Materials for forming nucleation-inhibiting coatings and devices incorporating same - Patents.com
The application of a nucleation inhibiting coating in optoelectronic devices addresses the challenges of high evaporation temperatures and debris in conductive coating deposition, enhancing precision and reducing costs by eliminating the need for fine metal masks, thus improving manufacturing yield.
Patent Information
- Application Number
- JP2021566295
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-14
- Filing Date
- 2020-05-07
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-05-07
AI Technical Summary
Existing methods for depositing conductive coatings in optoelectronic devices, such as OLEDs, face challenges due to high evaporation temperatures of electrode materials, which affect the reusability and accuracy of fine metal masks, leading to increased cost and complexity, and often result in debris that compromises manufacturing yield.
The use of a nucleation inhibiting coating (NIC) on a first layer surface and a conductive coating on a second layer surface, where the initial adhesion probability for the conductive coating on the NIC is lower, allowing for precise pattern deposition without the need for fine metal masks, thereby reducing debris and manufacturing complexity.
This approach enables precise and efficient deposition of conductive coatings with reduced material waste and cost, improving the yield and accuracy of optoelectronic devices by minimizing the use of fine metal masks and debris-related issues.
Smart Images

Figure 0007576337000048 
Figure 0007576337000049 
Figure 0007576337000050
Abstract
Description
[Technical Field]
[0001] Related Applications This application claims the benefit of priority to U.S. Provisional Patent Application No. 62 / 845,273, filed May 8, 2019, and U.S. Provisional Patent Application No. 62 / 886,896, filed August 14, 2019, the contents of which are incorporated herein by reference in their entireties.
[0002] The present disclosure relates to optoelectronic devices, and in particular to optoelectronic devices having first and second electrodes separated by a semiconductive layer and having a conductive coating deposited thereon that is patterned using a nucleation-inhibiting coating (NIC). [Background technology]
[0003] In an optoelectronic device such as an organic light-emitting diode (OLED), at least one semiconductive layer is disposed between a pair of electrodes, such as an anode and a cathode. The anode and cathode are electrically coupled to a power source and cause holes and electrons, respectively, to migrate toward each other through the at least one semiconductive layer. When the hole and electron pairs combine, photons may be emitted.
[0004] An OLED display panel may include multiple (sub)pixels, each of which has an associated pair of electrodes. The various layers and coatings of such panels are typically formed by vacuum-based deposition techniques.
[0005] In some applications, it may be desirable to provide a conductive coating in a pattern for each (sub)pixel of the panel, across either or both of the lateral and cross-sectional sides of the panel, by selective deposition of the conductive coating to form device features, such as, but not limited to, electrodes and / or conductive elements electrically coupled thereto, during the OLED manufacturing process. Summary of the Invention [Means for solving the problem]
[0006] One method for doing so, in some non-limiting applications, involves the insertion of a fine metal mask (FMM) during the deposition of the electrode material and / or conductive elements electrically coupled thereto. However, materials typically used as electrodes have relatively high evaporation temperatures, which affect the ability to reuse the FMM and / or the precision of the patterns that can be achieved, with attendant increases in cost, effort, and complexity.
[0007] One method for doing so involves depositing the electrode material and then removing the unwanted areas to form the pattern, including, in some non-limiting examples, by a laser drilling process. However, the removal process often involves the creation and / or presence of debris, which can affect the yield of the manufacturing process.
[0008] Furthermore, such methods may not be suitable for use in some applications and / or with some devices having particular topological features.
[0009] It would be beneficial to provide an improved mechanism for providing selective deposition of conductive coatings.
[0010] Examples of the present disclosure will now be described by reference to the following figures, in which identical reference numbers in different figures indicate identical elements and / or, in some non-limiting examples, similar and / or corresponding elements: [Brief explanation of the drawings]
[0011] [Figure 1] 1 is a cross-sectional side block diagram of an example electroluminescent device according to an example of the present disclosure. [Figure 2]2 is a cross-sectional view of an example backplane layer of the substrate of the device of FIG. 1 showing thin film transistors (TFTs) embodied in the backplane layer. [Figure 3] 3 is a circuit diagram of an example of circuitry such as may be provided by one or more of the TFTs shown in the backplane layer of FIG. 2. [Figure 4] FIG. 2 is a cross-sectional view of the device of FIG. 1. [Figure 5] 2 is a cross-sectional view of an example version of the device of FIG. 1 showing an example of at least one pixel-defining layer (PDL) that supports the deposition of at least one second electrode of the device. [Figure 6] 1 is an example of an energy profile showing the relative energy states of adatoms absorbed on a surface, according to an example of the present disclosure. [Figure 7] 2 is a schematic diagram illustrating an example process for depositing a selective coating in a pattern onto an exposed layer surface of a base material of an example version of the device of FIG. 1 according to an example of the present disclosure. [Figure 8] FIG. 8 is a schematic diagram illustrating an example of a process for depositing a conductive coating in a first pattern on an exposed layer surface including the selective coating deposition pattern of FIG. 7, where the selective coating is a nucleation inhibiting coating (NIC). [Figure 9A] 9 is a schematic diagram illustrating an example of an open mask suitable for use in the process of FIG. 7, having apertures therein, according to an example of the present disclosure. [Figure 9B] 9 is a schematic diagram illustrating an example of an open mask suitable for use in the process of FIG. 7, having apertures therein, according to an example of the present disclosure. [Figure 9C] 9 is a schematic diagram illustrating an example of an open mask suitable for use in the process of FIG. 7, having apertures therein, according to an example of the present disclosure. [Figure 9D] 9 is a schematic diagram illustrating an example of an open mask suitable for use in the process of FIG. 7, having apertures therein, according to an example of the present disclosure. [Figure 10]2 is an example of a version of the device of FIG. 1 with an example of an additional deposition step, according to an example of the present disclosure. [Figure 11A] 10 is a schematic diagram illustrating an example of a process for depositing a selective coating that is a nucleation promoting coating (NPC) in a pattern on an exposed layer surface, including the selective coating deposition pattern of FIG. 9. [Figure 11B] 11B is a schematic diagram illustrating an example of a process for depositing a conductive coating in a pattern on an exposed layer surface, including the deposited pattern of the NPC of FIG. 11A. [Figure 12A] 2A-2C are schematic diagrams illustrating an example process for depositing NPCs in a pattern onto an exposed layer surface of a base material of an example version of the device of FIG. 1, according to an example of the present disclosure. [Figure 12B] 12B is a schematic diagram illustrating an example of a process for depositing NIC in a pattern onto an exposed layer surface containing the NPC deposition pattern of FIG. 12A. [Figure 12C] 12C is a schematic diagram illustrating an example of a process for depositing a conductive coating in a pattern on an exposed layer surface, including the deposited pattern of NIC of FIG. 12B. [Figures 13A-13C] 2A-2C are schematic diagrams illustrating example stages of an example printing process for depositing a selective coating in a pattern onto an exposed layer surface in an example version of the device of FIG. 1 , according to an example of the present disclosure. [Figure 14] 2 is a schematic diagram illustrating, in plan view, an example of a patterned electrode suitable for use in a version of the device of FIG. 1, according to an example of the present disclosure. [Figure 15] FIG. 15 is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 14 taken along line 15-15. [Figure 16A] 2A-2C are schematic diagrams illustrating, in plan view, several example patterns of electrodes suitable for use in example versions of the device of FIG. 1, according to examples of the present disclosure. [Figure 16B] 16B is a schematic diagram showing an example of a cross-sectional view of the device of FIG. 16A at an intermediate stage taken along line 16B-16B. [Figure 16C] FIG. 16C is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 16A taken along line 16C-16C. [Figure 17] FIG. 2 is a schematic diagram showing a cross-sectional view of an example version of the device of FIG. 1 with an example patterned auxiliary electrode, according to an example of the present disclosure. [Figure 18A] 2A-2C are schematic diagrams illustrating, in plan view, example arrangements of emissive and / or non-emissive regions in example versions of the device of FIG. 1, according to examples of the present disclosure. [Figure 18B] 18B are schematic diagrams illustrating segments of a portion of FIG. 18A, each showing an example of an auxiliary electrode overlapping a non-emissive region, according to an example of the present disclosure. [Figure 18C] 18B are schematic diagrams illustrating segments of a portion of FIG. 18A, each showing an example of an auxiliary electrode overlapping a non-emissive region, according to an example of the present disclosure. [Figure 18D] 18B are schematic diagrams illustrating segments of a portion of FIG. 18A, each showing an example of an auxiliary electrode overlapping a non-emissive region, according to an example of the present disclosure. [Figure 19] 1A-1C are schematic diagrams illustrating, in plan view, example patterns of auxiliary electrodes overlapping at least one emissive region and at least one non-emissive region, according to examples of the present disclosure. [Figure 20A] 2 is a schematic diagram illustrating, in plan view, an example pattern for an example version of the device of FIG. 1 having multiple groups of diamond-configured light-emitting regions, according to an example of the present disclosure. [Figure 20B] FIG. 20B is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 20A taken along line 20B-20B. [Figure 20C] FIG. 20C is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 20A taken along line 20C-20C. [Figure 21] 5 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 4 with an example additional deposition step, according to an example of the present disclosure. [Figure 22] 5 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 4 with an example additional deposition step, according to an example of the present disclosure. [Figure 23] 5 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 4 with an example additional deposition step, according to an example of the present disclosure. [Figure 24]5 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 4 with an example additional deposition step, according to an example of the present disclosure. [Figures 25A-25C] 2A-2C are schematic diagrams illustrating example stages of an example process for depositing a conductive coating in a pattern on an exposed layer surface of an example version of the device of FIG. 1 by a selective deposition and subsequent removal process, according to an example of the present disclosure. [Figure 26A] 2 is a schematic diagram illustrating, in plan view, an example of a transparent version of the device of FIG. 1 including at least one example pixel region having at least one auxiliary electrode and at least one example light-transmitting region, according to an example of the present disclosure. [Figure 26B] FIG. 26B is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 26A taken along line 26B-26B. [Figure 27A] 2 is a schematic diagram illustrating, in plan view, an example of a transparent version of the device of FIG. 1 including at least one example pixel region and at least one example light-transmitting region, according to an example of the present disclosure. [Figure 27B] FIG. 27B is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 27A taken along line 27B-27B. [Figure 27C] FIG. 27B is a schematic diagram illustrating an example cross-sectional view of the device of FIG. 27A taken along line 27B-27B. [Figure 28A] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 that provides a light-emitting region with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 28B] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 that provides a light-emitting region with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 28C] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 that provides a light-emitting region with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 28D]2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 that provides a light-emitting region with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 29A] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 having subpixel regions with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 29B] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 having subpixel regions with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 29C] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 having subpixel regions with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 29D] 2A-2C are schematic diagrams illustrating example stages of an example process for fabricating an example version of the device of FIG. 1 having subpixel regions with second electrodes of different thicknesses, according to examples of the present disclosure. [Figure 30] 2 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 1 in which the second electrode is coupled to an auxiliary electrode, according to an example of the present disclosure. [Figure 31A] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31B] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31C] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31D] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31E]2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31F] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31G] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31H] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 31I] 2A-2C are schematic diagrams illustrating various potential behaviors of NIC at the deposition interface with a conductive coating for example versions of the device of FIG. 1, according to various examples of the present disclosure. [Figure 32] 2 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 1 having a partition and a protected area, such as a recess, in a non-light-emitting area of the device, according to an example of the present disclosure. [Figure 33A] FIG. 2 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 1 having partitions and protected areas, such as recesses, in non-emissive regions prior to deposition of a semiconducting layer on the device, according to an example of the present disclosure. [Figure 33B] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33C] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33D] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33E] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33F] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33G] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33H] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33I] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33J] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33K] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33L] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33M] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33N] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33O] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 33P] 33B is a schematic diagram showing various examples of interactions between the partition of FIG. 33A after deposition of a semiconductive layer and a NIC with a second electrode and a conductive coating deposited thereon, according to various examples of the present disclosure. [Figure 34A] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 34B] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 34C] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 34D] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 34E] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 34F] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 34G] 33B is a schematic diagram illustrating various examples of auxiliary electrodes in the device of FIG. 33A according to various examples of the present disclosure. [Figure 35A] 2 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 1 having a partition in the non-emitting area and a protected area such as an aperture, according to various examples of the present disclosure. [Figure 35B]2 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 1 having a partition in the non-emitting area and a protected area such as an aperture, according to various examples of the present disclosure. [Figure 36] FIG. 1 is a schematic diagram illustrating the formation of membrane nuclei, according to an example of the present disclosure. DETAILED DESCRIPTION OF THE INVENTION
[0012] In this disclosure, for purposes of explanation and not limitation, specific details are set forth to provide a thorough understanding of the disclosure, including but not limited to particular architectures, interfaces, and / or techniques. In some instances, detailed descriptions of well-known systems, techniques, components, devices, circuits, methods, and applications are omitted so as not to obscure the description of the disclosure with unnecessary detail.
[0013] Moreover, it will be understood that the block diagrams reproduced herein may represent conceptual views of illustrative components embodying principles of the technology.
[0014] Accordingly, the components of the systems and methods are suitably represented by conventional symbols in the drawings, and only those specific details relevant to understanding the examples of the disclosure are shown, so as not to obscure the disclosure with details that will be readily apparent to those skilled in the art having the benefit of the description herein.
[0015] Any drawings provided herein are not drawn to scale and are not to be construed as limiting the present disclosure in any way.
[0016] Any features or acts shown in dashed outline may be considered optional in some instances. (Summary of the Invention)
[0017] It is an object of the present disclosure to obviate or mitigate at least one disadvantage of the prior art.
[0018] The present disclosure discloses, in lateral aspect, an optoelectronic device having a plurality of layers including a first portion and a second portion, wherein in the first portion, the device includes a nucleation inhibiting coating (NIC) disposed on a surface of the first layer.
[0019] In the second portion, a conductive coating is disposed on the second layer surface.
[0020] The initial adhesion probability for forming a conductive coating on the surface of the NIC in the first portion is substantially lower than the initial adhesion probability for forming a conductive coating on the surface of the second layer in the second portion. Thus, in some embodiments, the first portion is substantially free of the conductive coating.
[0021] According to a broad aspect of the present disclosure, there is provided an optoelectronic device having multiple layers, comprising: a nucleation-inhibiting coating (NIC) disposed on a surface of a first layer within a first portion of a lateral side of the device; and a conductive coating disposed on a surface of a second layer within a second portion of the lateral side of the device, wherein the surface of the NIC within the first portion is substantially free of the conductive coating, and wherein the NIC comprises a compound of formula (I), (II), (III), (IV), (V), (VI), (VII), (VIII), (IX), (X), (XI), (XII), (XIII), (XIV), (XV), (XVI), (XVII), (XVIII), (XIX), and / or (XX); [Table 2-1] [Table 2-2] During the ceremony, L 1 However, independently, C, CR 2 , C.R. 2 R 3 , N, NR 3, S, O, a substituted or unsubstituted cycloalkylene group having 3 to 6 carbon atoms, a substituted or unsubstituted arylene group having 5 to 60 carbon atoms, or a substituted or unsubstituted heteroarylene group having 4 to 60 carbon atoms; Ar 1 each independently represents a substituted or unsubstituted aryl group having 5 to 60 carbon atoms, a substituted or unsubstituted haloaryl group having 5 to 60 carbon atoms, or a substituted or unsubstituted heteroaryl group having 4 to 60 carbon atoms; R 1 , R 2 , and R 3 are independently H, D (deuterium), F, Cl, alkyl including C1 to C6 alkyl, cycloalkyl including C3 to C6 cycloalkyl, alkoxy including C1 to C6 alkoxy, fluoroalkyl, haloaryl, heteroaryl, haloalkoxy, fluoroaryl, fluoroalkoxy, fluoroalkylsulfanyl, fluoromethyl, difluoromethyl, trifluoromethyl, difluoromethoxy, trifluoromethoxy, fluoroethyl, polyfluoroethyl, 4-fluorophenyl, 3,4,5-trifluorophenyl, polyfluoroaryl, 4-(trifluoromethoxy)phenyl, SF4Cl, SF5, (CF2) a SF5, (O(CF2) b ) d CF3, (CF2) e (O(CF2) b ) d )CF3, or trifluoromethylsulfanyl; Z independently represents F or Cl; s represents an integer of 0 to 4, and the sum of r and s is 5; r represents an integer of 1 to 3; p represents an integer of 0 to 6; q represents an integer of 1 to 8; v represents an integer of 2 to 4; j represents an integer of 1 to 3; k represents an integer of 1 to 4; t represents an integer of 2 to 6; u represents an integer of 0 to 2, and the sum of r and u is 3; h represents an integer of 0 to 4, and the sum of r and h is 4; i represents an integer of 1 to 4; a represents an integer of 2 to 6; b represents an integer of 1 to 4; d represents an integer of 1 to 3; An optoelectronic device is disclosed wherein e represents an integer from 1 to 4.
[0022] The examples are described above in conjunction with the aspects of the present disclosure in which they may be implemented. Those skilled in the art will understand that the examples may be implemented in conjunction with the aspect for which they are described, but may also be implemented with other examples of that aspect or another aspect. When the examples are mutually exclusive or otherwise incompatible with each other, it will be apparent to those skilled in the art. Some examples may be described in relation to one aspect, but may also be applicable to other aspects, as will be apparent to those skilled in the art.
[0023] Some embodiments or examples of the present disclosure include an optoelectronic device having a first portion of a lateral side of the optoelectronic device including a nucleation inhibiting coating (NIC) on a first layer surface of the optoelectronic device, and a second portion having a conductive coating on a second layer surface of the optoelectronic device, wherein an initial adhesion probability for forming the conductive coating on the surface of the NIC in the first portion is substantially lower than an initial adhesion probability for forming the conductive coating on the second layer surface in the second portion, such that the first portion is substantially free of the conductive coating.
[0024] explanation optoelectronic devices FIELD OF THE DISCLOSURE This disclosure relates generally to electronic devices, and more particularly to optoelectronic devices. Optoelectronic devices generally encompass any device that converts electrical signals into photons and vice versa.
[0025] In this disclosure, the terms "photon" and "light" may be used interchangeably to refer to similar concepts. In this disclosure, photons may have wavelengths that lie in the infrared (IR) and / or ultraviolet (UV) regions of the visible light spectrum.
[0026] An organic optoelectronic device can include any optoelectronic device in which one or more active layers and / or layers of the device are formed primarily from organic (carbon-containing) materials, and more specifically, organic conductive materials.
[0027] Those skilled in the art will understand that, in the present disclosure, organic materials may include, but are not limited to, a wide variety of organic molecules and / or organic polymers. Furthermore, those skilled in the art will understand that organic materials doped with various inorganic substances, including, but not limited to, elements and / or inorganic compounds, may still be considered organic materials. Those skilled in the art will further understand that a variety of organic materials may still be used, and that the processes described herein are generally applicable to the full range of such organic materials.
[0028] In the present disclosure, inorganic material may refer to a material that primarily comprises inorganic materials. In the present disclosure, inorganic material may include any material that is not considered to be an organic material, including, but not limited to, metals, glasses, and / or minerals.
[0029] If an optoelectronic device emits photons through a luminescent process, the device can be considered an electroluminescent device. In some non-limiting examples, the electroluminescent device can be an organic light-emitting diode (OLED) device. In some non-limiting examples, the electroluminescent device can be part of an electronic device. As a non-limiting example, the electroluminescent device can be an OLED lighting panel or module, and / or an OLED display or module of a computing device such as a smartphone, tablet, laptop, e-reader, and / or some other electronic device such as a monitor and / or television.
[0030] In some non-limiting examples, the optoelectronic device can be an organic photovoltaic (OPV) device that converts photons into electricity. In some non-limiting examples, the optoelectronic device can be an electroluminescent quantum dot device. In this disclosure, unless otherwise stated, reference will be made specifically to OLED devices, with the understanding that such disclosure may be equally applicable to other optoelectronic devices, including, but not limited to, OPV and / or quantum dot devices, in a manner apparent to those skilled in the art.
[0031] The structure of such devices is described from each of two sides: from a cross-sectional side and / or from a lateral (plan view) side.
[0032] In this disclosure, the terms "layer" and "layer portion" may be used interchangeably to refer to similar concepts.
[0033] In the context of introducing the cross-sectional views below, components of such devices are depicted with substantially planar lateral layers. Those skilled in the art will understand that such substantially planar representations are for illustrative purposes only and encompass the lateral extent of such devices, and that in some non-limiting examples there may be localized substantially flat layers of different thicknesses and dimensions, including a substantially complete absence of layers, and / or layers separated by non-planar transition regions (including lateral gaps and discontinuities). Thus, for illustrative purposes, while devices are depicted below in their cross-sectional views as substantially layered structures, in the planar view embodiments discussed below, such devices may exhibit a variety of topographies for defining features, each of which may substantially exhibit the layered profile described in the cross-sectional view.
[0034] cross section side 1 is a simplified block diagram of a cross-sectional side view of an example electroluminescent device according to the present disclosure. Generally, the electroluminescent device, designated 100, includes a substrate 110 on which is disposed a front plane 10 including multiple layers, each of which includes a first electrode 120, at least one semiconductive layer 130, and a second electrode 140. In some non-limiting examples, the front plane 10 may provide a mechanism for photon emission and / or manipulation of emitted photons. In some non-limiting examples, a barrier coating 1650 (FIG. 16C) may be provided to surround and / or encapsulate the layers 120, 130, 140, and / or the substrate 110 disposed thereon.
[0035] For illustrative purposes, the exposed layer surface of the base material is referred to as 111. In Figure 1, exposed layer surface 111 is shown as being that of second electrode 140. Those skilled in the art will understand that, as a non-limiting example, upon deposition of first electrode 120, exposed layer surface 111 is shown as 111a of substrate 110.
[0036] Those skilled in the art will understand that when a component, layer, region and / or portion thereof is referred to as being "formed," "disposed," and / or "deposited" on another base material, component, layer, region and / or portion, such forming, disposing, and / or depositing may be directly on the exposed layer surface 111 of such base material, component, layer, region and / or portion (at the time of such forming, disposing, and / or depositing), and / or indirectly, with the possibility of intervening materials, components, layers, regions, and / or portions therebetween.
[0037] In accordance with directional conventions in this disclosure, substrate 110 is considered to be the "bottom surface" of device 100, extending substantially perpendicular to the aforementioned lateral aspects on which layers 120, 130, 140 are disposed on the "top surface" of substrate 11. In accordance with such convention, second electrode 140 is on the top surface of device 100 as shown, even if substrate 110 is physically inverted such that the top surface on which one of layers 120, 130, 140, such as, but not limited to, first electrode 120, is to be disposed is physically below substrate 110 to allow deposition material (not shown) to migrate upward and deposit as a thin film on its top surface (as may be the case in some instances, including but not limited to, during a manufacturing process, where one or more layers 120, 130, 140 may be introduced by a vapor deposition process).
[0038] In some non-limiting examples, device 100 may be electrically coupled to a power source 15. When so coupled, device 100 may emit photons as described herein.
[0039] In some non-limiting examples, device 100 can be classified according to the emission direction of photons generated therefrom. In some non-limiting examples, device 100 may be considered a bottom-emitting device if the generated photons are emitted toward and through substrate 110 on the bottom surface of device 100 and away from layers 120, 130, 140 disposed on the top surface of substrate 110. In some non-limiting examples, device 100 may be considered a top-emitting device if the photons are emitted away from substrate 110 on the bottom surface of device 100 and toward and / or through top layer 140 disposed on the top surface of substrate 110 along with intermediate layers 120, 130. In some non-limiting examples, device 100 may be considered a dual-sided light-emitting device if it is configured to emit photons from both the bottom surface (toward and through substrate 110) and the top surface (toward and through top layer 140).
[0040] Thin film formation The front plane 10 layers 120, 130, 140 can be sequentially disposed on a target exposed layer surface 111 (and / or in some non-limiting examples, including but not limited to, at least one target area and / or portion of such surface, in the case of selective deposition as disclosed herein) of a base material, which in some non-limiting examples can sometimes be a substrate 110 and intervening underlayers 120, 130, 140 as thin films. In some non-limiting examples, the electrodes 120, 140, 1750, 4150 can be formed from at least one thin film conductive layer of a conductive coating 830 (FIG. 8).
[0041] The thicknesses of each layer, including but not limited to layers 120, 130, 140, and substrate 110 shown in FIG. 1 and throughout the figures are for illustrative purposes only and do not necessarily represent thicknesses relative to other layers 120, 130, 140 (and / or substrate 110).
[0042] The formation of a thin film during deposition onto an exposed layer surface 111 of a base material involves a process of nucleation and growth. During the initial stages of film formation, a sufficient number of vapor monomers (which may be molecules and / or atoms, in some non-limiting examples) typically condense from the gas phase to form initial nuclei on the presented surface 111, whether that be the substrate 110 (or an intervening underlayer 120, 130, 140). As the vapor monomers continue to impinge on such surfaces, the size and density of these initial nuclei increase, forming small clusters or islands. After the island density is saturated, neighboring islands generally begin to coalesce, increasing the average island size while decreasing the island density. The coalescence of neighboring islands can continue until a substantially closed film is formed.
[0043] There are at least three basic growth modes that can occur in thin films: 1) island (Volmer-Weber), 2) layer-by-layer (Frank-van der Merwe), and 3) Stranski-Krastanov. Island growth typically occurs when stable clusters of monomers nucleate at the surface and grow to form discrete islands. This growth mode occurs when the interactions between monomers are stronger than the interactions between the monomers and the surface.
[0044] The nucleation rate describes how many nuclei of a given size (when free energy does not push clusters of such nuclei to grow or shrink) ("critical nuclei") will form on a surface per unit time. During the early stages of film formation, the density of nuclei is low, which causes nuclei to cover a relatively small portion of the surface (e.g., there are large gaps / spaces between adjacent nuclei), making it unlikely that nuclei will grow from direct collisions of monomers with the surface. Therefore, the rate at which critical nuclei grow typically depends on the rate at which adatoms (e.g., adsorbed monomers) on the surface can migrate and attach to nearby nuclei.
[0045] After an adatom adsorbs on a surface, it can either desorb from the surface or move for some time on the surface before desorbing and interacting with other adatoms to form small clusters or attaching to growing nuclei. The average time an adatom remains on the surface after initial adsorption is given by
number
[0046] In the above equation, ν is the vibrational frequency of the adatoms on the surface, k is the Boltzmann constant, T is the temperature, and E des 631 (Figure 6) is the energy required to desorb an adatom from the surface. From this equation, E des The lower the value of 631, the easier it is for adatoms to desorb from the surface, and therefore the shorter the time they remain on the surface. The average distance an adatom can diffuse is given by:
number
[0047] During the initial stages of film formation, the adsorbed adatoms can interact to form clusters, and the critical concentration of clusters per unit area is given by
number
number
number
[0048] The critical monomer supply rate for growing clusters is given by the rate of vapor collisions and the average area over which adatoms can diffuse before desorbing.
number
[0049] The critical nucleation rate is therefore given by the combination of the above equations.
number
[0050] From the above equation, it can be seen that the critical nucleation rate is suppressed on surfaces with low desorption energies of adsorbed adatoms, high activation energies for adatom diffusion, high temperatures, and / or surfaces subject to vapor impingement rates.
[0051] Sites of substrate heterogeneity, such as defects, ledges, or step edges, are identified by E des 631, which may increase the density of nuclei observed at such sites. Impurities or surface contamination may also increase E des 631 and may increase nucleation density. For deposition processes performed under high vacuum conditions, the type and density of surface contaminants are influenced by the vacuum pressure and the composition of the residual gases that make up that pressure.
[0052] Under high vacuum conditions, the flux of molecules impinging on the surface (cm 2-per sec) is given as follows:
number
[0053] Although this disclosure discusses thin film formation with reference to at least one layer or coating in terms of vapor deposition, those skilled in the art will understand that, in some non-limiting examples, various components of electroluminescent device 100 may be selectively deposited using a wide variety of techniques, including, but not limited to, evaporation (including but not limited to thermal evaporation and / or electron beam evaporation), photolithography, printing (including but not limited to inkjet and / or vapor jet printing, reel-to-reel printing, and / or microcontact transfer printing), physical vapor deposition (PVD) (including but not limited to sputtering), chemical vapor deposition (CVD) (including but not limited to plasma-enhanced CVD (PECVD) and / or organic vapor phase deposition (OVPD)), laser annealing, laser-induced thermal imaging (LITI) patterning, atomic layer deposition (ALD), coating (including but not limited to spin coating, dip coating, line coating, and / or spray coating), and / or combinations of any two or more thereof. Some processes may be used in combination with a shadow mask, which may be an open mask and / or a fine metal mask (FMM) in some non-limiting examples, during the deposition of any of the various layers and / or coatings to achieve various patterns by covering and / or eliminating the deposition of the deposited material onto certain portions of the surface of the base material that are exposed to the surface.
[0054] In this disclosure, the terms “evaporation” and / or “sublimation” may be used interchangeably to generally refer to a deposition process in which a source material is converted, including but not limited to, by heating, into a vapor and deposited on a target surface in a solid state, including but not limited to. As will be appreciated, evaporation is a type of PVD process in which one or more source materials are evaporated and / or sublimated in a low-pressure (including but not limited to vacuum) environment, and then deposited on a target surface by de-sublimation of the evaporated source material(s). Those skilled in the art will appreciate that a variety of different evaporation sources are used to heat the source material, and thus, the source material may be heated in a variety of ways. As non-limiting examples, the source material may be heated by an electric filament, an electron beam, induction heating, and / or resistance heating. In some non-limiting examples, the source material may be loaded into a heated crucible, a heated boat, a Knudsen cell (which may be an effusion evaporation source), and / or any other type of evaporation source.
[0055] In some non-limiting examples, the deposition source material may be a mixture, in which at least one component of the mixture of deposition source materials may not be deposited (or, in some non-limiting examples, may be deposited in a relatively small amount compared to other components of such a mixture) during the deposition process.
[0056] In this disclosure, references to a layer thickness of a material refer to an amount of material deposited on the target exposed layer surface 111 that corresponds to an amount of material that coats the target surface with a uniformly thick layer of material having the referenced layer thickness, regardless of the mechanism of deposition. As a non-limiting example, depositing a layer thickness of 10 nanometers (nm) of material indicates that the amount of material deposited on the surface corresponds to the amount of material to form a uniformly thick layer of material that is 10 nm thick. With respect to the mechanisms by which thin films are formed discussed above, it will be understood that the actual thickness of the deposited material may be non-uniform due to, as a non-limiting example, possible stacking or clustering of monomers. As a non-limiting example, depositing a layer thickness of 10 nm may result in some portions of the deposited material having an actual thickness greater than 10 nm, or other portions of the deposited material having an actual thickness less than 10 nm. Thus, a particular layer thickness of a material deposited on a surface may correspond, in some non-limiting examples, to the average thickness of the deposited material across the target surface.
