Positive electrode plate for non-aqueous secondary battery, non-aqueous secondary battery, method for manufacturing positive electrode plate for non-aqueous secondary battery, and method for manufacturing non-aqueous secondary battery
By optimizing the specific surface area and density of the positive electrode plate in non-aqueous secondary batteries with carbon nanotubes and a non-aqueous solvent, the internal resistance, overcharge resistance, and storage characteristics are improved, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2022128381
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-08-10
AI Technical Summary
Existing non-aqueous secondary batteries do not fully optimize the specific surface area of the positive electrode plate, leading to issues with internal resistance, overcharge resistance, and storage characteristics.
The specific surface area of the positive electrode plate is adjusted to be between 1.5 m²/g and 3.0 m²/g, with a difference of 0.66 m²/g to 1.8 m²/g after manufacturing, using a positive electrode active material with a density of 2.2 g/cm³ to 3.0 g/cm³, and incorporating a highly conductive material like carbon nanotubes or nanofibers, and a non-aqueous solvent to minimize new surface formation during pressing.
This approach reduces internal resistance, overcharge resistance, and storage characteristic deterioration, enhancing the overall performance of non-aqueous secondary batteries.
Smart Images

Figure 0007576762000001 
Figure 0007576762000002 
Figure 0007576762000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode plate for a non-aqueous secondary battery, a non-aqueous secondary battery, a method for manufacturing a positive electrode plate for a non-aqueous secondary battery, and a method for manufacturing a non-aqueous secondary battery, and more particularly to a positive electrode plate for a non-aqueous secondary battery, a non-aqueous secondary battery, a method for manufacturing a positive electrode plate for a non-aqueous secondary battery, and a method for manufacturing a non-aqueous secondary battery that can improve the characteristics of the non-aqueous secondary battery. [Background technology]
[0002] Conventionally, non-aqueous secondary batteries include an electrode assembly having a negative electrode plate, a positive electrode plate, and a separator. Such an electrode assembly is housed in a battery case together with a non-aqueous electrolyte, with the negative electrode plate, the positive electrode plate, and the separator stacked in a stacking direction. In each electrode plate, an electrode mixture layer is formed on an electrode base material, and the electrode mixture layer contains at least an active material. When manufactured as each electrode plate, the specific surface area of the electrode plate affects the characteristics of the non-aqueous secondary battery, such as the capacity of the non-aqueous secondary battery.
[0003] As a method for producing such a non-aqueous secondary battery, for example, Patent Document 1 discloses a method for producing a non-aqueous secondary battery having a specific surface area of 0.6 to 1.5 m 2 The positive electrode plate has a specific surface area of 0.5 to 2 m 2 / g or less, thereby making it possible to provide a nonaqueous secondary battery with excellent discharge characteristics and output characteristics. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-272611 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the invention described in Patent Document 1, it is desired to further improve the characteristics of nonaqueous secondary batteries by using a new index for the specific surface area in the production of positive electrode plates. [Means for solving the problem]
[0006] An embodiment of a positive electrode plate for a nonaqueous secondary battery that solves the above problems will be described below. [Aspect 1] A positive electrode plate for a non-aqueous secondary battery comprising a positive electrode substrate and a positive electrode mixture layer containing at least a positive electrode active material, the positive electrode plate having a specific surface area of 1.5 m before manufacture. 2 / g or more 3.0m 2 / g or less, and a difference between a specific surface area of the positive electrode plate for a nonaqueous secondary battery after the production of the positive electrode plate for a nonaqueous secondary battery and a specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less.
[0007] According to the above configuration, it is possible to suppress the deterioration of the internal resistance of the nonaqueous secondary battery while minimizing the formation of new surfaces of the positive electrode active material, thereby suppressing the deterioration of the overcharge resistance and the deterioration of the storage characteristics of the nonaqueous secondary battery, thereby improving the characteristics of the nonaqueous secondary battery.
[0008] An embodiment of a nonaqueous secondary battery that solves the above problems will be described below. [Aspect 2] A nonaqueous secondary battery including a positive electrode plate having a positive electrode substrate and a positive electrode mixture layer containing at least a positive electrode active material, the positive electrode plate having a specific surface area of 1.5 m before manufacture. 2 / g or more 3.0m 2 / g or less, and the difference between the specific surface area of the positive plate after the manufacture of the positive plate and the specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less.
[0009] Various aspects of a method for producing a positive electrode plate for a nonaqueous secondary battery that solves the above problems will be described below. [Aspect 3] A method for producing a positive electrode plate for a non-aqueous secondary battery comprising a positive electrode substrate and a positive electrode mixture layer containing at least a positive electrode active material, the method comprising the steps of: 2 / g or more 3.0m 2 / g or less, and a difference between a specific surface area of the positive electrode plate for a nonaqueous secondary battery after the production of the positive electrode plate for a nonaqueous secondary battery and a specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less.
[0010] [Aspect 4] In the method for producing a positive electrode plate for a non-aqueous secondary battery according to [Aspect 3], after the production of the positive electrode plate for a non-aqueous secondary battery, the density of the positive electrode mixture layer is 2.2 g / cm 3 Above 3.0 g / cm 3 The following is a method for producing a positive electrode plate for a nonaqueous secondary battery.
