Composites, polymer electrolytes, electrochemical devices, polymer-based solid-state batteries and actuators
A fluorine-containing copolymer composite with controlled volatile content addresses safety and performance issues in solid-state batteries by providing high ionic conductivity, oxidation resistance, and flame retardancy, ensuring reliable battery operation.
Patent Information
- Application Number
- JP2022518123
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-01
- Filing Date
- 2021-04-28
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-04-28
AI Technical Summary
Conventional polymer-based solid-state batteries suffer from safety issues due to the presence of volatile organic solvents, which limit their operating temperature range and long-term reliability, and lack adequate oxidation resistance and flame retardancy.
A composite electrolyte composed of a fluorine-containing copolymer with specific ratios of tetrafluoroethylene (TFE) and vinylidene fluoride (VdF) units, combined with an alkali metal salt and ionic liquid, minimizing volatile components to less than 0.1% by mass, enhancing oxidation resistance and flame retardancy.
The composite electrolyte provides high ionic conductivity, excellent oxidation resistance, and flame retardancy, ensuring safe and reliable operation of electrochemical devices like solid-state batteries.
Smart Images

Figure 0007575696000004 
Figure 0007575696000001 
Figure 0007575696000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to composites, polymer electrolytes, electrochemical devices, polymer-based solid-state batteries and actuators. [Background technology]
[0002] In recent years, solid electrolytes that exhibit high ionic conductivity comparable to that of non-aqueous electrolytes have been developed, accelerating the development of all-solid-state batteries for practical use.
[0003] Patent Document 1 discloses a polymer electrolyte in which a vinylidene copolymer having a melting point of 80° C. or higher and a crystallinity of 20 to 80%, which consists of 35 to 99 mol % of repeating units derived from vinylidene fluoride, 1 to 50 mol % of repeating units derived from tetrafluoroethylene, and 0 to 20 mol % of a monomer copolymerizable therewith, is impregnated with a nonaqueous electrolyte.
[0004] Patent Document 2 discloses a composition containing a vinylidene fluoride-tetrafluoroethylene copolymer in which 1 to 15 mass % of tetrafluoroethylene is copolymerized, and an organic solvent capable of dissolving a lithium salt. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 1999 / 028916 [Patent Document 2] JP 2001-35534 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present disclosure is to provide a composite that has excellent oxidation resistance and flame retardancy and can be suitably used as an electrolyte, and various electrochemical devices that use the composite. [Means for solving the problem]
[0007] The present disclosure relates to a polymer electrolyte comprising a fluorine-containing copolymer having tetrafluoroethylene (TFE) units and vinylidene fluoride (VdF) units, and a complex containing an alkali metal salt, the content of VdF units in the fluorine-containing copolymer is 60.0 mol % or more and 95.0 mol % or less based on the total monomer units, and the content of TFE units is 5.0 mol % or more and 40.0 mol % or less based on the total monomer units, The present invention relates to a polymer electrolyte comprising a composite having a volatile component content of 0.1% by mass or less based on the entire composite. The above fluorine-containing copolymer preferably further contains 0.1 to 10 mol % of hexafluoropropylene (HFP) units.
[0008] The alkali metal salt is at least one lithium salt selected from LiPF6, LiBF4, LiTFSI, LiFSI, LiPO2F2, and LiBOB; The content of the above alkali metal salt is preferably from 0.1 to 90% by mass relative to the fluorine-containing copolymer.
[0009] The above complex may further include, as an organic cation, a 1-butyl-3-methylimidazolium (BMI) cation or an N-methyl-N-butyl-pyrrolidium (Pyr14) cation; The anion includes at least one ionic liquid selected from a combination of a BF4 anion and a bis(trifluoromethanesulfonyl)imide (TFSI) anion; The content of the ionic liquid is preferably 1.0 to 500% by mass relative to the fluorine-containing copolymer.
[0010] The present disclosure also relates to a polymer electrolyte comprising the above-mentioned composite. The present disclosure also relates to an electrochemical device comprising the above-mentioned polymer electrolyte. The present disclosure also relates to a polymer-based solid-state battery comprising the above-mentioned polymer electrolyte. The polymer-based solid battery is preferably a lithium-ion secondary battery. The present disclosure also relates to an actuator comprising the above-mentioned polymer electrolyte. Effect of the Invention
[0011] The composite of the present disclosure is a copolymer composition that has excellent oxidation resistance, flame retardancy, and the like, and can therefore be suitably used as an electrolyte in electrochemical devices such as solid secondary batteries. [Brief description of the drawings]
[0012] [Figure 1] 1 shows data on oxidation resistance tests for Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present disclosure will be described in detail below. In recent years, polymer-based solid batteries have been developed as a type of solid-state battery. The polymer-based solid battery is usually equipped with a polymer electrolyte that is made of a polymer, an electrolyte, an additive, a plasticizer, an electrolytic solution, etc., and has the advantage of being highly safe since there is no risk of leakage.
[0014] Fluorine-containing polymers have also been developed as polymers used in the above-mentioned polymer electrolytes. Fluorine-containing polymers are components with excellent oxidation resistance, flame retardancy, etc., and therefore have the advantages of being less likely to ignite and being applicable to the roll-to-roll method. The present disclosure aims to develop a composite that has the performance of a fluorine-containing polymer and is also excellent in safety.
[0015] The composite of the present disclosure contains a fluorine-containing copolymer containing 1 to 99 mol% in total of tetrafluoroethylene (TFE) units and vinylidene fluoride (VdF) units, and has a volatile content of 0.1 mass% or less, thereby providing excellent oxidation resistance and flame retardancy. The electrolyte of the conventional polymer solid battery described in Patent Document 2 contains a large amount of volatile components due to swelling of the volatile organic solvent, and thus has safety problems. The composite of the present disclosure will be described in detail below.
[0016] The composite of the present disclosure is a composite containing a fluorinated copolymer and an alkali metal salt. The fluorine-containing copolymer contains tetrafluoroethylene (TFE) units and vinylidene fluoride (VdF) units, and the total content of the TFE units and the VdF units is 1 to 99 mol %. The total content is preferably 10 mol % or more, and more preferably 20 mol % or more.
[0017] The content of VdF units in the fluorine-containing copolymer is preferably 60.0 mol% or more, more preferably 65.0 mol% or more, even more preferably 70.0 mol% or more, particularly preferably 75.0 mol% or more, preferably 95.0 mol% or less, and most preferably 90.0 mol% or less, based on all monomer units.
