Marine ecological project construction method, asphalt cement coating and its manufacturing method
By treating waste concrete surfaces with emulsified asphalt cement paint and strategically placing oyster-attaching substrates, the method addresses ecosystem destruction and low marine organism density, promoting oyster growth for ecological restoration and waste recycling.
Patent Information
- Application Number
- JP2022533426
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-02
- Filing Date
- 2020-12-01
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-12-01
AI Technical Summary
The rapid development of coastal regions in China has led to the destruction of marine ecosystems, with breakwater construction further damaging the environment and low density of marine sessile organisms on concrete surfaces, necessitating ecological restoration and effective waste concrete disposal.
A method involving the treatment of waste concrete surfaces with emulsified asphalt cement paint to attract oyster larvae, using a lightweight concrete base with a rough surface, and strategic placement of oyster-attaching substrates to enhance marine ecological projects, including monitoring and managing oyster adhesion.
The method effectively attracts and promotes the growth of oysters on concrete structures, purifying water bodies, preventing shoreline erosion, maintaining biodiversity, and contributing to ecosystem restoration while recycling waste concrete.
Smart Images

Figure 0007575809000001 
Figure 0007575809000002 
Figure 0007575809000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority from Chinese Patent Application No. 201911210495.X, filed on December 2, 2019, for "Construction method for marine ecological project of waste concrete," and claims the benefit of priority from Chinese Patent Application No. 201911210405.7, filed on December 2, 2019, for "Emulsified asphalt cement coating and manufacturing method thereof," the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to marine ecological engineering technology, especially to a construction method for marine ecological project, asphalt cement coating and its manufacturing method, which belong to the field of marine ecological engineering. [Background technology]
[0003] In recent decades, the rapid development of the economy in China's coastal areas, but the lack of attention to environmental protection, has caused large-scale destruction of the ecosystem in China's coastal areas, which has serious impacts on the ecosystem and economy of China's coastal areas. At present, with the implementation of a series of relevant national policies, China's marine project construction is also entering a peak period, and at the same time, the large-scale construction of marine projects and breakwaters to ensure the stabilization of the surrounding sea areas will further damage the already fragile marine ecosystem. If proper protection of the ecological environment is not taken, it will more seriously damage the ecosystem in China's coastal areas. At the same time, most of the infrastructure in China's coastal areas cannot be dismantled and the ecosystem of the sea area needs to be restored, so people gradually realize that by applying ecological technologies to many infrastructures, the ecosystem of the sea area can be effectively improved or restored. Therefore, building breakwaters with high ecological effect or ecologicalizing existing breakwaters is very important and urgent for the improvement of the ecological environment of China's coastal areas. Summary of the Invention
[0004] The main objective of the present invention is to solve the problem that the current breakwater expansion and repair destroys the ecosystem in China's coastal areas, and the problem that currently, the density of marine sessile organisms on the surface of most marine concrete projects is low, requiring artificial intervention. The present invention uses coating technology to treat the surface of waste concrete, and uses the treated waste concrete to build a new marine ecological project with sessile organisms such as oysters, which has excellent wave-dissipating function and at the same time solves the problem that it is difficult to treat a large amount of waste concrete due to the environmental efficiency caused by the attachment of a large amount of oysters. The specific technical solutions are as follows:
[0005] (1) Investigating the marine area where the breakwater will be constructed, the dominant species of oysters in said marine area and the presence or absence of oysters attached thereto shall be investigated, and the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca, etc. in different seasons in said marine area shall be investigated. 2+ , Zn 2+ , K + We will also investigate the number of typhoons that have occurred in the past and their intensity.
[0006] (2) Regarding the manufacture of a concrete bonding base, a lightweight concrete oyster bonding base with a rough surface is manufactured using one of the following shapes: a plate-shaped bonding base, a corrugated bonding base, or a cylindrical bonding base.
[0007] (3) To quantitatively harvest and cultivate oyster larvae, during the period when the floating oyster larvae in the local sea area are concentrated and attach to the sea and metamorphose, the attachment substrate is placed in the seeding area of the nearby sea area, and the attachment amount of oyster larvae is 15 to 25 oysters / 100 cm 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of sea where food is abundant for floating culture.
[0008] (4) Regarding the treatment of the surface of the waste concrete blocks, the alkalinity, internal ion concentration, and permeability of the waste concrete should be evaluated. If the pH is > 12.5, the alkalinity should be reduced. Then, an emulsified asphalt cement paint with high adhesive strength that effectively attracts oysters should be sprayed or applied to the surface of the concrete blocks.
[0009] (5) Regarding the placement of waste concrete blocks, in the second year, during the period when the floating oyster larvae are concentrated in local waters and attach and metamorphose, they are placed in a dispersed manner, and the waste concrete blocks with a volume of more than 1 cubic meter are placed individually, and each waste concrete block is covered with a rope cage, and the rope cage is used to cover multiple waste concrete blocks with a volume of less than 1 cubic meter, thereby forming a pile of waste concrete blocks with a volume of 1 to 5 cubic meters, the internal porosity of which is 40% to 60%, and the waste concrete blocks or piles of waste concrete blocks are connected with ropes, etc.
[0010] (6) Regarding the placement of oyster attachment substrates on site, the substrates carrying oysters at the mature stage of gonad development in (3) shall be transported to the sea area where the breakwater is to be constructed, and one or two oyster attachment substrates shall be placed on each waste concrete block or pile of waste concrete blocks, and the waste concrete block or pile of waste concrete blocks shall be secured with ropes. In addition, feeding or feeding nutrients shall be added as necessary based on the planktonic organism conditions in the local sea area.
[0011] (7) Monitoring and management of oyster larvae attachment: Monitor the attachment status of oyster larvae on the concrete surface, and keep the number at 30-40 per 100 cm. 2 In this case, the oyster attachment substrate will be removed and the ecological condition of the breakwater will be monitored over the long term, with improvement measures being taken according to the actual situation.
[0012] For the lightweight concrete adhesion base with a rough surface described in the specific measures in (2), the components of the material are cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, bio-calcium powder, calcium carbonate powder, trace elements, short fiber, and superplasticizer, and the weight percentages thereof are 21.8%~34.5%, 24.6%~37.5%, 15.8%~29.6%, 8.4%~16.4%, 0.6%~3.0%, 0.4%~2.0%, 0.4%~2.0%, 0.2%~1.8%, 0.15%~1.5%, and 0.03%~0.18%, respectively.
[0013] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.
[0014] Preferably, the dark pigments are modified with one of the following materials depending on their impact on concrete performance: transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material.
[0015] Preferably, the biocalcium powder is bovine bone powder. or It contains one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and the fineness of the powder is 100 mesh to 1000 mesh. Here, oyster shell powder, fish bone powder, eggshell powder, and coral powder are referred to as bio-calcium carbonate powder. )
[0016] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.
[0017] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.
[0018] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to realize sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.
[0019] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.
[0020] Preferably, the short fibers are inorganic fibers (length 12 to 20 mm) including one or more of basalt fibers, alkali-resistant glass fibers, and carbon fibers.
[0021] Preferably, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt, lightweight ceramsite having a maximum particle size of less than 20mm.
[0022] Preferably, the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm.
