Polymer electrolyte membrane and membrane electrode assembly including the same
The polymer electrolyte membrane with a composite layer and specific ionomer ratio addresses the durability and conductivity trade-off, ensuring high-cycle performance and cost-effective production of fuel cell assemblies.
Patent Information
- Application Number
- JP2022580036
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-30
- Filing Date
- 2021-11-24
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-11-24
AI Technical Summary
Existing polymer electrolyte membranes in fuel cells face a trade-off between mechanical durability and ionic conductivity, limiting their performance and longevity, with durability evaluations being time-consuming and costly.
A polymer electrolyte membrane comprising a composite layer with a porous support and ionomer ratio (IS/FS) of 0.4 to 1.0, ensuring high mechanical durability and ionic conductivity, allowing more than 30,000 wet/dry cycles without deteriorating performance.
The membrane achieves excellent mechanical durability and ionic conductivity, enabling the production of membrane electrode assemblies that withstand over 30,000 cycles, reducing development time and cost by predicting durability through the IS/FS ratio measurement.
Smart Images

Figure 0007576110000002 
Figure 0007576110000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer electrolyte membrane and a membrane electrode assembly including the same, and more particularly, to a polymer electrolyte membrane and a membrane electrode assembly including the same, which have excellent mechanical properties without a decrease in performance such as ionic conductivity, thereby ensuring the manufacture of a membrane electrode assembly having high durability of about 30,000 or more wet / dry cycles as measured by the accelerated durability test method of the NEDO protocol. [Background technology]
[0002] Polymer electrolyte membrane fuel cells (PEMFCs), which generate electricity using a stacked structure of unit cells consisting of a membrane electrode assembly (MEA) and a separator (also called a bipolar plate), are attracting attention as a next-generation energy source that can replace fossil energy due to their high energy efficiency and environmentally friendly characteristics.
[0003] The membrane electrode assembly generally includes an anode (also called the "fuel electrode"), a cathode (also called the "air electrode"), and a polymer electrolyte membrane (PEM) therebetween.
[0004] When a fuel such as hydrogen gas is supplied to the anode, hydrogen is oxidized at the anode to produce hydrogen ions (H + ) and electrons (e -) is produced. The produced hydrogen ions are transferred to the cathode via a polymer electrolyte membrane (PEM), and the produced electrons are transferred to the cathode via an external circuit. Oxygen in the air supplied to the cathode combines with the hydrogen ions and the electrons and is reduced to produce water.
[0005] There are still many technical barriers to be overcome in order to commercialize polymer electrolyte membrane fuel cells. The essential improvements are to achieve high performance, long life, and low cost. The component that has the greatest impact on these is the membrane electrode assembly, and the polymer electrolyte membrane is one of the key elements that has the greatest impact on the performance and cost of the membrane electrode assembly.
[0006] In particular, for a membrane electrode assembly applied to a fuel cell for transportation, ensuring mechanical durability for long-term operation is of paramount importance. In general, the mechanical durability of a membrane electrode assembly substantially depends on the durability of a polymer electrolyte membrane that repeatedly expands and contracts during operation of the fuel cell.
[0007] As a way to improve the mechanical durability of polymer electrolyte membranes, a reinforced composite membrane type polymer electrolyte membrane has been proposed, which is manufactured by impregnating a porous support with an ionomer dispersion. However, as the thickness of the porous support increases, the electrical performance of the polymer electrolyte membrane, such as ion conductivity, decreases (i.e., the ion conductivity decreases), so the thickness of the porous support cannot be increased without limit. Therefore, due to this trade-off between mechanical durability and ion conductivity, it is known that there is a limit to improving the mechanical durability of the polymer electrolyte membrane by adjusting the thickness of the porous support.
[0008] Meanwhile, the mechanical durability of membrane electrode assemblies is generally evaluated by measuring the number of wet / dry cycles according to the accelerated durability evaluation method of the NEDO protocol. This evaluation has the problem of taking a long time (50 days or more). Furthermore, since membrane electrode assembly samples must be actually made to evaluate the durability of membrane electrode assemblies, (i) it takes a long time to produce membrane electrode assembly samples for durability evaluation, and (ii) it is expensive to produce membrane electrode assembly samples because expensive precious metals are used to form the electrodes. Summary of the Invention [Problem to be solved by the invention]
[0009] Therefore, the present invention relates to a polymer electrolyte membrane and a membrane electrode assembly including the same, which can avoid problems caused by the limitations and shortcomings of the related art as described above.
[0010] One aspect of the present invention is to provide a polymer electrolyte membrane that can ensure the manufacture of a membrane electrode assembly having high durability of about 30,000 or more wet / dry cycles as measured by the accelerated durability evaluation method of the NEDO protocol by having excellent mechanical properties without decreasing performance such as ionic conductivity.
[0011] Another aspect of the present invention is to provide a membrane electrode assembly having high durability of about 30,000 or more wet / dry cycles as measured by the accelerated durability evaluation method of the NEDO protocol, by including a polymer electrolyte membrane having excellent mechanical properties without deterioration of performance such as ionic conductivity.
[0012] In addition to the above-mentioned aspects of the present invention, other features and advantages of the present invention will be described below or will be apparent to those skilled in the art from such description. [Means for solving the problem]
[0013] According to one aspect of the present invention, there is provided a polymer electrolyte membrane, the polymer electrolyte membrane comprising a composite layer including a porous support having a number of voids and an ionomer filling the voids, wherein a ratio (IS / FS) of an initial stab strain (IS) of the polymer electrolyte membrane to a stab final strain (FS) of the polymer electrolyte membrane is 0.4 to 1.0.
[0014] The polymer electrolyte membrane may have an in-plane ion conductivity of 0.03 to 0.1 S / cm and a through-thickness ion conductivity of 0.03 to 0.1 S / cm under conditions of 80° C. and 50% RH.
[0015] The polymer electrolyte membrane may have an initial puncture deformation (IS) of 1 to 6% and a final puncture deformation (FS) of 2 to 8%.
[0016] The composite layer has a first surface and a second surface opposite to the first surface, and the polymer electrolyte membrane further includes a first pure layer disposed on the first surface and including a first ionomer, and a second pure layer disposed on the second surface and including a second ionomer, and a thickness of the composite layer can be 30 to 80% of a thickness of the polymer electrolyte membrane.
[0017] The polymer electrolyte membrane may have a thickness of 10 to 50 μm.
[0018] At least a portion of the ionomer of the composite layer may be the same as at least one of the first ionomer and the second ionomer.
