Articles containing expanded poly(tetramethyl-p-silphenylene siloxane) and methods for making same

Poly(tetramethyl-p-silphenylene siloxane) polymers address the need for non-fluoropolymer articles by providing high-strength, porous articles with crystallinity and fibril microstructures, suitable for diverse applications through processing methods like lubrication and stretching, achieving high matrix tensile strength and porosity without fluorocarbons.

JP7576098B2Active Publication Date: 2024-10-30WL GORE & ASSOC INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022560256
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-03
Filing Date
2021-03-31
Publication Date
2024-10-30
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

There is a need for non-fluoropolymer articles that exhibit properties such as high strength, high porosity, and high crystallinity, similar to those of microporous fluoropolymer membranes, particularly in applications like water filtration, dialysis, battery separators, and gas separation, while avoiding the use of fluorochemical compounds.

Method used

The development of poly(tetramethyl-p-silphenylene siloxane) polymers with a melting point of 130°C to 150°C, crystallinity of at least 70%, and a microstructure of nodes interconnected by fibrils, which can be processed below their melting temperature to form articles with high porosity and strength, including methods like lubrication, calendering, and stretching to create porous and dense articles.

Benefits of technology

The poly(tetramethyl-p-silphenylene siloxane) polymers achieve high matrix tensile strength, matrix modulus, and porosity, with asymmetric pore sizes and the ability to incorporate filler materials or bioactive moieties, making them suitable for various applications without the use of fluorocarbons.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576098000006
    Figure 0007576098000006
  • Figure 0007576098000007
    Figure 0007576098000007
  • Figure 0007576098000008
    Figure 0007576098000008
Patent Text Reader

Abstract

Poly(tetramethyl-p-silphenylenesiloxane) (PTMPS) membranes and porous articles made therefrom are provided, having a matrix tensile strength of about 1 MPa to about 50 MPa in at least one direction, a matrix modulus of greater than about 100 MPa in at least one direction, a porosity of greater than about 30%, and a microstructure of nodes interconnected by fibrils. The PTMPS polymer forming the PTMPS membranes and porous articles has a crystallinity of at least about 70%, a polydispersity of 1 to 5, and a weight average molecular weight of about 350 kDa to about 5 MDa. The PTMPS membranes can be asymmetric, meaning that the pore structure observed on one side of the PTMPS membrane is different from the pore structure on the opposite side of the PTMPS membrane. Methods for forming porous PTMPS articles are also provided. Dense PTMPS articles and methods for making them are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to poly(tetramethyl-p-silphenylene siloxane), and more specifically to porous articles comprising expanded poly(tetramethyl-p-silphenylene siloxane) membranes having a melting point of about 130° C. to about 150° C. and a node-and-fibril microstructure. Methods for forming porous and dense articles containing poly(tetramethyl-p-silphenylene siloxane) polymers are also provided. [Background technology]

[0002] It is known in the art that microporous fluoropolymer membranes are useful in a variety of applications. Articles made from microporous fluoropolymer membranes have properties such as toughness, impact strength, low coefficient of friction, and resistance to attack by solvents and corrosive chemicals. Due to the favorable properties associated with microporous fluoropolymer membranes, microporous fluoropolymer membranes have been utilized in a variety of applications such as water filtration, dialysis, battery separators, vents, desalination, and gas separation.

[0003] Although microporous fluoropolymer membrane articles have attractive properties and are used in many applications, there is a recent movement away from the use of fluorochemical compounds.Therefore, there is a need in the art for non-fluoropolymer articles that at least exhibit the promising properties that fluoropolymers exhibit.In particular, there is a need for a method for producing poly(tetramethyl-p-silphenylenesiloxane) articles that are processed below melting temperature and have high strength, high porosity and high crystallinity. Summary of the Invention

[0004] According to one embodiment ("Embodiment 1"), the poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a melting point of about 130°C to about 150°C, a crystallinity of at least about 70%, a porosity of greater than about 30%, and a microstructure of nodes interconnected by fibrils.

[0005] According to another embodiment ("embodiment 2"), further to embodiment 1, the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%.

[0006] According to another embodiment ("embodiment 3"), in addition to embodiments 1 and 2, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity of greater than about 30%.

[0007] According to another embodiment ("Embodiment 4"), in addition to any of the embodiments described above, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa.

[0008] According to another embodiment ("Embodiment 5"), in addition to any of the embodiments described above, the stretched poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix modulus in at least one direction of from about 100 MPa to about 1000 MPa.

[0009] According to another embodiment ("Embodiment 6"), in addition to any of the embodiments described above, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a poly(tetramethyl-p-silphenylene siloxane) polymer having a weight average molecular weight of about 350 kDa to 5 MDa.

[0010] According to another embodiment ("embodiment 7"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5.

[0011] According to another embodiment ("Embodiment 8"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer film includes at least one comonomer in an amount of about 0.001 mol% to about 10 mol%.

[0012] According to another embodiment ("Embodiment 9"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer film comprises at least one filler material.

[0013] According to another embodiment ("embodiment 10"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a biologically active moiety therein.

[0014] According to another embodiment ("Embodiment 11"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer membrane has an asymmetric pore size from the first side to the second side.

[0015] According to another embodiment ("embodiment 12"), in addition to any of the embodiments above, the fibrils comprise polymer chains, the polymer chains being oriented along a fibril axis.

[0016] According to another embodiment ("embodiment 13"), in addition to any of the embodiments described above, each of the fibrils comprises extended chain crystals.

[0017] According to another embodiment ("Embodiment 14"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer article is in the form of a fiber, a tube, a tape, a sheet, or a three-dimensional free-standing structure.

[0018] According to another embodiment ("Embodiment 15"), in addition to any one of embodiments 1-14, a composite comprises the poly(tetramethyl-p-silphenylene siloxane) article.

[0019] According to another embodiment ("embodiment 16"), in addition to any one of embodiments 1-14 or embodiment 15, the laminate includes a poly(tetramethyl-p-silphenylene siloxane) polymer article.

[0020] According to another embodiment ("Embodiment 17"), in addition to any one of embodiments 1-14, the device includes a porous poly(tetramethyl-p-silphenylene siloxane) polymer article.

[0021] According to one embodiment ("Embodiment 18"), a method of making a poly(tetramethyl-p-silphenylene siloxane) polymer article includes lubricating a poly(tetramethyl-p-silphenylene siloxane) polymer having a melting point of about 130°C to about 150°C and a crystallinity of at least 70% to form a lubricated poly(tetramethyl-p-silphenylene siloxane) polymer, pressing the lubricated poly(tetramethyl-p-silphenylene siloxane) polymer at a temperature of 60°C to 140°C to form a preform, and stretching the preform at a temperature of 60°C to 140°C to form a porous poly(tetramethyl-p-silphenylene siloxane) polymer article having a structure of nodes interconnected by fibrils.

[0022] According to another embodiment ("Embodiment 19"), in addition to embodiment 18, the method includes calendering the lubricated poly(tetramethyl-p-silphenylene siloxane) polymer at a temperature between 60°C and 140°C to form a preform, or ram extruding the lubricated poly(tetramethyl-p-silphenylene siloxane) polymer at a temperature between 60°C and 140°C to form a preform.

[0023] According to another embodiment ("embodiment 20"), in addition to embodiments 18 and 19, the method includes removing lubricant from the preform before stretching.

[0024] According to another embodiment ("embodiment 21"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa.

[0025] According to another embodiment ("embodiment 22"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5.

[0026] According to another embodiment ("Embodiment 23"), in addition to any of the embodiments described above, the method includes compressing the porous poly(tetramethyl-p-silphenylene siloxane) polymer article to form a dense poly(tetramethyl-p-silphenylene siloxane) polymer article.

[0027] According to another embodiment ("embodiment 24"), in addition to any of the above embodiments, the method includes adding one of a filler material and a bioactive moiety to the poly(tetramethyl-p-silphenylene siloxane) polymer.

[0028] According to another embodiment ("Embodiment 25"), in addition to any of the embodiments described above, the poly(tetramethyl-p-silphenylene siloxane) polymer article has an asymmetric pore size from the first side to the second side.

[0029] According to one embodiment ("Embodiment 26"), a method for making a poly(tetramethyl-p-silphenylene siloxane) polymer article includes pressurizing and heating a poly(tetramethyl-p-silphenylene siloxane) polymer having a melting point of 130°C to 150°C and a crystallinity of at least 70% at a temperature of 60°C to 140°C to form a preform article, and subsequently stretching the preform article at a temperature of 60°C to 140°C to form a porous poly(tetramethyl-p-silphenylene siloxane) polymer article.

[0030] According to another embodiment ("embodiment 27"), in addition to embodiment 26, the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa.

[0031] According to another embodiment (“embodiment 28”), further to embodiment 26 or embodiment 27, the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5.

[0032] According to another embodiment ("embodiment 29"), further to embodiments 26-28, the porous poly(tetramethyl-p-silphenylene siloxane) polymer article has a porosity of greater than about 30%.

[0033] According to another embodiment ("Embodiment 30"), in addition to embodiments 26-29, the method includes compressing the porous poly(tetramethyl-p-silphenylene siloxane) polymer article to form a dense poly(tetramethyl-p-silphenylene siloxane) polymer article.

[0034] According to one embodiment ("Embodiment 31"), a method of making a poly(tetramethyl-p-silphenylene siloxane) polymer article includes casting a poly(tetramethyl-p-silphenylene siloxane) polymer solution onto a substrate to form a cast poly(tetramethyl-p-silphenylene siloxane) polymer tape, drying the poly(tetramethyl-p-silphenylene siloxane) polymer tape to form a dried cast poly(tetramethyl-p-silphenylene siloxane) polymer tape, and removing the cast microporous poly(tetramethyl-p-silphenylene siloxane) polymer tape from the substrate.

[0035] According to another embodiment ("Embodiment 32"), in addition to embodiment 31, the method includes stretching the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape to form an expanded poly(tetramethyl-p-silphenylene siloxane) membrane having a node and fibril microstructure.

[0036] According to another embodiment ("embodiment 33"), in addition to embodiment 31 or embodiment 32, the drying comprises air drying, vacuum drying, and combinations thereof.

[0037] According to another embodiment ("Embodiment 34"), in addition to any one of embodiments 31-33, the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape has an asymmetric pore size from the first side to the second side of the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape.

[0038] According to another embodiment ("Embodiment 35"), in addition to embodiments 31-34, the poly(tetramethyl-p-silphenylene siloxane) polymer solution includes a poly(tetramethyl-p-silphenylene siloxane) polymer and an organic solvent.