[0057] In this disclosure, references to reference layer thickness refer to a layer thickness of magnesium (Mg) deposited on a reference surface exhibiting a high initial sticking probability S (i.e., a surface having an initial sticking probability S of about 1 and / or close to 1.0). The reference layer thickness does not refer to the actual thickness of Mg deposited on a target surface (such as, but not limited to, the surface of a nucleation-inhibiting coating (NIC) 810 (FIG. 8)). Rather, the reference layer thickness refers to a layer thickness of Mg deposited on a reference surface, in some non-limiting examples, a surface of quartz positioned in a deposition chamber for monitoring deposition rate and reference layer thickness when the target surface and reference surface are exposed to the same Mg vapor flux for the same deposition duration. Those skilled in the art will understand that appropriate tooling factors may be used to determine and / or monitor the reference layer thickness when the target surface and reference surface are not exposed to the same vapor flux simultaneously during deposition.
[0058] In this disclosure, a reference to depositing a number X of monolayers of a material refers to depositing an amount of material to cover a desired area of the exposed layer surface 111 with X monolayers of the material's constituent monomers. In this disclosure, a reference to depositing a fraction 0.X of a monolayer of a material refers to depositing an amount of material to cover a fraction 0.X of the desired area of the surface with monolayers of the material's constituent monomers. Those skilled in the art will understand that, by way of non-limiting example, the actual local thickness of the deposited material across the desired area of the surface may be non-uniform due to possible stacking and / or clustering of the monomers. As a non-limiting example, depositing one monolayer of a material may result in some localized regions of the desired area of the surface not being covered by the material, while other localized regions of the desired area of the surface may have multiple atomic and / or molecular layers deposited thereon.
[0059] In the present disclosure, a target surface (and / or target region thereof) may be considered to be "substantially free of," "substantially free of," and / or "substantially uncoated by" a material if there is a substantial absence of material on the target surface as determined by any suitable determination mechanism.
[0060] In some non-limiting examples, one measure of the amount of material on a surface is the coverage of the surface by such material. In some non-limiting examples, surface coverage can be determined using various imaging techniques, including, but not limited to, transmission electron microscopy (TEM), atomic force microscopy (AFM), and / or scanning electron microscopy (SEM).
[0061] Conductive materials, including but not limited to metals, including but not limited to Mg in some non-limiting examples, attenuate and / or adsorb photons, so in some non-limiting examples, one measure of the amount of conductive material on a surface is (light) transmittance.
[0062] Thus, in some non-limiting examples, a surface of a material can be considered to be substantially free of conductive material if the light transmission through the surface of such material is greater than 90%, greater than 92%, greater than 95%, and / or greater than 98% of the transmission of a reference material of similar composition and dimensions of such material, in some non-limiting examples in the visible portion of the electromagnetic spectrum.
[0063] In this disclosure, for ease of illustration, details of the deposited materials, including but not limited to layer thickness profiles and / or edge profiles, are omitted. A variety of possible edge profiles at the interface between the NIC 810 and the conductive coating 830 are discussed herein.
[0064] substrate In some examples, the substrate 110 may comprise a base substrate 112. In some examples, the base substrate 112 may be formed from a material suitable for its use, including, but not limited to, inorganic materials, including, but not limited to, silicon (Si), glass, metal (including, but not limited to, metal foil), sapphire, and / or other inorganic materials, and / or organic materials, including, but not limited to, polymers, including, but not limited to, polyimides and / or silicon-based polymers. In some examples, the base substrate 112 may be rigid or flexible. In some examples, the substrate 112 may be defined by at least one planar surface. The substrate 110 has at least one surface that supports the remaining front plane 10 components of the device 100, including, but not limited to, the first electrode 120, at least one semiconductive layer 130, and / or the second electrode 140.
[0065] In some non-limiting examples, such surfaces can be organic and / or inorganic surfaces.
[0066] In some examples, the substrate 110 may include, in addition to the base substrate 112, one or more additional organic and / or inorganic layers (not shown or specifically described herein) supported on the exposed layer surface 111 of the base substrate 112.
[0067] In some non-limiting examples, such additional layers may include and / or form one or more organic layers, which may include, replace, and / or supplement one or more of the at least one semiconductive layer 130.
[0068] In some non-limiting examples, such additional layers may include one or more inorganic layers, which may include and / or form one or more electrodes, which may, in some non-limiting examples, include, replace, and / or supplement first electrode 120 and / or second electrode 140.
[0069] In some non-limiting examples, such additional layers may include and / or be formed from and / or as a backplane layer 20 (FIG. 2) of semiconductive material. In some non-limiting examples, backplane layer 20 contains power circuitry and / or switching elements for driving device 100, including, but not limited to, electronic TFT structures and / or components thereof 200 (FIG. 2), which may be formed by photolithographic processes that may not be provided under and / or precede the introduction of a low pressure (including, but not limited to, a vacuum) environment.
[0070] In the present disclosure, a semiconducting material can generally be described as a material that exhibits a band gap. In some non-limiting examples, the band gap can be formed between the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) of the semiconducting material. Thus, a semiconducting material generally exhibits a lower conductivity than a conductive material (including, but not limited to, metals) but a higher conductivity than an insulating material (including, but not limited to, glass). In some non-limiting examples, the semiconducting material can include an organic semiconducting material. In some non-limiting examples, the semiconducting material can include an inorganic semiconducting material.
[0071] Backplane and TFT structure embodied therein FIG. 2 is a simplified cross-sectional view of an example substrate 110 of device 100, including its backplane layer 20. In some non-limiting examples, the backplane 20 of substrate 110 may include one or more electronic and / or optoelectronic components, including, but not limited to, transistors, resistors, and / or capacitors, capable of supporting device 100 operating as an active matrix and / or passive matrix device. In some non-limiting examples, such a structure may be a thin film transistor (TFT) structure, such as that shown at 200. In some non-limiting examples, TFT structure 200 may be fabricated using organic and / or inorganic materials to form a portion of the backplane layer 20 of substrate 110 above various layers 210, 220, 230, 240, 250, 270, 280, and / or base substrate 112. In FIG. 2, the TFT structure 200 shown is a top-gate TFT. In some non-limiting examples, TFT technology and / or structures, including but not limited to one or more of layers 210, 220, 230, 240, 250, 270, 270, 280, may be employed to implement non-transistor components, including but not limited to resistors and / or capacitors.
[0072] In some non-limiting examples, the backplane 20 may include a buffer layer 210 deposited on the exposed layer surface 111 of the base substrate 112 to support components of the TFT structure 200. In some non-limiting examples, the TFT structure 200 may include a semiconductive active region 220, a gate insulating layer 230, a TFT gate electrode 240, an interlayer insulating layer 250, a TFT source electrode 260, a TFT drain electrode 270, and / or a TFT insulating layer 280. In some non-limiting examples, the semiconductive active region 220 is formed on a portion of the buffer layer 210, and the gate insulating layer 230 is deposited to substantially cover the semiconductive active region 220. In some non-limiting examples, the gate electrode 240 is formed on top of the gate insulating layer 230, and the interlayer insulating layer 250 is deposited thereon. The TFT source electrode 270 and the TFT drain electrode 270 are formed such that they extend through openings formed through both the interlayer insulating layer 250 and the gate insulating layer 230 so that they are electrically coupled to the semiconductor active area 220. A TFT insulating layer 280 is then formed over the TFT structure 200.
[0073] In some non-limiting examples, one or more of the layers 210, 220, 230, 240, 250, 270, 270, 280 of the backplane 20 can be patterned using photolithography, using a photomask to expose selected portions of the photoresist covering the underlying device layer to UV light. Depending on the type of photoresist used, the exposed or unexposed portions of the photomask can then be removed to expose desired portions of the underlying device layer. In some examples, the photoresist is a positive-tone photoresist, where the selected portions exposed to UV light are subsequently substantially irremovable, while the remaining portions not so exposed are subsequently removable. In some non-limiting examples, the photoresist is a negative-tone photoresist, where the selected portions exposed to UV light are subsequently substantially removable, while the remaining portions not so exposed are subsequently substantially irremovable. Thus, the patterned surface can be etched, including but not limited to chemically and / or physically, and / or washed away and / or rinsed away to effectively remove exposed portions of such layers 210, 220, 230, 240, 250, 260, 270, 280.
[0074] Furthermore, although a top-gate TFT structure 200 is shown in FIG. 2, those skilled in the art will understand that other TFT structures, including but not limited to bottom-gate TFT structures, may be formed within backplane 20 without departing from the scope of the present disclosure.
[0075] In some non-limiting examples, the TFT structure 200 may be an n-type TFT and / or a p-type TFT. In some non-limiting examples, the TFT structure 200 may incorporate any one or more of amorphous Si (a-Si), indium gallium zinc (Zn) oxide (IGZO), and / or low temperature polycrystalline Si (LTPS).
[0076] First electrode A first electrode 120 is deposited on the substrate 110. In some non-limiting examples, the first electrode 120 is electrically coupled to a terminal of a power source 15 and / or to ground. In some non-limiting examples, the first electrode 120 is so coupled through at least one drive circuit 300 ( FIG. 3 ), which in some non-limiting examples may incorporate at least one TFT structure 200 in a backplane 20 of the substrate 110.
[0077] In some non-limiting examples, the first electrode 120 can include an anode 341 (FIG. 3) and / or a cathode 342 (FIG. 3). In some non-limiting examples, the first electrode 120 is an anode 341.
[0078] In some non-limiting examples, the first electrode 120 may be formed by depositing at least one conductive thin film on (a portion of) the substrate 110. In some non-limiting examples, there may be multiple first electrodes 120 arranged in a spatial arrangement on the lateral sides of the substrate 110. In some non-limiting examples, one or more of such at least one first electrode 120 may be deposited on (a portion of) the TFT insulating layer 280 arranged in a spatial arrangement on the lateral sides. If so, in some non-limiting examples, at least one of such at least one first electrode 120 may extend through an opening in the corresponding TFT insulating layer 280 and be electrically coupled to an electrode 240, 260, 270 of the TFT structure 200 in the backplane 20, as shown in FIG. 4 . In FIG. 4 , a portion of the at least one first electrode 120 is shown coupled to a TFT drain electrode 270.
[0079] In some non-limiting examples, the at least one first electrode 120 and / or at least one thin film thereof may comprise one or more of various materials, including but not limited to one or more metallic materials, including but not limited to Mg, aluminum (Al), calcium (Ca), Zn, silver (Ag), cadmium (Cd), barium (Ba), and / or ytterbium (Yb), and / or combinations of any two or more thereof, including but not limited to alloys containing any of such materials, one or more oxides, including but not limited to transparent conductive oxides (TCOs), including but not limited to ternary compositions such as fluorine tin oxide (FTO), indium zinc oxide (IZO), and / or indium tin oxide (ITO), and / or combinations of any two or more thereof and / or in various ratios and / or combinations of any two or more thereof within at least one layer, including but not limited to, any one or more of which may be a thin film.
[0080] In some non-limiting examples, the conductive thin film comprising the first electrode 120 may be selectively deposited, deposited, and / or processed using a variety of techniques, including, but not limited to, evaporation (including, but not limited to, thermal evaporation and / or electron beam evaporation), photolithography, printing (including, but not limited to, inkjet and / or evaporative jet printing, reel-to-reel printing, and / or microcontact transfer printing), PVD (including, but not limited to, sputtering), CVD (including, but not limited to, PECVD and / or OVPD), laser annealing, LTI patterning, ALD, coating (including, but not limited to, spin coating, dip coating, line coating, and / or spray coating), and / or a combination of any two or more thereof.
[0081] Second electrode A second electrode 140 is deposited on the at least one semiconductive layer 130. In some non-limiting examples, the second electrode 140 is electrically coupled to a terminal of a power source 15 and / or to ground. In some non-limiting examples, the second electrode 140 is so coupled through at least one drive circuit 300, which in some non-limiting examples may incorporate at least one TFT structure 200 in the backplane 20 of the substrate 110.
[0082] In some non-limiting examples, the second electrode 140 can include an anode 341 and / or a cathode 342. In some non-limiting examples, the second electrode 130 is a cathode 342.
[0083] In some non-limiting examples, the second electrode 140 can be formed by depositing a conductive coating 830, in some non-limiting examples as at least one thin film on (a portion of) the at least one semiconductive layer 130. In some non-limiting examples, there can be multiple second electrodes 140 arranged in a spatial arrangement on lateral sides of the at least one semiconductive layer 130.
[0084] In some non-limiting examples, the at least one second electrode 140 may comprise a variety of materials, including, but not limited to, one or more metallic materials, including, but not limited to, Mg, Al, Ca, Zn, Ag, Cd, Ba, and / or Yb, and / or combinations of any two or more thereof, including, but not limited to, alloys containing any of such materials; one or more oxides, including, but not limited to, TCOs, including, but not limited to, ternary compositions such as FTO, IZO, and / or ITO; and / or combinations of any two or more thereof and / or in various ratios; and / or other oxides containing zinc oxide (ZnO) and / or indium (In) and / or Zn in at least one layer; and / or combinations of any two or more thereof; and / or one or more non-metallic materials, any one or more of which may be conductive thin films. In some non-limiting examples, for Mg:Ag alloys, the composition of such alloys may range from about 1:9 to about 9:1 by volume.
[0085] In some non-limiting examples, the conductive thin film comprising the second electrode 140 may be selectively applied, deposited, and / or processed using a variety of techniques, including, but not limited to, evaporation (including, but not limited to, thermal evaporation and / or electron beam evaporation), photolithography, printing (including, but not limited to, inkjet and / or evaporative jet printing, reel-to-reel printing, and / or microcontact transfer printing), PVD (including, but not limited to, sputtering), CVD (including, but not limited to, PECVD and / or OVPD), laser annealing, LTI patterning, ALD, coating (including, but not limited to, spin coating, dip coating, line coating, and / or spray coating), and / or a combination of any two or more thereof.
[0086] In some non-limiting examples, deposition of the second electrode 140 can be performed using an open mask and / or a mask-free deposition process.
[0087] In some non-limiting examples, second electrode 140 can include multiple such layers and / or coatings, which, in some non-limiting examples, may be separate layers and / or coatings disposed on top of each other.
[0088] In some non-limiting examples, the second electrode 140 may comprise a Yb / Ag bilayer coating. By way of non-limiting example, such a bilayer coating may be formed by depositing a Yb coating followed by an Ag coating. The thickness of such an Ag coating may be greater than the thickness of the Yb coating.
[0089] In some non-limiting examples, the second electrode 140 can be a multi-layer electrode 140 including at least one metal layer and / or at least one oxide layer.
[0090] In some non-limiting examples, the second electrode 140 may comprise fullerenes and magnesium.
[0091] In this disclosure, the term "fullerene" may generally refer to a material comprising carbon molecules. Non-limiting examples of fullerene molecules include carbon cage molecules that include, but are not limited to, a three-dimensional framework comprising a large number of carbon atoms, which form a closed shell and may be, but are not limited to, spherical and / or hemispherical in shape. In some non-limiting examples, fullerene molecules are C n where n is an integer corresponding to the number of carbon atoms contained within the carbon skeleton of the fullerene molecule. Non-limiting examples of fullerene molecules include C n where n is C 70 , C 70 , C 72 , C 74 , C 76 , C78 , C 80 , C 82 , and C 84 and the like, but not limited to, in the range of 50 to 250. Further non-limiting examples of fullerene molecules include tubular and / or cylindrical shaped carbon molecules, including, but not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes.
[0092] As a non-limiting example, such a coating can be formed by depositing a fullerene coating followed by a Mg coating. In some non-limiting examples, fullerenes can be dispersed within the Mg coating to form a fullerene-containing Mg alloy coating. Non-limiting examples of such coatings are described in U.S. Patent Application Publication No. 2015 / 0287846 (published October 8, 2015) and PCT International Application No. PCT / IB2017 / 054970 (filed August 15, 2017, published February 22, 2018 as WO2018 / 033860).
[0093] Drive circuit In the present disclosure, the concept of sub-pixels 2641-2643 (FIG. 26) may be referred to herein as sub-pixel 264x, for ease of explanation only. Similarly, in the present disclosure, the concept of pixel 340 (FIG. 3) may be considered in conjunction with the concept of at least one sub-pixel 264x thereof. For ease of explanation only, such combined concept will be referred to herein as "(sub)pixel 340 / 264x," and such terminology will be understood to imply either or both of pixel 340 and / or its at least one sub-pixel 264x, unless the context dictates otherwise.
[0094] 3 is a circuit diagram of an example of a drive circuit such as may be provided by one or more of the TFT structures 200 shown in backplane 20. In the example shown, the circuit, generally designated 300, is for supplying current to first electrode 120 and second electrode 140 and for example a drive circuit for active-matrix OLED (AMOLED) device 100 (and / or its (sub)pixels 340 / 264x) for controlling the emission of photons from device 100 (and / or (sub)pixels 340 / 264x). While the illustrated circuit 300 is shown incorporating multiple p-type top-gate thin-film TFT structures 200, circuit 300 could equally incorporate one or more p-type bottom-gate TFT structures 200, one or more n-type top-gate TFT structures 200, one or more n-type bottom-gate TFT structures 200, one or more other TFT structures 200, and / or any combination thereof, whether formed as one or more thin-film layers. The circuit 300 includes, in some non-limiting examples, a switching TFT 310, a driving TFT 320, and a storage capacitor 330.
[0095] The (sub)pixel 340 / 264x of the OLED display 100 is represented by a diode 340. The source 311 of the switching TFT 310 is coupled to a data (or, in some non-limiting examples, a column select) line 30. The gate 312 of the switching TFT 310 is coupled to a gate (or, in some non-limiting examples, a row select) line 31. The drain 313 of the switching TFT 310 is coupled to a gate 322 of the driving TFT 320.
[0096] The source 321 of the driving TFT 320 is coupled to the positive (or negative) terminal of the power supply 15. The (positive) terminal of the power supply 15 is represented by the electrical supply line (VDD) 32.
[0097] The drain 323 of the driving TFT 320 is coupled to the anode 341 (which in some non-limiting examples may be the first electrode 120) of the diode 340 (which represents the (sub)pixel 340 / 264x of the OLED display 100) such that the driving TFT 320 and the diode 340 (and / or the (sub)pixel 340 / 264x of the OLED display 100) are coupled in series between the electrical supply line (VDD) 32 and ground.
[0098] The cathode 342 (which in some non-limiting examples may be the second electrode 140) of the diode 340 (representing the (sub)pixel 340 / 264x of the OLED display 100) is represented as a resistor 350 in the circuit 300.
[0099] The storage capacitor 330 is coupled at its respective ends to the source 321 and gate 322 of the driving TFT 320. The driving TFT 320 limits the current passing through the diode 340 (representing the (sub)pixel 340 / 264x of the OLED display 100) according to the voltage of the charge stored in the storage capacitor 330, so that the diode 340 outputs the desired brightness. The voltage of the storage capacitor 330 is set by the switching TFT 310, which couples it to the data line 30.
[0100] In some non-limiting examples, compensation circuit 370 is provided to compensate for any deviations in transistor characteristics from variations in the manufacturing process and / or degradation of switching TFT 310 and / or driving TFT 320 over time.
[0101] Semiconductive layer In some non-limiting examples, the at least one semiconductive layer 130 can include multiple layers 131, 133, 135, 137, 139, any of which can be arranged in a thin film in a stacked configuration that can include, in some non-limiting examples, any one or more of a hole injection layer (HIL) 131, a hole transport layer (HTL) 133, an emissive layer (EL) 135, an electron transport layer (ETL) 137, and / or an electron injection layer (EIL) 139. In the present disclosure, the term "semiconductive layer" can be used interchangeably with "organic layer" because the layers 131, 133, 135, 137, 139 in the OLED device 100 can include organic semiconductive materials in some non-limiting examples.
[0102] In some non-limiting examples, at least one semiconducting layer 130 may form a "tandem" structure that includes multiple ELs 135. In some non-limiting examples, such a tandem structure may also include at least one charge generation layer (CGL).
[0103] In some non-limiting examples, thin films, including layers 131, 133, 135, 137, 139 in the stack that make up at least one semiconductive layer 130, may be selectively applied, deposited, and / or processed using a variety of techniques, including, but not limited to, evaporation (including, but not limited to, thermal evaporation and / or electron beam evaporation), photolithography, printing (including, but not limited to, inkjet and / or evaporative jet printing, reel-to-reel printing, and / or microcontact transfer printing), PVD (including, but not limited to, sputtering), CVD (including, but not limited to, PECVD and / or OVPD), laser annealing, LTI patterning, ALD, coating (including, but not limited to, spin coating, dip coating, line coating, and / or spray coating), and / or combinations of any two or more thereof.
[0104] Those skilled in the art will readily appreciate that the structure of device 100 can be modified by omitting and / or combining one or more of semiconducting layers 131, 133, 135, 137, 139.
[0105] Furthermore, any of the layers 131, 133, 135, 137, 139 of the at least one semiconducting layer 130 can include any number of sublayers. Furthermore, such layers 131, 133, 135, 137, 139, and / or any of their sublayers can include various mixtures and / or compositional gradients. Additionally, those skilled in the art will understand that the device 100 can include one or more layers containing inorganic and / or organometallic materials and is not necessarily limited to devices composed solely of organic materials. As a non-limiting example, the device 100 can include one or more quantum dots.
[0106] In some non-limiting examples, the HIL 131 can be formed using a hole-injecting material that can facilitate the injection of holes by the anode 341.
[0107] In some non-limiting examples, HTL 133 can be formed using a hole transport material that can exhibit high hole mobility in some non-limiting examples.
[0108] In some non-limiting examples, the ETL 137 can be formed using an electron transporting material that can exhibit high electron mobility in some non-limiting examples.
[0109] In some non-limiting examples, the EIL 139 can be formed using an electron injection material that can facilitate injection of electrons by the cathode 342 .
[0110] In some non-limiting examples, EL135 can be formed by doping a host material with at least one emitter material, which can be a fluorescent emitter, a phosphorescent emitter, a thermally activated delayed fluorescence (TADF) emitter, and / or any combination of two or more thereof, as non-limiting examples.
[0111] In some non-limiting examples, device 100 may be an OLED that includes at least an EL 135 having at least one semiconductive layer 130 sandwiched between conductive thin-film electrodes 120, 140, such that when a potential difference is applied between them, holes are injected into the at least one semiconductive layer 130 through the anode 341 and electrons are injected into the at least one semiconductive layer 130 through the cathode 342.
[0112] The injected holes and electrons tend to travel through the various layers 131, 133, 135, 137, and 139 until they reach and meet each other. When holes and electrons are in close proximity, they tend to be attracted to each other by Coulomb forces and, in some instances, may combine to form a bound electron-hole pair called an exciton. Specifically, when an exciton is formed in the EL 135, the exciton can decay through a radiative recombination process, in which a photon is emitted. The type of radiative recombination process can depend on the spin state of the exciton. In some instances, the exciton can be characterized as having a singlet or triplet spin state. In some non-limiting examples, the radiative decay of a singlet exciton can result in fluorescence. In some non-limiting examples, the radiative decay of a triplet exciton can result in phosphorescence.
[0113] More recently, other photon emission mechanisms for OLEDs have been proposed and investigated, including, but not limited to, TADF. In some non-limiting examples, TADF emission occurs through the conversion of triplet excitons to singlet excitons via a thermal energy-assisted reverse intersystem crossing process, followed by radiative decay of the singlet excitons.
[0114] In some non-limiting examples, excitons can decay through non-radiative processes in which no photons are released, particularly if the excitons are not formed within the EL135.
[0115] In this disclosure, the term "internal quantum efficiency" (IQE) of OLED device 100 refers to the fraction of all electron-hole pairs generated within device 100 that decay through the process of radiative recombination and emit photons.
[0116] In this disclosure, the term "external quantum efficiency" (EQE) of OLED device 100 refers to the ratio of charge carriers delivered to device 100 to the number of photons emitted by device 100. In some non-limiting examples, an EQE of 100% indicates that one photon is emitted for every electron injected into device 100.
[0117] Those skilled in the art will appreciate that the EQE of a device 100 may, in some non-limiting examples, be substantially lower than the IQE of the same device 100. The difference between the EQE and IQE of a given device 100 may be due to many factors, including, but not limited to, in some non-limiting examples, photon absorption and reflection caused by various components of the device 100.
[0118] In some non-limiting examples, device 100 may be an electroluminescent quantum dot device that includes an active layer in which at least one semiconductive layer 130 includes at least one quantum dot. When an electric current is provided by power source 15 to first electrode 120 and second electrode 140, photons are emitted from the active layer, including at least one semiconductive layer 130 therebetween.
[0119] Those skilled in the art will readily appreciate that the structure of device 100 can be altered by introducing one or more additional layers (not shown) at appropriate locations within the at least one semiconducting layer 130 stack, including, but not limited to, a hole blocking layer (not shown), an electron blocking layer (not shown), an additional charge transport layer (not shown), and / or an additional charge injection layer (not shown).
[0120] Barrier Coating In some non-limiting examples, a barrier coating 1650 can be provided to surround and / or encapsulate the various layers of the first electrode 120, the second electrode 140, and the at least one semiconductive layer 130, and / or the substrate 110 disposed thereon of the device 100.
[0121] In some non-limiting examples, a barrier coating 1650 may be provided to inhibit exposure of the various layers 120, 130, 140 of the device 100, including at least one semiconductive layer 130 and / or cathode 342, to moisture and / or ambient air, as these layers 120, 130, 140 are prone to oxidation.
[0122] In some non-limiting examples, application of the barrier coating 1650 to a highly uneven surface may increase the likelihood of poor adhesion of the barrier coating 1650 to such a surface.
[0123] In some non-limiting examples, a lack of barrier coating 1650 and / or a poorly applied barrier coating 1650 may cause and / or contribute to defects and / or partial and / or total failure in the device 100. In some non-limiting examples, a poorly applied barrier coating 1650 may reduce adhesion of the barrier coating 1650 to the device 100. In some non-limiting examples, poor adhesion of the barrier coating 1650 may increase the likelihood that the barrier coating 1650 will delaminate from all or portions of the device 100, particularly when the device 100 is flexed and / or bent. In some non-limiting examples, a poorly applied barrier coating 1650 may trap air pockets during application of the barrier coating 1650 between the barrier coating 1650 and the base surface of the device 100 to which the barrier coating 1650 is applied.
[0124] In some non-limiting examples, the barrier coating 1650 may be a thin film encapsulation (TFE) layer 2050 (FIG. 20B), which may be selectively applied, deposited, and / or processed using a variety of techniques, including, but not limited to, evaporation (including, but not limited to, thermal evaporation and / or e-beam evaporation), photolithography, printing (including, but not limited to, inkjet and / or evaporative jet printing, reel-to-reel printing, and / or microcontact transfer printing), PVD (including, but not limited to, sputtering), CVD (including, but not limited to, PECVD and / or OVPD), laser annealing, LTI patterning, ALD, coating (including, but not limited to, spin coating, dip coating, line coating, and / or spray coating), and / or a combination of any two or more thereof.
[0125] In some non-limiting examples, the barrier coating 1650 may be provided by laminating a pre-formed barrier film onto the device 100. In some non-limiting examples, the barrier coating 1650 may include a multi-layer coating including at least one of an organic material, an inorganic material, and / or any combination thereof. In some non-limiting examples, the barrier coating 1550 may further include a getter material and / or a desiccant.
[0126] Side view In some non-limiting examples, including when OLED device 100 comprises a lighting panel, an entire lateral side of device 100 can correspond to a single lighting element. Thus, the substantially planar cross-sectional profile shown in FIG. 1 can extend substantially along the entire lateral side of device 100 such that photons are emitted from device 100 along substantially its entire lateral extent. In some non-limiting examples, such a single lighting element can be driven by a single drive circuit 300 of device 100.
[0127] In some non-limiting examples, including when OLED device 100 comprises a display module, the lateral aspect of device 100 can be subdivided into a plurality of light-emitting regions 1910 of device 100, where the cross-sectional aspect of device structure 100 within each of light-emitting regions 1910, as shown but not limited to in FIG. 1, causes photons to be emitted therefrom when energized.
[0128] Light-emitting area In some non-limiting examples, the individual light-emitting regions 1910 of device 100 may be arranged in a horizontal pattern. In some non-limiting examples, the pattern may extend along a first horizontal direction. In some non-limiting examples, the pattern may also extend along a second horizontal direction, which, in some non-limiting examples, may be substantially perpendicular to the first horizontal direction. In some non-limiting examples, the pattern may have many elements within such a pattern, with each element characterized by one or more features thereof, including, but not limited to, the wavelength of light emitted by that light-emitting region 1910, the shape of such light-emitting region 1910, its dimensions (along either or both of the first and / or second horizontal directions), its orientation (with respect to either and / or the first and / or second horizontal directions), and / or its spacing from the previous element in the pattern (with respect to either or both of the first and / or second horizontal directions). In some non-limiting examples, the pattern may be repeated in either or both of the first and / or second horizontal directions.
[0129] In some non-limiting examples, each individual light-emitting region 1910 of device 100 is associated with and driven by a corresponding drive circuit 300 in backplane 20 of device 100, where diode 340 corresponds to the OLED structure for the associated light-emitting region 1910. In some non-limiting examples, including but not limited to when light-emitting regions 1910 are arranged in a regular pattern extending in both a first (row) horizontal direction and a second (column) horizontal direction, there may be signal lines 30, 31 in backplane 20 corresponding to each row of light-emitting regions 1910 extending in the first horizontal direction, which may be gate lines (or row select) lines 31, and signal lines 30, 31 corresponding to each column of light-emitting regions 1910 extending in the second horizontal direction, which may be data (or column select) lines 30 in some non-limiting examples. In such a non-limiting configuration, the signal on the row select line 31 can energize the gate 312 of each of the switching TFTs 310 electrically coupled thereto, and the signal on the data line 30 can energize the source of each of the switching TFTs 310 electrically coupled thereto, such that the signal on the row select line 31 / data line 30 pair is electrically coupled to and energizes the positive terminal of the power source 15 (represented by the electrical supply line VDD32), the anode 341 of the OLED structure of the light-emitting region 1910 associated with such pair causing emission of photons therefrom, its cathode 342 being electrically coupled to the negative terminal of the power source 15.
[0130] In some non-limiting examples, each light-emitting region 1910 of device 100 corresponds to a single display pixel 340. In some non-limiting examples, each pixel 340 emits light in a given wavelength spectrum. In some non-limiting examples, the wavelength spectrum corresponds to, but is not limited to, a color in the visible light spectrum.