[0019] The porous support may include a first porous subsupport having the first surface and a second porous subsupport having the second surface, the first porous subsupport having a first void, the first void being filled with the same ionomer as the first ionomer, the second porous subsupport having a second void, a portion of the second void adjacent the first porous subsupport being filled with the same ionomer as the first ionomer, and a remainder of the second void adjacent the second pure layer being filled with the same ionomer as the second ionomer.
[0020] The first and second porous subsupports may be in contact with one another.
[0021] The porous support includes a first porous subsupport having the first surface, a second porous subsupport having the second surface, and at least one third porous subsupport between the first and second porous subsupports, and the first, second and third porous subsupports may be in contact with each other.
[0022] The first ionomer can be the same as the second ionomer.
[0023] According to another aspect of the present invention, there is provided a membrane electrode assembly comprising an anode, a cathode, and the polymer electrolyte membrane of claim 1 disposed between the anode and the cathode.
[0024] This general description of the invention is intended to be illustrative or explanatory only and does not limit the scope of the invention. Effect of the Invention
[0025] According to the present invention, it is possible to overcome the prejudice in the industry that there is a trade-off between the mechanical durability and ionic conductivity of a polymer electrolyte membrane, and to provide a polymer electrolyte membrane having excellent mechanical durability and ionic conductivity.
[0026] In particular, the polymer electrolyte membrane of the present invention has excellent mechanical durability with a ratio of stab initial strain (IS) to stab final strain (FS) (hereinafter referred to as "IS / FS ratio") of about 0.4 to 1.0, thereby ensuring the manufacture of a membrane electrode assembly with high durability of more than 30,000 wet / dry cycles as measured by the accelerated durability evaluation method of the NEDO protocol. In addition, despite having such excellent mechanical durability, the polymer electrolyte membrane exhibits excellent performance with both in-plane ionic conductivity and through-thickness ionic conductivity of about 0.03 to 0.1 S / cm at 80°C and 50% RH.
[0027] In addition, according to the present invention, it has been revealed that the mechanical durability of a membrane electrode assembly, which is generally measured by the accelerated durability evaluation method of the NEDO protocol, is directly related to the IS / FS ratio of a polymer electrolyte membrane. Therefore, by measuring the IS / FS ratio of a polymer electrolyte membrane during the manufacturing process, the mechanical durability of a membrane electrode assembly manufactured using the polymer electrolyte membrane can be easily predicted without actually manufacturing the membrane electrode assembly, thereby significantly reducing the time and cost required for research and development of membrane electrode assemblies and fuel cells. [Brief description of the drawings]
[0028] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0029] [Figure 1] 1 is a cross-sectional view of a polymer electrolyte membrane according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0031] FIG. 1 is a cross-sectional view of a polymer electrolyte membrane 100 according to one embodiment of the present invention.
[0032] As illustrated in FIG. 1, a polymer electrolyte membrane 100 of the present invention includes a composite layer 110 including a porous support 10 having a large number of voids and ionomers 21, 22 filling the voids.
[0033] The porous support 10 is made of a perfluorinated polymer that is highly resistant to thermal and chemical decomposition [e.g., polytetrafluoroethylene (PTFE), or tetrafluoroethylene and CF2=CFC]. n F 2n+1 (n is a real number from 1 to 5) or CF2 = CFO-(CF2CF(CF3)O) m C n F 2n+1 (m is a real number from 0 to 15, and n is a real number from 1 to 15). As a non-exclusive example, a commercially available expanded polytetrafluoroethylene film (e-PTFE film) can be used as the porous support 10.
[0034] Alternatively, the porous support 10 may be a nonwoven web formed of a hydrocarbon-based polymer. For example, the porous support 10 may be a nanoweb in which nanofibers having an average diameter of 40 to 5000 nm are randomly arranged. The hydrocarbon-based polymer may be a polymer having excellent chemical resistance and not susceptible to deformation due to moisture in a high humidity environment, for example, an aliphatic polyamide, an aromatic polyamide, a polyimide, a polyetherimide, a polyacrylonitrile, a polyaniline, a polyethylene oxide, a polyethylene naphthalate, a polybutylene terephthalate, a styrene butadiene rubber, a polystyrene, a polyvinyl chloride, a polyvinyl alcohol, a polyvinylidene fluoride, a polyvinyl butylene, a polyurethane, a polybenzoxazole, a polybenzimidazole, a polyamide imide, a polyethylene terephthalate, a polyphenylene sulfide, a polyethylene, a polypropylene, a copolymer of two or more of these, or a mixture of two or more of these. In particular, polyimide is one of the preferred candidate materials for forming the porous support 10, since it has excellent heat resistance, chemical resistance and dimensional stability.
[0035] The porosity of the porous support 10 may be 45% or more, preferably 50% or more, and more preferably 60 to 90%. If the porosity of the porous support 10 is less than 45%, the amount of ionomer in the porous support 10 is too small, resulting in a decrease in the ion conductivity of the polymer electrolyte membrane 100. On the other hand, if the porosity of the porous support 10 is more than 90%, not only is its inherent reinforcing function impaired, but its morphological stability is also reduced, which may prevent the smooth progress of subsequent processes.
[0036] The ionomers 21 and 22 are cation conductors having cation exchange groups or anion conductors having anion exchange groups.
[0037] The cationic conductor may be a fluoropolymer containing at least one cationic exchange group selected from the group consisting of sulfonic acid groups, carboxyl groups, boric acid groups, phosphoric acid groups, imide groups, sulfonimide groups, sulfonamide groups, sulfonic acid fluoride groups, and derivatives thereof. For example, the cationic conductor may be, but is not limited to, poly(perfluorosulfonic acid), poly(perfluorocarboxylic acid), a copolymer of tetrafluoroethylene and fluorovinyl ether containing a sulfonic acid group, defluorinated sulfurized polyether ketone, or a mixture of two or more of these.