[0011] According to the above-described configuration, it is possible to suppress deterioration of the internal resistance of the nonaqueous secondary battery while suppressing deterioration of the overcharge resistance and the storage characteristics, thereby improving the characteristics of the nonaqueous secondary battery.
[0012] [Aspect 5] The method for producing a positive electrode plate for a nonaqueous secondary battery according to [Aspect 3] or [Aspect 4], wherein the positive electrode active material is a ternary positive electrode active material. According to the above-mentioned configuration, even when compared with a positive electrode active material using, for example, lithium manganate, etc., it is possible to improve the charge-discharge cycle characteristics of the nonaqueous secondary battery while suppressing deterioration of the internal resistance, overcharge resistance, and storage characteristics of the nonaqueous secondary battery, thereby improving the characteristics of the nonaqueous secondary battery.
[0013] [Aspect 6] In the method for producing a positive electrode plate for a non-aqueous secondary battery according to any one of [Aspects 3] to [Aspect 5], the positive electrode mixture layer contains a positive electrode conductive material, and the positive electrode conductive material has a specific surface area of 150 m before the production of the positive electrode plate for a non-aqueous secondary battery.2 / g or more 300m 2 The positive electrode plate for a non-aqueous secondary battery is either a carbon nanotube or a carbon nanofiber having a molecular weight of 1000 or less.
[0014] According to the above-mentioned configuration, by using a highly conductive positive electrode conductive material, it is possible to suppress deterioration of the internal resistance of the nonaqueous secondary battery, and therefore to improve the characteristics of the nonaqueous secondary battery.
[0015] [Aspect 7], in the method for producing a positive electrode plate for a non-aqueous secondary battery according to any one of [Aspect 3] to [Aspect 6], the positive electrode composite layer is provided on the positive electrode substrate by applying a positive electrode composite paste containing at least the positive electrode active material and a positive electrode solvent to the positive electrode substrate and drying the applied positive electrode composite paste, and the positive electrode solvent is a non-aqueous solvent.
[0016] According to the above-mentioned configuration, compared to an aqueous solvent, it is possible to suppress the decrease in the amount of the positive electrode active material, to reduce the difference in specific surface area, and to suppress the deterioration of the overcharge resistance, thereby improving the characteristics of the nonaqueous secondary battery.
[0017] An embodiment of a method for producing a nonaqueous secondary battery that solves the above problems will be described below. [Embodiment 8] A method for producing a nonaqueous secondary battery including a positive electrode plate having a positive electrode substrate and a positive electrode mixture layer containing at least a positive electrode active material, the method comprising the steps of: 2 / g or more 3.0m 2 / g or less, and after the positive electrode plate is manufactured, the density of the positive electrode mixture layer is 2.2 g / cm 3 Above 3.0 g / cm 3 and the difference between the specific surface area of the positive electrode plate after production and the specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less. Effect of the Invention
[0018] According to the present invention, the characteristics of a nonaqueous secondary battery can be improved. [Brief description of the drawings]
[0019] [Figure 1] 1 is a perspective view of a lithium-ion secondary battery according to an embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of a laminate of an electrode body of a lithium ion secondary battery. [Diagram 3] 1 is a flowchart showing a source process for an electrode plate for a lithium ion secondary battery. [Figure 4] 1 is a schematic diagram showing an example and a comparative example of a lithium ion secondary battery. [Diagram 5] FIG. 2 is a schematic diagram showing a positive electrode plate. [Figure 6] FIG. 2 is a schematic diagram showing a positive electrode plate. [Figure 7] FIG. 2 is a schematic diagram showing a positive electrode plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] [Present embodiment] Hereinafter, an embodiment of a positive electrode plate for a nonaqueous secondary battery, a nonaqueous secondary battery, a method for manufacturing a positive electrode plate for a nonaqueous secondary battery, and a method for manufacturing a nonaqueous secondary battery will be described.
[0021] <Lithium-ion secondary battery 10> As an example of the nonaqueous secondary battery, the configuration of a lithium ion secondary battery will be described. As shown in FIG. 1, the lithium ion secondary battery 10 is configured as a cell battery. The lithium ion secondary battery 10 includes a battery case 11. The battery case 11 includes a lid body 12. The battery case 11 includes an opening (not shown) on the upper side. The lid body 12 seals the opening. The battery case 11 is made of a metal such as an aluminum alloy. The lid body 12 includes a negative electrode external terminal 13 and a positive electrode external terminal 14 used for charging and discharging power. The negative electrode external terminal 13 and the positive electrode external terminal 14 may have any shape.
[0022] The lithium ion secondary battery 10 includes an electrode assembly 15. The lithium ion secondary battery 10 includes a negative electrode current collector 16 and a positive electrode current collector 17. The negative electrode current collector 16 connects the negative electrode of the electrode assembly 15 to a negative electrode external terminal 13. The positive electrode current collector 17 connects the positive electrode of the electrode assembly 15 to a positive electrode external terminal 14. The electrode assembly 15 is accommodated inside a battery case 11.