[0131] In some non-limiting examples, each light-emitting region 1910 of device 100 corresponds to a sub-pixel 264x of display pixel 340. In some non-limiting examples, multiple sub-pixels 264x can be combined to form or represent a single display pixel 340.
[0132] In some non-limiting examples, a single display pixel 340 can be represented by three subpixels 2641-2643. In some non-limiting examples, the three subpixels 2641-2643 can be displayed as an R (red) subpixel 2641, a G (green) subpixel 2642, and / or a B (blue) subpixel 2643, respectively. In some non-limiting examples, a single display pixel 340 can be represented by four subpixels 264x, where three of such subpixels 264x can be displayed as R, G, and B subpixels 2641-2643, and the fourth subpixel 264x can be displayed as a W (white) subpixel 264x. In some non-limiting examples, the emission spectrum of light emitted by a given subpixel 264x corresponds to the color at which the subpixel 264x is displayed. In some non-limiting examples, the wavelength of light does not correspond to such a color, but further processing is performed to convert the wavelength to one that does correspond, in a manner apparent to one skilled in the art.
[0133] Because the wavelengths of the subpixels 264x of different colors may be different, the optical characteristics of such subpixels 264x may be different, especially when common electrodes 120, 140 having a substantially uniform thickness profile are employed for the subpixels 264x of different colors.
[0134] If a common electrode 120, 140 having a substantially uniform thickness is provided as the second electrode 140 of the device 100, the optical performance of the device 100 cannot be easily fine-tuned according to the emission spectrum associated with each (sub)pixel 340 / 264x. The second electrode 140 used in such an OLED device 100 can, in some non-limiting examples, be a common electrode 120, 140 covering multiple (sub)pixels 340 / 264x. As a non-limiting example, such a common electrode 120, 140 can be a relatively thin conductive layer having a substantially uniform thickness throughout the device 100. Efforts have been made in some non-limiting examples to tailor the optical microcavity effect associated with the color of each (sub)pixel 340 / 264x by varying the thickness of organic layers disposed within different (sub)pixels 340 / 264x; such an approach can, in some non-limiting examples, at least in some cases, provide a significant degree of tailoring of the optical microcavity effect. Additionally, in some non-limiting examples, such schemes may be difficult to implement in an OLED display manufacturing environment.
[0135] As a result, in some non-limiting examples, the presence of optical interfaces created by multiple thin film layers and coatings with different refractive indices, such as may be used to construct optoelectronic devices, including but not limited to OLED device 100, may create different optical microcavity effects for different color subpixels 264x.
[0136] In device 100, some factors that may affect the observed microcavity effect include, but are not limited to, the total path length (which in some non-limiting examples may correspond to the total thickness of device 100 through which photons emitted therefrom pass before being extracted), and the refractive indices of the various layers and coatings.
[0137] In some non-limiting examples, adjusting the thickness of the electrodes 120, 140 in and across the lateral sides 410 of the light-emitting region 1910 of the (sub)pixel 340 / 264x may affect the observable microcavity effect. In some non-limiting examples, such an effect may result from a change in the total optical path length.
[0138] In some non-limiting examples, a change in the thickness of the electrodes 120, 140 may also change the refractive index of light passing therethrough, in addition to changing the total optical path length, in some non-limiting examples, particularly when the electrodes 120, 140 are formed with at least one conductive coating 830.
[0139] In some non-limiting examples, optical properties across the lateral sides 410 of the light-emitting region 1910 of device 100 and / or of (sub)pixel 340 / 264x that can be altered by adjusting at least one optical microcavity effect include, but are not limited to, the emission spectrum, the intensity (including but not limited to luminosity), and / or the angular distribution of the emitted light, including but not limited to the angular dependence of the brightness and / or color shift of the emitted light.
[0140] In some non-limiting examples, a subpixel 264x is associated with a first set of other subpixels 264x to represent a first display pixel 340, and is also associated with a second set of other subpixels 264x to represent a second display pixel 340, such that the first and second display pixels 340 can have the same subpixel 264x associated with them.
[0141] The pattern and / or organization of the sub-pixels 264x into display pixels 340 continues to evolve, and all current and future patterns and / or organizations are considered to be within the scope of this disclosure.
[0142] Non-luminous area In some non-limiting examples, the various light-emitting regions 1910 of device 100 are substantially surrounded and separated in at least one lateral direction by one or more non-light-emitting regions 1920, where the structure and / or configuration along a cross-sectional side of device structure 100, such as shown but not limited to in FIG. 1 , is varied to substantially suppress photons emitted therefrom. In some non-limiting examples, non-light-emitting regions 1920 include those regions within the lateral side that are substantially free of light-emitting regions 1910.
[0143] Thus, as shown in the cross-sectional view of FIG. 4, the lateral topology of various layers of at least one semiconductive layer 130 can be varied to define at least one light-emitting region 1910 surrounded (in at least one lateral direction) by at least one non-light-emitting region 1920.
[0144] In some non-limiting examples, an emissive region 1910 corresponding to a single display (sub)pixel 340 / 264x can be understood to have at least one lateral side 410 laterally surrounded by at least one non-emissive region 1920 having a lateral side 420.
[0145] Non-limiting examples of implementations of a cross-sectional side view of device 100 as applied to a light-emitting region 1910 corresponding to a single display (sub)pixel 340 / 264x of OLED display 100 are now described. While features of such implementations are shown to be specific to light-emitting region 1910, those skilled in the art will understand that in some non-limiting examples, two or more light-emitting regions 1910 may include common features.
[0146] In some non-limiting examples, first electrode 120 can be disposed on exposed layer surface 111 of device 100, in some non-limiting examples within at least a portion of a lateral side 410 of light-emitting region 1910. In some non-limiting examples, at least within the lateral side 410 of light-emitting region 1910 of (sub)pixel 340 / 264x, exposed layer surface 111 can include TFT insulating layers 280 of various TFT structures 200 that, upon deposition of first electrode 120, make up drive circuitry 300 for light-emitting region 1910 corresponding to a single display (sub)pixel 340 / 264x.
[0147] In some non-limiting examples, the TFT insulating layer 280 can have an opening 430 formed therethrough to allow the first electrode 120 to be electrically coupled to one of the TFT electrodes 240, 260, 270, including but not limited to the TFT drain electrode 270, as shown in FIG.
[0148] Those skilled in the art will appreciate that the drive circuit 300 includes multiple TFT structures 200, including, but not limited to, a switching TFT 310, a drive TFT 320, and / or a storage capacitor 330. While only one TFT structure 200 is shown in Figure 4 for ease of illustration, those skilled in the art will appreciate that such TFT structure 200 is representative of multiple such TFT structures that make up the drive circuit 300.
[0149] In cross-sectional view, the configuration of each light-emitting region 1910 can be defined, in some non-limiting examples, by introducing at least one pixel-defining layer (PDL) 440 substantially across the entire lateral side 420 of the surrounding non-light-emitting region 1920. In some non-limiting examples, the PDL 440 can include an insulating organic material and / or an insulating inorganic material.
[0150] In some non-limiting examples, the PDL 440 is deposited substantially on the TFT insulating layer 280, although as shown, in some non-limiting examples, the PDL 440 may also extend over at least a portion of the deposited first electrode 120 and / or its outer edge.
[0151] In some non-limiting examples, as shown in FIG. 4, the cross-sectional thickness and / or profile of the PDL 440 can impart a substantially valley-shaped configuration to the emissive region 1910 of each (sub)pixel 340 / 264x with regions of increased thickness along the boundary between the lateral sides 420 of the surrounding non-emissive region 1920 and the lateral sides 410 of the surrounded emissive region 1910 corresponding to the (sub)pixel 340 / 264x.
[0152] In some non-limiting examples, the profile of the PDL 440 may have a reduced thickness beyond such a valley-shaped configuration, including, but not limited to, away from the boundary between the lateral side 420 of the surrounding non-emitting region 1920 and the lateral side 410 of the surrounded emitting region 1910, in some non-limiting examples, substantially well within the lateral side 420 of such non-emitting region 1920.
[0153] While the PDL 440 is generally shown as having linearly sloped surfaces to form a valley-shaped configuration that defines the enclosed light-emitting area 1910, those skilled in the art will understand that, in some non-limiting examples, at least one of the shape, aspect ratio, thickness, width, and / or configuration of such a PDL 440 can be varied. As a non-limiting example, the PDL 440 can be formed with steeper or more gently sloping portions. In some non-limiting examples, such a PDL 440 can be configured to extend substantially normal away from the surface on which it is deposited, covering one or more edges of the first electrode 120. In some non-limiting examples, such a PDL 440 can be configured to deposit at least one semiconducting layer 130 thereon by solution processing techniques, including but not limited to, by printing, including but not limited to, inkjet printing.
[0154] In some non-limiting examples, at least one semiconductive layer 130 may be deposited on exposed layer surfaces 111 of device 100, including at least a portion of lateral sides 410 of such light-emitting area 1910 of (sub)pixel 340 / 264x. In some non-limiting examples, at least within lateral sides 410 of light-emitting area 1910 of (sub)pixel 340 / 264x, such exposed layer surfaces 111 may include first electrode 120 upon deposition of at least one semiconductive layer 130 (and / or its layers 131, 133, 135, 137, 139).
[0155] In some non-limiting examples, the at least one semiconductive layer 130 may also extend beyond the lateral sides 410 of the emissive region 1910 of the (sub)pixel 340 / 264x and at least partially into the lateral sides 420 of the surrounding non-emissive region 1920. In some non-limiting examples, such exposed layer surfaces 111 of such surrounding non-emissive region 1920 may include PDL 440 upon deposition of the at least one semiconductive layer 130.
[0156] In some non-limiting examples, second electrode 140 can be disposed on an exposed layer surface 111 of device 100, including at least a portion of a lateral side 410 of light-emitting region 1910 of (sub)pixel 340 / 264x. In some non-limiting examples, at least within the lateral side 410 of light-emitting region 1910 of (sub)pixel 340 / 264x, such exposed layer surface 111 can include at least one semiconducting layer 130 upon deposition of second electrode 130.
[0157] In some non-limiting examples, the second electrode 140 may also extend beyond the lateral sides 410 of the emissive region 1910 of the (sub)pixel 340 / 264x and at least partially into the lateral sides 420 of the surrounding non-emissive region 1920. In some non-limiting examples, such exposed layer surfaces 111 of such surrounding non-emissive region 1920 may include the PDL 440 upon deposition of the second electrode 140.
[0158] In some non-limiting examples, the second electrode 140 can extend across substantially all or a substantial portion of the lateral side 420 of the surrounding non-emitting region 1920 .
[0159] transparency Because OLED device 100 emits photons through first electrode 120 (in the case of a bottom-emitting and / or dual-emitting device) and either or both substrate 110 and / or second electrode 140 (in the case of a top-emitting and / or dual-emitting device), it may be desirable in some non-limiting examples to make either or both first electrode 120 and / or second electrode 140 substantially photon (or light) transmissive (“transmissive”), at least over a substantial portion of the lateral sides 410 of light-emitting region 1910 of device 100. In the present disclosure, such transmissive elements, including but not limited to electrodes 120, 140, the materials forming such elements, and / or the properties thereof, may include elements, materials, and / or properties thereof that are, in some non-limiting examples, substantially transmissive (“transparent”), and / or, in some non-limiting examples, partially transmissive (“semi-transparent”), in at least one wavelength band.
[0160] Various mechanisms have been employed to impart transmissive properties to device 100 over at least a substantial portion of the lateral sides 410 of its light-emitting region 1910 .
[0161] In some non-limiting examples, including but not limited to when device 100 is a bottom-emitting device and / or a double-sided emitting device, the TFT structure 200 of the drive circuit 300 associated with the light-emitting region 1910 of (sub)pixel 340 / 264x, which can at least partially reduce the transparency of the surrounding substrate 110, is positioned within the lateral side 420 of the surrounding non-light-emitting region 1920 to avoid affecting the transparency properties of the substrate 110 within the lateral side 410 of the light-emitting region 1910.
[0162] In some non-limiting examples where device 100 is a dual-sided light-emitting device, one of electrodes 120, 140 may be made substantially transparent, including but not limited to, by at least one of the mechanisms disclosed herein, with respect to a lateral side 410 of light-emitting region 1910 of (sub)pixel 340 / 264x, and the other of electrodes 120, 140 may be made substantially transparent, including but not limited to, by at least one of the mechanisms disclosed herein, with respect to a lateral side 410 of adjacent and / or neighboring (sub)pixel 340 / 264x. Thus, in an alternating (sub)pixel 340 / 264x arrangement, the lateral sides 410 of the first light-emitting region 1910 of a (sub)pixel 340 / 264x can be substantially top-emitting, while the lateral sides 410 of the second light-emitting region 1910 of an adjacent (sub)pixel 340 / 264x can be substantially bottom-emitting, such that a subset of the (sub)pixels 340 / 264x are substantially top-emitting and a subset of the (sub)pixels 340 / 264x are substantially bottom-emitting, while only a single electrode 120, 140 of each (sub)pixel 340 / 264x is made substantially transparent.
[0163] In some non-limiting examples, a mechanism for making the electrodes 120, 140 (the first electrode 120 in the case of a bottom-emitting device and / or a double-sided emitting device, and / or the second electrode 140 in the case of a top-emitting device and / or a double-sided emitting device) transparent is to form such electrodes 120, 140 of a transparent thin film.
[0164] In some non-limiting examples, the conductive coating 830 can exhibit transparent properties, including but not limited to, those formed by depositing a conductive thin film layer of a metal, including but not limited to, Ag, Al, and / or by depositing a thin layer of a metal alloy, including but not limited to, Mg:Ag alloy and / or Yb:Ag alloy. In some non-limiting examples, the alloy can have a composition ranging from about 1:9 to about 9:1 by volume. In some non-limiting examples, the electrodes 120, 140 can be formed from multiple conductive thin film layers of any combination of the conductive coating 830, any one or more of which can be comprised of a TCO, a metal thin film, a metal alloy thin film, and / or any combination of any of these.
[0165] In some non-limiting examples, particularly in the case of such conductive thin films, the relatively thin layer thickness can be up to substantially tens of nanometers, so as to contribute enhanced transmissive qualities for use in OLED device 100, but also favorable optical properties (including, but not limited to, reduced microcavity effects).
[0166] In some non-limiting examples, reducing the thickness of the electrodes 120, 140 to promote transparency qualities may be accompanied by an increase in the sheet resistance of the electrodes 120, 140.
[0167] In some non-limiting examples, a device 100 having at least one electrode 120, 140 with a high sheet resistance will produce a large current-resistance (IR) drop during operation when coupled to a power supply 15. In some non-limiting examples, such IR drop can be compensated for to some extent by increasing the level (VDD) of the power supply 15. However, in some non-limiting examples, increasing the level of the power supply 15 for at least one (sub)pixel 340 / 264x to compensate for the IR drop due to the high sheet resistance may require increasing the level of the voltage supplied to other components to maintain effective operation of the device 100.
[0168] In some non-limiting examples, auxiliary electrodes 1750 and / or busbar structures 4150 can be formed on device 100 to reduce the electrical supply demands of device 100 (by employing at least one thin film layer of any combination of TCO, metal thin film, and / or metal alloy thin film) without significantly affecting the ability of electrodes 120, 140 to be substantially transparent, allowing for more effective transport of current to various light-emitting regions of device 100, while simultaneously reducing the sheet resistance of the transparent electrodes 120, 140 and its associated IR drop.
[0169] In some non-limiting examples, the sheet resistance specification for the common electrodes 120, 140 of an AMOLED display device 100 may vary according to many parameters, including, but not limited to, the (panel) size of the device 100 and / or the tolerance for voltage variation across the device 100. In some non-limiting examples, as the panel size increases, the sheet resistance specification may increase (i.e., a lower sheet resistance is specified). In some non-limiting examples, as the tolerance for voltage variation decreases, the sheet resistance specification may increase.
[0170] In some non-limiting examples, sheet resistance specifications can be used to derive example thicknesses of auxiliary electrode 1750 and / or bus bar 4150 to comply with such specifications for various panel sizes. In one non-limiting example, an aperture ratio of 0.64 was assumed for all display panel sizes, and the thicknesses of auxiliary electrode 1750 for various example panel sizes were calculated for voltage tolerances of 0.1V and 0.2V, for example, in Table 1 below. [Table 1]
[0171] As a non-limiting example, for a top-emitting device, the second electrode 140 may be made transparent. On the other hand, in some non-limiting examples, such auxiliary electrodes 1750 and / or bus bars 4150 may not be substantially transparent, but may be electrically coupled to the second electrode 140, including but not limited to, by depositing a conductive coating 830 therebetween, to reduce the effective sheet resistance of the second electrode 140.
[0172] In some non-limiting examples, such auxiliary electrodes 1750 may be positioned and / or shaped on either or both of the lateral and / or cross-sectional sides so as not to interfere with the emission of photons from the lateral sides 410 of the light-emitting area 1910 of the (sub)pixel 340 / 264x.
[0173] In some non-limiting examples, a mechanism for fabricating first electrode 120 and / or second electrode 140 is to form such electrodes 120, 140 in a pattern that spans at least a portion of the lateral sides 410 of its emissive region 1910 and / or, in some non-limiting examples, at least a portion of the lateral sides 420 of the non-emissive region 1920 that surrounds them. In some non-limiting examples, such a mechanism can be employed to form auxiliary electrodes 1750 and / or bus bars 4150 in a position and / or shape on either or both of the lateral sides and / or cross-sectional sides so as not to interfere with the emission of photons from the lateral sides 410 of the emissive region 1910 of (sub)pixel 340 / 264x, as discussed above.
[0174] In some non-limiting examples, device 100 may be configured such that the optical path of photons emitted by device 100 is substantially free of conductive oxide material. As a non-limiting example, at least one of the layers and / or coatings deposited after at least one semiconductive layer 130, including, but not limited to, second electrode 140, NIC810, and / or any other layers and / or coatings deposited thereon, on the lateral side 410 of at least one light-emitting region 1910 corresponding to (sub)pixel 340 / 264x, may be substantially free of conductive oxide material. In some non-limiting examples, the substantial absence of conductive oxide material may reduce absorption and / or reflection of light emitted by device 100. As a non-limiting example, conductive oxide materials, including, but not limited to, ITO and / or IZO, can absorb light in at least the B (blue) region of the visible spectrum, which may generally reduce the efficiency and / or performance of device 100.
[0175] In some non-limiting examples, combinations of these and / or other mechanisms may be employed.
[0176] Additionally, in some non-limiting examples, in addition to making one or more of the first electrode 120, the second electrode 140, the auxiliary electrode 1750, and / or the bus bar 4150 substantially transparent across at least a substantial portion of the lateral side 410 of the light-emitting region 1910 corresponding to the (sub)pixel 340 / 264x of the device 100, to allow photons to be substantially emitted across that lateral side 410, as disclosed herein, it may be desirable to make at least one of the lateral sides 420 of the surrounding non-light-emitting region 1920 of the device 100 substantially transparent in both the bottom and top directions to make the device 100 substantially transparent to light incident on its external surface so that a significant portion of such external incident light can pass through the device 100 in addition to the emission of photons generated internally within the device 100 (in top-emission, bottom-emission, and / or dual-side emission).
[0177] conductive coating In some non-limiting examples, the conductive coating material 831 (FIG. 9) used to deposit the conductive coating 830 on the exposed layer surface 111 of the base material can be a mixture.
[0178] In some non-limiting examples, at least one component of such a mixture may not be deposited on such a surface, may not be deposited on such an exposed layer surface 111 during deposition, and / or may be deposited in a small amount relative to the amount of the remaining components of such a mixture that are deposited on such exposed layer surface 111.
[0179] In some non-limiting examples, such at least one component of such a mixture can have a property relative to the remaining components to selectively deposit substantially only the remaining components, which in some non-limiting examples can be vapor pressure.
[0180] In some non-limiting examples, such at least one component of such a mixture may have a lower vapor pressure relative to the remaining components.
[0181] In some non-limiting examples, the conductive coating material 831 can be a copper (Cu)-magnesium (Cu-Mg) mixture, where Cu has a lower vapor pressure than Mg.
[0182] In some non-limiting examples, the conductive coating material 831 used to deposit the conductive coating 830 on the exposed layer surface 111 can be substantially pure.
[0183] In some non-limiting examples, the conductive coating material 831 used to deposit the Mg includes, in some non-limiting examples, substantially pure Mg. In some non-limiting examples, the substantially pure Mg can exhibit properties substantially similar to pure Mg. In some non-limiting examples, the purity of the Mg can be about 95% or greater, about 98% or greater, about 99% or greater, about 99.9% or greater, and 99.99% or greater.
[0184] In some non-limiting examples, the conductive coating material 831 used to deposit the conductive coating 830 on the exposed layer surface 111 may include other metals as a substitute for and / or in combination with Mg. In some non-limiting examples, the conductive coating material 831 including such other metals may include high vapor pressure materials, including, but not limited to, Yb, Cd, Zn, and / or any combination of any of these.
[0185] In some non-limiting examples, the conductive coating 830 of the optoelectronic device according to various embodiments includes Mg. In some non-limiting examples, the conductive coating 830 includes substantially pure Mg. In some non-limiting examples, the conductive coating 830 includes other metals as a substitute for and / or in combination with Mg. In some non-limiting examples, the conductive coating 830 includes an alloy of Mg with one or more other metals. In some non-limiting examples, the conductive coating 830 includes an alloy of Mg with Yb, Cd, Zn, and / or Ag. In some non-limiting examples, such an alloy may be a binary alloy having a composition ranging from about 5% Mg by volume to about 95% Mg by volume, with the remainder being the other metal. In some non-limiting examples, the conductive coating 830 includes an Mg:Ag alloy having a composition ranging from about 1:10 to about 10:1 by volume.
[0186] Patterning As a result of the foregoing, it may be desirable to selectively deposit device features, including but not limited to, at least one of first electrode 120, second electrode 140, auxiliary electrode 1750, and / or bus bar 4150, and / or conductive elements electrically coupled thereto, in a pattern on exposed layer surface 111 of front plane 10 layer of device 100 across lateral sides 410 of emissive region 1910 of (sub)pixel 340 / 264x and / or lateral sides 420 of non-emissive region 1920 surrounding emissive region 1910. In some non-limiting examples, first electrode 120, second electrode 140, auxiliary electrode 1750, and / or bus bar 4150 may be deposited on at least one of multiple conductive coatings 830.
[0187] However, to achieve such patterning of the conductive coating 830, employing a shadow mask such as a fine metal mask (FMM), which may be used in some non-limiting examples to form relatively small features having feature sizes on the order of tens of microns or less, may not be feasible in some non-limiting examples for the following reasons. · FMMs may deform during deposition processes, especially at high temperatures, such as may be employed in the deposition of conductive thin films. · Limited mechanical (including but not limited to tensile) strength and / or shadowing effects of FMMs, particularly in high temperature deposition processes, may impose constraints on the aspect ratios of features that may be achievable using such FMMs. By way of non-limiting example, the types and number of patterns that may be achievable using such an FMM may be constrained because each portion of the FMM may be physically supported such that some patterns may not be achievable in a single processing step, including, by way of non-limiting example, when the pattern specifies an isolated feature. The FMM may exhibit a tendency to warp during high temperature deposition processes, which, in some non-limiting examples, may distort the shape and position of apertures in the FMM, which may alter selective deposition patterns and reduce performance and / or yield. FMMs that can be used to generate repeating structures that span the entire surface of device 100 may require a large number of apertures to be formed in the FMM, which may compromise the structural integrity of the FMM. Repeated use of an FMM in successive depositions, especially in metal deposition processes, can cause the deposited material to adhere to the FMM, which can obscure the features of the FMM, alter the selective deposition pattern, and reduce performance and / or yield. · FMMs may be cleaned periodically to remove bonded non-metallic materials, however, such cleaning procedures may not be suitable for use with bonded metals and, even so, may be time consuming and / or expensive in some non-limiting examples. Continued use of such FMMs, regardless of any such cleaning process, especially in high temperature deposition processes, may be wasteful in producing the desired patterning, resulting in their disposal and / or replacement in a complex and expensive process.
[0188] FIG. 5 shows an example cross-sectional view of a device 500 that is substantially similar to device 100, but further includes multiple raised PDLs 440 spanning the lateral sides 420 of a non-emissive region 1920 that surround the lateral sides 410 of an emissive region 1910 corresponding to (sub)pixel 340 / 264x.
[0189] When the conductive coating 830 is deposited using an open-mask deposition process and / or a mask-free deposition process, in some non-limiting examples, the conductive coating 830 is deposited over the lateral sides 410 of the emissive regions 1910 corresponding to (sub)pixels 340 / 264x (as shown) to form the second electrodes 140 thereon, as well as over the lateral sides 420 of the surrounding non-emissive regions 1920 to form regions of the conductive coating 830 on top of the PDLs 440. To ensure that each (segment) of the second electrodes 140 is not electrically coupled to any of the at least one conductive regions 830, the thickness of the PDLs 440 is greater than the thickness of the second electrodes 140. In some non-limiting examples, as shown in the figures, the PDLs 440 can be provided with an undercut profile to further reduce the likelihood that any (segment) of the second electrodes 140 is electrically coupled to any of the at least one conductive regions 830.
[0190] In some non-limiting examples, applying the barrier coating 1650 onto the device 500 may result in poor adhesion of the barrier coating 1650 to the device 500 given the highly uneven surface morphology of the device 500.
[0191] In some non-limiting examples, it may be desirable to tailor the optical microcavity effects associated with subpixels 264x of different colors (and / or wavelengths) by varying the thickness of at least one semiconducting material 130 (and / or layers thereof) across the lateral sides 410 of light-emitting region 1910 corresponding to subpixels 264x of one color relative to the lateral sides 410 of light-emitting region 1910 corresponding to subpixels 264x of another color. In some non-limiting examples, the use of an FMM to perform the patterning may not provide the precision needed to provide such optical microcavity modulation effects, at least in some cases, and / or in some non-limiting examples, in a production environment for OLED display 100.
[0192] Nucleation-inhibiting and / or nucleation-promoting material properties In some non-limiting examples, the conductive coating 830, which may be employed as at least one of multiple layers of conductive thin films to form device features including, but not limited to, at least one of the first electrode 120, the first electrode 140, the auxiliary electrode 1750, and / or the bus bar 4150, and / or conductive elements electrically coupled thereto, may exhibit a relatively low affinity for being deposited on the exposed layer surface 111 of the base material, thereby inhibiting deposition of the conductive coating 830.
[0193] The relative affinity or lack thereof of a material and / or its properties for having a conductive coating 830 deposited thereon may be referred to as being "nucleation promoting" or "nucleation inhibiting," respectively.
[0194] In this disclosure, "nucleation-inhibiting" refers to coatings, materials, and / or layers thereof that have surfaces that exhibit a relatively low affinity for (the deposition of) conductive coating 830 thereon, such that deposition of conductive coating 830 on such surfaces is inhibited.
[0195] In this disclosure, "nucleation promoting" refers to a coating, material, and / or layer thereof having a surface that exhibits a relatively high affinity for the deposition of conductive coating 830 onto such a surface, thereby facilitating the deposition of conductive coating 830 onto such a surface.
[0196] The term "nucleation" in these terms refers to the nucleation stage of the thin film formation process, where monomers in the gas phase condense onto a surface to form nuclei.
[0197] Without wishing to be bound by any particular theory, it is believed that the shape and size of such nuclei and their subsequent growth into islands and then into thin films may depend on many factors, including, but not limited to, the interfacial tension between the vapor, the surface, and / or the condensed film nuclei.
[0198] In the present disclosure, such affinity can be measured in a number of ways.
[0199] One measure of the nucleation-inhibiting and / or nucleation-promoting properties of a surface is the initial sticking probability, S, of the surface for a given conductive material, including but not limited to Mg. In this disclosure, the terms "sticking probability" and "sticking coefficient" may be used interchangeably.
[0200] In some non-limiting examples, the sticking probability S may be given by:
number
[0201] As the island density increases (e.g., the average film thickness increases), the sticking probability S may change. As a non-limiting example, a low initial sticking probability S may increase as the average film thickness increases. This can be understood based on the difference in sticking probability S between an area of a surface without islands, as a non-limiting example, a bare substrate 110, and an area with a high density of islands. As a non-limiting example, a monomer impinging on the surface of an island may have a sticking probability S close to 1.
[0202] Thus, the initial sticking probability S0 may be specified as the sticking probability S of a surface before any significant number of critical nuclei are formed. One measure of the initial sticking probability S0 may involve the sticking probability S of a surface for a material during the initial stages of deposition of the material, where the average thickness of the deposited material across the surface is at or below a threshold value. In illustrating some non-limiting examples, the threshold value for the initial sticking probability S0 may be specified as 1 nm, as a non-limiting example. Then, the average sticking probability
number
number
[0203] An example energy profile of an adatom adsorbed on an exposed layer surface 111 of a base material (shown as substrate 110) is shown in Figure 6. Specifically, Figure 6 shows example qualitative energy profiles corresponding to an adatom escaping from a localized low-energy site (610), adatom diffusion at the exposed layer surface 111 (620), and adatom desorption (630).
[0204] In 610, a localized low-energy site can be any site on the exposed layer surface 111 of the base material where adatoms become lower in energy. Typically, nucleation sites can include defects and / or anomalies on the exposed layer surface 111, including, but not limited to, step edges, chemical impurities, bond sites, and / or kinks. When adatoms are trapped at a localized low-energy site, there may typically be an energy barrier before surface diffusion can occur. Such an energy barrier is represented as ΔE 611 in FIG. 6. In some non-limiting examples, if the energy barrier ΔE 611 to escape from a localized low-energy site is sufficiently large, the site may act as a nucleation site.
[0205] In 620, adatoms may diffuse onto the exposed layer surface 111. As a non-limiting example, in the case of localized adsorbates, adatoms oscillate around a minimum in the surface potential and tend to move to various nearby sites until they desorb and / or become incorporated into the growing film and / or growing islands formed by clusters of adatoms. In the diagram of FIG. 6, the activation energy associated with surface diffusion of adatoms is E s It is represented as 621.
[0206] At 630, the activation energy associated with the desorption of adatoms from the surface is E des 631. Those skilled in the art will appreciate that any adatoms that are not desorbed may remain on exposed layer surface 111. By way of non-limiting example, such adatoms may diffuse onto exposed layer surface 111, become incorporated as part of a growing film and / or coating, and / or become part of clusters of adatoms that form islands on exposed layer surface 111.
[0207] Based on the energy profiles 610, 620, 630 shown in FIG. 6, the relatively low activation energy for desorption (E des 631), and / or a relatively high activation energy for surface diffusion, E sIt can be envisioned that NIC810 materials exhibiting (631) may be particularly advantageous for use in a variety of applications.