[0038] Alternatively, the cationic conductor may be a hydrocarbon-based polymer containing at least one cationic exchange group selected from the group consisting of a sulfonic acid group, a carboxyl group, a boric acid group, a phosphoric acid group, an imide group, a sulfonimide group, a sulfonamide group, a sulfonic acid fluoride group, and derivatives thereof. For example, the cationic conductor may be sulfonated polyimide (S-PI), sulfonated polyarylethersulfone (S-PAES), sulfonated polyetheretherketone (SPEEK), sulfonated polybenzimidazole (SPBI), sulfonated polysulfone (S-PSU), sulfonated polystyrene (S-PS), sulfonated polyphosphazene, sulfonated polyquinoxaline, sulfonated polyketone, sulfonated polyphenylene oxide, sulfonated polyethersulfone ... sulfone, sulfonated polyether ketone, sulfonated polyphenylene sulfone, sulfonated polyphenylene sulfide, sulfonated polyphenylene sulfide sulfone, sulfonated polyphenylene sulfide sulfone nitrile, sulfonated polyarylene etherThe polyarylene ether may be, but is not limited to, sulfonated polyarylene ether nitrile, sulfonated polyarylene ether ether nitrile, sulfonated polyarylene ether sulfone ketone, or a mixture of two or more thereof.
[0039] The anion conductor is a polymer capable of transporting anions. In general, the anion conductor may be a polymer doped with a metal hydroxide, and more specifically, may be poly(ether sulfone), polystyrene, vinyl polymer, poly(vinyl chloride), poly(vinyl fluoride), poly(tetrafluoroethylene), poly(benzimidazole), or poly(ethylene glycol) doped with a metal hydroxide.
[0040] The polymer electrolyte membrane 100 of the present invention has an MD tear strength of 150 N / mm or more (eg, 170 to 320 N / mm) and a TD tear strength of 150 N / mm or more (eg, 160 to 320 N / mm).
[0041] The terms "MD" and "TD" used in this specification mean "machine direction" and "traverse direction", respectively. The "machine direction" is the direction in which the polymer electrolyte membrane 100 moves when it is manufactured, and the "traverse direction" is the direction perpendicular to the "machine direction".
[0042] In the present invention, the "tear strength" of the polymer electrolyte membrane 100 is a value measured as follows.
[0043] [Tear strength]
[0044] After taking a sample of 50 mm×50 mm, a Universal Test Machine (UTM) (Instron 5966) is used to measure the maximum force applied until the sample is torn according to ASTM D624 under the following conditions:
[0045] -Temperature: 23±2℃
[0046] -Relative humidity: 50±5%
[0047] -Test speed: 500±50mm / min
[0048] The tear strength of the sample is then calculated using the following Equation 1:
[0049] "Formula 1" TS=F / d
[0050] Here, TS is the tear strength of the sample (N / mm), F is the maximum force applied to the sample (N), and d is the median thickness (mm), which is the arithmetic average of the thicknesses measured at three points in the center of the sample.
[0051] After the tear strength of each of the five samples is determined in this manner, the arithmetic average of these is calculated to obtain the tear strength of the polymer electrolyte membrane 100.
[0052] Even if the polymer electrolyte membrane 100 has MD tear strength and TD tear strength in the above-mentioned ranges, a membrane electrode assembly manufactured by a conventional method using such a polymer electrolyte membrane 100 does not always meet the high durability required by the industry (i.e., >30,000 wet / dry cycles measured by the accelerated durability evaluation method of the NEDO protocol). In other words, an MD tear strength of 150 N / mm or more and a TD tear strength of 150 N / mm or more are only necessary conditions for a membrane electrode assembly to meet 30,000 or more wet / dry cycles, but are not sufficient conditions.
[0053] Therefore, even if the polymer electrolyte membrane 100 has an MD tear strength of 150 N / mm or more and a TD tear strength of 150 N / mm or more, in order to determine whether a membrane electrode assembly manufactured by a conventional method using the polymer electrolyte membrane 100 has sufficient durability, it is necessary to actually manufacture a membrane electrode assembly sample and perform a durability test by the accelerated durability evaluation method of the NEDO protocol, which not only takes a long time but also increases costs.
[0054] According to the present invention, it has been found that when a polymer electrolyte membrane 100 having an MD tear strength of 150 N / mm or more and a TD tear strength of 150 N / mm or more has an IS / FS ratio [i.e., the ratio of initial puncture deformation rate (IS) to final puncture deformation rate (FS)] of 0.4 to 1.0, a membrane electrode assembly manufactured by a conventional method using the polymer electrolyte membrane 100 can always meet 30,000 or more wet / dry cycles. Therefore, according to the present invention, by measuring the IS / FS ratio of the polymer electrolyte membrane 100, it is possible to know whether the membrane electrode assembly meets the mechanical durability required by the industry without actually manufacturing the membrane electrode assembly, and as a result, it is possible to significantly reduce the time and cost required for research and development of membrane electrode assemblies and fuel cells.
[0055] In the present invention, the "initial puncture deformation rate (IS)" and the "final puncture deformation rate (FS)" of the polymer electrolyte membrane 100 are measured as follows.
[0056] [Initial and final deformation rates of thrust]
[0057] After taking a sample of 50 mm x 50 mm, the puncture resistance of the sample is measured using a universal testing machine (UTM) (Instron 5966). As an accessory for performing repeated punctures, a jig (sample holder and probe) for puncture testing according to ASTM F1342 provided by Instron is used. Specifically, the sample is fixed to a holder (distance from base level to the sample: 100 mm) and repeatedly punctured with a probe (load: 10 N) under the following conditions, and the reduction in the distance (i.e., "displacement") due to each puncture is measured. Here, the displacement when a load of 0.2 N is applied is regarded as the zero point.
[0058] -Temperature: 23±2℃
[0059] -Relative humidity: 50±5%
[0060] -Mode: Compressed mode
[0061] -Cyclic Period: 20 times
[0062] -Test Speed: 100mm / min
[0063] The deformation rate when the probe is repeatedly pierced (load: 10 N) twice [i.e., the "initial piercing deformation rate (IS)] and the deformation rate when the probe is repeatedly pierced 20 times [i.e., the "final piercing deformation rate (FS)] are calculated using the following formulas 2 and 3, respectively.
[0064] "Formula 2" IS(%)=[(D2-D1) / D1]×100
[0065] "Formula 3" FS(%)=[(D 20 -D1) / D1] × 100
[0066] where IS is the initial deformation rate, FS is the final deformation rate, D1 is the displacement due to the first thrust (mm), D2 is the displacement due to the second thrust (mm), and D 20 is the displacement (mm) due to the 20th thrust.
[0067] The polymer electrolyte membrane 100 of the present invention has an IS / FS ratio of 0.4 to 1.0, which ensures the production of a highly durable membrane electrode assembly capable of withstanding more than 30,000 wet / dry cycles as measured by the accelerated durability evaluation method of the NEDO protocol.