[0018] The content of TFE units in the fluorine-containing copolymer is preferably 5.0 mol% or more, more preferably 8.0 mol% or more, particularly preferably 10.0 mol% or more, and preferably 40.0 mol% or less, more preferably 38.0 mol% or less, particularly preferably 35.0 mol% or less, based on all monomer units.
[0019] In the present disclosure, the composition of the fluorine-containing copolymer is, for example, 19 It can be measured by F-NMR measurement.
[0020] In the above fluorocopolymer, the molar ratio of VdF units to TFE units (VdF units / TFE units) is preferably 60 / 40 to 90 / 10. By setting the molar ratio within the above range, a fluorocopolymer that can be easily processed into a film can be obtained.
[0021] The fluorine-containing copolymer may further contain other fluorinated monomer units. As the fluorinated monomer (excluding the above-mentioned TFE and VdF), at least one selected from the group consisting of vinyl fluoride, trifluoroethylene, chlorotrifluoroethylene (CTFE), fluoroalkyl vinyl ether, hexafluoropropylene (HFP), (perfluoroalkyl)ethylene, 2,3,3,3-tetrafluoropropene and trans-1,3,3,3-tetrafluoropropene is preferred, at least one selected from the group consisting of CTFE and HFP is more preferred, and HFP is particularly preferred.
[0022] These fluorinated monomer units may or may not have polar groups. The fluorine-containing copolymer may further contain a non-fluorinated monomer unit.
[0023] The molar ratio of VdF units to TFE units (VdF units / TFE units) in the fluorine-containing copolymer is preferably 60 / 40 to 95 / 5, more preferably 60 / 40 to 90 / 10, still more preferably 63 / 37 to 88 / 12, particularly preferably 70 / 30 to 88 / 12, and most preferably 75 / 25 to 88 / 12.
[0024] The mass average molecular weight (polystyrene equivalent) of the fluorine-containing copolymer is preferably from 10,000 to 7,200,000, and more preferably from 20,000 to 6,600,000. The mass average molecular weight can be measured by gel permeation chromatography (GPC) at 50° C. using dimethylformamide as a solvent.
[0025] The number average molecular weight (polystyrene equivalent) of the fluorine-containing copolymer is preferably from 10,000 to 1,200,000, and more preferably from 40,000 to 1,100,000. The number average molecular weight can be measured by gel permeation chromatography (GPC) at 50° C. using dimethylformamide as a solvent.
[0026] The melting point of the fluorocopolymer is preferably 100 to 240° C. The melting point can be determined as the temperature corresponding to the maximum value on the heat of fusion curve when the temperature is increased at a rate of 10° C. / min using a differential scanning calorimetry (DSC) device.
[0027] The fluorine-containing copolymer may be used alone or in combination with two or more kinds. In particular, it may be used in a form in which two kinds of copolymers having different molecular structures are used in combination. Examples of the form in which two kinds of copolymers having different molecular structures are used in combination include a form in which two kinds of copolymers (I) having different molecular structures are used, a form in which two kinds of copolymers (II) having different molecular structures are used, and a form in which one kind of copolymer (I) and one kind of copolymer (II) are used in combination.
[0028] (alkali metal salts) The complexes of the present disclosure are those that contain an alkali metal salt. The alkali metal salt can be represented by MX, where M is an alkali metal and X is a substance that serves as a counter anion. The above alkali metal salts may be used alone or in the form of a mixture of two or more kinds. The alkali metal salt is particularly preferably a lithium salt (that is, a compound represented by LiX).
[0029] Any lithium salt can be used as the lithium salt, and specific examples include the following: LiPF6, LiBF4, LiClO4, LiAlF4, LiSbF6, LiTaF6, LiWF7, LiAsF6, LiAlCl4, LiI, LiBr, LiCl, LiB 10 Cl 10 Inorganic lithium salts such as Li2SiF6, Li2PFO3, and LiPO2F2; Lithium tungstates such as LiWOF5; Lithium carboxylates such as HCO2Li, CH3CO2Li, CH2FCO2Li, CHF2CO2Li, CF3CO2Li, CF3CH2CO2Li, CF3CF2CO2Li, CF3CF2CF2CO2Li, and CF3CF2CF2CF2CO2Li; Lithium salts having an S=O group, such as FSO3Li, CH3SO3Li, CH2FSO3Li, CHF2SO3Li, CF3SO3Li, CF3CF2SO3Li, CF3CF2CF2SO3Li, CF3CF2CF2CF2SO3Li, lithium methyl sulfate, lithium ethyl sulfate (C2H5OSO3Li), and lithium 2,2,2-trifluoroethyl sulfate; Lithium imide salts such as LiTFSI, LiFSI, LiN(FCO)2, LiN(FCO)(FSO2), LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium bisperfluoroethanesulfonylimide, lithium cyclic 1,2-perfluoroethanedisulfonylimide, lithium cyclic 1,3-perfluoropropanedisulfonylimide, lithium cyclic 1,2-ethanedisulfonylimide, lithium cyclic 1,3-propanedisulfonylimide, lithium cyclic 1,4-perfluorobutanedisulfonylimide, LiN(CF3SO2)(FSO2), LiN(CF3SO2)(C3F7SO2), LiN(CF3SO2)(C4F9SO2), and LiN(POF2)2; Lithium methide salts such as LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3; Others, Formula: LiPF a (C n F 2n+1 ) 6-a(wherein a is an integer of 0 to 5, and n is an integer of 1 to 6) (e.g., LiPF3(C2F5)3, LiPF3(CF3)3, LiPF3(iso-C3F7)3, LiPF5(iso-C3F7), LiPF4(CF3)2, LiPF4(C2F5)2), LiPF4(CF3SO2)2, LiPF4(C2F5SO2), LiBF Fluorine-containing organic lithium salts such as 3CF3, LiBF3C2F5, LiBF3C3F7, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, LiBF2(C2F5SO2)2, LiBOB, LiTDI, LiSCN, LiB(CN)4, LiB(C6H5)4, Li2(C2O4), LiP(C2O4)3, Li2B 12 F b H 12-b (b is an integer of 0 to 3), etc.