[0023] The method for manufacturing a rough surface cement concrete oyster adhesion base is as follows: Step S1 of designing different roughness according to the preferred characteristics of oyster larvae to attach to rough surfaces, and then manufacturing molding forms with different roughness; Step S2 of measuring the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water, the dark color pigment, the bio-calcium powder, the calcium carbonate powder, the trace elements, the short fibers and the superplasticizer; First, put the lightweight coarse aggregate and the lightweight fine aggregate into the concrete mixer and mix for 0.5-1 minute, then add the cementitious material, dark color pigment, bio-calcium powder, calcium carbonate powder and trace elements and mix for another 1-2 minutes, then add short fiber, water and superplasticizer and mix for 2-6 minutes, and then mix evenly, then pour and vibrate; step S3; Step S4 may include placing the molded concrete specimen in a high-concentration CO2 maintenance box for 0.5 to 5 hours to reduce the alkalinity of the cement specimen, and then performing standard maintenance for 28 days or maintenance based on actual conditions.
[0024] This makes it possible to produce a cement concrete oyster attachment base having a rough surface and excellent attracting effect.
[0025] For the lightweight concrete adhesion base having a rough surface described in the specific measures in (2), the components of the material are dark color pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of the dark color pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6%-3.0%, 21.8%-34.5%, 24.6%-37.5%, 15.8%-29.6%, 8.4%-16.4% and 0.03%-0.18%, respectively.
[0026] For the lightweight concrete adhesion base having a rough surface described in the specific measures in (2), the components of the material are calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.4% to 2.35%, 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4% and 0.03% to 0.18%, respectively.
[0027] For the lightweight concrete adhesion base with a rough surface described in the specific measures in (2), the ingredients of the material are cow bone powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of the cow bone powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.4% to 2.35%, 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4% and 0.03% to 0.18%, respectively.
[0028] For the lightweight concrete adhesion base having a rough surface described in the specific measures in (2), the ingredients of the material are modified dark pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of the modified dark pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6%-3.0%, 0.4-2.35%, 21.8-34.5%, 24.6%-37.5%, 15.8%-29.6%, 8.4%-16.4% and 0.03%-0.18%, respectively.
[0029] In the cement bioadhesion base described in the specific measures in (2), circular holes with a diameter of 3 to 5 mm are created during molding, and the shape of the base is one of plate-shaped, wavy, and cylindrical.
[0030] Regarding the concentrated attachment and metamorphosis period of oyster larvae described in the specific measures in (3), it is generally from May to August in North China and from April to October in South China.
[0031] The emulsified asphalt cement paint described in the specific measures in (4) is as follows: The specific technical solutions are as follows: The ingredients of the material are cementitious material, emulsified asphalt, sand, water, bio-calcium powder, calcium carbonate powder, trace elements, acrylic emulsion, and superplasticizer, and the weight ratio thereof is 1:(0.4~0.8):(0.5~1.3):(0.10~0.30):(0.02~0.10):(0.02~0.10):(0.01~0.08):(0.08~0.15):(0.001~0.008) in order.
[0032] Preferably, the biocalcium powder is bovine bone powder. or The powder contains one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and has a powder size of 100 mesh to 1000 mesh.
[0033] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.
[0034] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to realize sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.
[0035] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.
[0036] Preferably, the acrylic emulsion is a polyurethane modified emulsion.
[0037] Preferably, the emulsified asphalt is one of cationic emulsified asphalt and anionic emulsified asphalt, whose performance index is: evaporation residue content >55%, 5-day stability ≦5%, and sieve residue (1.18 mm sieve) ≦0.1%.
[0038] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.
[0039] Preferably, the sand is one or more of river sand, machine-made sand (whose parent material is limestone, basalt, or granite), and sea sand, each having a particle size of 0.16 mm to 2.36 mm.
[0040] Preferably, the superplasticizer is, for example, one of the following: polycarboxylic acid, naphthalene type.
[0041] The manufacturing method of emulsified asphalt cement paint is as follows: Step S1 of measuring emulsified asphalt, cementitious material, sand, water, biocalcium powder, calcium carbonate powder, trace elements, acrylic emulsion, and superplasticizer; Step S2: putting the cementitious material, biocalcium powder, calcium carbonate powder, trace elements and powdered superplasticizer into a mixer and uniformly mixing for 4 to 8 minutes at a rotation speed of 1000 to 1500 revolutions per minute; Next, add sand, adjust the rotation speed to 500 to 1000 revolutions per minute, and mix for 2 to 5 minutes to prepare for use. Step S3. and step S4 of uniformly mixing the acrylic emulsion, emulsified asphalt, and water, and putting the uniformly mixed materials into a high-speed mixer at 200 to 500 rpm and mixing for 5 to 10 minutes.
[0042] Thus, an emulsified asphalt cement paint with excellent attracting effect can be produced for attracting sessile organisms to the surface of marine projects. The object of the present invention is to invent a paint that can be directly applied and cured in a humid environment, which allows sessile organisms to attach quickly and densely to the concrete surface, and utilizes the adhesion properties of oysters to achieve biological corrosion prevention effect, and the large amount of sessile organisms also plays a role in purifying water areas and restoring ecosystems. Solving the problems of limited effect, short service life, high cost, and urgent need to restore marine ecosystems due to ecosystem degradation of corrosion prevention measures in tidal and underwater areas of marine concrete projects.
[0043] The realization method of the present invention is as follows: by using low-alkalinity cementitious material, acrylic emulsion and superplasticizer, and adding emulsified asphalt, modified bio-calcium powder, calcium carbonate powder and trace elements to the paint, the emulsified asphalt cement paint produced has the function of effectively inducing the attachment and metamorphosis of oyster larvae, and has the function of directly applying and hardening in a humid environment, so as to achieve the effect of dense and uniform attachment of oysters, and utilize the fastening properties of oysters to ensure the durability of concrete structures, and does not pollute the marine environment.
[0044] The present invention further has the following structural features:
[0045] The ingredients of the material are cementitious material, emulsified asphalt, sand, water, bio-calcium powder, calcium carbonate powder, trace elements, acrylic emulsion, and superplasticizer, and the weight ratio thereof is 1:(0.4~0.8):(0.5~1.3):(0.10~0.30):(0.02~0.10):(0.02~0.10):(0.01~0.08):(0.08~0.15):(0.001~0.008) in that order.
[0046] Preferably, the biocalcium powder is bovine bone powder. or The powder contains one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and has a powder size of 100 mesh to 1000 mesh.
[0047] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.
[0048] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to realize sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.
[0049] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.
[0050] Preferably, the acrylic emulsion is a polyurethane modified emulsion.
[0051] Preferably, the emulsified asphalt is one of cationic emulsified asphalt and anionic emulsified asphalt, whose performance index is: evaporation residue content >55%, 5-day stability ≦5%, and sieve residue (1.18 mm sieve) ≦0.1%.
[0052] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.
[0053] Preferably, the sand is one or more of river sand, machine-made sand (whose parent material is limestone, basalt, or granite), and sea sand, each having a particle size of 0.16 mm to 2.36 mm.
[0054] Preferably, the superplasticizer is, for example, one of the following: polycarboxylic acid, naphthalene type.
[0055] The manufacturing method of emulsified asphalt cement paint is as follows: Step S1 of measuring emulsified asphalt, cementitious material, sand, water, biocalcium powder, calcium carbonate powder, trace elements, acrylic emulsion, and superplasticizer; Step S2: putting the cementitious material, biocalcium powder, calcium carbonate powder, trace elements and powdered superplasticizer into a mixer and uniformly mixing for 4 to 8 minutes at a rotation speed of 1000 to 1500 revolutions per minute; Next, add sand, adjust the rotation speed to 500 to 1000 revolutions per minute, and mix for 2 to 5 minutes to prepare for use. Step S3. and step S4 of uniformly mixing the acrylic emulsion, emulsified asphalt, and water, and putting the uniformly mixed materials into a high-speed mixer at 200 to 500 rpm and stirring for 5 to 10 minutes. This allows the production of an emulsified asphalt cement paint with excellent attracting effect for attracting sessile organisms to the marine project surface.
