Low-temperature solder, manufacturing method thereof, and low-temperature solder-coated lead wire
A low-temperature solder made from Sn, Bi, and In alloys with trace elements addresses the weakness and cost of lead-free solders, providing strong adhesion to resin film electrodes at reduced temperatures.
Patent Information
- Application Number
- JP2022553794
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-28
- Filing Date
- 2021-09-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-09-15
AI Technical Summary
Conventional lead-free solders are weaker and more expensive than tin-lead solder, and high soldering temperatures pose challenges for solar cells on flexible resin films.
A low-temperature solder composed of Sn, Bi, In, or alloys thereof, with trace amounts of Al, P, Sb, and In, is developed, which is alloyed with a melting temperature equal to or lower than the base material, enhancing adhesion and reducing costs.
The low-temperature solder achieves strong adhesion to electrodes on resin films at lower temperatures, overcoming strength and cost issues of conventional lead-free solders.
Smart Images

Figure 0007576805000001 
Figure 0007576805000002 
Figure 0007576805000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a low-temperature solder used in resin films used in solar cell substrates, liquid crystal substrates, etc., a method for producing the low-temperature solder, and a low-temperature solder-coated lead wire. [Background technology]
[0002] Conventionally, tin-lead solder has been widely used for soldering lead wires to electrodes of solar cell substrates, liquid crystal substrates, etc., due to its high strength and low cost.
[0003] Furthermore, in the case of electrodes made of aluminum or the like, sufficient soldering strength could not be obtained, so silver paste was applied and sintered, and then the lead wire was soldered onto this with tin-lead solder.
[0004] Recently, there has been a growing demand for lead-free solder due to concerns about pollution.
[0005] Furthermore, there is a demand for forming a solar cell on a flexible resin film such as PET, and low-temperature soldering of lead wires to the electrodes (aluminum electrodes, copper electrodes, etc.). DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0006] Conventional lead-free solder has problems compared to tin-lead solder, such as its strength being slightly less than the required strength and its high price, preventing it from becoming an alternative.
[0007] Furthermore, in solar cells and the like formed on a resin film, there has been a problem in that the soldering temperature is too high. [Means for solving the problem]
[0008] The inventors have discovered that low-temperature solders consisting of Sn, a type of lead-free solder, and Bi, In, or an alloy of Bi and In, which are melted and alloyed by mixing one or more of Al, P, Sb, In (except when the base material contains In) in a total amount of up to 3 wt%, preferably 1 wt% to 1.5 wt%, can be soldered extremely firmly to electrodes (aluminum, copper, etc.) such as resin films.
[0009] Therefore, in the low-temperature solder made of Sn and Bi, In, or an alloy of Bi and In, the present inventors mix a main material made of one or more of Al, P, Sb, and In (except when the base material contains In) in a total amount of up to 3 wt%, preferably up to 1.0 to 1.5 wt%, and more preferably 0.01 wt% or more into the base material, which is an alloy of Sn, Bi, In, or Bi and In, and melt and alloy it to increase the adhesion strength.
[0010] In this case, the melting temperature of the low-temperature solder after melting and alloying is set to be the same as or lower than the melting temperature of the base material.
[0011] In addition, a sub-material made of an alloy containing one or more of Al, P, Sb, and In is mixed into the base material as required, and melted and alloyed.
[0012] In addition, the secondary material is an alloy of Cu and P.
[0013] The base material is mixed with main elements Al, CuP, and if necessary In, in a total amount of up to 3 wt%, preferably up to 1.0 to 1.5 wt%, and more preferably 0.1 wt% or more, and melted and alloyed.
[0014] In addition, the base material, main material, and secondary material are mixed together or divided into several parts and then melted and alloyed.
[0015] It is also used for soldering lead wires to the electrodes of solar cell substrates and liquid crystal substrates (resin films).
[0016] The low-temperature solder is melted and applied to the surface of the wire or ribbon.