[0030] Among them, LiPF6, LiBF4, LiSbF6, LiTaF6, LiPO2F2, FSO3Li, CF3SO3Li, LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium cyclic 1,2-perfluoroethane disulfonylimide, lithium cyclic 1,3-perfluoropropane disulfonylimide, LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5 SO2)3, LiBF3CF3, LiBF3C2F5, LiPF3(CF3)3, LiPF3(C2F5)3, LiTFSI, LiFSI, LiBOB, LiTDI, and the like are particularly preferred because they have the effect of improving output characteristics, high-rate charge / discharge characteristics, high-temperature storage characteristics, cycle characteristics, and the like, and at least one lithium salt selected from the group consisting of LiPF6, LiBF4, LiTFSI, LiFSI, LiPO2F2, and LiBOB is most preferred.
[0031] These electrolyte salts may be used alone or in combination of two or more. A preferred example of a combination of two or more is the combination of LiPF6 and LiBF4, which has the effect of improving high-temperature storage characteristics, load characteristics, and cycle characteristics.
[0032] In the composite of the present disclosure, the amount of the alkali metal salt is preferably 0.1% by mass or more, more preferably 1.0% by mass or more, relative to the fluorocopolymer, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0033] Another example is the combined use of an inorganic lithium salt and an organic lithium salt, which has the effect of suppressing deterioration due to high-temperature storage. The organic lithium salt is preferably CF3SO3Li, LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, lithium cyclic 1,2-perfluoroethane disulfonylimide, lithium cyclic 1,3-perfluoropropane disulfonylimide, LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiBF3CF3, LiBF3C2F5, LiPF3(CF3)3, LiPF3(C2F5)3, etc. In this case, the ratio of the organic lithium salt to the entire complex (100 mass%) is preferably 0.1 mass% or more, particularly preferably 0.5 mass% or more, and preferably 30 mass% or less, particularly preferably 20 mass% or less.
[0034] The concentration of these alkali metal salts in the composite is not particularly limited as long as it does not impair the effects of the present disclosure. In order to keep the electrical conductivity of the composite in a good range and ensure good battery performance, the total molar concentration of lithium in the composite is preferably 0.3 mol / L or more, more preferably 0.4 mol / L or more, even more preferably 0.5 mol / L or more, and is preferably 5.0 mol / L or less, more preferably 4.5 mol / L or less, even more preferably 4.0 mol / L or less.
[0035] If the total molar concentration of lithium is too low, the electrical conductivity of the composite may be insufficient, whereas if the concentration is too high, the electrical conductivity may decrease due to increased viscosity, which may result in reduced battery performance.
[0036] (Ionic Liquid) The composite of the present disclosure may further include an ionic liquid. The "ionic liquid" is a liquid consisting of ions that combine organic cations and anions. By including an ionic liquid, the ionic conductivity can be increased. In addition, another preferable feature is that it has almost no vapor pressure and is non-flammable.
[0037] The organic cation is not particularly limited, but examples thereof include imidazolium ions such as dialkylimidazolium cations and trialkylimidazolium cations; tetraalkylammonium ions; alkylpyridinium ions; dialkylpyrrolidinium ions; and dialkylpiperidinium ions.
[0038] The anions that serve as counters to these organic cations are not particularly limited, but examples thereof that can be used include PF6 anion, PF3(C2F5)3 anion, PF3(CF3)3 anion, BF4 anion, BF2(CF3)2 anion, BF3(CF3) anion, bisoxalatoborate anion, P(C2O4)F2 anion, Tf (trifluoromethanesulfonyl) anion, Nf (nonafluorobutanesulfonyl) anion, bis(fluorosulfonyl)imide anion, bis(trifluoromethanesulfonyl)imide (TFSI) anion, bis(pentafluoroethanesulfonyl)imide anion, dicyanoamine anion, and halide anions.
[0039] The ionic liquid is preferably at least one selected from a combination of an organic cation such as 1-butyl-3-methylimidazolium (BMI) cation or N-methyl-N-butyl-pyrrolidinium (Pyr14) cation and an anion such as a BF4 anion, a bis(fluorosulfonyl)imide (FSI) anion, or a bis(trifluoromethanesulfonyl)imide (TFSI) anion. Among these, TFSI is particularly preferred.
[0040] The content of the ionic liquid is preferably 1.0 to 500% by mass relative to the fluorine-containing copolymer, more preferably 10% by mass, and more preferably 300% by mass.
[0041] (Other additives) As other additives, metal fillers such as TiO2 and Al2O3 may be added to improve electrical conductivity. The content of the additives is preferably 0.1 to 10 mass% relative to the fluorine-containing copolymer, and more preferably 0.2 to 5 mass%.
[0042] The composite of the present disclosure has a volatile component content of 0.1 mass % or less based on the entire composite. By having such an extremely low volatile component content, it has the advantage of long-term reliability.
[0043] The composite of the present disclosure is preferably flame retardant, which is particularly preferable since it can be safely used in various electrochemical devices. The term "flame retardant" means that, in the flame retardancy evaluation in the examples described in detail below, the evaluation result shows that there was no flame spread from an open flame.
[0044] By setting the amount of volatile components to 0.1% by mass or less, the composite has high ionic conductivity, excellent oxidation resistance, flame retardancy, heat resistance, and film-forming properties. Polymer compositions that have been used as electrolytes for polymer-based solid batteries up to now have a volatile component amount of about 10% by mass, which is more than the composite of the present disclosure. For this reason, the composite has disadvantages such as a limited operating temperature range and poor long-term reliability.
[0045] The method for adjusting the amount of volatile components in the composite to fall within the above range is not particularly limited, and examples thereof include a method in which the composite film obtained in a thin film form is heated under reduced pressure and dried. The amount of volatile components in this disclosure is a value determined by the method described later in the examples.
[0046] (Manufacturing method) The method for producing the above-mentioned composite is not particularly limited, and the composite can be prepared by any method. For example, the composite can be obtained by dispersing the above-mentioned fluorine-containing copolymer, an alkali metal salt, an ionic liquid, and, if necessary, additives in a solvent, and applying the obtained dispersion in the form of a thin film.
[0047] The solvent for forming such a dispersion liquid is not particularly limited in type as long as it is a solvent capable of dissolving or dispersing each of the above-mentioned components, and either an aqueous solvent or an organic solvent may be used. Examples of aqueous solvents include water and a mixture of alcohol and water. Examples of organic solvents include aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; and aprotic polar solvents such as hexamethylphosphatamide and dimethylsulfoxide. Alternatively, it can be produced by kneading the fluorine-containing copolymer, the alkali metal salt, the ionic liquid, and, if necessary, additives, etc., without using a solvent, and then molding the mixture.