[0056] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0057] The present invention utilizes lumpy construction waste generated by buildings and infrastructure to construct a marine ecological breakwater, which not only fully utilizes waste concrete, but also has the characteristics of waste recycling and energy saving. Furthermore, by inducing the growth of oyster attachment bases, it can purify water bodies, prevent coastline erosion, maintain biodiversity, fix carbon, and mitigate ocean acidification, and has the ability to restore the ecosystem.
[0058] At present, there is no environmentally friendly and economical method for the durability of marine concrete or the ecologicalization of marine concrete projects. Oysters, as marine "ecological engineers", have the function of densifying the surface of concrete structures and improving the ecological environment. The emulsified asphalt cement paint for attracting sessile organisms provided by the present invention not only has the characteristics of quickly inducing the attachment and metamorphosis of sessile organisms and promoting their long-term growth, but also has the characteristics of easy construction and application. It can be applied to new marine projects, especially marine projects with a large amount of in-use. It can not only improve the durability of reinforced concrete structures, but also easily and economically realize the restoration of the marine ecological environment. It can not only greatly expand the application of corrosion prevention of marine sessile organisms to in-use reinforced concrete structures, but also can be widely used in marine ecological environment restoration projects. [Brief description of the drawings]
[0059] [Figure 1] Mold grows on the surface of concrete that has a different mix ratio, that is, 10% cow bone powder mixed in. [Diagram 2] The powder size is 200 mesh, and the mixing ratio is different when 10% modified cow bone powder is mixed. [Diagram 3] FIG. 1 is a schematic diagram of a 210-day actual marine adhesion experiment. [Figure 4] This is a schematic diagram of a 300-day actual marine adhesion experiment. [Diagram 5] 1 is a schematic diagram of concrete oyster attachment bases of different shapes. [Figure 6] 1 is a schematic diagram of concrete oyster attachment bases of different shapes. [Figure 7] 1 is a schematic diagram of concrete oyster attachment bases of different shapes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0060] The present invention is described in detail below through examples, which are only used to illustrate the present invention and do not limit the scope of the present invention. The specific technical solutions of the project plan are as follows:
[0061] Example 1 (1) In the marine area where the breakwater will be constructed, the dominant species of oysters in the marine area and the presence or absence of oysters shall be surveyed, and tests shall be conducted 15 times every quarter to measure the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca, and other substances in the marine area. 2+ , Zn 2+ , K + record the occurrence of tropical cyclones, investigate the number of tropical cyclones and their intensity in the past, examine meteorological and hydrological data of the sea area over the years, and analyze feasible methods and solutions for the construction of ecological riprap breakwaters;
[0062] (2) Regarding the production of the concrete adhesion base, eco-concrete is used to produce a lightweight concrete oyster adhesion base with a rough surface. The size of the adhesion base is 10 cm x 10 cm x 2 cm. After being demolded, it is immediately subjected to CO2 curing at 10 atmospheres for 1 hour, and then subjected to standard curing for 28 days.
[0063] (3) To ensure the timely and quantitative harvesting and cultivation of oyster larvae, a rough lightweight concrete oyster attachment base was placed in a nearby sea area in July, and the attachment rate of oyster larvae was set at 20 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of sea where food is abundant for floating culture.
[0064] (4) Regarding the treatment of the waste concrete surface, the alkalinity, internal ion concentration, and permeability of the waste concrete should be detected by sampling (5% of the total). If the pH is greater than 12.5, the waste concrete should be subjected to CO2 curing under 10 atmospheres for 1 hour to reduce the alkalinity. Next, the concrete block should be moistened and an emulsified asphalt cement paint with high adhesive strength, which effectively attracts oysters, should be sprayed or applied to its surface.
[0065] (5) Regarding the placement of the waste concrete, in June of the second year, the waste concrete blocks were placed in a dispersed manner, with waste concrete blocks with a volume of more than 1 cubic meter placed individually, and each waste concrete block was covered with a rope basket. In addition, the rope basket was used to cover multiple waste concrete blocks with a volume of less than 1 cubic meter, forming a pile of waste concrete blocks with a volume of 1 to 5 cubic meters, with an internal void ratio of 50%, and the waste concrete blocks (piles) were connected with ropes, etc., and the distance between each waste concrete block (piles) was maintained at 4 meters.
[0066] (6) Regarding the placement of oyster attachment substrates on site, substrates with a concrete surface to which oysters (at the mature stage of gland development) can attach well will be transported to the sea area where the breakwater will be constructed, and an oyster attachment substrate will be placed on each (pile of) discarded concrete blocks, and each (pile of) discarded concrete blocks will be secured with ropes.
[0067] (7) Regarding the management and monitoring of oyster larvae attachment, the attachment density of oyster larvae on the concrete surface is 35 pieces / 100 cm 2 When the number of oysters reaches 100, the oyster attachment substrate is removed, and at the same time, it is decided whether or not to feed the oysters based on the type and number of planktonic organisms in the sea area.
[0068] Example 2 (1) In the marine area where the breakwater will be constructed, the dominant species of oysters in the marine area and the presence or absence of oysters shall be surveyed, and tests shall be conducted 15 times every quarter to measure the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca, and other substances in the marine area. 2+ , Zn2+ , K + record the occurrence of tropical cyclones, investigate the number of tropical cyclones and their intensity in the past, examine meteorological and hydrological data of the sea area over the years, and analyze feasible methods and solutions for the construction of ecological riprap breakwaters;
[0069] (2) In the manufacture of the concrete adhesion base, eco-concrete is used to manufacture a lightweight concrete oyster adhesion base with a rough surface. The size of the adhesion base is 10 cm x 10 cm x 3 cm. After being demolded, it is immediately subjected to CO2 curing under 10 atmospheres for 1.5 hours, and then to standard curing for 28 days.
[0070] (3) To ensure the timely and quantitative harvesting and cultivation of oyster larvae, a rough lightweight concrete oyster attachment base was placed in a nearby sea area in August, and the attachment rate of oyster larvae was set at 25 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of sea where food is abundant for floating culture.
[0071] (4) Regarding the treatment of the waste concrete surface, the alkalinity, internal ion concentration, and permeability of the waste concrete should be detected by sampling (5% of the total). If the pH is greater than 12.5, the waste concrete should be subjected to CO2 curing under 10 atmospheres for 1 hour to reduce the alkalinity. Next, the concrete block should be moistened and an emulsified asphalt cement paint with high adhesive strength, which effectively attracts oysters, should be sprayed or applied to its surface.
[0072] (5) Regarding the placement of the waste concrete, in July of the second year, the waste concrete was placed in a dispersed manner, with waste concrete blocks with a volume of more than 1 cubic meter placed individually, and each waste concrete block was covered with a rope basket. In addition, the rope basket was used to cover multiple waste concrete blocks with a volume of less than 1 cubic meter, forming a pile of waste concrete blocks with a volume of 1 to 5 cubic meters, with an internal void ratio of 60%, and the waste concrete blocks (piles) were connected with ropes, etc., and the distance between each waste concrete block (piles) was maintained at 5 meters.