[0023] The lithium ion secondary battery 10 includes a nonaqueous electrolyte 18. The nonaqueous electrolyte 18 is injected into the battery case 11 through an injection hole (not shown). The lithium ion secondary battery 10 is configured as a sealed battery container by attaching a lid 12 to an opening in the battery case 11. In this manner, the battery case 11 contains the electrode assembly 15 and the nonaqueous electrolyte 18.
[0024] <Nonaqueous electrolyte 18> The non-aqueous electrolyte 18 is a composition in which a supporting salt is contained in a non-aqueous solvent. In this embodiment, ethylene carbonate (EC) can be used as the non-aqueous solvent. The non-aqueous solvent may be one or more materials selected from the group consisting of propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and the like.
[0025] In addition, as the supporting salt, LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, etc. can be used. In addition, one or more lithium compounds (lithium salts) selected from these can be used. Thus, the nonaqueous electrolyte 18 contains a lithium compound.
[0026] <Electrode body 15> As shown in FIG. 2, the electrode body 15 includes a negative electrode plate 20, a positive electrode plate 30, and a separator 40. The longitudinal direction of the electrode body 15 is referred to as the "length direction Z". The thickness direction of the electrode body 15 is referred to as the "thickness direction D". The direction intersecting the length direction Z and the thickness direction D of the electrode body 15 is referred to as the "width direction W". One direction of the width directions W is referred to as the "first width direction W1", and the other direction of the width directions W is referred to as the "second width direction W2". In other words, the second width direction W2 is the opposite direction to the first width direction W1.
[0027] The electrode body 15 is formed by stacking a negative electrode plate 20, a positive electrode plate 30, and a separator 40 in the thickness direction D. The separator 40 is provided between the negative electrode plate 20 and the positive electrode plate 30. In detail, the electrode body 15 is formed by stacking the separator 40, the positive electrode plate 30, the separator 40, and the negative electrode plate 20 in this order.
[0028] The electrode assembly 15 is formed by stacking the negative electrode plate 20, the positive electrode plate 30, and the separator 40 in the thickness direction D and winding them in the length direction Z. The electrode assembly 15 has a flat shape in the thickness direction D at the center in the length direction Z.
[0029] In this way, the thickness direction D in which the negative electrode plate 20, the positive electrode plate 30, and the separator 40 are stacked can also be referred to as the stacking direction. Also, the length direction Z in which the negative electrode plate 20, the positive electrode plate 30, and the separator 40 are wound can also be referred to as the winding direction. The electrode body 15 has a flat shape in the thickness direction D.
[0030] <Negative electrode plate 20> The negative electrode plate 20 functions as an example of a negative electrode of the lithium ion secondary battery 10. The negative electrode plate 20 includes a negative electrode substrate 21 and a negative electrode mixture layer 22. The negative electrode substrate 21 is an electrode substrate of the negative electrode. The negative electrode mixture layer 22 is an electrode mixture layer of the negative electrode, and is provided on both sides of the negative electrode substrate 21.
[0031] The negative electrode substrate 21 includes a negative electrode connection portion 23. The negative electrode connection portion 23 is a region where the negative electrode composite layer 22 is not provided on either side of the negative electrode substrate 21. The negative electrode connection portion 23 is provided at an end portion in the first width direction W1 of the electrode body 15. The negative electrode connection portion 23 is exposed from the positive electrode plate 30 and the separator 40 in the first width direction W1.
[0032] In this embodiment, the negative electrode substrate 21 is made of Cu foil. The negative electrode substrate 21 serves as a base for the aggregate of the negative electrode mixture layer 22. The negative electrode substrate 21 functions as a current collecting member that collects electricity from the negative electrode mixture layer 22.
[0033] The negative electrode mixture layer 22 has a negative electrode active material and a negative electrode additive. The negative electrode plate 20 is produced, for example, by kneading the negative electrode active material and the negative electrode additive, applying the kneaded negative electrode mixture paste to the negative electrode substrate 21, and drying the paste.
[0034] In this embodiment, the negative electrode active material is an active material of a negative electrode, and is a material capable of absorbing and releasing lithium ions. As the negative electrode active material, for example, a powdered carbon material made of graphite or the like can be used.
[0035] The negative electrode additive is an additive for the negative electrode, and includes a negative electrode solvent, a negative electrode binder, and a negative electrode thickener. The negative electrode solvent may be, for example, water. The negative electrode binder may be, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), etc. The negative electrode thickener may be, for example, carboxymethyl cellulose (CMC), etc. The negative electrode additive may further include, for example, a negative electrode conductive material, etc.
[0036] <Positive electrode plate 30> The positive electrode plate 30 functions as an example of a positive electrode of the lithium ion secondary battery 10. The positive electrode plate 30 includes a positive electrode substrate 31 and a positive electrode mixture layer 32. The positive electrode substrate 31 is an electrode substrate of the positive electrode. The positive electrode mixture layer 32 is an electrode mixture layer of the positive electrode, and is provided on both sides of the positive electrode substrate 31.