[0208] One measure of the nucleation-inhibiting or nucleation-promoting properties of a surface is the initial deposition rate of a given conductive material, including but not limited to Mg, on a surface relative to the initial deposition rate of the same conductive material on a reference surface, both surfaces being exposed to and / or exposed to an evaporation flux of the conductive material.
[0209] Selective coatings to influence nucleation-suppressing and / or nucleation-promoting material properties In some non-limiting examples, one or more selective coatings 710 (FIG. 7) may be selectively deposited on at least a first portion 701 (FIG. 7) of the exposed layer surface 111 of the base material that is presented for depositing a thin film conductive coating 830 thereon. Such selective coatings 710 have nucleation-inhibiting properties (and / or conversely, nucleation-promoting properties) with respect to the conductive coating 830 that differ from those of the exposed layer surface 111 of the base material. In some non-limiting examples, there may be a second portion 702 (FIG. 7) of the exposed layer surface 111 of the base material that does not have such selective coatings 710 deposited thereon.
[0210] Such selective coating 710 can be NIC810, and / or a nucleation promoting coating (NPC1120 (FIG. 11)).
[0211] Those skilled in the art will appreciate that the use of such a selective coating 710 can, in some non-limiting examples, facilitate and / or allow for selective deposition of the conductive coating 830 without employing an FMM in the step of depositing the conductive coating 830.
[0212] In some non-limiting examples, such selective deposition of conductive coating 830 can be a pattern. In some non-limiting examples, such a pattern can facilitate providing and / or increasing transparency of at least one of the top and / or bottom surfaces of device 100 within lateral sides 410 of one or more emissive regions 1910 of (sub)pixel 340 / 264x and / or within lateral sides 420 of one or more non-emissive regions 1920 that may surround such emissive regions 1910.
[0213] In some non-limiting examples, a conductive coating 830 can be deposited on a conductive structure and / or form a layer of the device 100, which in some non-limiting examples may be the first electrode 120 and / or the second electrode 140 acting as one of the anode 341 and / or cathode 342, and / or an auxiliary electrode 1750 and / or bus bar 4150 for supporting its conductivity and / or electrically coupled thereto in some non-limiting examples.
[0214] In some non-limiting examples, the NIC 810 of a given conductive coating 830, including but not limited to Mg, may refer to a coating having a surface that exhibits a relatively low initial sticking probability, S, for the conductive coating 830 (in example, Mg) in vapor form, such that deposition of the conductive coating 830 (in example, Mg) onto the exposed layer surface 111 is inhibited. Thus, in some non-limiting examples, selective deposition of the NIC 810 may reduce the initial sticking probability, S, of the exposed layer surface 111 (of the NIC 810) presented for depositing the conductive coating 830 thereon.
[0215] In some non-limiting examples, the NPC 1120 of a given conductive coating 830, including but not limited to Mg, may refer to a coating having an exposed layer surface 111 that exhibits a relatively high initial sticking probability S for the conductive coating 830 in vapor form, so as to facilitate deposition of the conductive coating 830 onto the exposed layer surface 111. Thus, in some non-limiting examples, selective deposition of the NPC 1120 may increase the initial sticking probability S of the exposed layer surface 111 (of the NPC 1120) that is presented for depositing the conductive coating 830 onto the exposed layer surface 111.
[0216] When the selective coating 710 is NIC 810, the first portion 701 of the exposed layer surface 111 of the base material on which the NIC 810 is deposited will then present a treated surface (of the NIC 810) with increased nucleation-inhibiting properties or, alternatively, reduced nucleation-promoting properties, such that it has a reduced affinity for the deposition of the conductive coating 830 thereon relative to the affinity of the exposed layer surface 111 of the base material on which the NIC 810 was deposited. In contrast, the second portion 702 on which no such NIC 810 is deposited will continue to present an exposed layer surface 111 (of the base substrate 110) with an affinity for the deposition of the conductive coating 830 thereon whose nucleation-inhibiting or, alternatively, nucleation-promoting properties are substantially unchanged (in either case, the exposed layer surface 111 of the base substrate 110 substantially free of the selective coating 710).
[0217] When the selective coating 710 is NPC 1120, the first portion 701 of the exposed layer surface 111 of the base material on which the NPC 1120 is deposited will then present a treated surface (of the NPC 1120) with reduced nucleation-inhibiting properties or, alternatively, increased nucleation-promoting properties (in either case, the surface of the NPC 1120 deposited on the first portion 701) so as to have an increased affinity for deposition of the conductive coating 830 thereon relative to the affinity of the exposed layer surface 111 of the base material on which the NPC 1120 was deposited. In contrast, the second portion 702 on which no such NPC 1120 is deposited will continue to present an exposed layer surface 111 (of the base substrate 110) with an affinity for deposition of the conductive coating 830 thereon whose nucleation-inhibiting or, alternatively, nucleation-promoting properties are substantially unchanged (in either case, the exposed layer surface 111 of the base substrate 110 substantially free of NPC 1120).
[0218] In some non-limiting examples, both NIC 810 and NPC 1120 can be selectively deposited on respective first portion 701 and NPC portion 1103 ( FIG. 11A ) of exposed layer surface 111 of the base material to respectively modify the nucleation-inhibiting properties (and / or conversely, nucleation-promoting properties) of exposed layer surface 111 as presented for depositing conductive coating 830 thereon. In some non-limiting examples, there may be a second portion 702 of exposed layer surface 111 of the base material on which selective coating 710 is not deposited, such that the nucleation-inhibiting properties (and / or conversely, the nucleation-promoting properties) as presented for depositing conductive coating 830 thereon are not substantially modified.
[0219] In some non-limiting examples, first portion 701 and NPC portion 1103 may overlap such that a first coating of NIC 810 and / or NPC 1120 can be selectively deposited on the exposed layer surface 111 of the base material in such overlapping areas, and a second coating of NIC 810 and / or NPC 1120 can be selectively deposited on the treated exposed layer surface 111 of the first coating. In some non-limiting examples, the first coating is NIC 810. In some non-limiting examples, the first coating is NPC 1120.
[0220] In some non-limiting examples, the first portion 701 (and / or NPC portion 1103) on which the selective coating 710 is deposited can include a removal area where the deposited selective coating 710 has been removed, presenting an uncoated surface of the base material for depositing the conductive coating 830 thereon such that its nucleation-inhibiting properties (and / or conversely, its nucleation-promoting properties) are not substantially altered as presented for depositing the conductive coating 830 thereon.
[0221] In some non-limiting examples, the base material may be at least one layer selected from the substrate 110, and / or at least one of the front plane 10 layers, including but not limited to the first electrode 120, the second electrode 140, the at least one semiconductive layer 130 (and / or at least one of the layers), and / or any combination of any of these.
[0222] In some non-limiting examples, conductive coating 830 can have specific material properties. In some non-limiting examples, conductive coating 830 can include Mg, whether alone or in compounds and / or alloys.
[0223] As a non-limiting example, pure and / or substantially pure Mg may not be easily deposited on some organic surfaces due to the low sticking probability S of Mg on some organic surfaces.
[0224] Selective Coating Deposition In some non-limiting examples, thin films including selective coating 710 may be selectively deposited and / or processed using a variety of techniques, including, but not limited to, evaporation (including, but not limited to, thermal evaporation and / or electron beam evaporation), photolithography, printing (including, but not limited to, inkjet and / or evaporative jet printing, reel-to-reel printing, and / or microcontact transfer printing), PVD (including, but not limited to, sputtering), CVD (including, but not limited to, PECVD and / or OVPD), laser annealing, LTI patterning, ALD, coating (including, but not limited to, spin coating, dip coating, line coating, and / or spray coating), and / or combinations of any two or more thereof.
[0225] FIG. 7 is an example schematic diagram illustrating a non-limiting example of an evaporation process, generally designated 700, in a chamber 70 for selectively depositing a selective coating 710 on a first portion 701 of an exposed layer surface 111 of a base material (shown here only as a substrate 110 for ease of illustration).
[0226] In process 700, a quantity of selective coating material 711 is heated under vacuum to evaporate and / or sublimate 712 the selective coating material 711. In some non-limiting examples, the selective coating material 711 comprises entirely and / or substantially the material used to form the selective coating 710. The evaporated selective coating material 712 is directed through chamber 70 toward exposed layer surface 111, including in the direction indicated by arrow 71. As the evaporated selective coating material 712 impinges on exposed layer surface 111, i.e., in first portion 701, selective coating 710 is formed thereon.
[0227] In certain non-limiting examples, as shown in the figures for process 700, selective coating 710 may be selectively deposited only on a portion of exposed layer surface 111, first portion 701 in the illustrated example, by inserting a shadow mask 715, which in certain non-limiting examples may be an FMM, between the selective coating material 711 and exposed layer surface 111. Shadow mask 715 has at least one aperture 716 extending therethrough such that a portion of evaporated selective coating material 712 passes through aperture 716 and impinges on exposed layer surface 111 to form selective coating 710. If evaporated selective coating material 712 does not pass through aperture 716 and impinges on surface 717 of shadow mask 715, it is prevented from being disposed on exposed layer surface 111 to form selective coating 710 in second portion 703. Thus, second portion 702 of exposed layer surface 111 is substantially free of selective coating 710. In some non-limiting examples (not shown), selective coating material 711 incident on shadow mask 715 may be deposited on its surface 717 .
[0228] Thus, a patterned surface is created upon completion of deposition of selective coating 710.
[0229] In some non-limiting examples, for ease of illustration, the selective coating 710 employed in Figure 7 may be NIC810. In some non-limiting examples, for ease of illustration, the selective coating 710 employed in Figure 7 may be NPC1120.
[0230] 8 is an example schematic diagram illustrating non-limiting examples of the results of an evaporation process, generally designated 800, within chamber 70 for selectively depositing a conductive coating 830 on a second portion 702 of an exposed layer surface 111 of a base material (shown here, for ease of illustration, only substrate 110) that is substantially free of NIC 810 selectively deposited on a first portion 701, including but not limited to by evaporation process 700 of FIG. 7. In some non-limiting examples, second portion 702 includes that portion of exposed layer surface 111 that is located beyond first portion 701.
[0231] Once NIC 810 is deposited on a first portion 701 of the exposed layer surface 111 of the base material (in the figure, substrate 110), a conductive coating 830 may be deposited on a second portion 702 of the exposed layer surface 111 that is substantially free of NIC 810.
[0232] In process 800, a quantity of conductive coating material 831 is heated under vacuum to evaporate and / or sublimate 832 the conductive coating 831. In some non-limiting examples, the conductive coating material 831 comprises entirely and / or substantially the material used to form the conductive coating 830. The evaporated conductive coating material 832 is directed inside the chamber 70, including in the direction indicated by arrow 81, toward the exposed layer surface 111 of the first portion 701 and the second portion 702. As the evaporated conductive coating material 832 impinges on the second portion 702 of the exposed layer surface 111, the conductive coating 830 is formed thereon.
[0233] In some non-limiting examples, deposition of the conductive coating material 831 can be performed using an open-mask deposition process and / or a mask-free deposition process such that the conductive coating 830 is formed substantially over the entire exposed layer surface 111 of the base material (shown as substrate 110) to produce a treated surface (of the conductive coating 830).
[0234] Those skilled in the art will understand that, as opposed to the size of the FMM, the size of the features of the open mask is generally comparable to the size of the device 100 being manufactured. In some non-limiting examples, such an open mask may have an aperture that may generally correspond to the size of the device 100, which may correspond, in some non-limiting examples, to about 1 inch for a microdisplay, about 4-6 inches for a mobile display, and / or about 8-17 inches for a laptop and / or tablet display, in order to mask the edges of such device 100 during manufacturing. In some non-limiting examples, the size of the features of the open mask may be on the order of about 1 cm or larger. In some non-limiting examples, the aperture formed in the open mask may be sized to encompass the lateral sides 410 of the multiple emissive regions 1910, each corresponding to a (sub)pixel 340 / 264x, and / or the surrounding and / or lateral sides 420 of the surrounding and / or intervening non-emissive regions 1920.
[0235] Those skilled in the art will appreciate that in some non-limiting examples, the use of an open mask may be omitted if desired. In some non-limiting examples, the open mask deposition processes described herein may alternatively be performed without the use of an open mask, such that the entire target exposure layer surface 111 is exposed.
[0236] In some non-limiting examples, as shown in the figures for process 800, deposition of conductive coating 830 can be performed using an open-mask deposition process and / or a mask-free deposition process such that conductive coating 830 is formed substantially over the entire exposed layer surface 111 of the base material (in the figure, of substrate 110) to produce a treated surface (of conductive coating 830).
[0237] In fact, as shown in FIG. 8, the evaporated conductive coating material 832 is incident on both the exposed layer surface 111 of the NIC 810 over the first portion 701 and the exposed layer surface 111 of the substrate 110 over the second portion 702 that is substantially free of the NIC 810.
[0238] Because the exposed layer surface 111 of the NIC 810 in the first portion 701 exhibits a relatively low initial sticking probability S for the conductive coating 830 compared to the exposed layer surface 111 of the substrate 110 in the second portion 702, the conductive coating 830 is deposited substantially selectively only on the exposed layer surface 111 of the substrate 110 in the second portion 702, which is substantially free of the NIC 810. In contrast, evaporated conductive coating material 832 incident on the exposed layer surface 111 of the NIC 810 across the first portion 701 tends not to be deposited as shown (833), leaving the exposed layer surface 111 of the NIC 810 across the first portion 701 substantially free of the conductive coating 830.
[0239] In some non-limiting examples, the initial deposition rate of evaporated conductive coating material 832 on the exposed layer surface 111 of substrate 110 in second portion 702 may be at least about 200 times and / or more, at least about 550 times and / or more, at least about 900 times and / or more, at least about 1,000 times and / or more, at least about 1,500 times and / or more, at least about 1,900 times and / or more, and / or about 2,000 times and / or more than the initial deposition rate of evaporated conductive coating material 832 on the exposed layer surface 111 of NIC 810 in first portion 701.
[0240] The foregoing can be combined to result in the selective deposition of at least one conductive coating 830 to form device features including, but not limited to, patterned electrodes 120, 140, 1750, 4150, and / or conductive elements electrically coupled thereto, without employing FMM within the conductive coating 830 deposition process. In some non-limiting examples, such patterning can allow and / or enhance transparency of device 100.
[0241] In some non-limiting examples, the selective coating 710, which may be NIC 810 and / or NPC 1120, may be applied multiple times during the manufacturing process of the device 100 to pattern device features including multiple electrodes 120, 140, 1750, 4150, and / or various layers thereof, and / or conductive coatings 830 electrically coupled thereto.
[0242] 9A-9D show non-limiting examples of open masks.
[0243] 9A shows a non-limiting example of an open mask 900 having and / or defining an aperture 910 formed therein. In some non-limiting examples as shown, the aperture 910 of the open mask 900 is smaller than the size of the device 100, such that when the mask 900 is overlaid on the device 100, the mask 900 covers the edges of the device 100. In some non-limiting examples, as shown, the lateral sides 410 of the light-emitting regions 1910 corresponding to all and / or substantially all of the (sub)pixels 340 / 264x of the device 100 are exposed through the aperture 910, while unexposed regions 920 are formed between the outer edge 91 of the device 100 and the aperture 910. Those skilled in the art will understand that in some non-limiting examples, electrical contacts and / or other components (not shown) of the device 100 can be positioned in such unexposed regions 920, such that these components remain substantially unaffected throughout the open mask deposition process.
[0244] 9B shows non-limiting examples of an open mask 901 having and / or defining an aperture 911 formed therein that is smaller than the aperture 910 of FIG. 9A such that when the mask 901 is overlaid on the device 100, the mask 901 covers at least the lateral sides 410 a of the light-emitting regions 1910 corresponding to at least some of the (sub)pixels 340 / 264x. As shown, in some non-limiting examples, the lateral sides 410 a of the light-emitting regions 1910 corresponding to the outermost (sub)pixels 340 / 264x are positioned within the non-exposed regions 913 of the device 100 formed between the outer edge 91 of the device 100 and the aperture 911 and are masked during the open mask deposition process to inhibit evaporated conductive coating material 832 from impinging on the non-exposed regions 913.
[0245] 9C shows a non-limiting example of an open mask 902 having and / or defining apertures 912 formed therein that define a pattern that covers lateral sides 410 a of light-emitting regions 1910 corresponding to at least some of (sub)pixels 340 / 264 x while exposing lateral sides 410 b of light-emitting regions 1910 corresponding to at least some of (sub)pixels 340 / 264 x. As shown, in some non-limiting examples, lateral sides 410 a of light-emitting regions 1910 corresponding to at least some of (sub)pixels 340 / 264 x positioned within non-exposed regions 914 of device 100 are masked during the open mask deposition process to inhibit evaporated conductive coating material 830 from impinging on non-exposed regions 914.
[0246] In Figures 9B-9C, as illustrated, the lateral sides 410a of the light-emitting regions 1910 corresponding to at least some of the outermost (sub)pixels 340 / 264x are masked, but those skilled in the art will understand that in some non-limiting examples, the apertures of the open masks 900-902 may be shaped to mask the lateral sides 410 of other light-emitting regions 1910 and / or the lateral sides 420 of non-light-emitting regions 1920 of the device 100.
[0247] Furthermore, although Figures 9A-9C show open masks 900-902 having a single aperture 910-912, those skilled in the art will understand that such open masks 900-902 may, in some non-limiting examples (not shown), have additional apertures (not shown) for exposing multiple areas of the exposed layer surface 111 of the base material of the device 100.
[0248] 9D shows a non-limiting example of an open mask 903 having and / or defining a plurality of apertures 917a-917d. The apertures 917a-917d, in some non-limiting examples, are positioned such that they can selectively expose certain regions 921 of the device 100 while masking other regions 922. In some non-limiting examples, the lateral sides 410b of certain light-emitting regions 1910 corresponding to at least some of the (sub)pixels 340 / 264x are exposed through the apertures 917a-917d within the region 921, while the lateral sides 410a of other light-emitting regions 1910 corresponding to at least one of some of the (sub)pixels 340 / 264x are located within the region 922 and are therefore masked.
[0249] Referring now to FIG. 10, there is shown an example of a version 1000 of device 100 shown in FIG. 1 but with many additional deposition steps as described herein.
[0250] Device 1000 shows a lateral profile of exposed layer surface 111 of a base material. The lateral profile includes a first portion 1001 and a second portion 1002. In first portion 1001, NIC 810 is disposed on exposed layer surface 111. However, in second portion 1002, exposed layer surface 111 is substantially free of NIC 810.
[0251] After selective deposition of NIC 810 over first portion 1001, a conductive coating 830 is deposited on device 1000 using, in some non-limiting examples, an open-mask deposition process and / or a mask-free deposition process, but remains substantially only within second portion 1002, which is substantially free of NIC 810.
[0252] The NIC 810 provides a surface in the first portion 1001 with a relatively low initial sticking probability S0 for the conductive coating 830 that is substantially lower than the initial sticking probability S0 for the conductive coating 830 on the exposed layer surface 111 of the underlying material of the device 1000 in the second portion 1002.
[0253] Thus, the first portion 1001 is substantially free of the conductive coating 830 .
[0254] In this manner, the NIC 810 may be selectively deposited, including using a shadow mask, to allow the conductive coating 830 to be deposited, including but not limited to, using an open mask deposition process and / or a mask-free deposition process, to form device features including, but not limited to, at least one of the first electrode 120, the second electrode 140, the auxiliary electrode 1750, the bus bar 4150, and / or at least one layer thereof, and / or conductive elements electrically coupled thereto.
[0255] 11A-11B show a non-limiting example of an evaporation process generally designated 1100 in chamber 70 for selectively depositing a conductive coating 830 on a second portion 702 of an exposed layer surface 111 of a base material (shown in the figures, for ease of illustration, only substrate 110) that is substantially free of NIC 810 selectively deposited on the first portion 701, and on an NPC portion 1103 of the first portion 701 on which NIC 810 has been deposited, including but not limited to by evaporation process 700 of FIG.
[0256] 11A illustrates stage 1101 of process 1100, in which, once NIC 810 is deposited on a first portion 701 of an exposed layer surface 111 of a base material (shown as substrate 110), NPC 1120 can be deposited on NPC portion 1103 of the exposed layer surface 111 of NIC 810 deposited on substrate 110 within first portion 701. In the figure, as a non-limiting example, NPC portion 1103 extends completely within first portion 701.
[0257] In step 1101, a quantity of NPC material 1121 is heated under vacuum to evaporate and / or sublimate 1122 the NPC material 1121. In some non-limiting examples, the NPC material 1121 completely and / or substantially comprises the material used to form the NPC 1120. The evaporated NPC material 1122 is directed through the chamber 70 toward the first portion 701 and the exposed layer surface 111 of the NPC portion 1103, including in the direction indicated by arrow 1110. As the evaporated NPC material 1122 impinges on the NPC portion 1103 of the exposed layer surface 111, the NPC 1120 is formed thereon.
[0258] In some non-limiting examples, deposition of the NPC material 1121 can be performed using open-mask deposition techniques and / or mask-free deposition techniques, such that the NPC 1120 is formed substantially across the entire exposed layer surface 111 of the base material (which in the figure may be the NIC 810 across the first portion 701 and / or the substrate 110 through the second portion 702) to produce a treated surface (of the NPC 1120).
[0259] In some non-limiting examples, as shown in the figures for stage 1101, NPC 1120 may be selectively deposited in part, in the example shown, only on NPC portion 1103 of exposed layer surface 111 (of NIC 810 in the figure), by inserting a shadow mask 1125, which in some non-limiting examples may be an FMM, between NPC material 1121 and exposed layer surface 111. Shadow mask 1125 has at least one aperture 1126 extending therethrough such that a portion of evaporated NPC material 1122 passes through aperture 1126 and impinges on exposed layer surface 111 (of only NIC 810 in NPC portion 1103 in the figure, as a non-limiting example) to form NPC 1120. If evaporated NPC material 1122 does not pass through aperture 1126 and is incident on surface 1127 of shadow mask 1125, it is prevented from being disposed on exposed layer surface 111 to form NPC 1120. Thus, portion 1102 of exposed layer surface 111 located beyond NPC portion 1103 is substantially free of NPC 1120. In some non-limiting examples (not shown), evaporated NPC material 1122 incident on shadow mask 1125 may be deposited on its surface 1127.
[0260] Although the exposed layer surface 111 of the NIC 810 in the first portion 701 exhibits a relatively low initial adhesion probability S0 for the conductive coating 830, in some non-limiting examples, this may not necessarily be the case for the NPC coating 1120, such that the NPC coating 1120 is still selectively deposited on the exposed layer surface (in the figure, of the NIC 810) in the NPC portion 1103.
[0261] Thus, a patterned surface is generated upon completion of the deposition of NPC 1120.
[0262] FIG. 11B illustrates stage 1104 of process 1100, in which NIC 810 is deposited on a first portion 701 of the exposed layer surface 111 of the base material (in the figure, substrate 110) and NPC 1120 is deposited on the NPC portion 1103 of the exposed layer surface 111 (in the figure, of NIC 810), and then a conductive coating 830 can be deposited on the NPC portion 1103 and the second portion 702 of the exposed layer surface 111 (in the figure, substrate 110).
[0263] In step 1104, a quantity of conductive coating material 831 is heated under vacuum to evaporate and / or sublimate 832 the conductive coating 831. In some non-limiting examples, the conductive coating material 831 completely and / or substantially comprises the material used to form the conductive coating 830. The evaporated conductive coating material 832 is directed through the chamber 70 toward the exposed layer surfaces 111 of the first and second portions 701 and 702 of the NPC portion 1103, including in the direction indicated by arrow 1120. When the evaporated conductive coating material 832 impinges on the NPC portion 1103 of the exposed layer surface 111 (of the NPC 1120) and the second portion 702 of the exposed layer surface 111 (of the substrate 110), i.e., other than the exposed layer surface 111 of the NIC 810, the conductive coating 830 is formed thereon.
[0264] In some non-limiting examples, as shown in the figure for step 1104, deposition of the conductive coating 830 can be performed using an open-mask deposition process and / or a mask-free deposition process such that the conductive coating 830 is formed substantially over the entire exposed layer surface 111 of the base material (other than when the base material is NIC 810) to produce a treated surface (of the conductive coating 830).
[0265] In fact, as shown in FIG. 11B , the evaporated conductive coating material 832 impinges on both the exposed layer surface 111 of the NIC 810 over the first portion 701 located beyond the NPC portion 1103, as well as the exposed layer surface 111 of the NPC 1120 over the NPC portion 1103 and the exposed layer surface 111 of the substrate 110 over the second portion 702 that is substantially free of the NIC 810.
[0266] Because the exposed layer surface 111 of the NIC 810 in the first portion 701 located beyond the NPC portion 1103 exhibits a relatively low initial adhesion probability S0 for the conductive coating 830 compared to the exposed layer surface 111 of the substrate 110 in the second portion 702, and / or because the exposed layer surface 111 of the NPC 1120 in the NPC portion 1103 exhibits a relatively high initial adhesion probability S0 for the conductive coating 830 compared to both the exposed layer surface 111 of the NIC 810 in the first portion 701 located beyond the NPC portion 1103 and the exposed layer surface 111 of the substrate 110 in the second portion 702, the conductive coating 830 is deposited substantially selectively only on the exposed layer surface 111 of the substrate 110 in the NPC portion 1103 and the second portion 702, which is substantially free of NIC 810. In contrast, evaporated conductive coating material 832 incident on exposed layer surface 111 of NIC 810 over first portion 701 located beyond NPC portion 1103 tends not to be deposited as shown (1123), and exposed layer surface 111 of NIC 810 over first portion 701 located beyond NPC portion 1103 is substantially free of conductive coating 830.
[0267] Thus, a patterned surface is created upon completion of deposition of conductive coating 830.
[0268] 12A-12C show a non-limiting example of an evaporation process, generally designated 1200, in chamber 70 for selectively depositing a conductive coating 830 onto a second portion 1202 (FIG. 12C) of the exposed layer surface 111 of the base material.
[0269] 12A illustrates stage 1201 of process 1200, in which a quantity of NPC material 1121 is heated under vacuum to evaporate and / or sublimate 1122 the NPC material 1121. In some non-limiting examples, NPC material 1121 entirely and / or substantially comprises the material used to form NPC 1120. Vaporized NPC material 1122 is directed through chamber 70 toward exposed layer surface 111 (shown as substrate 110), including in the direction indicated by arrow 1210.
[0270] In some non-limiting examples, deposition of the NPC material 1121 can be performed using an open-mask deposition process and / or a mask-free deposition process such that the NPC 1120 is formed substantially over the entire exposed layer surface 111 of the base material (in the figure, the substrate 110) to produce a treated surface (of the NPC 1120).
[0271] In some non-limiting examples, as shown in the figure for stage 1201, NPC 1120 can be selectively deposited, in part, only on NPC portion 1103 of exposed layer surface 111, in the example shown, by inserting a shadow mask 1125, which in some non-limiting examples can be an FMM, between NPC material 1121 and exposed layer surface 111. Shadow mask 1125 has at least one aperture 1126 extending therethrough such that a portion of evaporated NPC material 1122 passes through aperture 1126 and impinges on exposed layer surface 111 to form NPC 1120 in NPC portion 1103. If evaporated NPC material 1122 does not pass through aperture 1126 and impinges on surface 1127 of shadow mask 1125, it is prevented from being disposed on exposed layer surface 111 to form NPC 1120 in portion 1102 of exposed layer surface 111 located beyond NPC portion 1103. Thus, portion 1102 is substantially free of NPC 1120. In some non-limiting examples (not shown), NPC material 1121 incident on shadow mask 1125 may be deposited on surface 1127 thereof.
[0272] When evaporated NPC material 1122 impinges on exposed layer surface 111, ie, within NPC portion 1103, NPC 1120 is formed thereon.
[0273] Thus, a patterned surface is generated upon completion of the deposition of NPC 1120.
[0274] 12B illustrates stage 1202 of process 1200, in which, once NPC 1120 has been deposited onto NPC portion 1103 of exposed layer surface 111 of base material (shown as substrate 110), NIC 810 can be deposited onto first portion 701 of exposed layer surface 111. In the illustration, by way of non-limiting example, first portion 701 extends completely into NPC portion 1103. As a result, in the illustration, by way of non-limiting example, portion 1102 includes that portion of exposed layer surface 111 that lies beyond first portion 701.
[0275] In step 1202, a quantity of NIC material 1211 is heated under vacuum to evaporate and / or sublimate 1212 the NIC material 1211. In some non-limiting examples, the NIC material 1211 comprises entirely and / or substantially the material used to form the NIC 810. The evaporated NIC material 1212 is directed through chamber 70, including in the direction indicated by arrow 1220, toward first portion 701 of NPC portion 1103 extending beyond first portion 701 and toward exposed layer surface 111 of portion 1102. As the evaporated NIC material 1212 impinges on first portion 701 of exposed layer surface 111, NIC 810 is formed thereon.
[0276] In some non-limiting examples, deposition of the NIC material 1211 can be performed using an open-mask deposition process and / or a mask-free deposition process such that the NIC 810 is formed substantially over the entire exposed layer surface 111 of the base material to produce a treated surface (of the NIC 810).
[0277] In some non-limiting examples, as shown in the figures for stage 1202, NIC 810 can be selectively deposited, in part, on only a first portion 701 of exposed layer surface 111 (in the illustrated example, of NPC 1120) by inserting a shadow mask 1215, which in some non-limiting examples can be an FMM, between NIC material 1211 and exposed layer surface 111. Shadow mask 1215 has at least one aperture 1216 extending therethrough such that a portion of evaporated NIC material 1212 passes through aperture 1216 and impinges on exposed layer surface 111 (in the illustrated example, of NPC 1120, as a non-limiting example) to form NIC 810. If evaporated NIC material 1212 does not pass through aperture 1216 and impinges on surface 1217 of shadow mask 1215, it is prevented from being disposed on exposed layer surface 111 to form NIC 810 in a second portion 702 beyond first portion 701. Thus, the second portion 702 of the exposed layer surface 111 located beyond the first portion 701 is substantially free of the NIC 810. In some non-limiting examples (not shown), evaporated NIC material 1212 incident on the shadow mask 1215 may be deposited on its surface 1217.
[0278] Although the exposed layer surface 111 of the NPC 1120 in the NPC portion 1103 exhibits a relatively high initial sticking probability S for the conductive coating 830, in some non-limiting examples, this may not necessarily be the case for the NIC coating 810. Even so, in some non-limiting examples, such affinity for the NIC coating 810 can still cause the NIC coating 810 to be selectively deposited on the exposed layer surface 111 (of the NPC 1120 in the figure) in the first portion 701.