[0073] (6) Regarding the placement of the oyster attachment base on site, a base with a concrete surface on which oysters (at the mature stage of gland development) can attach well will be transported to the sea area where the breakwater will be constructed, and a lightweight concrete oyster attachment base with a rough surface will be placed on each (pile of) discarded concrete blocks, and the discarded concrete blocks will be secured with ropes.
[0074] (7) Regarding the management and monitoring of oyster larvae attachment, the attachment density of oyster larvae on the concrete surface is 40 pieces / 100 cm 2 When the number of oysters reaches 100, the oyster attachment substrate is removed, and at the same time, it is decided whether or not to feed the oysters based on the type and number of planktonic organisms in the sea area.
[0075] Specific examples of the oyster adhesion base and asphalt cement paint described in Example 1 and Example 2 are as follows.
[0076] The specific steps of the technical solution are as follows:
[0077] The concrete mix ratio of the rough surface lightweight concrete oyster attachment base (1-25) and the emulsified asphalt cement paint (26-36) for attracting sessile organisms on the marine project surface are as follows, and the shape of the concrete oyster attachment base is designed, specifically referring to Figures 5-7.
[0078] 1. Regarding the concrete mix ratio of ordinary Portland cement, the weight percentages of ordinary Portland cement, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water-reducing agent powder are 29.37%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0079] The lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite, the maximum particle size of which is less than 20 mm. The lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, the particle size of which is 0.2 mm to 5 mm and has a high grade. The water must meet the standard for water for concrete (JGJ63-2006) and must be free of Cl. - The content is <1000mg / L, the pH value is >4.5, and there is almost no effect on the initial hardening time difference, final hardening time, strength, and permeability of the cement. In addition, the above materials selected in Examples 1 to 25 are the same.
[0080] 2. Regarding the mix ratio of the standard concrete, the weight percentages of ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 17.62%, 1.47%, 10.28%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0081] 3. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0082] 4. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0083] 5. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0084] 6. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0085] 7. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0086] 8. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0087] The modified dark pigment is 196 transparent resin, mixed with 3% hardener and 1.5% accelerator, and the volume ratio of pigment to resin is 1:0.2. It is cured at room temperature for 4 hours, then cured at 60℃ for 4 hours, and then crushed by beating and ground by vibration mill until the powder size exceeds 400 mesh.
[0088] 9. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0089] 10. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0090] 11. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0091] 12. The weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 0.87%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0092] 13. The weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 1.47%, 17.62%, 1.10%, 7.71%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0093] 14. The weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 2.35%, 17.62%, 0.99%, 6.94%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0094] 15. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0095] 16. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0096] 17. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0097] 18. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.
[0098] 19. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0099] 20. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0100] The method for modifying the bone powder is as follows: 100 mesh bone powder is added to a 2% phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30°C, the mixer is stirred at 200-500 revolutions / min for 30 minutes, the centrifuge is centrifuged at 3000-5000 revolutions / min for 3 minutes, the supernatant is discarded, and the centrifuged solid is washed with water 2-3 times, the washing water is not acidic, the centrifuged solid is vacuum dried at 40°C, and the dried bone powder and the 1:4 slag powder are ground in a vibration mill until the fineness exceeds 200 mesh, and then prepared for use.
[0101] 21, the weight percentages of calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 0.5%, 1.47%, 17.62%, 0.93%, 6.50%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0102] 22, the weight percentages of calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 1.2%, 1.47%, 17.62%, 0.84%, 5.89%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0103] 23, the weight percentages of zinc sulfate, modified dark pigment (iron black:aniline black mixture mass ratio = 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder = 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.5%, 1.47%, 1.47%, 0.87%, 17.62%, 0.93%, 6.50%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0104] 24, the weight percentages of zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder in a ratio of 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.6%, 1.47%, 1.47%, 0.87%, 17.62%, 0.84%, 5.89%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.
[0105] The method of modifying zinc sulfate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it to the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain the modified zinc sulfate.
[0106] 25, the weight percentages of zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder in a ratio of 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, short fiber and polycarboxylate water reducer powder are 0.5%, 1.47%, 1.47%, 0.87%, 17.62%, 0.94%, 6.50%, 33.07%, 24.14%, 12.59%, 0.8%, and 0.03%, respectively.
[0107] 26, the weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.05:0.05:0.04:0.12:0.005, respectively.
[0108] 27, the weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.08:0.08:0.06:0.12:0.005, respectively.
[0109] 28, the weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.08:0.08:0.02:0.12:0.005, respectively.
[0110] 29. The weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.03:0.03:0.06:0.12:0.005, respectively.
[0111] 30, the weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.03:0.03:0.04:0.12:0.005, respectively.
[0112] 31. The weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.05:0.05:0.02:0.12:0.005, respectively.
[0113] 32, the weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.08:0.08:0.04:0.12:0.005, respectively.
[0114] 33. The weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.08:0.08:0.06:0.12:0.005, respectively.
[0115] 34. The weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.03:0.05:0.02:0.12:0.005, respectively.
[0116] 35, the weight ratio of emulsified asphalt, cementitious material, sand, water, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, zinc sulfate, acrylic emulsion and superplasticizer is 0.6:1:1:0.20:0.03:0.03:0.02:0.12:0.005, respectively.
[0117] The method for modifying the bone powder is as follows: 100 mesh bone powder is added to a 2% phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30°C, the mixer is stirred at 200-500 revolutions / min for 30 minutes, the centrifuge is centrifuged at 3000-5000 revolutions / min for 3 minutes, the supernatant is discarded, and the centrifuged solid is washed with water 2-3 times, the washing water is not acidic, the centrifuged solid is vacuum dried at 40°C, the dried bone powder and slag powder are mixed in a ratio of 1:4, and the powder is ground in a vibration mill until the powder size exceeds 200 mesh, and then it is prepared for use.
[0118] The method of modifying zinc sulfate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it to the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain the modified zinc sulfate.
[0119] Reference 1, (Living Breakwaters - Green Infrastructure along the New York Coast - Mago Ichiro)
[0120] In Reference 1, the construction of a "living" breakwater, with its macro-design, surface texture, and concrete components manufactured with low-alkali cement, increased the number of marine organisms; the increased marine organisms were marine plants and marine sessile organisms, primarily marine plants.
[0121] In the present invention, in addition to reducing the alkalinity of cement, dark color pigments, bio-calcium powder, calcium carbonate powder, trace elements, etc. are mixed into the concrete to attract oyster larvae. The attraction is characterized by rapid and high density, and is highly effective in greatly improving the ecological environment of the marine area.
[0122] Compared with Reference 2 (Biomimetic concrete artificial reef and its manufacturing method 2015 CN104938384 A), the differences are as follows:
[0123] (1) The object of the present invention is different from that of Reference 2, in which a cement mortar mixed with crushed oyster shells is applied to the surface of concrete, but the object is to improve the aquatic environment by attracting fish, microorganisms and algae through biomimetic surface and increasing the number of microorganisms, and oysters are not mentioned. The object of the emulsified asphalt cement paint of the present invention is to attract the attachment of oysters.
[0124] (2) According to Reference 2, in cement mortar, biocalcium carbonate powder (150-200 mesh) less than 10% of the cement dosage is ineffective against adhesion by attraction. However, in the course of research into the present invention, it is found that the optimal dosage of bovine bone powder and biocalcium carbonate powder is less than 10% of the cementitious material by using an emulsified asphalt cement paint (fineness of 100-1000 mesh) mixed with modified cow bone powder and biocalcium carbonate powder.