[0037] The positive electrode substrate 31 includes a positive electrode connection portion 33. The positive electrode connection portion 33 is a region where the positive electrode composite layer 32 is not provided on either side of the positive electrode substrate 31. The positive electrode connection portion 33 is provided at an end portion in the second width direction W2 of the electrode body 15. The positive electrode connection portion 33 is exposed from the negative electrode plate 20 and the separator 40 in the second width direction W2.
[0038] In this embodiment, the positive electrode substrate 31 is made of an Al foil or an Al alloy foil. The positive electrode substrate 31 serves as a base for the aggregate of the positive electrode mixture layer 32. The positive electrode substrate 31 functions as a current collecting member that collects electricity from the positive electrode mixture layer 32.
[0039] The positive electrode mixture layer 32 has a positive electrode active material and a positive electrode additive. The positive electrode plate 30 is produced, for example, by kneading the positive electrode active material and the positive electrode additive, applying the kneaded positive electrode mixture paste to the positive electrode substrate 31, and drying the paste.
[0040] The positive electrode active material is an active material of the positive electrode, and is a material capable of absorbing and releasing lithium. The positive electrode active material is, for example, a ternary (NMC) lithium-containing composite oxide containing nickel, manganese, and cobalt, and lithium nickel cobalt manganese oxide (LiNiCoMnO2) can be used. The positive electrode active material may be, for example, any one of lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), and lithium nickel oxide (LiNiO2). The positive electrode active material may be, for example, a lithium-containing composite oxide containing nickel, cobalt, and aluminum (NCA).
[0041] The positive electrode additive is an additive for the positive electrode, and includes a positive electrode solvent, a positive electrode conductive material, and a positive electrode binder. As the positive electrode solvent, for example, a non-aqueous solvent such as NMP (N-methyl-2-pyrrolidone) solution can be used. As the positive electrode conductive material, for example, carbon fibers such as carbon nanotubes (CNT) and carbon nanofibers (CNF) can be used, but graphite, acetylene black (AB), ketjen black, and other carbon blacks can also be used. As the positive electrode binder, for example, the same material as the negative electrode binder can be used. The positive electrode additive may further include, for example, a positive electrode thickener.
[0042] <Separator 40> The separator 40 is provided between the negative electrode plate 20 and the positive electrode plate 30. The separator 40 holds the non-aqueous electrolyte 18. The separator 40 is a non-woven fabric made of polypropylene or the like, which is a porous resin. As the separator 40, a porous polymer membrane such as a porous polyethylene membrane, a porous polyolefin membrane, and a porous polyvinyl chloride membrane, or a lithium ion or ion conductive polymer electrolyte membrane can be used alone or in combination. When the electrode body 15 is immersed in the non-aqueous electrolyte 18, the non-aqueous electrolyte 18 permeates the separator 40 from the end toward the center.
[0043] <Manufacturing process of lithium ion secondary battery 10> Here, a manufacturing process of the lithium ion secondary battery 10 of this embodiment will be described. In this embodiment, a source process is performed. As will be described in detail later, the source process is a process for producing the battery elements of the lithium-ion secondary battery 10. Specifically, the source process is a process for producing the negative electrode plate 20 and the positive electrode plate 30 that constitute the battery elements of the lithium-ion secondary battery 10.
[0044] After the source process is completed, the assembly process is performed. The assembly process is a process for assembling the lithium ion secondary battery 10. In the assembly process, the electrode body 15 is manufactured first. Specifically, the positive electrode plate 30 and the negative electrode plate 20 are first stacked with the separator 40 interposed therebetween, then wound and pressed flat. Thereafter, the negative electrode connection portion 23 is pressure welded, and the positive electrode connection portion 33 is pressure welded. Through the above procedure, the electrode body 15 is manufactured.
[0045] Next, the electrode body 15 is housed in the battery case 11. At this time, the positive electrode connection part 33 is electrically connected to the positive electrode external terminal 14 via the positive electrode current collector 17. The negative electrode connection part 23 is electrically connected to the negative electrode external terminal 13 via the negative electrode current collector 16. The opening of the battery case 11 is closed by the lid body 12. Then, the nonaqueous electrolyte 18 is injected into the battery case 11. After the injection of the nonaqueous electrolyte 18 into the battery case 11 is completed, the battery case 11 is sealed. Through the above procedures, the lithium ion secondary battery 10 is assembled.
[0046] <Source process> Here, the source process of this embodiment will be described with reference to Fig. 3. Hereinafter, the process of producing the positive electrode plate 30 will be described, and the description of the process of producing the negative electrode plate 20 will be omitted.
[0047] As shown in Fig. 3, in step S11, a preparation step is performed. The preparation step includes a step of preparing a positive electrode active material and a positive electrode additive, which are raw materials for the positive electrode mixture layer 32. As a result, a positive electrode mixture paste is generated. Then, in step S12, a kneading step is performed. The kneading step includes a step of kneading the positive electrode mixture paste.
[0048] After the kneading step is completed, a coating step is performed in step S13. In the coating step, the positive electrode composite paste is applied to both sides of the positive electrode substrate 31 so as to form positive electrode connection portions 33 at both ends in the width direction W. Then, in step S14, a drying step is performed. In the drying step, the positive electrode composite paste applied to the positive electrode substrate 31 is dried to form a positive electrode composite layer 32.