[0068] According to an embodiment of the present invention, the polymer electrolyte membrane 100 may have an initial puncture deformation (IS) of 1 to 6% and a final puncture deformation (FS) of 2 to 8%.
[0069] According to the present invention, the polymer electrolyte membrane 100 may have an in-plane ion conductivity of 0.03 to 0.1 S / cm, more specifically 0.040 to 0.1 S / cm, and even more specifically 0.040 to 0.050 S / cm, and a through-plane ion conductivity of 0.03 to 0.1 S / cm, more specifically 0.038 to 0.1 S / cm, and even more specifically 0.038 to 0.045, under conditions of 80° C. and 50% RH (the specific reasons why the polymer electrolyte membrane 100 of the present invention can have such high ion conductivity while having excellent mechanical properties will be described later).
[0070] Therefore, the polymer electrolyte membrane 100 according to one embodiment of the present invention has excellent mechanical properties (i.e., IS / FS ratio of 0.4 to 1.0) without any deterioration in performance such as ionic conductivity, thereby ensuring the manufacture of a membrane electrode assembly having excellent electrical performance as well as high durability of more than 30,000 wet / dry cycles.
[0071] In the present invention, the in-plane ion conductivity and the thickness ion conductivity of the polymer electrolyte membrane 100 are measured by the following methods.
[0072] [In-plane ionic conductivity]
[0073] The in-plane ionic conductivity of the polymer electrolyte membrane 100 is measured at 80° C. and 50% RH using a Magnetic Suspension Balance device (manufactured by Bell Japan).
[0074] [Thickness ionic conductivity]
[0075] The through-plane ionic conductivity of the polymer electrolyte membrane 100 is measured by a constant current four-terminal method using a through-plane membrane test system (Scribner Associates, MTS 740). Specifically, an AC current is applied to both sides of a sample (10 mm x 30 mm) at 80°C and 50% RH, and the AC potential difference generated within the sample is measured to obtain the membrane resistance (R) (Ω). The through-plane ionic conductivity of the polymer electrolyte membrane 100 is then calculated using the following Equation 4.
[0076] "Formula 4" σ=L / [R×A]
[0077] [where σ is the thickness ionic conductivity (S / cm), L is the distance between the electrodes (cm), R is the membrane resistance (Ω), and A is the effective area of the membrane (cm 2 ) is
[0078] As illustrated in FIG. 1, according to one embodiment of the present invention, the composite layer 110 has a first surface and a second surface opposite to the first surface, and the polymer electrolyte membrane 100 may further include a first pure layer 120 disposed on the first surface and a second pure layer 130 disposed on the second surface.
[0079] The first pure layer 120 may include a first ionomer 21 and the second pure layer 130 may include a second ionomer 22 .
[0080] At least a portion of the ionomer in the composite layer 110 may be identical to at least one of the first ionomer 21 of the first pure layer 120 and the second ionomer 22 of the second pure layer 130 .
[0081] According to one embodiment of the present invention, the thickness (T total ) may be 10 to 50 μm, and the thickness (T c ) is the thickness (T total ) can be 30 to 80%, more specifically 35 to 75%, and even more specifically 40 to 70%.
[0082] That is, according to one embodiment of the present invention, the thickness (T c ) is the thickness (T total ), the IS / FS ratio is 30% or more, more specifically 35% or more, and even more specifically 40% or more, so that the polymer electrolyte membrane 100 can have excellent mechanical properties (i.e., an IS / FS ratio of 0.4 to 1.0) that can ensure the manufacture of a membrane electrode assembly having high durability of 30,000 or more wet / dry cycles.
[0083] Meanwhile, the thickness (T c ) is the thickness (T total ) (ie, if the first and second pure layers 120 and 130 are relatively too thin), the polymer electrolyte membrane 100 is unlikely to have a high ionic conductivity within the range of the present invention.
[0084] As illustrated in FIG. 1, a porous support 10 according to one embodiment of the present invention includes a first porous sub-support 11 and a second porous sub-support 12 .
[0085] The first porous sub-support 11 comprises the first surface of the composite layer 110. That is, one surface of the first porous sub-support 11 constitutes the first surface of the composite layer 110. Similarly, the second porous sub-support 12 comprises the second surface of the composite layer 110. That is, one surface of the second porous sub-support 12 constitutes the second surface of the composite layer 110.
[0086] The first and second porous sub-supports 11, 12 may be the same or different supports. For example, the first and second porous sub-supports 11, 12 may both be e-PTFE films, or the first and second porous sub-supports 11, 12 may both be nonwoven webs. When the first and second porous sub-supports 11, 12 are both e-PTFE films, they may be laminated such that their stretch directions are perpendicular to each other.
[0087] As illustrated in Fig. 1, the first and second porous sub-supports 11 and 12 may be in contact with each other. Since the first and second porous sub-supports 11 and 12 are in tight contact with each other, it may be impossible to visually confirm the interface therebetween unless they are different types of porous supports that can be distinguished from each other. That is, the porous support 10 may be an apparent single porous support.
[0088] The polymer electrolyte membrane 100 according to one embodiment of the present invention having the first and second porous sub-supports 11 and 12 provides many advantages in many aspects compared to a polymer electrolyte membrane reinforced by an actual single porous support having the same thickness as the porous support 10 (i.e., providing the same or similar mechanical properties). For example, according to one embodiment of the present invention, compared to a case where an actual single porous support having the same thickness as the porous support 10 is impregnated with an ionomer, (i) since the surface area of the porous support 10 that directly contacts the ionomer in the ionomer impregnation process is larger, the wettability of the porous support 10 with respect to the ionomer solution or dispersion is good, and the decrease in ion conductivity of the polymer electrolyte membrane 100 due to the use of the support can be minimized (i.e., the air that was present in the voids of the support 10 is more efficiently discharged and the space is filled with the ionomer, thereby preventing microbubbles that adversely affect ion conductivity from remaining in the final polymer electrolyte membrane 100, and thus water channels, which are paths for the movement of hydrogen ions, can be well formed in the thickness direction of the support 10); and (ii) since the area that can mitigate deformation of the polymer electrolyte membrane 100 is increased, the puncture deformation rate of the polymer electrolyte membrane 100 can be reduced (i.e., the puncture resistance can be improved).
[0089] As a result, the polymer electrolyte membrane 100 having the first and second porous sub-supports 11 and 12 according to an embodiment of the present invention can have excellent mechanical properties without any degradation in performance such as ion conductivity.