[0017] The melt coating is performed while applying ultrasonic waves. Effect of the Invention
[0018] As described above, the present invention relates to low-temperature solders made of Sn and Bi, In, or alloys of Bi and In. The low-temperature solders melted and alloyed by mixing one or more of Al, P, Sb, In (except when the base material contains In) in a total amount of up to 3 wt%, preferably 1 wt% to 1.5 wt%, can be soldered very firmly to electrodes (aluminum, copper, etc.) such as resin films, and in particular, low-temperature solders made of Sn and Bi can be produced very cheaply.
[0019] In addition, the melting temperature of the low-temperature solder after melting and alloying is the same as or lower than the melting temperature of the base material, eliminating the rise in melting temperature caused by contamination.
[0020] In addition, by mixing one or more of Al, P, Sb, In (except when the base material contains In), melting and alloying them to produce low-temperature solder, it is possible to significantly increase the adhesive strength to the soldered object. Example 1
[0021] FIG. 1 is an explanatory diagram of low-temperature solder production according to the present invention.
[0022] FIG. 1(a) shows a flow chart, and FIG. 1(b) shows example materials.
[0023] In (a) of Fig. 1, S1 prepares the base material and main material. For this, the following materials shown as material examples in (b) of Fig. 1 are prepared.
[0024] ·Base material: Sn42 Bi58 ·Main material: Al, GuP, In Here, the base material is the basic material (base material) of the alloy forming the low-temperature solder of the present invention, and for example, 42 wt% Sn and 58 wt% Bi (melting temperature 139°C) were used as one. The weight ratio of Sn and Bi is arbitrary within the range in which an alloy can be created, for example, 3 to 58 wt% Bi and the remainder Sn. The ratio can be appropriately selected so as to obtain the desired value by experimenting with the melting temperature (the more Bi, the lower the temperature, and the melting temperature is 139°C at 58 wt%). Note that for other low-temperature solders, Sn-In type, and Sn-Bi-In type, the ratio can be appropriately selected in the same manner as described in FIG. 5 and its explanation.
[0025] The main material is a material that affects soldering such as the removal of oxide film on the surface of the soldered object, adhesion, wettability, fluidity, and viscosity during soldering, and in the present invention, the total amount of the main material is a maximum of 3 wt% or less, preferably 1 to 1.5 wt% or less, and 0.01 wt% or more. Here, the main material is a material to be melted and alloyed by mixing with one or more of Al (adhesion of the soldered object), P (or CuP, removal of oxide film on the soldered object, adhesion), In (wettability, fluidity), and Sb (adhesion). The main material is a total amount of a maximum of 3 wt% or less, preferably 1 to 1.5 wt% or less, and combined with a small amount of 0.01 wt% or more, the melting temperature of the low-temperature solder after mixing the main material with the base material and melting and alloying is equal to or slightly lower (for example, about 1 to 3°C lower) than the melting temperature of the base material. This is presumably because the total amount of the main materials is a very small amount, a maximum of 3 wt% or less, preferably 1 to 1.5 wt% or less, relative to the matrix, and so they penetrate into the skeleton of the matrix and reconstitute the skeleton.
[0026] In S2, the main material is mixed with the base material. This is done by mixing the main material with the base material prepared in S1.
[0027] In S3, the base material and main material are melted and alloyed. In S2, the base material is mixed with the main material, heated and melted, and thoroughly stirred to form an alloy. In cases where the main material is oxidized by oxygen in the air and alloying is difficult, an inert gas (such as nitrogen gas) can be blown into the crucible as necessary, or a melting furnace or vacuum melting furnace filled with an inert gas can be used.
[0028] S4: Low temperature solder material is completed.
[0029] As described above, by preparing the base material and main material, mixing them, and melting and alloying them, it is possible to manufacture the low-temperature solders according to the present invention (Sn-Bi, Sn-In, and Sn-Bi-In low-temperature solders). The details will be explained in order below.
[0030] FIG. 2 is an explanatory diagram of the low-temperature solder material manufacturing apparatus of the present invention.
[0031] In FIG. 2, the solder material 1 is the base material or main material prepared in S1 of FIG. 1 already described, and is here a metal fragment (coarsely crushed).
[0032] The solder material input tray 2 is used to place the solder material 1 thereon and input it into the melting furnace 3 .