[0049] After the drying process is completed, a pressing process is performed in step S15. In the pressing process, positive electrode mixture layer 32 formed on both sides of positive electrode substrate 31 is pressed to increase the adhesive strength of positive electrode mixture layer 32 to positive electrode substrate 31 and adjust the thickness of positive electrode mixture layer 32.
[0050] After the pressing step is completed, a cutting step is performed in step S16. In the cutting step, the positive electrode plate 30 is cut at the center in the width direction W. Through the above steps, two positive electrode plates 30 are produced at once.
[0051] <Method of manufacturing the positive electrode plate 30> Here, a method for manufacturing the positive electrode plate 30 will be described in detail. The positive electrode plate 30 is manufactured based on the specific surface area of the positive electrode active material before manufacturing the positive electrode plate 30 and the specific surface area of the positive electrode plate 30 after manufacturing the positive electrode plate 30. The specific surface area is measured, for example, by a gas adsorption measurement method using the BET method, that is, the BET method.
[0052] Before the manufacture of the positive electrode plate 30, the specific surface area is 1.5 m 2 / g or more 3.0m 2 Particles with a specific surface area of 1.5 m or less are used as the positive electrode active material. "Before the positive electrode plate 30 is manufactured" refers to before the blending step is performed in the source process. In other words, the specific surface area of the positive electrode active material before the positive electrode plate 30 is manufactured is the specific surface area of the positive electrode active material particles before they are blended in the blending step. Thus, the specific surface area of the positive electrode active material before the positive electrode plate 30 is manufactured is 1.5 m 2 / g or more 3.0m 2 / g or less. Hereinafter, the specific surface area of the positive electrode active material before the manufacture of the positive electrode plate 30 may be referred to as the "specific surface area of the positive electrode active material."
[0053] In addition, after the manufacture of the positive electrode plate 30, the density of the positive electrode mixture layer 32 is 2.2 g / cm 3 Above 3.0 g / cm 3The positive electrode plate 30 is manufactured as follows. After the manufacturing process of the positive electrode plate 30, the density of the positive electrode mixture layer 32 after the manufacturing process of the positive electrode plate 30 is 2.2 g / cm 3 Above 3.0 g / cm 3 The density of positive electrode mixture layer 32 after the manufacture of positive electrode plate 30 is equal to the density of positive electrode mixture layer 32 after the pressing step is performed. Hereinafter, the density of positive electrode mixture layer 32 after the manufacture of positive electrode plate 30 may be referred to as the "positive electrode density."
[0054] In addition, when the positive electrode plate 30 is manufactured, the difference between the specific surface area of the positive electrode plate 30 after the manufacture of the positive electrode plate 30 and the specific surface area of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less. The specific surface area of the positive electrode plate 30 after the manufacture of the positive electrode plate 30 is adjusted in the pressing process based on the difference with the specific surface area of the positive electrode active material. The specific surface area of the positive electrode plate 30 after the manufacture of the positive electrode plate 30 is equal to the specific surface area of the positive electrode plate 30 after the pressing process is performed. In other words, the specific surface area of the positive electrode plate 30 after the manufacture of the positive electrode plate 30 can be said to be the specific surface area of the positive electrode plate 30 after it is pressed in the pressing process. Hereinafter, the specific surface area of the positive electrode plate 30 after the manufacture of the positive electrode plate 30 may be referred to as the "positive electrode plate specific surface area". Also, the difference between the positive electrode plate specific surface area and the positive electrode active material specific surface area may be referred to as the "specific surface area difference".
[0055] <Examples and Comparative Examples> Here, an example and a comparative example of the lithium ion secondary battery 10 will be described with reference to Fig. 4. In the examples and comparative examples, the evaluation was performed under the following conditions, but these are merely examples and are not limited to these. In the examples and comparative examples, the evaluation targets are lithium ion secondary batteries 10 with a C (Capacity) rate of 50C and a SOC (State Of Charge) of 20 to 90%.
[0056] In the examples and comparative examples, a ternary lithium-containing composite oxide or a lithium-containing composite oxide containing nickel cobalt aluminum (NCA) is used as the positive electrode active material. In the examples and comparative examples, the specific surface area of the positive electrode plate is adjusted by pressing in the pressing process. For the pressing in the pressing process, a pressing pressure of 50 to 196 kN and a pressing speed of 6 to 60 m / min are adopted.
[0057] In the examples and comparative examples, a powdered carbon material such as graphite is used as the negative electrode active material. In the examples and comparative examples, a non-aqueous solvent is used as the solvent for the non-aqueous electrolyte 18, and one or more materials selected from the group consisting of ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate, etc. are used. In the examples and comparative examples, LiPF6 is used as the supporting salt for the non-aqueous electrolyte 18.
[0058] As shown in Fig. 4, in the examples and comparative examples, various judgment results are verified by changing the positive electrode density, the positive electrode plate specific surface area, and the positive electrode active material specific surface area under the above-mentioned conditions. In the examples and comparative examples, the relationship between the positive electrode density, the positive electrode plate specific surface area, the positive electrode active material specific surface area, the specific surface area difference, and the judgment results of various characteristics is shown.