[0048] (Electrochemical Devices) The composite of the present disclosure can be suitably used as an electrolyte for various electrochemical devices. The present disclosure also includes an electrochemical device including a polymer electrolyte made of the composite. The electrochemical device is not particularly limited, and may be applied to conventionally known electrochemical devices, specifically, secondary batteries such as lithium ion batteries, primary batteries such as lithium batteries, sodium ion batteries, magnesium ion batteries, radical batteries, solar cells (particularly dye-sensitized solar cells), and fuel cells; Capacitors such as lithium ion capacitors, hybrid capacitors, electrochemical capacitors, and electric double layer capacitors; actuators such as cylinders, rocking motors, and motors; Various capacitors such as aluminum electrolytic capacitors and tantalum electrolytic capacitors; Examples of the electrochemical element include an electrochemical element, an electrochemical switching element, and various electrochemical sensors.
[0049] In particular, the present invention can be suitably used in secondary batteries that have a high capacity and large output, and therefore undergo a large change in volume due to the movement of a large amount of metal ions.
[0050] (Secondary solid battery) The present disclosure also relates to a secondary solid-state battery comprising the above-described composite of the present disclosure as a polymer electrolyte. The secondary solid-state battery of the present disclosure is a polymer-based solid-state battery including a positive electrode and a negative electrode each composed of a positive electrode or negative electrode active material, a binder, and a current collector, and a polymer electrolyte layer composed of the above-mentioned composite interposed between the positive electrode and the negative electrode. Such a secondary solid-state battery is preferably a lithium-ion battery.
[0051] The positive electrode active material and the negative electrode active material are not particularly limited, and examples thereof include those used in known electrochemical devices such as secondary batteries, such as lead batteries, nickel-cadmium batteries, nickel-metal hydride batteries, lithium ion batteries, and alkali metal sulfur batteries, and electric double layer capacitors.
[0052] (positive electrode) The positive electrode active material is not particularly limited, and may be one used in known electrochemical devices. To explain the positive electrode active material of the lithium ion secondary battery in detail, it is not particularly limited as long as it can electrochemically absorb and release lithium ions, and may be, for example, a lithium-containing transition metal composite oxide, a lithium-containing transition metal phosphate compound, a sulfur-based material, or a conductive polymer. Among them, the positive electrode active material is preferably a lithium-containing transition metal composite oxide or a lithium-containing transition metal phosphate compound, and in particular, a lithium-containing transition metal composite oxide that produces a high voltage is preferred.
[0053] The transition metal of the lithium-containing transition metal composite oxide is preferably V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc., and specific examples of the lithium transition metal composite oxide include lithium-cobalt composite oxides such as LiCoO2, lithium-nickel composite oxides such as LiNiO2, lithium-manganese composite oxides such as LiMnO2, LiMn2O4, and Li2MnO3, and those in which a part of the transition metal atoms that are the main components of these lithium transition metal composite oxides is replaced with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, and Si. Examples of the above-mentioned replacements include lithium-nickel-manganese composite oxide, lithium-nickel-cobalt-aluminum composite oxide, lithium-nickel-cobalt-manganese composite oxide, lithium-manganese-aluminum composite oxide, and lithium-titanium composite oxide, and more specifically, LiNi 0.5 Mn 0.5 O2, LiNi 0.85 Co 0.10 Al 0.05 O2, LiNi 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, LiMn 1.8 Al0.2 O4, LiMn 1.5 Ni 0.5 O4, Li4Ti5O 12 , LiNi 0.82 Co 0.15 Al 0.03 O2, etc.
[0054] The transition metal of the lithium-containing transition metal phosphate compound is preferably V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc., and specific examples of the lithium-containing transition metal phosphate compound include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7, cobalt phosphates such as LiCoPO4, and lithium transition metal phosphate compounds in which a part of the transition metal atoms that constitute the main components of these lithium transition metal phosphate compounds has been substituted with other metals such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Nb, Si, etc.
[0055] In particular, from the viewpoints of high voltage, high energy density, charge / discharge cycle characteristics, etc., LiCoO2, LiNiO2, LiMn2O4, LiNi 0.82 Co 0.15 Al 0.03 O2, LiNi 0.33 Mn 0.33 Co 0.33 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, LiFePO4 are preferred.
[0056] The sulfur-based material may be, for example, a material containing a sulfur atom, and is preferably at least one selected from the group consisting of elemental sulfur, metal sulfides, and organic sulfur compounds, and more preferably elemental sulfur. The metal sulfide may be a metal polysulfide. The organic sulfur compound may be an organic polysulfide.
[0057] The above metal sulfides include LiSx A compound represented by (0 < x ≤ 8); Li2S x A compound represented by (0 < x ≤ 8); a compound having a two-dimensional layered structure such as TiS2 or MoS2; general formula Me x Examples include Chevrel compounds having a strong three-dimensional skeletal structure represented by Mo6S8 (Me is various transition metals including Pb, Ag, Cu, etc.).
[0058] Examples of the above organic sulfur compound include carbon sulfide compounds and the like.
[0059] The above organic sulfur compound may be supported on a material having pores such as carbon and used as a carbon composite material. As the sulfur content in the carbon composite material, since the cycle performance is further excellent and the overvoltage is further reduced, 10 to 99% by mass is preferable with respect to the above carbon composite material, 20% by mass or more is more preferable, 30% by mass or more is still more preferable, 40% by mass or more is particularly preferable, and 85% by mass or less is preferable. When the above positive electrode active material is the above sulfur simple substance, the sulfur content contained in the above positive electrode active material is equal to the content of the above sulfur simple substance.
[0060] Examples of the conductive polymer include p-doping type conductive polymers and n-doping type conductive polymers. Examples of the conductive polymer include polyacetylene-based, polyphenylene-based, heterocyclic polymers, ionic polymers, ladder and network polymers, etc.
[0061] In the present disclosure, one kind of positive electrode active material may be used alone, or two or more kinds having different compositions or different powder physical properties may be used in combination at an arbitrary combination and ratio.