[0090] According to one embodiment of the present invention, the ratio of MD tensile elongation to TD tensile elongation of each of the first and second porous sub-supports 11 and 12 (hereinafter, "MD / TD tensile elongation ratio") may be 0.9 to 1.5, more specifically, 1 to 1.3. That is, according to one embodiment of the present invention, by using highly isotropic supports having an MD / TD tensile elongation ratio in this range as the first and second porous sub-supports 11 and 12, it is possible to manufacture a polymer electrolyte membrane 100 having excellent mechanical properties (i.e., an IS / FS ratio of 0.4 to 1.0) that can ensure the manufacture of a membrane electrode assembly having high durability of more than 30,000 wet / dry cycles.
[0091] The first porous sub-support 11 has a number of first voids, which may be filled with an ionomer that is the same as the first ionomer 21 of the first pure layer 120 .
[0092] The second porous sub-support 12 has a number of second voids, and a portion of the second voids adjacent to the first porous sub-support 11 can be filled with the same ionomer as the first ionomer 21 of the first pure layer 120, and the remainder of the second voids adjacent to the second pure layer 130 can be filled with the same ionomer as the second ionomer 22 of the second pure layer 130.
[0093] That is, according to one embodiment of the present invention, since the interface between the first and second ionomers 21, 22 exists within the second porous sub-support 12 [i.e., the first ionomer 21 existing within the second porous sub-support 12 functions as an anchor], (i) a strong adhesive force between the first and second porous sub-supports 11, 12 comparable to a laminated structure in which the porous supports are bonded by an adhesive and / or thermocompression bonding can be secured, and (ii) a decrease in ion conductivity that may be caused when the supports are bonded by the adhesive and / or thermocompression bonding can be prevented. Thus, the polymer electrolyte membrane 100 according to one embodiment of the present invention can have excellent mechanical properties without a decrease in performance such as ion conductivity.
[0094] The first ionomer 21 can be the same as or different from the second ionomer 22.
[0095] Hereinafter, a method for manufacturing the polymer electrolyte membrane 100 according to an embodiment of the present invention shown in FIG. 1 will be described in detail.
[0096] The method according to one embodiment of the present invention includes the steps of: (i) casting a first ionomer dispersion containing a first ionomer 21 onto a glass plate; (ii) placing a first porous sub-support 11 in a dry state on the first ionomer dispersion, thereby making the first porous sub-support 11 entirely wet. (iii) immediately after the first porous sub-support 11 has become entirely wet, adding a second porous sub-support 12 in a dry state to the first porous sub-support 11 so that the first and second porous sub-supports 11, 12 are in contact with each other; (iv) applying a second ionomer dispersion including a second ionomer 22 onto the second porous sub-support 12 to make the second porous sub-support 12 entirely wet; and (v) drying the first and second porous sub-supports 11, 12 in the wet state.
[0097] While the first porous sub-support 11 is maintained in a generally wet state with the first ionomer dispersion, the second porous sub-support 12 is bonded thereon, so that a portion of the second voids of the second porous sub-support 12 can be filled with the first ionomer dispersion. Therefore, as described above, the first ionomer 21 present in a portion of the second voids of the second porous sub-support 12 functions as an anchor, so that strong adhesive force between the first and second porous sub-supports 11 and 12 can be secured, and the mechanical properties of the polymer electrolyte membrane 100 can be significantly improved.
[0098] Furthermore, according to the present invention, such high adhesive strength between the first and second porous sub-supports 11 and 12 can be obtained without using a separate adhesive and / or a hot press process, so that a decrease in ion conductivity that may be caused when the supports are bonded by the adhesive and / or hot press can be prevented. Therefore, the polymer electrolyte membrane 100 according to an embodiment of the present invention can have excellent mechanical properties without a decrease in performance such as ion conductivity.
[0099] That is, the polymer electrolyte membrane 100 of the present invention is distinguished from a laminated polymer electrolyte membrane produced by producing two or more polymer electrolyte membranes and then bonding them with an adhesive and / or thermocompression bonding in that it does not include a pure layer consisting of only an ionomer between the first and second porous sub-supports 11, 12. Unlike the present invention, such a laminated polymer electrolyte membrane not only (i) inevitably accompanies a decrease in ion conductivity due to the adhesive and / or thermocompression bonding as described above, but also (ii) the presence of a pure layer consisting of only an ionomer between the porous supports relatively reduces resistance to hydrogen gas movement, resulting in a significantly reduced chemical durability due to a relatively high hydrogen permeability.
[0100] As previously mentioned, the first and second porous sub-supports 11, 12 can be the same or different supports, for example, the first and second porous sub-supports 11, 12 can both be e-PTFE films, or the first and second porous sub-supports 11, 12 can both be nonwoven webs.
[0101] As described above, according to one embodiment of the present invention, each of the first and second porous sub-supports 11 and 12 is a support having relatively high isotropy, with a MD / TD tensile elongation ratio of 0.9 to 1.5, more specifically, 1 to 1.3.
[0102] Nevertheless, in the case of an e-PTFE film that can be used as the first and second porous sub-supports 11 and 12 of the present invention, there is a certain degree of difference between the mechanical properties in the stretching direction (i.e., MD direction) and the mechanical properties in the direction perpendicular to the stretching direction (i.e., TD direction) (i.e., the MD / TD tensile elongation ratio is slightly lower or slightly higher than 1). Therefore, when the first and second porous sub-supports 11 and 12 are both e-PTFE films, the second porous sub-support 12 is bonded onto the first porous sub-support 11 so that their stretching directions are perpendicular to each other, thereby further enhancing the overall isotropy of the porous support 10 and further improving the mechanical properties of the polymer electrolyte membrane 100.
[0103] The step of applying a second ionomer dispersion containing a second ionomer 22 onto the second porous sub-support 12 to wet the second porous sub-support 12 entirely may include (i) attaching the second porous sub-support 12 to the first porous sub-support 11 and then immersing the first and second porous sub-supports 11, 12 together in the second ionomer dispersion when the first ionomer 21 and the second ionomer 22 are the same, or (ii) applying the second ionomer dispersion onto the exposed surface of the second porous sub-support 12 by a method such as bar coating, comma coating, slot die, screen printing, spray coating, or doctor blade.
[0104] Each of the first and second ionomer dispersions may be a dispersion in which the first ionomer 21 or the second ionomer 22 is dispersed in water, a hydrophilic solvent, an organic solvent, or a mixed solvent of two or more of these.