[0125] (3) The modification of beef bone powder and biocalcium carbonate powder is specifically performed by treating eggshell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of tannic acid, acetic acid, silicic acid, and sulfurous acid, and treating beef bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.
[0126] (4) In the references, it is difficult to embed oyster shells on the concrete surface, and not all project surfaces use this method, which is not feasible. The present invention can achieve the excellent effect of attracting sessile organisms by applying an emulsion asphalt cement paint layer to the concrete surface, which does not require embedding oyster shells, is not only easy to apply, but also greatly improves the amount of oyster adhesion.
[0127] (5) In recent years, serious corrosion of artificial reefs has been observed in marine environments. The serious corrosion is mainly caused by the combined action of biological sulfuric acid secreted by anaerobic microorganisms such as Thiobacillus subtilis and acidic substances secreted by other bacteria. However, calcium carbonate has very poor resistance to acid corrosion. If the content of calcium carbonate with large fineness is too high, it can cause serious acid corrosion.
[0128] Compared to Reference 3 (Fan Ruiliang: The effects of substrate type on oyster attachment, growth, population establishment and reef development [D]), the differences are as follows:
[0129] (1) In Reference 3, 80 mesh cow bone powder, calcium powder, and gypsum powder are taken and mixed into concrete separately. The fineness of all calcium materials in this invention is more than 100 mesh, which is larger than the fineness of the materials in Reference 3. Similarly, cow bone powder is modified for mixing, taking into account the grading of paint and concrete particles and their attracting ability.
[0130] (2) At room temperature, when the cow bone powder is crushed by a vibrating mill and the fineness exceeds 80 mesh, the cow bone powder contains a large amount of collagen, so it becomes lumpy and cannot be crushed further. In the present invention, by using the dilute acid modification technology and crushing with other substances, cow bone powder with small particle size and modified bio-calcium powder with fineness > 200 mesh can be obtained. The obtained bio-calcium powder retains the original substance of bio-calcium, improves the release rate of the substance for attracting oyster larvae to attach, and reduces the dosage of bio-calcium powder, thereby reducing the impact on paint and concrete performance.
[0131] (3) Bone powder contains a large amount of organic substances such as collagen. Mixing a large amount of these substances will reduce the strength and permeation resistance of paint and concrete. Especially when the dosage exceeds 5%, the strength of paint and concrete will rapidly decrease, the permeation resistance will be significantly reduced, and mold will grow on the paint and concrete surface under standard curing conditions. Figure 1 shows the mold growing on the concrete surface. Figure 2 shows the surface of the modified concrete.
[0132] As can be seen from Figure 1, the mold on the concrete surface is white and cotton-like, covering almost the entire concrete surface, while when the cow bone powder, age and curing conditions are the same, there is no mold on the concrete surface in Figure 2.
[0133] The present invention uses dilute acid modification and composite crushing technology to fully utilize the attractant ability of cow bone powder, greatly reduce the dosage of cow bone powder, and perform anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which is low in dosage and has little effect on the strength and permeability of paint and concrete. At the same time, it has high oyster larvae adhesion ability and solves the problem of mold growth on paint and concrete. In addition, compared with concrete without attractant, the number of oyster larvae attached to concrete mixed with attractant is greatly increased. Specifically, see Figure 3.
[0134] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that mixing an appropriate amount of calcium carbonate material into cement-based materials can promote the attachment and growth of oyster larvae. However, cement paint and cement concrete contain a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5, and at room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the concrete pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5×10 -5 mol / L(9.5×10 -2Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment. 2+ Furthermore, while Ca(OH)2 in cement paint and concrete can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when calcium carbonate materials are mixed into paint and concrete to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.
[0135] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:
[0136] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the paint and concrete is diluted, and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the paint and concrete increases, and the HCO3 in the solution increases. - The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of the paint and concrete will increase rapidly, and the alkali and carbonate in the paint and concrete will rapidly leach out, the adverse effect of the alkali will become obvious, and the critical effect or adverse effect of the carbonate will begin to appear, resulting in a decrease in the adhesion amount;
[0137] 2) With the same amount of substitute aggregate, the permeability of paint and concrete decreased with increasing dosage, and calcium ions and OH -The leaching of calcium ions decreased, but the permeability of carbonate ions gradually improved and reached a certain value, and the attachment of oysters reached its maximum value. As the dosage continued to increase, the calcium ions decreased significantly, and carbonates may also decrease. The calcium ion concentration limited the attachment of oyster larvae, which was manifested as a decrease in the attachment amount.
[0138] 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.
[0139] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:
[0140] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to realize low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristics of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the low alkalinity sulfoaluminate cement is mixed to adjust the alkalinity of cement concrete and provide a suitable pH value for the attachment of oyster larvae. In addition, marine plants and sessile organisms such as oysters and barnacles have different alkali tolerances, and the environments required during the attachment and later stages are different. For example, the attachment, metamorphosis and later growth of barnacles and oysters require large amounts of calcium ions.
[0141] In Reference 4, concrete is used to attract marine organisms, which mainly starts from the size and diversity of the attached organisms, the main attached organisms being various algae. In the present invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look similar, they are actually quite different. Figures 4 and 5 respectively show a comparison of the biofouling situation after about 210 days of actual sea attachment experiment in Reference 3 and the biofouling situation after 300 days of actual sea attachment experiment in the present invention.
[0142] In Reference 4, concrete is used to attract marine organisms, mainly due to the size and diversity of the attached organisms, the main of which are various algae. In this invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look the same, they are actually quite different.
[0143] Thus, similarly, this piece of knowledge relates to the interdisciplinary fusion of marine sessile organisms, marine plants and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain, according to Reference 3, the technical features in the present invention in which the reduction in alkalinity of concrete and the balance of calcium ion concentration are closely related to the attachment of marine sessile organisms.
[0144] The unique features and beneficial effects of the present invention are as follows:
[0145] Deep color pigment or emulsified asphalt
[0146] Taking advantage of the phototaxis of oyster eyespot larvae, dark color pigments (one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red) or asphalt are mixed into concrete to change the color of the concrete, making the concrete darker and making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark concrete surface by themselves, increasing the probability of contact between the oyster larvae and the concrete surface, and increasing the probability of attracting the oyster larvae to attach. Specifically, it is as follows.
[0147] Marine biology researchers have looked into the use of different colored substrates to cultivate and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are two major fields entirely. The interdisciplinary fusion of marine sessile organisms and concrete materials science has led to the use of dark-colored paints and concrete to attract oyster larvae to attach. The present invention adds dark-colored pigments or asphalt to darken the color of the paints and concrete and promote the attachment of oyster larvae. Other materials are mixed into the paints and concrete, which will affect their performance. The present invention considers that concretes with different cements have different surface colors. Therefore, the dosage of the dark-colored material is determined based on the cement type and dosage. The dark-colored pigments or asphalt also affect the paint and concrete performance. Most importantly, the dark-colored pigments or asphalt can be mixed in while simultaneously reducing the alkali and Ca in the paints and concrete. 2+ If the permeability of concrete is not controlled, the released alkali will affect the attachment, metamorphosis and growth of sessile organism larvae, and if the dosage exceeds a certain value, the amount of larvae attachment will decrease. In the present invention, the permeability prevention of concrete is designed and controlled, and the main measures are the selection of the type of dark pigment or asphalt, the control of the dosage and modification. With the increase in the dosage of dark pigment, the amount of larvae attachment will increase, and when the dosage is 0.5%-6% of the cementitious material, the amount of larvae attachment is the highest, and then increases slightly or remains unchanged.