[0039] According to another embodiment ("embodiment 36"), in addition to embodiments 31-35, the substrate is a porous or non-porous substrate.

[0040] According to another embodiment ("Embodiment 37"), in addition to embodiments 31-36, the substrate is a non-porous substrate, and the non-porous substrate is selected from a glass dish, a glass plate, polytetrafluoroethylene, polyethylene, polypropylene, and polyethylene terephthalate.

[0041] According to another embodiment ("Embodiment 38"), in addition to embodiments 31-37, the method includes cutting the dried cast poly(tetramethyl-p-silphenylene siloxane) tape to a desired size before stretching.

[0042] According to another embodiment ("embodiment 39"), in addition to embodiments 31-38, the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%.

[0043] According to another embodiment ("embodiment 40"), further to embodiments 31-39, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity greater than about 30%.

[0044] According to another embodiment ("Embodiment 41"), further to embodiments 31-40, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa.

[0045] According to another embodiment ("Embodiment 42"), further to embodiments 31-41, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix modulus in at least one direction of from about 100 MPa to about 1000 MPa.

[0046] According to another embodiment ("embodiment 43"), further to embodiments 31-42, the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa.

[0047] According to one embodiment ("Embodiment 44"), a method for making a dense article includes feeding poly(tetramethyl-p-silphenylene siloxane) polymer powder directly into the nip of two calender rolls to produce a coherent dense poly(tetramethyl-p-silphenylene siloxane) tape.

[0048] According to one embodiment ("Embodiment 45"), a method includes casting a poly(tetramethyl-p-silphenylene siloxane) polymer solution onto a substrate to form a cast poly(tetramethyl-p-silphenylene siloxane) polymer tape, submerging the cast poly(tetramethyl-p-silphenylene siloxane) polymer tape in a non-solvent bath for solvent-induced phase separation, removing the cast poly(tetramethyl-p-silphenylene siloxane) polymer tape from the substrate, and drying the cast poly(tetramethyl-p-silphenylene siloxane) polymer tape to form a microporous cast poly(tetramethyl-p-silphenylene siloxane) polymer tape.

[0049] According to another embodiment ("Embodiment 46"), in addition to embodiment 45, the method includes stretching the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape to form an expanded poly(tetramethyl-p-silphenylene siloxane) membrane having a node and fibril microstructure.

[0050] According to another embodiment ("embodiment 47"), in addition to embodiment 45 or embodiment 46, the method includes cutting the dry cast poly(tetramethyl-p-silphenylene siloxane) polymer tape before stretching.

[0051] According to another embodiment ("embodiment 48"), in addition to embodiments 45-47, the substrate is a porous or non-porous substrate.

[0052] According to another embodiment ("Embodiment 49"), in addition to embodiments 45-48, the substrate is a non-porous substrate, and the non-porous substrate is selected from a glass dish, a glass plate, polytetrafluoroethylene, polyethylene, polypropylene, and polyethylene terephthalate.

[0053] According to another embodiment ("embodiment 50"), in addition to embodiments 45-49, the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%.

[0054] According to another embodiment ("Embodiment 51"), in addition to embodiments 45-50, the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape has an asymmetric pore size from a first side to a second side of the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape.

[0055] According to another embodiment ("embodiment 52"), further to embodiments 45-51, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity greater than about 30%.

[0056] According to another embodiment ("embodiment 53"), further to embodiments 45-52, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa.

[0057] According to another embodiment ("Embodiment 54"), further to embodiments 45-53, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix modulus in at least one direction of from about 100 MPa to about 1000 MPa.

[0058] According to another embodiment ("Embodiment 55"), in addition to embodiments 45-54, the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a poly(tetramethyl-p-silphenylene siloxane) polymer having a weight average molecular weight of about 350 kDa to 5 MDa.

[0059] According to one embodiment ("Embodiment 56"), a poly(tetramethyl-p-silphenylene siloxane) polymer tape formed from a poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least about 70%, a polydispersity of 1 to 5, and a weight average molecular weight of about 350 kDa to about 5 MDa.

[0060] According to another embodiment ("Embodiment 57"), in addition to embodiment 56, the poly(tetramethyl-p-silphenylene siloxane) polymer tape is opaque.

[0061] According to another embodiment ("Aspect 58"), in addition to embodiment 56 or embodiment 57, the poly(tetramethyl-p-silphenylene siloxane) polymer tape is formed using a casting method, a solvent-induced casting method, a paste calendaring method, or a paste extrusion method.

[0062] According to one embodiment ("Embodiment 59"), the article includes a poly(tetramethyl-p-silphenylene siloxane) polymer cast tape.

[0063] According to another embodiment ("Embodiment 60"), in addition to embodiment 59, the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape has asymmetric pore size from a first side to a second side of the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape.

[0064] According to another embodiment ("embodiment 61"), in addition to embodiment 59 or embodiment 60, the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%.

[0065] According to another embodiment ("embodiment 62"), in addition to embodiments 59-61, the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa.

[0066] According to one embodiment ("Embodiment 63"), a method for making a poly(tetramethyl-p-silphenylene siloxane) polymer article includes lubricating a poly(tetramethyl-p-silphenylene siloxane) polymer having a melting point of about 130°C to about 150°C and a crystallinity of at least 70% with a lubricant to form a poly(tetramethyl-p-silphenylene siloxane) powder / lubricant mixture, and paste extruding the poly(tetramethyl-p-silphenylene siloxane) powder / lubricant mixture to form cohesive PTMPS beads, tapes, tubes, or three-dimensional free-standing structures.

[0067] According to another embodiment ("Embodiment 64"), in addition to embodiment 63, the method includes tumbling the poly(tetramethyl-p-silphenylene siloxane) polymer powder / oil mixture prior to paste extrusion.

[0068] According to another embodiment ("Aspect 65"), in addition to embodiment 63 or embodiment 64, the method includes thermally conditioning the poly(tetramethyl-p-silphenylene siloxane) polymer powder / oil mixture prior to paste extrusion.

[0069] According to another embodiment ("Embodiment 66"), in addition to embodiments 63-65, the method includes stretching cohesive poly(tetramethyl-p-silphenylenesiloxane) polymer beads to form a stretched poly(tetramethyl-p-silphenylenesiloxane) polymer film.

[0070] According to another embodiment ("embodiment 67"), in addition to embodiments 63-66, the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa.

[0071] According to another embodiment ("embodiment 68"), further to embodiments 63-67, the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5. [Brief description of the drawings]

[0072] The accompanying drawings are included to provide a further understanding of the disclosure, are incorporated in and constitute a part of this specification, illustrate embodiments, and together with the description, serve to explain the principles of the disclosure.

[0073] [Figure 1A] FIG. 1A is a scanning electron micrograph (SEM) of the dried cast PTMPS film of Example 3 showing the pore structure of the air side of the PTMPS film according to some embodiments.

[0074] [Figure 1B] FIG. 1B is a scanning electron micrograph (SEM) of the dried cast PTMPS of Example 3 showing the pore structure of the glass side of the PTMPS film according to some embodiments.

[0075] [Figure 1C] FIG. 1C is a scanning electron micrograph (SEM) of a cross-section of a dried cast PTMPS film of Example 3 according to some embodiments.

[0076] [Figure 2A]FIG. 2A is a scanning electron micrograph (SEM) of the uniaxially stretched PTMPS membrane of Example 4, showing the presence of node-and-fibril microstructure on the glass side of the cast PTMPS membrane.

[0077] [Figure 2B] FIG. 2B is a scanning electron micrograph (SEM) of the uniaxially stretched PTMPS membrane of Example 4, showing the presence of a microporous node-and-fibril microstructure on the air side of the cast PTMPS membrane according to some embodiments. [Figure 2C] FIG. 2C is a scanning electron micrograph (SEM) of the uniaxially stretched PTMPS membrane of Example 4, showing the presence of a microporous node-and-fibril microstructure on the air side of the cast PTMPS membrane according to some embodiments.

[0078] [Figure 3A] FIG. 3A is a scanning electron micrograph of the biaxially stretched PTMPS membrane of Example 5, showing the presence of node-and-fibril microstructure on the glass side of the cast PTMPS membrane according to some embodiments.

[0079] [Figure 3B] FIG. 3B is a scanning electron micrograph (SEM) of the biaxially stretched PTMPS membrane of Example 5, showing the presence of node-and-fibril microstructure on the air-side of the cast PTMPS membrane according to some embodiments. [Figure 3C] FIG. 3C is a scanning electron micrograph (SEM) of the biaxially stretched PTMPS membrane of Example 5, showing the presence of node-and-fibril microstructure on the air-side of the cast PTMPS membrane according to some embodiments.

[0080] [Figure 3D] FIG. 3D is a scanning electron micrograph (SEM) of a cross-section of the PTMPS membrane of Example 5, according to some embodiments.

[0081] [Figure 4]FIG. 4 is a scanning electron micrograph (SEM) of the uniaxially stretched PTMPS membrane of Example 8, showing a node-and-fibril microstructure according to some embodiments.

[0082] [Diagram 5] FIG. 5 is a scanning electron micrograph (SEM) of a cross-section of the PTMPS membrane of Example 10, showing a microporous node-and-fibril microstructure according to some embodiments.

[0083] [Figure 6] FIG. 6 is a scanning electron micrograph (SEM) of the expanded PTMPS membrane of Example 16, showing a porous node-and-fibril microstructure, according to some embodiments.

[0084] [Figure 7] FIG. 7 is a scanning electron micrograph of the expanded PTMPS membrane of Example 17, showing a porous node-and-fibril microstructure.

[0085] [Figure 8] FIG. 8 is a scanning electron micrograph (SEM) of the biaxially stretched PTMPS membrane of Example 18, showing a porous node-and-fibril microstructure according to some embodiments.

[0086] [Figure 9] FIG. 9 is a differential scanning calorimetry (DSC) showing the melting point of precipitated PTMPS polymer at 127° C. according to some embodiments.

[0087] [Figure 10] FIG. 10 is a DSC showing the melting point of PTMPS powder at 129° C. according to some embodiments.

[0088] [Figure 11] FIG. 11 is an SEM of a simultaneously biaxially stretched PTMPS membrane; and

[0089] [Figure 12]FIG. 12 is a DSC showing extended chain crystals associated with the fibrils. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0090] Those skilled in the art will readily appreciate that the various aspects of the present disclosure may be implemented by any number of methods and devices configured to perform the intended functions. It should also be noted that the accompanying figures referenced herein are not necessarily drawn to scale and may be exaggerated to illustrate various aspects of the present disclosure, and in that respect the figures should not be construed as limiting. It should be understood that the terms "melting temperature", "melting temperature" and melting point may be used interchangeably herein.