[0062] The above positive electrode preferably further contains a binder, a thickener, a conductive assistant, etc. Any material can be used as the binder as long as it is safe against the solvent and electrolyte used in the production of the electrodes. Examples of the binder include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, SBR (styrene-butadiene rubber), isoprene rubber, butadiene rubber, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, NBR (acrylonitrile-butadiene rubber), fluororubber, ethylene-propylene rubber, styrene-butadiene rubber, etc. Examples of such materials include styrene block copolymers or hydrogenated products thereof, EPDM (ethylene-propylene-diene terpolymer), styrene-ethylene-butadiene-ethylene copolymer, styrene-isoprene-styrene block copolymers or hydrogenated products thereof, syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymer, propylene-α-olefin copolymer, polyvinylidene fluoride, vinylidene fluoride-tetrafluoroethylene copolymer, tetrafluoroethylene-ethylene copolymer, polymer compositions having ionic conductivity for alkali metal ions (especially lithium ions), etc. These materials may be used alone or in any combination and ratio of two or more.
[0063] The content of the binder is usually 0.1% by mass or more, preferably 1% by mass or more, more preferably 1.5% by mass or more, and usually 80% by mass or less, preferably 60% by mass or less, more preferably 40% by mass or less, and most preferably 10% by mass or less, as the ratio of the binder in the positive electrode active material layer. If the ratio of the binder is too low, the positive electrode active material cannot be sufficiently held, resulting in insufficient mechanical strength of the positive electrode, which may deteriorate the battery performance such as cycle characteristics. On the other hand, if the ratio is too high, it may lead to a decrease in battery capacity and conductivity.
[0064] Examples of the thickener include carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. One type may be used alone, or two or more types may be used in any combination and ratio.
[0065] The ratio of the thickener to the positive electrode active material is usually 0.1% by mass or more, preferably 0.2% by mass or more, more preferably 0.3% by mass or more, and usually 5% by mass or less, preferably 3% by mass or less, more preferably 2% by mass or less. If it is below this range, the coating property may be significantly reduced. If it is above this range, the ratio of the active material in the positive electrode active material layer may decrease, causing problems such as a decrease in the capacity of the battery and an increase in the resistance between the positive electrode active materials.
[0066] The conductive assistant is not particularly limited as long as it can improve the conductivity of the electrolyte, and examples thereof include carbon black such as acetylene black and ketjen black; carbon fibers such as multi-walled carbon nanotubes, single-walled carbon nanotubes, carbon nanofibers, graphene, and vapor grown carbon fibers (VGCF); metal powders such as SUS powder and aluminum powder; and the like.
[0067] (Negative electrode) The negative electrode is composed of a negative electrode active material layer containing a negative electrode active material and a current collector. The negative electrode active material is not particularly limited, and may be any material used in known electrochemical devices. The negative electrode active material of the lithium ion secondary battery is specifically described as being not particularly limited as long as it can electrochemically absorb and release lithium ions. Specific examples include carbonaceous materials, alloy-based materials, lithium-containing metal composite oxide materials, conductive polymers, and the like. These may be used alone or in any combination of two or more.
[0068] As the carbonaceous material capable of absorbing and releasing lithium, artificial graphite or purified natural graphite produced by high-temperature treatment of graphitizable pitch obtained from various raw materials, or those obtained by subjecting these graphites to surface treatment with pitch or other organic matter and then carbonizing them are preferred, and those selected from natural graphite, artificial graphite, artificial carbonaceous material, and carbonaceous material obtained by heat-treating artificial graphite material at least once in the range of 400 to 3200 ° C, carbonaceous material in which the negative electrode active material layer is made of carbonaceous material having at least two or more different types of crystallinity and / or has an interface where the carbonaceous material having the different crystallinity is in contact, and carbonaceous material in which the negative electrode active material layer has an interface where the carbonaceous material having at least two or more different orientations is in contact are more preferred, as they have a good balance between initial irreversible capacity and high current density charge / discharge characteristics. Moreover, these carbonaceous materials may be used alone or in any combination and ratio of two or more.
[0069] Examples of carbonaceous materials obtained by heat-treating the above-mentioned artificial carbonaceous substances and artificial graphite substances at least once in the range of 400 to 3200°C include carbon nanotubes, graphene, coal-based coke, petroleum-based coke, coal-based pitch, petroleum-based pitch, and these pitches that have been oxidized, needle coke, pitch coke, and carbon agents obtained by partially graphitizing these, furnace black, acetylene black, pitch-based carbon fiber, and other organic substances that can be carbonized and their charcoals, or solutions in which carbonizable organic substances are dissolved in low-molecular organic solvents such as benzene, toluene, xylene, quinoline, and n-hexane, and their charcoals, etc.
[0070] The metal material (excluding lithium titanium composite oxide) used as the negative electrode active material is not particularly limited, and may be any of lithium alone, elemental metals and alloys forming lithium alloys, or compounds such as oxides, carbides, nitrides, silicides, sulfides, or phosphides thereof, so long as it is capable of absorbing and releasing lithium. The elemental metals and alloys forming lithium alloys are preferably materials containing metal or semimetal elements of Groups 13 and 14, and more preferably elemental metals of aluminum, silicon, and tin (hereinafter abbreviated as "specific metal elements") and alloys or compounds containing these atoms. These may be used alone or in any combination and ratio of two or more.
[0071] Examples of the negative electrode active material having at least one atom selected from the specific metal elements include a single metal of any one of the specific metal elements, an alloy of two or more specific metal elements, an alloy of one or more specific metal elements and one or more other metal elements, and a compound containing one or more specific metal elements, and a composite compound such as an oxide, carbide, nitride, silicide, sulfide, or phosphide of the compound. By using these single metals, alloys, or metal compounds as the negative electrode active material, it is possible to increase the capacity of the battery.
[0072] Any conventionally known metal particles that can be alloyed with Li can be used, but from the viewpoint of capacity and cycle life, the metal particles are preferably a metal or a compound thereof selected from the group consisting of Fe, Co, Sb, Bi, Pb, Ni, Ag, Si, Sn, Al, Zr, Cr, P, S, V, Mn, Nb, Mo, Cu, Zn, Ge, In, Ti, etc. Also, an alloy consisting of two or more metals may be used, and the metal particles may be alloy particles formed of two or more metal elements. Among these, a metal or a metal compound thereof selected from the group consisting of Si, Sn, As, Sb, Al, Zn, and W is preferred. Examples of the metal compound include metal oxides, metal nitrides, metal carbides, etc. In addition, an alloy made of two or more metals may be used.