[0148] trace elements
[0149] The oyster body contains a large amount of zinc, much higher than the seawater in which it lives, and at the same time, the oyster body contains a lot of Fe, P, and K elements. At the same time, adequate Zn in the solution 2+ and K +The concentration can promote the early attachment and metamorphosis of oyster larvae. Therefore, zinc phosphate, potassium phosphate, ammonium phosphate, zinc sulfate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, iron phosphate, and calcium phosphate are used as trace elements and mixed into concrete, and the modification of these substances basically does not change the strength and penetration prevention properties of the concrete, but greatly improves the attachment attraction rate of oyster larvae. The specific details are as follows:
[0150] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms, which belongs to the field of marine biology, in order to clarify the attachment mechanism of oysters and the purpose of their cultivation and propagation. It is completely different from marine concrete engineering and concrete materials science, which are completely two major fields. It can be seen that the interdisciplinary fusion of marine sessile organisms and concrete materials science can add corresponding substances into paint and concrete to attract oyster larvae to attach to the cleat surface. Since soluble salts have a great impact on concrete performance such as early workability, hardening time, and later strength and anti-penetration properties, the present invention uses diatomaceous earth as a carrier to fix these inorganic salts inside diatomaceous earth, reducing the impact of soluble salts on paint and concrete performance, while utilizing the effect of diatomaceous earth to improve paint and concrete performance, and realizes that the excellent performance of paint and concrete can be maintained even if these attractants are added. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, and the release rate is kept at a very low level, especially after immersion in seawater for a certain period of time. Therefore, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, due to the conventional background, in the present invention, by mixing trace elements into paint and concrete, changing the ion content of trace elements on the paint and concrete surface, and controlling the permeability of concrete, it is impossible to obtain technical characteristics closely related to paint and concrete with excellent ability to attract oyster larvae to attach.
[0151] Permeability of paint and concrete
[0152] The strength and permeability of paint and concrete are the two most important performances of paint and concrete. Mixing different attractants into paint and concrete will affect the performance of paint and concrete, so when mixing different substances to promote the attachment, metamorphosis and subsequent growth of oyster larvae, first, it is necessary to control as a whole so as not to have a significant effect on the strength and permeability of paint and concrete, and second, select raw materials according to the suitability of various raw materials, and if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related research considers the effect of calcium content on the attachment of oyster larvae, but does not consider the performance of the concrete itself, and does not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of paint and concrete will change the permeability of alkali and ions inside the paint and concrete, and the lower the permeability of paint and concrete, the higher the permeability of alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkalis and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may become more serious, especially when the cement dosage is high. Therefore, by mixing the attractant into the paint and concrete, it is necessary to ensure that the change in the impermeability of the paint and concrete is within a controllable range, for example, the change does not exceed 10%. In this way, the attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect on oyster larvae cannot be evaluated.
[0153] Thus, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain the technical features closely related to the paint and concrete having the ability to effectively attract oysters to attach and high durability, by mixing dark color pigments or asphalt into concrete in the present invention, modification of cow bone powder, crushing technology, and control of the permeability of paint and concrete, according to References 1 to 3. Also, according to Reference 4, the reduction in alkalinity of concrete and the balance of calcium ion concentration in the present invention cannot obtain the technical features closely related to the attachment of marine sessile organisms.
[0154] It is necessary to grasp the optimal environment required for marine sessile organisms to attach, transform and grow later, and to design paints and concrete starting from the penetration resistance of paints and concrete, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the penetration resistance of paints and concrete. Therefore, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, according to the conventional background, in the present invention, the overall control of the penetration resistance of paints and concrete cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.
[0155] Since this example is the same as the emulsified asphalt cement paint (26-36) for attracting sessile organisms to the marine project surface, detailed description will be omitted. Also, these examples are used only to explain the present invention, but do not limit the scope of the present invention.
[0156] Compared with Reference 2 (Biomimetic concrete artificial reef and its manufacturing method 2015 CN104938384 A), the differences are as follows:
[0157] (1) The object of the present invention is different from that of Reference 2, in which a cement mortar mixed with crushed oyster shells is applied to the concrete surface, but the object is to improve the aquatic environment by attracting fish, microorganisms and algae through biomimetic surface and increasing the number of microorganisms, and oysters are not mentioned. The object of the emulsified asphalt cement paint of the present invention is to attract oysters to attach, which is mainly oysters, but the attachment of barnacles is taken into consideration when the reinforced concrete in the tidal area has an anticorrosive effect.
[0158] (2) According to Reference 2, in cement mortar, biocalcium carbonate powder (150-200 mesh) less than 10% of the cement dosage is ineffective against adhesion by attraction. However, in the course of research into the present invention, it is found that the optimal dosage of bovine bone powder and biocalcium carbonate powder is less than 10% of the cementitious material by using an emulsified asphalt cement paint (fineness of 100-1000 mesh) mixed with modified cow bone powder and biocalcium carbonate powder.
[0159] (3) The modification of beef bone powder and biocalcium carbonate powder specifically involves treating eggshell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid, sulfurous acid, etc., and treating beef bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.
[0160] (4) In the references, it is difficult to embed oyster shells on the concrete surface, and not all project surfaces use this method, which is not feasible. The present invention can achieve the excellent effect of attracting sessile organisms by applying an emulsion asphalt cement paint layer to the concrete surface, which does not require embedding oyster shells, is not only easy to apply, but also greatly improves the amount of oyster adhesion.
[0161] (5) In recent years, serious corrosion of artificial reefs has been observed in marine environments. The serious corrosion is mainly caused by the combined action of biological sulfuric acid secreted by anaerobic microorganisms such as Thiobacillus subtilis and acidic substances secreted by other bacteria. However, calcium carbonate has very poor resistance to acid corrosion. If the content of calcium carbonate with large fineness is too high, it can cause serious acid corrosion.
[0162] Compared to Reference 3 (Fan Ruiliang: The effects of substrate type on oyster attachment, growth, population establishment and reef development [D]), the differences are as follows:
[0163] (1) In Reference 3, 80 mesh cow bone powder, calcium powder, and gypsum powder are taken and mixed into concrete separately. The fineness of all calcium materials in this invention is more than 100 mesh, which is larger than the fineness of the materials in Reference 3. In addition, modified cow bone powder is mixed in, taking into account the grading of the paint particles and their attracting ability.
[0164] (2) At room temperature, when the cow bone powder is ground by a vibrating mill and the fineness exceeds 80 mesh, the cow bone powder contains a large amount of collagen, so it becomes lumpy and cannot be ground further. In the present invention, by using the dilute acid modification technology and grinding with other substances, cow bone powder with small particle size and modified bio-calcium powder with fineness > 200 mesh can be obtained. The obtained bio-calcium powder retains the original substance of bio-calcium, improves the release rate of the substance for attracting oyster larvae to attach, and reduces the dosage of bio-calcium powder, thereby reducing the impact on paint performance.
[0165] (3) Bone powder contains a large amount of organic substances such as collagen. Mixing a large amount of these substances will result in a decrease in the strength and permeation resistance of the paint. Especially when the dosage exceeds 5%, the strength of the paint will decrease rapidly, the permeation resistance will decrease significantly, and the paint will grow mold under standard curing conditions.