[0091] The present disclosure relates to poly(tetramethyl-p-silphenylene siloxane) (PTMPS) membranes and porous articles processed below the melting temperature of poly(tetramethyl-p-silphenylene siloxane) and having high strength, high porosity and high crystallinity. The crystallinity of PTMPS polymers can be measured by differential scanning calorimetry (DSC). In addition, PTMPS membranes have a higher and broader melting temperature compared to PTMPS polymers, from about 130°C to about 150°C, indicating that the original lamellar crystals have been partially converted to extended chain crystals. In addition, PTMPS membranes can be asymmetric, meaning that the pore structure observed on one side of the PTMPS membrane is different from the pore structure on the opposite side of the PTMPS membrane. In some embodiments, based on scanning electron microscopy (SEM) of porous PTMPS membrane samples, the pore size gradually increases from one side of the PTMPS membrane to the opposite side of the PTMPS membrane.

[0092] PTMPS polymer formation In forming the PTMPS polymer, in one embodiment, anhydrous benzene is added to the 1,4-bis(hydroxydimethylsilyl)benzene monomer produced in Example 1 (described below) in a jacketed glass reactor to form a reaction mixture. Tetramethylguanidinium bis-2-ethylhexanoate catalyst is added to the reactor while the reaction mixture is heated to a high reflux temperature. The reaction mixture is then refluxed. After reflux, the reaction mixture is cooled to 35° C. and the poly(tetramethyl-p-silphenylenesiloxane) (PTMPS) polymer is precipitated in methanol. The PTMPS polymer is dried under vacuum. The dried PTMPS polymer has a weight average molecular weight of about 460 kilodaltons (kDa) and a polydispersity of 1.8. The melting point of the precipitated PTMPS polymer is 127° C. based on differential scanning calorimetry (DSC) (see FIG. 9).

[0093] In another embodiment, PTMPS polymer can be formed by adding anhydrous benzene to 1,4 bis(hydroxydimethylsilyl)benzene monomer as produced in Example 1 in a reactor to create a slurry. Tetramethylguanidinium bis-2-ethylhexanoate catalyst is added to the reactor while the reaction mixture is heated to high reflux temperature. The PTMPS polymer is precipitated in methanol at room temperature and dried under vacuum. The dried PTMPS polymer is characterized using size exclusion chromatography (SEC). The weight average molecular weight of the PTMPS polymer is determined to be 356 kilodaltons (kDa) with a polydispersity of 1.7.

[0094] In a further embodiment, PTMPS polymer can be made by adding anhydrous toluene to 1,4 bis(hydroxydimethylsilyl)benzene monomer as prepared in Example 11 to make a slurry. 1,1,3,3-tetramethylguanidine catalyst is then added to the reactor while the reaction mixture is heated to high reflux temperature. The PTMPS polymer is precipitated in methanol at room temperature and dried under vacuum. The dried PTMPS polymer is characterized using size exclusion chromatography (SEC). The weight average molecular weight of the PTMPS polymer is determined to be one million daltons (1 MDa) with a polydispersity of 2.

[0095] In yet another embodiment, PTMPS powder can be produced from PTMPS polymer. For example, PTMPS polymer as produced in Example 2 below can be dissolved in 1,3,5-trimethylbenzene in a jacketed glass reactor. After maintaining the reactor at a temperature of 80° C. for 3 hours, the reactor is cooled and the reaction mixture is gently stirred. After 24 hours, crystallized particles of PTMPS are visible in the reactor. The PTMPS wet powder is washed with excess methanol and dried to obtain PTMPS powder. The melting point of the PTMPS powder is 129° C. using DSC (see FIG. 10).

[0096] Paste-processed PTMPS polymer powder In one embodiment, the PTMPS polymer powder can be formed into a microporous article by pasting the PTMPS polymer powder. When forming a porous article from the PTMPS polymer powder, the PTMPS polymer powder is first mixed with a lubricant, such as a light oil. Other suitable lubricants include aliphatic hydrocarbons, aromatic hydrocarbons, and the like, and are selected according to flammability, evaporation rate, and economic considerations. It should be understood that the term "lubricant" as used herein is intended to describe a processing aid that includes (or consists of) an incompressible fluid that is not a solvent for the polymer at the process conditions. The surface interaction of the fluid and the polymer can create a homogeneous mixture. It should also be noted that the choice of lubricant is not particularly limited, and the choice of lubricant is primarily a matter of safety and convenience. It should be understood that any of the lubricants described herein can be utilized as a lubricant, so long as the fluid-polymer surface interaction is such that a homogeneous mixture can be produced. The lubricant may be added to the PTMPS polymer powder in a ratio of about 1 ml / 100 g to about 100 ml / 100 g, or about 10 ml / 100 g to about 70 ml / 100 g.

[0097] In at least one embodiment, the PTMPS polymer powder and the lubricant are mixed to distribute the lubricant uniformly or substantially uniformly throughout the mixture. As used herein, "substantially uniform" is meant to indicate that the powder is distributed as uniformly as possible, with no visible agglomeration of the powder. It is understood that various times and mixing methods can be used to distribute the PTMPS polymer powder in the lubricant. In one embodiment, the lubricated PTMPS polymer powder is heated to a temperature below the melting temperature of the PTMPS polymer powder and above 70°C, the solid / state transition of the PTMPS polymer. Sufficient pressure and shear can be applied to form interparticle bonds and create a solid shape. Non-limiting examples of solid forms that can be formed without exceeding the melting temperature of the PTMPS polymer include fibers, tubes, tapes, sheets, and three-dimensional free-standing structures. Non-limiting examples of methods of applying pressure and shear include paste extrusion (e.g., ram extrusion, calendering, and combinations thereof).

[0098] In one embodiment, once the PTMPS polymer powder and lubricant are blended, the PTMPS polymer powder is calendered to produce a cohesive flexible tape. As used herein, the term "cohesive" is intended to describe a tape that is strong enough for further processing. Calendering is performed at a temperature below the melting point of the PTMPS polymer, such as, for example, about 140°C or less, or 60°C to 140°C, 75°C to 130°C, 80°C to 125°C, 90°C to 120°C, or 80°C to 110°C. The length of the tape formed is variable and the thickness is less than 100 μm. Tapes having thicknesses of about 10 μm to about 500 μm, about 15 μm to about 250 μm, or about 25 μm to about 150 μm can be formed. In another embodiment, the lubricated PTMPS polymer powder can be ram extruded to produce a cohesive PTMPS tape.

[0099] In the next step, the lubricant can be removed from the PTMPS tape. In the case where mineral oil is used as the lubricant, the lubricant can be removed by washing the tape with methanol, hexane or other suitable solvent. The washing solvent is selected to have good solubility for the lubricant and sufficient volatility to be removed below the melting point of the PTMPS polymer. If the lubricant has sufficient volatility, the lubricant can be removed without a washing step or can be removed by heat and / or vacuum. The PTMPS tape is then optionally dried, typically by air drying. However, any conventional drying method can be used as long as the temperature to which the PTMPS tape is heated remains below the melting point of the PTMPS polymer.

[0100] Once dried, the tape can be cut to the appropriate size for stretching. Stretching of the sample occurs at a temperature below the melting temperature of the PTMPS polymer. In some embodiments, the sample is stretched at a temperature between 60°C and 140°C, 75°C and 130°C, 80°C and 125°C, 90°C and 120°C, or 80°C and 110°C. The sample can be stretched in one or more directions (i.e., uniaxially or biaxially) to form a porous (e.g., microporous) PTMPS membrane. Biaxial stretching of the PTMPS tape can occur sequentially or simultaneously. Either uniaxial or biaxial stretching can be performed at a rate of about 0.1% / sec to about 1000% / sec, about 1% / sec to about 500% / sec, or about 10% / sec to about 100% / sec. The porous microstructure of the stretched membrane is affected by the temperature and speed of stretching. The node and fibril geometry can be controlled by the selection of the PTMPS polymer, the stretching speed, the stretching temperature, and / or the total amount of stretching. The tapes are also suitable for continuous processing, for example into porous PTMPS articles. Furthermore, the porous PTMPS polymer films can be compressed to form dense poly(tetramethyl-p-silphenylenesiloxane) polymer articles with porosity of 10% or less.

[0101] Casting method for forming porous PTMPS articles In at least one embodiment, the PTMPS polymer can be formed into a microporous article by a casting method. In some embodiments, the PTMPS polymer formed as described above is placed in a solution containing an organic solvent, such as p-xylene, to create a PTMPS solution of the desired wt%. As an example, p-xylene can be added to the PTMPS polymer to create a 1%, 3%, 5%, 7%, 10%, 12%, 15%, 17%, or 20% solution ("PTMPS solution"). Other non-limiting examples of organic solvents suitable for use herein include toluene, tetrahydrofuran (THF), and xylene. In one casting method, the PTMPS solution can be cast or placed on a nonporous substrate, such as a glass dish or plate, and air dried. Once air dried, the PTMPS cast tape is peeled off the nonporous substrate (e.g., glass dish) and further dried under vacuum. Other suitable non-porous substrates that can be used to form the PTMPS cast tape include, but are not limited to, polytetrafluoroethylene (PTFE), polyethylene, polypropylene, and polyethylene terephthalate (PET).

[0102] As an example, the PTMPS solution as described above can be cast onto a non-porous substrate, such as a glass plate, or onto a porous substrate to form a wet tape. The PTMPS wet tape is then submerged in a non-solvent, such as isopropanol (IPA) or methanol, to effect solvent-induced phase separation and form a PTMPS cast tape. It should be understood that any non-solvent for PTMPS that is miscible with the solvent used to make the PTMPS solution can be used in the casting method. The solvent-induced phase separation results in an opaque PTMPS tape that can be peeled off from the porous or non-porous substrate (e.g., a glass plate). The PTMPS cast tape can then be air-dried to remove residual solvent.