[0073] In addition, the above-mentioned composite compounds may be compounds in which the above-mentioned composite compounds are intricately bonded with several elements such as simple metals, alloys, or nonmetallic elements. Specifically, for example, in the case of silicon or tin, alloys of these elements and metals that do not function as negative electrodes can be used. For example, in the case of tin, complex compounds containing 5 to 6 elements in combination with a metal that acts as a negative electrode other than tin and silicon, a metal that does not function as a negative electrode, and a nonmetallic element can also be used.
[0074] Among metal particles that can be alloyed with Li, Si or a Si metal compound is preferred. The Si metal compound is preferably a Si metal oxide. Si or a Si metal compound is preferred in terms of increasing capacity. In this specification, Si or a Si metal compound is collectively referred to as a Si compound. Specific examples of the Si compound include SiOx, SiNx, SiCx, and SiZxOy (Z=C, N). The Si compound is preferably a Si metal oxide, which is generally represented by SiOx. This general formula SiOx is obtained from Si dioxide (SiO2) and metal Si (Si), and the value of x is usually 0≦x<2. SiOx has a larger theoretical capacity than graphite, and furthermore, amorphous Si or nano-sized Si crystals are easy for alkali ions such as lithium ions to enter and exit, making it possible to obtain a high capacity. Specifically, the Si metal oxide is represented as SiOx, where x is 0≦x<2, more preferably 0.2 or more and 1.8 or less, even more preferably 0.4 or more and 1.6 or less, particularly preferably 0.6 or more and 1.4 or less, and it is particularly preferable that X = 0. Within this range, it is possible to achieve high capacity and at the same time reduce irreversible capacity due to the bond between Li and oxygen.
[0075] Also, there is a composite material containing Si or Sn as the first constituent element, as well as a second and a third constituent element. The second constituent element is, for example, at least one of cobalt, iron, magnesium, titanium, vanadium, chromium, manganese, nickel, copper, zinc, gallium, and zirconium. The third constituent element is, for example, at least one of boron, carbon, aluminum, and phosphorus.
[0076] The lithium-containing metal composite oxide material used as the negative electrode active material is not particularly limited as long as it can absorb and release lithium, but from the viewpoint of high current density charge / discharge characteristics, a material containing titanium and lithium is preferred, more preferably a lithium-containing composite metal oxide material containing titanium, and further preferably a composite oxide of lithium and titanium (hereinafter abbreviated as "lithium titanium composite oxide"). That is, when a lithium titanium composite oxide having a spinel structure is contained in a negative electrode active material for a battery and used, the output resistance is significantly reduced, and therefore it is particularly preferred.
[0077] The lithium titanium composite oxide may be represented by the general formula: Li x Ti y M z O4 [In the formula, M represents at least one element selected from the group consisting of Na, K, Co, Al, Fe, Ti, Mg, Cr, Ga, Cu, Zn, and Nb.] It is preferable that the compound is represented by the following formula: Among the above compositions, (i)1.2≦x≦1.4, 1.5≦y≦1.7, z=0 (ii)0.9≦x≦1.1, 1.9≦y≦2.1, z=0 (iii)0.7≦x≦0.9, 2.1≦y≦2.3, z=0 The structure of is particularly preferred because it has a good balance of battery performance.
[0078] A particularly preferred representative composition of the above compound is (i) Li 4 / 3 Ti 5 / 3 O4, (ii) Li1Ti2O4, (iii) Li4 / 5 Ti 11 / 5 O4. For structures with Z≠0, for example, Li 4 / 3 Ti 4 / 3 Al 1 / 3 O4 is mentioned as being preferred.
[0079] The negative electrode preferably further contains a binder, a thickener, and a conductive assistant.
[0080] The binder may be the same as the binder that can be used for the positive electrode. The ratio of the binder to the negative electrode active material is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, particularly preferably 0.6% by mass or more, and preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, and particularly preferably 8% by mass or less. If the ratio of the binder to the negative electrode active material exceeds the above range, the ratio of the binder that does not contribute to the battery capacity increases, which may lead to a decrease in the battery capacity. If the ratio is below the above range, the strength of the negative electrode may be decreased.
[0081] In particular, when the binder contains a rubber-like polymer such as SBR as a main component, the ratio of the binder to the negative electrode active material is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 0.6% by mass or more, and usually 5% by mass or less, preferably 3% by mass or less, and more preferably 2% by mass or less. When the binder contains a fluorine-based polymer such as polyvinylidene fluoride as a main component, the ratio of the binder to the negative electrode active material is usually 1% by mass or more, preferably 2% by mass or more, and more preferably 3% by mass or more, and usually 15% by mass or less, preferably 10% by mass or less, and more preferably 8% by mass or less. When the binder contains a non-fluorine-based polymer such as polyacrylic acid as a main component, the ratio of the binder to the negative electrode active material is usually 0.1% by mass or more, preferably 0.5% by mass or more, and more preferably 0.6% by mass or more, and usually 5% by mass or less, preferably 3% by mass or less, and more preferably 2% by mass or less.
[0082] The thickener may be the same as the thickener that can be used for the positive electrode. The ratio of the thickener to the negative electrode active material is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 0.6% by mass or more, and usually 5% by mass or less, preferably 3% by mass or less, and more preferably 2% by mass or less. If the ratio of the thickener to the negative electrode active material is below the above range, the coating property may be significantly reduced. If the ratio exceeds the above range, the ratio of the negative electrode active material in the negative electrode active material layer may be reduced, causing a problem of a decrease in the capacity of the battery and an increase in the resistance between the negative electrode active materials.
[0083] The conductive assistant is not particularly limited as long as it can improve the conductivity of the electrolyte, and examples thereof include the same thickeners as those that can be used in the positive electrode described above.
[0084] Examples of the current collectors (positive and negative current collectors) include metal foils or metal meshes of iron, stainless steel, copper, aluminum, nickel, titanium, etc. Among these, the positive current collector is preferably aluminum foil, and the negative current collector is preferably copper foil.
[0085] (Manufacturing method of secondary solid state battery) The method for producing the secondary solid-state battery of the present disclosure is not particularly limited, and the battery can be produced by a conventionally known method. For example, the electrode can be produced by dispersing and mixing the above-mentioned electrode active material in a solution or dispersion in which a binder is dissolved or dispersed in a dispersion medium to prepare an electrode mixture. The obtained electrode mixture is uniformly applied to a current collector such as a metal foil or a metal net, dried, and pressed as necessary to form a thin electrode mixture layer on the current collector to form a thin-film electrode.