[0166] The present invention uses dilute acid modification and composite crushing technology to fully utilize the attracting ability of cow bone powder, greatly reducing the dosage of cow bone powder, and carrying out anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which has a low dosage, has little effect on the performance of the paint, and at the same time has a high oyster larvae attachment ability, and solves the problem of mold growth after coating. The amount of oyster larvae attached to concrete coated with paint containing an attractant is significantly higher than that of paint without the attractant.
[0167] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that mixing an appropriate amount of calcium carbonate material into cement-based materials can promote the attachment and growth of oyster larvae. However, cement paint contains a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5. At room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5×10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment. 2+ Furthermore, while the Ca(OH)2 in the paint can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when mixing calcium carbonate material into the paint to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.
[0168] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:
[0169] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the cement-based material is diluted and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the cement-based material increases, and the amount of HCO3 in the solution increases. - The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of the cement-based material will increase rapidly, and the alkali and carbonate will be rapidly leached out, the adverse effect of the alkali will become obvious, and the critical effect or adverse effect of the carbonate will begin to appear, resulting in a decrease in the adhesion amount;
[0170] 2) With the same amount of substitute aggregate, the permeability of the cement-based material decreased with increasing dosage, and the calcium ions and OH - The leaching of calcium ions decreased, but the permeability of carbonate ions gradually improved and reached a certain value, and the attachment of oysters reached its maximum value. As the dosage continued to increase, the calcium ions decreased significantly, and carbonates may also decrease. The calcium ion concentration limited the attachment of oyster larvae, which was manifested as a decrease in the attachment amount.
[0171] 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.
[0172] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:
[0173] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to realize low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristics of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the low alkalinity sulfoaluminate cement is compounded to adjust the alkalinity of the emulsified asphalt cement paint and provide a suitable pH value for the attachment of oyster larvae. In addition, marine plants and sessile organisms such as oysters and barnacles have different alkali tolerances, and the environments required during the attachment and later stages are different. For example, the attachment, metamorphosis and later growth of barnacles and oysters require large amounts of calcium ions.
[0174] In Reference 4, concrete is used to attract marine organisms, mainly due to the size and diversity of the attached organisms, the main of which are various algae. In this invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of cement-based materials look similar, they are actually quite different.
[0175] The unique features and beneficial effects of the present invention are as follows:
[0176] dark colored substance
[0177] Taking advantage of the phototaxis of oyster eyespot larvae, emulsified asphalt is mixed into the paint to change the color of the paint, making the paint darker, making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark concrete surface by themselves, improving the contact probability between the oyster larvae and the concrete surface, and improving the probability of attracting the oyster larvae to attach. Specifically, as follows.
[0178] Marine biology researchers have looked into the use of different colored substrates to cultivate and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are two major fields entirely. The interdisciplinary fusion of marine sessile organisms and concrete materials science has led to the use of dark-colored paints to attract oyster larvae to attach. The present invention adds emulsified asphalt to darken the color of the paint and promote the attachment of oyster larvae. Since other materials are mixed into the paint, it affects its performance. The present invention considers that paints of different cements have different surface colors. Therefore, the dosage of the dark-colored material is determined based on the cement type and dosage. The emulsified asphalt also affects the performance of the paint. Most importantly, the emulsified asphalt is mixed in while the alkali and Ca in the paint are removed. 2+ If the permeability of the is not controlled, the released alkali will affect the attachment, metamorphosis and growth of the sessile organism larvae, and if the dosage exceeds a certain value, the amount of larvae attachment will decrease. In the present invention, the permeation prevention property of the emulsion asphalt cement paint is designed and controlled, and the main countermeasure is to control and modify the dosage. With the increase in the dosage of the dark color substance, the amount of larvae attachment will increase, and when the dosage is 0.5% to 6% of the cementitious material, the amount of larvae attachment is the highest, and then increases slightly or remains unchanged.
[0179] trace elements
[0180] The oyster body contains a large amount of zinc, much higher than the seawater in which it lives, and at the same time, the oyster body contains a lot of Fe, P, and K elements. At the same time, adequate Zn in the solution 2+ and K+ The concentration can promote the early attachment and metamorphosis of oyster larvae. Therefore, zinc sulfate, potassium sulfate, potassium nitrate, iron sulfate, zinc phosphate, ammonium nitrate, potassium phosphate, ammonium phosphate, iron phosphate, and calcium phosphate are used as trace elements and mixed into the paint, and the modification of these substances basically does not change the strength and penetration prevention of the paint, but greatly improves the attachment attraction rate of oyster larvae. The specific details are as follows:
[0181] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms, which belong to the field of marine biology, in order to clarify the attachment mechanism of oysters and the purpose of their cultivation and propagation. It is completely different from marine concrete engineering and concrete materials science, which are completely two major fields. Through the interdisciplinary fusion of marine sessile organisms and concrete materials science, it can be found that the corresponding substances are added to the paint to attract oyster larvae to attach to the cleat surface. Since soluble salts have a great impact on the performance of paints, such as early workability, curing time, and later strength and anti-penetration properties, the present invention uses diatomaceous earth as a carrier to fix these inorganic salts inside the diatomaceous earth, reducing the impact of soluble salts on the performance of paints, while at the same time utilizing the effect of diatomaceous earth in improving the performance of emulsified asphalt cement paints, and realizing that the excellent performance of emulsified asphalt cement paints can be maintained even when these attractants are added. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, especially after immersion in seawater for a certain period of time, the release rate is kept at a very low level. Therefore, similarly, this part of knowledge is related to the interdisciplinary fusion of marine sessile organisms, chemistry, and marine concrete engineering, and whether it is a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, due to the conventional background, in the present invention, by mixing trace elements into concrete, changing the ion content of trace elements on the paint surface, and controlling the permeability of the paint, it is not possible to obtain technical features closely related to the paint with excellent ability to attract oyster larvae to attach.
[0182] Paint penetration
[0183] The strength and permeability of the paint are of utmost importance. Mixing different attractants into the cement paint will affect the performance of the paint, so when mixing different substances to promote the attachment, metamorphosis and later growth of oyster larvae, first, it is necessary to control it as a whole so as not to have a significant effect on the performance of the paint, and secondly, select the raw materials according to the suitability of various raw materials, and if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related studies consider the effect of calcium content on the attachment of oyster larvae, but do not consider the performance of the paint itself, and do not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of the paint will change the permeability of the alkali and ions inside it, and the lower the permeability prevention of the paint, the higher the permeability of the alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkalis and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may be more serious, especially when the cement dosage is high. Therefore, it is necessary to ensure that the change in the performance of the paint by mixing the attractant into the paint is within a controllable range, for example, the change does not exceed 10%, so that their attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect on oyster larvae cannot be evaluated.
[0184] It is necessary to grasp the optimal environment required for marine sessile organisms to attach, transform and grow later, and to design the paint starting from the penetration prevention of the paint, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the penetration prevention of the paint. Therefore, similarly, this part of the knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, according to the conventional background, in the present invention, the overall control of the penetration prevention of the paint cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.
[0185] Therefore, similarly, this part of knowledge is related to the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and whether one is skilled in the field of concrete engineering or marine biology, according to References 1-2, the color change by mixing emulsified asphalt into the paint, the modification of cow bone powder, the crushing technique, and the control of the permeability of the paint cannot obtain technical features closely related to the ability to effectively attract oysters to attach and the paint having high durability. Also, according to Reference 4, the reduction in alkalinity of the paint and the balance of calcium ion concentration cannot obtain technical features closely related to the attachment of marine sessile organisms.