[0103] The PTMPS cast tape can be cut to a size suitable for stretching. Stretching of the cast tape occurs at a temperature below the melting temperature of the PTMPS polymer. In some embodiments, the PTMPS cast tape is stretched at a temperature between 60°C and 140°C, 75°C and 130°C, 80°C and 125°C, 90°C and 120°C, or 80°C and 110°C. The PTMPS tape can be stretched in one or more directions (i.e., uniaxially or biaxially) to form a porous PTMPS membrane. Either uniaxial or biaxial stretching can be performed at a rate of about 0.1% / sec to about 1000% / sec, about 1% / sec to about 500% / sec, or about 10% / sec to about 100% / sec. Biaxial stretching can be performed sequentially (i.e., machine direction and transverse direction stretching are performed separately) or simultaneously (i.e., machine direction and transverse direction stretching are performed simultaneously). When the PTMPS tape is stretched, the stretched PTMPS membrane has a node-and-fibril structure. Node as defined herein is meant to describe the connection point of at least three fibrils. The porous microstructure of the stretched PTMPS membrane is affected by the conditions of the tape formation process (e.g., the solvent used, the rate at which the tape is dried, the concentration of the polymer in the solution, the substrate used, etc.).

[0104] Stretched PTMPS polymer articles (e.g., stretched PTMPS membranes) produced according to the methods described herein have a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa, from about 10 MPa to about 50 MPa, from about 20 MPa to about 50 MPa, from about 30 MPa to about 50 MPa, or from about 40 MPa to about 50 MPa. Additionally, stretched PTMPS articles have a matrix modulus in at least one direction of greater than about 100 MPa, greater than about 250 MPa, or greater than about 500 MPa, or up to 1000 MPa. The matrix modulus of the expanded PTMPS polymer article can be in the range of about 100 MPa to about 1000 MPa, about 200 MPa to about 1000 MPa, about 300 MPa to about 1000 MPa, about 400 MPa to about 1000 MPa, about 500 MPa to about 1000 MPa, about 600 MPa to about 1000 MPa, about 700 MPa to about 1000 MPa, about 800 MPa to about 1000 MPa, or about 900 MPa to about 1000 MPa.

[0105] Additionally, the expanded PTMPS polymer article can have a percent porosity of greater than about 30%, about 35% or more, about 40% or more, about 45% or more, about 50% or more, about 55% or more, about 60% or more, about 65% or more, about 70% or more, about 75% or more, about 80% or more, about 85% or more, or about 90% or more. In some embodiments, the PTMPS polymer article can have a percent porosity of about 30% to about 90%, about 40% to about 90%, about 50% to about 90%, about 60% to about 90%, about 70% to about 90%, or about 80% to about 90%.

[0106] The PTMPS polymer has a high degree of crystallinity. As used herein, the phrase "high degree of crystallinity" is meant to include PTMPS polymers having a degree of crystallinity of at least 70% as measured by DSC. The PTMPS polymer can have a degree of crystallinity of at least 75%, at least 80%, at least 85%, at least 90%, or at least 95%. Alternatively, the PTMPS polymer can have a degree of crystallinity of about 70% to about 95%, about 80% to about 95%, about 85% to about 95%, or about 90% to about 95%. Additionally, the PTMPS polymer has a weight average molecular weight of about 350 kDa to about 5 MDa, about 800,000 kDa to about 5 MDa, or about 1.5 MDa to about 5 MDa.

[0107] As discussed herein, PTMPS polymer articles have a node and fibril microstructure. With respect to the PTMPS polymers and PTMPS articles described herein, a node can be described as a larger volume of polymer, where a fibril begins or ends without a clear continuation of the same fibril through the node. A node is also a connection point of at least three fibrils. In at least one embodiment, the PTMPS polymer chains are oriented along the fibril axis. PTMPS membranes have a broad melting point of 135°C to 150°C, indicating that the original lamellar crystals are partially converted to elongated chain crystals. The higher melting temperatures of PTMPS polymers (e.g., 135°C to 150°C) represent elongated chain crystals. Additionally, each fibril contains elongated chain crystals, as evidenced by the DSC curve shown in FIG. 12.

[0108] Additionally, the PTMPS polymer may contain at least one additional comonomer, thereby forming a modified PTMPS polymer. Suitable comonomers that may be included in the PTMPS polymer include, but are not limited to, m-bis(dimethylhydroxysilyl)benzene, o-bis(dimethylhydroxysilyl)benzene, or a comonomer having formula I. The comonomer may be present in the copolymer in an amount greater than about 0.001 mol%, greater than about 1 mol%, greater than about 5 mol%, greater than about 10 mol%, greater than about 15 mol%, or greater than about 20 mol%. In some embodiments, the comonomer may be present in the copolymer in an amount between about 0.001 mol% and about 30 mol%, between about 0.001 mol% and about 25 mol%, between about 0.001 mol% and about 20 mol%, between about 0.001 mol% and about 15 mol%, or between about 0.001 mol% and about 10 mol%, between about 0.01 mol% and about 5 mol%, or between about 0.1 mol% and about 1 mol%. [ka] (wherein R and R' belong to a C1-C6 alkyl or aromatic group, for example an aromatic group containing a phenyl ring).

[0109] In a further embodiment, a dense PTMPS polymer article is provided. The dense PTMPS article can be formed by compressing a porous PTMPS polymer film with or without the addition of heat (but remaining below the melting point of the PTMPS polymer). Pressure can be applied by calendering or plate pressing. In another embodiment, PTMPS polymer powder can be directly calendered (i.e., PTMPS polymer powder can be fed directly into the nip of two calender rolls) to produce a coherent dense tape. The dense tape formed is of indefinite length and has a thickness of less than about 1 mm. The dense tape can be processed continuously or cut to a size suitable for stretching. Stretching of the dry dense tape occurs at a temperature below the melting temperature of the PTMPS polymer and above 70° C., which is the solid / state transition of the PTMPS polymer. Either uniaxial or biaxial stretching can be carried out at a rate of about 0.1% / sec to about 1000% / sec, about 1% / sec to about 500% / sec, or about 10% / sec to about 100% / sec. It should be understood by those skilled in the art that various times, temperatures and pressures can be utilized to achieve a densified article.

[0110] The incorporation of filler materials and / or coatings into or on the PTMPS polymer articles described herein is considered within the scope of the present invention. For example, the filler materials can be blended with the PTMPS polymer prior to calendering or ram extrusion (and optionally stretching), or can be placed on the PTMPS polymer article and fixed in place with a suitable hydrogel. Non-limiting examples of suitable filler materials include inorganic materials (e.g., silica), carbon black, aerogels, metals, semi-metals, ceramics, carbon / metal particulate mixtures, activated carbon, hydrogel materials, bioactive agents, curing agents, and combinations thereof. The filler materials can be incorporated into the PTMPS polymer article in an amount of about 1.0% to about 80%, or about 20% to about 60%, or about 1% to about 30% by weight of the PTMPS article. Alternatively, suitable non-reactive filler materials can be incorporated into the PTMPS polymer article during formation of the PTMPS polymer.

[0111] Various components can be co-processed with or disposed on and / or in the PTMPS article. In particular, components (or chemical compositions) can be added to the PTMPS polymer either during or after polymer synthesis, such as in a blend or as a covalently attached component of the PTMPS polymer chain, such that the added component is intimately mixed in the polymer. The added component can alternatively or additionally be disposed on the outside of the polymer, on the surface of the fibrils of the stretched PTMPS polymer. Furthermore, the component can be disposed in the void spaces (e.g., pores) or between the fibrils in the stretched PTMPS article. Components added to or in the PTMPS article can be absorbable or non-absorbable. The added composition can include a useful substance releasably contained therein. Non-limiting examples of components that can be added to or otherwise contained in the PTMPS polymer or PTMPS article include cells, viruses, viral vectors, bacteria, proteins, antibodies, and other bioactive moieties.

[0112] The advantages of the porous PTMPS membrane described herein include creep resistance, ease of processing over a wide range of temperatures, solvents and concentrations, and radiation resistance (e.g., gamma radiation).In addition, PTMPS membranes do not contain fluorocarbons.Unlike other types of silicone substrates, PTMPS membranes provide high matrix modulus and matrix tensile strength without the need for crosslinking. EXAMPLES

[0113] Test Method Although specific methods and equipment are described below, it should be understood that other methods or equipment may be substituted as deemed suitable by one of ordinary skill in the art. It should be understood that the following examples were performed on a laboratory scale, but can be readily adapted to continuous or semi-continuous processes.

[0114] Differential Scanning Calorimetry (DSC) DSC data was collected using a TA Instruments Discovery DSC from -50°C to 160°C using a heating rate of 10°C / min. For resin samples, approximately 5 mg of powder was placed into a standard pan and lid combination available from TA Instruments. Membrane samples were prepared by punching out 4 mm disks. The 4 mm disks were placed flat in the pan and the lid was crimped to sandwich the membrane disk between the pan and lid.

[0115] Scanning electron microscope (SEM) SEM samples were imaged at 1.0–10 kV using a Hitachi SU8000 field emission scanning electron microscope equipped with a mixed top and bottom secondary electron detector.

[0116] Average thickness measurement The thickness was measured by placing the sample between two plates of a Miyutoyo thickness gauge (Miyutoyo Corporation, Kawasaki, Japan). The average of three measurements was reported.

[0117] Matrix tensile strength and matrix elastic modulus Matrix tensile strength and matrix modulus were measured by measuring the stress response to a constant uniaxial displacement rate using axial testing on a dynamic mechanical analyzer (DMA) (model: RSA-G2 manufactured by TA Instruments-Waters LLC, New Castle, Delaware, USA). Rectangular specimens of the membrane were die-cut with a width of 4.7 mm. The DMA was equipped with film / fiber tension clamps. The clamp gap was referenced to the same test conditions at room temperature. The prepared specimens were mounted in the DMA clamps with a sample length / gap of 10 mm. The axial testing consisted of applying a constant displacement rate of 0.1 mm / s for up to 200 s and measuring the corresponding transient axial force. For longitudinal MTS measurements, the larger dimension of the sample was oriented in the direction of stretching, referred to as the "machine direction". For transverse MTS measurements, the larger dimension of the sample was oriented perpendicular to the direction of stretching, referred to as the "transverse direction".

[0118] The tensile strength of the matrix was calculated using the following formula: MTS = (maximum stress / cross-sectional area) * (skeletal density of PTMPS) / density of sample, The true / skeletal density of PTMPS was deemed to be 1.025 g / cc as measured by helium pycnometer.

[0119] The matrix modulus was calculated using the following formula: Matrix elastic modulus = (small strain slope of load-displacement curve / cross-sectional area) * (skeletal density of PTMPS) / density of sample

[0120] Airflow measurements with ATEQ Air flow through the PTMPS membrane was measured using an ATEQ D570 at a pressure of 12 mbar and a sample port size of 2.99 cm 2 was measured.