[0086] In addition, for example, the binder and the electrode active material may be mixed first, and then the dispersion medium may be added to prepare a mixture. Alternatively, the binder and the electrode active material may be heated and melted, extruded with an extruder to prepare a thin mixture, and then attached to a collector coated with a conductive adhesive or a general-purpose organic solvent to prepare an electrode sheet. Furthermore, a solution or dispersion of the binder may be applied to a preformed electrode active material. EXAMPLES
[0087] The present disclosure will now be described in detail with reference to examples. In the following examples, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0088] Preparation Example 1 In a SUS polymerization tank with a stirrer having an internal volume of 4 L, 1352 g of pure water prepared with 1 mass% emulsifier F(CF2)5COONH4 was placed and sealed. After vacuum nitrogen replacement, the tank was evacuated and ethane equivalent to 400 cc as a chain transfer agent was charged while vacuum suction using a syringe. Then, while stirring at 70 °C and 450 rpm, a mixed gas monomer with a VDF / TFE / HFP composition ratio of 50 / 38 / 12 mol% was charged into the tank up to 0.9 MPaG. Then, the reaction was started by pressing in an aqueous solution of 137.2 mg of APS (ammonium persulfate) dissolved in 10 g of water with nitrogen. The reaction was started again with 10 g of water with nitrogen so that no liquid remained in the middle of the reaction tube. A mixed monomer with a VDF / TFE / HFP composition ratio of 60 / 35 / 5 mol% was additionally charged to maintain the pressure in the tank. When the amount of added monomer reached 73 g, the stirring speed was slowed down and the gas in the tank was blown out to terminate the reaction. The tank was cooled and the contents were collected in a container. The reaction product was washed with water and dried to obtain 72 g of a white powder of fluorocopolymer 2. The resulting fluorocopolymer 1 had the following composition and physical properties. VdF / TFE / HFP=60.1 / 34.8 / 5.1 (mol%) Number average molecular weight: 82300 Mass average molecular weight: 165000
[0089] Preparation Example 2 1.3 kg of pure water was put into an autoclave with an internal volume of 4 L, and after sufficient nitrogen replacement, 1.3 kg of octafluorocyclobutane was charged, and the system was kept at 37 ° C. and agitation speed of 580 rpm. Then, 200 g of a mixed gas of TFE / VdF = 6 / 94 mol % and 0.4 g of ethyl acetate were charged, and then 1 g of a 50 mass % methanol solution of di-n-propyl peroxydicarbonate was added to start polymerization. Since the pressure in the system decreased with the progress of polymerization, a mixed gas of TFE / VdF = 19 / 81 mol % was continuously fed to maintain the pressure in the system at 1.3 MPaG. Stirring was continued for 11 hours. Then, the pressure was released to return to atmospheric pressure, and the reaction product was washed with water and dried to obtain 130 g of a white powder of fluorine-containing copolymer 2. The resulting fluoropolymer 2 had the following composition and physical properties. VdF / TFE=80.0 / 20.0 (mol%) Number average molecular weight: 283000 Mass average molecular weight: 795000
[0090] Preparation Example 3 1.9 kg of pure water was put into an autoclave with an internal volume of 6 L, and after sufficient nitrogen replacement, 1.8 kg of octafluorocyclobutane was charged, and the system was kept at 37 ° C. and agitation speed of 580 rpm. Then, 260 g of a mixed gas of TFE / VdF = 5 / 95 mol % and 0.6 g of ethyl acetate were charged, and then 2.8 g of a 50 mass % methanol solution of di-n-propyl peroxydicarbonate was added to start polymerization. Since the pressure in the system decreased with the progress of polymerization, a mixed gas of TFE / VdF = 5 / 85 mol % was continuously fed to keep the pressure in the system at 1.3 MPaG. Stirring was continued for 32 hours. Then, the pressure was released to return to atmospheric pressure, and the reaction product was washed with water and dried to obtain 900 g of a white powder of fluorine-containing copolymer 3. The resulting fluorine-containing copolymer 3 had the following composition and physical properties. VdF / TFE=83.0 / 17.0 (mol%) Number average molecular weight: 270000 Mass average molecular weight: 870000
[0091] Preparation Example 4 Fluorine-containing copolymer 4 was prepared with reference to Preparation Example 2. The obtained fluorine-containing copolymer 4 had the following composition and physical properties. VdF / TFE=95.0 / 5.0 (mol%) Number average molecular weight: 272000 Mass average molecular weight: 880000
[0092] Preparation Example 5 Fluorocopolymer 5 was prepared with reference to Preparation Example 2. The obtained fluorine-containing copolymer 5 had the following composition and physical properties. VdF / TFE=70.0 / 30.0 (mol%) Number average molecular weight: 288000 Mass average molecular weight: 830000
[0093] As a comparative example, polyethylene oxide manufactured by Wako Pure Chemical Industries, Ltd. was used.
[0094] Examples 1 to 5 and Comparative Example 1: Preparation of the Composite The obtained fluorine-containing copolymers 1 to 5 and polyethylene oxide were used as Comparative Example 1. For each, 20 mass % of LiTFSI as an alkali metal salt and 60 mass % of BMI-TFSI as an ionic liquid were dissolved in dimethylformamide (DMF) to prepare polymer electrolyte solutions 1 to 6. The polymer electrolyte solutions were cast onto copper foil using an applicator and adjusted to have a thickness of about 60 μm after drying. The cast polymer electrolyte solutions were dried under reduced pressure at 100° C. for 24 hours to produce composite films 1 to 6.
[0095] (Measurement of volatile components) The composite film prepared as described above was further heated and decompressed at 100° C. for 48 hours, and the amount of volatile components was calculated from the change in mass before and after drying.
[0096] (Flammability test) The composite film thus prepared was exposed to the open flame of a lighter for 3 seconds, and the ease with which the flame spread and the flammability were visually observed. If there was no ignition, it was determined to be flame retardant.
[0097] (Measurement of ionic conductivity) The same composite as in Examples 1 and 2 was used as the measurement sample. The composite film was punched out to a size of Φ13 mm, and a two-electrode cell was prepared by using stainless steel as the working electrode and counter electrode. The prepared battery was connected to a complex AC impedance measuring device using a moving wire in a thermostatic chamber set at 60°C, and was left for 3 hours to allow the electrolyte and electrodes to fully blend, after which it was measured and the ionic conductivity was calculated from the following formula. σ=C / R (C=l / S) Here, l is the thickness of the sample, S is its area, and R is its resistance. The results in Table 3 show that the composite films of Examples 1 to 5 exhibit sufficient ionic conductivity as electrolytes for polymer-based solid state batteries.