[0279] Thus, a patterned surface is created upon completion of the deposition of NIC 810.
[0280] Figure 12C illustrates stage 1204 of process 1200, in which once NIC 810 has been deposited on a first portion 701 of the exposed layer surface 111 of the base material (shown as NPC 1120), a conductive coating 830 can be deposited on a second portion 702 of the exposed layer surface 111 (shown as NPC 1120 over portion 1102 of the substrate 110 that extends beyond NPC portion 1103, and NPC 1120 over NPC portion 1103 that extends beyond first portion 701).
[0281] In step 1204, a quantity of conductive coating material 831 is heated under vacuum to evaporate and / or sublimate 832 the conductive coating 831. In some non-limiting examples, the conductive coating material 831 completely and / or substantially comprises the material used to form the conductive coating 830. The evaporated conductive coating material 832 is directed through the chamber 70, including in the direction indicated by arrow 1230, toward the first portion 701 of the NPC portion 1103 and the exposed layer surface 111 of the portion 1102 beyond the NPC portion 1103. When the evaporated conductive coating material 832 impinges on the NPC portion 1103 of the exposed layer surface 111 (of the NPC 1120) beyond the first portion 701 and the portion 1102 of the exposed layer surface 111 (of the substrate 110) beyond the NPC portion 1103, i.e., the second portion 702 other than the exposed layer surface 111 of the NIC 810, the conductive coating 830 is formed thereon.
[0282] In some non-limiting examples, as shown in the figure for step 1204, deposition of the conductive coating 830 can be performed using an open-mask deposition process and / or a mask-free deposition process such that the conductive coating 830 is formed substantially over the entire exposed layer surface 111 of the base material (other than when the base material is NIC 810) to produce a treated surface (of the conductive coating 830).
[0283] In fact, as shown in FIG. 12C , the evaporated conductive coating material 832 is incident on both the exposed layer surface 111 of the NIC 810 over the first portion 701 located within the NPC portion 1103, as well as the exposed layer surface 111 of the NPC 1120 over the NPC portion 1103 located beyond the first portion 701 and the exposed layer surface 111 of the substrate 110 over the portion 1102 located beyond the NPC portion 1103.
[0284] Because the exposed layer surface 111 of the NIC 810 in the first portion 701 exhibits a relatively low initial adhesion probability S0 for the conductive coating 830 compared to the exposed layer surface 111 of the substrate 110 in the second portion 702 located beyond the NPC portion 1103, and / or because the exposed layer surface 111 of the NPC 1120 in the NPC portion 1103 located beyond the first portion 701 exhibits a relatively high initial adhesion probability S0 for the conductive coating 830 compared to both the exposed layer surface 111 of the NIC 810 in the first portion 701 and the exposed layer surface 111 of the substrate 110 in the portion 1102 located beyond the NPC portion 1103, the conductive coating 830 is deposited substantially selectively only on the NPC portion 1103 located beyond the first portion 701 and the exposed layer surface 111 of the substrate 110 in the portion 1102 located beyond the NPC portion 1103, which are substantially free of NIC 810. In contrast, evaporated conductive coating material 832 incident on exposed layer surface 111 of NIC 810 over first portion 701 tends not to be deposited as shown (1233), and exposed layer surface 111 of NIC 810 over first portion 701 is substantially free of conductive coating 830.
[0285] Thus, a patterned surface is created upon completion of deposition of conductive coating 830.
[0286] In some non-limiting examples, the initial deposition rate of evaporated conductive coating material 832 on the exposed layer surface 111 in second portion 702 may be at least about 200 times and / or more, at least about 550 times and / or more, at least about 900 times and / or more, at least about 1,000 times and / or more, at least about 1,500 times and / or more, at least about 1,900 times and / or more, and / or about 2,000 times and / or more than the initial deposition rate of evaporated conductive coating material 832 on the exposed layer surface 111 of NIC 810 in first portion 701.
[0287] 13A-13C illustrate a non-limiting example of a printing process, generally designated 1300, for selectively depositing a selective coating 710, which may be NIC810 and / or NPC1120 in some non-limiting examples, onto an exposed layer surface 111 of a base material (shown here as substrate 110 only, for ease of illustration).
[0288] 13A illustrates a stage in process 1300 in which a stamp 1310 having protrusions 1311 thereon is provided with a selective coating 710 on an exposed layer surface 1312 of the protrusions 1311. Those skilled in the art will appreciate that the selective coating 710 can be deposited and / or deposited on the protrusion surface 1312 using a variety of suitable mechanisms.
[0289] FIG. 13B illustrates a stage of process 1300 in which stamp 1310 is brought into close proximity 1301 with exposed layer surface 111 such that selective coating 710 contacts and adheres to exposed layer surface 111.
[0290] FIG. 13C illustrates a stage in the process 1300 in which the stamp 1310 is moved 1303 away from the exposed layer surface 111 , leaving behind the selective coating 710 deposited on the exposed layer surface 111 .
[0291] Selective deposition of patterned electrodes The foregoing can be combined to provide selective deposition of at least one conductive coating 830 to form patterned electrodes 120, 140, 1750, 4150, which in some non-limiting examples may be second electrodes 140 and / or auxiliary electrodes 1750, without employing FMM within the high temperature conductive coating 830 deposition process. In some non-limiting examples, such patterning can allow and / or enhance transparency of the device 100.
[0292] 14 shows an example of a patterned electrode 1400 in plan view, shown as a second electrode 140 suitable for use in an example version 1500 of device 100 (FIG. 15). Electrode 1400 is formed with a pattern 1410 that includes a single continuous structure having or defining a plurality of patterned apertures 1420 therein, where apertures 1420 correspond to areas of device 100 that are free of cathode 342.
[0293] In the figure, as a non-limiting example, pattern 1410 is disposed across the entire lateral extent of device 1500, without distinguishing between lateral sides 410 of emissive regions 1910 corresponding to (sub)pixel 340 / 264x and lateral sides 420 of non-emissive regions 1920 surrounding such emissive regions 1910. The example shown can therefore correspond to device 1500, as disclosed herein, that is substantially transparent to light incident on the external surface of device 1500, such that a significant portion of such externally incident light can be transmitted through device 1500 in addition to photon emissions generated internally within device 1500 (in top-emitting, bottom-emitting, and / or dual-sided emission).
[0294] The transparency of the device 1500 can be adjusted and / or tuned by varying the pattern 1410 employed, including but not limited to the average size of the apertures 1420 and / or the spacing and / or density of the apertures 1420.
[0295] 15, which illustrates a cross-sectional view of a device 1500 taken along line 15-15 of FIG. 14. The device 1500 is shown in the figure as including a substrate 110, a first electrode 120, and at least one semiconductive layer 130. In some non-limiting examples, an NPC 1120 is disposed on substantially all of the exposed layer surface 111 of the at least one semiconductive layer 130. In some non-limiting examples, the NPC 1120 can be omitted.
[0296] The NIC 810 is selectively disposed in a pattern that substantially corresponds to the pattern 1410 on the exposed layer surface 111 of the base material, which is the NPC 1120 (but in some non-limiting examples may be at least one semiconductive layer 130 if the NPC 1120 is omitted), as shown in the figure.
[0297] In the figure, a conductive coating 830 suitable for forming a patterned electrode 1400, which is the second electrode 140, is disposed on substantially all of the exposed layer surface 111 of the base material using an open-mask deposition process and / or a mask-free deposition process that does not employ any FMM during the high-temperature conductive coating deposition process. The base material includes both areas of NIC 810 disposed in pattern 1410 and areas of NPC 1120 in pattern 1410 where no NIC 810 is deposited. In some non-limiting examples, the area of NIC 810 can substantially correspond to a first portion including aperture 1420 shown in pattern 1410.
[0298] Due to the nucleation-inhibiting properties of those areas of pattern 1410 where NIC 810 is disposed (corresponding to apertures 1420), the conductive coating 830 disposed on such areas tends not to remain, resulting in a pattern of selective deposition of conductive coating 830 that substantially corresponds to the remainder of pattern 1410, while leaving those areas of the first portion of pattern 1410 corresponding to apertures 1420 substantially free of conductive coating 830.
[0299] In other words, the conductive coating 830 forming the cathode 342 is deposited substantially selectively only on the second portion, including those areas of the NPC 1120 that surround but do not occupy the apertures 1420 in the pattern 1410.
[0300] FIG. 16A shows a schematic diagram showing multiple patterns 1620, 1640 of electrodes 120, 140, 1750 in plan view.
[0301] In some non-limiting examples, the first pattern 1620 includes a plurality of elongated spaced apart regions extending in a first laterally direction. In some non-limiting examples, the first pattern 1620 can include a plurality of first electrodes 120. In some non-limiting examples, the multiple regions making up the first pattern 1620 can be electrically coupled.
[0302] In some non-limiting examples, the second pattern 1640 includes a plurality of elongated spaced apart regions extending in a second lateral direction. In some non-limiting examples, the second lateral direction can be substantially perpendicular to the first lateral direction. In some non-limiting examples, the second pattern 1640 can include a plurality of second electrodes 140. In some non-limiting examples, the multiple regions making up the second pattern 1640 can be electrically coupled.
[0303] In some non-limiting examples, the first pattern 1620 and the second pattern 1640 may form part of an example version of device 100, generally shown at 1600 (FIG. 16C), which may include multiple PMOLED elements.
[0304] In some non-limiting examples, the lateral side 410 of the emissive region 1910 corresponding to (sub)pixel 340 / 264x is formed by the overlap of the first pattern 1620 with the second pattern 1640. In some non-limiting examples, the lateral side 420 of the non-emissive region 1920 corresponds to any lateral side other than the lateral side 410.
[0305] In some non-limiting examples, a first terminal, which in some non-limiting examples may be a positive terminal of the power source 15, is electrically coupled to at least one electrode 120, 140, 1750 of the first pattern 1620. In some non-limiting examples, the first terminal is coupled to at least one electrode 120, 140, 1750 of the first pattern 1620 through at least one drive circuit 300. In some non-limiting examples, a second terminal, which in some non-limiting examples may be a negative terminal of the power source 15, is electrically coupled to at least one electrode 120, 140, 1750 of the second pattern 1640. In some non-limiting examples, the second terminal is coupled to at least one electrode 120, 140, 1750 of the second pattern 1740 through at least one drive circuit 300.
[0306] 16B, which shows a cross-sectional view of device 1600 at deposition stage 1600b taken along line 16B-16B of FIG. 16A. Device 1600 at stage 1600b is shown in the figure as including substrate 110. In some non-limiting examples, NPC 1120 is disposed on exposed layer surface 111 of substrate 110. In some non-limiting examples, NPC 1120 can be omitted.
[0307] The NICs 810 are selectively disposed in a pattern that substantially corresponds to the inverse of the first pattern 1620 on the exposed layer surface 111 of the base material, which is NPC 1120, as shown.
[0308] In the figure, a conductive coating 830 suitable for forming a first pattern 1620 of electrodes 120, 140, 1750, which is the first electrode 120, is disposed on substantially all of the exposed layer surface 111 of the base material using an open-mask deposition process and / or a mask-free deposition process that does not employ any FMM during the high-temperature conductive coating deposition process. The base material includes both regions of NIC 810 disposed inversely to the first pattern 1620 and regions of NPC 1120 disposed in the first pattern 1620 where no NIC 810 is deposited. In some non-limiting examples, the regions of NPC 1120 can substantially correspond to the elongated spaced apart regions of the first pattern 1620, while the regions of NIC 810 can substantially correspond to the first portion including the gap therebetween.
[0309] Due to the nucleation-inhibiting properties of those regions of the first pattern 1620 where the NIC 810 is disposed (corresponding to the gaps therebetween), the conductive coating 830 disposed on such regions tends not to remain, resulting in a pattern of selective deposition of the conductive coating 830 that substantially corresponds to the elongated spaced regions of the first pattern 1620, while leaving a first portion including the gaps therebetween that is substantially free of the conductive coating 830.
[0310] In other words, the conductive coating 830 forming the first pattern 1620 of the electrodes 120, 140, 1750 is deposited substantially selectively only on the second portion including those regions of the NPC 1120 (or, in some non-limiting examples, the substrate 110 if the NPC 1120 is omitted) that define the elongated spaced apart regions of the first pattern 1620.
[0311] 16C, which shows a cross-sectional view of device 1600 taken along line 16C-16C of FIG. 16A, device 1600 is shown as including substrate 110, a first pattern 1620 of electrodes 120 deposited as shown in FIG. 16B, and at least one semiconducting layer 130.
[0312] In some non-limiting examples, at least one semiconductive layer 130 can be provided as a common layer across substantially all of the lateral sides of device 1600 .
[0313] In some non-limiting examples, the NPC 1120 is disposed on substantially all of the exposed layer surface 111 of the at least one semiconductive layer 130. In some non-limiting examples, the NPC 1120 can be omitted.
[0314] The NIC 810 is selectively disposed in a pattern that substantially corresponds to a second pattern 1640 on the exposed layer surface 111 of the base material, which is the NPC 1120 as shown (but in some non-limiting examples may be at least one semiconductive layer 130 if the NPC 1120 is omitted).
[0315] In the figure, a conductive coating 830 suitable for forming a second pattern 1640 of electrodes 120, 140, 1750, which is second electrode 140, is disposed on substantially all of the exposed layer surface 111 of the base material using an open-mask deposition process and / or a mask-free deposition process that does not employ any FMM during the high-temperature conductive coating deposition process. The base material includes both regions of NIC 810 disposed inversely of the second pattern 1640 and regions of NPC 1120 in the second pattern 1640 where no NIC 810 is deposited. In some non-limiting examples, the regions of NPC 1120 can substantially correspond to first portions, including elongated spaced apart regions, of second pattern 1640, while the regions of NIC 810 can substantially correspond to the gaps therebetween.
[0316] Due to the nucleation-inhibiting properties of those regions of the second pattern 1640 where the NIC 810 is disposed (corresponding to the gaps therebetween), the conductive coating 830 disposed on such regions tends not to remain, resulting in a pattern of selective deposition of the conductive coating 830 that substantially corresponds to the elongated spaced regions of the second pattern 1640, while leaving the first portion including the gaps therebetween that are substantially free of the conductive coating 830.
[0317] In other words, the conductive coating 830 forming the second pattern 1640 of the electrodes 120, 140, 1750 is deposited substantially selectively only on the second portion including those areas of the NPC 1120 that define the elongated spaced apart areas of the second pattern 1640.
[0318] In some non-limiting examples, the thickness of the NIC 810 and the conductive coating 830 subsequently deposited to form either or both of the first pattern 1620 and / or second pattern 1640 of the electrodes 120, 140, 1750 can vary according to various parameters, including, but not limited to, the desired application and desired performance characteristics. In some non-limiting examples, the thickness of the NIC 810 can be comparable to and / or substantially less than the thickness of the subsequently deposited conductive coating 830. The use of a relatively thin NIC 810 to achieve selective patterning of the subsequently deposited conductive coating can be suitable for providing flexible devices 1600, including, but not limited to, PMOLED devices. In some non-limiting examples, the relatively thin NIC 810 can provide a relatively flat surface on which the barrier coating 1650 can be deposited. In some non-limiting examples, providing such a relatively flat surface for application of the barrier coating 1650 can enhance adhesion of the barrier coating 1650 to such surfaces.
[0319] At least one of the first patterns 1620 of the electrodes 120, 140, 1750 and at least one of the second patterns 1640 of the electrodes 120, 140, 1750 may be electrically coupled to a power source 15, whether directly and / or, in some non-limiting examples, through their respective drive circuits 300 for controlling photon emission from the lateral side 410 of the light-emitting region 1910 corresponding to the (sub)pixel 340 / 264x.
[0320] 16A-16C , the process for forming the second electrode 140 in the second pattern 1640 can be used in a similar manner to form the auxiliary electrode 1750 for the device 1600, in some non-limiting examples. In some non-limiting examples, the second electrode 140 can include a common electrode, and the auxiliary electrode 1750 can be deposited in the second pattern 1640 above the second electrode 140, in some non-limiting examples, or below the second electrode 140, in some non-limiting examples, to be electrically coupled to the second electrode 140. In some non-limiting examples, the second pattern 1640 for such an auxiliary electrode 1750 can be such that the elongated spaced apart regions of the second pattern 1640 are located substantially within the lateral sides 420 of the non-emissive regions 1920 that surround the lateral sides 410 of the emissive regions 1910 corresponding to the (sub)pixel 340 / 264x. In some non-limiting examples, the second pattern 1640 for such auxiliary electrode 1750 can be such that the elongated spaced apart regions of the second pattern 1640 are substantially located within the lateral sides 410 of the emissive regions 1910 corresponding to the (sub)pixels 340 / 264x and / or within the lateral sides 420 of the non-emissive regions 1920 surrounding them.
[0321] FIG. 17 shows an example cross-sectional view of an example version 1700 of device 100 that is substantially similar to device 100 but further includes at least one auxiliary electrode 1750 (not shown) arranged in the pattern described above and electrically coupled to second electrode 140.
[0322] The auxiliary electrode 1750 is electrically conductive. In some non-limiting examples, the auxiliary electrode 1750 may be formed of at least one metal and / or metal oxide. Non-limiting examples of such metals include Cu, Al, molybdenum (Mo), and / or Ag. As a non-limiting example, the auxiliary electrode 1750 may include a multilayer metal structure, including, but not limited to, one formed by Mo / Al / Mo. Non-limiting examples of such metal oxides include ITO, ZnO, IZO, and / or other oxides containing In and / or Zn. In some non-limiting examples, the auxiliary electrode 1750 may include a multilayer structure formed by a combination of at least one metal and at least one metal oxide, including, but not limited to, Ag / ITO, Mo / ITO, ITO / Ag / ITO, and / or ITO / Mo / ITO. In some non-limiting examples, the auxiliary electrode 1750 includes a plurality of such electrically conductive materials.
[0323] The device 1700 is shown as including a substrate 110 , a first electrode 120 , and at least one semiconducting layer 130 .
[0324] In some non-limiting examples, the NPC 1120 is disposed on substantially all of the exposed layer surface 111 of the at least one semiconductive layer 130. In some non-limiting examples, the NPC 1120 can be omitted.
[0325] A second electrode 140 is disposed on substantially all of the exposed layer surface 111 of the NPC 1120 (or of the at least one semiconductive layer 130 if the NPC 1120 is omitted).
[0326] In some non-limiting examples, particularly in top-emitting device 1700, second electrode 140 may be formed by depositing a relatively thin conductive film layer (not shown) to, by way of non-limiting example, reduce optical interference (including, but not limited to, attenuation, reflection, and / or diffusion) associated with the presence of second electrode 140. In some non-limiting examples, as discussed elsewhere, reducing the thickness of second electrode 140 may generally increase the sheet resistance of second electrode 140, which may, in some non-limiting examples, reduce the performance and / or efficiency of device 1700. By providing an auxiliary electrode 1750 electrically coupled to second electrode 140, the sheet resistance, and therefore the IR drop associated with second electrode 140, may be reduced in some non-limiting examples.
[0327] In some non-limiting examples, device 1700 may be a bottom-emitting and / or dual-sided emitting device 1700. In such examples, second electrode 140 may be formed as a relatively thick conductive layer without substantially affecting the optical characteristics of such device 1700. Nevertheless, even in such circumstances, second electrode 140 may nevertheless be formed, by way of non-limiting example, as a relatively thin conductive film layer (not shown), such that device 1700 may be substantially transparent to light incident on its external surface such that a significant portion of such external incident light can transmit through device 1700 in addition to photon emission generated internally within device 1700, as disclosed herein.
[0328] The NICs 810 are selectively disposed in a pattern on the exposed layer surface 111 of the base material, which is NPC 1120, as shown in the figures. In some non-limiting examples, the NICs 810 can be disposed in a first portion of the pattern as a series of parallel rows 1720, as shown in the figures.
[0329] A conductive coating 830 suitable for forming a patterned auxiliary electrode 1750 is disposed on substantially all of the exposed layer surface 111 of the base material using an open mask deposition process and / or a mask-free deposition process that does not employ any FMM during the high temperature conductive coating deposition process. The base material includes both areas of NIC 810 arranged in a pattern of rows 1720 and areas of NPC 1120 where no NIC 810 is deposited.
[0330] Due to the nucleation-inhibiting properties of those rows 1720 on which NIC 810 is disposed, the conductive coating 830 disposed on such rows 1720 tends not to remain, resulting in a pattern of selective deposition of conductive coating 830 that substantially corresponds to at least one second portion of the pattern while leaving a first portion including rows 1720 that are substantially free of conductive coating 830.
[0331] In other words, the conductive coating 830 forming the auxiliary electrode 1750 is deposited substantially selectively only on the second portion, including those areas of the NPC 1120 that surround but do not occupy the rows 1720 .
[0332] In some non-limiting examples, optical interference associated with the presence of the auxiliary electrodes 1750 can be controlled and / or reduced by selectively depositing the auxiliary electrodes 1750 so that only certain rows 1720 of the lateral sides of the device 1700 are covered, while other areas remain uncovered.
[0333] In some non-limiting examples, the auxiliary electrodes 1750 may be selectively deposited in a pattern that is not easily detectable by the naked eye from a normal viewing distance.
[0334] In some non-limiting examples, auxiliary electrode 1750 may be formed in a device other than an OLED device, including to reduce the effective resistance of the electrode in such a device.
[0335] Auxiliary electrode By employing selective coating 710, including but not limited to the process illustrated in FIG. 17, the ability to pattern electrodes 120, 140, 1750, 4150, including but not limited to the second electrode 140 and / or auxiliary electrode 1750, without employing FMM during the high temperature conductive coating 830 deposition process allows for numerous configurations of the auxiliary electrode 1750 to be deployed.
[0336] 18A shows in plan view a portion of an example version 1800 of device 100 having multiple emissive regions 1910a-1910j and at least one surrounding non-emissive region 1820. In some non-limiting examples, device 1800 may be an AMOLED device in which each of emissive regions 1910a-1910j corresponds to (sub)pixel 340 / 264x.
[0337] 18B-18D show examples of portions of device 1800 corresponding to adjacent light-emitting regions 1910a and 1910b, along with different configurations 1750b-1750d of auxiliary electrodes 1750 overlying adjacent light-emitting regions 1910a and 1910b, and a portion of at least one non-light-emitting region 1820 therebetween. In some non-limiting examples, although not explicitly shown in FIGS. 18B-18D, it is understood that second electrode 140 of device 1800 substantially covers at least both light-emitting regions 1910a and 1910b and a portion of at least one non-light-emitting region 1820 therebetween.
[0338] 18B , auxiliary electrode configuration 1750b is disposed between two adjacent light-emitting regions 1910a and 1910b and is electrically coupled to second electrode 140. In this example, auxiliary electrode configuration 1750b has a width α that is less than the separation distance δ between adjacent light-emitting regions 1910a and 1910b. As a result, a gap exists in at least one non-light-emitting region 1820 on each side of auxiliary electrode configuration 1750b. In some non-limiting examples, such an arrangement can reduce the likelihood that auxiliary electrode configuration 1750b will interfere with the optical output of device 1800, in some non-limiting examples, from at least one of light-emitting regions 1910a and 1910b. In some non-limiting examples, such an arrangement can be appropriate when auxiliary electrode configuration 1750b is relatively thick (in some non-limiting examples, greater than several hundred nm and / or on the order of several microns in thickness). In some non-limiting examples, the ratio of the height (thickness) of auxiliary electrode configuration 1750b to its width ("aspect ratio") may be greater than about 0.05, e.g., about 0.1 or greater, about 0.2 or greater, about 0.5 or greater, about 0.8 or greater, about 1 or greater, or about 2 or greater. As non-limiting examples, the height (thickness) of auxiliary electrode configuration 1750b may be greater than about 50 nm, e.g., about 80 nm or greater, about 100 nm or greater, about 200 nm or greater, about 500 nm or greater, about 700 nm or greater, about 1000 nm or greater, about 1500 nm or greater, about 1700 nm or greater, or about 2000 nm or greater.
[0339] 18C , auxiliary electrode configuration 1750c is disposed between two adjacent light-emitting regions 1910a and 1910b and is electrically coupled to second electrode 140. In this example, auxiliary electrode configuration 1750c has a width α that is substantially the same as the separation distance δ between adjacent light-emitting regions 1910a and 1910b. As a result, there is no gap in at least one non-light-emitting region 1820 on either side of auxiliary electrode configuration 1750c. In some non-limiting examples, such an arrangement may be appropriate when the separation distance δ between adjacent light-emitting regions 1910a and 1910b is relatively small, as in, for example, a high pixel density device 1800.
[0340] 18D , auxiliary electrode 1750d is disposed between two adjacent light-emitting regions 1910a and 1910b and is electrically coupled to second electrode 140. In this example, auxiliary electrode configuration 1750d has a width α that is greater than the separation distance δ between adjacent light-emitting regions 1910a and 1910b. As a result, a portion of auxiliary electrode configuration 1750d overlaps a portion of at least one of adjacent light-emitting regions 1910a and / or 1910b. While this figure illustrates the degree of overlap between auxiliary electrode configuration 1750d and each of adjacent light-emitting regions 1910a and 1910b, in some non-limiting examples, the degree of overlap and / or the profile of the overlap between auxiliary electrode configuration 1750d and at least one of adjacent light-emitting regions 1910a and 1910b can be varied and / or adjusted.
[0341] FIG. 19 shows a schematic diagram in plan view illustrating an example pattern 1950 of auxiliary electrodes 1750 formed as a grid superimposed on both the lateral sides 410 of an emissive region 1910, which may correspond to (sub)pixel 340 / 264x of example version 1900 of device 100, as well as the lateral sides 420 of a non-emissive region 1920 surrounding the emissive region 1910.
[0342] In some non-limiting examples, the auxiliary electrode pattern 1950 extends substantially over only some but not all of the lateral sides 420 of the non-emitting region 1920 so as not to substantially cover any of the lateral sides 410 of the emitting region 1910.
[0343] Those skilled in the art will understand that while the figures show the auxiliary electrode pattern 1950 as formed as a continuous structure such that all of its elements are physically connected and electrically coupled to each other and to at least one electrode 120, 140, 1750, 4150, which in some non-limiting examples may be the first electrode 120 and / or the second electrode 140, in some non-limiting examples the auxiliary electrode pattern 1950 may be provided as multiple individual elements of the auxiliary electrode pattern 1950 that remain electrically coupled to each other but are not physically coupled to each other. Even so, such individual elements of the auxiliary electrode pattern 1950 may still substantially lower the sheet resistance of the at least one electrode 120, 140, 1750, 4150 to which they are electrically coupled, and consequently the sheet resistance of the device 1900, so as to increase the efficiency of the device 1900, without substantially interfering with their optical characteristics.
[0344] In some non-limiting examples, auxiliary electrodes 1750 may be employed in devices 100 having various arrangements of (sub)pixels 340 / 264x. In some non-limiting examples, the (sub)pixel 340 / 264x arrangement may be substantially diamond-shaped.
[0345] 20A shows in plan view a plurality of groups 2041-2043 of emissive regions 1910, each corresponding to a subpixel 264x, surrounded laterally by a plurality of non-emissive regions 1920 including PDLs 440 in a diamond configuration in example version 2000 of device 100. In some non-limiting examples, this configuration is defined by the pattern of emissive regions 1910 2041-2043 and the pattern of PDLs 440 in an alternating first and second row pattern.
[0346] In some non-limiting examples, the lateral sides 420 of the non-emitting regions 1920 including the PDLs 440 can be substantially elliptical. In some non-limiting examples, the major axes of the lateral sides 420 of the non-emitting regions 1920 in a first row are aligned and substantially perpendicular to the major axes of the lateral sides 420 of the non-emitting regions 1920 in a second row. In some non-limiting examples, the major axes of the lateral sides 420 of the non-emitting regions 1920 in a first row are substantially parallel to the axis of the first row.
[0347] In some non-limiting examples, the first group 2041 of emissive regions 1910 correspond to subpixels 264x that emit light at a first wavelength, and in some non-limiting examples, the subpixels 264x of the first group 2041 may correspond to red (R) subpixels 2641. In some non-limiting examples, the lateral sides 410 of the emissive regions 1910 of the first group 2041 may have a substantially diamond-shaped configuration. In some non-limiting examples, the emissive regions 1910 of the first group 2041 are in the pattern of a first row before and after the PDL 440. In some non-limiting examples, the lateral sides 410 of the emissive regions 1910 of the first group 2041 slightly overlap with the lateral sides 420 of the non-emissive regions 1920 before and after the PDL 440 in the same row, and with the lateral sides 420 of the adjacent non-emissive regions 1920 including the PDL 440 in the pattern before and after the second row.
[0348] In some non-limiting examples, the second group 2042 of light-emitting regions 1910 corresponds to subpixels 264x that emit light at a second wavelength, and in some non-limiting examples, the subpixels 264x of the second group 2042 may correspond to green (G) subpixels 2642. In some non-limiting examples, the lateral sides 410 of the light-emitting regions 1910 of the second group 2041 may have a substantially elliptical configuration. In some non-limiting examples, the light-emitting regions 1910 of the second group 2041 are located in a second row pattern before and after the PDL 440. In some non-limiting examples, the major axes of some of the lateral sides 410 of the light-emitting regions 1910 of the second group 2041 may be at a first angle, which in some non-limiting examples may be 45°, relative to the axis of the second row. In some non-limiting examples, the other major axis of the lateral side 410 of the light emitting regions 1910 of the second group 2041 may be at a second angle, which in some non-limiting examples may be substantially perpendicular to the first angle. In some non-limiting examples, the light emitting regions 1910 of the first group 2041 whose lateral sides 410 have a major axis at the first angle alternate with the light emitting regions 1910 of the first group 2041 whose lateral sides 410 have a major axis at the second angle.
[0349] In some non-limiting examples, the third group 2043 of emissive regions 1910 corresponds to subpixels 264x that emit light at a third wavelength, and in some non-limiting examples, the subpixels 264x of the third group 2043 may correspond to blue (B) subpixels 2643. In some non-limiting examples, the lateral sides 410 of the emissive regions 1910 of the third group 2043 may have a substantially diamond-shaped configuration. In some non-limiting examples, the emissive regions 1910 of the third group 2043 are in the pattern of the first row before and after the PDL 440. In some non-limiting examples, the lateral sides 410 of the emissive regions 1910 of the third group 2043 slightly overlap with the lateral sides 410 of the non-emissive regions 1920 before and after the PDL 440 in the same row, and with the lateral sides 420 of the adjacent non-emissive regions 1920 before and after the PDL 440 in the pattern of the second row. In some non-limiting examples, the second row pattern includes a first group 2041 of light emitting areas 1910, a third group 2043 of alternating light emitting areas 1910, each before and after a PDL 440.