[0033] The melting furnace 3 is heated by a heater 4 or the like, and the solder material 1 is put inside, where the base material and main material are melted and stirred to form an alloy. The melting furnace 3 is usually operated in the atmosphere, where the base material and main material put inside are melted and stirred to form an alloy. During this process, an inert gas (such as nitrogen gas) is blown in as necessary to reduce oxidation caused by oxygen in the air, and the furnace is sealed and filled with an inert gas (or evacuated) as necessary.
[0034] In this manner, the base material and main material prepared in S1 of FIG. 1 are mixed, melted in the melting furnace 3, and alloyed by stirring, making it possible to manufacture the low-temperature solder of the present invention (Sn-Bi, Sn-In, and Sn-Bi-In low-temperature solders).
[0035] FIG. 3 is an explanatory diagram of low-temperature soldering of the lead wire of the present invention.
[0036] FIG. 3(a) shows a flow chart, and FIG. 3(b) shows an example of a substrate / lead.
[0037] In (a) of Fig. 3, S11 is ultrasonic pre-soldering of a substrate pattern with low-temperature solder. For example, the low-temperature solder of the present invention (the low-temperature solder produced in S4 of Fig. 1) is supplied to the tip of an ultrasonic soldering iron and melted on the portion (pattern) to be soldered on a substrate for a solar cell (PET board, 0.1 mm thickness, etc.), and ultrasonic waves are applied to solder the pattern portion on the substrate in advance (called ultrasonic pre-soldering).
[0038] In S12, the lead wire is soldered with or without ultrasonic waves. In S11, the lead wire is placed along the portion (pattern) of the electrode (e.g., aluminum foil) of the substrate (PET plate) of a solar cell, for example, and the low-temperature solder of the present invention is melted and the lead wire is soldered while applying ultrasonic waves from above or without applying ultrasonic waves. Note that when the low-temperature solder has been pre-soldered to the lead wire, it is not necessary to supply solder.
[0039] As a result of the above, pre-soldering is performed with the low-temperature solder of the present invention using ultrasound on the part to be soldered (for example, the electrode part (aluminum part) of a solar cell substrate (PET plate)) (S11), and then the lead wire is ultrasonically soldered or soldered without ultrasound using the low-temperature solder of the present invention on the pre-soldered part (pattern) (S12).This makes it possible to ultrasonically pre-solder the electrode part (aluminum foil part) of a solar cell substrate, which cannot be soldered using conventional methods, and then ultrasonically solder the lead wire on top of that.
[0040] Furthermore, ultrasonic soldering is performed at a power of 10 W or less, usually around 1 to 3 W. A strong power can damage the film (such as the nitride film) formed on the solar cell substrate and the crystals on the surface of the substrate, so it is not made too strong.
[0041] FIG. 3(b) shows an example of a substrate / lead.
[0042] In Fig. 3(b), the substrate is a heat-resistant resin substrate such as PET (e.g., a flexible resin substrate with a thickness of about 0.1 mm), which is an example of a substrate that is extremely difficult to solder using normal soldering. The parts (patterns) of these substrates that will become electrodes (aluminum electrodes, copper electrodes, etc.) are ultrasonically pre-soldered with the adhesive low-temperature solder of the present invention. Then, lead wires are ultrasonically soldered or non-ultrasonically soldered to these pre-soldered parts (patterns), making it possible to solder the lead wires to the substrate (aluminum electrodes, copper electrodes).
[0043] The lead wire is soldered to the electrode portion (pattern) on the substrate using the adhesive low-temperature solder of the present invention, and may be a wire (a circular copper wire solder-plated (ultrasonic solder plating) with the low-temperature solder of the present invention; it is easier to solder if it is crushed into a slight oval), a ribbon (a ribbon made by cutting a thin copper sheet to a width of about 1 mm, which is solder-plated (ultrasonic solder plating) with the low-temperature solder of the present invention in advance), etc.
[0044] FIG. 4 shows an explanatory diagram of low temperature soldering according to the present invention.