[0121] Porosity measurement using a helium pycnometer The true or skeletal density of the PTMPS polymer was determined using a helium pycnometer (AccuPyc 1330 Pycnometer by Micromeritics Instrument Corporation) and was 1.025 g / cc (average of three measurements). Samples were die cut to form rectangular sections of 9 cm x 5 cm. The weight of each sample was measured using a Mettler Toledo ML54 balance and the thickness of the samples was measured using a Miyutoyo thickness gauge (Miyutoyo Corporation, Kawasaki, Japan). Using this data, the bulk density of the samples can be calculated with the following formula:

number

number

[0122] Average weight average molecular weight by size exclusion chromatography (SEC) SEC was performed using a Malvern OMNISEC® Reveal (Malvern PANanalytical, Westborough, MA) equipped with Shodex columns KF-806L, KF-807L and KF-803, tetrahydrofuran (Sigma-Aldrich, GPC grade) solvent at a flow rate of 0.8 mL / min, and an injection volume of 100 μL at PTMPS concentrations of 2–3 mg / mL at 30 °C.

[0123] Crystallinity measurement The crystallinity of PTMPS was determined using the enthalpy of fusion from differential scanning calorimetry (DSC). Specifically, the enthalpy of fusion of PTMPS was determined by integrating the DSC data measured at a rate of 10 °C / min from 80 °C to 160 °C. The crystallinity was calculated by the following equation:

number

[0124] Example 1 Preparation of purified 1,4-bis(hydroxydimethylsilyl)benzene monomer powder using tetrahydrofuran. 29 g of 1,4 bis(hydroxydimethylsilyl)benzene (Gelest Inc., Tech-95, CAS number 2754-32-7) monomer was dissolved in 125 mL of tetrahydrofuran (THF) (Sigma-Aldrich, CAS number 109-99-9). The solution was filtered through Whatman® grade 52 filter paper (Sigma-Aldrich, WHA1452090, hardened, low ash) to remove large insoluble impurities. The monomer powder was recrystallized by precipitating the solution with 1600 mL of hexane (purity >= 99%, Sigma-Aldrich). The recrystallized monomer powder was filtered and dried overnight at room temperature (approximately 22 °C) under vacuum. The final yield of 1,4 bis(hydroxydimethylsilyl)benzene monomer was 70 wt%.

[0125] Example 2 Preparation of poly(tetramethyl-p-silphenylene siloxane) (PTMPS) polymer 20 g of purified 1,4 bis(hydroxydimethylsilyl)benzene monomer powder from Example 1 was added to a 125 mL jacketed glass reactor equipped with a polytetrafluoroethylene (PTFE) stirring blade. A Dean-Stark condenser was connected to one of the reactor outlets to collect the water produced as a reaction by-product. The glassware was purged with nitrogen for 4 hours. Then, 106 g of anhydrous benzene (Sigma-Aldrich) was added to the reactor at room temperature (about 22 °C) to create a slurry containing the monomer. 0.8 wt% (based on monomer weight) of tetramethylguanidinium bis-2-ethylhexanoate catalyst was added to the reactor while the reaction mixture reached the reflux temperature (80 °C). The reaction was refluxed (80 °C) for 4 days. Finally, the reaction was stopped by cooling the reaction mixture to 30 °C, and the poly(tetramethyl-p-silphenylenesiloxane) (PTMPS) polymer was precipitated in methanol (22 °C) and then vacuum dried. The dried PTMPS polymer was characterized using size exclusion chromatography (SEC). The weight average molecular weight of the PTMPS polymer was measured by SEC to be 447 kilodaltons (kDa) with a polydispersity of 1.8. The melting point of the PTMPS polymer was determined to be 127° C. based on differential scanning calorimetry. The percent crystallinity of the PTMPS polymer was 68% based on the enthalpy of melting from DSC.

[0126] Example 3 Preparation of PTMPS cast tapes from 1 wt% solution The PTMPS polymer prepared in Example 2 was dissolved in p-xylene (Sigma-Aldrich) at 75 °C to make a 1 wt% solution in p-xylene. The solution was cast into a glass Petri dish and dried at approximately 22 °C. The dried PTMPS cast tape was peeled off the Petri dish and further dried under vacuum at 30 °C. The dried PTMPS cast tape was measured to have an average thickness of 40 μm (average of three measurements) using a Mitutoyo Digimatic Snap Gauge (Mitutoyo America, Aurora, IL). Scanning electron micrographs (SEM) of the dried PTMPS cast tape showed a porous morphology with asymmetric pore structure from the air side of the tape (Figure 1A) to the glass side of the tape (Figure 1B). Figure 1C is a scanning electron micrograph of a cross-section of the dried cast PTMPS tape. The melting point of the PTMPS tape was measured to be 126 °C based on differential scanning calorimetry (DSC). The % crystallinity of the PTMPS polymer was 67% based on the enthalpy of fusion from DSC.

[0127] Example 4 Preparation of uniaxially stretched PTMPS membranes A rectangular sample 4 inches long (about 10.16 cm) by 1 inch wide (about 2.54 cm) from the PTMPS cast tape prepared in Example 3 was cut with a sharp razor blade and restrained between two pneumatic grips (Instron® 5965 tensile tester with flat grip, "1124 lbs" (about 5 kN) load cell, and built-in convection oven (Illinois Tools Works, Norwood, Massachusetts)). The restrained PTMPS cast tape was thermally equilibrated at 120°C for 10 minutes at 20 mm gauge length and uniaxially stretched at 120°C to 5 times its original length at a rate of 1.25% / sec to form a uniaxially stretched PTMPS membrane. Scanning electron micrographs of the uniaxially stretched PTMPS membrane showed the presence of a microporous node-and-fibril microstructure (glass side, FIG. 2A; air side, FIG. 2B and 2C). The uniaxially stretched PTMPS membranes were asymmetric with respect to the observed pore structure from the air side to the glass side. Thermal analysis using DSC showed that the melting point shifted to higher temperatures and a broad melting range from 135 °C to 150 °C was present, indicating a partial conversion of the original lamellar crystals to extended chain crystals.

[0128] Example 5 Preparation of biaxially stretched PTMPS membranes A rectangular sample measuring 4 inches (about 10.16 cm) in length and 1 inch (about 2.54 cm) in width was cut from the PTMPS cast tape prepared in Example 3 with a sharp razor blade and restrained between two pneumatic grips (Instron® 5965 tensile tester with built-in convection oven). The rectangular sample of PTMPS cast tape was thermally equilibrated at 120° C. for 10 minutes with a gauge length of 20 mm and biaxially stretched at 120° C. to an area 5 times its original area at a rate of 1% / sec to form a biaxially stretched PTMPS membrane. SEM micrographs of the biaxially stretched PTMPS membrane showed the presence of a microporous node-and-fibril microstructure (glass side, FIG. 3A; air side, FIG. 3B and 3C; cross-sectional view, FIG. 3D). The biaxially stretched membrane was asymmetric with respect to the pore structure observed from the air side to the glass side.

[0129] Example 6 Preparation of PTMPS fine powder 2 g of PTMPS polymer as prepared in Example 2 was dissolved in 2 liters of 1,3,5-trimethylbenzene (Sigma-Aldrich) in a glass jacketed reactor equipped with a glass stir bar at 80° C. for 3 hours. The reactor was cooled to 3° C. and then maintained at 3° C. for 24 hours with gentle stirring (100 rpm). After 24 hours, crystallized particles of PTMPS were visible in the reactor. The stirrer was stopped and the PTMPS particles were filtered using a coarse filter paper (VWR grade 315; VWR International, Radnor, PA). The wet powder was washed five times with excess methanol (purity >= 99%, Sigma-Aldrich) and dried at 22° C. to obtain a fine powder of PTMPS. The melting point of the PTMPS fine powder was determined to be 129° C. using DSC. The % crystallinity of the PTMPS polymer was 85% based on the enthalpy of fusion from DSC (FIG. 10).

[0130] Example 7 Preparation of paste-extruded PTMPS tapes The PTMPS fine powder prepared in Example 6 was mixed with mineral oil (30 g mineral oil for 100 g PTMPS fine powder) in a glass jar. The PTMPS powder / mineral oil mixture contained in the glass jar was tumbled in a jar mill (US Stoneware, East Palestine, OH) for 1 hour and allowed to sit at room temperature (about 22° C.) for 12 hours. The PTMPS powder / mineral oil mixture was then thermally conditioned in a convection oven at 50° C. for 30 minutes. The thermally conditioned powder was poured by hand between two co-rotating rollers moving at a linear speed of 3 ft / min (about 0.914 m / min). The rollers were set at 120° C. and the gap between the rollers was set at 25.4 μm to yield a cohesive PTMPS tape about 100 μm thick. The cohesive PTMPS tape was washed with hexane (purity >= 99%, Sigma-Aldrich) at about 22° C. to remove the mineral oil. The % crystallinity of the PTMPS tape was 85% based on the enthalpy of fusion from DSC.

[0131] Example 8 Preparation of stretched PTMPS membrane A rectangular sample 4 inches (10.16 cm) long by 1 inch (about 2.54 cm) wide was cut from the cohesive PTMPS tape of Example 7 using a sharp razor blade and the sample was restrained between two pneumatic grips (Instron® 5965 tensile tester with built-in convection oven). The restrained PTMPS tape sample was thermally equilibrated at 120° C. for 10 minutes with a gauge length of 10 mm, and then uniaxially stretched to twice its original length at a rate of 1% / sec to form a uniaxially stretched PTMPS membrane. SEM micrographs of the stretched PTMPS membrane showed a porous node-and-fibril microstructure ( FIG. 4 ).

[0132] Example 9 Preparation of PTMPS polymer using tetramethylguanidinium bis-2-ethylhexanoate catalyst 16 g of purified 1,4 bis(hydroxydimethylsilyl)benzene monomer from Example 1 was added to a 125 mL jacketed glass reactor equipped with a PTFE stirring blade. A Dean-Stark condenser was attached to one of the reactor outlets to collect water produced as a reaction by-product. The glassware was purged with nitrogen for several hours. Then, 85 g of anhydrous benzene (Sigma-Aldrich) was added to the reactor at approximately 22 °C to create a slurry containing the monomer. While the reaction mixture reached reflux temperature (80 °C), 0.84 wt% (based on the weight of the monomer powder) of tetramethylguanidinium bis-2-ethylhexanoate catalyst (prepared as described in General Methods) was added to the reactor. The reaction was carried out at reflux (80 °C) for 3 days. On the third day, the reaction was stopped by cooling the reaction mixture to 30 °C and the PTMPS polymer was precipitated in methanol (Sigma-Aldrich, >99%) at room temperature (approximately 22 °C) and then dried under vacuum. The dried PTMPS polymer was characterized using size exclusion chromatography. The weight average molecular weight of the PTMPS polymer was determined to be 356 kilodaltons (kDa) with a polydispersity of 1.7.