[0105] The hydrophilic solvent contains a linear or branched, saturated or unsaturated hydrocarbon having 1 to 12 carbon atoms as a main chain, and may have one or more functional groups selected from the group consisting of alcohol, isopropyl alcohol, ketone, aldehyde, carbonate, carboxylate, carboxylic acid, ether and amide, and may contain an alicyclic or aromatic cyclo compound as at least a part of the main chain.
[0106] The organic solvent may be N-methylpyrrolidone, dimethylsulfoxide, tetrahydrofuran, or a mixture of two or more thereof.
[0107] In order to completely fill the voids of the first and second porous sub-supports 11 and 12 with the ionomers 21 and 22, various factors such as temperature and time, for example, at least one of the thicknesses of the first and second porous sub-supports 11 and 12, the concentrations of the first and second mixed liquids, and the type of solvent / dispersion medium, may be appropriately adjusted.
[0108] The step of drying the first and second porous sub-supports 11 and 12 that have been bonded together may be performed by performing a primary drying at 60°C to 150°C for 15 minutes to 1 hour, and a secondary drying at 150°C to 190°C for 3 minutes to 1 hour, specifically, performing a primary drying at 60°C to 120°C for 15 minutes to 1 hour, and a secondary drying at 170°C to 190°C for 3 minutes to 1 hour. If the primary drying temperature is less than 60°C or the primary drying time is less than 15 minutes, the solvent / dispersion medium cannot flow out primarily, and a dense membrane cannot be obtained. If the secondary drying temperature exceeds 190°C or the secondary drying time exceeds 1 hour, the ion exchange group (e.g., sulfonic acid group) is decomposed, and the membrane performance may be deteriorated.
[0109] Although the polymer electrolyte membrane 100 illustrated in FIG. 1 includes only two porous sub-supports 11, 12, the polymer electrolyte membrane 100 of the present invention may include more than two porous sub-supports depending on the specific physical properties required.
[0110] According to another embodiment of the present invention, the polymer electrolyte membrane 100 includes a single porous support 10 instead of multiple porous sub-supports 11 and 12, and the ionomer dispersion impregnated in the voids of the single porous support 10 can be prepared by adding an ionomer to a solvent and then mixing them using a resonant ultrasonic method. The ionomer dispersion prepared in this manner has high dispersion stability.
[0111] By applying high pressure to the mixture obtained by the resonant sonic mixing, the dispersion stability of the ionomer dispersion can be further improved.
[0112] In the present invention, the ionomer dispersion liquid having high dispersion stability is obtained by controlling the shear rate to 0.001 s using a rheometer. -1 From 1000s -1 After increasing to 1000s -1 From 0.001s -1 When the viscosity and shear stress of the ionomer dispersion are measured while decreasing the temperature to 100° C., the ionomer dispersion has a viscosity ratio defined by the following Equation 5 of 1.7 or less and a shear stress ratio defined by the following Equation 6 of 1.5 or less.
[0113]
[0113] "Formula 5" Viscosity ratio=η2 / η1
[0114] (Here, η1 is the shear rate measured during the shear rate increase process, -1 η2 is the first viscosity of the ionomer dispersion when the shear rate is 1 s -1 is the second viscosity of the ionomer dispersion at
[0115] "Formula 6" Shear stress ratio = σ2 / σ1
[0116] (where σ1 is the shear rate measured during the shear rate increase process, -1 σ2 is the first shear stress measured during the shear rate decrease process when the shear rate is 1s -1 (The second shear stress is the shear stress at
[0117] An ionomer dispersion that contains a high content of ionomer solids while having sufficiently high dispersion stability can optimize the morphology of the ionomer in the polymer electrolyte membrane 100, thereby improving the ionic conductivity of the polymer electrolyte membrane 100.
[0118] Specifically, an ionomer dispersion having high dispersion safety has excellent impregnation properties and small and uniform particle size. Therefore, when the ionomer dispersion is impregnated and coated on a porous support 10 to form a reinforced composite membrane type polymer electrolyte membrane 100, water channels that provide paths for hydrogen ion migration are well formed not only in the planar direction but also in the thickness direction, thereby improving the ionic conductivity of the polymer electrolyte membrane 100 in both the planar direction and the thickness direction.
[0119] Therefore, the thickness of the composite layer 110 (T c ) is the thickness (T total Even when a sufficiently thick single porous support 10, equivalent to 30 to 80% of the total surface area of the support 10, is used, the use of the ionomer dispersion of the present invention having high dispersion stability can offset the decrease in ion conductivity that may be caused by the use of the thick single porous support 10. Therefore, the polymer electrolyte membrane 100 obtained according to this embodiment not only has excellent mechanical durability (i.e., IS / FS ratio of 0.4 to 1.0) thanks to the thick single porous support 10, but also has excellent ion conductivity (i.e., in-plane and thickness ion conductivity of 0.03 to 0.1 S / cm under conditions of 80° C. and 50% RH) thanks to the ionomer dispersion having high dispersion stability.
[0120] It goes without saying that the above-mentioned ionomer dispersion having high dispersion stability can be preferably applied to the polymer electrolyte membrane 100 having a large number of porous sub-supports 11 and 12.
[0121] The membrane electrode assembly of the present invention includes an anode, a cathode, and the polymer electrolyte membrane 100 disposed between the anode and the cathode. The membrane electrode assembly is a polymer electrolyte membrane, and is similar to a membrane electrode assembly for a general fuel cell except that the polymer electrolyte membrane 100 according to the present invention is used, so a detailed description thereof will be omitted in this specification.
[0122] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as being limited to the embodiments set forth herein, but the present invention is not limited to the embodiments set forth herein.
[0123] [Manufacturing example: Manufacturing of polymer electrolyte membrane]
[0124] Example 1
[0125] A first porous sub-support (e-PTFE, pore size: 0.10 μm-0.2 μm, thickness: 8 μm, MD / TD tensile elongation ratio: 1.3) was wetted with a first ionomer dispersion ("resonant ultrasonic mixing + high pressure dispersion", viscosity ratio: 1.31, shear stress ratio: 1.08) containing a highly fluorinated polymer with an equivalent weight (EW) of 700 g / eq at a content of 20 wt%.
[0126] While the first porous sub-support was wetted, a second porous sub-support (e-PTFE, pore size: 0.10 μm to 0.2 μm, thickness: 8 μm, MD / TD tensile elongation ratio: 1.3) was bonded to the first porous sub-support so that the stretching directions crossed.