[0045] FIG. 4(a) shows an example of pre-soldering, and FIG. 4(b) shows an example of ribbon or wire soldering.
[0046] In FIG. 4(a), a substrate (eg, a PET plate with a thickness of 0.1 mm) 11 is an example of a substrate for a solar cell, and an aluminum film (foil) 12 is formed on the entire back surface of the substrate 11, for example.
[0047] The aluminum film (foil) 12 is an electrode (aluminum electrode) formed by forming (adhering, vapor deposition, etc.) an aluminum foil (film) on the entire back surface of the illustrated substrate (PET plate) 11, which is the substrate of the solar cell.
[0048] The ultrasonic soldering iron tip 13 is a soldering iron tip which is heated while ultrasonic waves are applied from an ultrasonic generator (not shown).
[0049] The low-temperature solder 14 is the low-temperature solder of the present invention (the low-temperature solder manufactured in S4 in FIG. 1).
[0050] Next, the soldering operation will be described.
[0051] (1) The substrate 11 is transported onto a preheating table, fixed thereon by vacuum suction, and preheated (for example, to about 130° C.).
[0052] (2) Low-temperature solder 14 is automatically supplied to the tip 13 of the ultrasonic soldering iron shown in the figure from the start point to the end point of the electrode pattern (strip-shaped pattern) to be formed on the aluminum film (foil) 12, and while melting it, ultrasonic waves are applied and the iron is moved at a constant speed while being close enough to the aluminum film (foil) 12 but not scraping it, thereby forming a strip-shaped preliminary solder pattern on the aluminum film (foil) 12.
[0053] As a result of the above, it becomes possible to low-temperature solder 14 of the present invention to low-temperature solder a predetermined preliminary solder pattern onto aluminum film (foil) 12.
[0054] FIG. 4(b) shows an example of low temperature soldering of ribbons or wires.
[0055] In FIG. 4(b), an ultrasonic soldering iron tip 13-1 is a soldering iron tip that is heated with or without application of ultrasonic waves from an ultrasonic generator (not shown).
[0056] The low-temperature soldered ribbon or wire 15 is a ribbon or wire that has been pre-soldered with the low-temperature solder of the present invention. The wire 15 has better solderability if it is slightly deformed into an oval shape.
[0057] Next, the soldering operation of the ribbon or wire to the preliminary solder pattern portion will be described.
[0058] (1) As in FIG. 4(a), the substrate 11 is preheated.
[0059] (2) The low-temperature soldered ribbon or wire 14 is arranged along the preliminary solder pattern portion formed on the aluminum film (foil) 12 on the top (back side) of the substrate 11, and the low-temperature soldered ribbon or wire 15 is lightly pressed from above with the tip 13-1 of a soldering iron with or without ultrasonic waves and moved at a constant speed to the right as shown in the figure, melting the solder of the low-temperature soldered ribbon or wire 15 and soldering it to the preliminary solder pattern portion.
[0060] As a result of the above, it becomes possible to solder the ribbon or wire 15 pre-soldered with the low-temperature solder 14 of the present invention to the pre-solder pattern portion on the aluminum film (foil) 12.
[0061] The quality of the soldering with or without ultrasonic waves of the present invention can be judged by performing soldering with or without ultrasonic waves on a ribbon or wire to a soldering target part, and pulling the ribbon or wire to measure the force at which the board breaks (the bending force, about 2 to 5 kg). If the sample does not peel off from the substrate, etc., it is judged as good, and if it peels off, it is judged as bad.
[0062] FIG. 5 shows an example of the composition of the low-temperature solder of the present invention.
[0063] In FIG. 5, the base material and main material are the same as those described in FIG.
[0064] The composition examples are examples of the base material and main material.
[0065] The wt% examples are examples of the wt% of the composition of the base material and main material.
[0066] The wt% ranges are examples of the wt% ranges of the base material and main material compositions.
[0067] The composition, wt% example, and wt% range are shown in Figure 5 below.