[0059] The various characteristics include the internal resistance of the positive plate 30, an overcharge margin, and storage characteristics, and the index of the judgment result corresponds to the judgment result. As the internal resistance of the positive plate 30, it is judged whether the internal resistance at a very low temperature is within an appropriate range. As the overcharge margin, it is judged whether the time it takes to reach 5.0V from the upper limit voltage of 4.75V is within an appropriate range. As the storage characteristics, it is judged whether the charge and discharge after storage for a period of, for example, 30 days in a high temperature environment such as 70°C is within an appropriate range. As the index of the judgment result, the appropriate range is indexed as a numerical value of 1 or more, and is indicated as indexed in the figure.
[0060] First, as a first comparative example, the positive electrode density is 2.2g / cm 3 Above 3.0 g / cm 3 Although the specific surface area difference is 1.8m 2 / g, and the specific surface area of the positive electrode active material is 1.5 m 2 / g. Under these circumstances, in the first comparative example, the internal resistance, overcharge margin, and storage characteristics of the positive electrode plate 30 were all not determined to be within the appropriate range.
[0061] In the second comparative example, the positive electrode density is 2.2 g / cm 3 Above 3.0 g / cm 3 The specific surface area difference is 0.66 m 2 / g or more 1.8m 2 / g or less, but the specific surface area of the positive electrode active material is 1.5 m 2 / g. Under these circumstances, in the second comparative example, like the first comparative example, the internal resistance, overcharge margin, and storage characteristics of the positive electrode plate 30 were all not determined to be within the appropriate range.
[0062] As a third comparative example, a positive electrode active material specific surface area of 1.5 m 2 / g or more 3.0m 2 / g or less, but the positive electrode density is 3.0 g / cm 3 The difference in specific surface area is 1.8m 2 / g. In this situation, in the third comparative example, the internal resistance of the positive electrode plate 30 was determined to be within the appropriate range, but the overcharge margin and storage characteristics were not determined to be within the appropriate range. The fourth comparative example also showed a similar result to the third comparative example.
[0063] As a fifth comparative example, the positive electrode density was 2.2 g / cm 3 Above 3.0 g / cm 3 The positive electrode active material specific surface area is 1.5 m or less. 2 / g or more 3.0m 2 / g or less, but the specific surface area difference is smaller than 0.66. Under these circumstances, in the fifth comparative example, the overcharge margin and storage characteristics were determined to be within the appropriate range, but the internal resistance of the positive electrode plate 30 was not determined to be within the appropriate range.
[0064] On the other hand, in the first to fifth examples, the positive electrode density was 2.2 g / cm 3 Above 3.0 g / cm 3 The positive electrode active material specific surface area is within the range of 1.5 m 2 / g or more 3.0m 2 / g or less. And the specific surface area difference is 0.66 m 2 / g or more 1.8m 2 / g or less. Under these circumstances, in the first to fifth examples, the internal resistance, overcharge margin, and storage characteristics of the positive electrode plate 30 were all determined to be within the appropriate range.
[0065] <Verification of Examples and Comparative Examples> Thus, the internal resistance of the positive electrode plate 30 was not determined to be within the appropriate range in Comparative Examples 1, 2, and 5. This is considered to be partly due to the fact that the specific surface area of the positive electrode active material was small to begin with, resulting in a small reaction area of the positive electrode plate 30.
[0066] In particular, in Comparative Example 2, even though the positive electrode density and the specific surface area difference were within the appropriate range, the positive electrode active material specific surface area was small, and the overcharge margin and storage characteristics were not determined to be within the appropriate range. In Comparative Example 1, not only was the positive electrode active material specific surface area small, but the specific surface area difference was large. In Comparative Example 5, not only was the positive electrode active material specific surface area small, but the positive electrode density and the specific surface area difference were small.
[0067] In Comparative Examples 3 and 4, even though the specific surface area of the positive electrode active material was within the appropriate range, the positive electrode plate specific surface area and the positive electrode density were large, resulting in a large specific surface area difference, and the overcharge margin and storage characteristics were not determined to be within the appropriate range. This is thought to be partly due to the fact that the positive electrode active material is crushed by pressing the positive electrode mixture layer 32 in the pressing process, resulting in many newly formed surfaces of the positive electrode active material.
[0068] In addition, in Comparative Examples 1 and 2, the specific surface area of the positive electrode active material was small, but the positive electrode density was not small and was adjusted to an appropriate range by pressing. For this reason, it is considered that in Comparative Examples 1 and 2, as in Comparative Examples 3 and 4, the overcharge margin and storage characteristics were not determined to be in the appropriate range, partly due to the large amount of newly generated surface of the positive electrode active material.
[0069] <Formation of new surface> Here, the formation of the new surface will be described with reference to Figures 5 to 7. In Figures 5 to 7, the formation of the new surface is shown in a schematic manner in order to facilitate understanding of the invention.
[0070] 5, the positive electrode mixture layer 32 contains a positive electrode active material 34 and a positive electrode conductor 35. Before the manufacture of the positive electrode plate 30, the positive electrode active material 34 is in a chemically stable state because it is in the form of hollow particles with the surfaces in contact with air.