[0127] With the first and second porous sub-supports bonded together, a second ionomer dispersion ("resonant ultrasonic mixing + high pressure dispersion", viscosity ratio: 1.31, shear stress ratio: 1.08) containing a highly fluorinated polymer with an equivalent weight (EW) of 700 g / eq at a content of 20 wt% was further applied.
[0128] After that, it was dried at 60°C for 1 hour, and then further dried at 150°C for 30 minutes to a thickness of 20 μm (T total A polymer electrolyte membrane having a composite layer thickness (T c ) is the thickness of the polymer electrolyte membrane (T total ) was 40%.
[0129] Example 2
[0130] The first porous sub-support (e-PTFE, pore size: 0.10 μm-0.2 μm, thickness: 8 μm, MD / TD tensile elongation ratio: 1.2) was wetted with a first ionomer dispersion (resonant sonic wave method mixing, viscosity ratio: 1.36, shear stress ratio: 1.06) containing a highly fluorinated polymer with an equivalent weight (EW) of 700 g / eq at a content of 20 wt%.
[0131] While the first porous sub-support was wet, a second porous sub-support (e-PTFE, pore size: 0.10 μm to 0.2 μm, thickness: 8 μm, MD / TD tensile elongation ratio: 1.2) was bonded to the first porous sub-support so that the stretching directions crossed each other. At this time, the first and second porous sub-supports were laminated so that the stretching directions of the first and second porous sub-supports crossed each other perpendicularly.
[0132] With the first and second porous sub-supports bonded together, a second ionomer dispersion (resonant sonic mixing, viscosity ratio: 1.36, shear stress ratio: 1.06) containing a highly fluorinated polymer with an equivalent weight (EW) of 700 g / eq at a content of 20 wt% was further applied.
[0133] After that, it was dried at 60°C for 1 hour, and then further dried at 150°C for 30 minutes to obtain a thickness of 20 μm (T totalA polymer electrolyte membrane having a composite layer thickness (T c ) is the thickness of the polymer electrolyte membrane (T total ) was 40%.
[0134] Comparative Example 1
[0135] A porous support (e-PTFE, pore size: 0.10 μm-0.2 μm, thickness: 6 μm, MD / TD tensile elongation ratio: 1.4) was wetted with a first ionomer dispersion ("resonant sonic wave method mixing + high pressure dispersion", viscosity ratio: 1.36, shear stress ratio: 1.08) containing a highly fluorinated polymer with an equivalent weight (EW) of 700 g / eq at a content of 20 wt%.
[0136] Next, a second ionomer dispersion ("resonant ultrasonic mixing + high pressure dispersion", viscosity ratio: 1.31, shear stress ratio: 1.08) containing a highly fluorinated polymer with an equivalent weight (EW) of 700 g / eq at a content of 20 wt% was further coated onto the porous support.
[0137] After that, it was dried at 60°C for 1 hour, and then further dried at 150°C for 30 minutes to obtain a thickness of 12 μm (T total A polymer electrolyte membrane having a composite layer thickness (T c ) is the thickness of the polymer electrolyte membrane (T total ) was 25%.
[0138] [Measurement of physical properties of polymer electrolyte membranes]
[0139] The IS / FS ratio, in-plane ionic conductivity and thickness ionic conductivity of the polymer electrolyte membranes of the Examples and Comparative Examples were measured by the following methods, and the results are shown in Table 1 below.
[0140] *Ratio of initial deformation rate to final deformation rate (IS / FS ratio)
[0141] After taking a sample of 50 mm x 50 mm, the puncture resistance of the sample was measured using a universal testing machine (UTM) (Instron 5966). As an accessory for performing repeated punctures, a puncture test jig (sample holder and probe) according to ASTM F1342 provided by Instron was used. Specifically, the sample was fixed to a holder (distance from base level to the sample: 100 mm) and repeatedly punctured with a probe (load: 10 N) under the following conditions, and the reduction in the distance (i.e., "displacement") due to each puncture was measured. In this case, the displacement when a load of 0.2 N was applied was regarded as the zero point.
[0142] -Temperature: 23±2℃
[0143] -Relative humidity: 50±5%
[0144] -Mode: Compressed mode
[0145] -Circulation cycle: 20 times
[0146] -Test speed: 100mm / min
[0147] The deformation rate when the probe was repeatedly pierced (load: 10 N) twice (i.e., "initial piercing deformation rate") and the deformation rate when the probe was repeatedly pierced 20 times (i.e., "final piercing deformation rate") were calculated using the following formulas 2 and 3, respectively.
[0148] "Formula 2" IS(%)=[(D2-D1) / D1]×100
[0149] "Formula 3" FS(%)=[(D 20 -D1) / D1] × 100
[0150] where IS is the initial deformation rate, FS is the final deformation rate, D1 is the displacement due to the first thrust (mm), D2 is the displacement due to the second thrust (mm), and D 20 is the displacement (mm) due to the 20th thrust.
[0151] The IS / FS ratio was calculated by dividing the IS by the FS.
[0152] * Planar ionic conductivity
[0153] The in-plane ionic conductivity of the polymer electrolyte membrane was measured at 80° C. and 50% RH using a Magnetic Suspension Balance device (Bell Japan).
[0154] *Ion conductivity through thickness
[0155] The through-plane ionic conductivity of the polymer electrolyte membrane was measured by a constant current four-terminal method using a through-plane membrane test system (Scribner Associates, MTS740). Specifically, an alternating current was applied to both sides of a sample (10 mm x 30 mm) at 80°C and 50% RH, and the difference in the AC potential generated within the sample was measured to obtain the membrane resistance (R) (Ω). The through-plane ionic conductivity of the polymer electrolyte membrane was then calculated using the following Equation 4.