[0068] Base material Main material Notes (melting point example) Composition example Sn-Bi alloy Al P Sb In Melting point: Example 139°C (In is not included in the base material) Sn-In alloy Melting point: 120℃ SnBi-In alloy Melting point: 90℃ Example of wt% Sn Bi In Al CuP8 Sb In 42 58 -- 0.5 0.5 0.5 0.5 52 -- 48 0.5 0.5 0.5 0.5 AA / 2 A 0.5 0.5 0.5 0.5 wt% range 0.1 Trace amount 0.1 0.1 | |(P) | | 1.0 0.1 1.0 1.0 Total amount: Maximum 3wt%, preferably 1.0-1.5wt% or less As an example of the composition, the prototype used a base material with 42wt% Sn and 58wt% Bi as shown in the figure. The composition range may be as long as it is stable within the range in which low-temperature solder alloys (Sn-Bi, Sn-In, and Sn-Bi-In solder alloys) can be made, and for example, a Sn-Bi solder alloy may be made with 3wt% to 58wt% Bi and the remainder Sn, and the melting temperature of the low-temperature solder alloy (base material) may be measured and appropriately selected through experiments.
[0069] The main materials are Al, P (or CuP8), In, Bi, Sb, etc., but for P, P (red phosphorus) and CuP8 alloy (an alloy of 8 wt% P and the remainder Cu, copper phosphide where the wt% of P is 8% of CuP8) were used in the prototype. In the case of P, it is saturated at about 0.1 wt% (or about P = 0.16 wt% in the case of CuP8), and if it is added further, the viscosity increases significantly. For this reason, it is desirable to add P below saturation for normal use to ensure fluidity, wettability, etc. (The amount of P added should be about one-tenth of that of other materials (preferably about 0.1 wt% to 0.01 wt%)). Similarly, the same tendency is seen in other main materials, so the optimal amount of addition can be determined by experiment as necessary.
[0070] The total amount of the main materials is a maximum of 3 wt% or less, preferably 1 to 1.5 wt% or less, and desirably 0.1 wt% or more. When the main materials are added within this range, the melting temperature is approximately the same as or just slightly lower than the base material.
[0071] Figure 6 shows a prototype of the low-temperature solder of the present invention. The illustration shows examples of the many prototypes that can be used for the soldering of Figure 4 described above. Unusable ones are omitted.
[0072] In FIG. 6, the base material of the low-temperature solder of the present invention (the low-temperature solder produced in S4 of FIG. 1) is Sn52 / In48 (melting point: 120℃) Sn42 / Bi58 (melting point: 139℃) Sn48 / Bi52(Melting point: ) Sn40 / In40 / Bi20 (melting point: 90℃) Four types were used:
[0073] The main materials used were the metallic materials Al, CuP8, and In (each 0.5wt%). CuP8 is copper phosphide with 8wt% P and the remainder Cu.
[0074] The sample number is the number of the sample produced.
[0075] The above prototype samples were subjected to ultrasonic soldering and non-ultrasonic soldering as shown in Figure 5, and only the good ones are listed. The ones that could not be soldered are omitted. The results are shown in Figure 7.
[0076] FIG. 7 shows an example of low-temperature soldering of the present invention. -Ultrasonic refers to the distinction between soldering with ultrasonics and soldering without ultrasonics.
[0077] The soldering object is the material to be soldered using the low-temperature solder sample of FIG. 7 of the present invention, and is classified into Al plate (0.1mmt), Cu plate (0.1mmt), Cu wire (0.3 to 0.4mmφ) / ribbon (100μmt, 50μmt, 30μmt), and Si wafer (0.2mmt).
[0078] ·◎ indicates that the low-temperature solder of the present invention has excellent adhesion to the object to be soldered (the force is slightly weaker than the force at which a Si wafer breaks when a 0.4 mmφ tin-plated wire is soldered and pulled (tensile strength of about 1 to 5 kg)).
[0079] ·△ indicates that the low-temperature solder of the present invention has poor adhesion to the object to be soldered (when a tin-plated wire of 0.4 mmφ is soldered and pulled, it comes off with a small force).
[0080] From the above experiment in Figure 7, it was found that when ultrasonic waves were used, sufficient soldering strength was obtained for Al plate, Cu plate, Cu wire / ribbon, and Si wafer.