[0071] 6 and 7, the positive electrode active material 34 is pressed in the pressing step, whereby a new surface 34A is formed on the surface of the positive electrode active material 34.
[0072] The new surface 34A is a surface that is not exposed to the surface before the manufacture of the positive electrode plate 30, and is a surface that is formed to be exposed to the surface by pressing in the pressing process. The new surface 34A is not in a chemically stable state, is highly active, and may be a factor that reduces safety from the viewpoint of overcharge resistance. In addition, the new surface 34A is likely to form an irreversible coating, which may be a factor that deteriorates storage characteristics. Such a new surface 34A is more likely to be formed as the specific surface area difference becomes larger. For this reason, a new indicator for whether the specific surface area difference is within an appropriate range from the viewpoint of the formation of the new surface 34A has been created.
[0073] As shown in FIG. 6, if many new surfaces 34A are formed by pressing in the pressing process, the specific surface area difference becomes large, and even if the deterioration of the internal resistance can be suppressed, there is a risk that the overcharge resistance and the storage characteristics may deteriorate.
[0074] On the other hand, if pressing is performed so as to avoid the formation of new surface 34A as much as possible during the pressing process, the specific surface area difference becomes too small, and even if the deterioration of overcharge resistance and storage characteristics can be suppressed, there is a risk of an increase in internal resistance.
[0075] Therefore, as shown in FIG. 7, if a minimum amount of newly formed surface 34A is formed by pressing in the pressing process, the specific surface area difference will be within an appropriate range, and the deterioration of internal resistance can be suppressed, as well as the deterioration of overcharge resistance and storage characteristics can be suppressed.
[0076] <Actions and Effects of the Present Embodiment> The operation and effects of the embodiment will be described. (1) Before the manufacture of the positive electrode plate 30, the specific surface area is 1.5 m 2 / g or more 3.0m 2 The positive electrode active material particles are used in such a manner that the difference between the specific surface area of the positive electrode plate and the specific surface area of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less.
[0077] Conventionally, the positive electrode plate specific surface area has been adjusted by pressing the positive electrode mixture layer 32 in the pressing process, and this has made it possible to suppress deterioration of the internal resistance of the lithium-ion secondary battery 10. However, conventionally, the formation of new surfaces by pressing has not been taken into consideration, and this has sometimes caused deterioration of the overcharge resistance and storage characteristics of the lithium-ion secondary battery 10.
[0078] In this embodiment, it was found that the formation of new surfaces by pressing is one of the causes of deterioration in the overcharge resistance and storage characteristics of the lithium-ion secondary battery 10, and the above-mentioned new index was created. As a result, it is possible to suppress deterioration in the overcharge resistance and storage characteristics of the lithium-ion secondary battery 10 by minimizing the formation of new surfaces of the positive electrode active material while suppressing deterioration in the internal resistance of the lithium-ion secondary battery 10. Therefore, it is possible to improve the characteristics of the lithium-ion secondary battery 10.
[0079] (2) Positive electrode density is 2.2 g / cm 3 Above 3.0 g / cm 3 This makes it possible to suppress deterioration of the overcharge resistance and the storage characteristics while suppressing deterioration of the internal resistance of the lithium ion secondary battery 10. Therefore, the characteristics of the lithium ion secondary battery 10 can be improved.
[0080] (3) The positive electrode active material is a ternary positive electrode active material. As a result, even when compared with a positive electrode active material using, for example, lithium manganate, it is possible to improve the charge / discharge cycle characteristics of the lithium ion secondary battery 10 while suppressing deterioration of the internal resistance, overcharge resistance, and storage characteristics of the lithium ion secondary battery 10. As a result, it is possible to improve the characteristics of the lithium ion secondary battery 10.
[0081] (4) The positive electrode conductive material has a specific surface area of 150 m before the positive electrode plate 30 is manufactured. 2 / g or more 300m 2 / g or less. By using a positive electrode conductive material with high conductivity, it is possible to suppress deterioration of the internal resistance of the lithium ion secondary battery 10. Therefore, it is possible to improve the characteristics of the lithium ion secondary battery 10.
[0082] (5) The positive electrode mixture layer 32 is provided on the positive electrode substrate 31 by applying a positive electrode mixture paste containing at least a positive electrode active material and a positive electrode solvent to the positive electrode substrate 31 and drying the applied paste. The positive electrode solvent is a non-aqueous solvent. This makes it possible to suppress the decrease in the amount of the positive electrode active material, reduce the specific surface area difference, and suppress the deterioration of the overcharge resistance, compared to an aqueous solvent. Therefore, the characteristics of the lithium ion secondary battery 10 can be improved.
[0083] [Example of change] This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that there is no technical contradiction.
[0084] In this embodiment, for example, the positive electrode active material, the positive electrode conductive material, the positive electrode solvent, and the positive electrode binder may be of any type. In this embodiment, for example, as long as the positive electrode active material specific surface area and the specific surface area difference are in appropriate ranges, the positive electrode density does not matter, but it is preferable that the positive electrode density is in an appropriate range.