[0350] Referring now to FIG. 20B, an example cross-sectional view of device 2000 is shown taken along line 20B-20B in FIG. 20A. In the figure, device 2000 is shown as including a substrate 110 and multiple elements of first electrode 120 formed on its exposed layer surface 111. Substrate 110 may include a base substrate 112 (not shown for ease of illustration) and / or at least one TFT structure 200 corresponding to and driving each subpixel 264x. PDLs 440 are formed across substrate 110 between elements of first electrode 120 to define emissive regions 1910 on each element of first electrode 120 separated by non-emissive regions 1920 including PDLs 440. In the figure, emissive regions 1910 all correspond to second group 2042.
[0351] In some non-limiting examples, at least one semiconductive layer 130 is deposited on each element of the first electrode 120 between the surrounding PDLs 440 .
[0352] In some non-limiting examples, a second electrode 140, which in some non-limiting examples may be a common cathode, may be deposited on the light-emitting region 1910 of the second group 2042 and on the surrounding PDL 440 to form its G (green) subpixel 2642.
[0353] In some non-limiting examples, NIC 810 is selectively deposited on the second electrode 140 over the lateral sides 410 of the emissive regions 1910 of the second group 2042 of G (green) subpixels 2642, enabling selective deposition of the conductive coating 830 over portions of the second electrode 140 that are substantially free of NIC 810, i.e., over the lateral sides 420 of the non-emissive regions 1920 that include the PDL 440. In some non-limiting examples, the conductive coating 830 may tend not to remain on the sloped portions of the PDL 440 but may tend to descend to the base of such sloped portions that are coated with NIC 810, such that the conductive coating 830 may tend to accumulate along the substantially flat portions of the PDL 440. In some non-limiting examples, the conductive coating 830 on the substantially flat portions of the PDL 440 may form at least one auxiliary electrode 1750 that may be electrically coupled to the second electrode 140.
[0354] In some non-limiting examples, device 2000 may include a capping layer and / or an outcoupling layer. By way of non-limiting example, such a capping layer and / or an outcoupling layer may be provided directly on the surface of second electrode 140 and / or on the surface of NIC 810. In some non-limiting examples, such a capping layer and / or an outcoupling layer may be provided across lateral sides 410 of at least one light-emitting region 1910 corresponding to (sub)pixel 340 / 264x.
[0355] In some non-limiting examples, the NIC 810 may also act as an index-matching coating. In some non-limiting examples, the NIC 810 may also act as an outcoupling layer.
[0356] In some non-limiting examples, device 2000 includes an encapsulation layer. Non-limiting examples of such encapsulation layers include a glass cap, a barrier film, a barrier adhesive, and / or a TFE layer 2050, as shown in dashed outline in the figure, provided to encapsulate device 2000. In some non-limiting examples, TFE layer 2050 may be considered a type of barrier coating 1650.
[0357] In some non-limiting examples, an encapsulation layer may be disposed over at least one of second electrode 140 and / or NIC 810. In some non-limiting examples, device 2000 includes additional optical and / or structural layers, coatings, and components, including, but not limited to, polarizers, color filters, anti-reflective coatings, anti-glare coatings, cover glazing, and / or optically clear adhesives (OCAs).
[0358] 20C, which illustrates an example cross-sectional view of device 2000 taken along line 20C-20C of FIG. 20A. In the figure, device 2000 is shown as including substrate 110 and multiple elements of first electrode 120 formed on its exposed layer surface 111. PDLs 440 are formed across substrate 110 between the elements of first electrode 120 to define emissive regions 1910 on each element of first electrode 120 separated by non-emissive regions 1920 that include PDLs 440. In the figure, emissive regions 1910 alternately correspond to first groups 2041 and third groups 2043.
[0359] In some non-limiting examples, at least one semiconductive layer 130 is deposited on each element of the first electrode 120 between the surrounding PDLs 440 .
[0360] In some non-limiting examples, the second electrode 140, which in some non-limiting examples may be a common cathode, may be deposited on the light-emitting areas 1910 of the first group 2041 to form its R (red) subpixel 2641, on the light-emitting areas 1910 of the third group 2043 to form its B (blue) subpixel 2643, and on the surrounding PDL 440.
[0361] In some non-limiting examples, the NIC 810 is selectively deposited on the second electrode 140 over the lateral sides 410 of the emissive regions 1910 of the first group 2041 of R (red) subpixels 2641 and the third group 2643 of B (blue) subpixels, enabling selective deposition of the conductive coating 830 over portions of the second electrode 140 that are substantially free of the NIC 810, i.e., over the lateral sides 420 of the non-emissive regions 1920 that include the PDL 440. In some non-limiting examples, the conductive coating 830 may tend not to remain on the sloped portions of the PDL 440 but may tend to descend to the base of such sloped portions that are coated with the NIC 810, such that the conductive coating 830 may tend to accumulate along the substantially flat portions of the PDL 440. In some non-limiting examples, the conductive coating 830 on the substantially flat portions of the PDL 440 may form at least one auxiliary electrode 1750 that may be electrically coupled to the second electrode 140.
[0362] Referring now to FIG. 21, there is shown an example of a version 2100 of device 100 that encompasses the device 100 shown in cross section in FIG. 4 but with many of the additional deposition steps described herein.
[0363] Device 2100 shows NIC 810 selectively deposited on the base material, shown as the exposed layer surface 111 of second electrode 140, within a first portion of device 2100 substantially corresponding to the lateral side 410 of emissive region 1910 corresponding to (sub)pixel 340 / 264x, but not within a second portion of device 2100 substantially corresponding to the lateral side 420 of non-emissive region 1920 surrounding the first portion.
[0364] In some non-limiting examples, the NIC 810 can be selectively deposited using a shadow mask.
[0365] The NIC 810 is then deposited to provide a surface in the first portion with a relatively low initial sticking probability S 0 for the conductive coating 830 to form the auxiliary electrode 1750 .
[0366] After selective deposition of the NIC 810 , a conductive coating 830 is deposited over the device 2100 but remains substantially only in the second portion that is substantially free of the NIC 810 to form the auxiliary electrode 1750 .
[0367] In some non-limiting examples, the conductive coating 830 can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0368] The auxiliary electrode 1750 is positioned above the second electrode 140 over a second portion that is substantially free of the NIC 810, as shown, and is electrically coupled to the second electrode 140 so as to reduce the sheet resistance of the second electrode 140, including by being in physical contact therewith.
[0369] In some non-limiting examples, the conductive coating 830 may comprise substantially the same material as the second electrode 140 to ensure a high initial sticking probability S for the conductive coating 830 within the second portion.
[0370] In some non-limiting examples, the second electrode 140 can comprise substantially pure Mg and / or an alloy of Mg with another metal, including, but not limited to, Ag. In some non-limiting examples, the Mg:Ag alloy composition can range from about 1:9 to about 9:1 by volume. In some non-limiting examples, the second electrode 140 can comprise a metal oxide, including, but not limited to, a ternary metal oxide, such as, but not limited to, ITO and / or IZO, and / or a combination of metals and / or metal oxides.
[0371] In some non-limiting examples, the conductive coating 830 used to form the auxiliary electrode 1750 can include substantially pure Mg.
[0372] Referring now to FIG. 22, there is shown an example of a version 2200 of device 100 that encompasses the device 100 shown in cross section in FIG. 4 but with many of the additional deposition steps described herein.
[0373] Device 2200 shows NIC 810 selectively deposited on the base material, shown as exposed layer surface 111 of second electrode 140, in a first portion of device 2200 that substantially corresponds to a portion of a lateral side 410 of light-emitting region 1910 corresponding to (sub)pixel 340 / 264x, but not in a second portion. In the figure, the first portion extends partially along the extent of the sloped portion of PDL 440 that defines light-emitting region 1910.
[0374] In some non-limiting examples, the NIC 810 can be selectively deposited using a shadow mask.
[0375] The NIC 810 is then deposited to provide a surface in the first portion with a relatively low initial sticking probability S 0 for the conductive coating 830 to form the auxiliary electrode 1750 .
[0376] After selective deposition of NIC 810, conductive coating 830 is deposited across device 2200, but remains substantially only in the second portion that is substantially free of NIC 810, forming auxiliary electrode 1750. Thus, in device 2200, auxiliary electrode 1750 extends partially across the sloped portion of PDL 440 that defines light-emitting region 1910.
[0377] In some non-limiting examples, the conductive coating 830 can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0378] The auxiliary electrode 1750 is positioned above the second electrode 140 over a second portion that is substantially free of the NIC 810, as shown, and is electrically coupled to the second electrode 140 so as to reduce the sheet resistance of the second electrode 140, including by being in physical contact therewith.
[0379] In some non-limiting examples, the material that the second electrode 140 may comprise may not have a high initial sticking probability S 0 for the conductive coating 830 .
[0380] FIG. 23 illustrates such a situation, illustrating an example version 2300 of device 100, shown in cross section in FIG. 4, but encompassing device 100 with many of the additional deposition steps described herein.
[0381] Device 2300 shows NPC 1120 deposited on the base material, shown as the exposed layer surface 111 of second electrode 140 .
[0382] In some non-limiting examples, the NPC 1120 can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0383] NIC810 is then selectively deposited on the base material, in the figure, the exposed layer surface 111 of NPC1120, within a first portion of device 2300 that substantially corresponds to a portion of the lateral side 410 of the emissive region 1910 corresponding to (sub)pixel 340 / 264x, but not within a second portion of device 2300 that substantially corresponds to the lateral side 420 of the non-emissive region 1920 that surrounds the first portion.
[0384] In some non-limiting examples, the NIC 810 can be selectively deposited using a shadow mask.
[0385] The NIC 810 is then deposited to provide a surface in the first portion with a relatively low initial sticking probability S 0 for the conductive coating 830 to form the auxiliary electrode 1750 .
[0386] After selective deposition of the NIC 810 , a conductive coating 830 is deposited over the device 2300 but remains substantially only in the second portion that is substantially free of the NIC 810 to form the auxiliary electrode 1750 .
[0387] In some non-limiting examples, the conductive coating 830 can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0388] The auxiliary electrode 1750 is electrically coupled to the second electrode 140 so as to reduce sheet resistance. As shown, the auxiliary electrode 1750 is not located above or in physical contact with the second electrode 140; nevertheless, one skilled in the art will understand that the auxiliary electrode 1750 can be electrically coupled to the second electrode 140 by many well-understood mechanisms. As a non-limiting example, the presence of a relatively thin film (in some non-limiting examples, up to about 50 nm) of NIC 810 and / or NPC 1120 can still allow current to pass through the film, thus reducing the sheet resistance of the second electrode 140.
[0389] Referring now to FIG. 24, there is shown an example of a version 2400 of device 100 that encompasses the device 100 shown in cross section in FIG. 4 but with many of the additional deposition steps described herein.
[0390] Device 2400 shows NIC 810 deposited on a base material, shown as the exposed layer surface 111 of second electrode 140 .
[0391] In some non-limiting examples, the NIC 810 can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0392] The NIC 810 provides a surface with a relatively low initial sticking probability S 0 for the conductive coating 830 that is subsequently deposited to form the auxiliary electrode 1750 .
[0393] After deposition of NIC810, NPC1120 is selectively deposited on the base material, in the figure, the exposed layer surface 111 of NIC810, within the NPC portion of device 2400 that substantially corresponds to a portion of the lateral side 420 of non-emissive region 1920 that surrounds a second portion of device 2400 that substantially corresponds to the lateral side 410 of emissive region 1910 corresponding to (sub)pixel 340 / 264x.
[0394] In some non-limiting examples, the NPC 1120 can be selectively deposited using a shadow mask.
[0395] NPC 1120 is subsequently deposited to provide a surface in the first portion with a relatively high initial sticking probability S 0 for conductive coating 830 to form auxiliary electrode 1750 .
[0396] After selective deposition of the NPC 1120 , a conductive coating 830 is deposited on the device 2400 , but remains substantially only in the portion of the NPC where the NIC 810 overlaps the NPC 1120 to form the auxiliary electrode 1750 .
[0397] In some non-limiting examples, the conductive coating 830 can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0398] The auxiliary electrode 1750 is electrically coupled to the second electrode 140 to reduce the sheet resistance of the second electrode 140 .
[0399] Selective Coating Removal In some non-limiting examples, the NIC 810 may be removed after deposition of the conductive coating 830 such that at least a portion of the previously exposed layer surface 111 of the base material that was covered by the NIC 810 may be re-exposed. In some non-limiting examples, the NIC 810 may be selectively removed by etching and / or dissolving the NIC 810 and / or by employing plasma and / or solvent processing techniques that do not substantially affect or damage the conductive coating 830.
[0400] 25A, there is shown an example cross-sectional view of an example version 2500 of device 100 at a deposition stage 2500a, in which NIC 810 has been selectively deposited on a first portion of an exposed layer surface 111 of a base material. In the figure, the base material may be substrate 110.
[0401] 25B, device 2500 is shown at deposition stage 2500b, in which conductive coating 830 is deposited on exposed layer surfaces 111 of the base material, i.e., both on exposed layer surfaces 111 of NIC 810 where NIC 810 was deposited during stage 2500a, and on exposed layer surfaces 111 of substrate 110 where NIC 810 was not deposited during stage 2500a. Due to the nucleation-inhibiting properties of the first portion on which NIC 810 is disposed, the conductive coating 830 disposed thereon tends not to remain, resulting in a pattern of selective deposition of conductive coating 830 corresponding to the second portion while leaving the first portion substantially free of conductive coating.
[0402] In Figure 25C, device 2500 is shown at deposition stage 2500c, in which NIC 810 has been removed from a first portion of exposed layer surface 111 of substrate 110, such that conductive coating 830 deposited during stage 2500b remains on substrate 110 and the area of substrate 110 on which NIC 810 was deposited during stage 2500a is now exposed or uncovered.
[0403] In some non-limiting examples, removal of the NIC 810 in step 2500c can be achieved by exposing the device 2500 to a solvent and / or plasma that reacts with and / or etches away the NIC 810 without substantially affecting the conductive coating 830.
[0404] Transparent OLED 26A, there is shown an example of a plan view of a transmissive (clear) version of device 100, generally designated 2600. In some non-limiting examples, device 2600 is an AMOLED device having a plurality of pixel regions 2610 and a plurality of transmissive regions 2620. In some non-limiting examples, at least one auxiliary electrode 1750 can be deposited on the exposed layer surface 111 of the base material between the pixel regions 2610 and / or the transmissive regions 2620.
[0405] In some non-limiting examples, each pixel region 2610 may include multiple light-emitting regions 1910, each corresponding to a sub-pixel 264x. In some non-limiting examples, the sub-pixels 264x may correspond to an R (red) sub-pixel 2641, a G (green) sub-pixel 2642, and / or a B (blue) sub-pixel 2643, respectively.
[0406] In some non-limiting examples, each transmissive region 2620 is substantially transparent, allowing light to pass through its entire cross-sectional side.
[0407] Referring now to FIG. 26B, an example cross-sectional view of a device 2600 taken along line 26B-26B in FIG. 26A is shown. In the figure, the device 2600 is shown to include a substrate 110, a TFT insulating layer 280, and a first electrode 120 formed on the surface of the TFT insulating layer 280. The substrate 110 may include a base substrate 112 (not shown for ease of illustration) and / or at least one TFT structure 200 positioned substantially below the at least one TFT structure 200, corresponding to and driving each subpixel 264x electrically coupled to its first electrode 120. A PDL 440 is formed on the substrate 110 within a non-emissive region 1920 to define an emissive region 1910 on the corresponding first electrode 120, which also corresponds to each subpixel 264x. The PDL 440 covers the edges of the first electrode 120.
[0408] In some non-limiting examples, at least one semiconductive layer 130 is deposited over the exposed area of the first electrode 120 and, in some non-limiting examples, at least a portion of the surrounding PDL 440.
[0409] In some non-limiting examples, the second electrode 140 can be at least partially deposited on at least one semiconductive layer 130, including on the pixel region 2610 to form that subpixel 264x, and in some non-limiting examples, on the surrounding PDL 440 in the transparent region 2620.
[0410] In some non-limiting examples, the NIC 810 is selectively deposited on a first portion of the device 2600, including both the pixel region 2610 and the transparent region 2620, but not the region of the second electrode 140 corresponding to the auxiliary electrode 1750.
[0411] Then, in some non-limiting examples, the entire surface of device 2600 is exposed to a vapor flux of conductive coating 830, which in some non-limiting examples can be Mg. Conductive coating 830 is selectively deposited on a second portion of second electrode 140 that is substantially free of NIC 810 to form auxiliary electrode 1750 that is electrically coupled to, and in some non-limiting examples physically contacts, the uncoated portion of second electrode 140.
[0412] At the same time, the transmissive region 2620 of the device 2600 remains substantially free of any material that may substantially affect the transmission of light therethrough. In particular, as shown, the TFT structure 200 and the first electrode 120 are positioned within the cross-sectional side below their corresponding subpixels 264x and, together with the auxiliary electrode 1750, are located beyond the transmissive region 2620. As a result, these components do not attenuate or impede the transmission of light through the transmissive region 2620. In some non-limiting examples, such an arrangement allows a viewer of the device 2600 from a normal viewing distance to see through the device 2600 when, in some non-limiting examples, all of the (sub)pixels 340 / 264x are non-emitting, thus creating a transparent AMOLED device 2600.
[0413] Although not shown, in some non-limiting examples, the device 2600 may further include an NPC 1120 disposed between the auxiliary electrode 1750 and the second electrode 140. In some non-limiting examples, the NPC 1120 may also be disposed between the NIC 810 and the second electrode 140.
[0414] In some non-limiting examples, NIC 810 may be formed simultaneously with at least one semiconductive layer 130. As a non-limiting example, at least one material used to form NIC 810 may also be used to form at least one semiconductive layer 130. In such non-limiting examples, many steps for fabricating device 2600 may be eliminated.
[0415] Those skilled in the art will understand that various other layers and / or coatings may cover portions of the transparent region 2620, including, but not limited to, those forming at least one semiconductive layer 130 and / or second electrode 140, in some non-limiting examples, particularly if such layers and / or coatings are substantially transparent. In some non-limiting examples, the PDL 440 may have a reduced thickness, including, but not limited to, forming wells therein, in some non-limiting examples not significantly different from wells defined for the light emitting region 1910, to further facilitate light transmission through the transparent region 2620.
[0416] Those skilled in the art will understand that (sub)pixel 340 / 264x arrangements other than those shown in Figures 26A and 26B may be employed in some non-limiting examples.
[0417] 26A and 26B , auxiliary electrodes 1750 may be disposed between pixel region 2610 and transmissive region 2620. As a non-limiting example, auxiliary electrodes 1750 may be disposed between sub-pixels 264x within pixel region 2610.
[0418] 27A, which shows an example of a plan view of a transparent version of device 100, generally designated 2700. In some non-limiting examples, device 2700 is an AMOLED device having a plurality of pixel regions 2610 and a plurality of transmissive regions 2620. Device 2700 differs from device 2600 in that auxiliary electrode 1750 is not located between pixel regions 2610 and / or transmissive regions 2620.
[0419] In some non-limiting examples, each pixel region 2610 may include multiple light-emitting regions 1910, each corresponding to a sub-pixel 264x. In some non-limiting examples, the sub-pixels 264x may correspond to an R (red) sub-pixel 2641, a G (green) sub-pixel 2642, and / or a B (blue) sub-pixel 2643, respectively.
[0420] In some non-limiting examples, each transmissive region 2620 is substantially transparent, allowing light to pass through its entire cross-sectional side.
[0421] Referring now to FIG. 27B, an example cross-sectional view of device 2700 taken along line 27B-27B in FIG. 27A is shown. In the figure, device 2700 is shown to include a substrate 110, a TFT insulating layer 280, and a first electrode 120 formed on the surface of TFT insulating layer 280. Substrate 110 may include a base substrate 112 (not shown for ease of illustration) and / or at least one TFT structure 200 positioned substantially below at least one TFT structure 200 corresponding to and driving each subpixel 264x electrically coupled to its first electrode 120. PDLs 440 are formed on substrate 110 within non-emissive regions 1920 to define emissive regions 1910 on the corresponding first electrodes 120 that also correspond to each subpixel 264x. PDLs 440 cover the edges of the first electrodes 120.
[0422] In some non-limiting examples, at least one semiconductive layer 130 is deposited over the exposed area of the first electrode 120 and, in some non-limiting examples, at least a portion of the surrounding PDL 440.
[0423] In some non-limiting examples, the first conductive coating 830a may be deposited on at least one semi-conductive layer 130, including over the pixel region 2610 to form its subpixel 264x and over the surrounding PDL 440 in the transmissive region 2620. In some non-limiting examples, the thickness of the first conductive coating 830a may be relatively thin such that the presence of the first conductive coating 830a over the transmissive region 2620 does not substantially attenuate the transmission of light through the transmissive region 2620. In some non-limiting examples, the first conductive coating 830a may be deposited using an open-mask deposition process and / or a mask-free deposition process.
[0424] In some non-limiting examples, the NIC 810 is selectively deposited on a first portion of the device 2700, including the transparent region 2620.
[0425] Then, in some non-limiting examples, the entire surface of device 2700 is exposed to a vapor flux of conductive coating 830, which in some non-limiting examples may be Mg, to selectively deposit second conductive coating 830b on the second portion of first conductive coating 830a that is substantially free of NIC 810 (in some examples, pixel region 2610), such that second conductive coating 830b is electrically coupled to, and in some non-limiting examples, physically contacted with, the uncoated portion of first conductive coating 830a to form second electrode 140.
[0426] In some non-limiting examples, the thickness of the first conductive coating 830a may be less than the thickness of the second conductive coating 830b. In this manner, a relatively high transmittance can be maintained within the transparent region 2620, through which only the first conductive coating 830a extends. In some non-limiting examples, the thickness of the first conductive coating 830a may be less than about 30 nm, less than about 25 nm, less than about 20 nm, less than about 15 nm, less than about 10 nm, less than about 8 nm, and / or less than about 5 nm. In some non-limiting examples, the thickness of the second conductive coating 830b may be less than about 30 nm, less than about 25 nm, less than about 20 nm, less than about 15 nm, less than about 10 nm, and / or less than about 8 nm.
[0427] Thus, in some non-limiting examples, the thickness of second electrode 140 can be less than about 40 nm, and / or in some non-limiting examples, between about 5 nm and 30 nm, between about 10 nm and about 25 nm, and / or between about 15 nm and about 25 nm.
[0428] In some non-limiting examples, the thickness of the first conductive coating 830a may be greater than the thickness of the second conductive coating 830b. In some non-limiting examples, the thickness of the first conductive coating 830a and the thickness of the second conductive coating 830b may be substantially the same.
[0429] In some non-limiting examples, at least one material used to form first conductive coating 830 a can be substantially the same as at least one material used to form second conductive coating 830 b. In some non-limiting examples, such at least one material can be substantially as described herein with respect to first electrode 120, second electrode 140, auxiliary electrode 1750, and / or conductive coatings 830 thereof.
[0430] In some non-limiting examples, the transmissive region 2620 of the device 2700 remains substantially free of any material that may substantially affect the transmission of light therethrough. In particular, as shown, the TFT structures 200 and / or first electrodes 120 are positioned within the cross-sectional sides below their corresponding subpixels 264x and beyond the transmissive region 2620. As a result, these components do not attenuate or impede light from passing through the transmissive region 2620. In some non-limiting examples, such an arrangement allows a viewer of the device 2700 from a normal viewing distance to see through the device 2700 when, in some non-limiting examples, all of the (sub)pixels 340 / 264x are non-emitting, thus creating a transparent AMOLED device 2700.
[0431] Although not shown, in some non-limiting examples, device 2700 may further include NPC 1120 disposed between second conductive coating 830b and first conductive coating 830a. In some non-limiting examples, NPC 1120 may also be disposed between NIC 810 and first conductive coating 830a.
[0432] In some non-limiting examples, NIC 810 may be formed simultaneously with at least one semiconductive layer 130. As a non-limiting example, at least one material used to form NIC 810 may also be used to form at least one semiconductive layer 130. In such non-limiting examples, many steps for fabricating device 2700 may be eliminated.
[0433] Those skilled in the art will appreciate that various other layers and / or coatings, including but not limited to those forming at least one semiconductive layer 130 and / or first conductive coating 830a, in some non-limiting examples, may cover portions of transparent region 2620, particularly if such layers and / or coatings are substantially transparent. In some non-limiting examples, PDL 440 may have a reduced thickness, including but not limited to, in some non-limiting examples, forming wells therein not significantly different from wells defined for light emitting region 1910 to further facilitate light transmission through transparent region 2620.
[0434] Those skilled in the art will understand that (sub)pixel 340 / 264x arrangements other than those shown in Figures 27A and 27B may be employed in some non-limiting examples.
[0435] Referring now to FIG. 27C, an example cross-sectional view of a different version of device 100, designated device 1910, is shown taken along the same line 27B-27B of FIG. 27A. In the figure, device 1910 is shown to include a substrate 110, a TFT insulating layer 280, and a first electrode 120 formed on the surface of the TFT insulating layer 280. The substrate 110 may include a base substrate 112 (not shown for ease of illustration) and / or at least one TFT structure 200 positioned substantially below the base substrate 112 and corresponding to and driving each subpixel 264x electrically coupled to its first electrode 120. A PDL 440 is formed on the substrate 110 within the non-emissive region 1920 to define an emissive region 1910 on the corresponding first electrode 120 that also corresponds to each subpixel 264x. The PDL 440 covers the edges of the first electrode 120.
[0436] In some non-limiting examples, at least one semiconductive layer 130 is deposited over the exposed area of the first electrode 120 and, in some non-limiting examples, at least a portion of the surrounding PDL 440.
[0437] In some non-limiting examples, the NIC 810 is selectively deposited on a first portion of the device 2700, including the transparent region 2620.
[0438] In some non-limiting examples, the conductive coating 830 may be deposited on at least one semiconductive layer 130, including over the pixel region 2610 to form that subpixel 264x, but not over the surrounding PDL 440 in the transparent region 2620. In some non-limiting examples, the first conductive coating 830a may be deposited using an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, such deposition may be achieved by exposing the entire surface of the device 1910 to a vapor flux of the conductive coating 830, which may be Mg in some non-limiting examples, to selectively deposit the conductive coating 830 on a second portion of the at least one semiconductive layer 130 that is substantially free of the NIC 810 (in some examples, the pixel region 2610), such that the conductive coating 830 is deposited on the at least one semiconductive layer 130 to form the second electrode 140.
[0439] In some non-limiting examples, the transmissive region 2620 of the device 1910 remains substantially free of any material that may substantially affect the transmission of light therethrough. In particular, as shown, the TFT structures 200 and / or first electrodes 120 are positioned within the cross-sectional sides below their corresponding subpixels 264x and beyond the transmissive region 2620. As a result, these components do not attenuate or impede light from passing through the transmissive region 2620. In some non-limiting examples, such an arrangement allows a viewer of the device 2700 from a normal viewing distance to see through the device 2700 when, in some non-limiting examples, all of the (sub)pixels 340 / 264x are non-emitting, thus creating a transparent AMOLED device 1910.
[0440] By providing a transparent region 2620 that does not include and / or is substantially free of conductive coating 830, the transmittance within such region can be preferably enhanced in some non-limiting examples, by comparison to device 2700 of FIG. 27B, as a non-limiting example.
[0441] Although not shown, in some non-limiting examples, device 1910 may further include NPC 1120 disposed between conductive coating 830 and at least one semi-conductive layer 130. In some non-limiting examples, NPC 1120 may also be disposed between NIC 810 and PDL 440.
[0442] In some non-limiting examples, the NIC 810 may be formed simultaneously with the at least one semiconductive layer 130. As a non-limiting example, the at least one material used to form the NIC 810 may also be used to form the at least one semiconductive layer 130. In such non-limiting examples, many steps for fabricating the device 1910 may be eliminated.
[0443] Those skilled in the art will understand that various other layers and / or coatings may cover portions of the transparent region 2620, including, but not limited to, those forming at least one semiconductive layer 130 and / or conductive coating 830, in some non-limiting examples, particularly if such layers and / or coatings are substantially transparent. In some non-limiting examples, the PDL 440 may have a reduced thickness, including, but not limited to, forming wells therein, in some non-limiting examples not significantly different from the wells defined for the light emitting region 1910, to further facilitate light transmission through the transparent region 2620.
[0444] Those skilled in the art will understand that (sub)pixel 340 / 264x arrangements other than those shown in Figures 27A and 27C may be employed in some non-limiting examples.
[0445] Selective deposition of conductive coatings on light-emitting areas As discussed above, adjusting the thickness of the electrodes 120, 140, 1750, 4150 in and across the lateral sides 410 of the light-emitting regions 1910 of the (sub)pixels 340 / 264x may affect the observable microcavity effect. In some non-limiting examples, selective deposition of at least one conductive coating 830 through deposition of at least one selective coating 710, such as NIC 810 and / or NPC 1120, into the lateral sides 410 of the light-emitting regions 1910 corresponding to different subpixels 264x within the pixel region 2610 controls and / or adjusts the optical microcavity effect within each light-emitting region 1910 to optimize the desired optical microcavity effect on a subpixel 264x basis, including, but not limited to, the emission spectrum, luminous intensity, and / or angular dependence of the brightness and / or color shift of the emitted light.
[0446] Such effects can be controlled by modulating the thickness of selective coatings 710, such as NIC 810 and / or NPC 1120, disposed independently within each emissive region 1910 of subpixel 264x. As a non-limiting example, the thickness of NIC 810 disposed over blue subpixel 2643 may be thinner than the thickness of NIC 810 disposed over green subpixel 2642, which may be thinner than the thickness of NIC 810 disposed over red subpixel 2641.
[0447] In some non-limiting examples, such effects can be controlled to an even greater extent by independently adjusting the thickness of the conductive coating 830 deposited within a portion of each light-emitting region 1910 of the subpixel 264x, as well as the selective coating 710.
[0448] Such a mechanism is illustrated in the schematic diagrams of Figures 28A-28D, which show various stages in the fabrication of an example version of device 100, generally designated 2800.
[0449] 28A shows stage 2810 of fabricating device 2800. In stage 2810, substrate 110 is provided. Substrate 110 includes first light-emitting region 1910a and second light-emitting region 1910b. In some non-limiting examples, first light-emitting region 1910a and / or second light-emitting region 1910b may be surrounded by and / or separated by at least one non-light-emitting region 1920a-1920c. In some non-limiting examples, first light-emitting region 1910a and / or second light-emitting region 1910b may each correspond to (sub)pixel 340 / 264x.