[0081] In addition, when there was no ultrasonic wave, the solder came off when pulled. When the surface of the soldering object was cleaned, a fairly strong adhesion was sometimes obtained, but in other cases it was not, and the adhesion was unstable.
[0082] FIG. 8 shows an example of low-temperature soldering (metal-metal) of the present invention. FIG. 8(a) shows an example of soldering. Here, the soldering conditions are as shown in the figure: Solder melting point: approx. 138°C Maximum process temperature: 180℃ or less
[0083] The low-temperature solder used was 42wt% Sn, 58wt% Bi, with 0.5wt% each of Al, CuP, and In added (Figures 8 to 13 below will be explained using an example in which this low-temperature solder was used). The same applies to other low-temperature solders made of Sn-In alloys and Sn-Bi alloys.
[0084] 8(a), a sheet in which aluminum foil is bonded to a PET base film using a Co-PET adhesive is cut to the dimensions shown in the figure. Then, as shown in the figure, the aluminum foil surfaces are partially overlapped vertically, and the low-temperature solder (Sn-Bi low-temperature solder) of the present invention is soldered to the overlapping portions.
[0085] The soldering method is, for example, to pre-solder the upper and lower aluminum foil parts with low-temperature solder. Note that soldering with ultrasonic waves applied (ultrasonic soldering) can be used to ensure reliable soldering. Then, overlap the pre-soldered part on the upper aluminum foil with the pre-soldered part on the lower aluminum foil as shown in the figure, press the whole thing down with the tip of a soldering iron from above, and melt the low-temperature solder to solder it. At this time, ultrasonic soldering can be used to ensure reliable soldering.
[0086] In this way, the aluminum foil attached to the PET film surface was able to be soldered together at low temperature as shown in Figure 8(a). Soldering without ultrasonics is also possible, but ultrasonic soldering is preferable for reliability.
[0087] Figure 8(b) shows a photographic example of soldering. These photographs show an example of placing a long, thin piece of aluminum foil horizontally on the surface of a PET film, and then ultrasonically low-temperature soldering only on the "soldering portion" in the center of the film. The aluminum foil was strongly soldered to the PET film at the "soldering portion" shown in the figure.
[0088] Next, the example of laminating the PET film shown in FIG. 8 will be described in detail with reference to FIG. FIG. 9 shows an example of lamination of a PET film according to the present invention. FIG. 9(a) shows a flow chart, and FIG. 9(b) shows an explanatory diagram thereof.
[0089] In (a) of Fig. 9, S21 fixes a film to a sponge. This is done by fixing a film (e.g., a PET film) to a heat-resistant sponge (e.g., with a heat-resistant polyimide tape coated with an adhesive) as shown in (b-1) on the right side.
[0090] In S22, a large amount of solder is applied to the tip of the iron. This is shown in (b-2) on the right side, where a large amount of the low-temperature solder of the present invention is applied to the tip of the iron. S23 is soldered ultrasonically so that the tip of the soldering iron does not touch the film.
[0091] For S24, flip one of the films over and place the other solder side over it. This is done so that the pre-soldered film sides overlap, as shown in (b-3) on the right.
[0092] S25 cuts the copper plate to the size of the soldering area. S26 is a method of pressing a copper plate with the tip of a soldering iron like an iron. S27 is completed when it is confirmed that the molten solder overflows from the edge. As shown in (b-4) on the right, S26 and S27 are performed by pressing the tip of the soldering iron (with ultrasonic waves) onto a copper plate with good thermal conductivity, so that the low-temperature solder on the pre-soldered joint surface melts and overflows from the edge. This allows for beautiful ultrasonic low-temperature soldering, just like ironing, without the film melting or softening and shrinking if the tip of the iron is placed directly on the film.