[0133] Example 10 Preparation of PTMPS cast tape - methanol phase induced separation - 20wt% The PTMPS polymer prepared in Example 9 was dissolved in p-xylene (Sigma-Aldrich) to make a 20 wt% solution. This solution was coated onto a glass plate using a 3 mil (approximately 76.2 μm) drawdown bar. The wet tape was immediately submerged in a methanol (>99% purity, Sigma Aldrich) bath for solvent-induced phase separation. After a few minutes, the opaque PTMPS cast tape was peeled off from the glass plate. The PTMPS cast tape was air-dried at approximately 22 °C to remove excess solvent. The dried cast PTMPS tape was determined to have a thickness in the range of 25-30 μm. It was noted that after applying 0.25 mL of methanol, the dried PTMPS cast tape became more transparent, indicating that the PTMPS cast tape was microporous (cross-sectional view, Figure 5). The matrix modulus and matrix tensile strength of the microporous PTMPS tape were measured using a Dynamic Mechanical Analyzer (DMA, TA Instruments). The PTMPS cast tape was determined to have a matrix modulus of 212 MPa and a matrix tensile strength of 6.5 MPa. The PTMPS cast tape was determined to have a porosity of 35% by helium pycnometer (Micromeritics AccuPyc 1330; Micromeritics Instrument Corp., Norcross, GA). The % crystallinity of the PTMPS tape was 71% based on the enthalpy of fusion from DSC.

[0134] Example 11 Preparation of purified 1,4 bis(hydroxydimethylsilyl)benzene monomer using dichloromethane 25 g of 1,4 bis(hydroxydimethylsilyl)benzene monomer (Gelest Inc., Tech-95) was dissolved in 936 mL of dichloromethane (DCM, Sigma Aldrich) to prepare a clear solution. The solution was filtered through WHATMAN® grade 52 filter paper to remove large insoluble impurities. 1,4 bis(hydroxydimethylsilyl)benzene monomer was recrystallized from the filtered solution by refrigerating the solution at −3° C. overnight. The recrystallized 1,4 bis(hydroxydimethylsilyl)benzene monomer powder was filtered using a coarse filter paper (VWR grade 315) and dried under vacuum for 6 hours (at 30° C.). The final yield of 1,4 bis(hydroxydimethylsilyl)benzene monomer powder was 70 wt%.

[0135] Example 12 Preparation of PTMPS powder using 1,1,3,3-tetramethylguanidine catalyst 9 g of purified 1,4 bis(hydroxydimethylsilyl)benzene monomer from Example 11 was added to a 125 mL jacketed glass reactor equipped with a PTFE stirring blade. A Dean-Stark condenser was attached to one of the outlets of the reactor to collect the water produced as a reaction by-product. The entire reactor was placed in a nitrogen glove box. Then, 40 g of anhydrous toluene (Sigma-Aldrich) was added to the reactor at room temperature (about 22 °C) to create a slurry. While the reaction mixture reached the reflux temperature (115 °C), 0.24 g of 1,1,3,3-tetramethylguanidine (Sigma-Aldrich, 99%, catalog 241768-100ML) catalyst was added to the reactor. The reaction was carried out under reflux (115 °C) for 7 days. Finally, the reaction was stopped by cooling the reaction mixture to 30 °C. The PTMPS polymer was precipitated into methanol at room temperature (about 22 °C) and then dried under vacuum. The dried PTMPS polymer was characterized using size exclusion chromatography (SEC). The weight average molecular weight of the PTMPS polymer was determined to be 1 million daltons (1 MDa) with a polydispersity of 2.

[0136] Example 13 Preparation of PTMPS cast tapes using methanol for phase-induced separation - 10wt% The PTMPS polymer prepared in Example 12 was dissolved in p-xylene (Sigma-Aldrich) to make a 10 wt% solution. This solution was coated onto a glass plate using a 3 mil (approximately 76.2 μm) drawdown bar. The wet tape was immediately submerged in a 22°C methanol (Sigma-Aldrich) bath for solvent-induced phase separation. After a few minutes, the opaque PTMPS cast tape was peeled off from the glass plate. The PTMPS cast tape was allowed to dry in air (approximately 22°C) to obtain a thickness of 17 μm. It was noted that after applying 0.25 mL of methanol, the dried PTMPS cast tape became more transparent, indicating that the PTMPS cast tape was microporous. The porosity of the PTMPS cast tape was 34%, as determined by a helium pycnometer (Micromeritics Accupyc 1330).

[0137] Example 14 Preparation of PTMPS cast tapes using isopropanol for phase-induced separation - 10 wt% The PTMPS polymer prepared in Example 12 was dissolved in p-xylene (Sigma-Aldrich) to make a 10 wt% solution. This solution was coated onto a glass plate using a 3 mil (approximately 76.2 μm) drawdown bar. For solvent-induced phase separation of the PTMPS cast tape, the wet tape was immediately submerged in a 22°C isopropanol (IPA) (purity >= 99%, Sigma-Aldrich) bath. After 10 min, the opaque PTMPS cast tape was peeled off from the glass plate. The PTMPS cast tape was dried in air (approximately 22°C) to obtain a thickness of 30 μm. The dried PTMPS cast tape became more transparent after applying 0.25 mL of methanol, indicating that the PTMPS cast tape was microporous. The porosity of the PTMPS cast tape was 67%, as determined by a helium pycnometer (Micromeritics Accupyc 1330).

[0138] Example 15 Preparation of PTMPS cast tapes using isopropanol for phase-induced separation - 7wt% The PTMPS polymer prepared in Example 12 was dissolved in p-xylene to make a 7 wt% solution. This solution was coated onto a glass plate using a 3 mil (about 76.2 μm) drawdown bar. The wet tape was immediately submerged in an isopropanol (IPA) (Sigma-Aldrich) bath for solvent-induced phase separation of the PTMPS cast tape. After 10 minutes, the opaque PTMPS tape was peeled off from the glass plate. The PTMPS cast tape was dried in air (about 22° C.) to obtain a thickness of 20 μm. The dried PTMPS cast tape became more transparent after applying 0.25 mL of methanol, indicating that the PTMPS cast tape was microporous. The porosity of the PTMPS cast tape was 44%, as measured by a helium pycnometer.

[0139] Example 16 Preparation of stretched PTMPS membrane A rectangular sample measuring 4 inches (about 10.16 cm) in length and 1 inch (about 2.54 cm) in width was cut from the PTMPS cast tape prepared in Example 14 using a sharp razor blade. The PTMPS tape sample was restrained between two pneumatic grips (Instron® 5965 tensile tester with built-in convection oven). The restrained tape was thermally equilibrated at 120° C. for 10 minutes with a gauge length of 20 mm, and then uniaxially stretched at a rate of 10% / sec to twice its original length to form a stretched PTMPS membrane. SEM micrographs of the stretched PTMPS membrane showed that it contained a porous node-and-fibril microstructure ( FIG. 6 ). After applying 0.25 mL of methanol, the stretched PTMPS membrane became more transparent (indicating that the stretched PTMPS membrane was microporous). The porosity of the stretched PTMPS membrane was 87%, as measured by helium pycnometer. The elastic modulus and matrix tensile strength of the microporous PTMPS membranes were determined using a Dynamic Mechanical Analyzer (DMA, TA Instruments). The expanded PTMPS membrane had an elastic modulus of 278 MPa and a matrix tensile strength of 5 MPa.

[0140] Example 17 Preparation of stretched PTMPS membranes from pressed membranes Rectangular samples from the PTMPS cast tape prepared in Example 14, with dimensions of 76 mm in length and 60 mm in width, were cut using a sharp razor blade, pressed between Kapton® films (polyimide film commercially available from DePont, de Nemours Inc., Wilmington, Delaware) and covered with a polished steel plate of the same dimensions in a hot press (Pasadena Hydraulics Inc., City of Industry, Calif.) at 80° C. and 100 psi (about 689 kPa) pressure for 5 minutes. Samples measuring 30 mm in length and 24 mm in width were cut from the pressed PTMPS cast tape using a sharp razor blade and restrained between two pneumatic grips (Instron® 5965 tensile tester with in-built convection oven). The restrained PTMPS cast tape was thermally equilibrated at 120°C for 10 min with a gauge length of 20 mm, and then uniaxially stretched at 120°C to 3.75 times its original length at a rate of 10% / s to form a stretched PTMPS membrane. SEM micrographs of the stretched PTMPS membrane showed that it had a porous node-and-fibril microstructure (Figure 7). The stretched PTMPS membrane with node-and-fibril microstructure became more transparent after applying 0.25 mL of methanol, indicating that the stretched PTMPS membrane was microporous. The porosity of the stretched PTMPS membrane was 60% as measured by helium pycnometer. The elastic modulus and matrix tensile strength of the microporous film were determined using a dynamic mechanical analyzer (DMA, TA Instruments) in both the machine (along the uniaxial stretch direction) and transverse (perpendicular to the uniaxial stretch direction) directions. The microporous PTMPS membrane had a matrix modulus of 795 MPa and a matrix tensile strength of 33 MPa in the machine direction, and a matrix modulus of 164 MPa and a matrix tensile strength of 4 MPa along the transverse direction.

[0141] Example 18 Preparation of biaxially stretched PTMPS membranes The PTMPS polymer was polymerized using the method outlined in Example 12. The weight average molecular weight of the PTMPS polymer was determined to be 650 (kDa) with a polydispersity of 1.5. The PTMPS polymer was then dissolved in p-xylene to make a 10 wt% solution. This solution was coated onto a glass plate using a 10 mil (~254 μm) drawdown bar to form a cast film. The wet tape was immediately submerged in an isopropanol (IPA) (Sigma-Aldrich) bath for solvent-induced phase separation of the PTMPS cast tape.