[0085] In the present embodiment, the present invention has been described taking the lithium ion secondary battery 10 as an example. However, the present invention can be applied to other secondary batteries. In the present embodiment, the lithium ion secondary battery 10 is a thin plate-shaped battery for vehicle use, but the present invention can also be applied to cylindrical batteries. In addition, the present invention can also be applied to batteries for ships, aircraft, and stationary use, in addition to vehicle use.
[0086] It goes without saying that those skilled in the art may add, delete, or modify the components of the present invention, and change the order of the components, without departing from the scope of the claims. [Explanation of symbols]
[0087] D: Thickness direction W: Width direction Z: Length direction 10...Lithium-ion secondary battery 11…Battery case 12…Lid body 13...Negative external terminal 14…Positive external terminal 15...Electrode body 16...Negative electrode current collector 17...Positive electrode current collector 18...Nonaqueous electrolyte 20…Negative electrode plate 21...Negative electrode substrate 22...Negative electrode composite material layer 23...Negative electrode connection part 30…Positive electrode plate 31...Positive electrode substrate 32...Positive electrode mixture layer 33…Positive electrode connection 34...Cathode active material 34A…New surface 35…Positive electrode conductive material 40…Separator
Claims
1. A positive electrode plate for a non-aqueous secondary battery comprising a positive electrode substrate and a positive electrode mixture layer containing at least a positive electrode active material and a positive electrode conductive material, The positive electrode plate for the nonaqueous secondary battery has a specific surface area of 1.5 m before production. 2 / g or more 3.0m 2 / g or less of the positive electrode active material particles are used, The difference between the specific surface area of the positive electrode plate for a nonaqueous secondary battery after production of the positive electrode plate for a nonaqueous secondary battery and the specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less, the positive electrode conductive material is any one of carbon nanotubes and carbon nanofibers, each having a specific surface area of 150 m 2 / g or more and 300 m 2 / g or less before the positive electrode plate for the nonaqueous secondary battery is manufactured; Positive electrode plate for non-aqueous secondary batteries.
2. A non-aqueous secondary battery including a positive electrode plate having a positive electrode substrate and a positive electrode mixture layer including at least a positive electrode active material and a positive electrode conductive material, Before the manufacture of the positive electrode plate, the specific surface area is 1.5 m 2 / g or more 3.0m 2 / g or less of the positive electrode active material particles are used, The difference between the specific surface area of the positive electrode plate after production and the specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less, The positive electrode conductive material is any one of carbon nanotubes and carbon nanofibers having a specific surface area of 150 m 2 / g or more and 300 m 2 / g or less before the positive electrode plate is manufactured. Non-aqueous secondary battery.
3. A method for producing a positive electrode plate for a non-aqueous secondary battery, comprising: a positive electrode substrate; and a positive electrode mixture layer including at least a positive electrode active material and a positive electrode conductive material, The positive electrode plate for the nonaqueous secondary battery has a specific surface area of 1.5 m before production. 2 / g or more 3.0m 2 / g or less of the positive electrode active material particles are used, The difference between the specific surface area of the positive electrode plate for a nonaqueous secondary battery after production of the positive electrode plate for a nonaqueous secondary battery and the specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less, the positive electrode conductive material is any one of carbon nanotubes and carbon nanofibers, each having a specific surface area of 150 m 2 / g or more and 300 m 2 / g or less before the positive electrode plate for the nonaqueous secondary battery is manufactured; A method for producing a positive electrode plate for a non-aqueous secondary battery.
4. The method for producing a positive electrode plate for a nonaqueous secondary battery according to claim 3, After the positive electrode plate for the nonaqueous secondary battery is manufactured, the density of the positive electrode mixture layer is 2.2 g / cm 3 3.0g / cm or more 3 Below is the A method for producing a positive electrode plate for a non-aqueous secondary battery.
5. The method for producing a positive electrode plate for a nonaqueous secondary battery according to claim 3 or 4, The positive electrode active material is a ternary positive electrode active material. A method for producing a positive electrode plate for a non-aqueous secondary battery.
6. The method for producing a positive electrode plate for a nonaqueous secondary battery according to claim 3 or 4, the positive electrode mixture layer is provided on the positive electrode substrate by applying a positive electrode mixture paste containing at least the positive electrode active material and a positive electrode solvent to the positive electrode substrate and drying the applied positive electrode mixture paste; The positive electrode solvent is a non-aqueous solvent. A method for producing a positive electrode plate for a non-aqueous secondary battery.
7. A method for producing a nonaqueous secondary battery including a positive electrode plate having a positive electrode substrate and a positive electrode mixture layer including at least a positive electrode active material and a positive electrode conductive material, Before the manufacture of the positive electrode plate, the specific surface area is 1.5 m 2 / g or more 3.0m 2 / g or less of the positive electrode active material particles are used, The difference between the specific surface area of the positive electrode plate after production and the specific surface area of the particles of the positive electrode active material is 0.66 m 2 / g or more 1.8m 2 / g or less, The positive electrode conductive material is any one of carbon nanotubes and carbon nanofibers having a specific surface area of 150 m 2 / g or more and 300 m 2 / g or less before the positive electrode plate is manufactured. A method for manufacturing a non-aqueous secondary battery.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2003272611A
Power storage element
JP2018147644A
Electrode structure body
JP2022013199A