[0450] 28B shows stage 2820 of fabricating device 2800. In stage 2820, first conductive coating 830a is deposited on exposed layer surface 111 of a base material, in this case substrate 110. First conductive coating 830a is deposited over first light emitting region 1910a and second light emitting region 1910b. In some non-limiting examples, first conductive coating 830a is deposited over at least one of non-light emitting regions 1920a-1920c.
[0451] In some non-limiting examples, the first conductive coating 830a can be deposited using an open mask deposition process and / or a mask-free deposition process.
[0452] 28C illustrates stage 2830 of fabricating device 2800. In stage 2830, NIC 810 is selectively deposited on a first portion of first conductive coating 830a. As shown, in some non-limiting examples, NIC 810 is deposited over first light emitting region 1910a, while in some non-limiting examples, second light emitting region 1910b and / or in some non-limiting examples, at least one of non-light emitting regions 1920a-1920c are substantially free of NIC 810.
[0453] 28D shows stage 2840 of fabricating device 2800. In stage 2840, second conductive coating 830b can be deposited over those second portions of device 2800 that are substantially free of NIC 810. In some non-limiting examples, second conductive coating 830b can be deposited over second light emitting region 1910b and / or, in some non-limiting examples, at least one of non-light emitting regions 1920a-1920c.
[0454] Those skilled in the art will understand that the evaporation process shown in FIG. 28D and described in detail in connection with any one or more of FIGS. 7-8, 11A-11B, and / or 12A-12C may equally be applied to any one or more of the preceding steps described in FIGS. 28A-28C, although these steps are not shown for ease of illustration.
[0455] Those skilled in the art will appreciate that fabrication of device 2800 may, in some non-limiting examples, include additional steps not shown for ease of illustration. Such additional steps may include, but are not limited to, depositing one or more NICs 810, depositing one or more NPCs 1120, depositing one or more additional conductive coatings 830, depositing an outcoupling coating, and / or encapsulating device 2800.
[0456] Those skilled in the art will understand that while the fabrication of device 2800 is described and illustrated in relation to first light-emitting region 1910a and second light-emitting region 1910b, in some non-limiting examples, the principles derived therefrom may equally apply to the fabrication of devices having three or more light-emitting regions 1910.
[0457] In some non-limiting examples, such principles may be applied to deposit conductive coatings of various thicknesses for light-emitting regions 1910 corresponding to subpixels 264x in OLED display device 100 having different emission spectra. In some non-limiting examples, first light-emitting region 1910a may correspond to subpixel 264x configured to emit light of a first wavelength and / or emission spectrum, and / or in some non-limiting examples, second light-emitting region 1910b may correspond to subpixel 264x configured to emit light of a second wavelength and / or emission spectrum. In some non-limiting examples, device 2800 may include a third light-emitting region 1910c ( FIG. 29A ), which may correspond to subpixel 264x configured to emit light of a third wavelength and / or emission spectrum.
[0458] In some non-limiting examples, the first wavelength may be less than, greater than, and / or equal to at least one of the second wavelength and / or the third wavelength. In some non-limiting examples, the second wavelength may be less than, greater than, and / or equal to at least one of the first wavelength and / or the third wavelength. In some non-limiting examples, the third wavelength may be less than, greater than, and / or equal to at least one of the first wavelength and / or the second wavelength.
[0459] In some non-limiting examples, device 2800 may also include at least one additional light-emitting region 1910 (not shown), which may be configured to emit light having a wavelength and / or emission spectrum that is substantially the same as at least one of first light-emitting region 1910a, second light-emitting region 1910b, and / or third light-emitting region 1910c, in some non-limiting examples.
[0460] In some non-limiting examples, the NIC 810 may be selectively deposited using a shadow mask that may also be used to deposit at least one semiconductive layer 130 of the first light-emitting region 1910 a. In some non-limiting examples, such shared use of a shadow mask may modulate the optical microcavity effect for each subpixel 264 x in a cost-effective manner.
[0461] Use of such a mechanism to create an example version 2900 of device 100 having subpixel 264x of a given pixel 340 with a tailored microcavity effect is illustrated in Figures 29A-29D.
[0462] In FIG. 29A, a stage 2810 of the fabrication of a device 2900 is shown including a substrate 110, a TFT insulating layer 280, and a plurality of first electrodes 120a-120c formed on the surface of the TFT insulating layer 280.
[0463] The substrate 110 may include a base substrate 112 (not shown for ease of illustration) and / or at least one TFT structure 200a-200c positioned substantially below the at least one TFT structure 200a-200c and corresponding to and driving the light-emitting regions 1910a-1910c, each having a corresponding subpixel 264x electrically coupled to its associated first electrode 120a-120c. PDLs 440a-440d are formed on the substrate 110 to define the light-emitting regions 830a-1910c. The PDLs 440a-440d cover the edges of each first electrode 120a-120c.
[0464] In some non-limiting examples, at least one semiconductive layer 130a-130c is deposited over the exposed area of each first electrode 120a-120c and, in some non-limiting examples, at least a portion of the surrounding PDL 440a-440d.
[0465] In some non-limiting examples, the first conductive coating 830a can be deposited on at least one semiconductive layer 130a-130c. In some non-limiting examples, the first conductive coating 830a can be deposited using an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, such deposition can be achieved by exposing the entire exposed layer surface 111 of the device 2900 to a vapor flux of the first conductive coating 830a, which in some non-limiting examples can be Mg, to deposit the first conductive coating 830a on at least one semiconductive layer 130a-130c to form a first layer of the second electrode 140a (not shown), which in some non-limiting examples can be a common electrode for at least the first light emitting region 1910a. Such a common electrode can be deposited within the first light emitting region 1910a to a first thickness t c1 The first thickness t c1 may correspond to the thickness of the first conductive coating 830a.
[0466] In some non-limiting examples, the first NIC 810a is selectively deposited on a first portion of the device 2810 that includes the first light emitting region 1910a.
[0467] In some non-limiting examples, the second conductive coating 830b can be deposited on the device 2900. In some non-limiting examples, the second conductive coating 830b can be deposited using an open mask deposition process and / or a mask-free deposition process. In some non-limiting examples, such deposition can be achieved by exposing the entire exposed layer surface 111 of device 2810 to a vapor flux of second conductive coating 830b, which in some non-limiting examples may be Mg, such that second conductive coating 830b is deposited on a second portion of first conductive coating 830a that is substantially free of first NIC 810a to form a second layer of second electrode 140b (not shown), which in some non-limiting examples may be a common electrode for at least second light emitting region 1910b. Such a common electrode can be deposited on first conductive coating 830a that is substantially free of first NIC 810a, and in some examples on at least a portion of second and third light emitting regions 1910b, 1910c, and / or non-light emitting region 1920 where PDLs 440a-440d are located. Such a common electrode can be deposited within second light emitting region 1910b to a second thickness t c2 The second thickness t c2 may correspond to the total thickness of the first conductive coating 830a and the second conductive coating 830b, and in some non-limiting examples, the first thickness t c1 It may be thicker than
[0468] In FIG. 29B, a stage 2920 of the fabrication of device 2900 is shown.
[0469] In some non-limiting examples, the second NIC 810b is selectively deposited on a further first portion of the device 2900 that includes the second light emitting region 1910b.
[0470] In some non-limiting examples, the third conductive coating 830c can be deposited on the device 2900. In some non-limiting examples, the third conductive coating 830c can be deposited using an open mask deposition process and / or a mask-free deposition process. In some non-limiting examples, such deposition can be achieved by exposing the entire exposed layer surface 111 of device 2900 to a vapor flux of third conductive coating 830c, which in some non-limiting examples may be Mg, to deposit third conductive coating 830c on second conductive coating 830b that is substantially free of either first NIC 810a or second NIC 810b, and in some examples, third light-emitting region 1910c, and / or at least a portion of non-light-emitting region 1920 where PDLs 440a-440d are located, such that third conductive coating 830c is deposited on an additional second portion of second conductive coating 830b that is substantially free of second NIC 810b to form a third layer of second electrode 140c (not shown), which in some non-limiting examples may be a common electrode for at least third light-emitting region 1910c. Such a common electrode can be deposited on a third thickness t within third light-emitting region 1910c. c3 The third thickness t c3 may correspond to the total thickness of the first conductive coating 830a, the second conductive coating 830b, and the third conductive coating 830c, and in some non-limiting examples, the first thickness t c1 and the second thickness t c2 may be greater than either or both of
[0471] In FIG. 28C, a stage 2830 of fabrication of device 2900 is shown.
[0472] In some non-limiting examples, the third NIC 810c is selectively deposited on an additional first portion of the device 2900 that includes the third light-emitting region 1910b.
[0473] In FIG. 29D, a stage 2940 of the fabrication of device 2900 is shown.
[0474] In some non-limiting examples, at least one auxiliary electrode 1750 is disposed in a non-emissive region 1920 of device 2900 between its adjacent emissive regions 1910a-1910c, and in some non-limiting examples, on PDLs 440a-440d. In some non-limiting examples, the conductive coating 830 used to deposit at least one auxiliary electrode 1750 can be deposited using an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, such deposition can be achieved by exposing the entire exposed layer surface 111 of device 2900 to a vapor flux of conductive coating 830, which in some non-limiting examples can be Mg, to deposit conductive coating 830 on exposed portions of first conductive coating 830a, second conductive coating 830b, and third conductive coating 830c that are substantially free of first NIC 810a, second NIC 810b, and / or third NIC 810c, such that conductive coating 830 is deposited on an additional second portion including exposed portions of first conductive coating 830a, second conductive coating 830b, and / or third conductive coating 830c that are substantially free of first NIC 810a, second NIC 810b, and / or third NIC 810c to form at least one auxiliary electrode 1750. Each of the at least one auxiliary electrode 1750 is electrically coupled to a respective one of the second electrodes 140a-140c, and in some non-limiting examples, each of the at least one auxiliary electrode 1750 is in physical contact with such second electrode 140a-140c.
[0475] In some non-limiting examples, first light-emitting region 1910a, second light-emitting region 1910b, and third light-emitting region 1910c may be substantially free of the material used to form at least one auxiliary electrode 1750.
[0476] In some non-limiting examples, at least one of the first conductive coating 830 a, the second conductive coating 830 b, and / or the third conductive coating 830 c can be transmissive and / or substantially transparent in at least a portion of the visible wavelength range of the electromagnetic spectrum. Thus, when the second conductive coating 830 b and / or the third conductive coating 830 a (and / or any additional conductive coatings 830) are disposed on top of the first conductive coating 830 a to form a multi-coated electrode 120, 140, 1750 that can be transmissive and / or substantially transparent in at least a portion of the visible wavelength range of the electromagnetic spectrum. In some non-limiting examples, the transmittance of any one or more of the first conductive coating 830a, the second conductive coating 830b, the third conductive coating 830c, any additional conductive coatings 830, and / or the multi-coated electrodes 120, 140, 1750 may be greater than about 30%, greater than about 40%, greater than about 45%, greater than about 50%, greater than about 60%, greater than about 70%, greater than about 75%, and / or greater than about 80% in at least a portion of the visible wavelength range of the electromagnetic spectrum.
[0477] In some non-limiting examples, the thickness of first conductive coating 830a, second conductive coating 830b, and / or third conductive coating 830c can be relatively thin to maintain relatively high transmittance. In some non-limiting examples, the thickness of first conductive coating 830a can be about 5-30 nm, about 8-25 nm, and / or about 10-20 nm. In some non-limiting examples, the thickness of second conductive coating 830b can be about 1-25 nm, about 1-20 nm, about 1-15 nm, about 1-10 nm, and / or about 3-6 nm. In some non-limiting examples, the thickness of third conductive coating 830c can be about 1-25 nm, about 1-20 nm, about 1-15 nm, about 1-10 nm, and / or about 3-6 nm. In some non-limiting examples, the thickness of the multi-coated electrode formed by the combination of the first conductive coating 830a, the second conductive coating 830b, the third conductive coating 830c, and / or any additional conductive coatings 830 may be about 6-35 nm, about 10-30 nm, or about 10-25 nm, and / or about 12-18 nm.
[0478] In some non-limiting examples, the thickness of the at least one auxiliary electrode 1750 can be greater than the thickness of the first conductive coating 830 a, the second conductive coating 830 b, the third conductive coating 830 c, and / or the common electrode. In some non-limiting examples, the thickness of the at least one auxiliary electrode 1750 can be greater than about 50 nm, greater than about 80 nm, greater than about 100 nm, greater than about 150 nm, greater than about 200 nm, greater than about 300 nm, greater than about 400 nm, greater than about 500 nm, greater than about 700 nm, greater than about 800 nm, greater than about 1 μm, greater than about 1.2 μm, greater than about 1.5 μm, greater than about 2 μm, greater than about 2.5 μm, and / or greater than about 3 μm.
[0479] In some non-limiting examples, the at least one auxiliary electrode 1750 may not be substantially transparent and / or opaque. However, the at least one auxiliary electrode 1750 may, in some non-limiting examples, be provided in a non-emissive region 1920 of the device 2900 such that the at least one auxiliary electrode 1750 does not cause or contribute to significant optical interference. In some non-limiting examples, the transmittance of the at least one auxiliary electrode 1750 may be less than about 50%, less than about 70%, less than about 80%, less than about 85%, less than about 90%, and / or less than about 95% of at least a portion of the visible wavelength range of the electromagnetic spectrum.
[0480] In some non-limiting examples, the at least one auxiliary electrode 1750 can absorb light in at least a portion of the visible wavelength range of the electromagnetic spectrum.
[0481] In some non-limiting examples, the thickness of the first NIC 810a, second NIC 810b, and / or third NIC 810c disposed within first light-emitting region 1910a, second light-emitting region 1910b, and / or third light-emitting region 1910c, respectively, can be varied according to the color and / or emission spectrum of the light emitted by each light-emitting region 1910a-1910c. As shown in FIGS. 29C-29D, first NIC 810a has a first NIC thickness t n1 The second NIC 810b may have a second NIC thickness t n2 and / or the third NIC 810c may have a third NIC thickness t n3 In some non-limiting examples, the first NIC thickness t n1 , the second NIC thickness t n2 , and / or the third NIC thickness t n3 In some non-limiting examples, the first NIC thickness t n1 , the second NIC thickness t n2 , and / or the third NIC thickness t n3 may differ from each other.
[0482] In some non-limiting examples, device 2900 can also include any number of light-emitting regions 1910a-1910c and / or their (sub)pixels 340 / 264x. In some non-limiting examples, device 2900 can include multiple pixels 340, and each pixel 340 can include two, three, or more sub-pixels 264x.
[0483] Those skilled in the art will understand that the specific arrangement of the (sub)pixels 340 / 264x may vary depending on the device design. In some non-limiting examples, the subpixels 264x may be arranged according to known arrangement schemes, including, but not limited to, RGB side-by-side, diamond, and / or PenTile®.
[0484] A conductive coating for electrically coupling the electrode to the auxiliary electrode. 30, there is shown a cross-sectional view of an example version 3000 of device 100. Device 3000 includes a light emitting region 1910 and an adjacent non-light emitting region 1920 within a lateral aspect.
[0485] In some non-limiting examples, light-emitting region 1910 corresponds to subpixel 264x of device 3000. Light-emitting region 1910 has substrate 110, first electrode 120, second electrode 140, and at least one semiconductive layer 130 disposed therebetween.
[0486] A first electrode 120 is disposed on an exposed layer surface 111 of a substrate 110. The substrate 110 includes a TFT structure 200 that is electrically coupled to the first electrode 120. The edges and / or periphery of the first electrode 120 are generally covered by at least one PDL 440.
[0487] The non-emissive region 1920 includes an auxiliary electrode 1750, and a first portion of the non-emissive region 1920 includes a protruding structure 3060 disposed to protrude onto and overlap a lateral side of the auxiliary electrode 1750. The protruding structure 3060 extends laterally to provide a protected region 3065. As a non-limiting example, the protruding structure 3060 may be recessed at and / or near at least one side of the auxiliary electrode 1750 to provide the protected region 3065. As shown, the protected region 3065 can correspond to an area of the surface of the PDL 440 that overlaps with the lateral protrusion of the protruding structure 3060, in some non-limiting examples. The non-emissive region 1920 further includes a conductive coating 830 disposed within the protected region 3065. The conductive coating 830 electrically couples the auxiliary electrode 1750 to the second electrode 140.
[0488] The NIC 810a is disposed within the light emitting region 1910 on the exposed layer surface 111 of the second electrode 140. In some non-limiting examples, the exposed layer surface 111 of the protruding structure 3060 is coated with a remaining conductive thin film 3040 from the deposition of the conductive thin film to form the second electrode 140. In some non-limiting examples, the surface of the remaining conductive thin film 3040 is coated with a remaining NIC 810b from the deposition of the NIC 810.
[0489] However, due to the lateral protrusion of the protruding structures 3060 over the protected region 3065, the protected region 3065 is substantially free of the NIC 810. Thus, when the conductive coating 830 is deposited on the device 3000 after the deposition of the NIC 810, the conductive coating 830 is deposited and / or migrates into the protected region 3065, coupling the auxiliary electrode 1750 to the second electrode 140.
[0490] Those skilled in the art will understand that non-limiting examples are shown in FIG. 30 and that various modifications may be apparent. As a non-limiting example, the protruding structure 3060 may provide a protected area 3065 along at least two of its sides. In some non-limiting examples, the protruding structure 3060 may be omitted and the auxiliary electrode 1750 may include a recessed portion that defines the protected area 3065. In some non-limiting examples, the auxiliary electrode 1750 and the conductive coating 830 may be disposed directly on the surface of the substrate 110 in place of the PDL 440.
[0491] Selective Deposition of Optical Coatings In some non-limiting examples, device 100 (not shown), which in some non-limiting examples may be an optoelectronic device, includes a substrate 110, a NIC 810, and an optical coating. The NIC 810 covers a first lateral portion of the substrate 110. The optical coating covers a second lateral portion of the substrate. At least a portion of the NIC 810 is substantially free of the optical coating.
[0492] In some non-limiting examples, optical coatings can be used to tailor the optical properties of light transmitted, emitted, and / or absorbed by device 100, including, but not limited to, plasmonic modes. By way of non-limiting examples, optical coatings may be used as optical filters, index-matching coatings, optical extraction coatings, scattering layers, diffraction gratings, or portions thereof.
[0493] In some non-limiting examples, the optical coating can be used to tune at least one optical microcavity effect in device 100, including, but not limited to, by modulating the total optical path length and / or its refractive index. At least one optical property of device 100 can be affected by tuning at least one optical microcavity effect, including, but not limited to, the output light, including, but not limited to, the angular dependence of its luminance and / or color shift. In some non-limiting examples, the optical coating may be a non-electrical component, i.e., the optical coating may not be configured to conduct and / or transmit electrical current during normal device operation.
[0494] In some non-limiting examples, the optical coating can be formed by employing any material used as the conductive coating 830 and / or any mechanism for depositing the conductive coating 830 described herein.
[0495] Edge effects of NIC and conductive coatings 31A-31I illustrate various potential behaviors of the NIC 810 at the deposition interface with the conductive coating 830.
[0496] Referring to Figure 31A, a first example of a portion of an example version 3100 of device 100 at the NIC deposition boundary is shown. Device 3100 includes a substrate 110 having a layer surface 111. A NIC 810 is deposited on a first portion 3110 of layer surface 111. A conductive coating 830 is deposited on a second portion 3120 of layer surface 111. As shown, by way of non-limiting example, first portion 3110 and second portion 3120 are separate and non-overlapping portions of layer surface 111.
[0497] Conductive coating 830 includes a first portion 830 a and a remaining portion 830 b. As shown, by way of non-limiting example, first portion 830 a of conductive coating 830 substantially covers second portion 3120, and second portion 830 b of conductive coating 830 partially protrudes and / or overlaps the first portion of NIC 810.
[0498] In some non-limiting examples, the NIC 810 is formed such that its surface 3111 exhibits a relatively low affinity or initial sticking probability S for the material used to form the conductive coating 830, such that there is a gap 3129 formed between the protruding and / or overlapping second portion 830b of the conductive coating 830 and the surface 3111 of the NIC 810. As a result, the second portion 830b is not in physical contact with the NIC 810, but is spaced from the NIC 810 by the gap 3129 in the cross-sectional side. In some non-limiting examples, the first portion 830a of the conductive coating 830 can be in physical contact with the NIC 810 at the interface and / or boundary between the first portion 3110 and the second portion 3120.
[0499] In some non-limiting examples, the protruding and / or overlapping second portion 830b of the conductive coating 830 can extend laterally over the NIC 810 to an extent equivalent to the thickness t1 of the conductive coating 830. As a non-limiting example, as shown, the width w2 of the second portion 830b can be equivalent to the thickness t1. In some non-limiting examples, the ratio of w2:t1 can range from about 1:1 to about 1:3, from about 1:1 to about 1:1.5, and / or from about 1:1 to about 1:2. While the thickness t1 can be relatively uniform across the conductive coating 830 in some non-limiting examples, in some non-limiting examples, the extent to which the second portion 830b protrudes and / or overlaps with the NIC 810 (i.e., w2) can vary somewhat across different portions of the layer surface 111.
[0500] 31B, the conductive coating 830 is shown to include a third portion 830c disposed between the second portion 830b and the NIC 810. As shown, the second portion 830b of the conductive coating 830 extends laterally over and is spaced apart from the third portion 830c of the conductive coating 830, and the third portion 830c may be in physical contact with the surface 3111 of the NIC 810. The thickness t3 of the third portion 830c of the conductive coating 830 may be less than the thickness t1 of the first portion 830a of the conductive coating 830, and in some non-limiting examples, may be substantially less. In some non-limiting examples, the width w3 of the third portion 830c may be greater than the width w2 of the second portion 830b. In some non-limiting examples, the third portion 830c may extend laterally to overlap the NIC 810 to a greater extent than the second portion 830b. In some non-limiting examples, the ratio of w3:t1 may range from about 1:2 to about 3:1 and / or from about 1:1.2 to about 2.5:1. Thickness t1 may be relatively uniform across conductive coating 830 in some non-limiting examples, although in some non-limiting examples, the extent to which third portion 830c protrudes and / or overlaps with NIC 810 (i.e., w3) may vary somewhat across different portions of layer surface 111.
[0501] The thickness t3 of third portion 830c can be about 5% or less than the thickness t1 of first portion 830a. By way of non-limiting example, t3 can be about 4% or less, about 3% or less, about 2% or less, about 1% or less, and / or about 0.5% or less of t1. As shown, instead of and / or in addition to third portion 830c being formed as a thin film, the material of conductive coating 830 can be formed as islands and / or isolated clusters on a portion of NIC 810. By way of non-limiting example, such islands and / or isolated clusters can include features physically separated from one another such that the islands and / or clusters do not form a continuous layer.
[0502] Referring now to FIG. 31C , the NPC 1120 is disposed between the substrate 110 and the conductive coating 830. The NPC 1120 is disposed between a first portion 830a of the conductive coating 830 and a second portion 3120 of the substrate 110. The NPC 1120 is shown disposed on the second portion 3120, rather than the first portion 3110 on which the NIC 810 was deposited. The NPC 1120 may be formed such that the surface of the NPC 1120 exhibits a relatively high affinity, or initial sticking probability, S0, for the material of the conductive coating 830 at the interface and / or boundary between the NPC 1120 and the conductive coating 830. Thus, the presence of the NPC 1120 may facilitate the formation and / or growth of the conductive coating 830 during deposition.
[0503] 31D , the NPC 1120 is disposed on both the first portion 3110 and the second portion 3120 of the substrate 110, and the NIC 810 covers a portion of the NPC 1120 that is disposed on the first portion 3110. Another portion of the NPC 1120 is substantially free of the NIC 810, and the conductive coating 830 covers such portion of the NPC 1120.
[0504] 31E, conductive coating 830 is shown partially overlapping a portion of NIC 810 within third portion 3130 of substrate 110. In some non-limiting examples, in addition to first portion 830a and second portion 830b, conductive coating 830 further includes fourth portion 830d. As shown, fourth portion 830d of conductive coating 830 is disposed between first portion 830a and second portion 830b of conductive coating 830, and fourth portion 830d may be in physical contact with layer surface 3111 of NIC 810. In some non-limiting examples, the overlap in third portion 3130 may be formed as a result of lateral growth of conductive coating 830 during an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, the layer surface 3111 of the NIC 810 may exhibit a relatively low initial adhesion probability S0 for the material of the conductive coating 830, such that as the thickness of the conductive coating 830 grows, the material has a low probability of nucleating at the layer surface 3111, but the conductive coating 830 may also grow laterally, covering a subset of the NIC 810 as shown.
[0505] 31F, a first portion 3110 of substrate 110 is coated with NIC 810, and a second portion 3120 adjacent to first portion 3110 is coated with conductive coating 830. In some non-limiting examples, it has been observed that by performing open-mask deposition and / or mask-free deposition of conductive coating 830, it is possible to obtain conductive coating 830 that exhibits a tapered cross-sectional profile at and / or near the interface between conductive coating 830 and NIC 810.
[0506] In some non-limiting examples, the thickness of conductive coating 830 at and / or near the interface may be less than the average thickness of conductive coating 830. While such a tapering profile is shown as curved and / or arcuate, in some non-limiting examples, this profile may be substantially linear and / or non-linear. As non-limiting examples, the thickness of conductive coating 830 may decrease in a manner that is, but is not limited to, substantially linear, exponential, and / or quadratic in the region proximal to the interface.
[0507] The contact angle θ of the conductive coating 830 at and / or near the interface between the conductive coating 830 and the NIC 810 c It has been observed that the contact angle θ of the nuclei can vary depending on the properties of the NIC810, such as the relative affinity and / or initial sticking probability S0. c It is contemplated that, in some non-limiting examples, the contact angle θ can determine the thin film contact angle of the deposited conductive coating 830. Referring to FIG. 31F as a non-limiting example, the contact angle θ c can be determined by measuring the slope of a tangent to the conductive coating 830 at or near the interface between the conductive coating 830 and the NIC 810. In some non-limiting examples where the cross-sectional taper profile of the conductive coating 830 is substantially linear, the contact angle θ c can be determined by measuring the gradient of the conductive coating 830 at and / or near the interface. As will be appreciated by those skilled in the art, the contact angle θ c Generally, the angle may be measured relative to the angle of the base surface. In this disclosure, for ease of illustration, the coatings 810, 830 are shown deposited on planar surfaces. However, one skilled in the art will understand that such coatings 810, 830 may be deposited on non-planar surfaces.
[0508] In some non-limiting examples, the contact angle θ of the conductive coating 830 cmay exceed about 90°. Referring now to FIG. 31G, by way of non-limiting example, conductive coating 830 is shown as including a portion that extends past the interface between NIC 810 and conductive coating 830, and is separated from the NIC by gap 3129. In such a non-limiting situation, contact angle θ c may be greater than about 90° in some non-limiting examples.
[0509] In some non-limiting examples, a relatively high contact angle θ c It may be advantageous to form a conductive coating 830 that exhibits a contact angle θ c may be greater than about 10°, greater than about 15°, greater than about 20°, greater than about 25°, greater than about 30°, greater than about 35°, greater than about 40°, greater than about 50°, greater than about 70°, greater than about 70°, greater than about 75°, and / or greater than about 80°. c Conductive coating 830 having a contact angle θ of greater than about 90° can enable the creation of finely patterned features while maintaining a relatively high aspect ratio. c It may be desirable to form a conductive coating 830 that exhibits a contact angle θ c may be greater than about 90°, greater than about 95°, greater than about 100°, greater than about 105°, greater than about 110°, greater than about 120°, greater than about 130°, greater than about 135°, greater than about 140°, greater than about 145°, greater than about 150°, and / or greater than about 170°.
[0510] 31H-31I, conductive coating 830 overlaps a portion of NIC 810 in a third portion 3130 of substrate 100, the third portion 3130 being disposed between first portion 3110 and second portion 3120 of substrate 100. As shown, the subset of conductive coating 830 that overlaps with the subset of NIC 810 may be in physical contact with its surface 3111. In some non-limiting examples, the overlap in third region 3130 may be formed as a result of lateral growth of conductive coating 830 during an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, surface 3111 of NIC 810 may exhibit a relatively low affinity or initial sticking probability S for the material of conductive coating 830, such that as the thickness of conductive coating 830 grows, the probability of material nucleating at layer surface 3111 is low, but conductive coating 830 may also grow laterally, covering the subset of NIC 810.
[0511] In the cases of FIGS. 31H to 31I, the contact angle θ of the conductive coating 830 c may be measured at its edge near the interface between the conductive coating 830 and the NIC 810, as shown. In FIG. 31I, the contact angle θ c may be greater than about 90°, which in some non-limiting examples can result in a subset of conductive coating 830 being separated from NIC 810 by gap 3129.
[0512] Partitions and recesses 32, a cross-sectional view of an example version 3200 of device 100 is shown. Device 3200 includes a substrate 110 having a layer surface 111. Substrate 110 includes at least one TFT structure 200. As a non-limiting example, at least one TFT structure 200 may be formed, in some non-limiting examples, by depositing and patterning a series of thin films during fabrication of substrate 110, as described herein.
[0513] The device 3200 includes a light-emitting region 1910 having an associated lateral side 410 and at least one adjacent non-light-emitting region 1920, each having an associated lateral side 420. A layer surface 111 of the substrate 110 within the light-emitting region 1910 includes a first electrode 120 electrically coupled to at least one TTF structure 200. A PDL 440 is provided on the layer surface 111 such that the PDL 440 covers the layer surface 111 and at least one edge and / or periphery of the first electrode 120. The PDL 440 may, in some non-limiting examples, be provided on the lateral side 420 of the non-light-emitting region 1920. The PDL 440 defines a valley-shaped configuration that provides an opening generally corresponding to the lateral side 410 of the light-emitting region 1910, through which the layer surface of the first electrode 120 may be exposed. In some non-limiting examples, the device 3200 may include multiple such openings defined by the PDL 400, each of which may correspond to a (sub)pixel 340 / 264x region of the device 3200.
[0514] As shown, in some non-limiting examples, a divider 3221 is provided on the layer surface 111 of the lateral side 420 of the non-emissive region 1920 to define a protected region 3065, such as a recessed region 3222, as described herein. In some non-limiting examples, the recessed region 3222 can be formed by an edge of a lower section 3323 ( FIG. 33A ) of the divider 3221 being recessed, staggered, and / or offset relative to an edge of an upper section 3324 ( FIG. 33A ) of the divider 3221 that overlaps and / or protrudes beyond the recessed region 3222.
