition, are particles having a sedimentation coefficient in the range of 10,000 to 1,000,000 Sved in white spirit solvent.

4. The asphalt composition according to any one of claims 1 to 3, wherein the carbodiimide-modified monomeric MDI has a viscosity in the range of 20 to 100 mPa·s at 25°C.

5. 5. The asphalt composition according to any one of claims 1 to 4, wherein the amount of carbodiimide modified monomeric MDI is 0.5 to 5.0 wt. %, based on the total weight of the composition.

6. 6. The asphalt composition according to any one of claims 1 to 5, wherein the amount of carbodiimide modified monomeric MDI is 0.8 to 3.0 wt. %, based on the total weight of the composition.

7. The asphalt composition according to any one of claims 1 to 6, wherein the carbodiimide modified monomeric MDI has an iron content in the range of 1 to 80 ppm.

8. Steps below: a) heating the raw asphalt to a temperature of 110-190°C; b) adding a desired amount of monomeric MDI or carbodiimide modified monomeric MDI under stirring; c) after step b), stirring the reaction mixture at a temperature in the range of 110-190° C. for at least 2.5 hours; The method for producing the asphalt composition according to any one of claims 1 to 7, comprising the steps of:

9. The process according to claim 8, wherein the temperatures of steps a) and c) are the same and are in the range of 110-150°C.

10. The process of claim 8 or 9, wherein the reaction mixture is stirred for at least 4 hours after the addition step b).

11. The process according to any one of claims 8 to 10, wherein the completion of the reaction is determined by IR spectroscopy.

12. Use of the asphalt composition according to any one of claims 1 to 7 for preparing an asphalt mix composition.

Citation Information

Patent Citations

  • Polymer-modified bitumen

    EP0537638A1

  • JP1970013959B

  • JP1970013960B

  • Storage of moisture-curable composition

    JP1986126125A

  • Adhesive composition

    JP1998017845A