[0142] After 10 minutes, the opaque PTMPS tape was peeled off the glass plate. The PTMPS cast tape was dried in air (about 22° C.) to obtain a thickness of 146 μm. The air flow through the PTMPS cast tape was measured using an ATEQ D570 and determined to be 2.2 L / hr. A rectangular sample measuring 3.2 inches (about 8.1 cm) in length and 2.8 inches (about 7.2 cm) in width was cut from the PTMPS cast tape using a sharp razor blade, and the PTMPS tape sample was restrained between two pneumatic grips (Instron® 5965 tensile tester with built-in convection oven). The restrained PTMPS cast tape was thermally equilibrated at 111° C. for 5 minutes before being stretched uniaxially to 3 times its original length at a rate of 100% / sec with an initial gauge length of 20 mm to form a stretched PTMPS membrane. The stretched direction is called the machine direction (MD) and the direction 90° from the MD is called the transverse direction (TD). The stretched PTMPS membrane was removed from the grips, rotated 90°, and restrained again between two pneumatic grips such that the TD was along the grip movement direction. The restrained PTMPS membrane was thermally equilibrated at 111°C for 5 min and then uniaxially stretched to twice its original length at a rate of 100% / sec with an initial gauge length of 20 mm to obtain a biaxially stretched PTMPS membrane. SEM micrographs of the biaxially stretched PTMPS membrane showed a porous node-and-fibril microstructure (Figure 8). Figure 12 also depicts a DSC curve showing the presence of higher melting point extended chain crystals that make up the fibrils. The air flow through the biaxially stretched PTMPS membrane was measured using an ATEQ D570 and determined to be 45.3 L / hr.

[0143] Example 19 Preparation of simultaneous biaxially stretched PTMPS membranes PTMPS polymer was polymerized using the method outlined in Example 12. The weight average molecular weight of the PTMPS polymer was determined to be 550 (kDa) with a polydispersity of 1.7. The PTMPS polymer was dissolved in p-xylene to make a 10 wt% solution. The PTMPS polymer solution was coated onto a glass plate using a 10 mil (~254 μm) drawdown bar to form a cast film. For solvent-induced phase separation of the PTMPS cast tape, the wet tape was immediately submerged in an isopropanol (IPA) (Sigma-Aldrich) bath.

[0144] The opaque PTMPS tape was peeled off from the glass plate after 10 minutes. The PTMPS cast tape was dried in air (about 22° C.). The dried PTMPS cast tape was compressed between Kapton® films (polyimide film available from DuPont de Nemours Inc., Wilmington, DE) and covered with a polished steel plate of the same dimensions at 80° C. and 10 psi (about 68.9 kPa) pressure for 5 minutes on a hot press (Pasadena Hydraulics Inc., City of Industry, CA). The final thickness of the PTMPS cast tape was 110 μm. The compressed PTMPS cast tape was then loaded into a Karo IV biaxial stretcher (available from Bruckner Group, GmbH) and, after thermal equilibration at 120° C. for 3 minutes, the PTMPS cast tape was simultaneously biaxially stretched at 10% / s until an area ratio of 9 was reached. SEM micrographs of the simultaneously biaxially stretched PTMPS membranes showed a porous node-and-fibril microstructure (Figure 11). The porosity of the simultaneously biaxially stretched PTMPS membrane was 84%, as measured by helium pycnometer. The elastic modulus and matrix tensile strength of the simultaneously biaxially stretched porous PTMPS membranes were measured using a Dynamic Mechanical Analyzer (DMA, TA Instruments), respectively. The simultaneously biaxially stretched PTMPS membranes had an elastic modulus of 187 MPa and a matrix tensile strength of 9.6 MPa.

[0145] Example 20 Paste extrusion of fine PTMPS powder into beads. PTMPS polymer was polymerized using the method outlined in Example 12. The weight average molecular weight of the PTMPS polymer was determined to be 680 (kDa) with a polydispersity of 1.6. The PTMPS polymer was dissolved in dichloromethane (Sigma Aldrich purity >99.5%) to make a 5 wt% solution. The PTMPS solution was added to an equal part by weight of the water-surfactant solution in a plastic container. This mixture was emulsified at 25°C for 10 minutes at 10,000 rpm using an IKA T50 Basic homogenizer (IKA®-Works, Inc., Wilmington, NC). The emulsion was then transferred to a 250 mL glass jacketed reactor and the dichloromethane was removed from the emulsion by gentle stirring at 25°C to obtain PTMPS particles in water. The PTMPS particles were precipitated from the aqueous phase by adding salt and washed five times with an equal volume of water to remove excess surfactant and salt. Finally, the PTMPS particles were filtered from the water with a coarse filter paper (VWR grade 315) and dried under vacuum at 30 °C for 24 h to obtain PTMPS fine powder.

[0146] PTMPS fine powder was mixed with Isopar™ V oil (Exxon Mobile Chemicals) (30 g oil for 100 g PTMPS fine powder) in a glass jar. The PTMPS powder / oil mixture contained in the glass jar was tumbled in a jar mill (US Stoneware, Eastpalestine, OH) for 1 hour and allowed to sit at room temperature (approximately 22° C.) for 12 hours. The PTMPS powder / oil mixture was then thermally conditioned in a convection oven at 50° C. for 30 minutes. The PTMPS powder / oil mixture was poured into an aluminum cylindrical cavity with a 9:1 reduction die at the exit and equilibrated at 123° C. for 5 minutes. The powder / oil mixture was paste extruded through the 9:1 reduction die at 1 mm / sec to form cohesive PTMPS cylindrical beads.