[0515] In some non-limiting examples, the lateral side 410 of the light-emitting region 1910 includes at least one semiconductive layer 130 disposed on the first electrode 120, a second electrode 140 disposed on the at least one semiconductive layer 130, and a NIC 810 disposed on the second electrode 140. In some non-limiting examples, the at least one semiconductive layer 130, the second electrode 140, and the NIC 810 can extend laterally to cover at least the lateral side 420 of a portion of at least one adjacent non-light-emitting region 1920. In some non-limiting examples, as shown, the at least one semiconductive layer 130, the second electrode 140, and the NIC 810 can be disposed on at least a portion of the at least one PDL 440 and at least a portion of the divider 3221. Thus, as shown, the lateral sides 410 of the light-emitting region 1910, a portion of at least one adjacent non-light-emitting region 1920 and a portion of at least one PDL 440 and the lateral sides 420 of at least a portion of the partition 3221 can together form a first portion in which the second electrode 140 is located between the NIC 810 and the at least one semiconductive layer 130.
[0516] An auxiliary electrode 1750 is disposed adjacent to and / or within the recess 3221, and a conductive coating 830 is positioned to electrically couple the auxiliary electrode 1750 to the second electrode 140. Thus, as shown, the recess 3221 can include a second portion where the conductive coating 830 is disposed on the layer surface 111.
[0517] A non-limiting example of a method for manufacturing device 3200 will now be described.
[0518] At one stage, the method provides a substrate 110 and at least one TFT structure 200. In some non-limiting examples, at least some of the materials for forming the at least one semiconductive layer 130 may be deposited using an open-mask deposition process and / or a mask-free deposition process, such that the material is deposited into and / or across both lateral sides 410 of the light-emitting region 1910 and / or at least a portion of the lateral sides 420 of the at least one non-light-emitting region 1920. Those skilled in the art will understand that in some non-limiting examples, it may be appropriate to deposit the at least one semiconductive layer 130 in a manner that reduces reliance on patterned deposition (which, in some non-limiting examples, is performed using FMM).
[0519] At one stage, the method deposits a second electrode 140 on the at least one semiconductive layer 130. In some non-limiting examples, the second electrode 140 may be deposited using an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, the second electrode 140 may be deposited by exposing an exposed layer surface 111 of the at least one semiconductive layer 130 disposed on the lateral side 410 of the light emitting region 1910 and / or the lateral side 420 of at least a portion of at least one of the non-light emitting regions 1920 to an evaporated flux of a material for forming the second electrode 130.
[0520] At one stage, the method deposits NIC 810 on second electrode 140. In some non-limiting examples, NIC 810 may be deposited using an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, NIC 810 may be deposited by exposing exposed layer surface 111 of second electrode 140 disposed on lateral side 410 of light emitting region 1910 and / or at least a portion of lateral side 420 of at least one of non-light emitting regions 1920 to an evaporated flux of material for forming NIC 810.
[0521] As shown, recesses 3222 are substantially free of or not coated with NIC 810. In some non-limiting examples, this may be achieved by masking recesses 3222 at their lateral sides with partitions 3221 such that the evaporation flux of material for forming NIC 810 is substantially prevented from entering such recesses 3222 in layer surface 111. Thus, in such examples, recesses 3222 in layer surface 111 are substantially free of NIC 810. As a non-limiting example, a laterally protruding portion of partition 3221 may define recess 3222 at the base of partition 3221. In such examples, at least one surface of partition 3221 defining recess 3222 may also be substantially free of NIC 810.
[0522] At one stage, the method deposits a conductive coating 830 on the device 3200, in some non-limiting examples, after providing the NIC 810. In some non-limiting examples, the conductive coating 830 may be deposited using an open-mask deposition process and / or a mask-free deposition process. In some non-limiting examples, the conductive coating 830 may be deposited by exposing the device 3200 to an evaporation flux of the material for forming the conductive coating 830. As a non-limiting example, a source of the conductive coating 830 material (not shown) may be used to direct the evaporation flux of the material for forming the conductive coating 830 toward the device 3200 so that the evaporation flux is incident on such surface. However, in some non-limiting examples, the surface of the NIC 810 disposed on at least a portion of the lateral side 420 of at least one of the lateral sides 410 of the light-emitting region 1910 and / or the non-light-emitting region 1920 exhibits a relatively low initial adhesion probability S0 for the conductive coating 830, and the conductive coating 830 may be selectively deposited on a second portion, including, but not limited to, a recessed portion of the device 3200 where the NIC 810 is not present.
[0523] In some non-limiting examples, at least a portion of the evaporation flux of materials for forming conductive coating 830 can be directed at a non-perpendicular angle relative to a lateral plane of layer surface 111. By way of non-limiting example, at least a portion of the evaporation flux can be incident on device 3200 at an angle of incidence, i.e., less than 90°, less than about 85°, less than about 80°, less than about 75°, less than about 70°, less than about 60°, and / or less than about 50°, relative to such lateral plane of layer surface 111. By directing the evaporation flux of materials for forming conductive coating 830 (including at least a portion thereof incident at a non-perpendicular angle), at least one surface of recess 3222 and / or at least one surface therein can be exposed to such evaporation flux.
[0524] In some non-limiting examples, the likelihood that such evaporative flux will be prevented from impinging on at least one surface of recess 3222 and / or at least one surface therein due to the presence of partition 3221 may be reduced because at least a portion of such evaporative flux may flow at a non-perpendicular angle of incidence.
[0525] In some non-limiting examples, at least a portion of such evaporation flux may be uncollimated. In some non-limiting examples, at least a portion of such evaporation flux may be generated by an evaporation source that is a point source, a linear source, and / or a surface source.
[0526] In some non-limiting examples, device 3200 can be displaced during deposition of conductive coating 830. As non-limiting examples, device 3200 and / or its substrate 110 and / or any layers deposited thereon can undergo angular displacement in a lateral aspect and / or in an aspect substantially parallel to a cross-sectional aspect.
[0527] In some non-limiting examples, the device 3200 can be rotated about an axis that is substantially perpendicular to the lateral plane of the layer surface 111 while exposed to the evaporative flux.
[0528] In some non-limiting examples, at least a portion of such evaporation flux can be directed toward the layer surface 111 of the device 3200 in a direction substantially perpendicular to the lateral plane of the surface.
[0529] Without wishing to be bound by any particular theory, it is believed that material for forming conductive coating 830 may nevertheless be deposited within recesses 3222 due to lateral migration and / or desorption of adatoms adsorbed on the surface of NIC 810. In some non-limiting examples, it is believed that adatoms adsorbed on the surface of NIC 810 may tend to migrate and / or desorb from such surfaces due to unfavorable thermodynamic properties of the surfaces for forming stable nuclei. In some non-limiting examples, it is believed that at least some of the adatoms that migrate and / or desorb from such surfaces may be redeposited on the surfaces within recesses 3222 to form conductive coating 830.
[0530] In some non-limiting examples, the conductive coating 830 can be formed such that the conductive coating 830 is electrically coupled to both the auxiliary electrode 1750 and the second electrode 140. In some non-limiting examples, the conductive coating 830 is in physical contact with at least one of the auxiliary electrode 1750 and / or the second electrode 140. In some non-limiting examples, an intermediate layer can be present between the conductive coating 830 and at least one of the auxiliary electrode 1750 and / or the second electrode 140. However, in such examples, such an intermediate layer does not substantially prevent the conductive coating 830 from being electrically coupled to at least one of the auxiliary electrode 1750 and / or the second electrode 140. In some non-limiting examples, such an intermediate layer can be relatively thin to allow electrical coupling therethrough. In some non-limiting examples, the sheet resistance of the conductive coating 830 can be equal to and / or less than the sheet resistance of the second electrode 140.
[0531] 32 , recessed portion 3222 is substantially free of second electrode 140. In some non-limiting examples, during deposition of second electrode 140, recessed portion 3222 is masked by partition 3221 to substantially prevent an evaporation flux of material for forming second electrode 140 from impinging on at least one surface of recessed portion 3222 and / or at least one surface therein. In some non-limiting examples, at least a portion of the evaporation flux of material for forming second electrode 140 is incident on at least one surface of recessed portion 3222 and / or at least one surface therein such that second electrode 140 extends to cover at least a portion of recessed portion 3222.
[0532] In some non-limiting examples, auxiliary electrodes 1750, conductive coatings 830, and / or dividers 3221 may be selectively provided in specific regions of a display panel. In some non-limiting examples, any of these features may be provided at and / or near one or more edges of such a display panel to electrically couple at least one element of front plane 10, including but not limited to second electrode 140, to at least one element of backplane 20. In some non-limiting examples, providing such features at and / or near such edges may facilitate supplying and distributing current from auxiliary electrodes 1750 positioned at and / or near such edges to second electrodes 140. In some non-limiting examples, such a configuration may facilitate reducing the bezel size of a display panel.
[0533] In some non-limiting examples, auxiliary electrodes 1750, conductive coating 830, and / or dividers 3221 may be omitted from certain regions of such a display panel. In some non-limiting examples, such features may be omitted from portions of a display panel, including but not limited to, other than at least one edge of and / or adjacent to the edge of the display panel, if a relatively high pixel density is provided.
[0534] FIG. 33A shows a fragment of device 3200 in a region proximal to partition 3221, prior to deposition of at least one semiconductive layer 130. In some non-limiting examples, partition 3221 includes a lower section 3323 and an upper section 3324, the upper section 3324 overhanging the lower section 3323 such that the lower section 3323 forms a recess 3222 that is recessed laterally relative to the upper section 3324. As a non-limiting example, recess 3222 can be formed such that it extends substantially laterally into partition 3221. In some non-limiting examples, recess 3221 can correspond to a space defined between a ceiling 3325 defined by upper section 3324, a side surface 3326 of lower section 3323, and a floor 3327 that corresponds to layer surface 111 of substrate 110. In some non-limiting examples, upper section 3324 includes an angled section 3328. As a non-limiting example, the angled section 3328 may be provided by a surface that is not substantially parallel to the lateral plane of the layer surface 111. As a non-limiting example, the angled section may be defined by an angle θ p The angled section 3328 may be angled and / or offset from an axis substantially perpendicular to the layer surface 111. A lip 3329 is also provided by the top section 3324. In some non-limiting examples, the lip 3329 may be provided at or near the opening of the recess 3222. As a non-limiting example, the lip 3329 may be provided at the junction of the angled section 3328 and the ceiling 3325. In some non-limiting examples, at least one of the top section 3324, the sides 3326, and the floor 3327 may be conductive to form at least a portion of the auxiliary electrode 1750.
[0535] In some non-limiting examples, the angle θ represents the angle at which the angled section 3328 of the top section 3324 is tilted and / or offset from the axis. pmay be about 60° or less. By way of non-limiting example, the angle may be about 50° or less, about 45° or less, about 40° or less, about 30° or less, about 25° or less, about 20° or less, about 15° or less, and / or about 10° or less. In some non-limiting examples, the angle may be between about 60° and about 25°, between about 60° and about 30°, and / or between about 50° and about 30°. Without wishing to be bound by theory, it can be postulated that providing an angled section 3328 may inhibit deposition of material to form the NIC 810 at or near the lip 3329 so as to facilitate deposition of material to form the conductive coating 830 at or near the lip 3229.
[0536] 33B-33P illustrate various non-limiting examples of the fragment of device 3200 shown in FIG. 33A after the step of depositing conductive coating 830. For ease of illustration, FIGS. 33B-33P do not always show all features of partition 3221 and / or recess 3222 as described in FIG. 33A , and omit auxiliary electrode 1750, although one skilled in the art will understand that such features and / or auxiliary electrode 1750 may nevertheless be present in some non-limiting examples. One skilled in the art will understand that auxiliary electrode 1750 may be present in any of the examples in FIGS. 33B-33P in any form and / or position, including, but not limited to, those shown in any of the examples in FIGS. 34A-34G described herein.
[0537] In these figures, a device stack 3310 is shown that includes at least one semiconducting layer 130, a second electrode 140, and a NIC 810 deposited on a top section 3324.
[0538] In these figures, the remaining device stack 3311 is shown including at least one semiconductive layer 130, second electrode 140, and NIC 810 deposited on the substrate 100 beyond the partition 3221 and recess 3222. From a comparison with FIG. 32, it will be seen that the remaining device stack 3311 may, in some non-limiting examples, correspond to the semiconductive layer 130, second electrode 140, and NIC 810 as it approaches the recess 3221 of and / or adjacent to the lip 3329. In some non-limiting examples, the remaining device stack 3311 may be formed when open-mask and / or mask-free deposition processes are used to deposit the various materials of the device stack 3310.
[0539] 33B, the conductive coating 830 remains in and / or substantially fills all of the recesses 3222. Thus, in some non-limiting examples, the conductive coating 830 may be in physical contact with the ceiling 3325, the sides 3326, and the floor 3327 and thus electrically coupled to the auxiliary electrode 1750.
[0540] Without wishing to be bound by any particular theory, it can be assumed that substantially filling all of the recesses 3222 may reduce the likelihood of unwanted substances (including, but not limited to, gases) becoming trapped within the recesses 3222 during fabrication of the device 3200.
[0541] In some non-limiting examples, the bonding and / or contact region (CR) may correspond to a region of the device 3200 where the conductive coating 830 is in physical contact with the device stack 3310 to electrically couple the second electrode 140 to the conductive coating 830. In some non-limiting examples, the CR extends from about 50 nm to about 1500 nm from the edge of the device stack 3310 proximate the divider 3221. As non-limiting examples, the CR may extend from about 50 nm to about 1000 nm, from about 100 nm to about 500 nm, from about 100 nm to about 350 nm, from about 100 nm to about 300 nm, from about 150 nm to about 300 nm, and / or from about 100 nm to about 200 nm. In some non-limiting examples, the CR may extend substantially laterally away from the edge of the device stack 3310 into the device stack 3310 by such a distance.
[0542] In some non-limiting examples, the edges of the remaining device stack 3311 may be formed by at least one semiconductive layer 130, second electrode 140, and NIC 810, and the edges of the second electrode 140 may be coated and / or covered by NIC 810. In some non-limiting examples, the edges of the remaining device stack 3311 may be formed in other configurations and / or arrangements. In some non-limiting examples, the edges of the NIC 810 may be recessed relative to the edges of the second electrode 140 such that the edges of the second electrode 140 may be exposed such that the CR may include the exposed edges of the second electrode 140 so that the second electrode 140 can make physical contact with the conductive coating 830 and electrically couple them. In some non-limiting examples, the edges of the at least one semiconductive layer 130, second electrode 140, and NIC 810 may be aligned with one another such that the edges of each layer are exposed. In some non-limiting examples, the edges of the second electrode 140 and the NIC 810 may be recessed relative to the edges of at least one semiconductive layer 130 such that the edges of the remaining device stack 3311 are substantially provided by the semiconductive layer 130.
[0543] Additionally, as shown, in some non-limiting examples, within the small CR, the conductive coating 830 is disposed at and / or near the lip 3329 of the divider 3221, and extends to cover at least the edges of the NIC 810 in the remaining device stack 3311 disposed closest to the divider 3221. In some non-limiting examples, the NIC 810 may include a semiconductive material and / or an insulating material.
[0544] While it is described herein that direct deposition of material for forming conductive coating 830 onto the surface of NIC 810 is generally inhibited, it has been discovered that in some non-limiting examples, a portion of conductive coating 830 may nevertheless overlap at least a portion of NIC 810. As a non-limiting example, during deposition of conductive coating 830, material for forming conductive coating 830 may be initially deposited within recessed portion 3221. Thereafter, as deposition of material for forming conductive coating 830 continues, in some non-limiting examples, conductive coating 830 extends laterally beyond recessed portion 830a and overlaps at least a portion of NIC 810 in the remainder of device stack 3311.
[0545] Those skilled in the art will understand that while conductive coating 830 is shown overlapping a portion of NIC 810, lateral extent 410 of light emitting region 1910 remains substantially free of the material forming conductive coating 830. In some non-limiting examples, conductive coating 830 may be disposed within lateral extent 420 of at least a portion of at least one non-light emitting region 1920 of device 3200 without substantially interfering with the emission of photons from light emitting region 1910 of device 3200.
[0546] In some non-limiting examples, the conductive coating 830 may nevertheless be electrically coupled to the second electrode 140 despite the NIC 810 being interposed therebetween to reduce the effective sheet resistance of the second electrode 140.
[0547] In some non-limiting examples, the NIC 810 may be formed using a conductive material and / or may otherwise exhibit a level of charge mobility that allows current to tunnel and / or pass through the NIC 810.
[0548] In some non-limiting examples, the NIC 810 can have a thickness that allows electrical current to pass through the NIC 810. In some non-limiting examples, the thickness of the NIC 810 can be about 3 nm to about 65 nm, about 3 nm to about 50 nm, about 5 nm to about 50 nm, about 5 nm to about 30 nm, and / or about 5 nm to about 15 nm, about 5 nm to about 10 nm. In some non-limiting examples, the NIC 810 can be provided with a relatively thin thickness (in some non-limiting examples, a thin coating thickness) to reduce contact resistance that may arise in the path of such electrical current due to the presence of the NIC 810.
[0549] Without wishing to be bound by any particular theory, it can be assumed that substantially filling all of the recesses 3221 can, in some non-limiting examples, increase the reliability of the electrical coupling between the conductive coating 830 and at least one of the second electrode 140 and the auxiliary electrode 1750.
[0550] Additionally, as shown, in some non-limiting examples, the conductive coating 830 extends to cover at least a portion of the NIC 810 disposed on the top section 3324 of the divider 3221. In some non-limiting examples, a portion of the NIC 810 at and / or adjacent to the lip 3329 may be covered by the conductive coating 830. In some non-limiting examples, the conductive coating 830 may nevertheless be electrically coupled to the second electrode 140 despite the NIC 810 interposed therebetween.
[0551] 33C , the conductive coating 830 substantially remains in and / or partially fills the recess 3222. Thus, in some non-limiting examples, the conductive coating 830 can be in physical contact with at least a portion of the side 3326, the floor 3327, and, in some non-limiting examples, the ceiling 3325, and thus be electrically coupled to the auxiliary electrode 1750.
[0552] As shown, in some non-limiting examples, at least a portion of the ceiling 3325 is substantially free of the conductive coating 830. In some non-limiting examples, such portion is adjacent the lip 3329.
[0553] Additionally, as shown, in some non-limiting examples, within a small CR located at and / or near the lip 3329 of the partition 3221, the conductive coating 830 extends to cover at least the edges of the NICs 810 within the remaining device stack 3311 located closest to the partition 3221. In some non-limiting examples, the conductive coating 830 may nevertheless be electrically coupled to the second electrode 140 despite the NICs 810 interposed therebetween.
[0554] 33D , the conductive coating 830 substantially remains in and / or partially fills the recess 3222. Thus, in some non-limiting examples, the conductive coating 830 may be in physical contact with the floor 3327 and, in some non-limiting examples, at least a portion of the side surface 3326, and thus electrically coupled to the auxiliary electrode 1750.
[0555] As shown, in some non-limiting examples, the ceiling 3325 is substantially free of the conductive coating 830.
[0556] Additionally, as shown, in some non-limiting examples, within a small CR located at and / or near the lip 3329 of the partition 3221, the conductive coating 830 extends to cover at least the edges of the NICs 810 within the remaining device stack 3311 located closest to the partition 3221. In some non-limiting examples, the conductive coating 830 may nevertheless be electrically coupled to the second electrode 140 despite the NICs 810 interposed therebetween.
[0557] 33E, the conductive coating 83...
Claims
1. 1. An optoelectronic device, comprising: a nucleation inhibiting coating (NIC) disposed on a first layer surface of the device at a first portion of a lateral side of the device; a conductive coating disposed on a second layer surface of the device at a second portion of the lateral side of the device; an initial sticking probability for forming the conductive coating on a surface of the NIC in the first portion is lower than the initial sticking probability for forming the conductive coating on the surface in the second portion, such that the surface of the NIC in the first portion is substantially free of the conductive coating, where "substantially free of the conductive coating" means that the light transmission therethrough is greater than 90%; the NIC comprises at least one compound of formula (I), (II), (III), (IV), (V), (VI), (VII), (VIII), (IX), (X), (XI), (XII), (XIII), (XIV), (XV), (XVI), (XVII), (XVIII), (XIX), and (XX); 【Table 13-1】 【Table 13-2】 During the ceremony, L 1 However, independently, C, CR 2 , C.R. 2 R 3 , N.R. 3 , S, O, a substituted or unsubstituted cycloalkylene group having 3 to 6 carbon atoms, a substituted or unsubstituted arylene group having 5 to 60 carbon atoms, or a substituted or unsubstituted heteroarylene group having 4 to 60 carbon atoms; Ar 1 independently represent a substituted or unsubstituted aryl group having 5 to 60 carbon atoms, a substituted or unsubstituted haloaryl group having 5 to 60 carbon atoms, or a substituted or unsubstituted heteroaryl group having 4 to 60 carbon atoms; R 1 , R 2 , and R 3 are independently H, D (deuterium), F, Cl, alkyl including C1-C6 alkyl, cycloalkyl including C3-C6 cycloalkyl, alkoxy including C1-C6 alkoxy, fluoroalkyl, haloaryl, heteroaryl, haloalkenyl, koxy, fluoroaryl, fluoroalkoxy, fluoroalkylsulfanyl, fluoromethyl, difluoromethyl, trifluoromethyl, difluoromethoxy, trifluoromethoxy, fluoroethyl, polyfluoroethyl, 4-fluorophenyl, 3,4,5-trifluorophenyl, polyfluoroaryl, 4-(trifluoromethoxy)phenyl, SF 4 Cl, S.F. 5 , (CF 2 ) a Science fiction 5 , (O(CF 2 ) b ) d CF 3 , (CF 2 ) e (O(CF 2 ) b ) d ) CF 3 or trifluoromethylsulfanyl, Z independently represents F or Cl; s represents an integer from 0 to 4, and the sum of r and s is 5; r represents an integer from 1 to 3; p represents an integer from 0 to 6; q represents an integer from 1 to 8; v represents an integer from 2 to 4; j represents an integer from 1 to 3; k represents an integer from 1 to 4; t represents an integer from 2 to 6; u represents an integer from 0 to 2, the sum of r and u is 3, h represents an integer from 0 to 4, and the sum of r and h is 4; i represents an integer from 1 to 4; a represents an integer from 2 to 6; b represents an integer from 1 to 4; d represents an integer from 1 to 3; e represents an integer from 1 to 4; With the proviso that at least one compound of the formulas (I), (II), (III), (IV), (V), (VI), (VII), (VIII), (IX), (X), (XI), (XII), (XIII), (XIV), (XV), (XVI), (XVII), (XVIII), (XIX), and (XX) is selected from the group consisting of compounds (SF4), (SF7), (SF9), (SF21), (SF24), (SF25), (SF170), (SF316), (SF317), (SF319), (SF357), (SF358), (SF359), and (SF361): 【Chemistry 1A】 【Chemistry 1B】 【Chemistry 1C】 Not one of the Optoelectronic devices.
2. The optoelectronic device of claim 1 , wherein the first portion comprises at least one light emitting region.
3. The optoelectronic device of claim 1 , wherein the second portion comprises at least a portion of a non-emissive region.
4. 4. The optoelectronic device of claim 2 or 3, wherein a thickness of the NIC in the at least one light emitting region of the first portion is adjusted to adjust its optical microcavity effect.
5. 5. The optoelectronic device of claim 1, further comprising a first electrode, a second electrode, and a semiconductive layer between the first electrode and the second electrode, the second electrode extending between the NIC and the semiconductive layer in the first portion.
6. The optoelectronic device of claim 5 , wherein the conductive coating is electrically coupled to the second electrode.
7. An optoelectronic device according to claim 5 or 6, wherein the conductive coating coats at least a portion of the second electrode within the second portion.
8. An optoelectronic device according to any one of claims 5 to 7, comprising at least one intermediate coating between said second electrode and said conductive coating along at least a portion of said conductive coating.
9. The optoelectronic device of claim 8 , wherein the intermediate coating comprises a nucleation promoting coating (NPC).
10. 10. An optoelectronic device as claimed in claim 8 or 9, wherein the intermediate coating comprises a NIC that has been processed to increase the initial adhesion probability for forming the conductive coating on the surface of the NIC.
11. The optoelectronic device of claim 10 , wherein the intermediate coating is processed by exposure to radiation.
12. 12. The optoelectronic device of claim 5, wherein the second portion comprises a partition and a third electrode in a protected area of the partition, and the conductive coating is electrically coupled to the second electrode and the third electrode.
13. The optoelectronic device of claim 12 , wherein the protected area is free of the NIC.
14. An optoelectronic device according to claim 12 or 13, wherein the protected area comprises a recess defined by the partition.
15. An optoelectronic device according to any one of claims 12 to 14, wherein the conductive coating is in physical contact with the third electrode.
16. The optoelectronic device according to any one of claims 12 to 15, wherein the conductive coating is electrically coupled to the second electrode in a coupling region (CR).
17. An optoelectronic device according to any one of claims 12 to 16, wherein the protected area comprises an aperture defined by the partition.
18. 20. The optoelectronic device of claim 17, wherein the aperture is angled with respect to an axis extending normal away from a surface of the device.
19. 19. An optoelectronic device according to claim 17 or 18, further comprising an undercut portion overlapping a third layer surface of the third electrode in a cross-sectional side.
20. 20. The optoelectronic device of any one of claims 2 to 19, wherein at least a second portion of the second portion overlaps at least a first portion of the first portion, and a cross-sectional thickness of the conductive coating within the second portion is less than a cross-sectional thickness of the conductive coating within a remaining portion of the second portion.
21. 21. The optoelectronic device of claim 20, wherein the conductive coating is disposed on the NIC along at least a section of the first portion proximate to the first portion.
22. 22. The optoelectronic device of claim 21, wherein the conductive coating is spaced from the NIC in a cross-sectional side view.
23. 23. An optoelectronic device as claimed in claim 20 or 22, wherein the conductive coating abuts the NIC at an interface between the first and second portions.
24. 24. The optoelectronic device of claim 23, wherein said conductive coating forms a contact angle with said NIC at said interface.
25. 25. The optoelectronic device of claim 24, wherein the contact angle is greater than 10 degrees.
26. 26. An optoelectronic device according to claim 24 or 25, wherein the contact angle is greater than 90 degrees.
27. An optoelectronic device according to any one of claims 2 to 11, wherein at least a first part of the first portion overlaps at least a second part of the second portion.
28. 30. The optoelectronic device of claim 27, wherein the NIC is disposed on the surface of the device within the second portion, and the conductive coating is disposed therein on the NIC.
29. 30. The optoelectronic device of claim 28, wherein the conductive coating is spaced from the NIC in a cross-sectional side view.
30. 30. An optoelectronic device according to any one of claims 20 to 29 when dependent on claim 2, wherein the second portion extends between the first portion and a third portion of the second portion that includes the at least one light emitting region.
31. 31. The optoelectronic device of claim 30, wherein the at least one light emitting region of the third portion comprises a first electrode, a second electrode electrically coupled to the conductive coating, and a semiconductive layer between the first electrode and the second electrode, the second electrode extending between the NIC and the semiconductive layer in the third portion.
32. The optoelectronic device according to any one of claims 2 to 31, wherein the conductive coating is electrically coupled to an auxiliary electrode.
33. 33. The optoelectronic device of claim 32, wherein the conductive coating is in physical contact with the auxiliary electrode.
34. 34. An optoelectronic device according to claim 32 or 33 when dependent on claim 30 or 31, wherein the auxiliary electrode is on the first part.
35. An optoelectronic device according to any one of claims 5 to 11, wherein the second portion comprises at least one additional light emissive region.
36. 36. The optoelectronic device of claim 35, wherein at least one of the additional light emitting regions in the second portion of the device comprises a first electrode, a second electrode, and a semiconductive layer between the first electrode and the second electrode, the second electrode comprising the conductive coating.
37. 36. The optoelectronic device of claim 35, wherein a wavelength of light emitted from the at least one additional light-emitting region in the second portion of the device is different from a wavelength of light emitted from the at least one light-emitting region in the first portion of the device.
38. An optoelectronic device according to any one of claims 5 to 31, wherein the conductive coating comprises an auxiliary electrode.
39. The optoelectronic device of claim 1 , wherein the second portion comprises at least one light emitting region.
40. 40. The optoelectronic device of claim 39, wherein the first portion comprises at least a portion of a non-emissive region. device.
41. 41. An optoelectronic device according to claim 39 or 40, wherein the first portion is optically transparent through said first portion.
42. 42. The optoelectronic device of any one of claims 39 to 41, further comprising a first electrode, a second electrode, and a semiconductive layer between the first electrode and the second electrode, the second electrode extending between the NIC and the semiconductive layer in the first portion.
43. 43. The optoelectronic device of claim 42, wherein the second electrode extends between the conductive coating and the semiconductive layer in the second portion.
44. 44. An optoelectronic device according to any one of claims 39 to 43, further comprising a first electrode, a semi-conductive layer between the first electrode and the conductive coating, the conductive coating comprising a second electrode of the device.
45. Ar 1 45. An optoelectronic device according to any one of claims 1 to 44, wherein represents cyclopentadienyl, phenyl, 1-naphthyl, 2-naphthyl, 1-phenanthryl, 2-phenanthryl, 10-phenanthryl, 9-phenanthryl, 1-anthracenyl, 2-anthracenyl, 3-anthracenyl, 9-anthracenyl, benzanthracenyl, pyrenyl, chrysenyl, fluorenyl, pentacenyl, pyridine, quinoline, isoquinoline, pyrazine, quinoxaline, arcidine, pyrimidine, quinazoline, pyridazine, cinnoline, or phthalzine.
46. Each R 1 , R 2 , and R 3 are each independently H, D, F, Cl, methyl, methoxy, ethyl, t-butyl, fluoromethyl, difluoromethyl, trifluoromethyl, fluoromethoxy, difluoromethoxy, trifluoromethoxy, fluoroethyl, polyfluoroethyl, fluorophenyl, trifluorophenyl, trifluoromethoxyphenyl, SF 4 Cl, or SF 5 An optoelectronic device according to any one of claims 1 to 45, wherein
47. L 1 47. An optoelectronic device according to any one of claims 1 to 46, wherein represents cyclohexylene, phenylene, indenylene, naphthylene, fluorenylene, anthracylene, phenanthrylene, pyrylene, chrysenylene, cyclopentylene, or a heteroarylene group derived by replacing 1, 2, 3 or 4 ring carbon atoms of an arylene group with the corresponding number of heteroatoms.
48. 48. The optoelectronic device of claim 47, wherein the heteroarylene group comprises one or more heteroatoms individually selected from nitrogen, oxygen, sulfur, and silicon.
Citation Information
Patent Citations
Organic el display panel and its manufacturing method
JP2009266803A
Display device including auxiliary electrode
JP2018109758A
Surfaces containing patterned coatings and methods of patterning coatings on devices
JP2018533183A
Materials for forming nucleation-inhibiting coatings and devices incorporating same
JP2021512467A