[0156] "Formula 4" σ=L / [R×A]
[0157] [where σ is the thickness ionic conductivity (S / cm), L is the distance between the electrodes (cm), R is the membrane resistance (Ω), and A is the effective area of the membrane (cm 2 ) is
[0158] [Wet / dry cycle measurement of membrane electrode assembly (MEA)]
[0159] After preparing a membrane electrode assembly (MEA) using the polymer electrolyte membrane, its wet / dry cycle was measured by the accelerated durability evaluation method of the NEDO protocol. Specifically, a wet / dry cycle consisting of humidification (150% RH, 2 min) and drying (0% RH, 2 min) was repeated while injecting nitrogen gas at a flow rate of 800 NmL / min into the anode and cathode, respectively, at 80°C. The hydrogen crossover of the MEA was measured by LSV (linear sweep voltammetry) every 1000 cycles. Specifically, hydrogen gas was injected into the anode at a flow rate of 200 NmL / min and nitrogen gas was injected into the cathode at a flow rate of 200 NmL / min at 80°C and 100% RH, and the current density data in the 0.4-0.5 V section was extracted by sweeping the 0.2-0.5 V section at a scan rate of 0.5 mV / s. The data was linearly fitted to obtain the current density value in the range where the voltage was 0. When the measured hydrogen permeability was 10 times or more the initial hydrogen permeability, the evaluation was terminated, and the number of cycles performed up to that point was taken as the wet / dry cycle of the MEA. For example, if the hydrogen permeability measured after a total of 15,000 cycles was less than 10 times the initial hydrogen permeability, but the hydrogen permeability measured after a total of 16,000 cycles was 10 times or more the initial hydrogen permeability, the wet / dry cycle of the MEA would be "15,000 cycles or more."
[0160] [Table 1]
[0161] As can be seen from Table 1, the thickness of the composite layer (T c ) is the thickness of the polymer electrolyte membrane (T totalThe polymer electrolyte membrane of Comparative Example 1, in which the tensile elongation ratio of the porous support was 25% of the tensile elongation ratio of the porous support of 1.4, had good ionic conductivity but a low IS / FS ratio (i.e., the ratio of the initial puncture deformation rate to the final puncture deformation rate) of less than 0.4. In addition, the membrane electrode assembly (MEA) manufactured using the polymer electrolyte membrane of Comparative Example 1 showed low durability, with wet / dry cycles of about 20,000 cycles or less as measured by the accelerated durability evaluation method of the NEDO protocol.
[0162] In contrast, the thickness of the composite layer (T c ) is the thickness of the polymer electrolyte membrane (T total The polymer electrolyte membranes of Examples 1 and 2, in which the sub-porous supports having an MD / TD tensile elongation ratio of 40% and an MD / TD tensile elongation ratio of 1.3 or less were laminated so that the stretching directions crossed perpendicularly, not only had mechanical durability several times higher than that of the polymer electrolyte membrane of Comparative Example 1 (i.e., an IS / FS ratio of 0.4 or more), but also membrane electrode assemblies (MEAs) produced using them showed high durability of about 50,000 wet / dry cycles or more as measured by the accelerated durability evaluation method of the NEDO protocol. In addition, the polymer electrolyte membranes of Examples 1 and 2 showed excellent ionic conductivity that was not inferior to that of the polymer electrolyte membrane of Comparative Example 1, despite having mechanical durability several times higher than that of the polymer electrolyte membrane of Comparative Example 1.
Claims
1. A polymer electrolyte membrane, The composite layer includes a porous support having a number of voids and an ionomer that fills the voids, The polymer electrolyte membrane has an in-plane ion conductivity of 0.03 to 0.1 S / cm and a thickness ion conductivity of 0.03 to 0.1 S / cm under conditions of 80° C. and 50% RH, The polymer electrolyte membrane has an MD tear strength of 150 N / mm or more and a TD tear strength of 150 N / mm or more, a ratio (IS / FS) of an initial stab strain (IS) of the polymer electrolyte membrane to a final stab strain (FS) of the polymer electrolyte membrane is 0.4 to 1.0; The initial puncture deformation rate (IS) is the deformation rate when the probe is repeatedly punctured (load: 10N) twice, and the final puncture deformation rate (FS) is the deformation rate when the probe is repeatedly punctured (load: 10N) 20 times. The initial puncture deformation rate (IS) and the final puncture deformation rate (FS) are calculated by the following "Formula 1" and "Formula 2", respectively: "Formula 1" IS(%)=[(D 2 -D 1 ) / D 1 ]×100 "Formula 2" FS(%)=[(D 20 -D 1 ) / D 1 ]×100 where IS is the initial deformation rate of the thrust, FS is the final deformation rate of the thrust, and D 1 is the displacement (mm) due to the first piercing, D 2 is the displacement (mm) due to the second stab, and D 20 is the displacement (mm) due to the 20th thrust, Polymer electrolyte membrane.
2. 2. The polymer electrolyte membrane of claim 1, wherein the polymer electrolyte membrane has an initial puncture deformation (IS) of 1-6% and a final puncture deformation (FS) of 2-8%.
3. the composite layer has a first surface and a second surface opposite the first surface; The polymer electrolyte membrane is a first pure layer disposed on the first surface, the first pure layer comprising a first ionomer; a second pure layer disposed on the second surface, the second pure layer comprising a second ionomer, wherein the thickness of the composite layer is 30-80% of the thickness of the polymer electrolyte membrane.
4. The polymer electrolyte membrane according to claim 3, wherein the thickness of the polymer electrolyte membrane is 10 to 50 μm.
5. 4. The polymer electrolyte membrane of claim 3, wherein at least a portion of the ionomer of the composite layer is the same as at least one of the first ionomer and the second ionomer.
6. the porous support includes a first porous sub-support having the first surface and a second porous sub-support having the second surface; the first porous subsupport has a first void, the first void being filled with an ionomer that is the same as the first ionomer; 4. The polymer electrolyte membrane of claim 3, wherein the second porous subsupport has a second void, a portion of the second void adjacent the first porous subsupport being filled with the same ionomer as the first ionomer, and a remainder of the second void adjacent the second pure layer being filled with the same ionomer as the second ionomer.
7. The polymer electrolyte membrane of claim 6 , wherein the first and second porous subsupports are in contact with each other.
8. the porous support includes a first porous subsupport having the first surface, a second porous subsupport having the second surface, and at least one third porous subsupport between the first and second porous subsupports; the first and third porous subsupports are in contact with each other; the second and third porous sub-supports are in contact with each other; The polymer electrolyte membrane according to claim 3 .
9. The polymer electrolyte membrane of claim 3 , wherein the first ionomer is the same as the second ionomer.
10. An anode; A cathode; A membrane electrode assembly comprising the polymer electrolyte membrane of claim 1 disposed between the anode and the cathode.
Citation Information
Patent Citations
Multi-layered polymeric electrolyte membrane for fuel cell
JP2007109657A
Composition, copolymer, electrolyte membrane, method for producing them, and fuel cell
JP2010248488A
Ion exchange membrane, its manufacturing method, and energy storage device including the same
JP2019513164A
Ion exchange membrane, its manufacturing method, and energy storage device including the same
JP2019518588A
Highly reinforced ionomer membranes for high selectivity and strength
JP2020524367A