[0093] Fig. 9(c) shows an example of soldering conditions, which are the same as those shown in Fig. 9(a) and (b) above. Here, the following conditions were set. Tip temperature: 175℃±5℃ -Sliding value: 14 -Bedding: Poron sponge Ultrasonic output: 10W
[0094] Figure 9(d) shows a cross-sectional view of soldering. This is a schematic cross-sectional view of an example in which aluminum foil (Al) (ultrasonic pre-soldered) is bonded to a PET surface via polyimide tape, instead of the copper plate in Figure 9(a), and the two are ultrasonically low-temperature soldered together. In this case, if an adhesive-coated polyimide tape is attached so as to surround only the areas to be soldered, it is possible to prevent low-temperature soldering from being applied to unnecessary areas.
[0095] Figure 10 shows an example of an experiment using low-temperature solder under the conditions of Figures 8 and 9. This shows an example of soldering with and without ultrasonic waves. For example, the following results were obtained with the low-temperature soldering of the present invention.
[0096] No. Material Notes (Katsuragi, hardness, surface condition, etc.) 3. SUS plate: Low temperature soldering is possible if preheated. (Ultrasonic soldering, same below) ·4 Cutting board Low temperature soldering possible without preheating ·5 MDF Same as above 6 Corkboard Same as above 7 Acrylic plate Same as above 9 EPDM sponge rubber Same as above 10 NR sponge rubber Same as above 11 Boron sponge Same as above 12 NR rubber sheet Low temperature soldering is possible if preheated
[0097] The above-mentioned cellulose / resin materials can also be soldered using the low-temperature solder of the present invention. It was found that (if necessary, ultrasonic soldering or preheating (to a temperature about 10 degrees lower than the melting temperature) is used before soldering).
[0098] FIG. 10(b) shows a photographic example of the bedding material in FIG. 10(a). 11 shows an example of the results of a bonding test of the low-temperature solder of the present invention. The experimental results show the following: *1: Bonding feasibility: When a 0.2 mm diameter wire is bonded and the adhesion force is 300 g or more, it is judged as ◯. Ta. *2: US non-marked products can be attached without ultrasonic waves *3:29 PET is the No. 1 candidate for propskite.
[0099] The metals shown in Figure 11 (1 silver, 2 copper, 3 aluminum, etc.) could be soldered at low temperatures with and without ultrasonic waves. In addition, inorganic materials (7 alumina, 8 barium titanate, 10 silicon carbide, 11 silicon nitride, 12 fluorite, 13 quartz, 14 ceramic (pottery), etc.) formed by firing the oxides shown in Figure 11 were capable of low-temperature soldering with and without ultrasound.
[0100] In addition, the cellulose / resins shown in Figure 11 (16 polyethylene, 17 polypropylene) In addition, 4 cutting board and 6 cork board shown in Figure 10 were able to be soldered with ultrasonic waves.
[0101] FIG. 12 shows an example of ultrasonic output bedding of the present invention (without preheating). Fig. 12(a) shows an example of the experimental conditions. Here, the experiment was performed under the following conditions. Tip temperature: 180±5℃ - Variable speed setting (V): 14 Sunbonder display temperature (℃): 180±5 -Bedding material: Boron sponge
[0102] Figure 12(b) shows an example of the experimental results of ultrasonic output. Here, the horizontal items represent the following: · Ultrasonic output (W) indicates the ultrasonic power W applied to the tip of the soldering iron. Solderability indicates the ease of use and how well the solder adheres to the material. Adhesion when bent was judged by the way the film peeled off when bent. The film effect indicates how damage occurs when the soldering iron is applied.
[0103] When the ultrasonic output (W) was varied from 1, 2, 3, . . . 10, experiments were conducted on the other three items, and the experimental results shown in Figure 12(b) were obtained. From the results of this experiment, ultrasonic output of about 7W or more (preferably about 10W) is required for three items. It was found that good results (ultrasonic soldering results) could be obtained using this method.