[0186] Although embodiments of the present invention will be shown and described, it will be understood that those skilled in the art can make various changes, modifications, substitutions and variations to these embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the claims and their equivalents.
Claims
1. A method for constructing a waste concrete marine ecological project, comprising: (1) A step of investigating the sea area where the breakwater is to be constructed, investigating the dominant species of oysters in the sea area and the presence or absence of oyster attachment, and investigating the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in different seasons in the sea area. 2+ , Zn 2+ , and K + and further investigating the number of typhoons that have occurred in the past and their intensity. (2) A step of producing a concrete adhesion base, the shape of which is one of a plate-shaped adhesion base, a corrugated adhesion base, and a cylindrical adhesion base, and a step of producing a lightweight concrete scratch adhesion base having a rough surface; (3) A step of quantitatively harvesting and cultivating oyster larvae, in which an attachment base is placed in a nearby sea area during the period when the oyster floating larvae in the local sea area are concentrated and attached and metamorphosed, and the attachment amount of oyster larvae is 15 to 25 pieces / 100 cm 2 The step of stopping seedling collection for the attachment base of oysters, and then transferring the attachment base with an attachment amount of 15 to 25 oyster larvae per 100 cm 2 to a sea area rich in food for floating culture; (4) A step of treating the surface of the waste concrete block, which includes evaluating the alkalinity, internal ion concentration, and permeability of the waste concrete, and reducing the alkalinity when the pH is > 12.5; and then spraying or applying an emulsified asphalt cement paint that has high adhesive strength and effectively attracts oysters to the surface of the waste concrete block; (5) placing waste concrete blocks, in the second year, during the period when oyster larvae are concentrated in local waters to attach and metamorphose, and placing waste concrete blocks with a volume of more than 1 cubic meter separately, covering each waste concrete block with a rope cage, and the rope cage covers a plurality of waste concrete blocks with a volume of less than 1 cubic meter, forming a pile of waste concrete blocks with a volume of 1 to 5 cubic meters, the internal porosity of which is 40% to 60%, and connecting the waste concrete blocks or piles of waste concrete blocks with rope; (6) For the placement of the oyster-attached substrate on site, the substrate with oysters at the mature stage of gonad development in (5) is transported to the construction area of the breakwater, and one or two oyster-attached substrates are placed for each waste concrete block or pile of waste concrete blocks, and the waste concrete block or pile of waste concrete blocks is fixed with a rope; (7) A step of monitoring and managing the attachment of oyster larvae, in which the attachment status of oyster larvae on the concrete surface is monitored, and the attachment amount of oysters is 30 to 40 pieces / 100 cm 2 and removing the adhesion base of the waste concrete from the breakwater and monitoring the ecological condition of the breakwater in the long term.
2. The oyster adhesion base is composed of cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, short fibers and superplasticizer, and the weight percentages of the cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, short fibers and superplasticizer are 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4%, 0.6% to 3.0%, 0.4% to 2.0%, 0.4% to 2.0%, 0.2% to 1.8%, 0.15% to 1.5% and 0.03% to 0.18%, The bio-calcium powder is a combination of one or more of cow bone powder, oyster shell powder, fish bone powder, eggshell powder, and coral powder; 2. The method for constructing a marine ecological project of waste concrete according to claim 1, characterized in that the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers and ultrafine precipitated calcium carbonate.
3. In the raw material of the oyster attachment base, the dark pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red, and the dark pigment is modified, and one of transparent resin, organic silicon, dimethylsiloxane, and superhydrophobic material is used for the modification treatment; The trace elements are zinc, iron, potassium and phosphorus, which can be modified by selecting natural minerals, industrial products or chemical reagents containing one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to achieve sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance; but in the case of eutrophication areas, do not select materials containing nitrogen or phosphorus elements; The cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, in which the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material is one of alkali-activated slag, and alkali-activated slag + fly ash; The lightweight coarse aggregate is one or two of crushed lightweight porous basalt having a maximum particle size of less than 20 mm and lightweight ceramsite; The lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm; The method for constructing a marine ecological project using waste concrete according to claim 2, characterized in that the short fibers are inorganic fibers (length 12-20 mm), such as one or more of basalt fibers, alkali-resistant glass fibers, and carbon fibers.
4. The emulsified asphalt cement paint is composed of cementitious material, emulsified asphalt, sand, water, bio-calcium powder, calcium carbonate powder, trace elements, acrylic emulsion and superplasticizer, and the weight ratio of the cementitious material, emulsified asphalt, sand, water, bio-calcium powder, calcium carbonate powder, trace elements, acrylic emulsion and superplasticizer is 1:(0.4-0.8):(0.5-1.3):(0.10-0.30):(0.02-0.10):(0.02-0.10):(0.01-0.08):(0.08-0.15):(0.001-0.008) in this order.
5. Regarding the raw material of the emulsified asphalt cement paint, the bio-calcium powder includes one or more combinations of cow bone powder, oyster shell powder, eggshell powder, and coral powder, the fineness of which is 100 mesh to 1000 mesh, and also treats egg shell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid, and sulfurous acid, and treats cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid; The calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultrafine precipitated calcium carbonate, and has a fineness of more than 200 mesh; The trace elements zinc, iron, potassium and phosphorus can be modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to achieve sustained release of the corresponding ions and reduce or eliminate the adverse effects on concrete performance; however, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements should not be selected; The emulsified asphalt is one of cationic emulsified asphalt and anionic emulsified asphalt, and its performance index is evaporation residue content > 55%, 5-day stability ≦ 5%, sieve diameter 1.18mm, sieve residue ≦ 0.1%; The cementitious material is one of a Portland cement mixed with a mineral admixture, a sulfoaluminate cement, and an alkali-activated cementitious material, where the Portland cement mixed with a mineral admixture comprises a combination of one or more of silica fume, slag powder, and fly ash, the sulfoaluminate cement comprises one or two of a fast-setting sulfoaluminate cement, a high-strength sulfoaluminate cement, and an expanded sulfoaluminate cement, and the alkali-activated cementitious material comprises one of an alkali-activated slag, and an alkali-activated slag + fly ash; The sand is one or more of river sand, machine-made sand, and sea sand having a particle size of 0.16 mm to 2.36 mm; 5. The method for constructing a marine ecological project using waste concrete as claimed in claim 4, wherein the superplasticizer is one of polycarboxylic acid and naphthalene-based.
6. The method for constructing a marine ecological project using waste concrete as claimed in claim 1, wherein the period of concentrated attachment and metamorphosis of the oyster larvae is from April to October.
7. The construction method for the waste concrete marine ecological project according to claim 1, characterized in that, in the oyster attachment base, a round hole with a diameter of 3-5 mm is created during molding, and the size of the plate-shaped attachment base is 10 x 10 x 2-3 cm.
8. 2. The method for constructing a marine ecological project using waste concrete as claimed in claim 1, wherein the rope is one of palm rope, glass fiber rope, and basalt fiber rope.
Citation Information
Patent Citations
Novel concrete artificial fish reef and preparation method thereof
CN104529286A
Bionic concrete artificial fish reef and preparation method thereof
CN104938384A
Seed adhering method for oysters
CN107372242A
Coral-imitating porous structural material for modification of marine environment and preparation method of coral-imitating porous structural material
CN107805037A
Marine environment concrete crack repair material and preparation method thereof
CN109467354A