[0147] The invention of this application has been described above both generally and with reference to specific embodiments. It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments without departing from the scope of the present disclosure. Therefore, the embodiments are intended to cover the modifications and variations of the present invention provided they come within the scope of the appended claims and their equivalents. The aspects of the present invention are listed below. [Aspect 1] An article comprising an expanded poly(tetramethyl-p-silphenylene siloxane) polymer film having a melting point of about 130° C. to about 150° C. and a microstructure of nodes interconnected by fibrils. [Aspect 2] 2. The article of embodiment 1, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%. [Aspect 3] 3. The article of claim 1 or 2, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity of greater than about 30%. [Aspect 4] The article of any one of the preceding claims, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane further comprises a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa. [Aspect 5] 5. The article of any one of the preceding claims, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film has a matrix modulus in at least one direction of from about 100 MPa to about 1000 MPa. [Aspect 6] The article of any one of the preceding claims, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a poly(tetramethyl-p-silphenylene siloxane) polymer having a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 7] The article of any one of the preceding claims, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5. [Aspect 8] The article of any one of the preceding claims, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film further comprises at least one comonomer in an amount between about 0.001 mol % and about 10 mol %. [Aspect 9] The article of any one of the preceding embodiments, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film comprises at least one filler material. [Aspect 10] The article of any one of the preceding claims, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a bioactive moiety therein. [Aspect 11] 11. The article of any one of the preceding claims, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has an asymmetric pore size from the first side to the second side. [Aspect 12] 12. The article of any one of the preceding claims, wherein the fibrils comprise polymer chains, the polymer chains oriented along a fibril axis. [Aspect 13] 13. The article of any one of the preceding claims, wherein the fibrils each comprise extended chain crystals. [Aspect 14] The article of any one of the preceding claims, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer article is in the form of a fiber, a tube, a tape, a sheet, or a three-dimensional free-standing structure. [Aspect 15] 15. A composite material comprising the poly(tetramethyl-p-silphenylene siloxane) article of any one of embodiments 1-14. [Aspect 16] A laminate comprising the poly(tetramethyl-p-silphenylene siloxane) polymer article of any one of embodiments 1 to 14 or the composite of embodiment 15. [Aspect 17] A device comprising the porous poly(tetramethyl-p-silphenylene siloxane) polymer article of any one of embodiments 1-14. [Aspect 18] lubricating a poly(tetramethyl-p-silphenylene siloxane) polymer having a melting point of about 130° C. to about 150° C. and a crystallinity of at least 70% to form a lubricated poly(tetramethyl-p-silphenylene siloxane) polymer; Pressing the lubricated poly(tetramethyl-p-silphenylene siloxane) polymer at a temperature between 60° C. and 140° C. to form a preform; and stretching the preform at a temperature between 60°C and 140°C to form a porous poly(tetramethyl-p-silphenylene siloxane) polymer article having a structure of nodes interconnected by fibrils; A method for making a poly(tetramethyl-p-silphenylene siloxane) polymer article, comprising: [Aspect 19] 20. The method of embodiment 18, comprising calendering the lubricated poly(tetramethyl-p-silphenylene siloxane) polymer at a temperature between 60° C. and 140° C. to form a preform, or ram extruding the lubricated poly(tetramethyl-p-silphenylene siloxane) polymer at a temperature between 60° C. and 140° C. to form a preform. [Aspect 20] The method of any one of claims 18 to 19, further comprising removing lubricant from the preform before stretching. [Aspect 21] The method of any one of aspects 18 to 20, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 22] The method of any one of embodiments 18-21, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5. [Aspect 23] The method of any one of embodiments 18-22, further comprising compressing the porous poly(tetramethyl-p-silphenylene siloxane) polymer article to form a dense poly(tetramethyl-p-silphenylene siloxane) polymer article. [Aspect 24] The method of any one of aspects 18-23, further comprising adding one of a filler material and a bioactive moiety to the poly(tetramethyl-p-silphenylene siloxane) polymer. [Aspect 25] The method of any one of aspects 18-24, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer article has an asymmetric pore size from the first side to the second side. [Aspect 26] 1. A method for making a poly(tetramethyl-p-silphenylene siloxane) polymer article, comprising pressing and heating a poly(tetramethyl-p-silphenylene siloxane) polymer having a melting point of 130°C to 150°C and a crystallinity of at least 70% at a temperature of 60°C to 140°C to form a preform article, and subsequently stretching the preform article at a temperature of 60°C to 140°C to form a porous poly(tetramethyl-p-silphenylene siloxane) polymer article. [Aspect 27] The method of embodiment 26, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 28] 28. The method of any one of claims 26 to 27, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5. [Aspect 29] The method of any one of embodiments 26-28, wherein the porous poly(tetramethyl-p-silphenylene siloxane) polymer article has a porosity of greater than about 30%. [Aspect 30] The method of any one of embodiments 26-29, further comprising compressing the porous poly(tetramethyl-p-silphenylene siloxane) polymer article to form a dense poly(tetramethyl-p-silphenylene siloxane) polymer article. [Aspect 31] casting a poly(tetramethyl-p-silphenylene siloxane) polymer solution onto a substrate to form a poly(tetramethyl-p-silphenylene siloxane) polymer cast tape; drying the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape to form a dried poly(tetramethyl-p-silphenylene siloxane) polymer cast tape; and removing the dried poly(tetramethyl-p-silphenylene siloxane) polymer cast tape from the substrate; A method for making a poly(tetramethyl-p-silphenylene siloxane) polymer article, comprising: [Aspect 32] 32. The method of embodiment 31, further comprising stretching the dry poly(tetramethyl-p-silphenylene siloxane) polymer tape to form a stretched poly(tetramethyl-p-silphenylene siloxane) film having a node and fibril microstructure. [Aspect 33] 33. The method of embodiment 31 or 32, wherein drying comprises air drying, vacuum drying, and combinations thereof. [Aspect 34] 34. The method of any one of embodiments 31-33, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape has an asymmetric pore size from the first side to the second side of the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape. [Aspect 35] 35. The method of any one of aspects 31 to 34, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer solution comprises poly(tetramethyl-p-silphenylene siloxane) polymer and an organic solvent. [Aspect 36] The method of any one of aspects 31 to 35, wherein the substrate is a porous or non-porous substrate. [Aspect 37] 37. The method of any one of aspects 31 to 36, wherein the substrate is a non-porous substrate, and the non-porous substrate is selected from a glass dish, a glass plate, polytetrafluoroethylene, polyethylene, polypropylene, and polyethylene terephthalate. [Aspect 38] The method of any one of embodiments 31-37, further comprising cutting the dried poly(tetramethyl-p-silphenylene siloxane) cast tape to a desired size before stretching. [Aspect 39] The method of any one of embodiments 31-38, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%. [Aspect 40] The method of any one of embodiments 31-39, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity of greater than about 30%. [Aspect 41] The method of any one of embodiments 31-40, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa. [Aspect 42] 42. The method of any one of embodiments 31-41, wherein the stretched poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix modulus in at least one direction of from about 100 MPa to about 1000 MPa. [Aspect 43] The method of any one of aspects 31 to 42, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 44] A method for producing a dense article comprising feeding a poly(tetramethyl-p-silphenylene siloxane) polymer powder directly into the nip of two calender rolls to produce a coherent dense poly(tetramethyl-p-silphenylene siloxane) tape. [Aspect 45] casting a poly(tetramethyl-p-silphenylene siloxane) polymer solution onto a substrate to form a poly(tetramethyl-p-silphenylene siloxane) polymer cast tape; submerging the cast poly(tetramethyl-p-silphenylene siloxane) polymer tape in a non-solvent bath for solvent-induced phase separation; removing the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape from the substrate; and drying the poly(tetramethyl-p-silphenylene siloxane) polymer tape to form a microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape; A method comprising: [Aspect 46] The method of embodiment 45, further comprising stretching the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape to form an expanded poly(tetramethyl-p-silphenylene siloxane) membrane having a node and fibril microstructure. [Aspect 47] The method of embodiment 45 or embodiment 46, further comprising cutting the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape before stretching. [Aspect 48] 48. The method of any one of aspects 45 to 47, wherein the substrate is a porous or non-porous substrate. [Aspect 49] 49. The method of any one of aspects 45 to 48, wherein the substrate is a non-porous substrate, and the non-porous substrate is selected from a glass dish, a glass plate, polytetrafluoroethylene, polyethylene, polypropylene, and polyethylene terephthalate. [Aspect 50] The method of any one of embodiments 45-49, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%. [Aspect 51] 51. The method of any one of aspects 45-50, wherein the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape has asymmetric pore size from the first side to the second side of the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape. [Aspect 52] The method of any one of embodiments 45-51, wherein the stretched poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity of greater than about 30%. [Aspect 53] 53. The method of any one of embodiments 45-52, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a matrix tensile strength in at least one direction of from about 1 MPa to about 50 MPa. [Aspect 54] The method of any one of embodiments 45-53, wherein the stretched poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix modulus of about 100 MPa to about 1000 MPa in at least one direction. [Aspect 55] The method of any one of embodiments 45-54, wherein the stretched poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a poly(tetramethyl-p-silphenylene siloxane) polymer having a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 56] An article comprising a poly(tetramethyl-p-silphenylene siloxane) polymer tape formed from a poly(tetramethyl-p-silphenylene siloxane) polymer having a crystallinity of at least about 70%, a polydispersity of 1 to 5, and a weight average molecular weight of about 350 kDa to about 5 MDa. [Aspect 57] 57. The article of embodiment 56, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer tape is opaque. [Aspect 58] 58. The article of any one of claims 56 to 57, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer tape is formed using a casting method, a solvent-induced casting method, or a paste extrusion method. [Aspect 59] An article comprising a poly(tetramethyl-p-silphenylene siloxane) polymer cast tape. [Aspect 60] The article of embodiment 59, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%. [Aspect 61] The article of any one of embodiments 59 to 60, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer tape has an asymmetric pore size from the first side to the second side of the microporous poly(tetramethyl-p-silphenylene siloxane) polymer tape. [Aspect 62] The article of any one of aspects 59-61, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 63] lubricating a poly(tetramethyl-p-silphenylene siloxane) polymer having a melting point of about 130° C. to about 150° C. and a crystallinity of at least 70% with a lubricant to form a poly(tetramethyl-p-silphenylene siloxane) powder / lubricant mixture; paste extruding the poly(tetramethyl-p-silphenylene siloxane) powder / lubricant mixture to form coherent PTMPS beads, tapes, tubes, or three-dimensional free-standing structures; A method for making a poly(tetramethyl-p-silphenylene siloxane) polymer article, comprising: [Aspect 64] 64. The method of embodiment 63, further comprising tumbling the poly(tetramethyl-p-silphenylene siloxane) polymer powder / oil mixture prior to paste extrusion. [Aspect 65] 65. The method of embodiment 63 or embodiment 64, further comprising thermal conditioning the poly(tetramethyl-p-silphenylene siloxane) polymer powder / oil mixture prior to paste extrusion. [Aspect 66] The method of any one of embodiments 63-65, comprising stretching the cohesive PTMPS beads to form an expanded poly(tetramethyl-p-silphenylene siloxane) polymer film. [Aspect 67] The method of embodiment 66, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of about 350 kDa to 5 MDa. [Aspect 68] The method of any one of embodiments 63-67, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5.

Claims

1. An article comprising an expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane having a melting point of 130° C. to 150° C. and a microstructure of nodes interconnected by fibrils, each of said fibrils comprising extended chain crystals.

2. The article of claim 1, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%.

3. The article of claim 1 or 2, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity of greater than 30%.

4. The article of any one of claims 1 to 3, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane further comprises a matrix tensile strength in at least one direction of from 1 MPa to 50 MPa.

5. The article of any one of claims 1 to 4, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film has a matrix modulus in at least one direction of from 100 MPa to 1000 MPa.

6. The article of any one of claims 1 to 5, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a poly(tetramethyl-p-silphenylene siloxane) polymer having a weight average molecular weight of from 350 kDa to 5 MDa.

7. The article of any one of claims 1 to 6, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a polydispersity of 1-5.

8. The article of any one of claims 1 to 7, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film further comprises at least one comonomer in an amount of 0.001 mol % to 10 mol %.

9. The article of any one of claims 1 to 8, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film comprises at least one filler material.

10. The article of any one of claims 1 to 9, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer film comprises a bioactive moiety therein.

11. The article of any one of claims 1 to 10, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has an asymmetric pore size from the first side to the second side.

12. The article of any one of claims 1 to 11, wherein the fibrils comprise polymer chains, the polymer chains being oriented along a fibril axis.

13. The article of any one of claims 1 to 12, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer article is in the form of a fiber, tube, tape, sheet, or three-dimensional free-standing structure.

14. A composite material comprising the poly(tetramethyl-p-silphenylene siloxane) article of any one of claims 1 to 13.

15. A laminate comprising the poly(tetramethyl-p-silphenylene siloxane) polymer article of any one of claims 1 to 13 or the composite of claim 14.

16. A device comprising the porous poly(tetramethyl-p-silphenylene siloxane) polymer article of any one of claims 1 to 13.

17. casting a poly(tetramethyl-p-silphenylene siloxane) polymer solution onto a substrate to form a poly(tetramethyl-p-silphenylene siloxane) polymer cast tape; drying the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape to form a dried poly(tetramethyl-p-silphenylene siloxane) polymer cast tape; and removing the dried poly(tetramethyl-p-silphenylene siloxane) polymer cast tape from the substrate; and stretching the dried poly(tetramethyl-p-silphenylene siloxane) polymer cast tape to form a stretched poly(tetramethyl-p-silphenylene siloxane) film having a node and fibril microstructure. wherein each of said fibrils comprises extended chain crystals.

18. 20. The method of claim 17, wherein drying comprises air drying, vacuum drying, and combinations thereof.

19. 19. The method of claim 17 or 18, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer cast tape has an asymmetric pore size from the first side to the second side of the microporous poly(tetramethyl-p-silphenylene siloxane) polymer cast tape.

20. The method of any one of claims 17 to 19, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer solution comprises poly(tetramethyl-p-silphenylene siloxane) polymer and an organic solvent.

21. The method according to any one of claims 17 to 20, wherein the substrate is a porous or non-porous substrate.

22. The method according to any one of claims 17 to 21, wherein the substrate is a non-porous substrate, and the non-porous substrate is selected from a glass dish, a glass plate, polytetrafluoroethylene, polyethylene, polypropylene, and polyethylene terephthalate.

23. The method of any one of claims 17 to 22, further comprising cutting the dried cast poly(tetramethyl-p-silphenylene siloxane) tape to a desired size before stretching.

24. The method of any one of claims 17 to 23, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a crystallinity of at least 70%.

25. The method of any one of claims 17 to 24, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a porosity greater than 30%.

26. The method of any one of claims 17 to 25, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane comprises a matrix tensile strength in at least one direction of from 1 MPa to 50 MPa.

27. The method of any one of claims 17 to 26, wherein the expanded poly(tetramethyl-p-silphenylene siloxane) polymer membrane has a matrix modulus in at least one direction of from 100 MPa to 1000 MPa.

28. 28. The method of any one of claims 17 to 27, wherein the poly(tetramethyl-p-silphenylene siloxane) polymer has a weight average molecular weight of from 350 kDa to 5 MDa.

Citation Information

Patent Citations

  • Gas separation membrane

    JP1986192323A

  • Substrate-flattening material and flattening of substrate using the same

    JP1997059387A

  • Method for manufacturing stretched film of polytetramethyl-p-silphenylene siloxane

    JP2010253774A