[0104] Figure 13 shows an example of a temperature cycle test of the low-temperature solder of the present invention. This shows the intermediate result at 337.8 hours of the temperature cycle test. At the time of this intermediate result, no change in adhesion was observed between the start of the experiment and the intermediate result for both ultrasonic soldering and non-ultrasonic soldering. [Brief description of the drawings]
[0105] [Figure 1] FIG. 2 is an explanatory diagram of low-temperature solder manufacturing according to the present invention. [Diagram 2] 1 is an explanatory diagram of a low-temperature solder material manufacturing apparatus according to the present invention; [Diagram 3] FIG. 2 is an explanatory diagram of low-temperature soldering of the lead wire of the present invention. [Figure 4] FIG. 2 is an explanatory diagram of low-temperature soldering according to the present invention. [Diagram 5] 2 is a composition example of the low-temperature solder of the present invention. [Figure 6] 1 is a prototype of the low-temperature solder of the present invention. [Figure 7] 1 is an example of soldering using low-temperature solder of the present invention. [Figure 8] 1 is an example of low-temperature soldering (metal-metal) according to the present invention. [Figure 9] 1 is an example of laminating a PET film according to the present invention. [Figure 10] This is an experimental example of a low-temperature solder covering material of the present invention. [Figure 11] 1 shows an example of the results of a bonding test of low-temperature solder according to the present invention. [Figure 12] This is an experimental example of ultrasonic output bedding material of the present invention (without pre-heating). [Figure 13] 1 is an example of a temperature cycle test of the low-temperature solder of the present invention. [Explanation of symbols]
[0106] 1: Solder material 2: Solder material tray 3: Melting furnace 4: Heater 11: Substrate (e.g. PET board 0.1mmt) 12: Aluminum film (foil) 13, 13-1: Ultrasonic soldering iron tip 14: Low temperature soldering 15: Low temperature solder ribbon or wire
Claims
1. In low-temperature solders made of an alloy of Sn and In, A low-temperature solder containing Al, P, and optionally Cu, with the remainder being Sn and In, characterized in that the base material is an alloy of Sn and In, and the main materials are Al, which is a material that provides adhesion to an object to be soldered, and P or CuP, which is a material that removes oxides from the object to be soldered and provides adhesion, in a total amount of less than 0.73 wt% and 0.01 wt% or more, and Al and P are each excluding 0.05 wt% or less, thereby enhancing adhesion.
2. 2. The low-temperature solder according to claim 1, which is used for soldering lead wires to electrodes of solar cell substrates and liquid crystal substrates.
3. The low-temperature solder described in claim 1, characterized in that the enhanced adhesion is achieved by enhancing one or more of the adhesion forces of the objects to be soldered, that is, alloying of metals, sintering of inorganic materials formed by firing oxides, and solidifying and adhering by penetrating into gaps in the unevenness of the surface of cellulose / resin materials.
4. 4. The low-temperature solder according to claim 3, wherein the metal is aluminum, copper, iron, stainless steel, or silicon, the inorganic material is glass or ceramic, and the cellulose / resin is paper, wood, a resin film, a resin fiber, or a carbon fiber.
5. 5. The low temperature solder according to claim 4, wherein the soldering is ultrasonic soldering.
6. A low-temperature solder-coated lead wire, comprising the low-temperature solder according to any one of claims 1 to 5, melt-coated onto a surface of a wire or ribbon.
7. In a method for producing a low-temperature solder made of an alloy of Sn and In, A step of mixing a base material which is an alloy of Sn and In, Al which is a material that provides adhesion to an object to be soldered, and P or CuP which is a material that removes oxides from the object to be soldered and provides adhesion, in a total amount of less than 0.73 wt %, 0.01 wt % or more, except that Al and P are each 0.05 wt % or less; melting and alloying the entrained materials; A method for producing a low-temperature solder containing Al, P, and optionally Cu, with the remainder being Sn and In, characterized in that it has an improved adhesion.
Citation Information
Patent Citations
Leadless solder alloy
JP2000141079A
Solder alloy and solder ball
JP2005296983A
Solder, soldering method, and semiconductor device
JP2010167472A
Lead-free solder alloy and solder paste
JP2013248664A
Bi-Sn-Al BASED SOLDER ALLOY FOR MEDIUM TO LOW TEMPERATURES AND SOLDER PASTE
JP2016026884A
Cited By
Low temperature solder, method for manufacturing low temperature solder, and low temperature solder-coated lead wire
JP2024113075A