[0098] (Evaluation of oxidation resistance) The oxidation resistance of the composite film was evaluated by the LSV (Linear Sweep Voltammetry) method. For the LSV measurement, a solvent containing 3 mass% LiTFSI in propylene carbonate was used. Two types of solutions were prepared by adding 1 mass% of the above polymer (Example 1 or Comparative Example 1) to this solution. Each measurement solution prepared in advance was placed in a measurement container, and a platinum electrode was immersed in the working electrode, and lithium metal was immersed in the counter electrode and reference electrode to form an LSV measurement cell. A voltage of 8 V (vs. Li) was applied to the oxidation side from the OCV (open circuit voltage) at a sweep rate of 5 mV / s. + The potential was swept up to 1000 V / Li and the measurements were performed. The results are shown in Figure 1. Example 1 was shown to have high oxidation resistance.
[0099] [Table 1]
[0100] [Table 2]
[0101] [Table 3]
[0102] (Production of lithium-ion secondary batteries) [Preparation of positive electrode] LiNi as a positive electrode active material 0.5 Co 0.2 Mn 0.3 95% by mass of O2 (NMC), 3% by mass of acetylene black as a conductive material, and 2% by mass of polyvinylidene fluoride (PVdF) as a binder were mixed in N-methylpyrrolidone solvent to form a slurry. The obtained slurry was applied to one side of an aluminum foil with a thickness of 15 μm that had been previously coated with a conductive additive, dried, and roll-pressed in a press machine, and then cut out to form a positive electrode 1. LiMn 1.5 Ni 0.5 Positive electrode 2 was prepared in the same manner as above, except that O4(LNMO) was used.
[0103] [Preparation of negative electrode] 98 parts by mass of carbonaceous material (graphite) was mixed with 1 part by mass of aqueous dispersion of sodium carboxymethylcellulose (concentration of sodium carboxymethylcellulose: 1% by mass) and 1 part by mass of aqueous dispersion of styrene-butadiene rubber (concentration of styrene-butadiene rubber: 50% by mass) as a thickener and binder, and the mixture was mixed in a disperser to form a slurry. The obtained slurry was applied to a copper foil having a thickness of 10 μm, dried, and rolled in a press machine, and then cut out to form a negative electrode.
[0104] [Preparation of aluminum laminated cells] The above positive electrode, composite film 1, and negative electrode were placed facing each other and rolled with a roll press machine to enhance adhesion. Thereafter, the battery was punched out, an electrode tab was attached, the battery was sealed, and the battery was precharged and then aged to produce a lithium ion secondary battery 1 having a design capacity of 1 Ah. A lithium ion secondary battery 2 was produced in the same manner as above, except that a positive electrode 2 was used.
[0105] [Evaluation of initial discharge capacity] The secondary battery 1 produced above was sandwiched between plates and pressurized, and was then charged at a constant current and constant voltage at 25° C. with a current equivalent to 0.1 C up to 4.2 V. The secondary battery 2 produced above was sandwiched between plates and pressurized, and was then charged at a constant current and constant voltage at 25° C. with a current equivalent to 0.1 C up to 4.8 V.
[0106] (Nail penetration test) The fabricated lithium-ion secondary batteries 1 and 2 were fixed on a horizontal stand in an atmosphere of 25°C, and a nail penetration test was performed by inserting a ceramic nail having a diameter of 3 mm from above the battery toward the center of the battery at a nail penetration speed of 80 mm / s, and the behavior was observed and the temperature was measured. In the battery fabricated using composite film 1, no smoke, explosion or fire was observed, and the temperature change on the battery surface was within 5°C. From the above, it was confirmed that the battery is highly safe. [Industrial Applicability]
[0107] The composite of the present disclosure can be suitably used as an electrolyte for a polymer-based solid battery. The resulting polymer-based solid battery has both excellent oxidation resistance and flame retardancy.
Claims
1. A polymer electrolyte comprising a complex containing a fluorine-containing copolymer having tetrafluoroethylene (TFE) units and vinylidene fluoride (VdF) units, and an alkali metal salt, the content of VdF units in the fluorine-containing copolymer is 60.0 mol % or more and 95.0 mol % or less based on the total monomer units, and the content of TFE units is 5.0 mol % or more and 40.0 mol % or less based on the total monomer units, A polymer electrolyte comprising a composite having a volatile component content of 0.1% by mass or less based on the entire composite.
2. 2. The polymer electrolyte according to claim 1, wherein the fluorine-containing copolymer further contains 0.1 to 10 mol % of hexafluoropropylene (HFP) units.
3. 2. The polymer electrolyte according to claim 1, wherein the fluorine-containing copolymer consists only of TFE units and VdF units.
4. The alkali metal salt is LiPF 6 , LiBF 4 , LiTFSI, LiFSI, LiPO 2 F 2 and LiBOB, and the content of the alkali metal salt is 0.1 to 90 mass % based on the fluorine-containing copolymer.
5. Further, the organic cation is 1-butyl-3-methylimidazolium (BMI) cation or N-methyl-N-butyl-pyrrolidium (Pyr14) cation, and the anion is BF 4 5. The polymer electrolyte according to claim 1, further comprising at least one ionic liquid selected from a combination of an anion, a bis(trifluoromethanesulfonyl)imide (TFSI) anion, and a fluorine-containing copolymer, wherein the content of the ionic liquid is 1.0 to 500 mass % based on the fluorine-containing copolymer.
6. 6. An electrochemical device comprising the polymer electrolyte according to claim 1.
7. A polymer-based solid battery comprising the polymer electrolyte according to any one of claims 1 to 5.
8. 8. The polymer-based solid battery according to claim 7, which is a lithium-ion secondary battery.
9. An actuator comprising the polymer electrolyte according to any one of claims 1 to 5.
Citation Information
Patent Citations
Lithium battery
JP1998284127A
Gel composition
JP2001035534A
Electrolyte carrying polymer membrane and secondary battery using it
JP2001266942A
Composite ion exchange film and its manufacturing method
JP2004127846A
Solid electrolyte and its manufacturing method, membrane electrode assembly, and fuel cell